Lithium ion battery
By using lithium cobalt oxide positive electrode active substance containing Mg, F, Ni and Al and fluorocyclic carbonate electrolyte in lithium-ion batteries, the problem of insufficient charging and discharging performance of lithium-ion batteries from below freezing point to high temperature range is solved. It achieves excellent performance of the battery in a wide temperature range.
Patent Information
- Application Number
- CN202380028702.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-05
AI Technical Summary
The existing lithium-ion batteries have insufficient charging and discharging performance in high and low temperature environments, especially the battery characteristics below freezing point and the problem of battery capacity dropping at high temperatures have not been effectively solved.
Lithium cobalt oxide containing Mg, F, Ni and Al is used as the positive electrode active substance, and fluorocyclic carbonate and fluorochain carbonate are used as the electrolyte. By optimizing the crystal structure and the electrolyte composition of the positive electrode active substance, the crystal structure and electrolyte composition of the positive electrode active substance are improved. Charging and discharge performance of lithium-ion batteries from below freezing point to high temperature range.
It realizes excellent charging and discharging characteristics of lithium-ion batteries in a wide temperature range, ensures the efficient performance of the battery below freezing point and in high temperature environments, and the discharge capacity reaches more than 50% of the charging capacity of 25℃.
Smart Images

Figure CN118901159A_ABST
Abstract
Description
Technical Field
[0001] One embodiment of the present invention relates to a lithium ion battery.
[0002] In addition, one embodiment of the present invention is not limited to the above-mentioned fields, and relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, a vehicle, and a method for manufacturing the same. The semiconductor device, the display device, the light-emitting device, the power storage device, the lighting device, the electronic device, and the vehicle may use a lithium-ion battery of one embodiment of the present invention as a required power source. For example, the electronic device includes an information terminal device equipped with a lithium-ion battery, etc. Furthermore, the power storage device includes a fixed power storage device, etc.
[0003] A lithium ion battery (sometimes referred to as a lithium ion secondary battery) refers to a battery that uses lithium ions as carrier ions. A lithium ion battery is a secondary battery that can be used repeatedly by charging and discharging. However, the carrier ions of the present invention are not limited to lithium ions, and alkali metal ions or alkaline earth metal ions can also be used as carrier ions. Specifically, sodium ions or magnesium ions can be used. In this case, the present invention can be understood by replacing lithium ions with sodium ions or magnesium ions. Furthermore, in the case of not being limited to carrier ions, it is sometimes recorded as a secondary battery. Background Art
[0004] Lithium-ion batteries are expected to be able to be charged and discharged in a wide temperature range depending on their use. Therefore, research and development of lithium-ion batteries that can be charged and discharged at high or low temperatures is becoming increasingly popular. In Patent Document 1, in order to suppress the decrease in battery capacity at high temperatures, a fluorinated chain carboxylic acid ester is proposed as a non-aqueous electrolyte. In addition, in Non-Patent Document 1, in order to improve the output characteristics below the freezing point, an electrolyte mixed with methyl 3,3,3-trifluoropropionate (MTFP): fluoroethylene carbonate (FEC) = 9:1 is proposed. In addition, Non-Patent Document 2 reports on the crystal structure of the positive electrode active material. [Prior technical literature] [Patent Document]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2009-289414 [Non-patent literature]
[0006] [Non-patent document 1] John, H. et al, "An All-Fluorinated Ester Electrolyte forStable High-Voltage Li Metal Batteries Capable of Ultra-Low-TemperatureOperation", ACE Energy LETTERS, 2020, 5, 1438-1447 [Non-patent document 2] Zhaohui Chen et al., "Staging Phase Transitions in LixCoO2", Journal of The Electrochemical Society, 2002, 149(12)A1604-A1609 Summary of the invention Technical problem to be solved by the invention
[0007] In Example 1 of Patent Document 1, it is described that a material obtained by dissolving Al and Mg in lithium cobalt oxide (LiCoO2) and adding Zr to the particle surface is used as a positive electrode active material, and a material obtained by mixing 4-fluoroethylene carbonate (4-FEC) and CF3CH2COOCH3 in a volume ratio of 2:8 is used as an organic solvent for a non-aqueous electrolyte. However, Patent Document 1 does not explore the battery characteristics below the freezing point.
[0008] Non-patent document 1 states that, in order to investigate the battery characteristics below freezing point, a material in which methyl 3,3,3-trifluoropropionate (MTFP) and fluoroethylene carbonate (FEC) were mixed in a ratio of 9:1 was used as an organic solvent for a non-aqueous electrolyte, and NMC811 was used as a positive electrode active material in a cycle test. However, non-patent document 1 does not investigate the battery characteristics at high temperatures.
[0009] In view of the above, one object of the present invention is to provide a lithium ion battery comprising an electrolyte containing a novel organic solvent and a novel positive electrode active material, which can be charged and discharged in a wide temperature range from below freezing to high temperatures.
[0010] In addition, the above-mentioned purpose does not prevent the existence of other purposes. In addition, the above-mentioned purposes are considered to be independent of each other, and one mode of the present invention does not need to achieve all of the above-mentioned purposes. Furthermore, purposes other than the above-mentioned can be extracted from the description of the specification, drawings and claims (which are recorded as "this specification, etc."). Solutions to technical problems
[0011] To solve the above problems, one aspect of the present invention is a lithium-ion battery, comprising: a positive electrode containing a positive electrode active material; and an electrolyte, wherein the positive electrode active material contains lithium cobaltate containing Mg, F, Ni, and Al, and the electrolyte contains a fluorinated cyclic carbonate and a fluorinated chain carbonate.
[0012] Another aspect of the present invention is a lithium-ion battery, comprising: a positive electrode containing a positive electrode active material; and an electrolyte, wherein the positive electrode active material contains lithium cobaltate containing Mg, F, Ni, and Al, and the electrolyte contains fluoroethylene carbonate and methyl trifluoropropionate. When the total content of fluoroethylene carbonate and methyl trifluoropropionate is 100 vol%, the volume ratio of fluoroethylene carbonate to methyl trifluoropropionate is x:100 - x (note that 5 ≤ x ≤ 30).
[0013] Preferably, the lithium cobaltate of one aspect of the present invention is represented by Li x CoO2. When x is 1 in Li x CoO2, the lithium cobaltate has a layered rock salt-type crystal structure belonging to the space group R-3m. And when x is 0.1 < x ≤ 0.24 in Li x CoO2, i.e., in the charged state, the lithium cobaltate has a crystal structure with the space group P2 / m, lattice constant a = 0.488 ± 0.001 nm, lattice constant b = 0.282 ± 0.001 nm, lattice constant c = 0.484 ± 0.001 nm, α = 90°, β = 109.58 ± 0.01°, γ = 90°.
[0014] Preferably, the lithium cobaltate of another aspect of the present invention is represented by Li x CoO2. When x is 1 in Li x CoO2, the lithium cobaltate has a layered rock salt-type crystal structure belonging to the space group R-3m. And when x is 0.1 < x ≤ 0.24 in Li x CoO2, i.e., in the charged state, when analyzing the lithium cobaltate by X-ray diffraction, there are diffraction peaks at least at 2θ = 19.37° or more and 19.57° or less and at 2θ = 45.57° or more and 45.67° or less.
[0015] The median particle size (D50) of the lithium cobaltate of another aspect of the present invention is preferably 10 μm or more and 14 μm or less.
[0016] The median particle size (D50) of the lithium cobaltate of another aspect of the present invention is preferably 5 μm or more and 9 μm or less.
[0017] Another embodiment of the present invention is a lithium ion battery, comprising: a positive electrode active material comprising lithium cobalt oxide containing Mg, F, Ni and Al; and an electrolyte comprising a fluorinated cyclic carbonate and a fluorinated chain carbonate, wherein a half-cell comprising a positive electrode comprising the positive electrode active material, the electrolyte and a lithium metal for a counter electrode is prepared, the half-cell is arranged at an ambient temperature of 25°C, and a constant current charge is performed at a rate of 0.1C (note, 1C=200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.6V, and a constant voltage charge is performed at 4.6V until the current value reaches 0.05C, and then the half-cell is charged at a rate of 0.1C (note, 1C=200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.6V, and a constant voltage charge is performed at 4.6V until the current value reaches 0.05C, and then the half-cell is charged at a rate of 0.05C. .1C rate of constant current discharge until the voltage reaches 2.5V, thereby calculating the discharge capacity value, compared with the discharge capacity value, the discharge capacity value calculated by the following steps is 50% or more, that is, the half-cell is configured at an ambient temperature of 25°C, and constant current charging is performed at a rate of 0.1C (note, 1C = 200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.6V, and constant voltage charging is performed at 4.6V until the current value reaches 0.05C, and then the half-cell is configured at an ambient temperature of -40°C and constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V.
[0018] Another embodiment of the present invention is a lithium ion battery, comprising: a positive electrode having a positive electrode active material comprising lithium cobalt oxide containing Mg, F, Ni and Al; and an electrolyte, wherein a half-cell comprising a positive electrode comprising the positive electrode active material, the electrolyte and lithium metal for a counter electrode is prepared, the half-cell is arranged at an ambient temperature of 25°C, and a constant current charge is performed at a rate of 0.1C (note, 1C = 200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.6V, and a constant voltage charge is performed at 4.6V until the current value reaches 0.05C, and then a constant voltage charge is performed at a rate of 0.1C. The half-cell is discharged at a constant current until the voltage reaches 2.5V, and the discharge capacity value is calculated therefrom. Compared with the discharge capacity value, the discharge capacity value calculated by the following steps is 50% or more, that is, the half-cell is placed at an ambient temperature of 25°C, and is charged at a constant current rate of 0.1C (note, 1C = 200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.6V, and is charged at a constant voltage of 4.6V until the current value reaches 0.05C, and then the half-cell is placed at an ambient temperature of -40°C, and is discharged at a constant current rate of 0.1C until the voltage reaches 2.5V.
[0019] Another embodiment of the present invention is a lithium ion battery, comprising: a positive electrode active material comprising nickel, cobalt and manganese; and an electrolyte comprising a fluorinated cyclic carbonate and a fluorinated chain carbonate, wherein a half-cell comprising a positive electrode comprising the positive electrode active material, an electrolyte and a lithium metal for a counter electrode is arranged at an ambient temperature of 25°C, and a constant current charge is performed at a rate of 0.1C (note, 1C = 200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.5V, and a constant voltage charge is performed at 4.5V until the current value reaches 0.05C, and then the half-cell is arranged at -40°C. At an ambient temperature of , constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V, thereby obtaining a discharge capacity value that satisfies more than 50% of the discharge capacity value obtained by the following steps, i.e., the half-battery is configured at an ambient temperature of 25°C, and constant current charging is performed at a rate of 0.1C (note, 1C = 200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.5V, and constant voltage charging is performed at 4.5V until the current value reaches 0.05C, and then constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V.
[0020] Another embodiment of the present invention is a lithium ion battery, comprising: a positive electrode active material comprising nickel, cobalt and manganese; and an electrolyte, wherein the electrolyte comprises fluoroethylene carbonate and methyl trifluoropropionate, and when the total content of fluoroethylene carbonate and methyl trifluoropropionate is 100 vol%, the volume ratio of fluoroethylene carbonate to methyl trifluoropropionate is x:100-x (note, 5≤x≤30), and a half-cell comprising a positive electrode comprising the positive electrode active material, an electrolyte and a lithium metal for a counter electrode is arranged at an ambient temperature of 25°C, and is charged at a constant current rate of 0.1C (note, 1C=200 mA / g (the current per unit weight of the positive electrode active material is 200 mA / g)) until the voltage reaches 4.5 V, and is charged at a constant current rate of 4. 5V is charged at a constant voltage until the current value reaches 0.05C, and then the half-cell is configured at an ambient temperature of -40°C and discharged at a constant current rate of 0.1C until the voltage reaches 2.5V, thereby obtaining a discharge capacity value, which meets more than 50% of the discharge capacity value obtained by the following steps, that is, the half-cell is configured at an ambient temperature of 25°C, and charged at a constant current rate of 0.1C (note, 1C = 200mA / g (the current per unit weight of the positive electrode active material is 200mA / g)) until the voltage reaches 4.5V, and charged at a constant voltage of 4.5V until the current value reaches 0.05C, and then discharged at a constant current rate of 0.1C until the voltage reaches 2.5V.
[0021] In another embodiment of the present invention, in the positive electrode active material, the ratio of nickel:cobalt:manganese preferably satisfies 8:1:1 or in the vicinity thereof.
[0022] In another embodiment of the present invention, in the positive electrode active material, the proportion of nickel is preferably larger than the proportion of cobalt and the proportion of manganese.
[0023] In another embodiment of the present invention, the median particle size (D50) of the positive electrode active material is preferably 4 μm or more and 7 μm or less.
[0024] In another embodiment of the present invention, the separator of the half-cell preferably comprises polyimide.
[0025] In another embodiment of the present invention, the separator of the half-cell preferably comprises polypropylene. Effects of the Invention
[0026] According to one embodiment of the present invention, a lithium ion battery including an electrolyte containing a novel organic solvent and a novel positive electrode active material can be provided. According to one embodiment of the present invention, a lithium ion battery capable of being charged and discharged in a wide temperature range from below freezing to high temperature can be provided.
[0027] In addition, the above effects do not hinder the existence of other effects. In addition, the above effects are considered to be independent of each other, and one embodiment of the present invention does not need to have all of the above effects. Furthermore, effects other than the above can be extracted from the description of this specification, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1A and Figure 1B It is a diagram for explaining a lithium ion battery according to one embodiment of the present invention. FIG. 2A to FIG. 2C It is a diagram for explaining a method for producing a positive electrode according to one embodiment of the present invention. FIG. 3A to FIG. 3F This is a diagram for explaining a positive electrode active material according to one embodiment of the present invention. Figure 4 This is a diagram illustrating the crystal structure of a positive electrode active material according to one embodiment of the present invention. Figure 5 It is a diagram illustrating the crystal structure of the positive electrode active material. Figure 6 This is a diagram illustrating the diffraction peaks of the positive electrode active material. Figure 7 This is a diagram illustrating the diffraction peaks of the positive electrode active material. Fig. 8A and Figure 8B This is a diagram illustrating the diffraction peaks of the positive electrode active material. Fig. 9It is a diagram for explaining a method for producing a positive electrode according to one embodiment of the present invention. Fig.10 It is a diagram for explaining a method for producing a positive electrode according to one embodiment of the present invention. Fig.11 It is a diagram for explaining a method for producing a positive electrode according to one embodiment of the present invention. Fig.12 It is a diagram for explaining a method for producing a positive electrode according to one embodiment of the present invention. Fig.13 It is a diagram for explaining a method for producing a positive electrode according to one embodiment of the present invention. FIG. 14A to FIG. 14D This is a diagram for explaining a positive electrode according to one embodiment of the present invention. FIG. 15A to FIG. 15D This is a diagram for explaining a positive electrode according to one embodiment of the present invention. Fig.16A and Fig. 16B It is a diagram for explaining a lithium ion battery according to one embodiment of the present invention. 17A to 17C It is a diagram for explaining a lithium ion battery according to one embodiment of the present invention. 18A to 18D It is a diagram for explaining a lithium ion battery and a power storage system according to one embodiment of the present invention. FIG. 19A to FIG. 19C It is a diagram for explaining a lithium ion battery according to one embodiment of the present invention. FIG. 20A to FIG. 20C It is a diagram for explaining a lithium ion battery according to one embodiment of the present invention. FIG. 21A to FIG. 21C It is a diagram for explaining an electric vehicle according to one embodiment of the present invention. FIG. 22A to FIG. 22D It is a diagram for explaining a transport vehicle according to one embodiment of the present invention. FIG. 23A to FIG. 23C It is a figure explaining the two-wheeled vehicle etc. which are one embodiment of this invention. FIG. 24A to FIG. 24D It is a diagram for explaining an electronic device and the like according to one embodiment of the present invention. FIG. 25A to FIG. 25D is a diagram showing an example of space equipment. Fig.26A and Fig.26B This is a chart showing NMR of an organic solvent of an electrolyte according to one embodiment of the present invention. Fig.27A and Fig.27B This is a chart showing NMR of an organic solvent of an electrolyte according to one embodiment of the present invention. Fig.28A and Fig.28B This is a chart showing NMR of an organic solvent of an electrolyte according to one embodiment of the present invention. Fig.29A and Fig.29B It is a diagram for explaining the AC impedance measurement. FIG. 30A to FIG. 30C This is a graph showing the results of AC impedance measurement of a sample including an electrolyte and a positive electrode active material according to one embodiment of the present invention. FIG. 31A to FIG. 31C This is a graph showing the results of AC impedance measurement of a sample including an electrolyte and a positive electrode active material according to one embodiment of the present invention. Fig.32A and Fig.32B This is a graph showing the charge capacity and discharge capacity of samples including the electrolyte and the positive electrode active material according to one embodiment of the present invention. Fig.33A and Fig.33B This is a graph showing the charge capacity and discharge capacity of samples including the electrolyte and the positive electrode active material according to one embodiment of the present invention. Fig.34A and Fig.34B This is a graph showing the charge capacity and discharge capacity of samples including the electrolyte and the positive electrode active material according to one embodiment of the present invention. Fig.35A and Fig.35B It is a graph showing a charge curve and a discharge curve of a sample including an electrolyte and a positive electrode active material according to one embodiment of the present invention. FIG. 36A to FIG. 36C This is a graph showing the cycle characteristics of a sample including an electrolyte and a positive electrode active material according to one embodiment of the present invention. Fig.37 This is a graph showing the viscosity of an organic solvent in an electrolyte according to one embodiment of the present invention. Fig.38A and Fig.38B This is a graph showing the charge capacity and discharge capacity of samples including the electrolyte and the positive electrode active material according to one embodiment of the present invention. Fig.39A and Fig.39B is a graph showing DSC results of organic liquids. Fig.40 is a diagram showing a model used for calculation. Fig.41 is a graph showing the activation barrier for lithium ion diffusion. Fig.42A and Fig.42B It is a graph showing the charge and discharge curve (25° C.) of the full battery. Fig.43A and Fig.43B It is a graph showing the cycle characteristics (25° C.) of the full battery. Modes for Carrying Out the Invention
[0029] The embodiments are described in detail with reference to the accompanying drawings. Note that the present invention is not limited to the following description, and a person skilled in the art can easily understand that the method and details can be transformed into various forms without departing from the purpose and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the contents described in the embodiments shown below. Note that in the inventive structure described below, the same figure mark is used in different drawings to represent the same part or the part with the same function, and repeated description is omitted.
[0030] Note that ordinal numerals such as "first" and "second" in this specification, etc. are added to avoid confusion between constituent elements, and do not indicate a certain order or sequence such as process order or stacking order. Note that for terms that are not added with ordinal numerals in this specification, etc., ordinal numerals are sometimes added to the terms in the claims to avoid confusion between constituent elements. Note that for terms that are added with ordinal numerals in this specification, etc., different ordinal numerals are sometimes added to the terms in the claims. Note that for terms that are added with ordinal numerals in this specification, etc., their ordinal numerals are sometimes omitted in the claims, etc.
[0031] In this specification, etc., the positive electrode active material refers to a compound containing a transition metal and oxygen in which carrier ions can be embedded and released. Compounds containing oxygen are sometimes referred to as oxides or composite oxides. Lithium ions are typically used as carrier ions, but sodium ions or magnesium ions, etc., may also be used. Carbonic acid and hydroxyl groups adsorbed after the positive electrode active material is manufactured are not included in the positive electrode active material. In addition, electrolytes, organic solvents, adhesives, conductive materials or compounds derived from them that are attached to the positive electrode active material are also not included in the positive electrode active material.
[0032] In this specification, etc., "homogeneous" refers to the phenomenon that a certain element (such as A) in a solid containing multiple elements (such as A, B, C) has the same characteristics and is distributed in a specific area. Specifically, the element concentration between specific areas is substantially the same. For example, the difference in element concentration between specific areas is within 10%, and this situation is sometimes referred to as substantially the same concentration. As specific areas, for example, the surface part, convex part, concave part or interior of the active material can be cited, and as long as the element concentration in the convex part and the interior is substantially the same, it can be said that the elements exist homogeneously in the convex part and the interior.
[0033] In this specification, etc., "segregation" refers to a phenomenon in which a certain element (e.g., B) is spatially unevenly distributed in a solid containing multiple elements (e.g., A, B, C), that is, a certain element (e.g., B) has a different concentration in a specific area from another specific area. "Segregation" is synonymous with partiality, precipitation, unevenness, deviation, or a mixture of a high-concentration area and a low-concentration area.
[0034] In this specification, the term "particle" used for active material particles is not limited to spherical (circular in cross section). For example, particles include particles with elliptical or asymmetric cross sections, and the particles do not need to be aligned and may be non-aligned.
[0035] In this specification, “below freezing point” means below 0° C., “high temperature” means above 25° C., and room temperature means above 0° C. and below 25° C. In this specification, “temperature range from below freezing point to high temperature” includes the room temperature.
[0036] "Non-aqueous electrolyte" contains an organic solvent that exhibits carrier ion conductivity, and generally refers to a liquid electrolyte, but is not limited to a liquid in the present invention. Therefore, in this specification, etc., the concept related to the non-aqueous electrolyte is recorded as "electrolyte". In other words, the state of the electrolyte of one embodiment of the present invention is not limited, for example, it also includes an electrolyte whose viscosity is increased from a liquid state by adjusting the viscosity. Furthermore, the electrolyte also includes a solid or semi-solid state. Semi-solid refers to an intermediate state between a liquid and a solid state. Specifically, a semi-solid state includes a solid state with flexibility, typically including a gel state. In general, a semi-solid electrolyte is sometimes referred to as a semi-solid electrolyte, and an electrolyte of one embodiment of the present invention also includes a semi-solid electrolyte. The above-mentioned liquid, solid or semi-solid state or viscosity is confirmed when the lithium ion battery is placed at 25°C.
[0037] In this specification, "carbonate" refers to a compound containing at least one carbonate in its molecular structure, and includes "cyclic carbonate" and "chain carbonate" unless otherwise specified. The category of "chain" includes straight chain and branched chain.
[0038] In this specification and the like, a value indicating the magnitude of viscosity is referred to as viscosity, and moderate viscosity means having a viscosity suitable for lithium ion batteries.
[0039] In this specification and the like, “including A and / or B” may be described, which means “including A”, “including B”, or “including A and B”.
[0040] In this specification, a full cell refers to a battery unit assembled in a manner including different electrodes such as a positive electrode / negative electrode unit cell. In this specification, a half cell refers to a battery unit assembled using lithium metal as a negative electrode (counter electrode).
[0041] (Implementation Method 1) In this embodiment, a lithium ion battery according to one embodiment of the present invention is described with reference to the drawings.
[0042] <Lithium-ion battery> A lithium ion battery of one embodiment of the present invention includes an electrolyte capable of being charged and discharged in a wide temperature range from at least below freezing point to high temperature. In addition to the above-mentioned electrolyte, the lithium ion battery also includes a negative electrode, a positive electrode, a separator between the negative electrode and the positive electrode, and an outer packaging body covering the surroundings of the negative electrode and the positive electrode. Although lithium ion batteries are called laminated lithium ion batteries, coin cell lithium ion batteries, or cylindrical lithium ion batteries according to the form of the outer packaging body, the present invention is not limited to the form of the outer packaging body. When the electrolyte is solid or semi-solid, the separator can be omitted.
[0043] Figure 1A 1 shows the structure of a lithium ion battery 100. When viewed in cross section, it can be confirmed that the lithium ion battery 100 includes a negative electrode 106, a separator 108, and a positive electrode 107. In the lithium ion battery 100, it is assumed that the electrolyte 109 is in a liquid state, and the electrolyte 109 is present in the entire negative electrode 106, the separator 108, and the positive electrode 107. As described above, the electrolyte 109 is not limited to a liquid state.
[0044] The negative electrode 106 includes a negative electrode current collector 101 and a negative electrode active material layer 102. The negative electrode active material layer 102 contains at least a negative electrode active material, and may also contain a conductive material and / or a binder. The negative electrode active material may use a known material, and its details will be described later. The positive electrode 107 includes a positive electrode current collector 105 and a positive electrode active material layer 104. The positive electrode active material layer 104 contains at least a positive electrode active material, and may also contain a conductive material and / or a binder. The positive electrode active material may also use a known material, but by using a positive electrode active material in one embodiment of the present invention, it can withstand high voltage charging, thereby increasing the discharge capacity of the lithium ion battery. The positive electrode active material in one embodiment of the present invention will be described later.
[0045] The conductive material has the function of assisting the current path between the positive electrode active materials and / or between the positive electrode active materials and the current collector. In addition, the conductive material has the function of assisting the current path between the negative electrode active materials and / or between the negative electrode active materials and the current collector. As the conductive material, a known material can be used, and its details will be described later. The binder is also called a bonding agent, and has the function of assisting the adhesion between the positive electrode active materials and / or between the positive electrode active materials and the current collector. In addition, the binder has the function of assisting the adhesion between the negative electrode active materials and / or between the negative electrode active materials and the current collector. As the binder, a known material can be used, and its details will be described later.
[0046] Figure 1B The example shown is similar to Figure 1A Differently, the lithium ion battery 100 does not include the negative electrode active material layer 102. Depending on the material of the negative electrode collector 101, the negative electrode active material layer 102 may not be used. Figure 1BOther structures of the lithium-ion battery 100 are Figure 1A Since the lithium ion battery 100 is the same as that of the lithium ion battery 100, the description thereof will be omitted.
[0047] In this embodiment, a lithium ion battery having excellent discharge characteristics and / or excellent charging characteristics can be realized in a wide temperature range from below freezing point to high temperature. In particular, a lithium ion battery having excellent discharge characteristics and / or excellent charging characteristics can be realized at any temperature below freezing point (for example, below 0°C, below -20°C, preferably below -30°C, more preferably below -40°C, further preferably below -50°C, and further preferably below -60°C). To this end, the structure of the required lithium ion battery is described. Specifically, the description is centered on the positive electrode active material and the electrolyte. The details of the constituent elements other than the positive electrode active material and the electrolyte contained in the lithium ion battery will be described after Embodiment 3.
[0048] <Positive Electrode Active Material> The positive electrode active material has the function of absorbing lithium ions as carrier ions and / or releasing the lithium ions as the charge and discharge proceeds. As a positive electrode active material for one embodiment of the present invention, a material that can be charged and discharged with a high charge voltage at least below the freezing point and has little deterioration due to charge and discharge (or a material with little resistance increase) can be used. In this specification, etc., in the absence of special instructions, "charge voltage" is expressed as a reference to the potential of lithium metal. In this specification, etc., "high charge voltage" is, for example, a charge voltage of 4.4V or more, preferably a charge voltage of 4.5V or more, and more preferably a charge voltage of 4.6V or more.
[0049] The positive electrode active material is not limited to one, as long as it is a material that is less degraded by charge and discharge at least below the freezing point even at a high charging voltage, two or more materials with different median particle sizes (D50) can be mixed, and two or more materials with different compositions can also be mixed. In this specification, "different composition" includes not only the case where the structure of the elements contained in the material is different, but also includes the case where the structure of the elements contained in the material is the same but the proportion of the elements contained is different.
[0050] Note that, as described above, in this specification, etc., "high charge voltage" means 4.5 V or more based on the potential when lithium metal is used as the negative electrode, but based on the potential when a carbon material (e.g., graphite) is used as the negative electrode, a voltage of 4.4 V or more is referred to as "high charge voltage." Specifically, in the case of a half cell using lithium metal as the negative electrode, a charge voltage of 4.5 V or more is referred to as a high charge voltage, and in the case of a full cell using a carbon material (e.g., graphite) as the negative electrode, a charge voltage of 4.4 V or more is referred to as a high charge voltage.
[0051] By using a material that deteriorates less due to charging and discharging at any temperature below the freezing point and at a high charging voltage (or a material with less increase in resistance) as a positive electrode active material, a lithium-ion battery with a large charge capacity and / or discharge capacity at a temperature below the freezing point can be realized. Specifically, a lithium-ion battery having a charge capacity and / or discharge capacity at any temperature below the freezing point of more than 50% (preferably more than 60%, more preferably more than 70%, and most preferably more than 80%) of the charge capacity and / or discharge capacity at 25°C can be realized.
[0052] The temperature during charging or discharging described in this specification, etc., refers to the temperature of the environment in which the lithium-ion battery is placed (hereinafter, sometimes referred to as "ambient temperature" in this specification, etc.). In the measurement of battery characteristics, since a thermostatic bath that is stable at a desired temperature is used, the ambient temperature is equal to the temperature of the thermostatic bath. The measurement can be started after the test unit (e.g., a full battery or a half battery) of the measurement object is placed in the thermostatic bath and left for a sufficiently long time (e.g., more than 1 hour) until the temperature of the test unit reaches the same level as the temperature of the thermostatic bath, but the measurement of battery characteristics is not limited to this method.
[0053] <Electrolytes> The electrolyte used in one embodiment of the present invention may be a material having good lithium ion conductivity at any temperature below freezing (for example, 0°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C or -60°C).
[0054] The electrolyte contains an organic solvent. The organic solvent of the electrolyte of one embodiment of the present invention is not limited to being liquid at 25°C, but may be solid at 25°C or semi-solid at 25°C. In addition, the organic solvent of the electrolyte of one embodiment of the present invention is preferably liquid at any temperature below the freezing point (for example, 0°C, -20°C, preferably -30°C, more preferably -40°C, further preferably -50°C or -60°C), but is not limited thereto. The organic solvent of the electrolyte of one embodiment of the present invention may be liquid, solid or semi-solid at any temperature below the freezing point.
