Additive manufacturing powder with improved physical properties, method for the production thereof

By using spherical powder particles with a particle size distribution of 0 to 1000 micrometers and surface modification treatment, the problem of inconsistent powder flowability in additive manufacturing was solved, achieving stable flow and high packing density in high humidity environments, thereby improving the quality and production efficiency of finished parts.

CN118905220APending Publication Date: 2024-11-08TEKNA PLASMA SYST INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410891558.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-05-02
Filing Date
2020-05-01
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The inconsistent flowability of existing additive manufacturing powders in stereolithography processes leads to undesirable porosity, delamination, and incomplete melting, increasing scrap rates and reducing productivity. Existing solutions such as drying steps and surface modification methods have failed to effectively improve the flowability problem.

Method used

Spherical powder particles with a particle size distribution of about 0 micrometers to about 1000 micrometers are used. The hydrophilicity of the particles is reduced by plasma atomization and surface modification treatment, which increases the flowability and moisture resistance. An improved powder bed melt additive manufacturing method is used to improve the flowability and bulk density.

Benefits of technology

It achieves stable powder flowability and high packing density in high humidity environments, reduces defects, improves the surface finish and mechanical properties of finished parts, and reduces operating costs and production time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905220A_ABST
    Figure CN118905220A_ABST
Patent Text Reader

Abstract

In additive manufacturing operations, powder used in a stereolithography process needs to be precisely spread in a unified manner at each stage of the stereolithography process to ensure predictability of powder surface morphology. Typically, this is difficult to achieve by conventional powders, since these powders typically have poorer flowability that can further deteriorate over time, and impair the efficiency of stereolithography processes. The present disclosure describes additive manufacturing powders having improved physical properties, methods of manufacture thereof, and uses thereof, in particular additive manufacturing powders having improved physical properties such as flowability and tap density, which are less or insensitive to ambient humidity. For example, this application describes a powder comprising spherical particles having a particle size distribution of less than 1000 microns, and having a measurable flowability determined at 75% relative humidity according to ASTM B213.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This patent application is a divisional application of the patent application with application number 2020800410438, application date May 1, 2020, and invention name “Additive manufacturing powder with improved physical properties, its manufacturing method and its use”.

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 842,050, filed May 2, 2019. The contents of the above references are incorporated herein by reference in their entirety. Technical Field

[0004] The present application relates generally to the field of powder materials useful in additive manufacturing operations, and more particularly to additive manufacturing powders having improved physical properties, methods of making the same, and uses thereof. Background Art

[0005] In additive manufacturing operations, powders used in stereolithography processes need to be spread precisely and in a uniform manner at each stage of the stereolithography process to ensure predictable powder surface morphology.

[0006] Typically, this is difficult to achieve with conventional powders because fine powders exhibit inconsistent flow behavior and reduce the efficiency of the stereolithography process. For example, powders with poor flow properties reduce the efficiency of the powder rake (or "coater"), which translates into unpredictable powder surface morphology. Upon interaction with the laser, this can lead to undesirable porosity, delamination of stereolithography layers, and incomplete melting in the finished product. Such severe defects increase scrap rates because they render the finished part unusable, which increases manufacturing costs and reduces productivity. Furthermore, the unpredictability of such events has hindered the widespread dissemination of additive manufacturing technology because very large design safety factors are required to accommodate fluctuations in such properties, thereby losing the economic and performance advantages sought by adopting additive manufacturing in the process.

[0007] As particles become smaller, the relative effect of gravity on the particles becomes smaller, and the negligible cohesive forces become significant at large scales. Cohesive forces are critical because all forces contributing to cohesion and friction counteract gravity and reduce fluidity. Regarding cohesive forces, van der Waals interactions, polar interactions through local static charges and hydrogen bonds, and surface tension through adsorbed water are usually exemplified. Among these cohesive forces, static charge-mediated interactions in conductive powders are not a problem because all charge separations are immediately unconstrained as charges are freely reorganized in the conductor. Van der Waals interactions are inevitable when powders are to be processed at non-zero absolute temperatures.

[0008] Various solutions have been proposed to improve powder flowability.

[0009] For example, 3-D printing operators typically "reset" the powder state by drying the powder under the specific conditions of each operator to control the adsorbed water. Some powder manufacturers also include a drying step in their manufacturing process. However, this approach does not completely alleviate the problem because at each step of the method, the entire operation needs to be closely monitored to keep the powder away from moisture. In some environments, this is extremely difficult. Within the scope of ensuring quality, it is believed that this may be a major source of errors. In addition, the disadvantage of this known solution is that when the powder is exposed to the high temperatures required to remove water from the powder, it becomes a bottleneck in the production line, increases operating costs (e.g., electricity consumption) and increases the possibility of causing the presence of undesirable by-products. In addition, it is extremely difficult to remove adsorbed water from the surface of the powder particles, so that some residual water often remains, which still causes powder flowability problems.

[0010] U.S. Patent No. 8,894,739 and No. 7,943,084 teach that aluminum powder is impregnated into silane and alkane solution and slurried to produce a hydrophobic outer layer on the surface of the powder particles, thereby avoiding water adsorption on the particle surface. However, the thickness of the outer surface layer, the chemical composition of the powder and the nano-roughness are compromised because the chemical reaction between the metal aluminum powder and the solution can hardly be controlled. This method has not been successful, at least because the resulting particles tend to form secondary particles by agglomeration, which adversely affects the tap density of the powder. It is also worth noting that the slurrying method requires a large amount of solvent, which is contaminated by excess reactants (anhydrous methods use excess reactants). In addition, the powder needs to be physically separated from the solvent and dried, which is time-consuming and difficult in industrial-scale batch processing. In addition, most of these powders do not flow in the Hall test, which shows that there is still a problem with powder fluidity.

[0011] U.S. Patent No. 9,994,716 teaches dry mixing of powders with an effective amount of hydrophobic fumed silica to distribute a layer of hydrophobic fumed silica on the surface of the particles, thereby attempting to avoid water adsorption on the surface of the particles. This has not been successful, at least because additive manufacturing operators generally limit the presence of additives in powder materials (fumed silica is generally considered an undesirable additive) that may produce inclusions that are extremely detrimental to the mechanical properties of the reinforced parts. In addition, when the inclusions are placed in solution (e.g., by laser or electron beam melting), the chemical properties of the raw materials are changed. In view of the above, this proposed solution to the flowability problem has not yet been accepted by the market.

[0012] In view of the foregoing, there is a need to provide powders for additive manufacturing operations that mitigate at least some of the deficiencies of existing powders. Summary of the invention

[0013] This Summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key aspects or essential aspects of the claimed subject matter.

[0014] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm and a flowability of ≤ 20 s at 30% relative humidity determined according to ASTM B213.

[0015] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm and having a measurable flowability determined according to ASTM B213 at 75% relative humidity.

[0016] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, and having a first flowability determined at 30% relative humidity according to ASTM B213, and a second flowability determined at 75% relative humidity according to ASTM B213, wherein the ratio of the second flowability / first flowability is at least 0.90.

[0017] As embodied and generally described herein, the present disclosure relates to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, the PSD including a portion of fine particles having a size <20 μm containing up to 30 volume %, and a flowability of the powder determined at 30% relative humidity according to ASTM B213 of ≤40 s.

[0018] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, the PSD including a portion of fine particles having a size <20 μm content of up to 30 volume %, and the powder having a measurable flowability determined according to ASTM B213 at 75% relative humidity.

[0019] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, the PSD including a portion of fine particles having a size <20 μm containing up to 30% by volume, and the powder having a first flowability determined at 30% relative humidity according to ASTM B213, and a second flowability determined at 75% relative humidity according to ASTM B213, wherein the ratio of the second flowability / first flowability is at least 0.90.

[0020] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, wherein the particles have molecules attached to at least a portion of the surface of the particles that reduce the hydrophilicity of the powder, wherein the molecules that reduce the hydrophilicity of the powder are present in the powder in an amount less than 800 ppm.

[0021] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm and an apparent density of ≥ 2.440 g / cm2 at 30% relative humidity as determined according to ASTM B212. 3 .

[0022] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm and an apparent density of ≥ 2.400 g / cm2 at 75% relative humidity determined according to ASTM B212. 3 .

[0023] As embodied and generally described herein, the present disclosure is directed to an additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, and having a first apparent density determined at 30% relative humidity according to ASTM B212, and a second apparent density determined at 75% relative humidity according to ASTM B212, wherein the second apparent density shows a loss of ≤2% relative to the first apparent density.

[0024] As embodied and generally described herein, the present disclosure relates to a shipping container comprising additive manufacturing powder, the powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, wherein the shipping container includes a top layer of powder having a first D50, and a bottom layer of powder having a second D50, wherein the first D50>the second D50.

[0025] As embodied and generally described herein, the present disclosure is directed to a shipping container comprising additive manufacturing powder, the powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, wherein the powder in the shipping container forms a stratification along a longitudinal axis thereof, the stratification comprising a plurality of zones, wherein a D50 powder size of a first zone of the plurality of zones is different from a D50 powder size of a second zone of the plurality of zones.

[0026] As embodied and broadly described herein, the present disclosure is directed to an additively manufactured three-dimensional metal part, wherein the part includes a body having a surface perpendicular to a build plane of the part, the surface being characterized by Ra≤25 microns and / or Rz≤230 microns.

[0027] As embodied and broadly described herein, the present disclosure is directed to an additively manufactured three-dimensional metal component wherein the component includes a body having less than 5 ppm oxygen and a microstructure that is at least 95% free of porosity.

[0028] As embodied and generally described herein, the present disclosure relates to a method for obtaining an additive manufacturing powder, comprising providing a volume of spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, and attaching molecules to the surface of the particles to reduce the hydrophilicity of the particles to obtain an additive manufacturing powder, wherein the powder has a measurable flowability determined using ASTM B213 at 75% relative humidity.

[0029] As embodied and generally described herein, the present disclosure relates to a method for obtaining an additive manufacturing powder, comprising atomizing a feedstock with a plasma to obtain particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, contacting the particles with a reactive gas comprising a reagent and introducing the reagent into the surface of the particles, the reagent reducing the hydrophilicity of the particles, and the powder having a measurable flowability determined using ASTM B213 at 75% relative humidity.

[0030] As embodied and generally described herein, the present disclosure relates to a method for manufacturing a three-dimensional part, comprising providing a volume of plasma atomized spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, and attaching molecules to the surface of the particles to reduce the hydrophilicity of the particles to obtain an additive manufacturing powder, wherein the molecules that reduce the hydrophilicity of the powder are present in the powder in an amount of less than 800 ppm, and wherein the powder has a measurable flowability determined using ASTM B213 at 75% relative humidity.

[0031] As specifically implemented and generally described herein, the present disclosure relates to an apparatus for manufacturing three-dimensional parts, comprising a molten bed for supporting the part during the manufacturing process, a powder conveying system for supplying a continuous amount of powder to the molten bed, a unit for generating an energy beam to form layers of the part from powder layers, and a drainage system for discharging unsintered powder from the molten bed, the drainage system being configured to discharge powder having a fluidity ≤20s determined at 30% relative humidity according to ASTM B213.

[0032] As specifically embodied and generally described herein, the present disclosure relates to an apparatus for manufacturing a three-dimensional component, comprising a molten bed for supporting the component during the manufacturing process, a powder delivery system for supplying a continuous amount of powder to the molten bed, a unit for generating an energy beam to form a layer of the component from powder layers, and a recoated component configured to travel through the molten bed at a speed of at least 250 mm / s to produce a powder layer.

[0033] As specifically implemented and generally described herein, the present disclosure relates to a three-dimensional part manufactured by additive manufacturing, the part having a geometric structure, the three-dimensional part containing a metal material, wherein the three-dimensional part has an ultimate strength; and the ratio of the ultimate strength of the three-dimensional part to the ultimate strength of a conventionally manufactured part is at least 80%, wherein the conventionally manufactured part is different from the three-dimensional part, the geometric structure of the conventionally manufactured part is the same as the geometric structure of the three-dimensional part manufactured by additive manufacturing, and the metal material contained in the conventionally manufactured part is the same as the metal material of the three-dimensional part manufactured by additive manufacturing.

[0034] As specifically implemented and generally described herein, the present disclosure relates to a three-dimensional component manufactured by additive manufacturing, the three-dimensional component having a geometric structure, the three-dimensional component including a metal microstructure containing a metal material, wherein the ratio of the ultimate strength of the metal microstructure of the three-dimensional component to the ultimate strength of a bulk of the metal material is at least 80%.

[0035] As embodied and generally described herein, the present disclosure relates to a three-dimensional component manufactured by additive manufacturing, the three-dimensional component having a geometric structure, the three-dimensional component including a metal microstructure containing a metal material, wherein at 10 6 The maximum stress amplitude before fracture after 10 cycles is 10 times that of the bulk metal material. 6 The ratio of the maximum stress amplitude before fracture after 10 cycles is at least 80%.

[0036] As specifically implemented and generally described herein, the present disclosure relates to a three-dimensional component manufactured by additive manufacturing, the three-dimensional component having a geometric structure, the three-dimensional component including a metal microstructure containing a metal material, wherein the ratio of the tear elongation of the metal microstructure of the three-dimensional component to the tear elongation of the bulk of the metal material is at least 80%.

[0037] As specifically implemented and generally described herein, the present disclosure relates to a three-dimensional component manufactured by additive manufacturing, the three-dimensional component having a geometric structure, the three-dimensional component including a metal microstructure containing a metal material, wherein the ratio of the toughness of the metal microstructure of the three-dimensional component to the toughness of a bulk of the metal material is at least 80%.

[0038] As specifically implemented and generally described herein, the present disclosure relates to a powder for additive manufacturing, the powder comprising powder particles, the powder particles comprising a metal material having a certain density, the powder having a particle size distribution (PSD) of about 0 microns (μm) to about 1000 μm, and the powder having an apparent density, wherein the ratio of the apparent density of the powder to the minimum density of the metal material is at least 57.5%.