[0055] <Organic Solvents> The organic solvent described in the present embodiment preferably comprises fluorinated cyclic carbonate (sometimes denoted as fluorinated cyclic carbonate) or fluorinated chain carbonate (sometimes denoted as fluorinated chain carbonate). And, the above-mentioned organic solvent preferably comprises fluorinated cyclic carbonate and fluorinated chain carbonate simultaneously. Fluorinated cyclic carbonate and fluorinated chain carbonate both have a substituent that presents electron-withdrawing property, and the solvation energy of its lithium ion is lower than the organic compound that does not have a substituent that presents electron-withdrawing property. Therefore, fluorinated cyclic carbonate and fluorinated chain carbonate are all suitable for organic solvent.
[0056] As fluorinated cyclic carbonate, for example, fluorinated ethylene carbonate (also referred to as fluorinated ethylene carbonate, FEC, F1EC), difluoroethylene carbonate (DFEC, F2EC), trifluoroethylene carbonate (F3EC) or tetrafluoroethylene carbonate (F4EC) etc. can be used. In addition, as DFEC, isomers such as cis-4,5, trans-4,5 can be cited. Any fluorinated cyclic carbonate has a substituent that exhibits electron-withdrawing property, and therefore it is considered that the solvation energy of lithium ions is low.
[0057] The following structural formula (H10) is the structural formula of FEC. In FEC, the electron-withdrawing substituent is a F group.
[0058] [Chemical formula 1]
[0059] As a fluorinated chain carbonate, there is methyl 3,3,3-trifluoropropionate. The following structural formula (H22) is the structural formula of methyl 3,3,3-trifluoropropionate. Methyl 3,3,3-trifluoropropionate is abbreviated as "MTFP". In MTFP, the electron-withdrawing substituent is a CF3 group.
[0060] [Chemical formula 2]
[0061] As the fluorinated chain carbonate, there is trifluoromethyl 3,3,3-trifluoropropionate. The following structural formula (H23) is the structural formula of trifluoromethyl 3,3,3-trifluoropropionate. The electron-withdrawing substituent is a CF3 group.
[0062] [Chemical formula 3]
[0063] As a fluorinated chain carbonate, there is trifluoromethyl propionate. The following structural formula (H24) is the structural formula of trifluoromethyl propionate. The electron-withdrawing substituent is a CF3 group.
[0064] [Chemical formula 4]
[0065] As a fluorinated chain carbonate, there is methyl 2,2-difluoropropionate. The following structural formula (H25) is the structural formula of methyl 2,2-difluoropropionate. The electron-withdrawing substituent is the CF2 group.
[0066] [Chemical formula 5]
[0067] The organic solvent of the electrolyte as a mode of the present invention preferably contains one or more selected from the above fluorinated cyclic carbonates and one or more selected from the above fluorinated chain carbonates. For example, the organic solvent described in this embodiment preferably contains FEC and MTFP. The reasons are described below.
[0068] <FEC and MTFP> FEC is one of the cyclic carbonates. Because it has a high relative dielectric constant, it has the effect of promoting the dissociation of lithium salts when used as an organic solvent. And, FEC has a substituent that exhibits electron-withdrawing properties, so it is easily bonded to lithium ions by Coulomb force or the like. Specifically, it can be said that the solvation energy of FEC is smaller than that of ethylene carbonate (abbreviated as "EC") that does not have a substituent that exhibits electron-withdrawing properties, so it is easy to form solvation with lithium ions. And, it is considered that the highest occupied molecular orbital (HOMO: Highest Occupied Molecular Orbital) energy level of FEC is deep, and when the HOMO energy level is deep, it is not easily oxidized, and the antioxidant property is improved. On the other hand, the viscosity of FEC is high, and when only FEC is used as an organic solvent, it is difficult to use below the freezing point. Therefore, the organic solvent specifically described as a mode of the present invention contains not only FEC but also MTFP. MTFP is one of the chain carbonates, and it has the effect of reducing or maintaining the viscosity of the electrolyte. Of course, the solvation energy of MTFP is smaller than that of methyl propionate (abbreviated as "MP") that does not have a substituent that exhibits electron-withdrawing properties, so it can also form solvation with lithium ions.
[0069] It is preferable to set the total content of the organic solvent containing both FEC and MTFP having the above physical properties to 100 vol%, and mix them in a volume ratio of x:100 - x (note that 5 ≤ x ≤ 30, preferably 10 ≤ x ≤ 20) for use. It is preferable to mix them in such a way that MTFP in the mixed organic solvent is more than FEC. Note that the above volume ratio can also be the volume ratio measured before mixing the organic solvents, and the external air when mixing the organic solvents can also be at room temperature (typically 25°C). The organic solvent mixed with FEC and MTFP exhibits viscosity that can operate as a lithium-ion battery, and maintains appropriate viscosity even below the freezing point, so it is preferable.
[0070] Organic solvents commonly used in lithium-ion batteries solidify at around -20°C, so it is difficult to manufacture lithium-ion batteries that can be charged and discharged at -40°C, preferably -50°C or -60°C. However, the solidification point of the organic solvent described as an example in this embodiment can be below -40°C, preferably below -50°C, and a lithium-ion battery that can be charged and discharged in an environment below the freezing point can be realized. As a result, a lithium-ion battery that can be charged and discharged in a wide temperature range including at least below the freezing point can be realized.
[0071] Although described as representative with FEC in the above description, it can be said that all organic compounds described as fluorinated cyclic carbonate all have the effect of promoting the dissociation of lithium salts, and easily make lithium ion solvation because of the low solvation energy, and be difficult to use alone below freezing point because of its viscosity high.In addition, although described as representative with MTFP in the above description, it can be said that all organic compounds described as fluorinated chain carbonate all have the effect of reducing or maintaining the viscosity of the electrolyte of one mode of the present invention.Therefore, as long as the organic solvent of one mode of the present invention comprises fluorinated cyclic carbonate and fluorinated chain carbonate, it is possible to provide a lithium ion battery that can be charged and discharged in the wide temperature range comprising below freezing point.
[0072] Preferably, the content of the granular dust or elements other than the constituent elements of the organic solvent (hereinafter referred to as "impurities", including water or moisture) in the organic solvent is small and highly purified. Specifically, the ratio of impurities in the organic solvent is 1 mol% or less, preferably 0.1 mol% or less, and more preferably 0.01 mol% or less.
[0073] <Lithium Salt> As the lithium salt dissolved in the above organic solvent, for example, LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10 、Li2B 12 Cl 12 , LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2 and lithium bis(oxalate borate) (LiBOB). The lithium salt is one of the constituent elements contained in the electrolyte of one embodiment of the present invention, but it is not necessarily required to contain the lithium salt.
[0074] <Additives> In addition, in order to improve safety, etc., an organic solvent can also be mixed with an additive to form a coating at the interface of the active material and the electrolyte. The additive can be selected from one or more of dinitrile compounds such as vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate borate) (LiBOB) and SUN (octanonitrile), succinonitrile or adiponitrile. For example, the concentration of the additive can be set to more than 0.1wt% and less than 5wt% in the organic solvent as a whole. The additive is one of the constituent elements included in the electrolyte of one embodiment of the present invention, but it is not necessarily necessary to include an additive. In addition, it is preferred to select a material different from the organic solvent as an additive.
[0075] An example of an electrolyte that can be used in a lithium ion battery according to one embodiment of the present invention is described above, but the electrolyte that can be used in a lithium ion battery according to one embodiment of the present invention is not limited to this example. Other materials can be used as long as they have suitable viscosity below freezing point and have excellent lithium ion conductivity.
[0076] A lithium ion battery according to one embodiment of the present invention includes at least the above-described positive electrode active material and an electrolyte, thereby realizing a lithium ion battery that can be charged and discharged in a wide temperature range including at least below freezing.
[0077] (Implementation Method 2) In this embodiment, refer to FIG. 2A to FIG. 2C A positive electrode active material that can be used in a lithium ion battery according to one embodiment of the present invention (hereinafter sometimes referred to as “positive electrode active material that can be used in one embodiment of the present invention”) and a method for producing the same will be described.
[0078] In addition, as described in Embodiment 1, as a positive electrode active material of a lithium ion battery that can be used in one embodiment of the present invention, any material can be used as long as it is a material with little degradation associated with charging and discharging at a high charging voltage. Therefore, the positive electrode active material that can be used for the lithium ion battery disclosed in this specification, etc. does not need to be limited to the specific material described in this embodiment, etc., and a material known as a material with little degradation associated with charging and discharging even when a high charging voltage (e.g., above 4.5V) is used at the time of this patent application can also be used.
[0079] An example of a method for producing a positive electrode active material that can be used in one embodiment of the present invention is described below. In this embodiment, a case where a positive electrode active material is produced using a solid phase method is described, but the lithium ion battery of the present invention can use a positive electrode active material that uses a coprecipitation method or a hydrothermal method in addition to the solid phase method. Note that the flow chart used to illustrate the production method in this embodiment shows the order of elements connected by lines, and does not show the order of elements not connected by lines.
[0080] [Method for producing positive electrode active material] Reference FIG. 2A to FIG. 2C An example of a production process of the positive electrode active material 10 will be described.
[0081] <Step S11> exist Figure 2A In step S11 shown, as the starting materials of lithium and transition metal M, a lithium source (Li source) and a transition metal M source (M source) are prepared respectively. As the lithium source, a compound containing lithium is preferably used, for example, lithium carbonate, lithium hydroxide, lithium nitrate or lithium fluoride can be used. The transition metal M uses one or more of manganese, cobalt and nickel, for example. When lithium cobalt oxide (LCO) is manufactured as a positive electrode active material, cobalt is used as the transition metal M. When nickel-cobalt-manganese composite oxide (NCM) is manufactured as a positive electrode active material, cobalt, manganese and nickel are used as the transition metal M. In addition to the transition metal M, aluminum can also be used.
[0082] As the transition metal M source, a compound containing the above-mentioned transition metal M is preferably used, for example, an oxide or hydroxide of the metal shown as an example of the above-mentioned transition metal M can be used. As a cobalt source, cobalt oxide, cobalt hydroxide, etc. can be used. As a manganese source, manganese oxide, manganese hydroxide, etc. can be used. As a nickel source, nickel oxide, nickel hydroxide, etc. can be used. As an aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used. In addition, when using two or more transition metal M sources, it is preferred to prepare the two or more transition metal M sources in a ratio (mixing ratio) that can have a layered rock salt type crystal structure.
[0083] <Step S12> Then, as Figure 2A In step S12 shown, the Li source and the M source are crushed and mixed to produce a mixed material. The crushing and mixing process can be performed by a dry method or a wet method. When using the wet method, a solvent is prepared. As the solvent, ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. can be used. Acetone with a water content suppressed to less than 10 ppm and a purity of more than 99.5% is recorded as "dehydrated acetone", and dehydrated acetone is preferably used as a solvent.
[0084] <Step S13> Then, as Figure 2AIn step S13 shown, the mixed material is heated. The heating temperature is preferably 800°C or more and 1100°C or less, more preferably 900°C or more and 1000°C or less. When the temperature is too low, there is a concern that the decomposition and melting of the Li source and the M source are insufficient. On the other hand, when the temperature is too high, there is a concern that lithium sublimates from the Li source and / or the transition metal used as the M source is excessively reduced. When the heating time is too short, a composite oxide containing lithium and the transition metal M cannot be synthesized, and when the heating time is too long, the productivity decreases. Therefore, the heating time can be 1 hour or more and 100 hours or less, preferably 2 hours or more and 20 hours or less. The heating rate depends on the temperature reached by the heating temperature, preferably 80°C / h or more and 250°C / h or less, more preferably 100°C / h or more and 250°C / h or less.
[0085] The heating atmosphere is preferably an atmosphere with less moisture. An atmosphere with a specific low moisture content at a dew point can be used. For example, an atmosphere with a dew point of -50°C or less, more preferably -80°C or less, is preferably used as the heating atmosphere. Furthermore, the heating atmosphere is preferably an atmosphere containing oxygen such as dry air. For example, a method of continuously introducing oxygen into the reaction chamber can be cited. In this case, the oxygen flow rate is preferably 5 L / min or more and 15 L / min or less. The state of continuously introducing oxygen into the reaction chamber so that the oxygen flows through the reaction chamber is called "flow".
[0086] As a method for making the heating atmosphere an oxygen-containing atmosphere, in addition to the above process, for example, the following method can also be used: oxygen is introduced after the reaction chamber is depressurized, and then the oxygen is controlled not to enter or exit the reaction chamber. This method is called "purging". For example, the reaction chamber is depressurized to -970 hPa, and then oxygen is introduced until 50 hPa to stop the oxygen from entering or exiting. Sometimes this state is recorded as a state where the reaction chamber is filled with oxygen.
[0087] Cooling after heating can be performed by natural cooling, and the time from the specified temperature to room temperature is preferably in the range of 10 hours to 50 hours. Note that it is not necessary to cool to room temperature, as long as it is cooled to a temperature allowed by the next step.
[0088] The heating in this process can also be performed by using a rotary kiln or a roller kiln. The rotary kiln is a rotary roasting device that can heat the raw materials while stirring them, so it is preferred. The roller kiln is a roasting device that uses rollers to convey the raw materials, and the raw materials can continuously pass through the heating area and the cooling area, so it is preferred. Of course, the heating in this process can also be performed using a batch roasting device.
[0089] When heating, the container (specifically, a container called a crucible or a sagger) for holding the mixed material is preferably made of a material with high heat resistance such as alumina, mullite-cordierite, magnesia, zirconium oxide, etc. In addition, when heating, it is preferred to cover the crucible or the sagger with a lid to prevent the sublimation of the raw materials, etc.
[0090] After heating, the mixed material can also be moved from the crucible or the sagger to a mortar, then ground and recycled. In addition, the mortar is preferably made of a heat-resistant material such as aluminum oxide, mullite-cordierite, magnesium oxide, zirconium oxide, etc. In addition, the same heating conditions as step S13 can also be adopted in the heating process described later other than step S13.
[0091] After heating, the recovered mixture sometimes aggregates. In order to eliminate the aggregated state, the recovered mixture may also be ground. In order to further eliminate the aggregated state, the recovered mixture may also be screened. Screening may be performed after grinding, while grinding, or without grinding and only screening.
[0092] <Step S14> Through the above process, Figure 2A In step S14 shown, a composite oxide (LiMO2) containing lithium and a transition metal M is obtained. The composite oxide is represented by LiMO2, but its composition is not strictly limited to Li:M:O=1:1:2. In addition, when cobalt is used as the transition metal M, the composite oxide is called a composite oxide containing cobalt and is represented by LiCoO2, but its composition is not strictly limited to Li:Co:O=1:1:2.
[0093] Although an example in which the composite oxide is produced by a solid phase method as shown in steps S11 to S14 is shown, the composite oxide may also be produced by a coprecipitation method or a hydrothermal method.
[0094] <Step S15> Then, as Figure 2A In step S15, the composite oxide is heated. This heating is the first heating of the composite oxide, so the heating in step S15 can be called initial heating. Alternatively, this heating is performed before step S20 shown below, and is sometimes called preheating treatment or pretreatment.
[0095] The heating temperature of step S15 is preferably 500°C to 1000°C, more preferably 500°C to 950°C, and further preferably 500°C to 900°C. In addition, it is preferably 700°C to 1000°C, more preferably 700°C to 950°C, and further preferably 700°C to 900°C. In addition, it is preferably 800°C to 1000°C, more preferably 800°C to 950°C, and further preferably 800°C to 900°C. In addition, the heating temperature of step S15 is preferably lower than that of step S13.
[0096] By initial heating, lithium is sometimes separated from a part of the composite oxide. In addition, the effect of improving the crystallinity of the composite oxide can be expected. In addition, the Li source and / or M source prepared in step S11 etc. is sometimes mixed with impurities, but by performing initial heating, the impurities in the composite oxide can be reduced.
[0097] After the initial heating, the surface of the composite oxide is also smoothed. The surface smoothness of the composite oxide means that the composite oxide has fewer irregularities and is curved as a whole, and the corners are curved. In addition, sometimes the state where there are fewer foreign substances attached to the surface is called "smooth".
[0098] In the above-mentioned initial heating, it is not necessary to prepare raw materials such as a Li source. Alternatively, it is not necessary to prepare a material used as a flux (added to promote melting, also called a flux).
[0099] When the heating time of this step is too short, the full effect cannot be obtained, but when the heating time is too long, the productivity decreases. For example, it can be implemented by selecting from the heating conditions described in step S13. Supplementary explanation of the heating conditions: In order to maintain the crystal structure of the composite oxide, the heating temperature of this step is preferably lower than the temperature of step S13. In addition, in order to maintain the crystal structure of the composite oxide, the heating time of this step is preferably shorter than the heating time of step S13. For example, it is preferred to heat at a temperature of 700°C or more and 1000°C or less for 2 hours or more and 20 hours or less.
[0100] In addition, as the effect of improving the crystallinity of the composite oxide, for example, the distortion caused by the difference in shrinkage due to heating of the composite oxide is alleviated, the deviation caused by the difference in shrinkage is alleviated, and the like are mentioned.
[0101] In the above-mentioned composite oxide, a temperature difference sometimes occurs between the surface and the inside of the composite oxide due to the heating in step S13. Sometimes the temperature difference causes a shrinkage difference. It can also be considered that the shrinkage difference occurs because the fluidity between the surface and the inside is different according to the temperature difference. The energy associated with the shrinkage difference brings a difference in internal stress to the composite oxide, which causes distortion. The above energy is sometimes referred to as distortion energy. It can be considered that the internal stress is removed by the initial heating in step S15, in other words, the distortion energy is reduced by the initial heating in step S15. When the distortion energy is reduced, the distortion of the composite oxide is relaxed. Therefore, through step S15, the surface of the composite oxide may become smooth. In other words, it can be considered that the shrinkage difference generated in the composite oxide through step S15 is relaxed, so that the surface of the composite oxide becomes smooth. Step S15 can also be called tempering or annealing of the composite oxide.
[0102] In addition, the shrinkage difference sometimes leads to the generation of small deviations in the above-mentioned composite oxide, such as the generation of deviations of the crystal plane. In order to reduce this deviation, it is preferred to perform this process. Through this process, the deviation of the above-mentioned composite oxide can be reduced. When the deviation is uniformized, the surface of the composite oxide may become smooth. It can also be said that the crystal particles are arranged. In other words, it can be considered that: through step S15, the deviation of the crystals etc. generated in the composite oxide is alleviated, so that the surface of the composite oxide becomes smooth.
[0103] When the surface concavoconvex information is quantified based on the measurement data on a cross section of the composite oxide, it can be said that the surface smoothness of the composite oxide is a state having a surface roughness of at least 10 nm or less. A cross section is, for example, a cross section obtained by observation using a scanning transmission electron microscope (STEM).
[0104] By using a composite oxide having a smooth surface as a positive electrode active material, deterioration during charge and discharge as a lithium ion battery is reduced, and cracking of the positive electrode active material can be prevented.
[0105] In step S14, a pre-synthesized composite oxide containing lithium and transition metal M may be used. In this case, steps S11 to S13 may be omitted. By performing step S15 on the pre-synthesized composite oxide, a composite oxide having a smooth surface may be obtained.
[0106] It is considered that the lithium content of the composite oxide may be reduced by the initial heating. Since the lithium content is reduced, it is possible that the additive element described in the next step S20_1 etc. may easily enter the composite oxide. In addition, when the additive element is added to the composite oxide with a smooth surface, the additive element can be added uniformly, so it is preferable to add the additive element after the initial heating. Figure 2B Describes the steps to add an element.
[0107] <Step S20_1> and <Step S21_1> Figure 2B Show Figure 2A The details of step S20_1 are shown in FIG. Figure 2B In step S21_1, a source of an additional element A1 (A1 source) to be added to the composite oxide is prepared. In order to replenish lithium lost due to initial heating, a lithium source may be prepared in addition to the source of the additional element A1.
[0108] As the additive element A1, one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron and arsenic can be used.
[0109] When magnesium is selected as the additive element A1, the source of the additive element A1 may be referred to as a magnesium source (Mg source). As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. may be used. In addition, a plurality of the above magnesium sources may be used.
[0110] When fluorine is selected as the additive element A1, the source of the additive element A1 can be called a fluorine source (F source). As the fluorine source, for example, lithium fluoride, magnesium fluoride, aluminum fluoride, titanium fluoride, cobalt fluoride, nickel fluoride, zirconium fluoride, vanadium fluoride, manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride, calcium fluoride, sodium fluoride, potassium fluoride, barium fluoride, cerium fluoride, lanthanum fluoride or sodium aluminum hexafluoride can be used. Among them, lithium fluoride has a relatively low melting point of 848°C and is easily melted in the heating process described later, so it is preferred. Note that Figure 2B An example in which a Mg source and a F source are used as a source of the additive element A1 is shown.
[0111] Magnesium fluoride can be used as both a fluorine source and a magnesium source. In addition, lithium fluoride can also be used as a lithium source. As another lithium source used in step S21_1, lithium carbonate can be cited.
[0112] In the present embodiment, lithium fluoride is prepared as a fluorine source, and magnesium fluoride is prepared as a fluorine source and a magnesium source. When lithium fluoride and magnesium fluoride are mixed at a molar ratio of about LiF:MgF2=65:35, it is most effective in lowering the melting point. When there is more lithium fluoride, the amount of lithium becomes too much and may cause the cycle characteristics to deteriorate. For this reason, in the present embodiment, the molar ratio of lithium fluoride and magnesium fluoride is preferably LiF:MgF2=x:1 (0≤x≤1.9), more preferably LiF:MgF2=x:1 (0.1≤x≤0.5), and further preferably LiF:MgF2=x:1 (x=0.33 or its vicinity). Note that "near" refers to a value greater than 0.9 times and less than 1.1 times its value.
[0113] At the same time, preferably the amount of magnesium added is LiMO2 of step S14, typically LiCoO2, the number of Co atoms is higher than 0.1 atom% and is less than 3 atom%, more preferably more than 0.5 atom% and less than 2 atom%, and further preferably more than 0.5 atom% and less than 1 atom%. When the amount of magnesium added is less than 0.1 atom%, the initial discharge capacity is large, but the discharge capacity is likely to decrease sharply with repeated high-voltage charging. When the amount of magnesium added exceeds 0.1 atom% (i.e., higher than 0.1 atom%) and is less than 3 atom%, even if repeated high-voltage charging is performed, the initial discharge characteristics and charge-discharge cycle characteristics are also good. On the other hand, when the amount of magnesium added exceeds 3 atom%, there is a tendency that the initial discharge capacity is lower and the charge-discharge cycle characteristics are also gradually reduced.
[0114] <Step S22_1> Then, in Figure 2B In step S22_1 shown, the magnesium source and the fluorine source are pulverized and mixed at the same time. This step can be implemented by selecting the pulverization and mixing conditions explained in step S12.
[0115] Here, a heating process may be performed after step S22_1 as needed. The heating process at this time can be performed by selecting the heating conditions described in step S13. The heating time is preferably 2 hours or more, and the heating temperature is preferably 800° C. or more and 1100° C. or less.
[0116] <Step S23_1> Then, in Figure 2B In step S23_1, the crushed and mixed materials can be recovered to obtain the additive element A1 source (A1 source). In addition, the additive element A1 source shown in step S23_1 sometimes includes multiple raw materials such as Mg source and F source, and the A1 source can be called a mixture.
[0117] The median particle size (D50) of the particle size of the above mixture is preferably 600 nm or more and 20 μm or less, more preferably 1 μm or more and 10 μm or less. The median particle size (D50) when using one material as the source of the added element A1 is also preferably 600 nm or more and 20 μm or less, more preferably 1 μm or more and 10 μm or less.
[0118] When using a mixture having the above-mentioned median particle size (D50) (including the case where the added element A1 is one), it is easy to uniformly adhere the mixture to the surface of the composite oxide when mixed with the composite oxide in the subsequent process. When the mixture is uniformly attached to the surface of the composite oxide, it is easy to evenly distribute or diffuse fluorine and / or magnesium to the surface portion of the composite oxide after heating, so it is preferred. The area where fluorine and / or magnesium are distributed can also be referred to as the surface portion. When there is an area in the surface portion that does not contain fluorine and / or magnesium, it is sometimes not easy to become the O3' type crystal structure described later in the charged state. Note that fluorine is used for illustration, but chlorine can also be used instead of fluorine, and can be referred to as a halogen as a substance containing the above elements.
[0119] <Step S31> Then, in Figure 2A In step S31, the composite oxide and the additive element A1 source (A1 source) are mixed. The number of atoms of the transition metal M in the composite oxide containing lithium and the transition metal M is A M The number of atoms A of magnesium in the added element A1 Mg The ratio is preferably A M : A Mg =100:y(0.1≤y≤6), more preferably A M : A Mg =100:y(0.3≤y≤3).
[0120] In order not to damage the composite oxide, the mixing in step S31 is preferably performed under milder conditions than the conditions of the crushing and mixing in step S12. For example, it is preferably performed under conditions with a smaller number of rotations or a shorter time than the mixing in step S12. In addition, the dry method is a milder condition than the wet method, so it is preferred.
[0121] The mixing is preferably performed in an atmosphere having a dew point of -100° C. or higher and -10° C. or lower. For example, the mixing can be performed in a dry room. The atmosphere of the dry room preferably includes dry air.
[0122] <Step S32> Then, in Figure 2A In step S32, the mixed materials are recovered to obtain a mixture 903. When recovered, the mixture 903 may be ground to eliminate the aggregated state. In order to further eliminate the aggregated state, the mixture 903 may be screened. Screening may be performed after grinding, while grinding, or without grinding.
[0123] Note that in this embodiment, a method of adding lithium fluoride used as a fluorine source and magnesium fluoride used as a magnesium source to a composite oxide after initial heating is described, but the present invention is not limited to the above method. At the stage of step S11, that is, the stage of the starting material of the composite oxide, a magnesium source and a fluorine source can be prepared together with a Li source and an M source to enter step S12. Then, heating can be performed in step S13 to obtain LiMO2 added with magnesium and fluorine. In this case, it is not necessary to divide the process into steps S11 to S14 and the process from step S21_1 to step S23_1. It can be said that the above method is a simple method with high productivity.
[0124] In addition, a composite oxide to which magnesium and fluorine are added in advance may also be used. When a composite oxide to which magnesium and fluorine are added is used, the processes of step S11 to step S32 and step S20_1 may be omitted. It can be said that the above method is a simple method with high productivity.
[0125] Alternatively, a magnesium source and a fluorine source may be further added to the composite oxide to which magnesium and fluorine have been added in advance according to step S20_1. Alternatively, a nickel source and an aluminum source may be added instead of or in addition to the magnesium source and the fluorine source.
[0126] <Step S33> Then, in Figure 2A In step S33 shown, the mixture 903 is heated. The heating conditions can be selected from those described in step S13. The heating time is preferably 2 hours or more.
[0127] Here, the heating temperature is supplemented. The lower limit of the heating temperature in step S33 needs to be above the temperature at which the reaction of the composite oxide (LiMO2) and the source of the added element A1 progresses. The temperature at which the reaction progresses can be a temperature at which mutual diffusion of the elements contained in the composite oxide and the source of the added element A1 can occur, and it can also be lower than the melting point of the above materials. Taking oxides as an example, it is known that from the Tammann temperature T d (As the melting point of the oxide T m Solid phase diffusion begins at a temperature obtained by multiplying the temperature by 0.757 times of . Therefore, the heating temperature in step S33 may be 500° C. or higher.
[0128] Of course, the reaction is more likely to proceed when the heating temperature is above the temperature at which at least a portion of the mixture 903 is melted. For example, when LiF and MgF2 are included as the additive element A1 source, the eutectic point of LiF and MgF2 is around 742°C, so the lower limit of the heating temperature in step S33 is preferably set to 742°C or above.
[0129] In addition, a mixture 903 obtained by mixing LiCoO2:LiF:MgF2=100:0.33:1 (molar ratio) observed an endothermic peak at around 830° C. in differential scanning calorimetry (DSC measurement). Therefore, the lower limit of the heating temperature is more preferably set to 830° C. or more.
[0130] A higher heating temperature is preferred because the reaction proceeds more easily, the heating time is shortened, and the productivity is improved.
[0131] The upper limit of the heating temperature is lower than the decomposition temperature of the composite oxide. For example, in the case of LiCoO2, the upper limit of the heating temperature is lower than the decomposition temperature of 1130°C. At a temperature near the decomposition temperature, a slight decomposition of LiMO2 may occur. When decomposition of LiMO2 occurs, sometimes unwanted reaction products are generated in the composite oxide, such as Co3O4 in lithium cobalt oxide, so it is not preferred. Therefore, the upper limit of the heating temperature is preferably below 1000°C, more preferably below 950°C, and further preferably below 920°C.
[0132] In summary, the heating temperature in step S33 is preferably 500°C or higher and lower than 1130°C, more preferably 500°C or higher and lower than 1000°C, further preferably 500°C or higher and lower than 950°C, further preferably 500°C or higher and lower than 920°C, and further preferably 500°C or higher and lower than 900°C. In addition, it is preferably 742°C or higher and lower than 1130°C, more preferably 742°C or higher and lower than 1000°C, further preferably 742°C or higher and lower than 950°C, further preferably 742°C or higher and lower than 920°C, and further preferably 742°C or higher and lower than 900°C. In addition, it is preferably 800°C or higher and lower than 1130°C, more preferably 800°C or higher and lower than 1000°C, further preferably 800°C or higher and lower than 950°C, further preferably 800°C or higher and lower than 920°C, and further preferably 800°C or higher and lower than 900°C. In addition, it is preferably 830°C or higher and lower than 1130°C, more preferably 830°C or higher and 1000°C or lower, further preferably 830°C or higher and 950°C or lower, further preferably 830°C or higher and 920°C or lower, and still further preferably 830°C or higher and 900°C or lower.
[0133] In addition, the heating temperature of step S33 is preferably lower than the heating temperature of step S13. This is to prevent the composite oxide (LiMO2) from decomposing. In addition, the heating temperature of step S33 is preferably higher than the heating temperature of step S15.
[0134] In addition, when heating the mixture 903, it is preferred to control the partial pressure of fluorine or fluoride caused by the fluorine source in the processing chamber or crucible to be within an appropriate range. In the manufacturing method described in this embodiment, sometimes a part of the material such as LiF as a fluorine source is used as a flux. Through the above-mentioned function, the heating temperature can be reduced to a temperature lower than the decomposition temperature of the composite oxide (LiMO2), for example, above 742°C and below 950°C, and the added element A1 such as magnesium can be distributed in the surface layer, thereby manufacturing a positive electrode active material with good characteristics.
[0135] However, LiF may sublimate by heating, and the specific gravity of LiF in the gas state is lighter than that of oxygen, so it can be considered that the LiF in the mixture 903 is reduced. At this time, the function of LiF as a flux is reduced. Therefore, it is necessary to suppress the sublimation of LiF while heating. In addition, even if LiF is not used as a fluorine source, it is possible that Li on the surface of LiMO2 reacts with F in the fluorine source to generate LiF and the LiF is sublimated. Therefore, even if a fluoride having a higher melting point than LiF is used, it is also necessary to suppress sublimation.
[0136] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF in the processing chamber is high. By the above heating, it is possible to suppress the sublimation of LiF in the mixture 903. In addition, by covering the container with a lid as described above, it is possible to suppress the sublimation of LiF in the mixture 903.
[0137] The heating in this step is preferably performed in a manner that does not cause the mixture 903 to adhere together. When the mixture 903 adheres together during heating, the area of the mixture 903 in contact with oxygen in the atmosphere is reduced, and the diffusion path of the added element A1 (such as magnesium and / or fluorine) is blocked, thereby possibly preventing the added element A1 (such as magnesium and / or fluorine) from diffusing easily.
[0138] In addition, it is considered that when the added element A1 (such as fluorine) is evenly distributed in the surface layer, a smooth and less uneven positive electrode active material can be obtained. Therefore, in order to maintain the smooth state of the surface heated by step S15 or further smoothen it in this process, it is preferred not to make the mixture 903 bonded together.
[0139] Supplementary description of the heating time. The heating time varies according to the conditions such as the heating temperature, the size and composition of the LiMO2 in step S14. When the median particle size (D50) of LiMO2 is small, it is sometimes preferred to heat at a lower temperature or for a shorter time than when the median particle size (D50) is large. The median particle size (D50) can be obtained by a laser diffraction particle size distribution measuring device.
[0140] In being Figure 2AIn the case where lithium cobalt oxide is used for the LiMO2 in step S14, when the median particle size (D50) of the lithium cobalt oxide is about 12 μm (above 10 μm and below 14 μm), the heating temperature of step S33 is preferably, for example, above 800°C and below 920°C, and more preferably above 850°C and below 920°C. The heating time of step S33 is, for example, preferably above 10 hours, more preferably above 20 hours, and may also be above 60 hours. When the median particle size (D50) is large, the volume of the composite oxide (LiMO2) becomes larger, so sometimes a longer heating time is required to relax or remove the internal stress in the block layer of the composite oxide. When the median particle size (D50) is large, it takes time for the added element A1 such as magnesium to be evenly distributed in the surface layer, so as described above, the heating time sometimes becomes longer. The median particle size (D50) of lithium cobalt oxide may become larger after heat treatment, but the median particle size (D50) after heat treatment is preferably greater than 10 μm and less than 14 μm. In other words, the median particle size (D50) of the positive electrode active material is preferably greater than 10 μm and less than 14 μm.
[0141] In the case where lithium cobalt oxide is used as LiMO2 in step S14, when the median particle size (D50) of the lithium cobalt oxide is about 7 μm (5 μm or more and 9 μm or less), the heating temperature of step S33 is preferably within the same range as the heating temperature when the median particle size (D50) is about 12 μm. On the other hand, the heating time of step S33 can be shorter than the heating time when the median particle size (D50) is about 12 μm. The heating time is, for example, preferably more than 1 hour and less than 10 hours, more preferably more than 5 hours and less than 10 hours. When the median particle size (D50) is small, the time that added elements A1 such as magnesium are distributed in the surface portion becomes shorter, so the heating time can be shortened as described above. When the median particle size (D50) is small, the volume of the composite oxide (LiMO2) becomes smaller, so the time required for tempering or annealing of the bulk layer of the composite oxide can be shortened. The median particle size (D50) of lithium cobalt oxide may increase after heat treatment, but the median particle size (D50) after heat treatment is preferably 5 μm or more and 9 μm or less. That is, the median particle size (D50) of the positive electrode active material is preferably 5 μm or more and 9 μm or less.
[0142] It is preferable to provide a step of further adding an additional element different from the additional element A1 after step S33. Figure 2C Describe the step.
[0143] <Step S20_2> and <Step S21_2> Figure 2C Show Figure 2A The details of step S20_2 are shown in FIG. Figure 2CIn step S21_2, a source of an additional element A2 (A2 source) to be added to the composite oxide is prepared. In addition to the source of the additional element A2, a lithium source may also be prepared.
[0144] As the additive element A2, one or more selected from the group consisting of nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron and arsenic can be used. The additive element A2 preferably uses at least an element not selected as the additive element A1, but may also contain an element selected as the additive element A1. Figure 2C An example is shown in which a Ni source and an Al source are used as the source of the additional element A2.
[0145] In this embodiment, nickel hydroxide is prepared as a nickel source, and aluminum hydroxide is prepared as an aluminum source. Alternatively, nickel oxide or nickel carbonate may be used instead of nickel hydroxide. Alternatively, aluminum oxide or aluminum carbonate may be used instead of aluminum hydroxide.
[0146] <Step S22_2> Then, in Figure 2C In step S22_2 shown in FIG. 1 , the nickel source is mixed while being crushed, and the aluminum source is mixed while being crushed. This process can be implemented by selecting the crushing conditions and mixing conditions described in step S12. In addition, in this process, it is also possible to Figure 2B As in step S22_1, the nickel source and the aluminum source are combined together and then crushed and mixed.
[0147] Here, a heating process may be performed after step S22_2 as needed. The heating process at this time may be performed by selecting from the heating conditions described in step S13.
[0148] <Step S23_2> Then, in Figure 2C In step S23_2 shown, the above-mentioned crushed or mixed materials can be recovered to obtain the added element A2 source (A2 source).
[0149] <Step S34> Then, in Figure 2A In step S34 shown, the composite oxide heated in step S33 and the additive element A2 source (A2 source) are mixed. As described above, a plurality of additive element A2 sources (A2 sources) may be prepared. The number of atoms A of the transition metal M in the composite oxide is M The number of atoms A of nickel in the added element A2 Ni The ratio is preferably A M : A Ni =100:y(0.1≤y≤3), more preferably A M : A Ni=100:y (0.3≤y≤1). In addition, the number of atoms A of the transition metal M in the composite oxide is M The number of atoms A of aluminum in the added element A2 Al The ratio is preferably A M : A Al =100:y(0.1≤y≤3), more preferably A M : A Al =100:y(0.3≤y≤1).
[0150] The mixing conditions of step S34 can be selected from the mixing conditions described in step S31.
[0151] <Step S35> Then, in Figure 2A In step S35, the mixed materials are recovered to obtain a mixture 904. When recovered, the mixture 904 may be ground to eliminate the aggregated state. In order to further eliminate the aggregated state, the mixture 904 may be screened. Screening may be performed after grinding, while grinding, or without grinding.
[0152] <Step S36> Then, in Figure 2A In step S36 shown, the mixture 904 is heated. The heating conditions can be selected from those described in step S33. The heating time is preferably 2 hours or more.
[0153] As for the heating temperature of step S36, similarly to step S33, it is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, further preferably 500°C or higher and 950°C or lower, and further preferably 500°C or higher and 900°C or lower. In addition, it is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, further preferably 742°C or higher and 950°C or lower, and further preferably 742°C or higher and 900°C or lower. In addition, it is preferably 800°C or higher and 1100°C or lower, more preferably 830°C or higher and 1130°C or lower, further preferably 830°C or higher and 1000°C or lower, further preferably 830°C or higher and 950°C or lower, and further preferably 830°C or higher and 900°C or lower. In addition, the heating temperature of step S36 is preferably lower than the heating temperature of step S13. In addition, the heating temperature in step S36 is preferably lower than the heating temperature in step S33.
[0154] The heating in this step is preferably performed in a manner that does not cause the mixture 904 to stick together. When the mixture 904 sticks together during heating, the contact area with oxygen in the atmosphere is reduced, and the diffusion path of the additive element A2 is blocked, thereby possibly making it difficult for the additive element A2 to be distributed.
[0155] <Step S37> Then, in Figure 2A In step S37 shown, the heated material is recovered and ground as needed to obtain the positive electrode active material 10. At this time, it is preferred that the recovered positive electrode active material 10 is also screened. Through the above steps, the positive electrode active material 10 of one embodiment of the present invention can be manufactured. The surface of the positive electrode active material of one embodiment of the present invention is smooth. The above is an example of a method for manufacturing a positive electrode active material.
[0156] [Positive electrode active material] Reference Figure 3A A cross section of the positive electrode active material 10 obtained by the above-mentioned manufacturing method is described. Figure 3A different, Figure 3B A cross section of the positive electrode active material 10 is shown, in which the grain boundary 15 is indicated by a dashed line. Figure 3A and Figure 3B The positive electrode active material 10 shown includes a surface portion 10a and an inner portion (the inner portion is referred to as a "bulk portion") 10b, and the boundary between them is indicated by a dotted line. The surface portion 10a preferably covers more than 90% of the bulk portion 10b. Note that Figure 3A and Figure 3B The dashed line in is an example. Figure 3B The dot-dash line in FIG. 1 is an example, and the ratio of covering the surface layer portion is also an example.
[0157] The surface layer portion 10a may not cover the entire block portion 10b. Figure 3A and Figure 3B The positive electrode active material 10 is shown, wherein the surface layer portion 10a covers 50% or more of the outer periphery of the bulk portion 10b, specifically 65% or more and 75% or less. Figure 3B As shown, the positive electrode active material 10 may have a region where the bulk portion 10 b is exposed.
[0158] Figure 3BThe grain boundary 15 shown, for example, refers to the part where the positive electrode active material 10 is bonded together, the part where the crystal orientation changes inside the positive electrode active material 10, that is, the repeated discontinuous part of the bright line and the dark line in the STEM image, the part containing multiple crystal defects, or the part with a disordered crystal structure. Crystal defects refer to defects that can be observed through cross-sectional TEM (transmission electron microscope) images, cross-sectional STEM images, etc., and the defects can also be referred to as structures or voids between other elements entering the lattice. In other words, the grain boundary 15 can be said to be one of the surface defects. In addition, the vicinity of the grain boundary 15 refers to an area within 20nm, preferably within 10nm, centered on the grain boundary 15, and the vicinity of the grain boundary exists inside the particle and outside the particle. It can be distinguished by referring to it as the vicinity of the grain boundary on one side of the inside of the particle or the vicinity of the grain boundary on the outside of the particle.
[0159] The positive electrode active material 10 includes a composite compound containing transition metal and oxygen in which lithium can be embedded and released, so the interface between the region where the transition metal M (for example, Co, Ni, Mn, Fe, etc.) that is oxidized and reduced with the embedding and release of lithium and the region where the transition metal M is not present can be called the "surface" of the positive electrode active material. Additive elements sometimes exist in the region where the transition metal M is not present. Sometimes, the surface generated by sliding, cracks and / or fissures can also be called the surface of the positive electrode active material.
[0160] As described above, in this specification, etc., the surface portion 10a refers to, for example, an area within 50 nm from the surface to the inside, more preferably within 35 nm, further preferably within 20 nm, and most preferably within 10 nm. Alternatively, the surface portion may also be referred to as the vicinity of the surface, the area near the surface, or the shell. Note that the area within 50 nm from the surface to the inside, more preferably within 35 nm, further preferably within 20 nm, and most preferably within 10 nm refers to the distance in the depth direction perpendicular to or approximately perpendicular to the surface. Perpendicular or approximately perpendicular to the surface refers to a direction in which the angle formed with the tangent to the surface is greater than 80° and less than 100°. In addition, the bulk portion 10b refers to an area deeper than the surface portion 10a. The bulk portion 10b is sometimes referred to as the inside, and may also be referred to as the core. The bulk portion 10b sometimes includes the central portion of the positive electrode active material.
[0161] In the positive electrode active material 10, the region where lithium is inserted and released may also be referred to as the "surface". Therefore, the "surface" may be regarded as the region in contact with the electrolyte in the positive electrode active material 10. For example, the surface of the positive electrode active material 10 may include the surface of the surface layer portion 10a, and the bulk portion 10b may become the surface in the region where the bulk portion 10b is exposed.
[0162] It can be considered that the carbonate groups or hydroxyl groups chemically adsorbed on the positive electrode active material 10 after manufacturing are areas where lithium cannot be inserted or removed, and they do not constitute the surface of the positive electrode active material 10. Similarly, the electrolyte, binder, conductive material or compounds derived from them attached to the positive electrode active material 10 do not constitute the surface of the positive electrode active material 10.
[0163] In addition, the "surface" of the positive electrode active material 10 in a cross-sectional STEM (scanning transmission electron microscope) image or the like refers to the boundary between the region where the coupled image of the electron beam is observed and the region where the coupled image is not observed, and can be the outermost side of the region where the bright spot of the nucleus of the metal element having an atomic number greater than lithium is confirmed. The surface in a cross-sectional STEM image or the like can also be determined based on an analysis with a higher spatial resolution, such as an analysis result of an electron energy loss spectrum (EELS).
[0164] In order to keep the charge neutral during the insertion and removal of lithium ions, the positive electrode active material needs to contain a transition metal that can be oxidized and reduced. In the positive electrode active material 10 of one embodiment of the present invention, cobalt is mainly used as the transition metal M that causes the redox reaction, but in addition to cobalt, at least one or two or more selected from nickel and manganese can also be used. In the transition metal M contained in the positive electrode active material 10, cobalt preferably accounts for more than 75 atomic%, more preferably more than 90 atomic%, and further preferably more than 95 atomic%. At this time, there are many advantages such as: it can be synthesized more easily: easy to handle: has good cycle characteristics; etc.
[0165] When 33 atomic % or more, preferably 60 atomic % or more, and more preferably 80 atomic % or more of nickel is used as the transition metal M contained in the positive electrode active material 10, the raw material is sometimes cheaper than when the cobalt content is higher, and the discharge capacity per unit weight is sometimes improved, so it is preferred.
[0166] As described above, as the added element A (added element A1 and added element A2) contained in the positive electrode active material 10, it is preferred to use one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron and arsenic.
[0167] That is, it can be said that the positive electrode active material 10 is lithium cobalt oxide to which the additional element A is added. As described later, by adding the element A, the crystal structure of the positive electrode active material 10 can be further stabilized.
[0168] The additive element A does not necessarily include one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron and arsenic.
[0169] For example, by manufacturing a positive electrode active material 10 that does not substantially contain manganese as an added element A, the above advantages such as: relatively easy synthesis; easy handling; good cycle characteristics; etc. can be improved. The weight of manganese contained in the positive electrode active material 10 is preferably 600 ppm or less, and more preferably 100 ppm or less. The weight of manganese can be analyzed, for example, using a glow discharge mass spectrometry analyzer (GD-MS).
[0170] <Crystal Structure> use Figure 4 8 compares a conventional positive electrode active material with a positive electrode active material 10 that can be used in one embodiment of the present invention to illustrate the Li x The change of x in CoO2 changes the crystal structure. Figure 4 The crystal structure of the positive electrode active material 10 that can be used in one embodiment of the present invention is shown. Figure 5 The crystal structure of a conventional positive electrode active material is shown. Figure 5 The existing positive electrode active material shown is lithium cobalt oxide (LiCoO2) that does not contain an added element. Note that in this specification, "does not contain an added element" refers to a situation below the detection limit when measuring using an analysis unit or a situation in a range that does not affect the presence or absence of an effect even if the detection limit is included.
[0171] < <Li x When x is 1 in CoO2 >> Preferably, the positive electrode active material 10 that can be used in one embodiment of the present invention is in a discharged state, that is, in a Li x When x=1 in CoO2, it has a layered rock salt type crystal structure belonging to the space group R-3m. In this crystal structure, lithium occupies an octahedral position and includes three CoO2 layers in the unit cell. Therefore, this crystal structure is sometimes called an O3 type crystal structure. Note that the CoO2 layer refers to a structure in which an octahedral structure in which cobalt is coordinated to six oxygens is continuous on a plane in a state of edge sharing. The CoO2 layer is sometimes referred to as a layer composed of octahedra of cobalt and oxygen. Figure 4 In, Li x The crystal structure of CoO2 when x is 1 is represented by R-3m(O3). Figure 5 In, Li x The crystal structure of CoO2 when x is 1 is similar to Figure 4 The crystal structures shown are the same and are also represented by R-3m(O3).
[0172] The layered rock salt type composite oxide has a high discharge capacity and a two-dimensional lithium ion diffusion path, which is suitable for the insertion and extraction reaction of lithium ions, and is very good as a positive electrode active material for lithium ion batteries. Therefore, the bulk portion 10b that occupies most of the positive electrode active material 10 preferably has a layered rock salt type crystal structure.
[0173] The crystal structure of the surface portion 10a of the positive electrode active material 10 that can be used in one embodiment of the present invention may not be a layered rock salt type crystal structure. The surface portion 10a preferably has a function of reinforcing the layered structure composed of cobalt and oxygen octahedra of the bulk portion 10b so as to avoid the collapse of the layered structure even if lithium is separated from the positive electrode active material 10 due to charging. Alternatively, the surface portion 10a is preferably used as a barrier film for the positive electrode active material 10. Alternatively, the surface portion 10a of the peripheral portion of the positive electrode active material 10 preferably reinforces the positive electrode active material 10. Here, reinforcement refers to suppressing structural changes in the surface portion 10a and the bulk portion 10b of the positive electrode active material 10 such as the separation of oxygen and / or suppressing oxidative decomposition of the electrolyte on the surface of the positive electrode active material 10.
[0174] The surface part 10a is the area where lithium ions are first separated during charging, and is also the area where the lithium concentration is easier to reduce than that of the bulk part 10b. In addition, the atoms on the surface of the positive electrode active material 10 contained in the surface part 10a are in a state where some of their bonds are cut off when lithium ions are separated. Therefore, the surface part 10a is likely to become unstable and the change of crystal structure (i.e., degradation) is likely to begin. On the other hand, as long as the surface part 10a can be made sufficiently stable, the lithium ion can be charged at a high temperature. x When x in CoO2 is small, for example, when x is less than 0.24, the layered structure of the CoO2 layer of the bulk portion 10b is not easily collapsed. In addition, the deviation of the CoO2 layer of the bulk portion 10b can be suppressed.
[0175] In order to make the surface part 10a have a stable composition and crystal structure, the surface part 10a preferably contains an additive element A, and more preferably contains a plurality of additive elements A. In addition, the concentration of one or more selected from the additive elements A in the surface part 10a is preferably higher than that in the bulk part 10b. In addition, one or more selected from the additive elements A contained in the positive electrode active material 10 preferably have a concentration gradient. In addition, it is more preferred that the distribution of the additive element A in the positive electrode active material 10 is different. For example, it is more preferred that the depth of the concentration peak of the additive element A from the surface is different. Here, the concentration peak refers to the maximum value of the concentration in the surface part 10a or the range below 50 nm from the surface.
[0176] Here, refer to FIG. 3C to FIG. 3F The schematic diagram of FIG. 1 illustrates the above-mentioned concentration gradient and concentration peak, etc.
[0177] Figure 3C and Figure 3D Show enlarged Figure 3A The diagram near AB in . Figure 3C and Figure 3D It can be said that it is a cross section of the surface portion having a (001) plane (hereinafter referred to as the (001) plane, sometimes referred to as the c-plane or basal plane), that is, a cross-sectional view of the region oriented (001). In the layered rock salt type crystal structure, cations are arranged parallel to the (001) plane. In other words, the CoO2 layer and the lithium layer are alternately stacked in parallel to the (001) plane. Therefore, the diffusion path of the lithium ions is parallel to the (001) plane. Since the CoO2 layer is relatively stable, the (001) plane on the surface of the CoO2 layer is relatively stable and the main diffusion path of the lithium ions is not exposed on the (001) plane during charge and discharge.
[0178] In the case of showing such a (001) plane Figure 3C , the distribution of magnesium and the like is shown as an example of the added element A. Figure 3C The lightness and darkness in the (001) plane correspond to the change in magnesium concentration. Since the CoO2 layer in the (001) plane is relatively stable, the additive element A may not be detected. When the additive element A is detected, as an example of the distribution of the additive element A, Figure 3C An example is shown in which the additive element A exists at the highest concentration on the surface or near the surface in the surface layer 10a and the concentration of the additive element A decreases toward the bulk portion 10b. It can be said that there is a concentration peak of magnesium or the like at the position indicating the highest concentration. In addition, the state in which the concentration gradually decreases is sometimes described as a concentration gradient. Note that in this specification, the (001) plane is presented as Figure 3C The added element A of the distribution shown is called the added element X.
[0179] exist Figure 3D , the distribution of aluminum is shown as another example of the added element A. Figure 3D The lightness and darkness in the (001) plane correspond to the change in the concentration of aluminum. Since the CoO2 layer in the (001) plane is relatively stable, the additive element A may not be detected. When the additive element A is detected, as an example of the distribution of the additive element A, Figure 3D An example is shown in which the additive element A is present at the highest concentration in the surface layer 10a at a position deeper than the surface or near the surface, and the concentration of the additive element A decreases toward the surface and the bulk portion 10b. It can be said that there is a concentration peak of aluminum at the position indicating the highest concentration, and sometimes the position of the aluminum concentration peak is different from the concentration peak position of the above-mentioned magnesium, etc. and is located at a slightly deeper position. In addition, sometimes the state in which the concentration gradually decreases is described as a concentration gradient. Note that in this specification, the (001) plane is presented as follows Figure 3D The added element A of the distribution shown is called the added element Y.
[0180] Depending on the element of the added element A, the distribution may be different, such as the distribution of the added element X or the distribution of the added element Y. In addition, depending on the element of the added element A, the concentration peak position may be different, such as the concentration peak position of the added element X or the concentration peak position of the added element Y.
[0181] Figure 3E and Figure 3F Show enlarged Figure 3A Figure near the CD in . Figure 3E and Figure 3F It can be said that it is a cross-sectional view of the surface portion having a plane other than the (001) plane (hereinafter sometimes referred to as an ab plane or an edge plane), and the plane other than the (001) plane is a plane where a diffusion path of lithium ions exists in the layered rock salt type crystal structure.
[0182] In the above-mentioned plane other than the (001) plane Figure 3E In FIG. 1 , the distribution of magnesium and the like is shown as an example of the added element X. Figure 3C Compared with the (001) surface, sometimes Figure 3E The concentration of the added element X is higher in the planes other than the (001) plane of the surface layer 10a. The concentration peak of magnesium and the like is sometimes located on the surface or near the surface of the surface layer portion 10a, and sometimes appears higher than Figure 3C The concentration peak of the (001) plane is higher in intensity. Figure 3E The added element X on the planes other than the (001) plane is distributed in a wide range.
[0183] exist Figure 3F In FIG. 1 , the distribution of aluminum and the like is shown as an example of the added element Y. It is preferred that the concentration peak of aluminum is at Figure 3D The (001) face and Figure 3F All the surfaces other than the (001) surface are located in the region of 5 nm to 50 nm from the surface to the inside. Figure 3F The aluminum concentration peak of the surface other than the (001) surface in the Figure 3D The aluminum concentration peak of the (001) plane is deeper.
[0184] In this way, the distribution of the added elements may also differ depending on the surface direction of the positive electrode active material.
[0185] As described above, the diffusion path of lithium ions exists on the surface corresponding to the surface other than the (001) surface, and the diffusion path of lithium ions is exposed on the surface corresponding to the surface other than the (001) surface. Figure 3E and Figure 3FAs shown, the surface portion 10a corresponding to the surface other than the (001) surface is an important area for maintaining the diffusion path of lithium ions, and is the area where lithium ions first leave, so it tends to be unstable. Therefore, it is preferred that in order to maintain the overall crystal structure of the positive electrode active material 10, the surface other than the (001) surface and the surface portion 10a corresponding to the surface are preferentially strengthened. In other words, it is preferred that the added element A is preferably present in the surface other than the (001) surface and the surface portion 10a corresponding to the surface.
[0186] As described in the above manufacturing method, when the manufacturing method of heating the LiCoO2 mixed with the additive element formed by the initial heating is adopted, the additive element diffuses through the diffusion path of the lithium ion. Figure 3C and Figure 3D As shown, it is easy to make the distribution of the added elements in the planes other than (001) and the surface layer portion 10a corresponding to the planes within the preferred range.
[0187] In addition, it is preferred that the surface of the positive electrode active material 10 is smooth with few irregularities, but the positive electrode active material 10 does not need to be smooth as a whole. For example, the positive electrode active material 10 may also have irregularities caused by sliding of a surface parallel to the (001) plane (for example, a surface on which lithium is arranged). Sliding is also called a stacking defect. For example, when the positive electrode is manufactured, pressing is performed, and sometimes LiCoO2 is deformed along the lattice stripe direction (ab plane direction) due to the pressing, and this deformation is also included in sliding. Deformation includes the situation where the lattice stripes deviate from each other in the front-to-back direction. When the lattice stripes deviate from each other in the front-to-back direction, steps are generated on the surface in the direction perpendicular to the lattice stripes (c-axis direction).
[0188] In addition, the surface and the surface layer portion 10a generated by sliding are mostly (001) planes, and sometimes the added element does not exist in the surface layer portion 10a corresponding to the (001) plane or the added element is below the detection limit. As described above, the (001) plane is a relatively stable plane where the diffusion path of lithium ions is not exposed, so even if the added element does not exist or the added element is below the detection limit, it basically does not cause problems.
[0189] In a layered rock salt type composite oxide whose composition is LiCoO2 and whose crystal structure belongs to R-3m, cobalt is arranged parallel to the (001) plane. In addition, in the High-Angle Annular Dark Field Scanning TEM (HAADF-STEM) image, the brightness of cobalt, which has the largest atomic number in LiCoO2, is the highest. Therefore, in the HAADF-STEM image, the arrangement of atoms with higher brightness can be regarded as the arrangement of cobalt. In addition, the repetition of the above arrangement with higher brightness can also be synonymous with crystal stripes and lattice stripes.
[0190] Next, the additive elements are described. Magnesium, one of the additive elements X, is divalent. In the layered rock salt type crystal structure, magnesium ions are more stable at the lithium position than at the cobalt position in the layered rock salt type crystal structure, and thus easily enter the lithium position. When magnesium is present at the lithium position of the surface portion 10a at an appropriate concentration, the layered rock salt type crystal structure of the bulk portion 10b, etc. is easily enhanced. This is because the magnesium present at the lithium position is used as a support between the CoO2 layers. In addition, when magnesium is present, for example in the following Li x When x in CoO2 is 0.24 or less, the oxygen around magnesium can be suppressed from being released. In addition, it can be expected that the density of the positive electrode active material 10 is improved when magnesium is present. In addition, when the magnesium concentration of the surface layer 10a is high, it can be expected that the corrosion resistance to hydrofluoric acid generated by the decomposition of the electrolyte can be improved.
[0191] If magnesium has an appropriate concentration, it has no negative impact on the insertion and removal of lithium accompanying charge and discharge, so the above advantages can be achieved. However, excess magnesium may have a negative impact on the insertion and removal of lithium. In addition, the effect of contributing to the stabilization of the crystal structure sometimes becomes smaller. This is because magnesium not only enters the lithium position but also the cobalt position. In addition, there is also the following concern: unnecessary magnesium compounds (oxides, fluorides, etc.) that are not substituted at the lithium position or the cobalt position are segregated on the surface of the positive electrode active material and become the resistance component of the lithium ion battery. In addition, the increase in the magnesium concentration of the positive electrode active material sometimes reduces the discharge capacity of the positive electrode active material. This is because excess magnesium enters the lithium position and the amount of lithium contributing to charge and discharge is reduced.
[0192] Therefore, it is preferred that an appropriate amount of magnesium is included in the positive electrode active material 10 as a whole. For example, the number of magnesium atoms is preferably greater than 0.001 times and less than 0.1 times the number of cobalt atoms, more preferably greater than 0.01 times and less than 0.04 times, and further preferably about 0.02 times. Here, the amount of magnesium in the positive electrode active material 10 as a whole can be, for example, a value obtained by analyzing all elements of the positive electrode active material 10 using GD-MS (glow discharge mass spectrometry analysis), ICP-MS (Inductively Coupled Plasma Mass Spectrometry), etc., or a value based on the mixed value of the raw materials in the manufacturing process of the positive electrode active material 10.
[0193] In addition, nickel, which is one of the added elements X, may be present at the cobalt site or the lithium site. When nickel is present at the cobalt site, the redox potential is lower than that of cobalt, thereby increasing the discharge capacity, which is preferable.
[0194] In addition, when nickel is present at the lithium position, the deviation of the layered structure composed of octahedrons of cobalt and oxygen is suppressed. In addition, the volume change caused by charging and discharging is also suppressed. In addition, the elastic modulus is increased, that is, it becomes hard. This is because the nickel present at the lithium position is also used as a support between the CoO2 layers.