[0039] As embodied and generally described herein, the present disclosure is directed to a one-piece, integrally formed metal component manufactured by a powder bed fusion additive manufacturing method that uses a laser as a source of thermal energy to heat and melt selected areas of a metal powder bed to build the metal component in successive layers, the metal component including an interior cavity having a sidewall, and the interior cavity is in fluid communication with an exterior of the metal component via a channel, the sidewall having a portion configured to be inaccessible to a machining tool to preclude surface finishing of the portion by a machining tool from outside the metal component by a subtractive machining method, the portion having a surface finish characterized by a Ra of the metal powder. <D90。

[0040] As embodied and generally described herein, the present disclosure is directed to a one-piece, integrally formed metal component manufactured by a powder bed fusion additive manufacturing method that uses a laser as a source of thermal energy to heat and melt selected areas of a metal powder bed to build the metal component in successive layers. The metal component includes a surface having an inherent surface finish characterized by a Ra of the metal powder. <D90。

[0041] All features of the exemplary embodiments described in this disclosure and not mutually exclusive can be combined with each other. The elements of one embodiment can be used in other embodiments without further mention. By reading the following description of the specific embodiments in conjunction with the accompanying drawings, other aspects and features of the present invention will become apparent to those of ordinary skill in the art. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] A detailed description of specific exemplary embodiments is provided below with reference to the accompanying drawings, in which:

[0043] Figure 1 shows a non-limiting photograph of water droplets in contact with powder treated according to Example 3 according to an embodiment of the present disclosure;

[0044] Figure 2 shows a scanning electron microscope image of a powder according to an embodiment of the present disclosure;

[0045] Figure 3 A flow chart illustrating a manufacturing method for manufacturing a powder according to an embodiment of the present disclosure is shown;

[0046] Figure 4A and Figure 4B An example of a manufacturing apparatus for manufacturing atomized powder according to an embodiment of the present disclosure is shown;

[0047] FIG. 5A to FIG. 5C shows a non-limiting schematic diagram illustrating possible surface activation mechanisms in an inert gas plasma of a metal powder according to an embodiment of the present disclosure;

[0048] FIG. 6A to FIG. 6C shows a non-limiting schematic diagram illustrating a possible surface activation mechanism in an oxygen-containing plasma of a metal powder according to an embodiment of the present disclosure;

[0049] Figure 7 A non-limiting graph showing the flowability of prior art Ti-6Al-4Va powders made using different atomization techniques as a function of relative humidity (RH %);

[0050] FIG. 8A to FIG. 8D shows a non-limiting schematic diagram illustrating a possible attachment mechanism of an alkoxysilane to the surface of a metal powder according to an embodiment of the present disclosure;

[0051] Fig. 9 A non-limiting graph showing a comparison between the flowability of a comparative prior art powder ("original") as a function of relative humidity (RH%) and the flowability of a surface modified powder (53 / 20) as a function of relative humidity (RH%) according to embodiments of the present disclosure;

[0052] Fig.10 A non-limiting graph showing a comparison between the apparent density of a prior art powder ("original") and the apparent density of a surface modified powder at different RH (%) according to an embodiment of the present disclosure;

[0053] Fig.11A non-limiting graph showing a comparison of the behavior of a comparative prior art powder ("raw") and the behavior of a surface modified powder in a sieving test according to embodiments of the present disclosure;

[0054] Fig.12 A non-limiting graph showing the flowability of the surface modified powder according to Example 1 measured at different RH%;

[0055] Fig.13 A non-limiting graph showing the flowability of the surface modified powder according to Example 4 measured at different RH%;

[0056] Fig.14 A non-limiting graph showing the flowability of the surface modified powder according to Example 5 measured at different RH%;

[0057] Fig.15 A non-limiting graph showing the flowability of the surface modified powder according to Example 6 measured at different RH%;

[0058] Fig.16 A non-limiting graph showing the flowability of the surface modified powder according to Example 7 measured at different RH%;

[0059] Fig.17 A non-limiting graph showing the flowability of the surface modified powder according to Example 9 measured at different RH%;

[0060] Fig.18 A non-limiting graph showing the flowability of the surface modified powder according to Example 10 measured at different RH%;

[0061] Figures 19 to 24 The operation of an additive manufacturing apparatus according to an embodiment of the present disclosure is shown;

[0062] Fig.25A A diagram showing spreading of a powder layer comprising aggregates is shown;

[0063] Fig.25B The embodiment according to the present disclosure is shown Fig.25A Illustration of a relatively spread powder layer without aggregates;

[0064] Fig.26A A diagram showing the effects of defects in a powder layer before and after melting or sintering in an additive manufacturing operation;

[0065] Fig.26B The embodiment according to the present disclosure is shown Fig.26A A relatively defect-free powder layer before and after melting or sintering in an additive manufacturing operation;

[0066] Figures 27 to 31 Variations of the additive manufacturing apparatus are shown;

[0067] FIG. 32A to FIG. 32D shows surface details of an additively manufactured part made with a surface-modified powder according to an embodiment of the present disclosure;

[0068] FIG. 32E to FIG. 32H Surface details of an additively manufactured part made with comparative prior art powders are shown;

[0069] Fig.33 An example of the improvement in surface finish after the additive manufacturing process is shown. B1 and B2 are treated AlSi7Mg and AlSi10Mg, respectively. B2 and C2 are the same powders before treatment;

[0070] Fig.34 and Fig.35 A molten pool of molten material including powder is shown;

[0071] Fig.36 The separation of aggregates and impurities in the powder is shown;

[0072] Fig.37 An apparatus for assessing the purity of a powder and removing impurities and / or aggregates according to an embodiment of the present disclosure is shown;

[0073] Fig.38 A method of evaluating the purity of a powder and removing impurities and / or aggregates according to an embodiment of the present disclosure is shown;

[0074] Figures 39 to 46 A variation of an additive manufacturing apparatus according to an embodiment of the present disclosure is shown;

[0075] Fig.47 The yield strength (“YS”) and ultimate strength (“UTS”) along the X-axis, Y-axis, and Z-axis of two additively manufactured parts, including one additively manufactured part (labeled “ST”) manufactured with a surface-modified powder according to an embodiment of the present disclosure and one additively manufactured part (labeled “reg”) manufactured with a prior art powder having the same parameters, are shown;

[0076] Fig.48 Shown by Fig.47 The results obtained calculate the yield strength (“YS”) and ultimate strength (“UTS”) increments;

[0077] Figures 49 to 65 An example of a one-piece additively manufactured part manufactured using an embodiment of the powder of the present disclosure is shown, wherein the additively manufactured part includes a cavity defining an interior surface that is not accessible to a machining tool from outside the additively manufactured part;

[0078] Figure 65 to Figure 68 An example of a processing device of an additive manufacturing device according to an embodiment of the present disclosure is shown;

[0079] Fig.69 An example of a method of selecting a set of setting values ​​for operating an additive manufacturing apparatus according to an embodiment of the present disclosure is shown.

[0080] In the accompanying drawings, exemplary embodiments are shown by way of example. It should be clearly understood that the description and drawings are only for the purpose of illustrating certain embodiments and are intended to aid understanding. The description and drawings are not intended to define the limitations of the present invention. DETAILED DESCRIPTION

[0081] A detailed description of one or more embodiments of the present invention and drawings illustrating the principles of the present invention are provided below. The present invention is described in conjunction with these embodiments, but the present invention is not limited to any embodiment. The scope of the present invention is limited only by the claims. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. These details are provided for the purpose of non-limiting examples, and the present invention can be implemented according to the claims without some or all of these specific details. For the sake of clarity, technical materials known in the technical field related to the present invention are not described in detail, so as not to cause unnecessary obscurity of the present invention.

[0082] Additive manufacturing processes are typically operated with "fixed" parameters for specific applications, with existing equipment offering little opportunity for any form of response control. This means that inconsistent input material properties will translate directly into inconsistent finished part properties. Poor powder quality can produce defects in the final part, including holes, cracks, inclusions, residual stresses, and suboptimal surface roughness, and adversely affect yield. It should therefore be understood that the correlation between material properties, processing performance, and final component properties is critical to selecting the best powder for the application and ensuring the consistency of the powder (i.e., from component to component and from layer to layer), as well as recycling. The chemical and physical properties of metal powders are generally understood to define additive manufacturing performance.

[0083] In terms of chemistry, powders need to match the alloy composition of a specific material, and grades must be carefully selected to control the presence of interstitial elements such as oxygen or nitrogen, which can affect the properties of the finished part. In addition, powders must be free of contamination from foreign particles, such as from other material batches at the powder manufacturing plant or manufacturing facility, or debris from processing / recycling equipment. Contaminant levels of just a few parts per million can significantly affect component quality.

[0084] In addition to chemical effects, the physical characteristics of metal powders, such as the bulk properties of the powder and the properties of the individual metal particles, also affect the additive manufacturing process. The key bulk properties are packing density and flowability. Powders with consistently good packing and thus high density are associated with the manufacture of components with fewer defects and consistent quality. On the other hand, it can be argued that flowability is more closely related to process efficiency. For example, for powder bed fusion processes, the ability to spread evenly and smoothly on the bed and form a uniform layer without gas voids is essential, and directed energy deposition requires an aerated powder stream with consistent flowability under completely different conditions. These requirements increase with increasing processing speeds.

[0085] Both bulk density and flowability are directly (but not limited to) affected by particle size and shape. A range of particle properties known to affect flowability include, for example, hardness, porosity, surface texture, density, and electrostatic charge. In general, smooth, regularly shaped particles flow more easily than particles with rough surfaces and / or irregular shapes. Rougher surfaces lead to increased friction between particles, while irregularly shaped particles are more prone to mechanical interlocking; both effects reduce flowability.

[0086] Similarly, spherical particles tend to pack more efficiently than irregular particles, resulting in higher packing densities. Therefore, the packing powder property requirements for AM indicate that sphericity can be of great value, a conclusion widely accepted in the industry.

[0087] When reaching a certain particle size, metal powders used for additive manufacturing usually have particles with a size in the micrometer range, (for example) to meet the needs of forming a powder bed that is only tens of microns thick. However, smaller particle size powders can be problematic from a health and safety perspective and in terms of flowability. Because the attraction between particles increases as the particle size decreases, smaller sized powders are generally less free-flowing than their coarser analogs.

[0088] Surprisingly and unexpectedly, the present inventors, through extensive research and development work, have developed powders for additive manufacturing that have improved physical properties relative to comparative prior art powders.

[0089] These improved properties include, for example, the bulk properties of the powder and the properties of the individual metal particles.

[0090] In some embodiments, the improved physical properties of the powders of the present disclosure include improved static flowability as measured by a Hall flow meter (e.g., ASTM B213) and / or improved dynamic flowability (e.g., "avalanche angle") as measured by a revolution powder analyzer (RPA).

[0091] In some embodiments, the improved physical properties of the powders of the present disclosure provide greater tolerance to the presence of fine particles <20 microns in the powder particle size distribution (PSD). In other words, it is generally understood that powders for additive manufacturing can tolerate fine particles in their PSD up to a certain threshold, beyond which the powder properties will deteriorate. For example, at a level of 10% by volume, comparative prior art powders will generally exhibit significant disadvantages, such as reduced flowability; the chemical composition relative to BET will be too concentrated, which will cause artifacts when used for 3D laser printing; when the powder is poured, the fine particles create a cloud that plugs the filter inside the additive manufacturing device and causes laser attenuation; the fine particles increase the surface to volume ratio, which in turn will increase the absorption of oxygen, which may have an adverse effect on the mechanical properties of the part such as fatigue resistance or elongation. In contrast, the powders of the present disclosure will show some tolerance to fine particles <20 microns in their PSD at levels up to 30% by volume, and will not exhibit at least some of the above-mentioned disadvantages.

[0092] In some embodiments, the improved physical properties of the powders of the present disclosure are less sensitive (and in some cases, insensitive) to ambient humidity (typically described using relative humidity or RH%) or humidity exposure history. In other words, while the physical properties (e.g., flowability, apparent density) of comparative prior art powders for additive manufacturing typically deteriorate at higher ambient humidity levels, in contrast, the powders of the present disclosure typically remain unchanged at higher ambient humidity levels. Thus, advantageously, the powders of the present disclosure have substantially the same improved physical properties at both low levels of relative humidity and high levels of relative humidity (e.g., any RH% in the range of 10RH% to 75RH%, e.g., at 10RH% and 75RH%, or at 30RH% and 75RH%).

[0093] In some embodiments, the powders of the present disclosure show improved properties in the molten state (during the additive manufacturing process), such as wettability characteristics. For example, by improving the surface chemistry of the powder, the wettability of the powder particles after melting can be changed and preferably reduced. The lower wettability characteristics can minimize the diffusion of the molten material phase, which can be observed in the comparative prior art powders when melting after exposure to the additive manufacturing laser. In other words, the powders of the present disclosure will limit the molten pool to the energy deposition area. In some embodiments, this improved wettability characteristic improves the resolution and surface finish of the 3D parts by providing finer control over the molten pool width. In other words, a smaller molten pool will produce a part with a finer particle size. In another example, changing the wettability of the powder can prevent the inclusion of unmelted powder particles in the solidified molten pool. In general, the main component of the surface roughness of the parts obtained by powder-based additive manufacturing is attributed to the welded, unmelted powder particles connected to the surface of the part. In some embodiments, it is believed that this change in powder wettability changes the surface tension between the molten pool and the surfaces of the unmelted particles adjacent to the molten pool, thereby making the contact angle between the molten particles and the unmelted particles larger, which limits the expansion of the metal pool and also reduces the connection of the unmelted particles to the metal pool due to the solidification of the metal pool, thereby producing a part with an improved surface finish.

[0094] In some embodiments, the powders of the present disclosure provide greater flexibility when recycled during the additive manufacturing process. For example, it has been observed that the powders of the present disclosure substantially retain at least some of the improved physical properties after being used in the additive manufacturing process. This powder property allows for some flexibility and predictability in recycling the powder over multiple iterations, which can be improved relative to the prior art powders used as a comparison and / or when the recycled powder is mixed with new powder, so that although there may be mixed behavior (e.g., in terms of flowability, tap density, etc.), the resulting mixture still has the improved flowability described herein.

[0095] In some embodiments, the improved physical properties of the powders of the present disclosure provide greater flexibility when packaging the powders into containers, which can simplify the packaging process and / or reduce costs. Powders for additive manufacturing are typically packaged in packages such as drums, barrels, cans, etc. In some embodiments, since the powders of the present disclosure exhibit increased fluidity relative to comparative prior art powders, the packaging process time can be reduced due to the ease of pouring the powders. In some embodiments, since the powders of the present disclosure are less sensitive to high RH%, these powders can be packaged in containers without including a packaging desiccant (e.g., a pouch with AlSiMg therein), which eliminates this potential source of contamination (e.g., desiccant leaking from a pouch during transportation / storage). In some embodiments, because the powders of the present disclosure are less sensitive to RH% exposure history, these powders can be packaged in containers in air (dry or up to 75% relative humidity) or nitrogen, rather than argon (as used with comparative prior art powders), which reduces the packaging shrinkage issues observed when using argon, reduces the costs associated with the use of argon, and can simplify the packaging process.

[0096] In some embodiments, the improved physical properties of the powders of the present disclosure provide improved screening efficiency relative to the prior art powders used for comparison. For example, this improved screening efficiency can shorten the time of the screening process, thereby increasing the amount of powder processed in the same time period (kg / h), which can occur when the powder is fresh and / or during recycling. For example, this improved screening efficiency can increase the yield and apparent density of the powder, thereby enabling the use of 15 μm powder instead of 20 μm powder (e.g., Ti64 or AlSiMg).

[0097] In some embodiments, the powders of the present disclosure have increased batch-to-batch consistency / stability in expected performance during additive manufacturing processes relative to comparable prior art powders. For example, it has been observed that at least some of the improved physical properties described herein reduce the variation in product performance typically associated with poor apparent density and / or poor flowability of the powder, at least due to possible increased flowability, and particularly increased flowability that is less sensitive to ambient humidity. This can translate into better process control when handling powders in additive manufacturing, generally resulting in a final product with fewer defects and deficiencies.

[0098] In some embodiments, improvements in additive manufacturing powders can affect subsequent operations of the additive manufacturing process (e.g., cleaning, processing, etc.) and will likely improve process reliability. Thus, the confidence level of manufactured parts can be increased, enabling the application of standards that are too stringent for the actual state of the art. In addition, since the cost of powder feedstock is the most significant expense over the life cycle of an additive manufacturing device, costs will be significantly reduced.

[0099] For example, it has also been observed that the use of the powders described herein can result in less time required to clean finished parts than using comparative prior art powders. Typically, when using prior art powders, it is more difficult to remove unsintered powders from parts because they cannot flow freely, requiring a large and time-consuming cleaning process to remove such unsintered powders from finished parts. In addition, due to size and weight, it may be difficult to remove powder from large parts. The print bed containing printed parts and unsintered powders can weigh thousands of kilograms or more and may be difficult to manipulate. A technician will readily appreciate that when an operator retrieves a finished part from a powder bed, a powder that is more similar to a fluid (e.g., the powder of the present disclosure) will more easily fall off the part, thereby shortening the cleaning process of the finished part and generally improving productivity.

[0100] In addition, the inventors have discovered that the use of the powders described herein in conventional 3D printing devices (additive manufacturing devices) enables at least some such devices to have improved performance, for example, in terms of energy efficiency, part quality output, processing time, etc. For example, it has been observed that the use of the powders described herein can produce manufactured parts (also referred to herein as "final products") with better surface finishes, fewer wrinkles, cracks, or holes than the use of comparative prior art powders. For example, it has also been observed that the use of the powders described herein can enable the device to operate at a faster speed, for example, the device can operate to re-coat elements at a faster speed than is possible with comparative prior art powders, thereby shortening the overall time required to manufacture the part.

[0101] Powder properties

[0102] Figure 1 A photograph of a powder 10 comprising substantially spherical particles 20 is shown according to an embodiment of the present disclosure. Figure 2 It further shows Figure 1 Schematic representation of an embodiment of a powder 10 and a granule 20.

[0103] As discussed above, the powders described herein exhibit improved physical properties relative to comparative prior art powders.These properties can be determined using standard tests (eg, ASTM) and / or the tests discussed herein.

[0104] In some embodiments, the powder 10 of the present disclosure may have flow properties measured using a Hall flow meter funnel (static flowability) according to a standardized test procedure (i.e., without shaking) such as ASTM B213, or using RPA (dynamic flowability) such as GranuDrum TM (Granutools, Belgium)) that have improved flow properties relative to the flow properties of comparative prior art powders. For example, the inventors have observed that the avalanche angle of an exemplary embodiment of powder 10 (AlSi7Mg) is 31 degrees, while the avalanche angle of the comparative prior art powder (AlSi7Mg) is 42 degrees.

[0105] In some embodiments, such enhanced flow properties may be less sensitive (or in some cases, insensitive) to the presence of fine particles in the powder particle size distribution (PSD) relative to comparative prior art powders.

[0106] In some embodiments, such enhanced flow properties may be less sensitive (or in some cases, insensitive) to ambient humidity (RH %) and / or the humidity history exposure of the powder relative to comparable prior art powders.

[0107] For example, the powder 10 of the present disclosure can have flowability as measured using a Hall flow meter funnel at a relative humidity (RH%) of at least 75% in accordance with ASTM B213. This is unexpected and surprising because comparative prior art powders commonly used in the field of additive manufacturing typically stop flowing at much lower RH% levels, such as values ​​as low as 30 RH%, in the Hall flow meter funnel test (see Figure 7 : Atomized powder commonly used in additive manufacturing).

[0108] For example, the powder 10 of the present disclosure may have increased flowability compared to a comparative prior art powder, wherein the increased flowability is measurable in both lower ambient humidity (e.g., 10 RH%) and higher ambient humidity (e.g., 75 RH%). Fig. 9 The following embodiments are shown: Powder 10 has a faster curve under all tested ambient humidity conditions relative to the comparative prior art powder (also referred to herein as "untreated powder", "original powder", "unprocessed powder", etc.).

[0109] In some embodiments, the resistance to the increase of ambient humidity described herein can be quantified by determining the maximum RH%, at which the embodiments of the powder 10 of the present disclosure still flow in the Hall flow meter funnel test according to ASTM B213, compared to the comparative prior art powder. For example, in some embodiments, the powder 10 described herein can still flow at a maximum RH%, which is at least 5RH% higher than the maximum RH% of the comparative prior art powder, or at least 10RH% higher, or at least 15RH% higher, or even higher. In the Hall flow meter funnel test according to ASTM B213, the powder 10 flows at a RH% of at least 80% in some embodiments, flows at a RH% of at least 90% in some embodiments, flows at a RH% of at least 95% in some embodiments, and in some embodiments, the powder 10 flows regardless of the RH% (e.g., in the Hall flow meter funnel test according to ASTM B213, the powder 10 still flows at a RH% of 100%).

[0110] In some embodiments, the increased resistance to ambient humidity described herein can be quantified by determining the ratio of the maximum ambient humidity at which an embodiment of the powder 10 of the present disclosure still flows in a Hall flow meter funnel test according to ASTM B213 to the maximum ambient humidity at which a comparative prior art powder stops flowing (powder 10 / comparative powder). For example, in some embodiments, the ratio is at least 1.05, or at least 1.10, or at least 1.15, or at least 1.20, or at least 1.25, or even greater.

[0111] In some embodiments, the increased flowability described herein can be quantified by determining the duration (in seconds) for an embodiment of the powder 10 of the present disclosure to complete the Hall flow meter funnel test compared to the duration required for a comparative prior art powder. For example, in some embodiments, an embodiment of the powder 10 of the present disclosure will complete the Hall flow meter funnel test in a shorter duration than the prior art powder, i.e., at least 1 second shorter, or at least 3 seconds shorter, or at least 5 seconds shorter, or at least 7 seconds shorter, or at least 9 seconds shorter, or even more.

[0112] In some embodiments, the increased flowability described herein can be quantified by determining the ratio of the duration (in seconds) required for an embodiment of the powder 10 of the present disclosure to complete the Hall flow meter funnel test to the duration of a comparative prior art powder at high RH% (e.g., >50 RH%). For example, in some embodiments, at high RH%, the ratio of the Hall flow meter funnel test duration of an embodiment of the powder 10 to a comparative prior art powder will be less than 0.95 (powder 10 / comparative powder), or less than 0.90, or less than 0.85, or less than 0.80, or less than 0.75, or less than 0.70, or even less.

[0113] In some embodiments, powders 10 of the present disclosure may have an apparent density (also referred to as "tapped density") as tested according to a standardized test procedure (eg, ASTM B212) that is improved relative to the apparent density of comparative prior art powders.

[0114] In some embodiments, the improved relative apparent density described herein may also be less sensitive (or in some cases, insensitive) to ambient humidity (RH %) and / or the humidity exposure history of the powder.

[0115] In some embodiments, powder 10 may have an increased apparent density relative to a comparative prior art powder, whether under conditions of lower ambient humidity (e.g., 10% RH) or higher ambient humidity (e.g., 75% RH). For example, the inventors have observed that at the same ambient humidity (RH%), the apparent density (g / cm 3 ) typically has an increase in apparent density of at least 3% relative to comparative prior art powders.

[0116] For example, Fig.10 The apparent density of an embodiment of powder 10 (labeled "treated powder") and the apparent density of a comparative prior art powder (labeled "original powder") measured according to ASTM B212 at different ambient humidity values ​​are shown. Fig.10 In the embodiment of the powder 10, the surface-modified Ti-6Al-4Va powder (Ti64, Tekna Plasma Systems, Inc.) obtained according to Example 7 is shown in FIG. 1 . At 30% RH, the apparent density of the comparative prior art powder is 2.420 g / cm 3 , and the apparent density value of the embodiment of the powder 10 is about 2.490 g / cm 3 , thereby showing an increase in apparent density of about 3%. At 50% RH, the apparent density of the comparative prior art powder was 2.400 g / cm 3, and the apparent density value of the embodiment of the powder 10 is about 2.480 g / cm 3 , thus again showing an increase of about 3%. At 75% RH, the apparent density of the comparative prior art powder was 2.360 g / cm 3 , and the apparent density value of the embodiment of the powder 10 is about 2.470 g / cm 3 , thus showing an increase of about 4.45%.

[0117] In other words, at a given relative humidity, the powder 10 of the present disclosure will have an increased apparent density relative to a comparative prior art powder.

[0118] Fig.10 It is also shown that the apparent density of the prior art powder is more sensitive to increases in ambient humidity levels. It undergoes an apparent density increase from 2.420 g / cm at 30% RH to 1.340 g / cm at 1.20% RH. 3 Reduced to 2.360g / cm at 75%RH 3 , which represents a loss of about 2.5% in apparent density as a function of relative ambient humidity. In contrast, the apparent density of the embodiment of the powder 10 is less sensitive to increases in ambient humidity levels, with the apparent density increasing from 2.490 g / cm at 30% RH to 3 2.470g / cm2 at 75% RH 3 , which represents a loss of only 0.8% in apparent density as a function of relative ambient humidity.

[0119] In some embodiments, the apparent density of the powder 10 of the present invention is less sensitive to increases in ambient humidity (e.g., from 30% RH to 75% RH), which can be determined in accordance with ASTM B212. For example, when subjected to such an increase in RH%, the apparent density of the powder 10 can be at least 0.01 g / cm greater than the apparent density of a comparable prior art powder. 3 , or at least 0.04g / cm 3 , or at least 0.06g / cm 3 , or at least 0.08g / cm 3 , or at least 0.10g / cm 3 , or even greater. For example, the apparent density of powder 10 may vary by no more than 0.06 g / cm when subjected to such an increase in RH%. 3 , or not more than 0.04g / cm 3 , or not more than 0.02g / cm 3 , or even less.

[0120] In general, the relative increase in the apparent density of the powder 10 described herein enables the manufacture of 3D objects having a higher degree of compactness, better surface finish and enhanced mechanical properties such as ultimate tensile strength (UTS or Rm), elongation at break (A%) and fatigue resistance (for example, the description of the test and the values ​​to be determined are given in standard EN ISO 6892-1:2009). This can be achieved in Fig.47 and Fig.48 , which shows surface details of an additively manufactured part made with an embodiment of the surface modified powder 10, and Fig.47 and Fig.48 The effect on the mechanical properties of the printed parts is shown. FIG. 32E to FIG. 32H As shown, better surface finish can be observed when compared to additively manufactured parts made with comparative prior art powders.

[0121] In some embodiments, powders 10 of the present disclosure may exhibit altered wettability characteristics relative to comparative prior art powders.

[0122] For example, by changing the surface chemistry of the powder 10, the wettability of the powder particles 20 after melting can be changed and reduced. The lower wettability can minimize the spread of the molten material of the molten pool 710 by capillary forces that confine the molten pool to the energy deposition area, and the molten pool 710 is generated by the melting action of the laser on the powder particles 20. In this way, when the width of the molten pool is reduced, finer features can be obtained. Therefore, in addition to Fig.35 , the resolution of the 3D method can be enhanced and the energy loss can be reduced. For example, in some embodiments, for a radius R M 200 μm and depth D M The radius R of the melt pool 710 is 200 μm and the molten material diffused by capillary force is M It may be no greater than 600 μm, in some embodiments no greater than 400 μm, in some embodiments no greater than 300 μm, and in some embodiments even smaller (eg, no greater than 250 μm).

[0123] In some embodiments, the altered wettability of the powder particles 20 can prevent inclusion of unmelted powder particles in the solidified melt pool. In general, the major component of surface roughness of parts obtained by powder-based additive manufacturing is attributed to welded, unmelted powder particles attached to the surface of the part. As described herein, the change in wettability of the powder 10 caused by the metal results in a high contact angle between the melt and the cold metal particles, which inhibits its inclusion at the surface, thereby producing a part with an improved surface finish.