[0195] On the other hand, when the amount of nickel is too large, the influence of distortion due to the Jan-Teller effect increases, which is not preferable. In addition, when the amount of nickel is too large, it may have a negative impact on the insertion and extraction of lithium.
[0196] Therefore, it is preferred that an appropriate amount of nickel is included in the positive electrode active material 10 as a whole. For example, the number of nickel atoms contained in the positive electrode active material 10 is preferably higher than 0% and lower than 7.5% of the number of cobalt atoms, more preferably greater than 0.05% and less than 4%, further preferably greater than 0.1% and less than 2%, and further preferably greater than 0.2% and less than 1%. Alternatively, it is preferably higher than 0% and less than 4%. Alternatively, it is preferably higher than 0% and less than 2%. Alternatively, it is preferably greater than 0.05% and less than 7.5%. Alternatively, it is preferably greater than 0.05% and less than 2%. Alternatively, it is preferably greater than 0.1% and less than 7.5%. Alternatively, it is preferably greater than 0.1% and less than 4%. The amount of nickel shown here can be, for example, a value obtained by elemental analysis of the positive electrode active material as a whole using GD-MS, ICP-MS, etc., or a value obtained by mixing raw materials in the manufacturing process of the positive electrode active material.
[0197] In addition, aluminum, one of the added elements Y, may exist in the cobalt position in the layered rock salt type crystal structure. Aluminum is a typical trivalent element and its valence does not change, so the lithium around aluminum is not easy to move during charge and discharge. Therefore, aluminum and the lithium around it are used as a support to suppress changes in the crystal structure. In addition, aluminum has the effect of suppressing the dissolution of surrounding cobalt and improving continuous charging tolerance. In addition, the Al-O bond is stronger than the Co-O bond, so the oxygen around aluminum can be suppressed from detaching. Through the above effects, thermal stability is improved. Therefore, the safety of using a positive electrode active material containing aluminum as an added element in a lithium ion battery can be improved. In addition, a positive electrode active material 10 that is not prone to crystal structure collapse even after repeated charge and discharge can be achieved.
[0198] In addition, aluminum, which is one of the additive elements Y, is preferably present at a position slightly deeper than the surface (specifically, the aluminum concentration peak is present in a region deeper than the concentration peak of the additive element X). Alternatively, the presence of aluminum, which is one of the additive elements Y, is preferably confirmed in a region deeper than the deepest position where the presence of the additive element X is confirmed. This is because lithium present near the aluminum site substituted by the lithium site is fixed, so if aluminum is substituted by the lithium site on the surface, the diffusion path of lithium may be blocked.
[0199] On the other hand, when the amount of aluminum is too much, it sometimes has a negative impact on the insertion and extraction of lithium. Therefore, it is preferred that an appropriate amount of aluminum is included in the positive electrode active material 10 as a whole. For example, the number of aluminum atoms contained in the positive electrode active material 10 as a whole is preferably greater than 0.05% and less than 4% of the number of cobalt atoms, more preferably greater than 0.1% and less than 2%, and further preferably greater than 0.3% and less than 1.5%. Alternatively, it is preferably greater than 0.05% and less than 2%. Alternatively, it is preferably greater than 0.1% and less than 4%. The amount contained in the positive electrode active material 10 as a whole shown here can be, for example, a value obtained by elemental analysis of the positive electrode active material 10 as a whole using GD-MS, ICP-MS, etc., or a value obtained by mixing raw materials in the manufacturing process of the positive electrode active material 10.
[0200] In addition, fluorine, one of the added elements X, is a monovalent anion, and when part of the oxygen in the surface portion 10a is replaced by fluorine, the lithium detachment energy is reduced. This is because the valence change of the cobalt ion accompanying the detachment of lithium varies according to the presence or absence of fluorine, for example, from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine, and the redox potential is different. Therefore, when part of the oxygen in the surface portion 10a of the positive electrode active material 10 is replaced by fluorine, it can be said that the detachment and embedding of lithium ions near fluorine occur smoothly. Therefore, the charge and discharge characteristics, current characteristics, etc. can be improved when the positive electrode active material 10 is used in a lithium ion battery. In addition, by having fluorine in the surface portion 10a of the surface including the portion in contact with the electrolyte, the corrosion resistance to hydrofluoric acid can be effectively improved. In addition, as shown in the following embodiment, when the melting point of fluorides such as lithium fluoride is lower than the melting point of other added element sources, it can be used as a flux (also known as a solubility aid) to reduce the melting point of other added element sources.
[0201] In addition, when the surface layer 10a contains both magnesium and nickel, it is possible that divalent magnesium exists more stably near divalent nickel. x When x in CoO2 is small, the dissolution of magnesium is suppressed. Thus, magnesium and nickel contribute to the stabilization of the surface layer portion 10a.
[0202] In addition, when different additive elements such as additive element X and additive element Y are used at the same time, the crystal structure of a wider area can be stabilized, so it is preferred. For example, when the positive electrode active material 10 contains magnesium and nickel as additive element X and aluminum as additive element Y at the same time, the crystal structure of a wider area can be stabilized compared to the case where only one of the additive element X and the additive element Y is included. In this way, when the positive electrode active material 10 contains additive element X and additive element Y at the same time, the additive element X such as magnesium can fully stabilize the surface, so the additive element Y such as aluminum is not required on the surface. On the contrary, aluminum is preferably widely distributed in a deeper area, such as an area with a depth of more than 5nm and less than 50nm from the surface, so that the crystal structure of a wider area can be stabilized.
[0203] When a plurality of additive elements are included as described above, each additive element synergistically contributes to further stabilization of the surface layer portion 10a. In particular, when magnesium, nickel, and aluminum are included, the effect of achieving a stable composition and crystal structure is high, and therefore, it is preferred.
[0204] Note that it is not preferred that lithium is not easily inserted and removed when the surface portion 10a contains only a compound of an added element and oxygen. For example, a surface portion 10a containing only MgO, a structure containing MgO and NiO(II) in a solid solution, and / or a structure containing MgO and CoO(II) in a solid solution is not preferred. Therefore, it is preferred that the surface portion 10a contains at least cobalt and also contains lithium in a discharged state, and that a path for inserting and removing lithium is ensured.
[0205] In addition, in order to fully ensure the path for the insertion and extraction of lithium, the cobalt concentration of the surface portion 10a is preferably higher than the magnesium concentration. In addition, the cobalt concentration of the surface portion 10a is preferably higher than the nickel concentration. In addition, the cobalt concentration of the surface portion 10a is preferably higher than the aluminum concentration. In addition, the cobalt concentration of the surface portion 10a is preferably higher than the fluorine concentration.
[0206] If the nickel content is too high, the diffusion of lithium may be blocked. Therefore, the magnesium concentration in the surface layer portion 10 a is preferably higher than the nickel concentration.
[0207] In addition, the concentration of a part of the added elements, especially magnesium and nickel, in the surface part 10a is preferably higher than that in the bulk part 10b, and they are preferably also present irregularly and in small amounts in the bulk part 10b. In addition, aluminum, which is a part of the added elements, is preferably also present irregularly and in small amounts in the bulk part 10b. When magnesium and aluminum are present at appropriate concentrations at the lithium position of the bulk part 10b, the same effect as described above is achieved, such as facilitating the maintenance of the layered rock salt type crystal structure. In addition, when nickel is present at an appropriate concentration in the bulk part 10b, the deviation of the layered structure composed of octahedra of cobalt and oxygen is suppressed, as described above. In addition, when magnesium and nickel are used simultaneously, a synergistic effect of suppressing the dissolution of magnesium can be expected, as described above.
[0208] In addition, preferably, due to the concentration gradient of the added element, the crystal structure of lithium cobaltate continuously changes from the bulk portion 10b to the surface layer portion 10a. At this time, the composition and crystal structure of the surface layer portion 10a at room temperature (25 ° C) are preferably more stable than those of the bulk portion 10b. For example, at least a part of the surface layer portion 10a of the positive electrode active material 10 that can be used in one embodiment of the present invention preferably has a rock salt-type crystal structure. Alternatively, the surface layer portion 10a preferably has both a layered rock salt-type crystal structure and a rock salt-type crystal structure. Alternatively, the surface layer portion 10a preferably exhibits the characteristics of both a layered rock salt-type and a rock salt-type crystal structure.
[0209] In addition, preferably, due to the concentration gradient of the added element, the crystal orientations of the surface layer portion 10a and the bulk portion 10b are substantially the same. Alternatively, preferably, the surface layer portion 10a and the bulk portion 10b are in topotaxy.
[0210] In this specification and the like, topotaxy refers to a state having similarity in three-dimensional structure with substantially the same crystal orientation or a state having the same orientation crystallographically. In addition, epitaxy refers to the structural similarity of a two-dimensional interface.
[0211] When the relationship between the surface layer portion 10a and the bulk portion 10b is in topotaxy, the distortion of the crystal structure and / or the misalignment of the atomic arrangement can be reduced. Thereby, the cause of the pits can be suppressed. In addition, in this specification and the like, a pit refers to a hole formed by the expansion of a defect in the positive electrode active material.
[0212] <<Li x When x in CoO2 is small>> The positive electrode active material 10 that can be used in one embodiment of the present invention has the above-described distribution of the added element and / or crystal structure, and thus the charged state, that is, Li x The crystal structure in the state where x in CoO2 is small is different from that of the conventional positive electrode active material. As described above, in this specification and the like, "x is small" means the case where 0.1 <x ≤ 0.24.
[0213] First, in the existing Li x CoO2, lithium cobaltate with x = 0.5 where x is slightly small has Figure 5 As shown, the symmetry of lithium is improved and it has a crystal structure belonging to the space group P2 / m of the monoclinic system. In this structure, the unit cell includes one CoO2 layer. Therefore, it is sometimes referred to as monoclinic O1 type or O1 type. In Figure 5 , the crystal structure of x = 0.5 is represented by P2 / m (monoclinic O1).
[0214] Regarding the existing Li xCoO2, lithium cobalt oxide when x = 0 Figure 5 The crystal structure shown has a trigonal space group P-3m1, and the unit cell includes a CoO2 layer. Therefore, this crystal structure is sometimes called trigonal O1 type or O1 type. In addition, the trigonal crystal is sometimes transformed into a composite hexagonal lattice and called hexagonal O1 type. Figure 5 In the figure, the crystal structure with x=0 is represented by P-3m1 (trigonal O1).
[0215] In addition, the existing Li x When x in CoO2 is 0.12 (corresponding to the case where x is smaller), lithium cobalt oxide is as follows Figure 5 The crystal structure has a space group R-3m as shown. It can also be said that this structure is a structure in which a CoO2 structure such as the trigonal O1 type and a LiCoO2 structure such as the R-3m(O3) type are alternately stacked. Therefore, this crystal structure is sometimes called an H1-3 type crystal structure. In addition, in fact, the number of cobalt atoms in each unit cell of the H1-3 type crystal structure is twice that of other structures. However, in Figure 5 In this specification, for easy comparison with other crystal structures, the c-axis of the H1-3 type crystal structure is 1 / 2 of the unit cell. Figure 5 In the figure, the crystal structure with x=0.12 is represented by R-3m1(H1-3).
[0216] In the H1-3 type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be represented by Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are both oxygen atoms. For example, by performing a Rietveld analysis using an X-ray diffraction method (denoted as XRD), it can be determined which unit cell is used to represent a certain crystal structure. In the Rietveld analysis, a unit cell with a small GOF (goodness of fit) value can be used.
[0217] When the Li corresponding to the case of x being small is repeated x When x in CoO2 is less than 0.12, the charge and discharge Figure 5 As shown, the crystal structure of conventional lithium cobalt oxide changes repeatedly between the H1-3 type crystal structure and the R-3m O3 structure in a discharged state (ie, a non-equilibrium phase transition).
[0218] However, the CoO2 layers of the above two crystal structures deviate greatly. Figure 5As shown by the dotted line and arrow in the crystal structure represented by R-3m1(H1-3), in the H1-3 type crystal structure, the CoO2 layer deviates greatly from the R-3m(O3) in the discharge state. Such dynamic structural changes will have an adverse effect on the stability of the crystal structure.
[0219] Furthermore, the volume difference between the two crystal structures undergoing dynamic structural changes is also large. When comparing the same number of cobalt atoms, the volume difference between the H1-3 type crystal structure and the R-3m (O3) type crystal structure in the discharge state exceeds 3.5%, and is typically more than 3.9%.
[0220] In addition to the above, the structure of the H1-3 type crystal structure in which the CoO2 layer is continuous, such as the trigonal O1 type, is likely to be unstable.
[0221] Therefore, when charging and discharging are repeatedly performed when x becomes less than 0.12, the crystal structure of the existing lithium cobalt oxide collapses. The collapse of the crystal structure will cause the deterioration of the cycle characteristics. This is because the collapse of the crystal structure causes a decrease in the number of locations where lithium can exist stably, and the insertion and removal of lithium become difficult. Note that not only in the case of repeated charging and discharging when x becomes less than 0.12, but in fact, when x is less than 0.24, a lot of crystal structure collapses, resulting in deterioration of the cycle characteristics. Therefore, in practice, the lithium ion battery is repeatedly charged and discharged while the existing lithium cobalt oxide is controlled to be within the range of x greater than 0.24.
[0222] On the other hand, Figure 4 In the positive electrode active material 10 that can be used in one embodiment of the present invention, Li x The change in crystal structure between the discharge state where x is 1 in CoO2 and the state where x is 0.2 or x is 0.15 corresponding to x being less than 0.24 is less than that of existing positive electrode active materials. Specifically, the positive electrode active material 10 can reduce the deviation of the CoO2 layer between the state where x is 1 and the state where x is less than 0.24. In addition, the positive electrode active material 10 can reduce the volume change when compared per cobalt atom. Therefore, even if the positive electrode active material 10 is repeatedly charged and discharged with x being less than 0.24, it is not easy to cause the crystal structure to collapse and good cycle characteristics can be achieved. In addition, the positive electrode active material 10 is x When x in CoO2 is 0.24 or less, it can have a more stable crystal structure than the existing positive electrode active material. x When x in CoO 2 is 0.24 or less, short circuit is less likely to occur, thereby improving the safety of the lithium ion battery.
[0223] Figure 4The crystal structures of the positive electrode active material 10 are shown for 0.1 < x ≤ 0.24, x = 0.2, and x = 0.15. The positive electrode active material 10 has crystal structures different from the H1-3 type crystal structure of the existing lithium cobaltate at x = 0.2 and x = 0.15.
[0224] Specifically, the positive electrode active material 10 at x = 0.2 has a crystal structure belonging to the space group R-3m of the trigonal system. The symmetry of the CoO2 layer of this structure is the same as that of O3. Therefore, in this specification and the like, this crystal structure is referred to as the "O3' type crystal structure". In Figure 4 the crystal structure of x = 0.2 is represented by R-3m(O3)'. Although the O3' type crystal structure of the positive electrode active material 10 is described for the case of x = 0.2, it may also have the O3' type crystal structure when x is around 0.2. x being around 0.2 can be expressed as 0.18 ≤ x ≤ 0.24, typically 0.18 ≤ x ≤ 0.22.
[0225] The coordinates of cobalt and oxygen in the unit cell of the O3' type crystal structure can be expressed as Co(0, 0, 0.5), O(0, 0, x) within the range of 0.20 ≤ x ≤ 0.25. In addition, the lattice constant a of the unit cell is preferably 0.2797 ≤ a ≤ 0.2837 (nm), more preferably 0.2807 ≤ a ≤ 0.2827 (nm), typically a = 0.2817 (nm). In addition, the lattice constant c is preferably 1.368 ≤ c ≤ 1.388 (nm), more preferably 1.375 ≤ c ≤ 1.381 (nm), typically c = 1.378 (nm).
[0226] In addition, as an example of 0.1 < x ≤ 0.24, the positive electrode active material 10 at x = 0.15 has a crystal structure belonging to the space group P2 / m of the monoclinic system. The unit cell includes one CoO2 layer. Therefore, in this specification and the like, this crystal structure is referred to as the "monoclinic O1(15) type crystal structure". In Figure 4 the crystal structure of x = 0.15 is represented by P2 / m(monoclinic O1(15)). Although the monoclinic O1(15) type crystal structure of the positive electrode active material 10 is described for the case of x = 0.15, it may also have the monoclinic O1(15) type crystal structure when x is around 0.15. x being around 0.15 can be expressed as 0.13 ≤ x ≤ 0.24, typically 0.13 ≤ x ≤ 0.18.
[0227] The coordinates of cobalt and oxygen in the unit cell of the monoclinic O1(15) type crystal structure can be Co1(0.5, 0, 0.5), Co2(0, 0.5, 0.5), O1(X O1 , 0, Z O1 ), 0.23 ≤ XO1 ≤0.24、0.61≤Z O1 ≤0.65, O2(X O2 , 0.5, Z O2 )、0.75≤X O2 ≤0.78、0.68≤Z O2 ≤0.71. In addition, the lattice constant a of the unit cell is a=0.488±0.001 (nm), the lattice constant b is b=0.282±0.001 (nm), and the lattice constant c is c=0.484±0.001 (nm). The angles representing the monoclinic crystal are α=90°, β=109.58±0.01°, and γ=90°.
[0228] Note that, if a certain range of error is allowed, the crystal structure can also be fitted in the space group R-3m. The coordinates of cobalt and oxygen in the unit cell can be expressed as Co(0,0,0.5), O(0,0,Z O ), where 0.21≤Z O ≤0.23. In addition, the lattice constant a of the unit cell is a=0.2817±0.002 (nm), and the lattice constant c is c=1.368±0.002 (nm).
[0229] In each of the O3' type and monoclinic O1(15) type crystal structures, ions of cobalt, nickel, magnesium, etc. occupy the positions coordinated to six oxygen atoms. In addition, light elements such as lithium may occupy the positions coordinated to four oxygen atoms.
[0230] like Figure 4 In the figure, the dotted line along the end of the CoO2 layer indicates that there is almost no deviation in the CoO2 layer between the R-3m(O3) and O3' type crystal structures and the monoclinic O1(15) type crystal structures in the discharged state. In addition, the difference in volume of the same number of cobalt atoms between the R-3m(O3) and O3' type crystal structures in the discharged state is less than 2.5%, more specifically less than 2.2%, and typically 1.8%. In addition, the difference in volume of the same number of cobalt atoms between the R-3m(O3) and monoclinic O1(15) type crystal structures in the discharged state is less than 3.3%, more specifically less than 3.0%, and typically 2.5%.
[0231] In the positive electrode active material 10, it is known that Li xWhen x in CoO2 is smaller, that is, when more lithium is detached, the change in the crystal structure is suppressed compared with the existing positive active material. In addition, the change in volume when compared by the same number of cobalt atoms is also suppressed. Therefore, the crystal structure of the positive active material 10 is not easy to collapse even if x is repeatedly charged and discharged below 0.24, so it can be seen that the decrease in charge and discharge capacity caused by the charge and discharge cycle is suppressed. In addition, a larger amount of lithium can be stably used compared with the existing positive active material, so the discharge capacity per unit weight and unit volume of the positive active material 10 is larger. Therefore, by using the positive active material 10, a lithium-ion battery with a higher discharge capacity per unit weight and unit volume can be manufactured.
[0232] In addition, it was confirmed that the positive electrode active material 10 x When x in CoO2 is 0.15 or more and 0.24 or less, it sometimes has an O3' type crystal structure, and it is considered that when x is higher than 0.24 and 0.27 or less, it also has an O3' type crystal structure. x When x in CoO2 is higher than 0.1 and lower than 0.2, and typically when x is higher than 0.13 and lower than 0.18, it sometimes has a monoclinic O1(15) type crystal structure. x In addition to x in CoO2, it is also affected by the number of charge and discharge cycles, charge and discharge current, temperature, electrolyte, etc., and is therefore not limited to the above range of x.
[0233] Therefore, the positive electrode active material 10 is x When x in CoO2 is higher than 0.1 and less than 0.24, it may have only O3' type crystal structure, only monoclinic O1(15) type crystal structure, or both crystal structures. In addition, the bulk portion 10b of the positive electrode active material 10 does not need to have O3' type crystal structure and / or monoclinic O1(15) type crystal structure as a whole. In addition, it may have other crystal structures or may have amorphous in part.
[0234] In order to realize Li x In the case of CoO2 with a small x value, a high charging voltage is generally required for charging. xThe state in which x in CoO2 is small is called the state of charging at a high charging voltage. It can also be said that the positive electrode active material 10 can maintain the R-3m (O3) crystal structure even when charged at a high charging voltage of 4.6V or more at 25°C, so it is preferred. In addition, it can also be said that the positive electrode active material 10 can have an O3' type crystal structure when charged at a higher charging voltage of 4.65V or more and 4.7V or less at 25°C, so it is preferred. In addition, it can also be said that the positive electrode active material 10 can have a monoclinic O1 (15) type crystal structure when charged at a further high charging voltage of 4.8V or more at 25°C, so it is preferred.
[0235] The positive electrode active material 10 sometimes has H1-3 type crystals only observed when the charging voltage is further increased. In addition, as described above, the crystal structure is affected by the number of charge and discharge cycles, the charge and discharge current, the electrolyte, etc., so when the charging voltage is lower, for example, even at 25°C and the charging voltage is 4.5V or more and less than 4.6V, the positive electrode active material 10 that can be used in one embodiment of the present invention sometimes has an O3' type crystal structure. Similarly, when charged at 25°C and a charging voltage of 4.65V or more and 4.7V or less, it sometimes has a monoclinic O1(15) type crystal structure.
[0236] In addition, for example, when graphite is used as the negative electrode active material of a lithium ion battery, the voltage drop of the above-mentioned lithium ion battery is equivalent to the potential of the graphite. The potential of graphite is about 0.01V to 0.7V based on the potential of lithium metal. Therefore, the lithium ion battery using graphite as the negative electrode active material has the same crystal structure as the case where the voltage is obtained by subtracting the potential of graphite from the above voltage.
[0237] In addition, Figure 4 In the O3' type crystal structure and the monoclinic O1(15) type crystal structure, lithium exists in all lithium positions with equal probability, but is not limited to this. In addition, lithium may also exist in a concentrated manner in a part of the lithium positions. The distribution of lithium can be analyzed by neutron diffraction, for example.
[0238] In addition, although the O3' type crystal structure and the monoclinic O1(15) type crystal structure contain lithium irregularly between the layers, they can also have a crystal structure similar to the CdCl2 type crystal structure. This crystal structure similar to the CdCl2 type crystal structure is similar to the case where lithium nickelate is charged to become Li 0.06 However, pure lithium cobalt oxide or layered rock salt-type positive electrode active materials containing a large amount of cobalt generally do not have a CdCl2-type crystal structure.
[0239] In addition, the concentration gradient of the added element preferably has the same gradient in multiple regions of the surface portion 10a of the positive electrode active material 10. In other words, the reinforcement derived from the added element preferably exists homogeneously in the surface portion 10a. Even if reinforcement exists in a part of the surface portion 10a, if there is a part without reinforcement, stress may be concentrated in this part. When stress is concentrated in a part of the positive electrode active material 10, defects such as cracks may occur from this part, thereby causing the rupture of the positive electrode active material and a decrease in the discharge capacity. Note that it is not necessary for the added elements in the entire surface portion 10a of the positive electrode active material 10 to have the same concentration gradient.
[0240] <<Grain Boundary>> Preferably, the additive element of the positive electrode active material 10 that can be used in one embodiment of the present invention is distributed unevenly in addition to the above distribution. Figure 3B The grain boundary 15 and its vicinity are shown.
[0241] For example, the magnesium concentration at the grain boundary 15 and its vicinity of the positive electrode active material 10 is preferably higher than that in other regions of the bulk portion 10b. In addition, the fluorine concentration at the grain boundary 15 and its vicinity is also preferably higher than that in other regions of the bulk portion 10b. In addition, the nickel concentration at the grain boundary 15 and its vicinity is also preferably higher than that in other regions of the bulk portion 10b. In addition, the aluminum concentration at the grain boundary 15 and its vicinity is also preferably higher than that in other regions of the bulk portion 10b.
[0242] The grain boundary 15 is one of the surface defects and thus tends to be unstable like the surface and is prone to change in crystal structure. Therefore, by increasing the concentration of the added element at the grain boundary 15 and its vicinity, the change in crystal structure can be more effectively suppressed.
[0243] In addition, when the concentrations of magnesium and fluorine are high at the grain boundary 15 and its vicinity, even when cracks are generated along the grain boundary 15 of the positive electrode active material 10 that can be used in one embodiment of the present invention, the concentrations of magnesium and fluorine are high near the surface generated by the cracks. Therefore, the corrosion resistance of the positive electrode active material to hydrofluoric acid can also be improved after the cracks are generated.
[0244] <Analysis Method> In order to determine whether a positive electrode active material is in Li x The positive electrode active material 10 that can be used in one embodiment of the present invention, which has an O3' type crystal structure and / or a monoclinic O1(15) type crystal structure when x in CoO2 is small, can contain Li xThe positive electrode of the positive electrode active material in a charged state where x in CoO 2 is small is determined by analysis using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), or the like.
[0245] In particular, XRD is preferred because of the following advantages: the symmetry of transition metals such as cobalt in the positive electrode active material can be analyzed with high resolution; the height of crystallinity and the orientation of crystallinity can be compared; the periodic distortion of the lattice and the grain size can be analyzed; sufficient accuracy can be obtained when directly measuring the positive electrode obtained by disassembling a lithium ion battery, etc. Through XRD, especially powder XRD, a diffraction peak reflecting the crystal structure of the bulk portion 10b of the positive electrode active material 10 that occupies most of the volume of the positive electrode active material 10 can be obtained.
[0246] When the sample to be measured is a powder sample, the measurement is sometimes referred to as the above-mentioned powder XRD measurement, and the powder can be mounted by placing it in a glass sample holder; sprinkling the sample on a silicon non-reflective plate coated with grease; etc. When the sample to be measured is a positive electrode, the positive electrode active material layer can be mounted according to the measurement surface required by the device by attaching the positive electrode to the substrate with double-sided tape.
[0247] In addition, when x is too small, such as being less than 0.1, or when the charging voltage exceeds 4.9 V, an H1-3 type or trigonal O1 type crystal structure is also generated in the positive electrode active material 10 that can be used in one embodiment of the present invention. Therefore, in order to determine whether it is a positive electrode active material 10 that can be used in one embodiment of the present invention, analysis of the crystal structure such as XRD and information such as the charging capacity or the charging voltage are required.
[0248] In addition, sometimes the positive electrode active material in a state where x is small changes its crystal structure when exposed to the atmosphere. For example, sometimes it changes from an O3' type and a monoclinic O1(15) type crystal structure to an H1-3 type crystal structure. Therefore, all samples used in analyzing the crystal structure are preferably processed in an inert atmosphere such as an argon atmosphere.
[0249] In addition, by analyzing by XPS, Energy Dispersive X-ray Spectroscopy (EDX), EPMA (Electron Probe Micro Analysis), etc., it can be determined whether the distribution of the additional elements contained in a certain positive electrode active material is in the above-mentioned state.
[0250] The crystal structure of the surface layer portion 10 a , the grain boundary 15 , and the like can be analyzed by performing electron diffraction or the like on a cross section of the positive electrode active material 10 .
[0251] <<Evaluation Conditions>> As an evaluation condition for determining whether a composite oxide is a positive electrode active material 10 that can be used in one embodiment of the present invention, a method of manufacturing a coin battery (e.g., CR2032 type, with a diameter of 20 mm and a height of 3.2 mm) containing lithium metal as a counter electrode and charging it under specified conditions can be cited. In addition, as an evaluation condition for determining whether a certain electrolyte is an electrolyte that can be used in one embodiment of the present invention, a method of manufacturing a coin battery (e.g., CR2032 type, with a diameter of 20 mm and a height of 3.2 mm) containing lithium metal as a counter electrode and charging it under specified conditions can be cited.
[0252] Step 1 described below is an example for confirming the physical properties of the positive electrode active material 10 that can be used in one embodiment of the present invention. Therefore, its structure is different from that of the electrolyte in the lithium ion battery of one embodiment of the present invention.
[0253] <<Evaluation Step 1>> A lithium-ion battery is disassembled, and the positive electrode impregnated with the electrolyte is taken out, and the positive electrode is punched into the size of the prepared coin battery. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. In addition, the electrolyte is removed before punching the positive electrode. For example, the positive electrode can also be washed with an organic solvent after taking out the positive electrode.
[0254] The coin cell contains lithium metal as the counter electrode. In addition, materials other than lithium metal may be used as the counter electrode. Unless otherwise specified, the potential in this specification and the like is the potential of the positive electrode when lithium metal is used as the counter electrode.
[0255] The coin cell can use 1 mol / L lithium hexafluorophosphate (LiPF6) dissolved in an organic solvent as the electrolyte, which is a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC = 3:7 and 2 wt% of vinylene carbonate (VC).
[0256] The coin cell includes a polypropylene porous film having a thickness of 25 μm as a separator.
[0257] In the coin battery, stainless steel (SUS) is used as the positive electrode can and stainless steel (SUS) is used as the negative electrode can.
[0258] In this manner, the coin battery A for evaluation was prepared.
[0259] The evaluation coin cell A manufactured under the above conditions is subjected to constant current charging (also referred to as CC charging) at a current value of 10 mA / g (when 1C is 200 mA / g of the unit weight of the positive electrode active material, it is equivalent to 0.05C) until reaching any voltage (for example, 4.5 V, 4.55 V, 4.6 V, 4.65 V, 4.7 V, 4.75 V or 4.8 V). In order to observe the phase change of the positive electrode active material, it is preferred to charge at the above-mentioned smaller current value.