[0124] Fig.33This effect on surface finish is shown where the surfaces of parts manufactured by laser powder bed fusion using AlSi7Mg powder and AlSi10Mg powder are compared. The letter "B" represents AlSi7Mg and "C" represents AlSi10Mg, and the reference number "1" represents the method using the powder 10 described herein, while the reference number "2" represents the method using a comparative prior art powder.

[0125] In some embodiments, powders 10 of the present disclosure may have improved sieving efficiency as tested according to a standardized test procedure (e.g., such as using a stack of ASTM E11 mesh sieves 230, 450, 500, and 625) that is improved over the sieving efficiency of comparative prior art powders.

[0126] In some embodiments, the improved relative sieving efficiencies described herein may also be less sensitive (or in some cases, insensitive) to ambient humidity (RH %) and / or the humidity exposure history of the powder.

[0127] Fig.11 Results of a screening efficiency test using an embodiment of powder 10 are shown, with the results reported as the amount of particles less than 20 μm in size collected in the final stage of the screening stack as a function of the total amount of powder initially used. In this test, the embodiment of powder 10 was AlSi10Mg powder obtained according to Example 8, while the comparative prior art powder was prior art unprocessed AlSi10Mg powder (Tekna Plasma Systems, Inc.). Fig.11 It is shown that less powder is recovered using the comparative prior art powder, and this reduction in collected powder is further exacerbated when a higher initial powder volume is used. Without being bound by any theory, it is believed that this different behavior can be attributed to the lower cohesion of the powder 10, so that the overall increased mass of the material forces individual particles 20 to pass through the openings of the screen rather than forming agglomerates of material.

[0128] Thus, in some embodiments, the powder 10 of the present disclosure may demonstrate higher sieving efficiency and better resistance to high ambient humidity relative to comparable prior art powders.

[0129] For example, the ratio of the screening efficiency of the powder 10 to the screening efficiency of the comparative prior art powder can be at least 1.15, or at least 1.5, or at least 2, or at least 2.5, or at least 3, or even greater. For example, the ratio of the recovered sieved powder 10 to the total initial amount can be at least 0.15, or at least 0.20, or at least 0.25, or at least 0.30, or even greater. For example, for a total sieved amount ranging from 100 g to 1000 g, the change in the ratio can be less than 0.10, or less than 0.8, or less than 0.6, or less than 0.4, or less than 0.2, or even less. For example, in some embodiments, for a total initial amount of 100 g, the change in the ratio of the amount of the recovered sieved powder 10 relative to the total initial amount can be less than 50%, or less than 40%, or less than 30%, or less than 20%, or less than 10%, or even less.

[0130] For example, powders 10 described herein may have a sieving efficiency such that when 1000 g of powder 10 having a PSD of 0 to 1000 microns is sieved through a stack of ASTM E11 mesh sieves 230, 450, 500, and 625, at least 100 g of powder having a PSD < 20 microns is recovered.

[0131] In some embodiments, powders 10 of the present disclosure may have improved behavior during gas classification relative to the behavior of comparable prior art powders.

[0132] In some embodiments, the improved relative behavior in the gas staging processes described herein may also be less sensitive (or in some cases, insensitive) to ambient humidity (RH %) and / or the humidity exposure history of the powder.

[0133] Gas classification processes typically rely on particle inertia to separate them according to size. Therefore, gas classifiers are typically unable to distinguish between aggregates of two or more particles and larger particles. Because the powder 10 described herein is characterized in that aggregates are rarely formed, at least in part due to its reduced hydrophilicity, the powder 10 described herein has improved particle separation in subsequent gas classification processes. This improved particle separation minimizes classification errors. When the cohesion of individual powder particles decreases, the aggregate fraction in the gas stream decreases. Since aggregates appear as larger particles with lower density, aggregates belong to the larger fraction in this process, while the small particles that make up the aggregates should not.

[0134] A skilled artisan will readily appreciate that, in certain embodiments, the powder 10 of the present disclosure may have one or more of the advantageous physical properties described herein.

[0135] Powder material

[0136] A variety of materials can be used for additive manufacturing. A skilled person will readily understand how to proceed to analyze the chemical composition of a given powder using standardized tests. For example, the chemical composition of a powder can be determined by chemical analysis according to ASTM E34, ASTM E3061, or by other analytical methods acceptable in the art.

[0137] In one non-limiting embodiment, the powder 10 may include particles 20 that are pure metal-based particles, alloy-based particles, ceramic-based particles, and / or composite-based particles. For example, the powder 10 may include particles 20 that are (but not limited to) aluminum alloy-based particles, steel-based particles, stainless steel-based particles, copper alloy-based particles, nickel alloy-based particles, superalloy-based particles, palladium-based particles, silver-based particles, tungsten-based particles, refractory metal-based particles, ceramic-based particles, polyamide-based particles, or polystyrene-based particles. For example, the particles may be metal-based spherical particles.

[0138] For example, the powder 10 may include particles 20 that are, but are not limited to, aluminum (Al)-based particles, iron (Fe)-based particles, steel-based particles, copper (Cu)-based particles, nickel (Ni)-based particles, gold (Au)-based particles, silver (Ag)-based particles, bismuth (Bi)-based particles, manganese (Mn)-based particles, zinc (Zn)-based particles, cobalt (Co)-based particles, titanium (Ti)-based particles, chromium (Cr)-based particles, molybdenum (Mo)-based particles, platinum (Pt)-based particles, zirconium (Zr)-based particles, tantalum (Ta)-based particles, niobium (Nb)-based particles, tungsten (W)-based particles, iridium (Ir)-based particles, etc. These metals may be used alone as one substance, or in combination of two or more substances as an alloy.

[0139] Examples of alloys include, but are not limited to, aluminum alloys (e.g., AlSi10Mg, AlSi12, AlSi7Mg0.6, etc.), copper alloys (e.g., Cu-15Ni-8Sn, GRCop-84, CuNiSi(Cr), CuCr1Zr, CuAl10, CuSn10, CuSn15, etc.), nickel alloys (e.g., nickel-chromium superalloys such as Inconel 718, Inconel 713, Inconel 738, Inconel 625, etc.), magnesium alloys (e.g., Mg-5.9Zn-0.13Zr, Mg-9Al, etc.), zinc alloys (e.g., Zn-Al, Zn-Fe, etc.), cobalt alloys (e.g., ASTM F75CoCr, Co28Cr6Mo, etc.), and titanium alloys (e.g., Ti-6Al-4V, Ti-6Al-7Nb, Ti-6Al-4VELI [containing less nitrogen, oxygen, iron and carbon], etc.).

[0140] For example, the powder 10 may include particles 20 of a ceramic material (oxide-based ceramic material) formed of, but not limited to, an oxide and a ceramic material formed of a non-oxide such as carbide, boride, nitride, and apatite. There is no particular limitation on the oxide-based ceramic, and it may be an oxide of various metal substances. The metal forming the oxide-based ceramic may be, for example, one, two, or more substances selected from the following: metalloids such as B, Si, Ge, Sb, and Bi; typical elements such as Mg, Ca, Sr, Ba, Zn, Al, Ga, In, Sn, and Pb; transition metals such as Sc, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Ag, and Au; and lanthanides such as La, Ce, Pr, Nd, Sm, Er, and Lu. In particular, one, two, or more substances selected from Mg, Y, Ti, Zr, Cr, Mn, Fe, Zn, Al, and Er may be used.

[0141] More specific examples of oxide-based ceramics may include aluminum oxide, zirconium oxide, yttrium oxide, chromium oxide, titanium dioxide, cobaltite, magnesium oxide, silicon dioxide, calcium oxide, cerium dioxide, ferrite, spinel, zircon, nickel oxide, silver oxide, copper oxide, zinc oxide, gallium oxide, strontium oxide, scandium oxide, samarium oxide, bismuth oxide, lanthanum oxide, lutetium oxide, hafnium oxide, vanadium oxide, niobium oxide, tungsten oxide, manganese oxide, tantalum oxide, terbium oxide, europium oxide, neodymium oxide, tin oxide, antimony oxide, antimony-containing tin oxide, indium oxide, tin-containing indium oxide, zirconium oxide aluminate, zirconium oxide silicate, hafnium oxide aluminate, hafnium oxide silicate, titanium oxide silicate, lanthanum oxide silicate, lanthanum oxide aluminate, yttrium oxide silicate, titanium oxide silicate, and tantalum oxide silicate.

[0142] Examples of non-oxide-based ceramics may include carbides such as tungsten carbide, chromium carbide, vanadium carbide, niobium carbide, molybdenum carbide, tantalum carbide, titanium carbide, zirconium carbide, hafnium carbide, silicon carbide, and boron carbide; borides such as molybdenum boride, chromium boride, hafnium boride, zirconium boride, tantalum boride, and titanium boride; nitrides such as titanium nitride, silicon nitride, and aluminum nitride; composite compounds such as forsterite, talc, cordierite, mullite, barium titanate, lead titanate, lead zirconate titanate, Mn-Zn ferrite, Ni-Zn ferrite, and sialon; phosphate compounds such as hydroxyapatite and calcium phosphate. Any of these substances may be used alone, or two or more substances may be used in combination.

[0143] For example, the powder 10 described in this article may contain particles with a chemical formula of Al-10Si-0.35Mg, or Al-10Si-Mg, or Al-7Si-Mg, or 62Ni-21.5Cr-9.0Mo-3.65Nb, or Ti-6Al-4Va, or Ti-6Al-2Sn-4Zr-2Mo, or Ti-5Al-5V-5Mo-3Cr, or Ni alloy 625-based particles, or Ni alloy 718-based particles, or pure titanium-based particles (e.g., CP-Ti, commercially available pure titanium).

[0144] The skilled artisan will readily appreciate that a given powder 10 may contain certain controlled amounts of specific elements as determined using standardized tests. For example, a given powder 10 may contain one or more of the following elements: carbon as determined according to ASTM E 1941 or ASTM E 1019, hydrogen as determined according to ASTM E 1447, oxygen and nitrogen as determined according to ASTM E 1409, and other elements as determined according to ASTM E 539 and ASTM E 2371. Other analytical methods are also known in the art and will not be further described herein for the sake of brevity.

[0145] For example, a given powder 10 may include one or more of the following: an oxygen content of less than 2000 ppm, or less than 1500 ppm, or less than 1000 ppm, or less than 400 ppm, or less than 300 ppm, or less than 150 ppm, or even less; a carbon content of less than 1000 ppm, or less than 500 ppm, or less than 300 ppm, or less than 100 ppm, or even less; a hydrogen content of less than 200 ppm, or less than 150 ppm, or less than 100 ppm, or even less; and a nitrogen content of less than 500 ppm, or less than 400 ppm, or less than 300 ppm, or even less.

[0146] Powder size

[0147] Powders of various particle size distributions (PSD) may be used in additive manufacturing, where the PSD may be determined by one or more of the intended additive manufacturing device, the intended application, the intended component, etc. A skilled person will readily understand how to determine the particle size of a given powder. For example, a skilled person will readily understand that for powders of size 45 microns and larger, the particle size may be determined according to standard ASTM B214, while for powders of size 45 microns and smaller, the particle size should generally be determined using ATSM B822.

[0148] In one non-limiting embodiment, powder 10 may, for example, comprise particles 20 having a PSD having a conventional size range of about 0 μm to about 1000 μm, including any conventional size range contained therein, such as about 0 μm to about 20 μm, or about 0 μm to about 45 μm, or about 0 μm to about 53 μm, or about 0 μm to about 70 μm, or about 15 μm to about 45 μm, or about 15 μm to about 53 μm, or about 15 μm to about 70 μm, or about 15 μm to about 105 μm, or about 30 μm to about 53 μm, or about 30 μm to about 70 μm, or about 30 μm to about 105 μm, or about 45 μm to about 105 μm, or about 53 μm to about 105 μm, or about 100 μm to about 500 μm, or about 500 μm to about 1000 μm. In some cases, powder 10 may include particles having a size greater than 1000 μm, depending on the specifics of the additive manufacturing method and / or apparatus.

[0149] The skilled person will also readily appreciate that for a given conventional size PSD range, there may be room for a small portion of the powder 10 to have a particle size exceeding the conventional lower or upper limits, i.e., the PSD may have a fine inclusion and / or a coarse inclusion (in volume % or weight %).

[0150] For example, a powder 10 having a conventional size range of 25 μm to 45 μm for PSD may contain less than 20% by volume, or less than 15% by volume, or less than 10% by volume, or less than 5% by volume, or even less (e.g., 0% by volume) of particles having an average particle size of less than 25 μm according to ASTM B822 (fine inclusion). The powder 10 may also have a portion of particles having a diameter greater than 45 μm according to ASTM B214 (coarse inclusion) of less than 20% by weight, or less than 15% by weight, or less than 10% by weight, or less than 5% by weight, or even less (e.g., 0%).

[0151] For example, the following table shows various PSD size ranges for embodiments of the powder 10 of the present disclosure, which may be suitable for different applications:

[0152] Table 1 - Example of particle size distribution of powder A

[0153]

[0154] Table 2 - Example of particle size distribution of powder B

[0155]

[0156] Table 3 - Example of particle size distribution of powder C

[0157]

[0158] Preparation method of powder disclosed herein

[0159] Figure 3 A flow chart of a conventional method 200 for making powder 10 is shown.