[0260] The temperature of the evaluation coin battery A during charging may be 25° C. The temperature during charging may be the temperature of the thermostatic chamber in which the coin battery A is placed.
[0261] After charging under the above conditions, the coin cell A is disassembled in a glove box in an argon atmosphere and the positive electrode is taken out, thereby obtaining a positive electrode active material of any charge capacity. When various analyses are performed later, in order to prevent reaction with external components, it is preferably sealed under an argon atmosphere. For example, XRD can be performed under the condition of a sealed container sealed in an argon atmosphere. In addition, it is preferred to take out the positive electrode for analysis immediately after charging. Specifically, it is preferably performed within 1 hour after charging, and more preferably within 30 minutes after charging.
[0262] <<Evaluation Step 2>> A lithium-ion battery was disassembled, the positive electrode impregnated with electrolyte was taken out, and the nuclear magnetic resonance method (e.g. 1 H NMR) is used to measure the electrolyte and at least identify the organic solvent. The mixing ratio (volume ratio) of the organic solvent can also be identified by the nuclear magnetic resonance method. In addition, the lithium salt, additives, etc. contained in the electrolyte can also be identified.
[0263] Then, the positive electrode is punched into the size of a coin battery. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. In addition, the electrolyte is removed after the measurement of the nuclear magnetic resonance method and before the positive electrode is punched. For example, the positive electrode can also be washed with an organic solvent after taking out the positive electrode.
[0264] The coin cell contains lithium metal as a counter electrode. Alternatively, a material other than lithium metal may be used as the counter electrode.
[0265] In the coin battery, an electrolyte specified by nuclear magnetic resonance is prepared as an electrolyte. This electrolyte is an electrolyte of one embodiment of the present invention.
[0266] The coin cell includes a polypropylene porous film having a thickness of 25 μm as a separator.
[0267] In the coin battery, stainless steel (SUS) is used as the positive electrode can and stainless steel (SUS) is used as the negative electrode can.
[0268] In this manner, the coin battery B for evaluation was prepared.
[0269] The evaluation coin battery B manufactured under the above conditions is charged to any voltage (e.g., 4.5 V, 4.55 V, 4.6 V or 4.65 V, 4.7 V, 4.75 V, 4.8 V), and then discharged. The charging conditions can refer to the following examples, etc. In addition, the discharging conditions can refer to the following examples, etc.
[0270] The temperature during charging of the evaluation coin battery B can be set to 25° C. or below freezing point, and thereby the ratio of the charge / discharge capacity below freezing point to the charge / discharge capacity at 25° C. can be confirmed.
[0271] < <xrd>> The apparatus and conditions for XRD measurement of the coin cell A and the like are as follows. Note that the apparatus and conditions for XRD measurement are not limited to those described below. XRD device: D8 ADVANCE manufactured by Bruker AXS X-ray source: CuKα1 ray Output: 40KV, 40mA
[0272] <Powder XRD pattern> Figure 6 , Figure 7 , Fig. 8A and Figure 8B The ideal XRD patterns calculated by CuKα1 radiation from the models of O3' type crystal structure, monoclinic O1(15) type crystal structure and H1-3 type crystal structure are shown. In addition, for comparison, the XRD patterns calculated from Li x Ideal XRD pattern calculated from the crystal structures of LiCoO2 O3 where x is 1 and trigonal O1 where x is 0 in CoO2. Fig. 8A and Figure 8B The XRD patterns of O3' type, monoclinic O1(15) type and H1-3 type are shown. Fig. 8A The range of the enlarged 2θ is shown to be a region of 18° or more and 21° or less. Figure 8B The range of magnified 2θ is shown to be a region above 42° and below 46°. The patterns of LiCoO2(O3) and CoO2(O1) were made using the crystal structure information obtained from ICSD (Inorganic Crystal Structure Database) using Reflex PowderDiffraction, one of the modules of Materials Studio (BIOVIA). The range of 2θ was set to 15° to 75°, Step = 0.01°, and wavelength λ1 = 1.540562×10 -10 m, Monochromator is set to single. The pattern of the H1-3 type crystal structure is prepared in the same manner as the crystal structure information recorded in non-patent document 2. The patterns of the O3' type crystal structure and the monoclinic O1(15) type crystal structure are prepared by the following method: the crystal structure is inferred from the XRD pattern of the positive electrode active material that can be used in one embodiment of the present invention and fitted using TOPAS ver.3 (crystal structure analysis software manufactured by Bruker), and the XRD pattern is prepared in the same manner as other structures.
[0273] like Figure 6 , Fig. 8A and Figure 8B As shown, in the O3' type crystal structure, when analyzed by X-ray diffraction, diffraction peaks appear at 2θ of 19.25±0.12° (19.13° or more and less than 19.37°) and 2θ of 45.47±0.10° (45.37° or more and less than 45.57°).
[0274] In addition, in the monoclinic O1(15) type crystal structure, when analyzed by X-ray diffraction, diffraction peaks appear at 2θ of 19.47±0.10° (19.37° or more and 19.57° or less) and 2θ of 45.62±0.05° (45.57° or more and 45.67° or less).
[0275] On the other hand, Figure 7 , Fig. 8A and Figure 8B As shown, in the H1-3 type crystal structure and the trigonal O1 type crystal structure, the peak does not appear at the above position. x The presence of peaks at 19.13° to less than 19.37° and / or 19.37° to 19.57° and 45.37° to less than 45.57° and / or 45.57° to 45.67° in a state where x in CoO2 is small is a feature of the positive electrode active material 10 that can be used in one embodiment of the present invention.
[0276] This also indicates that: the position of the XRD diffraction peak appearing in the crystal structure when x=1 is close to the position of the XRD diffraction peak appearing in the crystal structure when x≤0.24; more specifically, regarding the peaks in the main diffraction peaks of the crystal structure when x=1 and the crystal structure when x≤0.24, the 2θ difference between the peaks appearing at 42° or more and 46° or less is less than 0.7°, preferably less than 0.5°.
[0277] In addition, the positive electrode active material 10 that can be used in one embodiment of the present invention is Li x When x in CoO2 is small, it has an O3' type crystal structure and / or a monoclinic O1(15) type crystal structure, but it is not necessary for all particles to have an O3' type crystal structure and / or a monoclinic O1(15) type crystal structure. It can have other crystal structures, and it can also be partially amorphous. Note that when performing Rietveld analysis on the XRD pattern, the O3' type crystal structure and / or the monoclinic O1(15) type crystal structure is preferably 50% or more, more preferably 60% or more, and further preferably 66% or more. When the O3' type crystal structure and / or the monoclinic O1(15) type crystal structure is 50% or more, more preferably 60% or more, and further preferably 66% or more, a positive electrode active material with sufficiently excellent cycle characteristics can be achieved.
[0278] Furthermore, the O3' type crystal structure and / or the monoclinic O1(15) type crystal structure as determined by Rietveld analysis after 100 or more charge and discharge cycles from the start of measurement is preferably 35% or more, more preferably 40% or more, and even more preferably 43% or more.
[0279] In addition, the sharpness of the diffraction peak in the XRD pattern indicates the height of crystallinity. Therefore, each diffraction peak after charging is preferably sharp, that is, the half-width is preferably narrow. The half-width of the peak of the same crystalline phase varies depending on the measurement conditions of XRD or the value of 2θ. When the above-mentioned measurement conditions are adopted, for example, the half-width of the peak observed at 2θ of 43° or more and 46° or less is preferably 0.2° or less, more preferably 0.15° or less, and further preferably 0.12° or less. Note that it is not necessary for all peaks to meet the above conditions. As long as a part of the peaks meet the above conditions, it can be said that the crystallinity of its crystalline phase is higher. Thus, it contributes to the stabilization of the crystal structure after charging.
[0280] In addition, the grain size of the O3' type crystal structure and the monoclinic O1(15) type crystal structure of the positive electrode active material 10 is reduced to only about 1 / 20 of that of LiCoO2(O3) in the discharged state. Therefore, even under the same XRD measurement conditions as the positive electrode before charge and discharge, the Li x When x in CoO2 is small, a clear peak of O3' type crystal structure is confirmed. On the other hand, even if a part of the existing LiCoO2 can have a structure similar to O3' type crystal structure, the grain size will become smaller and its peak will become wider and smaller. The grain size can be obtained from the half width of the XRD peak.
[0281] <<Surface roughness and specific surface area>> The positive electrode active material 10 that can be used in one embodiment of the present invention preferably has a smooth surface and few irregularities. A smooth surface and few irregularities indicate that the effect of the flux described later is fully exerted and the surface of the additive element source and the lithium cobalt oxide are melted (solid solution). Therefore, this is an element indicating that the distribution of the additive element in the surface layer portion 10a is good.
[0282] For example, whether the surface is smooth and has few irregularities can be determined by referring to a cross-sectional scanning electron microscope (SEM) image or a cross-sectional TEM image of the positive electrode active material 10 , the specific surface area of the positive electrode active material 10 , and the like.
[0283] <Other Features> The positive electrode active material 10 sometimes has a covering portion outside the surface layer portion 10a. The covering portion may not cover the entire positive electrode active material. The covering portion is sometimes an inorganic compound formed when the positive electrode active material is manufactured, and sometimes an electrolyte deposited during charge and discharge and a decomposition product of an organic electrolyte.
[0284] In the case where the covering portion includes an electrolyte and a decomposition product of an organic electrolyte, it is preferably carbon, oxygen and fluorine. In addition, a high-quality coating is easily obtained when LiBOB and / or SUN (suberonitrile) is used as a part of the electrolyte. Therefore, a covering portion including at least one or more than two selected from boron, nitrogen, sulfur and fluorine is sometimes a high-quality coating, so it is preferred.
[0285] This embodiment mode can be freely combined with other embodiment modes.
[0286] (Implementation 3) In this embodiment, a method for manufacturing a positive electrode active material that can be used in a lithium ion battery of the present invention is described. In this embodiment, a case where a positive electrode active material is manufactured using a coprecipitation method is described, but the lithium ion battery of the present invention can use a positive electrode active material that utilizes a solid phase method or a hydrothermal method in addition to the coprecipitation method. Note that the flowchart used to illustrate the manufacturing method, etc. in this embodiment shows the order of elements connected by lines, and does not show the order of elements not connected by lines. In addition, in this embodiment, when an oxide is manufactured as a positive electrode active material, a substance in the previous stage of the oxide, such as a hydroxide in the previous stage, is recorded as a precursor.
[0287] <Manufacturing method 1> In this production method 1, a method including a heating step according to one embodiment of the present invention will be described.
[0288] <Step S201: Prepare raw materials> First, in Fig. 9 In step S201, a raw material corresponding to the type of positive electrode active material is prepared. In the present manufacturing method 1, an aqueous solution in which at least a transition metal salt is dissolved is prepared. The aqueous solution in which the transition metal salt is dissolved can be recorded as a transition metal source. In addition, when the pH value of the aqueous solution in which the transition metal salt is dissolved is less than 7, preferably when the pH value is greater than 1 and less than 6, the aqueous solution is acidic, so the aqueous solution can be recorded as an acidic aqueous solution.
[0289] The transition metal is described. As the transition metal of the present invention, one or more selected from manganese, cobalt and nickel can be used. Specifically, as the transition metal, only cobalt, only nickel, two kinds of cobalt and manganese, two kinds of cobalt and nickel, or three kinds of cobalt, manganese and nickel can be used.
[0290] Sometimes, a composite oxide obtained by using three transition metals, namely nickel, cobalt and manganese, is referred to as a nickel-cobalt-manganese composite oxide. A nickel-cobalt-manganese composite oxide refers to a composite oxide before lithium mixed with a lithium nickel-cobalt-manganese composite oxide. In addition, in this specification, "lithium nickel-cobalt-manganese composite oxide" is referred to as "NCM". NCM can be represented by the chemical formula LiNi x Co y Mn z It is represented by O2 (x>0, y>0, 0.8<x + y + z<1.2). In NCM, according to the above chemical formula, Li is not limited to 1, and Li can be 0.58 or more and 1.10 or less, preferably 0.90 or more and 1.05 or less, more preferably 0.92 or more and 1.01 or less. NCM may also contain elements other than nickel, cobalt, and manganese.
[0291] In the above chemical formula LiNi x Co y Mn z In O2, the relational expression of the numerical values that x, y, and z can take preferably satisfies 0.1x < y < 8x and 0.1x < z < 8x. As the specific numerical values that x, y, and z can take, it preferably satisfies x:y:z = 1:1:1 or values near it. In addition, as another specific example of numerical values, x, y, and z preferably satisfy x:y:z = 5:2:3 or values near it. In addition, as another specific example of numerical values, x, y, and z preferably satisfy x:y:z = 8:1:1 or values near it. In addition, as another specific example of numerical values, x, y, and z preferably satisfy x:y:z = 9:0.5:0.5 or values near it. In addition, as another specific example of numerical values, x, y, and z preferably satisfy x:y:z = 6:2:2 or values near it. In addition, as another specific example, x, y, and z preferably satisfy x:y:z = 1:4:1 or values near it. In this paragraph, "near it" includes a range of ±10% of the numerical value. For example, when it is noted as near x:y:z = 8:1:1, x is 7.2 or more and 8.8 or less, and y and z are each 0.9 or more and 1.1 or more.
[0292] Sometimes the numerical values of the above x, y, and z are noted as the mixing ratios of nickel, cobalt, and manganese. The mixing ratio at least refers to the ratio of each element used when weighing the raw materials. When the mixing ratios of x, y, and z are satisfied, a layered rock salt-type crystal structure can be obtained, so it is preferred.
[0293] The ratio of each element obtained by analyzing and measuring NCM by X-ray photoelectron spectroscopy (XPS), inductively coupled plasma mass spectrometry (ICP-MS), or energy-dispersive X-ray analysis (TEM-EDX), that is, the numerical values corresponding to x, y, and z, is called the ratio of nickel, cobalt, and manganese. This ratio may not be consistent with the mixing ratio. For example, in the case where unreacted raw materials remain in the manufacturing process, etc., sometimes the mixing ratio is different from the ratio. When a part of the nickel raw material does not react, the ratio of nickel is less than the mixing ratio.
[0294] When the ratio of nickel in the transition metal is high, a cheap positive electrode active material can be provided, and a positive electrode active material with high potential or high capacity can be provided, so it is preferred. For example, when the sum of the number of atoms of nickel, cobalt and manganese contained in the positive electrode active material is 100, the number of atoms of nickel is preferably 33 or more, more preferably 50 or more, and further preferably 80 or more. However, when the ratio of nickel is too high, there is concern about reduced chemical stability and heat resistance. Therefore, when the sum of the number of atoms of nickel, cobalt and manganese contained in the positive electrode active material is 100, the number of atoms of nickel is preferably 95 or less.
[0295] When cobalt is included as a transition metal, the average discharge voltage is high and cobalt contributes to the stabilization of the layered rock salt structure to achieve a secondary battery with improved cycle characteristics or high reliability, so it is preferred. However, the price of cobalt is more expensive and unstable than nickel and manganese, so when the ratio of cobalt is too high, there is a concern about increased manufacturing costs. Therefore, for example, when the sum of the number of atoms of nickel, cobalt and manganese contained in the positive electrode active material is 100, the number of atoms of cobalt is preferably 2.5 or more and 34 or less.
[0296] When manganese is included as a transition metal, heat resistance and chemical stability are improved, so it is preferred. However, when the ratio of manganese is too high, there is a tendency for the discharge voltage and discharge capacity to decrease. Therefore, for example, when the sum of the number of atoms of nickel, cobalt and manganese included in the positive electrode active material is 100, the number of atoms of manganese is preferably 2.5 or more and 33 or less.
[0297] Description of the aqueous solution in which a transition metal salt is dissolved. In the present invention, as the aqueous solution in which a transition metal salt is dissolved, an aqueous solution in which the above-mentioned nickel salt is dissolved or an aqueous solution containing a water-soluble salt of nickel can be used, and typically an aqueous solution in which nickel sulfate or nickel nitrate or the like is dissolved in water can be used. In the aqueous solution, nickel ions are sometimes present, and nickel sometimes exists as a complex. In addition, in the present invention, as the aqueous solution in which a transition metal salt is dissolved, an aqueous solution in which a cobalt salt is dissolved or an aqueous solution containing a water-soluble salt of cobalt can be used, and typically an aqueous solution in which cobalt sulfate or cobalt nitrate or the like is dissolved in water can be used. In the aqueous solution, cobalt ions are sometimes present, and cobalt sometimes exists as a complex. In addition, in the present invention, as the aqueous solution in which a transition metal salt is dissolved, an aqueous solution in which a manganese salt is dissolved or an aqueous solution containing a water-soluble salt of manganese can be used, and an aqueous solution in which manganese sulfate or manganese nitrate or the like is dissolved in water can be used. In the aqueous solution, manganese ions are sometimes present, and manganese sometimes exists as a complex.
[0298] The purity of the aqueous solution in which the transition metal salt is dissolved is preferably high, and pure water is preferably used as the aqueous solution. The concentration of the transition metal ions in the aqueous solution in which the transition metal salt is dissolved is 1 mol / L or more and 5 mol / L or less, preferably 2 mol / L or more and 3 mol / L or less. When the aqueous solution contains a plurality of transition metal salts, the total concentration of the transition metal ions satisfies the above range.
[0299] In the present invention, when three metals, namely cobalt, manganese and nickel, are used as transition metals, an aqueous solution in which a cobalt salt, a manganese salt and a nickel salt are dissolved can be used as the aqueous solution in which a transition metal salt is dissolved. Typically, an aqueous solution in which nickel sulfate, cobalt sulfate and manganese sulfate are dissolved can be used as the aqueous solution in which a transition metal salt is dissolved.
[0300] Furthermore, in Fig. 9 In step S201, an alkaline aqueous solution (referred to as an alkaline aqueous solution) is prepared. In addition, an alkaline aqueous solution refers to an aqueous solution having a pH value greater than 7, preferably an aqueous solution having a pH value of 8 or more. As the alkaline aqueous solution of the present invention, an aqueous solution containing sodium hydroxide, potassium hydroxide, lithium hydroxide or ammonia can be used. For example, an aqueous solution in which sodium hydroxide, potassium hydroxide, lithium hydroxide or ammonia is dissolved in water can be used. In addition, an aqueous solution in which a plurality of selected from sodium hydroxide, potassium hydroxide, lithium hydroxide and ammonia are dissolved in water can also be used. Pure water is preferably used as the above-mentioned water. The alkali concentration of the alkaline aqueous solution is greater than 1 mol / L and less than 10 mol / L, preferably greater than 3 mol / L and less than 7 mol / L. When the aqueous solution contains multiple alkalis, the sum of the alkali concentrations satisfies the above-mentioned range.
[0301] As pure water used for the aqueous solution and alkaline aqueous solution in which the transition metal salt is dissolved, water having a resistivity of 1 MΩ·cm or more is preferably used, water having a resistivity of 10 MΩ·cm or more is more preferably used, and water having a resistivity of 15 MΩ·cm or more is further preferably used. Water satisfying the above resistivity has high purity and contains very few impurities.
[0302] <Step S203: Mixing process> Then, in Fig. 9 In step S203, the two aqueous solutions are mixed to produce a mixed aqueous solution (referred to as a mixed solution or a coprecipitation mixed solution). In this step, pure water different from the two aqueous solutions may also be prepared and a mixed aqueous solution may be produced in the pure water. In this step, an aqueous solution in which a transition metal salt is dissolved may react with an alkaline aqueous solution. The reaction is sometimes referred to as a neutralization reaction, an acid-base reaction or a coprecipitation reaction. In this step, as the reaction proceeds, a coprecipitate is precipitated. In this specification, etc., the product (reaction product) produced by the reaction is referred to as a coprecipitate. When an aqueous solution in which the transition metal salt is dissolved and an alkaline aqueous solution are mixed, a hydroxide is formed as a coprecipitate. In order to promote the reaction, it is preferred to keep the temperature and pH value of the mixed solution constant, and it is also preferred to stir the mixed solution. The temperature is preferably above 40°C and below 90°C, more preferably above 45°C and below 70°C. The pH value is preferably within the range of above 9.0 and below 13.0, more preferably within the range of above 10.5 and below 11.5. The rotation speed of the stirring is preferably 800 rpm or more and 1200 rpm or less, and more preferably 900 rpm or more and 1100 rpm or less.
[0303] As described above, in this step, a coprecipitate is precipitated as a reaction product in the mixed solution. The coprecipitate may be precipitated in the mixed solution, and is sometimes recorded as a precipitate. When the coprecipitate begins to precipitate, the mixed solution sometimes becomes a suspension. A suspension refers to a liquid in which particles of the coprecipitate are dispersed in a liquid.
[0304] <Step S205: Filtration process> Then, in Fig. 9 In step S205, the mixed solution is filtered to obtain a coprecipitate from the mixed solution. Specifically, the coprecipitate is taken out from the mixed solution. The filtration is preferably performed by suction filtration. The coprecipitate has a size (long axis) of more than 1 μm and less than 20 μm. In addition, in order to distinguish it from the coprecipitate in the mixed solution, an ordinal number can be added to the coprecipitate obtained by filtration, and sometimes the coprecipitate obtained by filtration is recorded as filtered powder.
[0305] As a coprecipitate, a hydroxide containing a transition metal can be obtained. When an aqueous solution containing a nickel salt, a cobalt salt and a manganese salt is used as an aqueous solution containing a transition metal, a hydroxide containing cobalt, manganese and nickel (referred to as a composite hydroxide containing cobalt, manganese and nickel) can be obtained as a coprecipitate. The coprecipitate obtained by filtration is typically a hydroxide containing impurities such as water.
[0306] The hydroxide obtained as a coprecipitate sometimes becomes a secondary particle in which primary particles are aggregated. Note that a primary particle refers to a particle (block) of the smallest unit confirmed when observed at 20,000 times using, for example, a SEM (scanning electron microscope). That is, a primary particle is a particle of the smallest unit. A secondary particle refers to a particle in which the above-mentioned primary particles are aggregated, and the above-mentioned primary particles share a part of the above-mentioned grain boundary (the periphery of the primary particles, etc.), and are not easily separated from each other (but are independent of each other).
[0307] <Step S207: Washing process> Then, in Fig. 9 In step S207, the coprecipitate is washed to obtain a hydroxide from which impurities have been removed. As the washing in this step, washing with water can be utilized. Washing with water is sometimes referred to as water washing. Note that water washing can be performed once or repeatedly multiple times. By water washing, impurities in the coprecipitate can be removed to a certain extent. As water, distilled water or pure water is preferably used. Regarding pure water, reference can be made to the contents described in step S201. In this step, suction filtration can also be performed after the coprecipitate is washed with water. In addition, when water washing is performed repeatedly multiple times, suction filtration is preferably performed after the water washing.
[0308] As the washing of the above steps, washing with an organic solvent can be utilized. In addition, washing with an organic solvent can be performed once or repeatedly for multiple times. By washing with an organic solvent, the coprecipitate can be dried. Drying includes removing the water or moisture attached by the previous washing or the like. As an organic solvent, an alcohol such as acetone or isopropanol (typically isopropanol) is preferably used. In this step, suction filtration can also be performed after washing the coprecipitate with an organic solvent. In addition, when washing with an organic solvent is repeatedly performed for multiple times, suction filtration is preferably performed after washing with an organic solvent.
[0309] In addition, as the washing of the above steps, washing with water and washing using an organic solvent can be combined. Preferably, suction filtration is used. For example, a suction filtration process can be implemented after washing with water, and then the suction filtration process is implemented again after washing with an organic solvent. At this time, it is preferred that the number of washing times with water is more than the number of washing times using an organic solvent.
[0310] <Step S209: Heating process> Fig. 9 Step S209 is a process of heating the coprecipitate, through which impurities can be fully removed. When there are few impurities, this step can be omitted. Specifically, through this step, hydrogen and oxygen in the coprecipitate can be removed in the form of water. Since the process of removing hydrogen and oxygen in the form of water is called dehydration, the heating process of this step includes a dehydration process. In addition, through this step, water or moisture contained in the coprecipitate can be removed. Since the process of removing water or moisture is called drying, the heating process of this step includes a drying process. In addition, in the heating process of this step, in addition to water or moisture, impurities can also be removed by gasifying them. For example, the organic solvent used in step S207 can also be removed through the heating process of this step.
[0311] Supplementary explanation of the temperature of this step. The upper limit of the heating temperature in this step is preferably lower than the temperature at which the hydroxide as the coprecipitate begins to transform into an oxide. That is, in this step, it is preferred not to transform the hydroxide into an oxide. In addition, the temperature at which the hydroxide transforms into an oxide can be determined by differential thermal-thermogravimetry (TG-DTA). When Ni is used as the hydroxide 0.8 Co 0.1 Mn 0.1 When (OH)2, in the region where the TG curve shows a decrease, the DTA curve starts to decrease at 210°C or above and 230°C or below, typically at 220°C or thereabouts, and the maximum peak of endothermic absorption is observed at 260°C or thereabouts. Based on this result, it can be deduced that the temperature at which the hydroxide begins to decompose, dehydrate or reduce, that is, the temperature at which the hydroxide begins to transform into an oxide is 220°C, so 220°C can be set as the upper limit of the heat treatment temperature.
[0312] The higher the temperature of the heat treatment, the easier the treatment is, the shorter the treatment time is, and the higher the productivity is, so it is preferred.
[0313] The lower limit of the temperature of the heat treatment may be a temperature at or above which water or moisture of the hydroxide can be removed. The process of removing water or moisture is also called drying.
[0314] In consideration of the above description, the specific heat treatment temperature is preferably 130° C. or higher and 220° C. or lower, more preferably 150° C. or higher and 220° C. or lower, and further preferably 180° C. or higher and 220° C. or lower.
[0315] The time of the heat treatment in this step is preferably 3 hours to 15 hours, more preferably 8 hours to 15 hours, further preferably 10 hours to 13 hours, and further preferably 11 hours to 12 hours.
[0316] In addition, the atmosphere of the heat treatment in this step is preferably an atmosphere that does not contain oxygen. The atmosphere that does not contain oxygen is recorded as an oxygen-free atmosphere. As an oxygen-free atmosphere, a dry atmosphere, a vacuum atmosphere or an inert atmosphere (typically a nitrogen atmosphere, an argon atmosphere) can be used. When heating under a dry atmosphere, it is preferred to set the dew point in the container to below -40°C, and more preferably to below -80°C. When heating under a vacuum atmosphere, a bell-shaped vacuum device can be used, which includes a container (referred to as a bell) that can evacuate the interior to a vacuum and a vacuum pump connected to the bell. In addition, when heating under a vacuum atmosphere, a vacuum drying furnace can also be used, and the vacuum drying furnace includes a vacuum pump connected to the drying furnace. The vacuum pumps of the bell-shaped vacuum device and the vacuum drying furnace can use a dry pump, a turbomolecular pump, an oil pump, a cryogenic pump or a mechanical booster pump. The vacuum atmosphere in the bell-shaped vacuum device and the vacuum drying furnace includes an atmosphere in which the pressure difference gauge of each device is greater than -0.1MPa and less than -0.08MPa. When heating is performed in a nitrogen atmosphere, a nitrogen-containing gas may be flowed through a container provided in a bell-jar type vacuum apparatus or a vacuum drying furnace.
[0317] In addition, as the heat treatment in this step, multiple heat treatments can also be performed. For example, a heat treatment can be performed at a first temperature for a first time, and then a heat treatment can be performed at a second temperature for a second time. The second temperature satisfies the temperature range of the above-mentioned heat treatment. The first temperature is lower than the second temperature, for example, a temperature in the range of 80°C or more and less than 90°C. The second time satisfies the range of the time of the above-mentioned heat treatment. The first time is shorter than the second time, for example, more than 0.5 hours and less than 1 hour. Impurities in the hydroxide can be easily removed by multiple treatments, so it is preferred.
[0318] <Step S210: Preparation of lithium source> Then, in Fig. 9 In step S210, a lithium source is prepared. The ratio of the lithium source to the hydroxide (lithium source / hydroxide) is set to be greater than 0.90 and less than 1.05, preferably greater than 0.92 and less than 1.01. In the present invention, a lithium compound can be used as a lithium source. As the lithium compound, lithium hydroxide, lithium carbonate or lithium nitrate can be cited. The purity of the lithium source is preferably high. In addition, the lithium source is preferably crushed, thereby promoting the solid phase reaction.
[0319] In addition, the melting point of lithium hydroxide is 462°C, which is the lowest among lithium compounds. When manufacturing a positive electrode active material with a high nickel ratio, it is necessary to heat at a low temperature in order to suppress cation mixing. Therefore, it is preferred to use a lithium compound with a low melting point such as lithium hydroxide when manufacturing a positive electrode active material with a high nickel ratio.
[0320] <Step S211: Mixing process> Then, in Fig. 9 In step S211, a lithium source is mixed with the hydroxide to produce a mixture. In this specification, the previous stage of becoming an oxide is called a precursor. In order to distinguish it from the above-mentioned mixing step, an ordinal number is sometimes added to this mixing step. In the present invention, the mixing in this step can be performed by a dry method or a wet method.
[0321] As a device for performing mixing, etc., a ball mill, a sand mill, a kneading machine, etc. can be used. When a ball mill is used, for example, zirconia balls are preferably used as the medium.
[0322] <Step S213: Heating process> Then, in Fig. 9 The mixture is heated in step S213. Since the mixture becomes an oxide after this heating process, the mixture is called a precursor. Note that in order to distinguish it from the previous heating process, a sequence number is sometimes added to the heating process of this step.
[0323] As the heating condition of this step, heating can be performed at a first temperature first and then at a second temperature. Sometimes, heating at the first temperature is recorded as the first roasting, and heating at the second temperature is recorded as the second roasting. Note that in the present invention, the second roasting can be performed without performing the first roasting. That is, this step can also be performed once.
[0324] In this step, the second temperature is preferably higher than the first temperature. In this case, the heating at the first temperature is sometimes recorded as pre-baking, and the heating at the second temperature is recorded as main baking. Note that in the present invention, the main baking may be performed without pre-baking. However, when lithium hydroxide is used as a lithium source, it is preferred to perform pre-baking.
[0325] In this step, the first temperature is preferably higher than the melting point of the lithium source. Typically, the first temperature is preferably 500° C. or higher and 700° C. or lower. In this step, the second temperature is preferably higher than 500° C. and lower than 1050° C., and when the second temperature is higher than the first temperature, the second temperature is preferably higher than 700° C. and lower than 1050° C.
[0326] In this step, the heating time of the first temperature and the second temperature is preferably more than 1 hour and less than 20 hours. The heating time of the first temperature can be equal to the heating time of the second temperature, and can be longer or shorter than the heating time of the second temperature.
[0327] In the present invention, the heating at the first temperature and the heating at the second temperature are preferably carried out in an oxygen atmosphere, and are particularly preferably carried out while supplying oxygen. For example, the heating rate is preferably 2 L / min to 15 L / min, more preferably 5 L / min to 10 L / min per 1 L of furnace volume. The heating atmosphere at the first temperature may be the same as or different from the heating atmosphere at the second temperature.
[0328] In the present invention, the roasting device used for heating at the first temperature and the second temperature may use an electric furnace or a rotary kiln. The roasting device used for heating at the first temperature may be the same as or different from the roasting device used for heating at the second temperature.
[0329] In the present invention, when heating, the mixture is placed in a crucible or a sagger. The crucible or sagger preferably contains a material with high heat resistance such as a material made of alumina (aluminum oxide), a material made of mullite-cordierite, a material made of magnesium oxide, and a material made of zirconium oxide. The aluminum oxide in the material is also a material that impurities are not easily mixed into, so it is preferred. For example, it is preferred to use a crucible or sagger made of alumina with a purity of more than 99%, preferably more than 99.5%. In the present embodiment, a crucible made of aluminum oxide with a purity of 99.9% is used. In addition, it is preferred to heat the crucible or sagger cover, thereby preventing the sublimation of the material contained in the mixture. The lid can be configured in a manner that the interior of the crucible is blocked from the internal air of the furnace, and can also be configured in a manner that a portion of the crucible is open in a manner that the interior of the crucible is in contact with the internal air of the furnace.
[0330] In the present invention, it is preferred to use a mortar to perform pulverization or grinding between the heating step at the first temperature and the heating step at the second temperature. By pulverizing or grinding, the adhesion state between the mixtures or the aggregation state between the mixtures can be eliminated. When the mixtures are adhered to each other during heating, the contact area with oxygen in the atmosphere is sometimes reduced, so it is preferred to pulverize or grind as described above. Furthermore, after pulverizing or grinding, classification can also be performed using a sieve.
[0331] When the material is transferred from the crucible to the mortar and the heated material is recovered, it is preferable that no impurities are mixed in the material. The mortar is also preferably formed of a material that does not easily release impurities. Specifically, it is preferable to use an alumina mortar with a purity of 90% or more, preferably 99% or more.
[0332] In this way, a lithium composite oxide as a positive electrode active material can be manufactured. In addition, according to manufacturing method 1, a positive electrode active material NCM can be obtained from the prepared raw materials. By using the obtained NCM, a battery characteristic with a high discharge capacity can be obtained, so it is preferred. Furthermore, the median particle size (D50) of NCM is greater than 3 μm and less than 13 μm, greater than 4 μm and less than 10 μm. When the median particle size (D50) is small, the discharge capacity increases, so the median particle size (D50) of NCM is preferably greater than 4 μm and less than 7 μm.
[0333] <Manufacturing method 2> In the present production method 2, a complexing agent, typically a chelating agent, is prepared as a raw material. Since the present production method 2 has the same steps as the production method 1, reference is made to Fig. 9 The flowchart is described below.
[0334] <Step S201: Preparation of Raw Materials> As in Fig. 9 The raw materials prepared in step S201 are preferably added with a complexing agent. A complexing agent is a compound that can form a complex with the ions of a transition metal in an aqueous solution. As a complexing agent, ammonia or an ammonium salt can be cited. Note that an aqueous solution in which they are dissolved in water, for example, pure water, is used as a complexing agent. When ammonia is used, it can be recorded as an aqueous ammonia solution.
[0335] Furthermore, as in Fig. 9 The raw materials prepared in step S201 can also be prepared as a chelating agent for forming a chelating compound. As chelating agents, glycine, oxine, 1-nitroso-2-naphthol, 2-mercaptobenzothiazole or EDTA (ethylenediaminetetraacetic acid) can be cited. In addition, multiple selected from glycine, oxine, 1-nitroso-2-naphthol or 2-mercaptobenzothiazole can also be used. Note that an aqueous solution in which they are dissolved in water (e.g., pure water) is used as a chelating agent. When glycine is used, it can be recorded as a glycine aqueous solution.
[0336] In this step, it is preferred to mix and dissolve an aqueous solution of a transition metal salt and a chelating agent. In other words, it is preferred to prepare an aqueous solution containing a transition metal and glycine. In the aqueous solution containing a transition metal and glycine, the glycine concentration is preferably 0.05 mol / L or more and 0.15 mol / L or less, and more preferably 0.07 mol / L or more and 0.12 mol / L or less.
[0337] By using a chelating agent, the generation of unwanted nuclei can be suppressed, thus a hydroxide with good particle size distribution can be obtained. In addition, by using a chelating agent, acid-base reaction can be slowed down, reaction is gradually carried out, thus a spherical secondary particle can be obtained. Therefore, the chelating agent is more preferably a general complexing agent, for example, an ammonia solution.
[0338] Furthermore, in Fig. 9 In step S201, a complexing agent, specifically a chelating agent, may also be prepared. Preferably, the complexing agent, specifically a chelating agent, is placed in the reaction tank. When distinguishing from a complexing agent or a chelating agent mixed in an aqueous solution in which a transition metal salt is dissolved, an ordinal number is sometimes added to the complexing agent or the chelating agent. The materials that can be used for the complexing agent or the chelating agent are as described above. In the case of preparing a glycine aqueous solution as a chelating agent, the glycine concentration in the glycine aqueous solution is preferably greater than 0.05 mol / L and less than 0.15 mol / L, and more preferably greater than 0.07 mol / L and less than 0.12 mol / L. The glycine concentration in the glycine aqueous solution is preferably equal to the glycine concentration mixed in an aqueous solution in which a transition metal salt is dissolved.
[0339] Then, the steps after step S203 are performed in the same manner as in the manufacturing method 1.
[0340] Here, refer to Fig.10 The coprecipitation synthesis device 170 used for the present manufacturing method 2 is described. The coprecipitation synthesis device 170 can be arranged in a ventilation chamber, and it includes at least a reaction tank 171. The reaction tank 171 can use a reaction vessel. The bottom of the reaction vessel preferably uses a detachable flask, and the top preferably uses a detachable lid. The detachable flask can be cylindrical or circular. When a cylindrical shape is adopted, the detachable flask is flat-bottomed. The detachable lid includes multiple introduction ports, for example, includes four introduction ports.
[0341] The atmosphere in the reaction tank 171 can be controlled using at least one of the inlets in the detachable cover. For example, the atmosphere preferably contains nitrogen. In this case, it is preferably controlled in a manner that nitrogen flows through the reaction tank 171. At this time, the gas flow rate is preferably the amount required to discharge the gas generated by the thermal decomposition reaction. Furthermore, nitrogen can also be bubbled in the aqueous solution 203 placed in the reaction tank 171. The coprecipitation synthesis device 170 can also include a reflux cooler connected to other inlets in the detachable cover, through which the atmospheric gas such as nitrogen in the reaction tank 171 can be discharged, and water can be returned to the reaction tank 171.
[0342] The above-mentioned chelating agent is placed as the aqueous solution 203. Note that the aqueous solution placed in the reaction tank 171 from the beginning, such as the aqueous solution 203, is sometimes referred to as a pre-filled solution. The pre-filled solution is sometimes referred to as an adjustment solution. The pre-filled solution and the adjustment solution refer to the aqueous solution before the reaction, that is, the aqueous solution in the initial state.
[0343] As the aqueous solution 201, an aqueous solution in which a transition metal salt is dissolved is prepared. The aqueous solution 201 is placed in the first tank 180. As the aqueous solution 202, an alkaline aqueous solution is prepared. Since the alkaline aqueous solution is used to maintain the pH value at a fixed value, it is sometimes referred to as a pH adjusting solution. The aqueous solution 202 is placed in the second tank 186. It is preferred that nitrogen is bubbled in the first tank 180 and the second tank 186 to remove oxygen in each aqueous solution. Furthermore, a tank different from the first tank 180 and the second tank 186 may be prepared and the above-mentioned chelating agent may be placed therein.
[0344] The first tank 180 includes a pump 182 and a tube 181 connected to the pump 182, the tube 181 is fixed to the inlet of the detachable cover, and the aqueous solution 201 can drip from the top of the tube 181 to the reaction tank 171. In addition, the second tank 186 includes a pump 188 and a tube 187 connected to the pump 188, the tube 187 is fixed to the inlet of the detachable cover, and the aqueous solution 202 drips from the top of the tube 187 to the reaction tank 171. The tops of the tubes 181 and 187 can also be immersed in the aqueous solution 203, in which case it is also recorded that the aqueous solution 201 and the aqueous solution 202 drip into the reaction tank 171. In this way, according to step S201, each raw material is prepared in the reaction tank 171, the first tank 180 and the second tank 186.
[0345] <Step S203: Mixing process> Next, the mixing process of step S203 will be described. First, the conditions of the coprecipitation method in this step will be described.
[0346] <Conditions of coprecipitation method> The pH value of the aqueous solution 203 in the reaction tank 171 is 9.0 or more and 13.0 or less, preferably 10.5 or more and 11.5 or less. The temperature of the aqueous solution 203 in the reaction tank 171 is 40°C or more and 90°C or less, preferably 45°C or more and 70°C or less. The water temperature can be managed according to the temperature in the reaction tank 171. The temperature in the reaction tank 171 is sometimes equal to or differs from the above-mentioned water temperature by 5°C, preferably within 2°C. Therefore, the temperature in the reaction tank 171 is set to 35°C or more and 95°C or less, preferably 40°C or more and 75°C or less. The stirring rotation number of the aqueous solution 203 in the reaction tank 171 is 800rpm or more and 1200rpm or less, preferably 900rpm or more and 1100rpm or less. The concentration of transition metal ions in the aqueous solution 201 is 1mol / L or more and 5mol / L or less, preferably 2mol / L or more and 3mol / L or less. When multiple transition metals are included, the total concentration of the transition metal ions satisfies the above range. The dripping speed of aqueous solution 201 is more than 0.03mL / minute and less than 1.0mL / minute, preferably more than 0.03mL / minute and 0.5mL / minute. When the dripping speed is slow, the size of the hydroxide, i.e., the median particle size (D50), can be reduced, and when the dripping speed is fast, the size of the hydroxide, i.e., the median particle size (D50) can be increased. When the size of the hydroxide is small, the positive electrode active material also becomes smaller, and when the size of the hydroxide is large, the positive electrode active material also becomes larger. At this time, the hydroxide that has an influence on the size of the positive electrode active material as a lithium composite oxide can also be referred to as a precursor.
[0347] The alkali concentration of the aqueous solution 202 is 1 mol / L to 10 mol / L, preferably 3 mol / L to 7 mol / L. The chelating agent concentration of the aqueous solution 203 is 0.05 mol / L to 0.15 mol / L, preferably 0.07 mol / L to 0.12 mol / L.
[0348] Reference Fig.10 The structure of the coprecipitation synthesis device 170 that can obtain a coprecipitate under the above conditions will be described. Fig.10 The reaction tank 171 is provided with a stirring section 172. The stirring section 172 can stir the aqueous solution 203 in the reaction tank 171, and has a stirring motor 173 as a power source for rotating the stirring section 172. The stirring section 172 has a paddle-type stirring wing (referred to as a paddle wing), and the paddle wing has more than two and less than six wings, and the wing can also have an inclination of more than 40 degrees and less than 70 degrees. In the stirring section 172, the above-mentioned wing can also be moved up and down. In the mixing process of step S203, the number of rotations of the stirring section 172, specifically the number of rotations of the paddle wing is preferably more than 800rpm and less than 1200rpm, and more preferably more than 900rpm and less than 1100rpm. Although not shown in the figure, a baffle can also be provided in the reaction tank 171.
[0349] The temperature of the reaction pool 171 or the water temperature of the aqueous solution 203 is measured by the thermometer 174. The temperature of the reaction pool 171 can be controlled using a thermoelectric element so that the temperature of the aqueous solution 203 is kept constant. As a thermoelectric element, for example, a Peltier element can be cited. When measuring the water temperature of the aqueous solution 203, the top of the thermometer 174 is preferably immersed in the aqueous solution 203. In the mixing process of step S203, it is preferred that the temperature of the aqueous solution 203 is heated to a temperature of 40°C or more and 90°C or less, preferably 45°C or more and 70°C or less. In order to manage the water temperature of the aqueous solution 203, the temperature of the reaction pool 171 can also be managed using the thermometer 174.
[0350] In order to control the dropping conditions or stirring conditions of each pump, the coprecipitation synthesis device 170 includes a control device 190, etc. The control device 190 can control the number of rotations of the stirring part 172, the amount of dripping of each aqueous solution, etc. according to the information obtained from the thermometer 174. In the mixing process of step S203, for example, the dripping speed of the aqueous solution 201 is set to be above 0.05mL / min and below 1.0mL / min, preferably above 0.08mL / min and 0.5mL / min. The concentration of the transition metal ions in the aqueous solution 201 is preferably above 1mol / L and below 5mol / L, more preferably above 2mol / L and below 3mol / L. In the case of including multiple transition metals, the sum of the concentrations of each transition metal ion preferably satisfies the above range.
[0351] Although not shown, a pH meter is also disposed in the reaction tank 171 to measure the pH of the aqueous solution 203. In the mixing process of step S203, the pH value is preferably in the range of 9.0 to 13.0, more preferably in the range of 10.5 to 11.5. The concentration of the chelating agent in the aqueous solution 203 is preferably 0.05 mol / L to 0.15 mol / L, more preferably 0.07 mol / L to 0.12 mol / L.
[0352] When the pH value changes from a desired value, the aqueous solution 202 is added dropwise. The alkali concentration of the aqueous solution 202 is preferably 1 mol / L or more and 10 mol / L or less, and more preferably 3 mol / L or more and 7 mol / L or less.
[0353] After the mixing process of step S203, a reaction product is precipitated in the reaction tank 171. The reaction product is a coprecipitate, specifically, a hydroxide.
[0354] The subsequent steps, specifically, the steps after step S205 are the same as those in the manufacturing method 1, and thus the description thereof is omitted.
[0355] In this way, a positive electrode active material can be manufactured. In addition, by manufacturing method 2, NCM with good particle size distribution can be obtained as a positive electrode active material. When the obtained NCM is used, the discharge capacity of the battery characteristics is improved, so it is preferred. And, when the obtained NCM is used, the unevenness of the discharge capacity of the battery characteristics is suppressed, so it is preferred.
[0356] <Manufacturing method 3> In the present invention, the above-mentioned NCM may also have one or more selected from calcium and aluminum at a concentration of 0.1 atm% or more and 5 atm% or less. Calcium and aluminum at the above concentrations are sometimes recorded as added elements. In many cases, the added elements are located in the surface portion of the active material, and the surface portion refers to the area within 50 nm, preferably within 30 nm, and more preferably within 10 nm from the surface of the active material. Regardless of whether the active material is a primary particle or a secondary particle, the surface portion is located in the same position, and the area within 50 nm, preferably within 30 nm, and more preferably within 10 nm from the surface of the primary particle or the surface of the secondary particle is called the surface portion. Note that the surface of the primary particle or the surface of the secondary particle refers to the interface between the region where a transition metal (for example, Co, Ni, Mn, Fe, etc.) oxidized or reduced due to the insertion and removal of lithium exists and the region where such a transition metal does not exist.
[0357] The NCM containing aluminum as a main component may be referred to as NCMA. NCMA may be referred to as a lithium composite oxide containing Ni, Co, Mn, and Al.
[0358] In addition, a lithium composite oxide containing aluminum as a main component and containing Ni and Co may be referred to as NCA. NCA may be referred to as a lithium composite oxide containing Ni, Co, and Al.
[0359] In the present manufacturing method 3, refer to Fig.11 A case where the above-mentioned additional element source is added in the same step (ie, simultaneously) with the raw material prepared in step S201 will be described. Fig.11 Steps S203 to S213 of the manufacturing method 3 shown are the same as those of the manufacturing method 1, and step S215 is newly added.
[0360] <Step S215: Preparation for adding element source> exist Fig.11 In step S215, prepare an additive element source. As the additive element source, an aqueous solution of a salt in which the additive element source is dissolved can be used. As the aqueous solution, an aqueous solution in which aluminum sulfate, aluminum chloride, aluminum nitrate, calcium oxide, calcium carbonate, calcium hydroxide or calcium sulfate is dissolved can be used. The additive element source is weighed in such a way that the additive element is greater than 0.1 atm% and less than 5 atm% of the NCM. Multiple additive elements may be included. When multiple additive elements are included, the total concentration of the additive elements satisfies the requirement of being greater than 0.1 atm% and less than 5 atm% of the NCM.
[0361] <Step S203: Mixing process> exist Fig.11 In step S203 of the method, an aqueous solution containing a transition metal salt, an alkaline aqueous solution, and an aqueous solution containing a salt containing an additional element source are mixed to produce a mixed solution. The mixing in this step is the same as step S203 of the production method 1.
[0362] The subsequent steps, specifically, the steps after step S205 are the same as those in the manufacturing method 1, and thus the description thereof is omitted.
[0363] In this way, a positive electrode active material can be manufactured. In addition, by manufacturing method 3, NCM containing an added element can be obtained as a positive electrode active material. The added element is preferably located in the surface layer of NCM. By manufacturing method 3, NCMA or NCA can also be obtained as a positive electrode active material.
[0364] <Manufacturing method 4> In the present manufacturing method 4, refer to Fig.12 A case where the above-mentioned additional element source and the lithium source prepared in step S210 are added in the same step (ie, simultaneously) will be described. Fig.12 The steps S201 to S210 of the manufacturing method 4 shown are the same as those of the manufacturing method 1, and a step S215 is newly added. In addition, the order of the step S215 is different from that of the manufacturing method 3 described above.
[0365] <Step S215: Preparation for adding element source> exist Fig.12 In step S215, prepare an additive element source. As an additive element source, aluminum sulfate, aluminum chloride, aluminum nitrate, calcium oxide, calcium carbonate, calcium hydroxide or calcium sulfate can be used. The additive element source is weighed in such a way that the additive element is greater than 0.1 atm% and less than 5 atm% of the NCM. Multiple additive elements may be included. When multiple additive elements are included, the total concentration of the additive elements satisfies the requirement of being greater than 0.1 atm% and less than 5 atm% of the NCM.
[0366] <Step S211: Mixing process> exist Fig.12 In step S211 of the method, the hydroxide, the lithium source and the additive element source are mixed to produce a mixture. The mixing in this step is the same as step S211 of the manufacturing method 1.
[0367] The subsequent steps, specifically, the steps after step S213 are the same as those in the manufacturing method 1, and thus the description thereof is omitted.
[0368] In this way, a positive electrode active material can be manufactured. In addition, by manufacturing method 4, NCM containing an added element can be obtained as a positive electrode active material. The added element is preferably located in the surface layer of NCM. By manufacturing method 4, NCMA or NCA can also be obtained as a positive electrode active material.
[0369] <Manufacturing method 5> In the present manufacturing method 5, referring to Fig.13 The case where the above-mentioned additional element source is added after the heating process in step S213 is described. Fig.13 The steps S201 to S213 of the manufacturing method 5 shown are the same as those of the manufacturing method 1, and steps S215 to S217 are newly added. In addition, the order of step S215 is different from that of the manufacturing methods 3 and 4 described above.
[0370] <Step S215: Preparation for adding element source> exist Fig.13 In step S215, prepare an additive element source. As an additive element source, aluminum sulfate, aluminum chloride, aluminum nitrate, calcium oxide, calcium carbonate, calcium hydroxide or calcium sulfate can be used. The additive element source is weighed in such a way that the additive element is greater than 0.1 atm% and less than 5 atm% of the NCM. Multiple additive elements may be included. When multiple additive elements are included, the total concentration of the additive elements satisfies the requirement of being greater than 0.1 atm% and less than 5 atm% of the NCM.
[0371] <Step S216: Mixing process> exist Fig.13 In step S216 of the method, the composite oxide and the added element source are mixed to produce a mixture. The mixing in this step is the same as step S211 of the production method 1.
[0372] <Step S217: Heating process> exist Fig.13 In step S217, the mixture is heated. The heating in this step is the same as step S213 of manufacturing method 1.
[0373] In this way, a positive electrode active material can be manufactured. In addition, by manufacturing method 5, NCM containing an added element can be obtained as a positive electrode active material. The added element is preferably located in the surface layer of NCM. By manufacturing method 5, NCMA or NCA can also be obtained as a positive electrode active material.
[0374] This embodiment mode can be freely combined with other embodiment modes.
[0375] (Implementation 4) In this embodiment, the structure of the lithium ion battery other than the positive electrode active material and the electrolyte is described.
[0376] <Positive electrode 1> The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer contains a positive electrode active material and may further contain at least one of a conductive auxiliary agent and a binder. As the positive electrode active material, the material described in Embodiment 1 may also be used.
[0377] Fig.14A An example of a schematic diagram showing a cross section of a positive electrode is shown.
[0378] The current collector 550 may be, for example, a metal foil. The positive electrode may be formed by applying the slurry on the metal foil and drying it. Alternatively, the slurry may be pressed after drying. In the positive electrode, an active material layer is formed on the current collector 550 .
[0379] The slurry is a material liquid used to form an active material layer on the current collector 550, and contains an active material, a binder, and a solvent, and preferably also contains a conductive additive. The slurry is sometimes referred to as an electrode slurry or an active material slurry. Sometimes, a positive electrode slurry is used when forming a positive electrode active material layer, and sometimes, a negative electrode slurry is used when forming a negative electrode active material layer.
[0380] The positive electrode active material 561 has the function of absorbing lithium ions and / or releasing lithium ions with charge and discharge. As a positive electrode active material 561 used in one embodiment of the present invention, a material with less degradation accompanying charge and discharge even when a high charge voltage is used. In this specification, etc., in the absence of special instructions, the charge voltage is expressed as a reference to the potential of lithium metal. In this specification, etc., a high charge voltage refers to, for example, a charge voltage of 4.6V or more, preferably 4.65V or more, more preferably 4.7V or more, further preferably 4.75V or more, and most preferably 4.8V or more.
[0381] As the positive electrode active material 561 used in one embodiment of the present invention, any material can be used as long as it is a material that has little degradation accompanying charge and discharge even when a high charging voltage is used, and the materials described in Embodiment 1 or Embodiment 2 can be used. In addition, as long as the positive electrode active material 561 is a material that has little degradation accompanying charge and discharge even when a high charging voltage is used, two or more materials with different particle sizes can be used.
[0382] Conductive aids are also called conductive agents or conductive materials, and in many cases, carbon materials can be used. By attaching the conductive aid between multiple active materials, multiple active materials are electrically connected to each other and the conductivity is improved. Note that in this specification, "attachment" does not mean that the active material and the conductive aid are physically in close contact, but refers to the concept of including the following situations: when a covalent bond occurs; when bonded by van der Waals force; when the conductive material covers a part of the surface of the active material; when the conductive material is embedded in the surface unevenness of the active material; when they are electrically connected without contact, etc.
[0383] Specific examples of carbon materials that can be used as the conductive auxiliary agent include carbon black (furnace black, acetylene black, graphite, etc.).
[0384] Fig.14A Carbon black 553 is shown as a conductive auxiliary agent.
[0385] In order to fix the current collector 550 such as metal foil and the active material, the positive electrode of the lithium ion battery may also be mixed with an adhesive (resin). The adhesive is also called a binder. The adhesive is a polymer material. When a large amount of adhesive is included, the ratio of the active material in the positive electrode is reduced and the discharge capacity of the lithium ion battery is reduced. Therefore, it is preferred to mix the amount of adhesive to a minimum. Fig.14A In FIG. 5 , the region not filled with the positive electrode active material 561 , the second active material 562 , and the carbon black 553 refers to a gap or a binder.
[0386] Fig.14A The example in which the positive electrode active material 561 is spherical is shown, but there is no particular limitation on the shape. The cross-sectional shape of the positive electrode active material 561 may be, for example, an ellipse, a rectangle, a trapezoid, a cone, a polygon with an arcuate corner, or an asymmetric shape. For example, Fig. 14B An example is shown in which the positive electrode active material 561 has a polygonal shape with rounded corners.
[0387] In addition, Fig. 14B In the positive electrode, graphene 554 is used as a carbon material used as a conductive auxiliary agent. Fig. 14B In the embodiment, a positive electrode active material layer including a positive electrode active material 561 , graphene 554 , and carbon black 553 is formed on the current collector 550 .
[0388] Note that in the step of mixing the graphene 554 and the carbon black 553 to obtain the electrode slurry, the weight of the mixed carbon black is preferably 1.5 times or more and 20 times or less, and preferably 2 times or more and 9.5 times or less, that of the graphene.
[0389] When the mixing of graphene 554 and carbon black 553 is set within the above range, the dispersion stability of carbon black 553 is excellent when adjusting the slurry, and it is not easy to generate an aggregation part. In addition, when the mixing of graphene 554 and carbon black 553 is set within the above range, a high electrode density can be achieved compared with a positive electrode in which only carbon black 553 is used as a conductive auxiliary agent. By increasing the electrode density, the capacity per unit weight can be increased. Specifically, the density of the positive electrode active material layer measured by weight can be 3.5 g / cc or more.
[0390] Compared with the positive electrode using only graphene as a conductive aid, the electrode density is low, but the mixing of the first carbon material (graphene) and the second carbon material (acetylene black) is within the above range, thereby enabling correspondingly fast charging. Therefore, this is particularly effective when used for automotive lithium-ion batteries.
[0391] exist Fig. 14C , an example of a positive electrode using carbon fiber 555 instead of graphene is shown. Fig. 14C Shown with Fig. 14B Different example: By using carbon fiber 555, aggregation of carbon black 553 can be prevented and dispersibility can be improved.
[0392] Note that Fig. 14C In the figure, the region not filled with the positive electrode active material 561, the carbon fiber 555, and the carbon black 553 refers to a void or a binder.
[0393] Fig.14D Other examples of positive electrodes are shown. Fig. 14C An example is shown in which carbon fiber 555 is used instead of graphene 554. By using graphene 554 and carbon fiber 555, aggregation of carbon black such as carbon black 553 can be prevented, and thus dispersibility can be improved.
[0394] Note that Fig.14D In the figure, the region not filled with the positive electrode active material 561, the carbon fiber 555, the graphene 554, and the carbon black 553 refers to a gap or an adhesive.
[0395] Lithium-ion batteries can be manufactured by the following steps: FIG. 14A to FIG. 14D Any positive electrode in the above, a separator is stacked on the positive electrode, and a stacked body in which a negative electrode is stacked on the separator is placed in a container (an outer packaging body, a metal can, etc.) and the container is filled with an electrolyte.
[0396] <Positive Electrode 2> The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer contains a positive electrode active material and sometimes also contains a conductive material. In addition, the positive electrode active material layer sometimes also contains a binder. Moreover, the positive electrode active material layer sometimes contains a conductive material and a binder.
[0397] <Positive Electrode Active Material> Fig.15A An example of a positive electrode active material 10 is shown. As the positive electrode active material, for example, the material described in the above-mentioned embodiment 2 can be used. The positive electrode active material manufactured according to the embodiment 2 is composed of secondary particles 12 including primary particles 11. Sometimes, gaps 13 are confirmed between the aggregated primary particles 11. In addition, there is an interface 14 between adjacent primary particles 11.
[0398] [Distribution of added elements] The positive electrode active material produced by the production methods 3 to 5 of the above-mentioned embodiment 3 may contain an additional element. Fig. 15B Shown along Fig.15A The concentration distribution of the added element in the cross section of the dotted line EF. Since the cross section EF passes through the interface 14, Fig. 15B The concentration distribution of the added element from the interface 14 to the inside of the primary particle is shown. In this specification, the concentration distribution is sometimes referred to as a concentration gradient, and the vicinity of the interface refers to the area of the primary particle less than 10 nm from the interface, preferably the area of the primary particle less than 8 nm from the interface 14. Sometimes the area less than 10 nm from the interface of the primary particle is referred to as the surface layer of the primary particle.
[0399] Fig. 15B The horizontal axis corresponds to the distance of the EF section, and the vertical axis corresponds to the concentration of the added element. The concentration peak of the added element is preferably located at a position overlapping with the interface 14. Calcium can be cited as an example of an added element. The positive electrode active material containing the added element having the above-mentioned concentration peak is preferred because the cycle degradation is suppressed. In addition, when a plurality of added elements are used to manufacture the positive electrode active material, the concentration peak position sometimes differs depending on the added element.
[0400] In addition, in the primary particle 11, if Fig. 15B As shown in FIG. 1 , the concentration of the added element preferably decreases from the surface to the inside. That is, in the primary particle, the concentration of the added element in the surface layer is preferably higher than that in the inside. For example, Fig. 15B As shown, the concentration of calcium, which is an example of an additive element, preferably decreases from the surface to the inside. In addition, when a plurality of additive elements are used to produce a positive electrode active material, the shape of the concentration distribution may differ depending on the additive element.