[0160] Without being bound by any theory, it is believed that powders used for additive manufacturing exhibit chemical moieties on the surface of the particles that interact favorably with water molecules, thereby making the surface hydrophilic. This increases the tendency of the powder to adsorb water from the ambient atmosphere, for example, during manufacturing or post-manufacturing stages, such as any of preparation, handling, storage and use. As a result, water will tend to adsorb on the surface of the particles, eventually until a layer (e.g., a molecular layer, a multi-molecular layer, etc.) is formed. The presence of adsorbed water on the surface of powder particles used for additive manufacturing is harmful, at least because at the contact points between the individual powder particles, the adsorbed water film on each particle can interact through hydrogen bonding and surface tension to form agglomerates (which can be "secondary particles" and / or the entire powder bed). This cohesive force is detrimental to the flowability of the powder because more energy is required to initiate a powder avalanche. Because in an additive manufacturing operation, the powder needs to be spread out precisely in a uniform manner at each stage of the operation, such cohesive forces or agglomerate formation caused by the presence of adsorbed water at the surface of the powder particles is highly undesirable.

[0161] In one aspect, the present disclosure solves the above-mentioned problems by using the exact same chemical moieties that cause the hydrophilicity of the powder to attach functional moieties that impart the desired properties to the powder surface.

[0162] For example, in step 210, the plasma atomization method can be used to obtain powder particles from a wide range of raw materials including, for example, pure metals, alloys, ceramics, and composites. For example, a wide range of dense spherical metal, ceramic, or composite powders can be obtained from raw materials of the same nature in the form of elongated parts, and non-limiting examples of elongated parts are, for example, rods, wires, or filled tubes disclosed in US9,718,131 and US 9,751,129, and the entire contents of these two patent documents are incorporated herein by reference for all purposes. In brief, the method for atomization includes plasma atomization, in which the raw material is guided at the apex of one or more plasma jets. The plasma jet impinges on the end of the material and heats the material until the material reaches its melting point, and the material is separated from the raw material in the form of molten droplets by the plasma jet, by a secondary plasma jet group, or by an additional gas jet. The raw material can be optionally preheated by one or more preheating mechanisms. The molten material droplets then enter a cooling zone, in which the droplets solidify in free fall, so that most of them are spherical. Plasma reactors for carrying out this method are known in the art, and the plasma reactor may be an inductively coupled plasma torch (ICP torch) (e.g., PL-50, PN-50, PL-35, PN-35, PL-70, PN-70, PN-100 from TEKNA Plasma Systems, Inc.), or may be a direct current (DC) plasma torch (e.g., DC plasma torches commercially available from Praxair, Oerlikon-Metco, Pyrogenesis, and Northwest Mettech).

[0163] Another possible method is gas atomization through a molten pool. In this embodiment, the powder is first melted in a crucible and then fed into a high-speed gas stream through a small hole, where the melt stream is sheared into smaller droplets. The atomization method can also use a feed rod that melts when passing through an induction coil. Then, the molten metal flows to an atomizing nozzle, where a high-speed gas stream splits the melt into fine droplets. Another method for atomization uses a rotating electrode in contact with a plasma jet. The centrifugal force generated by the rotation of the electrode sprays the molten material, which then solidifies in flight, thereby taking a spherical shape. Another method is to atomize the molten material from a heated storage by spreading the molten material on a rotating disk and then spraying it under the centrifugal force generated by the rotation of the disk. Then, the sprayed droplets solidify during free fall, thereby taking a spherical shape.

[0164] Other atomization methods are known in the art and, for the sake of brevity, will not be described further here.

[0165] The powder obtained by atomization may include, but is not limited to, micron-sized particles, which may be defined as particles having a diameter in the range of 0 microns to 1000 microns as discussed above and below in this specification.

[0166] In some embodiments, the raw material may include a powder with particles having an angular shape. Step 210 'includes processing such particles having an angular shape to manufacture a dense spherical product, such as described in US 9,023,259 and US9259785, and the entire contents of these two patent documents are incorporated herein by reference for all purposes. In short, the powder having an angular shape can be fed to a hot zone, where the energy sufficient to partially melt the particles is transferred to the particle surface by radiation, convection, induction, surface recombination or a combination thereof. In one embodiment, the powder is fed into an inert gas stream, which enters a chamber where there is a hot plasma generated by an alternating electromagnetic field in an ICP torch as mentioned above. The particle surface melts and is subsequently reshaped into a spherical shape required to minimize Gibbs free energy. In another contemplated embodiment, hot plasma is generated at the outlet of a DC plasma torch as mentioned above or at the apex of a plasma jet generated by a plurality of plasma torches. Optionally, a sheath gas protecting the wall of a plasma chamber can be provided. The sheath gas can also play an active role in the interaction with the powder material. When the sheath gas is brought into thermal contact with the plasma, the sheath gas becomes part of the heating medium. The hot zone at the apex of the plasma torch can then expand to a larger volume to facilitate interaction with the injected powder cloud.

[0167] The description provided herein is not meant to be limiting, and one skilled in the art will recognize that there are other ways in which powder particles can be heated to spheroidize.

[0168] In step 230, the surface of the powder may be activated, for example, it may contain more hydroxyl groups when the surface of the powder is exposed to the plasma compared to the native oxide layer. Prior to step 230, the powder includes a native oxide outer layer resulting from oxidation of the outer layer. This layer is also called a passivation layer and helps protect the metal from deeper corrosion. Metal oxides MOx naturally have OH groups on their surfaces. However, the concentration of hydroxyl groups varies from metal oxide to metal oxide and strongly depends on the synthesis method including the gas composition and water vapor concentration in the powder environment.

[0169] In the plasma state, the electromagnetic field ionizes and accelerates the atoms. When impacting the surface of the immersed material, these high-energy ions transfer part of their energy to the surface, causing the formation of hydroxyl groups, thus creating an "activated" surface. FIG. 5A to FIG. 5C A non-limiting scheme of the activation mechanism is shown for the case of a metal surface in an inert gas plasma, in this case argon. Figure 5AFigure 2 shows an active metal surface which typically has a certain amount of oxygen on it. Figure 5B As shown in FIG. 1 , when high-energy noble gas ions generated in the plasma hit the surface, they destroy the electronic structure in the target area, which can cause (for example) the breaking of bonds between oxygen and metal. Thus, very active surface free radicals are generated. Figure 5C As shown, when water vapor is present near the activated area, hydrolysis will occur in a sufficiently short time frame and the -OH moiety will attach to the surface. Water added intentionally or unintentionally at a concentration of about 1000 ppm, or 100 ppm, or even 10 ppm is sufficient to generate hydroxyl groups on the metal surface.

[0170] As another example, the plasma gas can contain oxygen. FIG. 6A to FIG. 6C Non-limiting possible mechanisms for activation in the presence of an oxygen-containing plasma are shown. Figure 6B As shown, Fig. 6A The oxygen free radicals shown hit the metal surface where they form bonds with the metal substrate. Figure 6C As shown, these oxygen atoms remain in a free radical state until they encounter water vapor, which hydrolyzes the oxygen atoms to produce -OH groups on the surface. Exposure to water vapor can occur during plasma processing or outside the plasma reactor, for example, during subsequent steps such as during handling, storage, or use.

[0171] As yet another example, free radicals can be generated by exposure to UV radiation. Plasmas such as DC and RF plasmas used in plasma atomization generate high energy UV radiation. These high energy photons interact with gaseous oxygen to form ozone, which then reacts with water vapor to form hydroxyl radicals, which then interact freely with the surface.

[0172] As another example of a mechanism for surface activation in the presence of plasma, the literature reports that exposure of titanium dioxide to UV light results in the creation of oxygen vacancies at surface bridging oxygen sites. These vacancies can then be repaired by hydrolysis of water and subsequent bonding to the damaged sites. The surface then undergoes a transition to a superhydrophilic state. In this mechanism, similar to other mechanisms, the hydrolysis step can follow the free radical formation step. In some embodiments, the hydrolysis step may be present as a post-treatment step.

[0173] In atomization schemes that do not use plasma, the generation of hydrophilic groups is not so important because these mechanisms cannot occur. However, at the solid / gas interface, when the bare metal comes into contact with oxygen or water, an oxide layer will still be formed. This layer will not be completely converted into stoichiometric MOx, and hydroxyl groups will still exist to a certain extent. Therefore, the hydroxyl groups that determine the flow behavior of the metal powder depend on the synthesis method. For example, the inventors expect that the hydroxyl concentration of the Ti alloy powder prepared by the plasma method will be higher than the hydroxyl concentration of the Ti alloy powder prepared by the gas atomization method. Figure 7 Hall flow curves versus relative humidity for Ti-6Al-4V powders prepared by different methods are shown. While the plasma atomized powder flows faster in low humidity but stops flowing at medium RH levels, the flowability of the gas atomized powder shows better resistance to humid atmosphere.

[0174] In step 240, surface modification by introducing a hydrophobic agent on the surface of the powder particles hinders the hydrophilicity of the powder by the hydroxyl groups present on the surface of the powder. The surface modification can be performed by different methods using coupling agents. These molecules interact with the interface by chelating with catechols, phosphates, phosphonates, sulfates, amines and carboxylates or by chemical covalent bonding with organosilanes, organotitanates, organozirconates and organoaluminates. The following non-limiting embodiments are mainly related to the surface modification of metal powders using silane coupling agents, however, the technician will readily understand that these embodiments are only for illustrative purposes and are not intended to limit the present invention, so that other types of powders and / or coupling agents can be expected without departing from the present disclosure.

[0175] FIG. 8A to FIG. 8D The figure shows a possible attachment mechanism for alkoxysilanes. This molecule requires water to react chemically. The functionalized silane is denoted by R n SiX (4-n) , wherein X is a hydrolyzable group (alkoxy, halogen, carboxylate, amine), and R is a non-hydrolyzable group (alkyl, amine, epoxy, mercapto, acrylate, haloalkyl) that retains the desired functionality, and n is an integer between 1, 2 and 3. Fig. 8A As shown, hydrolysis occurs in the first step of the reaction. Water molecules adsorbed on the surface or added to the mixture attack the silicon site of the silane, so that the leaving group (hydrolyzable group) is replaced by a silanol group (Si-OH) through a nucleophilic substitution mechanism (SN2). It is noted that the byproduct of this step is a hydrolyzable group (alcohol, hydrogen halide, carboxylic acid or amine) bonded to hydrogen. The kinetics of the hydrolysis step depends on several parameters: temperature, leaving group, chemical structure of the functional group, and acid / base catalysis. For example, in the case of a leaving group, hydrolysis follows the following order:

[0176] SiC 2 >SiCl>SiOOCH 3 >SiOCH 3 >SiOCH 2 CH 3 .

[0177] Note that when a leaving group generates an acid or base upon hydrolysis, the leaving group will contribute to the reactivity. At this point, two outcomes are possible. Figure 8C and Fig.8D As shown, the silanol reacts with another silanol from the second hydrolyzed silane molecule, or the silanol reacts with an -OH from the surface. In this case, water is released and the silane molecule is covalently attached to the surface. This step is called condensation.

[0178] Preferably, the target application requires a relatively low amount of silane to achieve maximum effect. Therefore, the preferred method aims to maximize coverage while reducing the thickness of the added layer. In this embodiment, this is achieved by promoting the reactive silanol to attach to the surface rather than to other silane molecules. In fact, this is achieved by regulating the rates of two competing processes in the reaction (i.e., hydrolysis and condensation).

[0179] In the process of the present invention, methyltrimethoxysilane, for example, which is an alkoxysilane, can be used, wherein X is a methoxy group and R is a methyl group (CH 3 ). This silane with a one carbon alkyl chain has minimal hydrophobic interactions compared to long chain silanes. This particular alkoxysilane may be advantageous because it can help remove hydrogen bonds between particles while keeping hydrophobic interactions to a minimum. In the absence of a catalyst, the alkoxy group as a leaving group has low reactivity at room temperature. This situation creates an opportunity to adjust the reaction kinetics by appropriate selection of catalysts. From studies on mesoporous silica, it is known that base catalysis tends to promote condensation at the expense of hydrolysis, while acid catalysis tends to follow the opposite trend. Therefore, acid catalysis will promote the formation of oligomers, especially in the presence of excess water, while the use of base catalysis will promote bonding. Base catalysis precisely meets the goals sought in adjusting the method of the present application.

[0180] In a preferred embodiment, the reaction is carried out in a water-alcohol medium. A coupling agent (e.g., silane molecules) is dissolved in an alcohol, and a second solution of alcohol and a catalyst is prepared. The solution is then added to the powder, mixed simultaneously to ensure that all powder particles have the same amount of wetting. The total amount of alcohol is selected so that it does not exceed the void volume in the powder bed, i.e., the mixture remains solid. It has been shown that the use of alcohol as a protic solvent helps to promote the hydrolysis reaction to a certain extent compared to the use of aprotic solvents, and the use of pure water may have limitations because most alkylsilanes are not miscible with water. In a preferred embodiment, the catalyst is ammonia, but is not limited thereto. Other catalysts that promote condensation more than hydrolysis can be used, such as triethylamine, trimethylamine calcium carbonate or sodium fluoride.

[0181] In this scheme, the reaction kinetics favors the surface connection of the silanol moiety. As the hydrolysis begins, condensation becomes possible. Since the possibility of the silanol moiety encountering the surface hydroxyl group at the beginning is much greater than the possibility of encountering the second silanol from another silane molecule, most molecules will be connected to the powder surface. Since the condensation kinetics are highly favorable, the balance will remain favorable for connection at the surface site rather than between free silanes. When n is greater than 1, n hydrolysis may occur on each silane molecule. Therefore, more molecules can be connected to the surface-bound silane. However, in this case, the lower reactivity of steric hindrance and bond to hydrolysis makes this event less likely than being connected to free hydroxyls. However, as more and more surface hydroxyls are occupied, the possibility of this event becomes larger.

[0182] The reaction is preferably carried out in a closed vessel with constant stirring and at a temperature between room temperature (about 20°C) and 79°C, and preferably at a temperature of about 50°C, to maintain constant solvent and catalyst concentrations, as it is believed that temperature affects reactivity.