[0401] [Cross-sectional view of positive electrode] Fig. 15C An example of a cross-sectional view of the positive electrode 107 is shown. The positive electrode 107 includes a positive electrode current collector 105 and a positive electrode active material layer 104 .
[0402] <Positive Electrode Current Collector> The positive electrode current collector 105 may be made of metal foil, for example. The positive electrode may be formed by applying the slurry on the metal foil and drying it. Alternatively, the slurry may be pressed after drying. In the positive electrode, the positive electrode active material layer 104 is formed on the positive electrode current collector 105 .
[0403] As metal foil, materials with high conductivity such as stainless steel, gold, platinum, aluminum, titanium and their alloys can be used. In addition, the material used for the positive electrode current collector is preferably not dissolved due to the potential of the positive electrode. In addition, aluminum alloys to which elements such as silicon, titanium, neodymium, scandium, molybdenum, etc. that improve heat resistance are added can be used. In addition, metal elements that react with silicon to form silicides can also be used. As metal elements that react with silicon to form silicides, there are zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, nickel, etc. As current collectors, foil, plate, sheet, mesh, punched metal mesh, drawn metal mesh and other shapes can be appropriately used. The thickness of the current collector is preferably 5 μm or more and 30 μm or less.
[0404] The slurry is a material liquid used to form the positive electrode active material layer 104 on the positive electrode current collector 105, and contains an active material, a binder and a solvent, and preferably also contains a conductive material. The slurry is sometimes referred to as an electrode slurry or an active material slurry. Sometimes, the positive electrode slurry is used when forming the positive electrode active material layer, and sometimes, it is referred to as the negative electrode slurry when forming the negative electrode active material layer.
[0405] The positive electrode active material layer 104 includes secondary particles 12a and secondary particles 12b as positive electrode active materials. The median diameter (D50) of the secondary particles 12a is different from that of the secondary particles 12b.
[0406] <Conductive Materials> Next, the conductive material is described. The conductive material is also called a conductive agent or a conductive auxiliary agent, and a carbon material can be used. By attaching the conductive material between multiple active materials, multiple active materials are electrically connected to each other and the conductivity is improved. Note that in this specification, "attachment" does not mean that the active material and the conductive material are physically in close contact, but refers to a concept including the following situations: when a covalent bond occurs; when bonded by van der Waals forces; when the conductive material covers a portion of the surface of the active material; when the conductive material is embedded in the surface unevenness of the active material; when they are electrically connected without contact, etc.
[0407] As specific examples of the carbon material that can be used as the conductive material, carbon black (furnace black, acetylene black, graphite, etc.), graphene, a graphene compound, or carbon fiber can be used.
[0408] [Graphene and graphene compounds] In this specification, graphene includes carbon, has a flat plate, a sheet, etc., and has a two-dimensional structure formed by a six-membered ring composed of carbon atoms, and includes multilayer graphene, multigraphene, etc. in addition to graphene. In addition, graphene can also be rolled into carbon nanofibers. In addition, graphene having a two-dimensional structure formed by a six-membered ring composed of carbon atoms can also be called a carbon sheet.
[0409] In this specification, the graphene compound has a flat plate shape, a sheet shape, etc., and includes graphene oxide, multilayer graphene oxide, multiple graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multiple graphene oxide, graphene quantum dots, etc. In addition, the graphene compound can also be curled up like a nanofiber. The graphene compound can also have a functional group, and as the functional group, an epoxy group, a carboxyl group, or a hydroxyl group is preferably used.
[0410] In this specification, etc., the reduced graphene oxide, the reduced multilayer graphene oxide, or the reduced multi-graphene oxide preferably has a portion having a carbon concentration greater than 80 atomic% and an oxygen concentration of 2 atomic% or more and 15 atomic% or less. By having such a carbon concentration and an oxygen concentration, a small amount of reduced graphene oxide can also function as a conductive material with high conductivity. In addition, it is preferred that the intensity ratio G / D of the G band to the D band in the Raman spectrum of the reduced graphene oxide, the reduced multilayer graphene oxide, or the reduced multi-graphene oxide is greater than 1. By having such an intensity ratio, a small amount of reduced graphene oxide can also function as a conductive material with high conductivity. Furthermore, by reducing graphene oxide, multilayer graphene oxide, or multi-graphene oxide, holes can sometimes be formed in the graphene compound.
[0411] Fig. 15C In the figure, carbon black 553 is shown as a conductive material. Since carbon black 553 is a microparticle, the carbon black 553 is aggregated in many cases. In addition, carbon black 553 can be located between secondary particles 12a and the like, and can be used as a current path between adjacent secondary particles 12a. Furthermore, carbon black 553 can be located between the positive electrode collector 105 and the secondary particles, and can be used as a current path between the positive electrode collector 105 and the secondary particles.
[0412] <Adhesive> The positive electrode of the lithium ion battery may also be mixed with a binder (resin) in order to fix the positive electrode current collector 105 and the active material. The binder is also called a bonding agent.
[0413] As the binder, for example, preferably used are rubber materials such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, and ethylene-propylene-diene copolymer. Fluorine rubber may also be used as the binder.
[0414] In addition, as the binder, for example, a water-soluble polymer is preferably used. As the water-soluble polymer, for example, polysaccharides can be used. As the polysaccharide, one or more of cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, regenerated cellulose, and starch can be used. It is more preferred to use these water-soluble polymers and the above-mentioned rubber material in combination.
[0415] As the binder, a plurality of the above-mentioned materials may be used in combination.
[0416] For example, materials with particularly good viscosity regulating effects can also be used in combination with other materials. For example, although rubber materials and the like have high cohesive force and / or high elasticity, it is sometimes difficult to regulate viscosity when mixed in a solvent. In such a case, for example, it is preferably mixed with materials with particularly good viscosity regulating effects. As materials with particularly good viscosity regulating effects, for example, water-soluble polymers can be used. In addition, as water-soluble polymers with particularly good viscosity regulating functions, the above-mentioned polysaccharides can be used, for example, cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, regenerated cellulose, or starch can be used.
[0417] The binder is a polymer material, and when a large amount of the binder is contained, the ratio of the active material in the positive electrode or the negative electrode decreases, and the discharge capacity of the lithium ion battery decreases. Therefore, it is preferable to mix the binder in a minimum amount.
[0418] Note that Fig. 15C In the embodiment, although the secondary particles 12a and 12b are spherical (circular in cross section), there is no particular limitation thereto. In many cases, projections and depressions as a part of the primary particles are confirmed on the surface of the cross section of the secondary particles where the primary particles are aggregated.
[0419] As another example, Fig.15D A positive electrode using carbon black 553 and graphene 554 as carbon materials used as conductive materials is shown. Note that in the step of mixing graphene 554 and carbon black 553 to obtain electrode slurry, it is preferred that the weight of the mixed carbon black is 1.5 times or more and 20 times or less, and preferably 2 times or more and 9.5 times or less, that of the graphene.
[0420] When the mixing of graphene 554 and carbon black 553 is set within the above range, the dispersion stability of carbon black 553 is excellent when adjusting the slurry, so it is preferred. In addition, when the mixing of graphene 554 and carbon black 553 is set within the above range, a high electrode density can be achieved compared to a positive electrode using only carbon black 553 as a conductive material. By increasing the electrode density, the capacity per unit weight can be increased. Specifically, the density of the positive electrode active material layer measured by weight can be 3.5 g / cc or more.
[0421] Compared with a positive electrode using only graphene as a conductive material, the electrode density is low, but the mixing of graphene 554 and carbon black 553 within the above range allows for relatively fast charging. Therefore, mixing graphene 554 and carbon black 553 is effective in manufacturing a lithium-ion battery for a vehicle.
[0422] Although not shown, carbon fiber (carbon nanotube) may be used instead of the graphene. By using carbon fiber as the conductive material, aggregation of the carbon black 553 can be prevented.
[0423] Lithium-ion batteries can be manufactured by the following steps: Fig. 15C and Fig.15D A positive electrode is stacked on the positive electrode, and a negative electrode is stacked on the separator, and the stacked body is placed in a container (an outer package, a metal can, etc.) and filled with an electrolyte. Fig. 15C and Fig.15D In the embodiment, the electrolyte is impregnated in the void area.
[0424] <Negative electrode> The negative electrode includes a negative electrode active material layer and a negative electrode current collector. In addition, the negative electrode active material layer may also include a negative electrode active material and further include a conductive material and a binder.
[0425] <Negative Electrode Active Material> As the negative electrode active material, for example, an alloy-based material and / or a carbon-based material can be used.
[0426] As the negative electrode active material, an element that can perform a charge and discharge reaction by alloying / de-alloying reaction with lithium can be used. For example, one or more materials selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium and indium can be used. The capacity of this element is higher than that of carbon, and in particular, the theoretical capacity of silicon is high, which is 4200mAh / g. Therefore, silicon is preferably used for the negative electrode active material. In addition, compounds containing these elements can also be used. For example, SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb and SbSn can be cited. Here, an element capable of performing a charge-discharge reaction through an alloying / de-alloying reaction with lithium, a compound containing the element, and the like are sometimes referred to as an alloy-based material.
[0427] In this specification, "SiO" refers to silicon monoxide, for example. Alternatively, SiO may also be represented as SiO x Here, x preferably represents a value of 1 or a value close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.
[0428] As the carbon material, one or more selected from graphite, easily graphitizable carbon (soft carbon), hardly graphitizable carbon (hard carbon), carbon fiber (carbon nanotube), graphene, carbon black, and the like can be used.
[0429] As graphite, artificial graphite or natural graphite can be cited. As artificial graphite, for example, mesocarbon microbeads (MCMB), coke-based artificial graphite, pitch-based artificial graphite, etc. can be cited. Here, spherical graphite with a spherical shape can be used as artificial graphite. For example, MCMB sometimes has a spherical shape, so it is preferred. In addition, MCMB is relatively easy to reduce its surface area, so it is sometimes preferred. As natural graphite, for example, flaky graphite, spheroidized natural graphite, etc. can be cited.
[0430] When lithium ions are intercalated in graphite (when lithium-graphite intercalation compounds are generated), graphite shows a potential as low as that of lithium metal (0.05 V or more and 0.3 V or less vs. Li / Li + ). As a result, lithium-ion batteries using graphite can show high operating voltages. Graphite also has the following advantages: large capacity per unit volume; relatively small volume expansion; relatively cheap; and higher safety than lithium metal, so it is preferred.
[0431] In addition, as the negative electrode active material, titanium dioxide (TiO2), lithium titanium composite oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5), tungsten dioxide (WO2), molybdenum dioxide (MoO2), etc., one or more oxides thereof.
[0432] In addition, as the negative electrode active material, Li 3N type structure containing lithium and transition metal nitride can be used. 3-x M x N (M = Co, Ni, Cu). For example, Li 2.6 Co 0.4 N shows a large discharge capacity (900 mAh / g (unit weight of negative electrode active material), 1890 mAh / cm 3 ), so it is preferred.
[0433] When a nitride containing lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so it can be combined with a material that does not contain lithium ions, such as V2O5 and Cr3O8, which is used as a positive electrode active material, and is therefore preferred. Note that when a material containing lithium ions is used as a positive electrode active material, a nitride containing lithium and a transition metal can also be used as a negative electrode active material by previously removing the lithium ions contained in the positive electrode active material.
[0434] In addition, materials that cause conversion reactions can also be used as negative electrode active materials. For example, transition metal oxides that do not form alloys with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can be used as negative electrode active materials. Oxides such as Fe2O3, CuO, Cu2O, RuO2, Cr2O3, CoS 0.89 Sulfides such as NiS, CuS, nitrides such as Zn3N2, Cu3N, Ge3N4, phosphides such as NiP2, FeP2, CoP3, and fluorides such as FeF3 and BiF3 also cause conversion reactions.
[0435] As the conductive material and the binder which may be contained in the negative electrode active material layer, the same conductive material and the binder which may be contained in the positive electrode active material layer may be used.
[0436] <Negative Electrode Current Collector> As the negative electrode current collector, copper or the like may be used in addition to the same materials as the positive electrode current collector. In addition, as the negative electrode current collector, it is preferable to use a material that does not alloy with carrier ions such as lithium.
[0437] [Electrolytes] As the electrolyte, the electrolyte described in Embodiment 1 and the like can be used.
[0438] [Isolated Body] When the electrolyte includes an electrolyte solution, a separator is arranged between the positive electrode and the negative electrode. As a separator, for example, the following materials can be used: paper and other cellulose fibers, non-woven fabrics, glass fibers, ceramics, or synthetic fibers containing nylon (polyamide), vinylon (polyvinyl alcohol fibers), polypropylene (denoted as PP), polyimide (denoted as PI), polyester, acrylic resin, polyolefin, polyurethane, etc. The porosity of the thickness of the separator can be greater than 35% and less than 90%, preferably greater than 60% and less than 85%. The porosity of the separator using polypropylene can be greater than 35% and less than 45%. The porosity of the separator using polyimide can be greater than 75% and less than 85%. The thickness of the separator is preferably greater than 10μm and less than 80μm, more preferably greater than 20μm and less than 60μm. The separator using polyimide can have a high porosity and can achieve thick film (typical thickness is greater than 50μm and less than 60μm), so it is preferred.
[0439] The separator is preferably processed into a bag shape and arranged so as to surround either the positive electrode or the negative electrode.
[0440] The separator may have a multilayer structure. For example, a ceramic material, a fluorine material, a polyamide material or a mixture thereof may be coated on a thin film of an organic material such as polypropylene or polyethylene. As a ceramic material, for example, aluminum oxide particles or silicon oxide particles may be used. As a fluorine material, for example, PVDF or polytetrafluoroethylene may be used. As a polyamide material, for example, nylon or aromatic polyamide (meta-aramid or para-aramid) may be used.
[0441] By adopting a separator with a multilayer structure, the safety of the lithium ion battery can be ensured even if the total thickness of the separator is small, and thus the capacity per unit volume of the lithium ion battery can be increased.
[0442] [Outer packaging] As the outer packaging body included in the lithium ion battery, for example, a metal material such as aluminum or a resin material can be used. In addition, a film-shaped outer packaging body can also be used. As the film, for example, a three-layer film can be used: a metal film with excellent flexibility such as aluminum, stainless steel, copper, nickel, etc. is arranged on a film composed of materials such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and an insulating synthetic resin film such as polyamide resin, polyester resin, etc. can also be arranged on the metal film as the outer surface of the outer packaging body.
[0443] <<Evaluation Conditions>> Whether or not the electrolyte of one embodiment of the present invention is contained can be determined by manufacturing a coin battery (for example, CR2032 type, 20 mm in diameter, 3.2 mm in height) containing lithium metal as a counter electrode and charging and discharging the battery under predetermined conditions.
[0444] <<Evaluation Steps>> A lithium-ion battery was disassembled, the positive electrode impregnated with electrolyte was taken out, and the positive electrode was analyzed by nuclear magnetic resonance (eg 1 H NMR) is used to measure the electrolyte and at least identify the organic solvent. The mixing ratio (volume ratio) of the organic solvent can also be identified by the nuclear magnetic resonance method. In addition, the lithium salt, additives, etc. contained in the electrolyte can also be identified.
[0445] Then, the positive electrode is punched into the size of a coin battery. The positive electrode contains a conductive material and a binder in addition to the positive electrode active material. In addition, the electrolyte is removed after the measurement of the nuclear magnetic resonance method and before the positive electrode is punched. For example, the positive electrode can also be washed with an organic solvent after taking out the positive electrode.
[0446] The coin cell contains lithium metal as a counter electrode. Alternatively, a material other than lithium metal may be used as the counter electrode.
[0447] In the coin battery, an electrolyte specified by nuclear magnetic resonance is prepared as an electrolyte. This electrolyte is an electrolyte of one embodiment of the present invention.
[0448] The coin cell includes a polypropylene porous film having a thickness of 25 μm as a separator.
[0449] In the coin battery, stainless steel (SUS) is used as the positive electrode can and stainless steel (SUS) is used as the negative electrode can.
[0450] In this manner, a coin battery for evaluation was prepared.
[0451] The evaluation coin cell manufactured under the above conditions is charged to an arbitrary voltage (for example, 4.4 V, 4.5 V, or 4.6 V) and then discharged. The charging conditions can refer to the following examples, etc. In addition, the discharging conditions can refer to the following examples, etc.
[0452] The temperature during charging of the evaluation coin battery can be set to 25° C. or below freezing point, and thereby the ratio of the charge / discharge capacity below freezing point to the charge / discharge capacity at 25° C. can be confirmed.
[0453] This embodiment mode can be used in combination with other embodiment modes.
[0454] (Implementation method 5) In this embodiment, an example of one form of a lithium ion battery is described.
[0455] [Laminated lithium-ion battery] Fig.16A and Fig. 16B An example of one embodiment of the laminated lithium ion battery 100 is shown. Fig.16A and Fig. 16B 16 is an external view, and the lithium ion battery 100 includes the electrolyte and separator (not shown in FIG. 16 ) described in the above embodiment, the negative electrode 106, and the positive electrode 107. In the lithium ion battery 100, the negative electrode 106 preferably has a larger area than the positive electrode 107. Furthermore, the lithium ion battery 100 includes a negative electrode lead electrode 510 electrically connected to the negative electrode 106 and a positive electrode lead electrode 511 electrically connected to the positive electrode 107. The electrolyte, the negative electrode 106, and the positive electrode 107 are accommodated in an outer package 509, and a portion of the negative electrode lead electrode 510 and a portion of the positive electrode lead electrode 511 protrude from the outer package 509. A bonding region 508 is provided at a portion of the outer periphery of the outer package 509. Fig.16A An example of a mode in which the negative lead electrode 510 and the positive lead electrode 511 protrude from the same side of the outer package 509 is shown, and the bonding area 508 is located at least on the side where each lead electrode protrudes and two sides adjacent to the side. Fig. 16B The example of a mode in which the side of the negative lead electrode 510 protruding from the outer package 509 and the side of the positive lead electrode 511 protruding from the outer package 509 are opposite to each other is shown, and the bonding area 508 is located at least on the two sides protruding from each lead electrode and one side sandwiched between the two sides. Fig.16A and Fig. 16B In the embodiment, the side where the adhesive region 508 is not provided preferably corresponds to the side where the outer packaging body 509 is folded.
[0456] When the organic solvent and the positive electrode active material of the present invention are used in the laminated lithium ion battery 100, excellent charge and discharge characteristics can be expected in a wide temperature range from below freezing to high temperatures.
[0457] [Coin-type lithium-ion battery] An example of a coin-type lithium-ion battery will be described. Fig.17A This is an exploded perspective view of a coin-type (single-layer flat) lithium-ion battery. Fig. 17B This is its appearance picture. Fig. 17C Coin-type lithium-ion batteries are mainly used in small electronic devices. In this specification, etc., coin-type lithium-ion batteries include button-type lithium-ion batteries.
[0458] In order to easily understand the overlapping relationship (upper and lower relationship and position relationship) of components, Fig.17A A schematic diagram is used. Therefore, Fig.17A Not with Fig. 17B Exactly the same picture.
[0459] exist Fig.17A In the embodiment, the positive electrode 304, the negative electrode 307, the spacer 342 and the gasket 332 are overlapped, and the negative electrode can 302 and the positive electrode can 301 are used to seal the above components. Fig.17A The electrolyte and separator described in the above embodiment are not shown. The spacer 342 and the gasket 332 are used to protect the inside or fix the position in the tank when the positive electrode tank 301 and the negative electrode tank 302 are pressed together. The spacer 342 and the gasket 332 are made of stainless steel or an insulating material.
[0460] A stacked structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 is referred to as a positive electrode 304 .
[0461] Fig. 17B It is a perspective view of the manufactured coin-type lithium-ion battery 100 .
[0462] In the coin-type lithium ion battery 100, the positive electrode can 301 also serving as the positive terminal and the negative electrode can 302 also serving as the negative terminal may be insulated and sealed by a gasket 303 formed of polypropylene or the like. The positive electrode 304 is formed of a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode. In addition, the negative electrode 307 is formed of a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0463] In the positive electrode 304 and the negative electrode 307 used in the coin-type lithium ion battery 100 , the active material layer may be formed on one surface respectively.
[0464] like Fig. 17C As shown, the positive electrode can 301 is placed at the bottom, the positive electrode 304, the negative electrode 307 and the negative electrode can 302 are stacked in order, and the positive electrode can 301 and the negative electrode can 302 are press-fitted with the gasket 303 interposed therebetween to manufacture the coin-type lithium ion battery 100.
[0465] When the organic solvent and the positive electrode active material of the present invention are used in the coin-type lithium ion battery 100, it can be expected that the battery will have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperatures.
[0466] [Cylindrical lithium-ion battery] Reference Fig.18A The following describes an example of a cylindrical lithium-ion battery. Fig.18A As shown, the top surface of the cylindrical lithium ion battery 616 includes a positive electrode cover (battery cover) 601, and the side and bottom surfaces thereof include a battery can (outer can) 602. The positive electrode cover 601 and the battery can (outer can) 602 are insulated by a gasket (insulating gasket) 610.
[0467] Fig.18B It is a diagram schematically showing a cross section of a cylindrical lithium ion battery. Fig.18B The cylindrical lithium ion battery shown has a positive electrode cover (battery cover) 601 on the top surface and a battery can (outer can) 602 on the side and bottom surfaces. The positive electrode cover and the battery can (outer can) 602 are insulated by a gasket (insulating gasket) 610.
[0468] A battery element is provided inside a hollow cylindrical battery can 602, in which a strip-shaped positive electrode 604 and a strip-shaped negative electrode 606 are wound with a separator 605 sandwiched therebetween. Although not shown in the figure, the battery element is wound around the central axis. One end of the battery can 602 is closed and the other end is open. Inside the battery can 602, the battery element in which the positive electrode, the negative electrode, and the separator are wound is sandwiched by a pair of opposing insulating plates 608 and insulating plates 609. In addition, an electrolyte (not shown) of one embodiment of the present invention is injected into the interior of the battery can 602 in which the battery element is provided.
[0469] Since the positive electrode and negative electrode used in the cylindrical storage battery are wound, it is preferable that the active material is formed on both sides of the current collector. 18A to 18D The lithium ion battery 616 is shown in which the height of the cylinder is greater than the diameter of the cylinder, but the present invention is not limited thereto. Alternatively, a lithium ion battery in which the diameter of the cylinder is greater than the height of the cylinder may be used. By adopting the above structure, for example, the lithium ion battery can be miniaturized.
[0470] The positive electrode 604 is connected to the positive terminal (positive electrode current collecting wire) 603, and the negative electrode 606 is connected to the negative terminal (negative electrode current collecting wire) 607. Metal materials such as aluminum can be used for both the positive terminal 603 and the negative terminal 607. The positive terminal 603 is resistance welded to the safety valve mechanism 613, and the negative terminal 607 is resistance welded to the bottom of the battery can 602. The safety valve mechanism 613 and the positive electrode cover 601 are electrically connected through a PTC (Positive Temperature Coefficient) element 611. When the internal pressure of the battery rises to exceed a specified threshold, the safety valve mechanism 613 cuts off the electrical connection between the positive electrode cover 601 and the positive electrode 604. In addition, the PTC element 611 is a thermally sensitive resistance element whose resistance increases when the temperature rises, and limits the current by increasing the resistance to prevent abnormal heating. As a PTC element, a barium titanate (BaTiO3) type ceramic material or the like can be used.
[0471] Fig. 18C An example of a power storage system 615 is shown. The power storage system 615 includes a plurality of lithium ion batteries 616, which is sometimes referred to as a battery pack. The positive electrode of each lithium ion battery contacts a conductor 624 separated by an insulator 625, and the positive electrodes are electrically connected to each other. The conductor 624 is electrically connected to a control circuit 620 via a wiring 623. In addition, the negative electrode of each lithium ion battery is electrically connected to the control circuit 620 via a wiring 626. As the control circuit 620, a protection circuit for preventing overcharge or overdischarge or the like can be used.
[0472] Fig.18D An example of a power storage system 615 is shown. The power storage system 615 includes a plurality of lithium-ion batteries 616, and the plurality of lithium-ion batteries 616 are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of lithium-ion batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 through a wiring 627. The plurality of lithium-ion batteries 616 can be connected in parallel, connected in series, or connected in parallel and then in series. By configuring the power storage system 615 including the plurality of lithium-ion batteries 616, a large amount of electric power can be obtained.
[0473] A plurality of lithium-ion batteries 616 may be connected in parallel and then in series.
[0474] In addition, a temperature control device may be included between the plurality of lithium-ion batteries 616. When the lithium-ion battery 616 is overheated, it can be cooled by the temperature control device, and when the lithium-ion battery 616 is overcooled, it can be heated by the temperature control device. Therefore, the performance of the power storage system 615 is not easily affected by the external temperature.
[0475] In addition, Fig.18D In FIG. 6 , the power storage system 615 is electrically connected to the control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of lithium ion batteries 616 via the conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of lithium ion batteries 616 via the conductive plate 614.
[0476] When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in the cylindrical lithium ion battery 100 , it can be expected that the battery will have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperatures.
[0477] [Other structural examples of lithium-ion batteries] An example of the structure of a lithium ion battery will be described using FIG. 19 and FIG. 20 .
[0478] Fig.19A The lithium ion battery 913 shown includes a winding body 950 provided with a terminal 951 and a terminal 952 inside a frame 930. The winding body 950 is impregnated with an electrolyte of one embodiment of the present invention inside the frame 930. The terminal 952 is in contact with the frame 930, and the terminal 951 is prevented from contacting the frame 930 by an insulating material. Note that for convenience, although Fig.19A Frame 930 is shown separately in the figure, but in reality, winding body 950 is covered by frame 930, and terminals 951 and 952 extend outside frame 930. Frame 930 can be made of a metal material (such as aluminum) or a resin material.
[0479] In addition, if Fig.19B As shown, multiple materials can also be used to form Fig.19A For example, in the frame 930 shown in FIG. Fig.19B In the illustrated lithium ion battery 913 , a frame body 930 a and a frame body 930 b are bonded together, and a wound body 950 is provided in a region surrounded by the frame bodies 930 a and 930 b .
[0480] As the frame 930a, an insulating material such as an organic resin can be used. In particular, by using a material such as an organic resin to form the surface of the antenna, it is possible to suppress the shielding of the electric field by the lithium ion battery 913. In addition, if the electric field shielding caused by the frame 930a is small, the antenna can be provided inside the frame 930a. As the frame 930b, for example, a metal material can be used.
[0481] Furthermore, Fig.19C The structure of the wound body 950 is shown. The wound body 950 includes a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is formed by overlapping the negative electrode 931 and the positive electrode 932 with the separator 933 interposed therebetween to form a laminated sheet, and then winding the laminated sheet. In addition, a plurality of layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.
[0482] Alternatively, you can use FIG. 20A to FIG. 20C A lithium-ion battery 913 including a jellyroll 950a is shown. Fig. 20A The wound body 950a shown includes a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 includes a negative electrode active material layer 931a. The positive electrode 932 includes a positive electrode active material layer 932a.
[0483] The separator 933 is wider than the negative electrode active material layer 931a and the positive electrode active material layer 932a, and the electrolyte layer 933 is wound so as to overlap with the negative electrode active material layer 931a and the positive electrode active material layer 932a. In addition, from the viewpoint of safety, it is preferable that the width of the negative electrode active material layer 931a is wider than the positive electrode active material layer 932a. In addition, the winding body 950a of the above shape is good in safety and productivity, so it is preferred.
[0484] like Fig. 20B As shown, the negative electrode 931 is electrically connected to the terminal 951. The terminal 951 is electrically connected to the terminal 911a. In addition, the positive electrode 932 is electrically connected to the terminal 952. The terminal 952 is electrically connected to the terminal 911b.
[0485] like Fig. 20C As shown, the wound body 950a is covered by the frame 930 to form a lithium ion battery 913. The frame 930 is preferably provided with a safety valve, an overcurrent protection element, etc. The safety valve is a valve that is opened at a specified internal pressure in the frame 930 to prevent battery rupture.
[0486] like Fig. 20B As shown, the lithium-ion battery 913 may also include a plurality of winding bodies 950a. By using a plurality of winding bodies 950a, a lithium-ion battery 913 with a larger charge and discharge capacity can be realized. Fig. 20A and Fig. 20B The other components of the lithium-ion battery 913 shown can be referred to FIG. 19A to FIG. 19C The lithium ion battery 913 is shown.
[0487] When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in the lithium ion battery 913 including the wound body, excellent charge and discharge characteristics can be expected in a wide temperature range from below freezing to high temperatures.
[0488] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.
[0489] (Implementation method 6) In this embodiment, an example of application to an electric vehicle (EV) will be described using FIG. 21 .
[0490] like Fig.21A As shown, in the electric vehicle, first batteries 1301a and 1301b are provided as lithium-ion batteries for main driving, and a second battery 1311 for supplying power to an inverter 1312 for starting an engine 1304. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used for the first batteries 1301a and 1301b, it can be expected that the battery has excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0491] The second battery 1311 is also called a cranking battery (also called a starting battery). The second battery 1311 only needs to have a high output and does not necessarily need to have a high capacity. In addition, the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.
[0492] The internal structure of the first battery 1301a may be either a winding type or a stacked type. In addition, the first battery 1301a may also use the all-solid-state battery of embodiment 5. By using the all-solid-state battery of embodiment 5 as the first battery 1301a, a high capacity can be achieved, safety is improved, and miniaturization and lightness can be achieved.
[0493] In this embodiment, an example of connecting the first batteries 1301a and 1301b in parallel is shown, but more than three batteries may be connected in parallel. In addition, as long as sufficient power can be stored in the first battery 1301a, the first battery 1301b may not be provided. By forming a battery pack with a plurality of lithium-ion batteries, a large amount of power can be taken out. A plurality of lithium-ion batteries may be connected in parallel, in series, or in series after being connected in parallel. Sometimes a plurality of lithium-ion batteries are referred to as a battery pack.
[0494] In order to cut off the power from the plurality of lithium-ion batteries, the vehicle-mounted lithium-ion battery includes a charging plug or a circuit breaker that can cut off the high voltage without using a tool, which is provided in the first battery 1301a.
[0495] In addition, the power of the first battery 1301a, 1301b is mainly used to rotate the engine 1304, and also supplies power to the 42V system vehicle components (electric power steering system 1307, heater 1308, defogger 1309, etc.) through the DCDC circuit 1306. In the case where the rear wheels include a rear engine 1317, the first battery 1301a is used to rotate the rear engine 1317.
[0496] Furthermore, the second battery 1311 supplies power to 14V system vehicle-mounted components (audio 1313 , power windows 1314 , lights 1315 , etc.) via the DCDC circuit 1310 .
[0497] In addition, use Fig.21B The first battery 1301a is described.
[0498] Fig.21B An example of using nine rectangular lithium-ion batteries 1300 as a battery pack 1415 is shown. In addition, the nine rectangular lithium-ion batteries 1300 are connected in series and one electrode is fixed using a fixing portion 1413 formed of an insulator and the other electrode is fixed using a fixing portion 1414 formed of an insulator. In this embodiment, an example of fixing using fixing portions 1413 and 1414 is shown, but it can also be stored in a battery storage box (also referred to as a frame). Assuming that the vehicle is subjected to vibration or shaking from the outside (road surface, etc.), it is preferable to use fixing portions 1413, 1414 and a battery storage box to fix multiple lithium-ion batteries. In addition, one electrode is electrically connected to the control circuit unit 1320 via wiring 1421. The other electrode is electrically connected to the control circuit unit 1320 via wiring 1422.
[0499] Alternatively, a memory circuit including a transistor using an oxide semiconductor may be used as the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor is sometimes referred to as a BTOS (Battery operating system or Battery oxide semiconductor).
[0500] It is preferred to use a metal oxide used as an oxide semiconductor. For example, as an oxide, it is preferred to use a metal oxide such as In-M-Zn oxide (element M is selected from one or more of aluminum, gallium, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten and magnesium). In particular, the In-M-Zn oxide that can be applied to the oxide is preferably CAAC-OS (C-Axis Aligned Crystal Oxide Semiconductor) or CAC-OS (Cloud-Aligned Composite Oxide Semiconductor). In addition, In-Ga oxide and In-Zn oxide can also be used as oxides. CAAC-OS is an oxide semiconductor including a plurality of crystalline regions, and the c-axis of the plurality of crystalline regions is oriented in a specific direction. In addition, the specific direction refers to the thickness direction of the CAAC-OS film, the normal direction of the formed surface of the CAAC-OS film, or the normal direction of the surface of the CAAC-OS film. In addition, the crystalline region is a region having a periodicity of atomic arrangement. Note that when the atomic arrangement is regarded as a lattice arrangement, the crystalline region is also a region with a consistent lattice arrangement. Furthermore, CAAC-OS has a region where multiple crystalline regions are connected in the ab plane direction, and sometimes the region has distortion. In addition, distortion refers to a portion where the direction of the lattice arrangement changes between a region with a consistent lattice arrangement and other regions with a consistent lattice arrangement in a region where multiple crystalline regions are connected. In other words, CAAC-OS refers to an oxide semiconductor that is oriented along the c-axis and has no obvious orientation in the ab plane direction. In addition, CAC-OS refers to, for example, a composition in which elements contained in a metal oxide are unevenly distributed, wherein the size of the material containing the unevenly distributed elements is greater than 0.5Nm and less than 10nm, preferably greater than 1nm and less than 3nm or a similar size. Note that the state in which one or more metal elements are unevenly distributed in a metal oxide and the regions containing the metal elements are mixed is also referred to as a mosaic or patch shape below, and the size of the region is greater than 0.5Nm and less than 10nm, preferably greater than 1nm and less than 3nm or a similar size.
[0501] In addition, the control circuit unit 1320 preferably uses a transistor containing an oxide semiconductor because the transistor can be used in a low temperature environment. In order to simplify the process, the control circuit unit 1320 can also be formed using a unipolar transistor. The operating ambient temperature range of the transistor containing an oxide semiconductor in the semiconductor layer is larger than that of single crystal Si, that is, above -40°C and below 150°C, and the characteristic change of the lithium-ion battery when heated is smaller than that of the single crystal. The off-state current of the transistor containing an oxide semiconductor is independent of the temperature and is below the lower limit of measurement at 150°C, but the temperature dependence of the off-state current characteristics of the single crystal Si transistor is large. For example, at 150°C, the off-state current of the single crystal Si transistor increases, and the current switching ratio does not become sufficiently large. The control circuit unit 1320 can improve safety.
[0502] The control circuit unit 1320 using a storage circuit including a transistor using an oxide semiconductor can also be used as an automatic control device for lithium-ion batteries for the causes of instability caused by ten conditions such as micro-short circuits. As functions for solving the causes of instability caused by the ten conditions, there can be cited prevention of overcharging, prevention of overcurrent, control of overheating during charging, cell balancing in a battery pack, prevention of overdischarge, a capacity meter, automatic control of charging voltage and current according to temperature, control of charging current according to the degree of degradation, detection of abnormal behavior of micro-short circuits, prediction of abnormalities regarding micro-short circuits, etc. The control circuit unit 1320 has at least one of the above functions. In addition, ultra-miniaturization of the automatic control device for lithium-ion batteries can be achieved.
[0503] In addition, micro short circuit refers to a very small short circuit inside a lithium-ion battery. One of the reasons for micro short circuit is believed to be that multiple charge and discharge cycles cause uneven distribution of the positive electrode active material, local current concentration occurs in part of the positive electrode and part of the negative electrode, or side reactions produce side reaction products, leading to micro short circuit.
[0504] In addition to micro short circuits, the control circuit unit 1320 detects the terminal voltage of the lithium-ion battery and manages the charging and discharging state of the lithium-ion battery. For example, to prevent overcharging, both the output transistor of the charging circuit and the blocking switch can be turned off at almost the same time.
[0505] in addition, Fig. 21C Show Fig.21B An example of a block diagram of a battery pack 1415 is shown.
[0506] The control circuit unit 1320 includes: a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging; a control circuit 1322 for controlling the switch unit 1324; and a voltage measuring unit for the first battery 1301a. In the control circuit unit 1320, the upper limit voltage and the lower limit voltage of the lithium ion battery used are set to control the upper limit of the current flowing from the outside and the upper limit of the output current flowing to the outside. The range above the lower limit voltage and below the upper limit voltage of the lithium ion battery is the recommended voltage range. When the voltage is outside this range, the switch unit 1324 functions and serves as a protection circuit. In addition, the control circuit unit 1320 controls the switch unit 1324 to prevent overdischarge and overcharge, so it can also be called a protection circuit. For example, when the control circuit 1322 detects a voltage that will become overcharge, the current is shielded by closing the switch of the switch unit 1324. In addition, the function of shielding the current according to the increase in temperature can also be set by setting a PTC element in the charge and discharge path. In addition, the control circuit unit 1320 includes an external terminal 1325 (+IN) and an external terminal 1326 (−IN).
[0507] The switch portion 1324 may be formed by combining an n-channel transistor and a p-channel transistor. In addition to switches including Si transistors using single crystal silicon, for example, Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenic), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaO x The switch section 1324 is composed of a power transistor such as an OS transistor (gallium oxide; x is a real number greater than 0). In addition, the storage element using the OS transistor can be freely configured by stacking it on a circuit using a Si transistor, so it is easy to achieve integration. By stacking the control circuit section 1320 using the OS transistor on the switch section 1324 for integration, the switch section 1324 and the control circuit section 1320 can be integrated into one chip, so miniaturization can be achieved.
[0508] The first battery 1301a and 1301b mainly supply power to the on-board equipment of the 42V system (high voltage system), while the second battery 1311 supplies power to the on-board equipment of the 14V system (low voltage system). In many cases, the second battery 1311 adopts a lead-acid battery because of cost advantages. Although there is an advantage of no maintenance when a lithium-ion secondary battery is used as the second battery 1311, an abnormality that cannot be distinguished during manufacturing may occur during a long period of use, such as more than three years. In particular, in order to prevent the situation in which the second battery 1311 of the starting inverter cannot work and the engine cannot be started even if the first battery 1301a and 1301b have residual capacity, when the second battery 1311 is a lead-acid battery, power is supplied from the first battery to the second battery to charge in a manner that always maintains a fully charged state.
[0509] This embodiment shows an example of using lithium ion batteries for both the first battery 1301a and the second battery 1311, but a lead acid battery, an all-solid-state battery, or an electric double layer capacitor may also be used for the second battery 1311. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in the above-mentioned lithium ion battery, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0510] In addition, the regenerative energy caused by the rotation of the tire 1316 is transmitted to the engine 1304 through the transmission 1305, and is charged to the second battery 1311 from the engine controller 1303 and the battery controller 1302 through the control circuit unit 1321. In addition, the first battery 1301a is charged from the battery controller 1302 through the control circuit unit 1320. In addition, the first battery 1301b is charged from the battery controller 1302 through the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is preferred that the first batteries 1301a and 1301b can be charged at a high speed.
[0511] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b, etc. The battery controller 1302 sets the charging conditions according to the charging characteristics of the lithium-ion battery used to perform high-speed charging.
[0512] In addition, although not shown in the figure, when connected to an external charger, the socket of the charger or the connecting cable of the charger is electrically connected to the battery controller 1302. The power supplied from the external charger is charged to the first battery 1301a, 1301b through the battery controller 1302. In addition, some chargers are provided with a control circuit without using the function of the battery controller 1302, but in order to prevent overcharging, it is preferred to charge the first battery 1301a, 1301b through the control circuit unit 1320. In addition, sometimes the connecting cable or the connecting cable of the charger is provided with a control circuit. The control circuit unit 1320 is sometimes referred to as an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. In addition, the ECU includes a microcomputer. In addition, the ECU uses a CPU or a GPU.
[0513] As external chargers installed in charging stations, there are 100V outlets, 200V outlets, three-phase 200V and 50kW outlets, etc. In addition, charging can also be performed by supplying power from an external charging device using a contactless power supply method.
[0514] Next, an example in which a lithium ion battery as one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.
[0515] In addition, lithium-ion batteries can be installed in hybrid vehicles (HV), electric vehicles (EV) or plug-in hybrid vehicles (PHV) and other new generation clean energy vehicles. In addition, lithium-ion batteries can also be installed in agricultural machinery, electric bicycles including electric-assisted bicycles, motorcycles, electric wheelchairs, electric karts, small or large ships, submarines, fixed-wing aircraft and rotary-wing aircraft, rockets, artificial satellites, space probes, planetary probes, spacecraft and other transportation vehicles.
[0516] FIG. 22A to FIG. 22D A transport vehicle using one embodiment of the present invention is shown. Fig.22A The car 2001 shown is an electric car using an electric motor as a power source for traveling. Alternatively, the car 2001 is a hybrid car that can appropriately select an electric motor and an engine as a power source for traveling. When the lithium-ion battery is installed in the vehicle, the example of the lithium-ion battery shown in the above embodiment can be set in one or more parts. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used for the lithium-ion battery installed in the vehicle, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0517] Fig.22A The automobile 2001 shown includes a battery pack 2200, which includes a battery module in which a plurality of lithium-ion batteries are connected. In addition, the battery pack 2200 preferably further includes a charge control device electrically connected to the battery module.
[0518] In addition, in the automobile 2001, the lithium-ion battery of the automobile 2001 can be charged by supplying power from an external charging device using a plug-in method and a contactless power supply method. When charging, the charging method and the specifications of the connector can be appropriately performed according to the methods specified by CHAdeMO (a registered trademark in Japan) or the combined charging system "Combined Charging System". As a lithium-ion battery, a charging station set up in a commercial facility or a home power supply can also be used. For example, by supplying power from the outside using plug-in technology, the power storage device installed in the automobile 2001 can be charged. Charging can be performed by converting AC power into DC power using a conversion device such as an ACDC converter.
[0519] In addition, although not shown in the figure, the power receiving device can also be installed in the vehicle and the power can be supplied non-contactly from the power transmission device on the ground for charging. When the non-contact power supply method is used, by assembling the power transmission device in the road or the outer wall, charging can be performed not only when the vehicle is parked but also when it is driving. In addition, the non-contact power supply method can also be used to send and receive power between two vehicles. Furthermore, solar cells can be installed on the outside of the vehicle to charge the lithium-ion battery when it is parked or driving. Such non-contact power supply can be achieved using electromagnetic induction and magnetic field resonance.
[0520] exist Fig. 22B In the diagram, a large transport vehicle 2002 including an electrically controlled engine is shown as an example of a transport vehicle. The battery module of the transport vehicle 2002 is, for example, a battery module having a maximum voltage of 170V, in which four lithium-ion batteries with a nominal voltage of 3.0V or more and 5.0V or less are connected in series. The battery pack 2201 has the same characteristics as the battery pack 2201 except for the number of lithium-ion batteries. Fig.21B When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in the lithium ion battery of the battery pack 2201, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0521] exist Fig. 22C 2 shows a large transport vehicle 2003 including an electrically controlled engine as an example. The battery module of the transport vehicle 2003 is, for example, a battery module having a maximum voltage of 600V and in which more than 100 lithium-ion batteries with a nominal voltage of 3.0V or more and 5.0V or less are connected in series. In addition, the battery pack 2202 has the same configuration as the battery module except for the number of lithium-ion batteries constituting the battery module. Fig. 22B The same functions are omitted for explanation. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in a lithium ion battery included in a module, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperatures.
[0522] exist Fig.22D , an aircraft 2004 equipped with an engine burning fuel is shown as an example. Fig.22D The aircraft 2004 shown includes wheels for taking off and landing, so it can be said that the aircraft 2004 is a part of a transportation vehicle. In the aircraft 2004, multiple lithium-ion batteries are connected to form a battery module and include a battery pack 2203 having a battery module and a charging control device.
[0523] The battery module of the aircraft 2004 has, for example, eight 4V lithium-ion batteries connected in series and having a maximum voltage of 32V. In addition to the number of lithium-ion batteries constituting the battery module of the battery pack 2203, the battery module has the same Fig.21B The functions are the same, so the description is omitted.
[0524] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.
[0525] (Implementation 7) In this embodiment, an example in which a lithium ion battery according to one embodiment of the present invention is mounted on a vehicle such as a two-wheeled vehicle or a bicycle is described.
[0526] Fig.23A An example of an electric bicycle using a lithium ion battery according to one embodiment of the present invention is shown. Fig.23A The lithium ion battery of one embodiment of the present invention can be used in the electric bicycle 8700 shown in the figure. The lithium ion battery of one embodiment of the present invention may also include a protection circuit.
[0527] The electric bicycle 8700 includes a power storage device 8702. The power storage device 8702 supplies power to a motor that assists the rider. In addition, the power storage device 8702 is portable. Fig. 23B The power storage device 8702 taken out of the bicycle is shown. The power storage device 8702 has a plurality of lithium ion batteries 8701 of one embodiment of the present invention built therein, and the remaining power can be displayed on the display unit 8703. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used for the lithium ion battery 8701, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0528] In addition, the power storage device 8702 includes the control circuit 8704 capable of performing charging control or abnormality detection of the lithium ion battery as shown in Embodiment 7. The control circuit 8704 is electrically connected to the positive electrode and the negative electrode of the lithium ion battery 8701. This greatly contributes to reducing accidents such as fires caused by lithium ion batteries.
[0529] Fig.23C This is an example of a two-wheeled vehicle using the lithium ion battery of one embodiment of the present invention. Fig.23C The illustrated scooter 8600 includes a power storage device 8602, a side mirror 8601, and a turn signal lamp 8603. The power storage device 8602 can supply power to the turn signal lamp 8603. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in a lithium ion battery, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0530] exist Fig.23C In the illustrated scooter 8600, the power storage device 8602 can be stored in the under-seat storage section 8604. Even if the under-seat storage section 8604 is small, the power storage device 8602 can be stored in the under-seat storage section 8604.
[0531] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.
[0532] (Implementation 8) In this embodiment, an example of installing a lithium ion battery of one embodiment of the present invention in an electronic device is described. As an electronic device equipped with a lithium ion battery, for example, a television device (also referred to as a television or a television receiver), a display for a computer, a digital camera, a digital video camera, a digital photo frame, a mobile phone (also referred to as a mobile phone, a mobile phone device), a portable game console, a portable information terminal, a sound reproduction device, a large game console such as a pinball machine, etc. can be cited. As a portable information terminal, a notebook personal computer, a tablet terminal, an electronic book terminal, a mobile phone, etc. can be cited.
[0533] Fig.24A An example of a mobile phone is shown. The mobile phone 2100 includes an operation button 2103, an external connection port 2104, a speaker 2105, a microphone 2106, etc. in addition to a display unit 2102 installed in a housing 2101. In addition, the mobile phone 2100 includes a lithium ion battery 2107. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in a lithium ion battery, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0534] The mobile phone 2100 can execute various application programs such as mobile phone, e-mail, article reading and writing, music playing, Internet communication, computer games, etc.
[0535] The operation button 2103 may have various functions in addition to time setting, such as power switch, wireless communication switch, silent mode setting and cancellation, power saving mode setting and cancellation, etc. For example, by using the operating system incorporated in the mobile phone 2100, the function of the operation button 2103 can be freely set.
[0536] In addition, the mobile phone 2100 can perform short-range wireless communication standardized by the communication. For example, by communicating with a headset capable of wireless communication, a hands-free call can be made.
[0537] In addition, the mobile phone 2100 has an external connection port 2104, and data can be directly sent to or received from other information terminals through a connector. In addition, charging can also be performed through the external connection port 2104. In addition, the charging operation can also be performed using wireless power supply without using the external connection port 2104.
[0538] The mobile phone 2100 preferably includes a sensor. For example, a fingerprint sensor, a pulse sensor, a human body sensor such as a temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, etc. are preferably installed as the sensor.
[0539] Fig. 24B An unmanned aerial vehicle 2300 including a plurality of rotors 2302 is shown. The unmanned aerial vehicle 2300 is also referred to as a drone. The unmanned aerial vehicle 2300 includes a lithium ion battery 2301 of one embodiment of the present invention, a camera 2303, and an antenna (not shown). The unmanned aerial vehicle 2300 can be remotely operated via the antenna. When the electrolyte and the positive electrode active material of one embodiment of the present invention are used in a lithium ion battery, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0540] Fig.24C An example of a robot is shown. Fig.24C The robot 6400 shown includes a lithium-ion battery 6409, an illumination sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a moving mechanism 6408, a computing device, and the like.
[0541] The microphone 6402 has a function of detecting the user's voice and surrounding sounds, etc. In addition, the speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user through the microphone 6402 and the speaker 6404.
[0542] The display unit 6405 has the function of displaying various information. The robot 6400 can display the information required by the user on the display unit 6405. The display unit 6405 can also be equipped with a touch panel. In addition, the display unit 6405 can be a detachable information terminal, and by setting it at a fixed position of the robot 6400, it can be charged and send and receive data.
[0543] The upper camera 6403 and the lower camera 6406 have the function of photographing the surrounding environment of the robot 6400. In addition, the obstacle sensor 6407 can detect whether there is an obstacle in the direction of the robot 6400 when it moves forward using the moving mechanism 6408. The robot 6400 can confirm the surrounding environment using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407 and move safely.
[0544] The internal area of the robot 6400 is equipped with a lithium ion battery 6409 according to one embodiment of the present invention and a semiconductor device or an electronic component. When the electrolyte and positive electrode active material according to one embodiment of the present invention are used in a lithium ion battery, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0545] Fig.24D An example of a sweeping robot is shown. The sweeping robot 6300 includes a display unit 6302 disposed on the top surface of a frame 6301, a plurality of cameras 6303 disposed on the side, a brush 6304, an operation button 6305, a lithium-ion battery 6306, various sensors, etc. Although not shown in the figure, the sweeping robot 6300 also has wheels, a suction port, etc. The sweeping robot 6300 can walk by itself and can detect garbage 6310 and suck the garbage from the suction port disposed below.
[0546] For example, the sweeping robot 6300 can determine whether there are obstacles such as walls, furniture, or steps by analyzing the image taken by the camera 6303. In addition, when objects such as wires that may be entangled with the brush 6304 are found through image analysis, the rotation of the brush 6304 can be stopped. The internal area of the sweeping robot 6300 is equipped with a lithium ion battery 6306 and a semiconductor device or electronic component according to one embodiment of the present invention. When the electrolyte and positive electrode active material of one embodiment of the present invention are used in a lithium ion battery, it can be expected to have excellent charge and discharge characteristics in a wide temperature range from below freezing to high temperature.
[0547] This embodiment mode can be implemented in combination with other embodiment modes as appropriate.
[0548] (Implementation method 9) In this embodiment, an example in which a lithium ion battery according to one embodiment of the present invention is mounted on space equipment will be described.
[0549] Fig.25A As an example of a space device, an artificial satellite 6800 is shown. The artificial satellite 6800 includes a main body 6801, a solar panel 6802, an antenna 6803, and a lithium-ion battery 6805. A solar panel is sometimes referred to as a solar cell module.
[0550] When sunlight shines on the solar panel 6802, the power required for the artificial satellite 6800 to operate is generated. However, for example, when sunlight does not shine on the solar panel or when the amount of sunlight shining on the solar panel is small, the amount of power generated is reduced. Therefore, it is possible that the power required for the artificial satellite 6800 to operate will not be generated. In order to operate the artificial satellite 6800 even when the generated power is small, it is preferred to provide a lithium ion battery 6805 in the artificial satellite 6800. When the electro...
Claims
1. A lithium-ion battery comprising: a positive electrode comprising a positive electrode active material; as well as Electrolytes, The positive electrode active material comprises lithium cobalt oxide containing Mg, F, Ni and Al. Furthermore, the electrolyte includes a fluorinated cyclic carbonate and a fluorinated chain carbonate.
2. A lithium-ion battery comprising: a positive electrode comprising a positive electrode active material; as well as Electrolytes, The positive electrode active material comprises lithium cobalt oxide containing Mg, F, Ni and Al. Furthermore, the electrolyte includes fluoroethylene carbonate and methyl trifluoropropionate, and when the total content of the fluoroethylene carbonate and the methyl trifluoropropionate is 100 vol%, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is x:100-x (note, 5≤x≤30).
3. The lithium ion battery according to claim 1 or 2, The lithium cobalt oxide is composed of Li x CoO2 indicates that In the Li x When x in CoO2 is 1, the lithium cobalt oxide has a layered rock salt type crystal structure belonging to the space group R-3m. And in the Li x When x in CoO2 satisfies 0.1 < x ≤ 0.24, the lithium cobaltate has a crystal structure with space group P2 / m, lattice constant a = 0.488 ± 0.001 nm, lattice constant b = 0.282 ± 0.001 nm, lattice constant c = 0.484 ± 0.001 nm, α = 90°, β = 109.58 ± 0.01°, and γ = 90°.
4. The lithium ion battery according to claim 1 or 2, The lithium cobalt oxide is composed of Li x CoO2 indicates that In the Li x When x in CoO2 is 1, the lithium cobalt oxide has a layered rock salt type crystal structure belonging to the space group R-3m. And in the case of Li x When x in CoO2 satisfies 0.1 < x ≤ 0.24, in the case of analyzing the lithium cobaltate by X-ray diffraction, diffraction peaks are present at least at 2θ ≥ 19.37° and ≤ 19.57° and at 2θ ≥ 45.57° and ≤ 45.67°.
5. The lithium ion battery according to claim 1 or 2, The median particle size (D50) of the lithium cobalt oxide is greater than or equal to 10 μm and less than or equal to 14 μm.
6. The lithium ion battery according to claim 1 or 2, The median particle size (D50) of the lithium cobalt oxide is greater than or equal to 5 μm and less than or equal to 9 μm.
7. A lithium ion battery comprising: A positive electrode active material comprising lithium cobalt oxide containing Mg, F, Ni and Al; as well as An electrolyte comprising a fluorinated cyclic carbonate and a fluorinated chain carbonate, Among them, a half-cell including a positive electrode containing the positive electrode active material, the electrolyte and lithium metal for the counter electrode is prepared, the half-cell is configured at an ambient temperature of 25°C, and constant current charging is performed at a rate of 0.1C (note, 1C=200mA / g) until the voltage reaches 4.6V, and constant voltage charging is performed at 4.6V until the current value reaches 0.05C, and then constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V, thereby obtaining a discharge capacity value, and compared with the discharge capacity value, the discharge capacity value obtained by the following steps is 50% or more, that is, the half-cell is configured at an ambient temperature of 25°C, and constant current charging is performed at a rate of 0.1C (note, 1C=200mA / g) until the voltage reaches 4.6V, and constant voltage charging is performed at 4.6V until the current value reaches 0.05C, and then the half-cell is configured at an ambient temperature of -40°C and constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V.
8. A lithium ion battery comprising: A positive electrode having a positive electrode active material comprising lithium cobalt oxide containing Mg, F, Ni and Al; as well as Electrolytes, The positive electrode active material comprises lithium cobalt oxide containing Mg, F, Ni and Al. The electrolyte comprises fluoroethylene carbonate and methyl trifluoropropionate, and when the total content of the fluoroethylene carbonate and the methyl trifluoropropionate is 100 vol%, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is x:100-x (note, 5≤x≤30), In addition, a half-cell including a positive electrode containing the positive electrode active material, the electrolyte and lithium metal for the counter electrode is prepared, the half-cell is configured at an ambient temperature of 25°C, and constant current charging is performed at a rate of 0.1C (note, 1C=200mA / g) until the voltage reaches 4.6V, and constant voltage charging is performed at 4.6V until the current value reaches 0.05C, and then constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V, thereby obtaining a discharge capacity value, and compared with the discharge capacity value, the discharge capacity value obtained by the following steps is 50% or more, that is, the half-cell is configured at an ambient temperature of 25°C, and constant current charging is performed at a rate of 0.1C (note, 1C=200mA / g) until the voltage reaches 4.6V, and constant voltage charging is performed at 4.6V until the current value reaches 0.05C, and then the half-cell is configured at an ambient temperature of -40°C and constant current discharge is performed at a rate of 0.1C until the voltage reaches 2.5V.
9. A lithium ion battery comprising: A positive electrode active material comprising nickel, cobalt and manganese; as well as An electrolyte comprising a fluorinated cyclic carbonate and a fluorinated chain carbonate, In which, a half-cell including a positive electrode containing the positive electrode active material, the electrolyte and a lithium metal for the counter electrode is configured at an ambient temperature of 25°C, and is charged at a constant current rate of 0.1C (note, 1C = 200mA / g) until the voltage reaches 4.5V, and is charged at a constant voltage at 4.5V until the current value reaches 0.05C, and then the half-cell is configured at an ambient temperature of -40°C, and is discharged at a constant current rate of 0.1C until the voltage reaches 2.5V, thereby obtaining a discharge capacity value, which satisfies more than 50% of the discharge capacity value obtained by the following steps, that is, the half-cell is configured at an ambient temperature of 25°C, and is charged at a constant current rate of 0.1C (note, 1C = 200mA / g) until the voltage reaches 4.5V, and is charged at a constant voltage at 4.5V until the current value reaches 0.05C, and then is discharged at a constant current rate of 0.1C until the voltage reaches 2.5V.
10. A lithium ion battery comprising: A positive electrode active material comprising nickel, cobalt and manganese; as well as Electrolytes, Wherein, the electrolyte comprises fluoroethylene carbonate and methyl trifluoropropionate, and when the total content of the fluoroethylene carbonate and the methyl trifluoropropionate is 100 vol%, the volume ratio of the fluoroethylene carbonate to the methyl trifluoropropionate is x:100-x (note, 5≤x≤30), Furthermore, a half-cell including a positive electrode containing the positive electrode active material, the electrolyte and a lithium metal for the counter electrode is arranged at an ambient temperature of 25°C, and is charged at a constant current rate of 0.1C (note, 1C = 200mA / g) until the voltage reaches 4.5V, and is charged at a constant voltage at 4.5V until the current value reaches 0.05C, and then the half-cell is arranged at an ambient temperature of -40°C, and is discharged at a constant current rate of 0.1C until the voltage reaches 2.5V, thereby obtaining a discharge capacity value, which satisfies more than 50% of the discharge capacity value obtained by the following steps, that is, the half-cell is arranged at an ambient temperature of 25°C, and is charged at a constant current rate of 0.1C (note, 1C = 200mA / g) until the voltage reaches 4.5V, and is charged at a constant voltage at 4.5V until the current value reaches 0.05C, and then is discharged at a constant current rate of 0.1C until the voltage reaches 2.5V.
11. The lithium ion battery according to claim 9 or 10, In the positive electrode active material, the ratio of nickel:cobalt:manganese satisfies 8:1:1 or is close to it.
12. The lithium ion battery according to claim 9 or 10, In the positive electrode active material, the proportion of nickel is greater than the proportion of cobalt and the proportion of manganese.
13. The lithium ion battery according to claim 9 or 10, The median particle size (D50) of the positive electrode active material is 4 μm or more and 7 μm or less.
14. The lithium ion battery according to claim 9 or 10, The separator of the half-cell comprises polyimide.
15. The lithium ion battery according to claim 9 or 10, The separator of the half-cell comprises polypropylene.