[0183] Materials used for additive manufacturing have restrictive restrictions on their composition. Therefore, it is preferred that all treatments do not substantially change the chemical composition of the raw powder. Ideally, the surface treatment only adds a molecular layer to the powder surface. The optimal silane coverage is reported to be about 2.7 × 10 14 Molecules / cm 2 The typical surface area of ​​the powder in the laser melting PSD range is 0.04 m 2 / g, or 400cm 2 / g. This method produces 1.08×10 17molecules / gram, since each silane molecule has 1 silicon atom, this means that 5 ppm of Si is obtained in the treated Ti64 powder. The alkoxysilane molecule also has an oxygen atom that reacts to a variable degree. Depending on the functional group, there will be carbon, fluorine, hydrogen or nitrogen atoms, without wishing to be limiting. In practice, the silicon content added to a typical laser melted Ti64 powder ranges from about 10 ppm to 100 ppm.

[0184] Variants

[0185] It is also expected that surface modification can be performed in the gas phase. In such an embodiment, the powder is placed in a fluidized bed and silane vapor is circulated through the powder bed. The gas composition is adjusted according to the type of silane to be reacted. For example, water vapor can be added to react when silane needs to be hydrolyzed. The temperature and water vapor pressure of the fluidized bed are controlled to provide enough water adsorption for reaction but not enough to make the powder cohesive. The water vapor pressure can change throughout the process. A catalyst such as acetic acid or ammonia can be provided to control the reaction kinetics. When the reaction is carried out in the absence of water, chlorosilane or azosilane can also be used. It can be expected that this embodiment can be combined with an atomization method to process the powder. In this embodiment, the reaction gas is injected from the downstream of the plasma torch to avoid dissociation. Then, the atomized powder reacts freely with the active substance on its surface. The geometric structure of the second reactor connected to the atomization reactor fluid controls the time spent by the powder particles in the aerosol phase, thereby controlling the reaction time.

[0186] In another embodiment, the particles 20 of the powder 10 may contain a metal that reacts with silane hydride. For example, the particles 20 may be titanium-based particles, zirconium-based particles, nickel-based particles, platinum-based particles, or gold-based particles. The silane may be adsorbed on a bare metal surface (a surface without a passivation layer) and then reacted to modify the surface and release hydrogen molecules. The process may be performed in the gas phase. In order for the reaction to occur; the surface may not have a native layer of oxide. Therefore, the method may be used in an oxygen-free environment.

[0187] In another contemplated embodiment, the powder is collected in a combined bubbler. The fluid in the bubbler has an active molecule solution that can react with the powder. The fluid is connected to a separator fluid that separates the powder from the liquid solution. In one embodiment, the separator can be a tangential flow filtration device. The fluid is then recirculated in the system with the fresh reactant added. The resulting slurry is then, for example, dried in a tray dryer.

[0188] As another variation, in some embodiments, the three-dimensional metal component 610 may be manufactured by direct metal laser sintering, electron beam melting, selective heat sintering, selective laser sintering, selective laser melting, or forming rather than by direct metal laser melting.

[0189] Those skilled in the art will recognize that it is advisable to limit the amount of solvent used to achieve the optimum, but it is not intended to be limiting in any way. Where a more dilute suspension is desired, the example of powder processing in a bubbler fluidly connected to an atomizer is an excellent example.

[0190] In some embodiments, the powder can be processed to obtain a surface treatment that causes increased flowability. For example, the powder can be removed from a manufacturing device (e.g., a DC plasma reactor, an ICP plasma reactor, etc.) and processed directly (without further processing or classification) to obtain the surface treatment. Alternatively, the powder can be removed from a manufacturing device (e.g., a DC plasma or an ICP plasma) and classified (e.g., gas classification or mesh screening) to separate the metal powders by particle size distribution.

[0191] The surface treatment may include stirring the powder in a solvent such as water or other suitable solvent containing a source of molecules that reduce the hydrophilicity of the powder under conditions to obtain less than 800 ppm, or less than 500 ppm, or less than 400 ppm, or less than 300 ppm, or less than 200 ppm, or less than 100 ppm, or less than 50 ppm, or less than 25 ppm, or less than 20 ppm, or less than 15 ppm, or less than 10 ppm of molecules that reduce the hydrophilicity of the powder that are absorbed by the powder. For example, the source of molecules that reduce the hydrophilicity of the powder contained in water or a suitable solvent may be less than 1000 ppm, or less than 800 ppm, or less than 500 ppm, or less than 400 ppm, or less than 300 ppm, or less than 200 ppm, or less than 100 ppm, or less than 50 ppm, or less than 25 ppm, or less than 20 ppm, or less than 15 ppm, or less than 10 ppm.

[0192] Ideally, the molecules that reduce the hydrophilicity of the powder form a molecular layer on at least a portion of the surface of each particle. For example, the molecules that reduce the hydrophilicity of the powder may form a molecular layer that encapsulates each particle.

[0193] Thus, the surface treatment provides the metal powder for additive manufacturing with increased flowability relative to powder that has not been so treated. For example, when water is used as a solvent, distilled water or demineralized water may be used.

[0194] For example, the source of molecules that reduce the hydrophilicity of the powder can include molecules that are capable of reacting with the reactive surface of the powder particles, thereby causing the molecules that reduce the hydrophilicity of the powder to be attached to the surface. For example, the source of molecules that reduce the hydrophilicity of the powder can include molecules having a portion that is capable of reacting with and / or attaching to an element present on the surface of the reactive powder particles and having a hydrophobic portion that is intended to reduce the hydrophilicity of the powders described herein.

[0195] For example, the molecular source that reduces the hydrophilicity of the powder can include a surfactant, such as an alkyl-based surfactant. For example, an amphiphilic surfactant with a hydrophilic group and a hydrophobic group can be particularly used for carrying out this surface treatment in water. The non-limiting examples of surfactants include alkanoic acid (octanoic acid, decanoic acid, dodecanoic acid, etc.), alkyl phosphates (decyl phosphate, dodecyl phosphate, tetradecyl phosphate, etc.), alkylamines (octylamine, decylamine, dodecylamine, etc.), alkyl sulfates (decyl sulfate, dodecyl sulfate, etc.), alkyl mercaptans (octyl mercaptan, decanethiol, dodecyl mercaptan). The bonding mechanism of surfactants to particles, especially metal particles, can be achieved in different ways, such as connecting surfactants with thiol end groups to metals under hydrogen elimination; silane halides and ethers, phosphonates, carboxylates, catechols, olefins and amines can be used to introduce ether bonds into oxides and functionalized particles with terminal OH groups; terminal OH groups (oxides, polymers) are multi-step functionalized to introduce reactive amine groups and esters. Those skilled in the art will readily appreciate that, in principle, any feasible chemical reaction on the particle surface may be utilized to attach the surfactant, and for the sake of brevity will not be described further herein.

[0196] Therefore, in some embodiments, surface treatment can include multiple steps.For example, the process can include starting to first carry out powder atomization manufacturing method, and the method includes making raw material contact with plasma to atomize raw material (for example, metal source) to manufacture the powder comprising spherical particles.The process can also include classifying powder (for example, sieving or gas classification) to obtain the powder with predetermined particle size distribution (PSD).Alternatively, the process of next step can be carried out without powder classification.Finally, the process includes making powder contact with water or other suitable solvents included in the molecular source that reduces the hydrophilicity of powder under certain conditions, to obtain following powder, the molecule that reduces the hydrophilicity of powder contained by the powder is less than 800ppm, or less than 500ppm, or less than 400ppm, or less than 300ppm, or less than 200ppm, or less than 100ppm, or less than 50ppm, or less than 25ppm, or less than 20ppm, or less than 15ppm, or less than 10ppm.

[0197] Additive Manufacturing Methods

[0198] In one broad aspect, the present disclosure describes methods and apparatus for powder bed fusion additive manufacturing that take advantage of the improved properties of the powder 10 described herein.

[0199] In various embodiments according to the present disclosure, a build platform that can be moved, tilted, or inverted is designed to separate the powder bed from the supporting build platform. The powder bed is formed by dispensing multiple layers of powder material during an additive manufacturing print cycle for a 3D object. Most of the powder material is collected in a hopper and transported to a storage chamber for reuse in subsequent printing jobs. The powder material can be sealed inside the storage chamber in a controlled atmosphere of, for example, air, nitrogen, argon, helium, or other inert or rare gas.

[0200] In powder bed fusion additive manufacturing, a powder bed can be formed by continuously dispensing multiple layers of powder material on a build platform. A light beam or electron beam of sufficient energy hits the surface of the powder bed and can cause the powder material to melt / sinter / merge or process to form an integral component. When parts of the powder layer corresponding to the geometry of the two-dimensional slice of the 3D object (component) are melted or bonded together, the next layer of powder material is dispensed on the surface of the powder bed to continue the printing cycle. When the printing job is completed, the printed parts and the remaining unsintered powder material need to be removed from the build platform to enable the next cycle to start.

[0201] The additive manufacturing system may include one or more energy sources positioned to emit one or more energy beams, including one or more laser beams or electron beams in one embodiment. The beam shaping optical device can receive one or more energy beams from the energy source and form a single beam. The energy patterning unit receives or generates a single beam and transfers a two-dimensional pattern to the beam, and unused energy that is not in the pattern can be discarded. The image relay receives the two-dimensional patterned beam and focuses it as a two-dimensional image to a desired position on a highly fixed or movable building platform (e.g., a powder bed). In certain embodiments, some or all of any discarded energy from the energy patterning unit is reused.

[0202] In some embodiments, a beam homogenizer is used to combine multiple beams from a laser array. The combined beam can be directed to an energy patterning unit comprising one of a transmissive or reflective pixel addressable light valve. In one embodiment, the pixel addressable light valve comprises both a liquid crystal module with a polarizing element and a light projection unit that provides a two-dimensional input pattern. The two-dimensional image focused by the image relay can be directed sequentially toward multiple locations on the powder bed to build a 3D structure.

[0203] The energy source generates photons (light), electrons, ions, or other suitable energy beams or energy fluxes that can be directed, shaped, and patterned. A variety of energy sources can be used in combination. The energy source can include lasers, incandescent light, concentrated solar energy, other light sources, electron beams, or ion beams. Possible laser types include (but are not limited to): gas lasers, chemical lasers, dye lasers, metal vapor lasers, solid-state lasers (e.g., optical fibers), semiconductor (e.g., diode) lasers, free electron lasers, gas-driven lasers, "nickel-like" samarium lasers, Raman lasers, or nuclear pumped lasers.

[0204] The gas laser may include a laser such as a helium-neon laser, an argon laser, a krypton laser, a xenon ion laser, a nitrogen laser, a carbon dioxide laser, a carbon monoxide laser, or an excimer laser.

[0205] The chemical laser may include lasers such as a hydrogen fluoride laser, a deuterium fluoride laser, a COIL (chemical oxygen-iodine laser), or an Agil (all gas phase iodine laser).

[0206] The metal vapor laser may include a laser such as a helium-cadmium (HeCd) metal vapor laser, a helium-mercury (HeHg) metal vapor laser, a helium-selenium (HeSe) metal vapor laser, a helium-silver (HeAg) metal vapor laser, a strontium vapor laser, a neon-copper (NeCu) metal vapor laser, a copper vapor laser, a gold vapor laser, or a manganese (Mn / MnCl 2 ) Vapor laser.

[0207] Solid-state lasers may include the following lasers, such as ruby ​​lasers, Nd:YAG lasers, NdCrYAG lasers, Er:YAG lasers, neodymium YLF (Nd:YLF) solid-state lasers, neodymium-doped yttrium vanadate (Nd:YVO 4 ) laser, Nd:YCa 4 O(BO 3 ) 3 or only Nd:YCOB, Neodymium Glass (Nd:Glass) Laser, Titanium Sapphire (Ti:Sapphire) Laser, Thulium YAG (Tm:YAG) Laser, Ytterbium YAG (Yb:YAG) Laser, Ytterbium:Yb 2 O 3(glass or ceramic) lasers, ytterbium-doped glass lasers (rods, plates / chips and fibers), holmium YAG (Ho:YAG) lasers, chromium ZnSe (Cr:ZnSe) lasers, cerium-doped lithium strontium (or calcium) aluminum fluoride (Ce:LiSAF, Ce:LiCAF), promethium 147-doped phosphate glass (147Pm+3:glass) solid-state lasers, chromium-doped chrysoberyl (alexandrite) lasers, erbium-doped glass lasers and erbium-ytterbium co-doped glass lasers, trivalent uranium-doped calcium fluoride (U:CaF 2 ) solid-state lasers, divalent samarium-doped calcium fluoride (Sm:CaF 2 ) laser or F center laser.

[0208] Semiconductor lasers may include laser medium types such as GaN, InGaN, AlGaInP, AlGaAs, InGaAsP, GaInP, InGaAs, InGaAsO, GaInAsSb, lead salts, vertical cavity surface emitting lasers (VCSELs), quantum cascade lasers, hybrid silicon lasers, or combinations thereof.

[0209] For example, in one embodiment, a single Nd:YAG q-switched laser can be used in conjunction with multiple semiconductor lasers. In another embodiment, an electron beam can be used in conjunction with an array of ultraviolet semiconductor lasers. In yet another embodiment, a two-dimensional array of lasers can be used. In some embodiments with multiple energy sources, pre-patterning of the energy beam can be accomplished by selectively activating and deactivating the energy source.

[0210] Figures 19 to 24 A practical example of an additive manufacturing method and an apparatus for implementing the additive manufacturing method is shown. In this practical example, the additive manufacturing method is powder bed fusion, and more specifically, the powder bed fusion method is direct metal laser melting (DMLM). Methods and apparatus for implementing the method and apparatus are discussed with reference to methods and apparatus that can benefit from using the powder 10 described herein, however, the skilled person will readily understand that any other suitable additive manufacturing method and / or apparatus may be used instead.

[0211] refer to Fig.19 , showing an additive manufacturing apparatus 600, which includes a chamber 602, a bed platform 622 and a wall 624 1 to 624 w The bed platform 622 may be provided on the wall 624.1 to 624 w In this particular embodiment, the three-dimensional metal component 610 can be manufactured using a layer-by-layer method. That is, the three-dimensional metal component 610 can be made of multiple layers 612 that are fused one above the other. 1 to 612 p The powder 10 may be laser melted into a layer 646 1 To 646 L Fabricating the individual layers 612 of the three-dimensional metal component 610 1 to 612 p .

[0212] Chamber 602 may include a build section 620, a powder pool 630, at least a portion of a delivery system 640, and optionally a laser 650 and a scanner 660. Chamber 602 may be filled with a preselected gas or gas mixture (e.g., one or more inert gases, such as argon, helium, etc.), and the internal pressure of chamber 602 may be controlled at a preselected value. In addition, the internal temperature of chamber 602 may be controlled to prevent undesirable chemical reactions that may produce undesirable byproducts and / or to promote melting of powder 642.

[0213] In this embodiment, the build section 620 defines a portion where the three-dimensional metal part 610 is manufactured. The bed platform 622 can define a surface where the powder pool 630 and the three-dimensional metal part 610 will be placed. In addition, the wall 624 can be used to form a plurality of metal parts. 1 to 624 w Surrounding the bed platform 622. Wall 624 1 to 624 w The number and shape of the bed 622 depends on the shape of the bed 622. Thus, in this non-limiting embodiment, for example, four flat walls 624 1 to 624 4 Surrounding the substantially rectangular bed platform 622.

[0214] The bed platform 622 can be opposite to the wall 624 1 to 624 w For example, in this embodiment, the bed platform 622 can be actuated by the actuator 626 so that it moves relative to the wall 624. 1 to 624 w and moves relative to chamber 602 toward elevation axis 628, while wall 624 1 to 624 w The bed platform 622 does not move relative to the chamber 602. 1 to 624 wEach movement of the three-dimensional metal component 610 can generally produce a new layer 612 '. Thus, after producing the layer 612 of the three-dimensional metal component 610, i Afterwards, if Fig.19 As shown, the bed platform 622 can be lowered by a certain dimension T by the actuator 624. L , the dimension T L corresponding to the thickness of the new layer 612' to be manufactured (or, in the case of manufacturing a three-dimensional metal component 610 with layers of constant thickness, corresponding to the thickness of each layer 612 i Thickness), such as Fig. 20 shown.

[0215] In a variation, the bed platform 622 may be fixed to the chamber 602 so that the wall 624 1 to 624 w Actuated and movable relative to chamber 602, the working principle can still be the same.

[0216] In this embodiment, the powder 10 may be deposited on the bed platform 622 and the wall 624. 1 to 624 w In this way, a powder pool 630 is produced. By melting the layers 646 i A portion of the powder 10 is used to form each layer 612 of the three-dimensional metal component 610 i Afterwards, the remaining portion of the powder 10 that has not been melted remains in powder form and constitutes a powder pool 630. The powder pool 630 may have several functions. First, the powder pool 630 serves as a layer 612 that is ready to be melted to produce a three-dimensional metal part 610. i The powder pool 630 can also support the three-dimensional metal part 610 during the manufacturing of the three-dimensional metal part 610: the shape of the final product may not be self-supporting. In addition, the powder pool 630 can help dissipate the powder in each layer 646. i The energy applied to the surface during the melting process is reduced because heat transfer by conduction is generally more efficient than heat transfer by convection, and therefore, it is easier to regulate the heat at the surface of the three-dimensional metal part 610 through the powder pool 630 than through other techniques (e.g., by regulating the gas temperature inside the chamber 602).

[0217] like Figure 21 to Figure 23As shown, in this embodiment, the powder delivery system 640 feeds a powder portion 642 (composed of the same powder 10 as the powder 10 of the powder pool 630) to the powder pool 630 using a spreading tool 644, which may be a roller, a rake, or any other suitable device. The spreading tool 644 may be made of a rigid material, may be longitudinal and oriented so that the longitudinal axis of the spreading tool 644 is perpendicular to the elevation axis 628 of the bed 622, and is movable relative to the building portion 620 in a direction perpendicular to the elevation axis 628 of the bed 622. Thus, the spreading tool 644 may enable the powder delivery system 640 to feed a new layer 646' of powder 10 onto the powder pool 630, such that each new layer 646' of powder 10 defines a surface that is flat and perpendicular to the elevation axis 628 of the bed 622. Although in this embodiment, the thickness T of the new layer 646' is L Preferably, the movement of the building platform 620 is defined and / or controlled, but the powder delivery system 640 can also ensure that the powder 10 is fully supplied and effectively spread to ensure that the thickness T of the new layer 646' is L is constant over its entire surface.

[0218] like Fig.24 As shown, in this embodiment, after a new layer 646' of powder 10 is prepared and is ready to be melted to form a new layer 612' of a three-dimensional metal part 610, the power supply and / or controller can activate the laser 650, thereby providing a laser beam 652 of a predetermined power to the scanner 660. The scanner 660 can redirect the laser beam 652 onto the new layer 646' of powder 10 to scan the new layer 646' according to the desired shape of the new layer 612', thereby melting the powder 10 of the new layer 646' to form the new layer 612'. According to the thickness T of the powder 10 and the new layer 646', L and a predetermined power of the laser beam 652 , the laser beam 652 may be run through the new layer 646 ′ of powder at a predetermined speed to sufficiently melt the particles 20 of the layer 10 .

[0219] In some embodiments, due to the improved properties described herein, the powder 10 can improve one or more of the additive manufacturing process, the manufacturing apparatus 600, and the manufactured three-dimensional metal part 610. For example, in the additive manufacturing industry, since the powder is the unprocessed material at the beginning of the additive manufacturing process and since the cost of the powder feedstock is generally the most significant expense during the life cycle of the additive manufacturing apparatus, the improved consistency of the powder can affect most operations of the additive manufacturing process.

[0220] For example, when the powder is sensitive to ambient humidity, the additive manufacturing user may need to reset the powder by drying the powder to remove water adsorbed at the surface of the particles of the powder. At least some of the improved properties of the powder 10 as described herein may make such a step unnecessary, particularly because the particles 20 of the powder 10 may have a hydrophobic surface that prevents water from adsorbing thereon, and therefore, the drying step is not strictly required.

[0221] As another example, when the powder is sensitive to ambient humidity, water will adsorb to the surface of the powder. In fact, the literature has proposed that the powder can have a hydration layer consisting of three different zones defined by the mobility of water molecules. The first zone consists of molecules that are firmly bound to the surface or hydroxyl groups. The binding of this layer is considered irreversible and remains on the surface even when heated for a long time in an oven. The second layer acquires mobility, but is still limited by the firmness of the first layer, while the third layer is considered free and can be removed when heated at 65°C. However, all three layers are easily recovered when exposed to air at ambient temperature. In an additive manufacturing device, the powder may be completely hydrated unless a very strict drying regimen is implemented. Even so, the first hydration layer is usually retained. When the laser hits the powder particles, all the adsorbed water suddenly evaporates and may dissociate. This will contribute to the vapor jet carrying the highly oxidized metal protrusions. Therefore, this adsorbed water can lead to environmental damage to the additive manufacturing process. In fact, when the laser encounters the adsorbed water, the adsorbed water evaporates and partially decomposes into oxygen and hydrogen elements. The liberated oxygen and hydrogen are then free to react with the unmelted powder and the molten (and therefore highly reactive) material. Oxygen absorption in unmelted powder is often the primary reason why powders have a limited life cycle, i.e. there is a limited number of usable cycles before the powder goes out of specification due to high levels of oxygen content. In some cases, oxygen absorption in the molten material will have a detrimental effect on the final part, including the embrittlement and fatigue resistance of the final part.

[0222] At least some of the improved properties of the powder 10 as described herein can minimize or avoid such damage to the additive manufacturing environment, particularly because the absence of adsorbed water on the surfaces of the particles 20 of the powder 10 helps maintain a chemically clean environment during the additive manufacturing process, which can be advantageous in avoiding undesirable chemical reactions and / or byproducts. Without being bound by any theory, the inventors believe that the presence of moisture on the particles of comparative prior art powders is responsible for most of the oxygen absorption in three-dimensional parts made using additive manufacturing processes and in unmelted powders produced by, for example, laser powder bed fusion and electron beam additive manufacturing processes.

[0223] As another example, the high flowability of powder 10 can minimize or prevent the formation of larger secondary particles (agglomerates), which in turn can soften (e.g., sinter) or melt particles of powder 10 using less laser energy than particles of comparative prior art powders that typically contain aggregates (or "secondary particles"). Due to the cohesive forces caused by the presence of adsorbed water on the particle surfaces, those aggregates of comparative prior art powders can be formed by three-dimensionally bonded primary particles with certain gaps. In contrast, one or more of the higher apparent density of powder 10, the higher absolute weight of powder 10 for a given build thickness, and the higher thermal conductivity of powder 10 can help save laser energy during softening and / or melting. For example, the laser power may tend to overshoot to avoid forming pores caused by voids in the powder bed, which are caused by stacking faults in the cohesive powder. Having less cohesive forces produces better density, thereby causing more reliable melting. The laser power can then be reduced accordingly.

[0224] As another example, at least some of the improved properties of powder 10 as described herein can reduce the maximum temperature at the surface of layer 612' / 646' during melting of layer 646' by at least 5%, in some embodiments by at least 25%, in some embodiments by at least 50%, and in some embodiments by even more. Reducing the laser energy required to soften or melt layer 612' / 646' can not only save energy costs, but can also help conserve material and / or reduce byproduct formation by reducing the maximum peak temperature reached in the powder and at the surface below the powder layer. For example, while keeping other parameters constant, powder 10 can reduce the power of laser 652 by at least 0.5%, in some embodiments by at least 1%, in some embodiments by at least 2%, in some embodiments by at least 5%, in some embodiments by at least 10%, and in some embodiments by even more.

[0225] The additive manufacturing process can be particularly time consuming because the layer-by-layer process involves repeated steps. Among these repeated steps, the re-coating step includes spreading a thin layer 646' of powder 10 on the three-dimensional metal part 610 and on the powder pool 630 using a spreading tool (e.g., roller, rake) 644. As another example, the enhanced flowability of the powder 10 described herein can speed up the process, and thus, the three-dimensional metal part 610 can be multiplied by the layer 612 1 to 612 p The additive manufacturing method is improved by a gain factor of the number of

[0226] In a similar manner, in a repeated step, the scanning step includes scanning the new layer 646' of the powder 10 with the laser beam 652 at a predetermined speed to melt the new layer 646' of the powder 10 and form a new layer 612' of the three-dimensional metal part 610. In this embodiment, because less energy can be used to soften or melt the particles 20 of the powder 10, the scanning speed of the laser beam 652 can be increased, thereby speeding up the scanning step. For example, in some embodiments, while keeping other parameters constant, the powder 10 can increase the scanning speed of the laser beam 652 by at least 0.5%, in some embodiments by at least 1%, in some embodiments by at least 2%, in some embodiments by at least 5%, in some embodiments by at least 10%, and in some embodiments by even more.

[0227] As another example, the increased apparent density of the powder 10 described herein can increase the thermal conductivity of the powder pool 630 and can improve the consistency of this property of the powder pool 630. The high thermal conductivity and its consistency can be easily predicted by the powder 10 and the layer 612 of the three-dimensional metal part 610. 1 to 612 p For example, in some embodiments, the ratio of the thermal conductivity of the powder pool 630 filled with powder 10 to the thermal conductivity of the powder pool 630 filled with a similar but untreated powder can be at least 1.05, in some embodiments at least 1.10, in some embodiments at least 1.15, in some embodiments at least 1.20, and in some embodiments even greater.

[0228] Much research effort has been spent on topological optimization of end products (with a strong bias towards the aviation and aerospace industries) using additive manufacturing, where the strength-to-weight ratio is of utmost importance. Since the regulations regarding all structural elements within an aircraft are extremely stringent, it is necessary to manufacture all structural elements with standardized materials and methods. Unfortunately, current additive manufacturing methods introduce inconsistencies, thus limiting the use of additive manufactured parts to non-structurally critical components.

[0229] As another example, at least some of the improved properties of the powder 10 as described herein can result in significantly reduced variability associated with the properties of the material (i.e., the powder used to make the three-dimensional metal part 610). Thus, batch-to-batch consistency of the powder 10 can be increased and product performance can be more stable by reducing differences associated with problems related to poor apparent density and / or powder flowability issues, such as unstable flowability values ​​in the funnel assay, powder non-flow, sensitivity to humidity, and sensitivity to humidity exposure history. This can mean better process control in the additive manufacturing device and, therefore, a final product with fewer defects and deficiencies.

[0230] For example, better flowability can reduce the proportion of aggregates 28 found in the particles. For example, in some embodiments, the weight of aggregates 28 that are at least 5 times larger than the average of the particles accounts for no more than 5 weight percent, in some embodiments no more than 2 weight percent, in some embodiments no more than 1 weight percent, in some embodiments no more than 0.1 weight percent, in some embodiments no more than 0.01 weight percent, and in some embodiments even less (e.g., 0%).

[0231] Metal parts

[0232] As discussed herein above and below, the improved physical properties of the powders of the present disclosure and / or the improved additive manufacturing methods and apparatus described herein provide three-dimensional metal parts with improved properties.

[0233] For example, compared to when using (for example) FIG. 32E to FIG. 32H The comparison shown is the surface finish obtained when manufacturing three-dimensional metal parts with prior art powders, when using (for example) FIG. 32A to FIG. 32D When the three-dimensional metal parts are manufactured according to the powder of the present disclosure, the three-dimensional metal parts can have better surface finish. In addition, due to the improved properties of the powder, the three-dimensional metal parts manufactured using the powder of the present disclosure can have better ultimate tensile strength (UTS) and / or elongation at break (A%), which in turn reduces the presence of pores and / or microcracks in the body of the metal part.

[0234] For example, the inventors compared the mechanical properties of three-dimensional metal parts made from Al-Si7-Mg powders printed with the same parameters in a blind test study. The as-printed parts were hot isostatic pressed (HIP) for 3 hours at 14.75 KSI pressure and 960℉+ / -25℉. The parts were then treated in a 1010-1013 solution for 90 minutes and aged at 317±5℉.

[0235] The obtained three-dimensional metal parts were tested according to ASTM E8 / E8M-16a. The test specimens constructed with the powder according to the present disclosure showed an increase in yield strength of approximately 12% to 18%, and an increase in ultimate tensile strength of approximately 8% to 13% (see Fig.47 and Fig.48 ). Increases were observed in all x, y, x=y(w), and z sample directions relative to the build orientation.

[0236] In some embodiments, as discussed in the context of this document, the surface finish of the surface of the three-dimensional metal 610 can be characterized as Ra < D90 for metal powders used in additive manufacturing methods.

[0237] In some embodiments, the ratio of the surface finish Ra of the outer surface of the three-dimensional metal part 610 to the surface finish of the outer surface of a similar final product made using a comparative prior art powder can be less than 0.95, in some embodiments less than 0.90, in some embodiments less than 0.85, and in some embodiments even less. For example, a three-dimensional metal part was made using an embodiment of the powder 10 described herein, and the inventors achieved a surface finish characterized by an Ra of 19 to 20 microns and / or an Rz of 126 to 143 microns, which is an improvement over the surface finish of a metal part made using a comparative prior art powder, which was characterized by an Ra of 25 to 35 microns and / or an Rz of 238 to 342 microns.

[0238] In some embodiments, the low proportion of aggregates in powder 10, the high apparent density of powder 10, and the layer 612 1 to 612 P and 646 1 To 646 L The reduced thickness T L The three-dimensional metal 610 may be made to have the properties described herein.

[0239] In some embodiments, a low proportion of aggregates 28 in powder 10 can result in layers having a better quality topology, resulting in a lower proportion of defects caused by aggregates when a spreading tool spreads the particles of the layer. Fig.25A Defects in the layer shown (left) can lead to defects such as pores and / or microcracks 38 in the final product, such as Fig.25A (right). These pores and / or microcracks 38 can change the structure of the final product. Fig.25B As shown, the final product using the powder 10 has significantly reduced porosity and / or microcracks 38 (if present). For example, in some embodiments, the final product additively manufactured using the powder 10 can be at least 90% free of porosity, in some embodiments at least 95% free of porosity, in some embodiments at least 98% free of porosity, in some embodiments at least 99% free of porosity, and in some embodiments even higher (e.g., about 100% free of porosity).

[0240] In some cases, the increase in the amount of pores and / or microcracks 38 can reduce the ultimate tensile strength and / or elongation at break of the metal component structure. This can be observed by comparing the tensile test results of the three-dimensional metal component 610 (e.g., rod) manufactured using additive manufacturing with the tensile test results of the same structure manufactured conventionally (e.g., by extrusion). In addition, in some cases, even if the pores and / or microcracks 38 have little or no effect on the ultimate tensile strength and / or elongation at break of the structure, the pores and / or microcracks can also cause cracks and reduce the fatigue resistance of the structure. This can be observed by comparing the fatigue test results of the three-dimensional metal component 610 (e.g., rod) manufactured using additive manufacturing with the fatigue test results of the same structure manufactured conventionally (e.g., by extrusion). For this reason, it is generally necessary to process the components manufactured using additive manufacturing of prior art powders to improve the surface finish. In this embodiment, the three-dimensional metal component 610 manufactured using powder 10 using additive manufacturing may not need to be processed after additive manufacturing.

[0241] In a similar manner, in this embodiment, the metal microstructure of the three-dimensional metal component 610 (including the metal material of the three-dimensional metal component 610 and the pores (if any) of the three-dimensional metal component 610) can have properties (e.g., mechanical properties) close to those of the bulk of the metal material. For example, in some embodiments, the ratio of the ultimate strength of the metal microstructure of the three-dimensional metal component 610 manufactured by additive manufacturing using the particles 10 to the ultimate strength of the bulk metal material can be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher (e.g., greater than 100%). In some embodiments, the ratio of the tensile elongation at break of the metal microstructure of the three-dimensional metal component 610 manufactured by additive manufacturing using the particles 10 to the tensile elongation at break of the bulk metal material can be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher. In some embodiments, the ratio of the toughness of the metal microstructure of the three-dimensional metal component 610 manufactured by additive manufacturing using the particles 10 to the toughness of the bulk metal material can be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher. In some embodiments, the ratio of the toughness of the metal microstructure of the three-dimensional metal component 610 manufactured by additive manufacturing using the particles 10 to the toughness of the bulk metal material can be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher. 6 The maximum stress amplitude before fracture after 10 cycles is 10 6The ratio of the maximum stress amplitude before fracture after 10 cycles may be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher.

[0242] As another example, the powder 10 may have a layer 612 that can reduce 1 to 612 P and 646 1 To 646 L Thickness T L properties (e.g., flowability, apparent density, PSD, low aggregate ratio, etc.). For example, in some embodiments, layer 646 1 To 646 L Thickness T L It may be no greater than 50 μm, in some embodiments no greater than 40 μm, in some embodiments no greater than 30 μm, in some embodiments no greater than 20 μm, in some embodiments no greater than 10 μm, and in some embodiments even smaller.

[0243] In one embodiment, the low proportion of aggregates in the particles 20, the high apparent density of the powder 10, and the layer 612 1 to 612 P and 646 1 To 646 L The reduced thickness T L The three-dimensional metal 610 can be made to have properties close to those of bulk powder materials, ie, maintain its ultimate strength, its elongation at break, its toughness and / or its fatigue resistance.

[0244] For example, in some embodiments, the ratio of the ultimate strength of the three-dimensional metal 610 manufactured by additive manufacturing using the particles 10 to the ultimate strength of a similar final product manufactured conventionally (e.g., by extrusion) may be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher (e.g., greater than 100%). In some embodiments, the ratio of the elongation at break of the three-dimensional metal 610 manufactured by additive manufacturing using the powder 10 to the elongation at break of a similar final product manufactured conventionally (e.g., by extrusion) may be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher. In some embodiments, the ratio of the toughness of the three-dimensional metal 610 manufactured by additive manufacturing using the powder 10 to the toughness of a similar final product manufactured conventionally (e.g., by extrusion) may be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher. In some embodiments, the final product 10 manufactured by additive manufacturing using the powder 10 6 The maximum stress amplitude before fracture after 10 cycles is 10 times that of a similar final product manufactured conventionally (e.g., extrusion). 6 The ratio of the maximum stress amplitude before fracture after 10 cycles may be at least 80%, in some embodiments at least 90%, in some embodiments at least 95%, in some embodiments at least 99%, and in some embodiments even higher.

[0245] In this embodiment, the powder 10 may exhibit Fig.36 10. The separation performance shown. More specifically, the powder 10 can be fluid so that particles with lower apparent density float and particles with higher apparent density settle. For example, in one embodiment, impurities and / or aggregates can penetrate into the pool 730 of powder 10 (e.g., during use or transportation of the powder 10). Impurities and aggregates can generally have lower apparent densities. After a certain period of time, when impurities and aggregates are present, the impurities and aggregates can be separated to the upper part of the powder pool 730.

[0246] Practical implementation

[0247] The improved surface finish of the three-dimensional metal parts described herein may provide the possibility of manufacturing three-dimensional metal parts for industries such as telecommunications, aerospace, etc., which have particularly stringent requirements for high-quality surface finish.

[0248] In some embodiments, the improved properties of the powders of the present disclosure described herein enable the fabrication of a one-piece integrally formed metal component, which is fabricated by a powder bed fusion additive manufacturing method that uses a laser as a source of thermal energy to heat and melt selected regions of a metal powder bed to build the metal component in successive layers. In particular, the metal component includes an internal cavity, and the internal cavity in turn has side walls, where the side walls have portions that are configured to exclude access to channels from the exterior of the metal component by using machining tools (e.g., rotary tools, electrical discharge machining, etc.) and performing surface finishing by subtractive machining of the side wall portions. For example, the portions having a surface finish are characterized in that the Ra of the powder < D90. The geometry of the cavity is such that the tool cannot reach. In other words, it is not possible to insert a tool from the exterior of the part into the cavity to machine the inner surfaces and provide a better finish for these surfaces than the finish obtained by the additive manufacturing method.

[0249] For this reason, Fig.49 Examples of such geometries that impede such tool access are shown. For example, such geometries can include fully enclosed cavities or open cavities, but the open cavities have portions that cannot be directly observed from the cavity opening on the outer side of the part and into which a machining tool (e.g., rotary tool, electrical discharge machining, etc.) cannot be inserted through the opening, or have portions that may be observable, but their access paths are too small or too deep for a machining tool to accommodate. For example, any other cavity arrangement having angled channels, fully enclosed cavities that do not open to the exterior of the part, or portions of the wall that cannot be observed from the cavity opening.

[0250] In some embodiments, the improved properties of the powders of the present disclosure described herein enable the fabrication of a one-piece integrally formed metal component, which is fabricated by a powder bed fusion additive manufacturing method that uses a laser as a source of thermal energy to heat and melt selected regions of a metal powder bed to build the metal component in successive layers. The metal component includes a surface having an inherent surface finish, which is characterized in that the Ra of the powder < D90. The reader will readily understand that herein, the term "inherent" is used to denote the natural finish obtained by the powder bed fusion method.

[0251] The surface finish described herein may be characterized by Ra <, or < 0.90x, or < 0.80, or < 0.70x, or < 0.60x, or < 0.50x, or < 0.40x, or < 0.30x, or 0.25x, or < 0.20x the D90 size of the additive manufacturing powder used in a powder bed fusion additive manufacturing process using a laser as the thermal energy source, which is surprising and unexpected, at least because one would typically expect the surface finish to reflect the D90 particle size determination of the additive manufacturing powder, in other words, one would expect the surface irregularities to be essentially the same as the D90 size of the powder.

[0252] For example, when manufacturing waveguides for microwave transmission, surface roughness is a key factor. Undesirable surface roughness may occur due to various reasons, such as polishing of irregular waveguide structures, uneven surface coating, or wrinkles on the surface when manufacturing the waveguide. The presence of surface roughness affects the propagation constant and attenuation constant of the waveguide and changes the cutoff frequency of each waveguide mode, thereby affecting electromagnetic wave propagation. Traditionally, passivated millimeter-wave and THz components are manufactured by computer numerical control (CNC), micromachining, electrical discharge machining (EDM), or injection molding.

[0253] In some embodiments, the one-piece, integrally formed metal component is a waveguide, which is a hollow metal tube used to carry radio waves. Waveguides are made almost entirely of metal and are mostly made of rigid structures. Due to the skin effect at high frequencies, the current along the wall typically only penetrates a few microns into the metal on the inner surface. Since most of the resistance losses occur here, it is important that the conductivity of the inner surface remains as high as possible.

[0254] In some embodiments, such as Figures 49 to 62 As shown, three-dimensional metal component 610 can be a one-piece component and can include cavity 720. Cavity 720 can include cavity surface 732 defining an outer peripheral surface of the cavity. At least a portion of cavity surface 732 is inaccessible from outside of component 610.

[0255] For example, in some cases, cavity 720 can be a closed cavity that is not connected to the exterior of component 610. Such a geometry can be achieved using additive manufacturing, but cannot be achieved using traditional machining (e.g., turning, milling, drilling, etc.) because cavity 720 is not connected to the exterior of one-piece component 610.

[0256] In some cases, likewise, cavity 720 may be connected to the exterior of one-piece component 610, but may be configured such that at least a portion 744 of cavity surface 732 is barely accessible or not accessible at all by conventional machining tools (e.g., turning tools, milling tools, drilling tools, etc.). Thus, in these embodiments, it may not be possible to improve the surface finish of portion 744 of cavity surface 732 using conventional machining tools.

[0257] Component 744 may be inaccessible due to a combination of factors. For example, in some embodiments, cavity 720 may be an elongated cavity, such as Figures 49 to 62 In some embodiments, the elongated cavity 720 can be relatively narrow (for example, the dimensions of the inner cavity of the rectangular waveguide WR3 are 0.034 inches [i.e., 0.8636 mm] and 0.017 inches [i.e., 0.4318 mm]). In some embodiments, the elongated cavity 720 can have a complex shape, such as an "H" shape, such as Figures 49 to 51 Other shapes of the elongated cavity 720 may include, for example, a circular shape (e.g. Fig.52 and Figure 59 to Figure 62 As shown), rectangle (as Figure 53 to Figure 58 as shown), or a square (as Fig.61 ). In some embodiments, the elongated cavity 720 can be relatively long. In some embodiments, the elongated cavity 720 can include one, two, three, or more bends 736 and / or offsets 738 of at least 5°, at least 15°, at least 30°, at least 45°, at least 60°, at least 90°, at least 135°, at least 180°, at least 360°, or even greater.

[0258] In some embodiments, the one-piece three-dimensional metal component 610 can be a waveguide. The waveguide 610 can be configured to guide waves (such as electromagnetic waves or sound waves) with minimal energy loss by limiting the energy transmission in one direction. To this end, the waveguide 610 can include an elongated body 810 having two ends 812 configured to receive and / or output waves. The elongated cavity 720 can extend between the ends 812. The elongated body 810 can also include a bend 736 and / or an offset 738.

[0259] The performance (e.g., efficiency, efficacy, durability, etc.) of the waveguide 610 can be related to the surface finish of the surface of the elongated body 810, including the surface finish of the cavity surface 732. For example, conductor surface roughness can result from the introduction of unsintered metal particles at the surface of a part made with additive manufacturing, and in particular from the printed part, which results in an imperfect conductor with wrinkles and / or microcracks. The inventors contemplate that the use of the additive manufacturing powders described herein in an additive manufacturing process can reduce conductor surface roughness.

[0260] The method for characterizing surface roughness is established in the DIN 4768 standard. Alternatively, this parameter can be determined using conventional techniques using a surface roughness tester that uses a scanning cantilever in physical contact with the sample to determine the roughness parameter.

[0261] Powder recovery / recycling

[0262] In one aspect, the present disclosure provides a method and system for powder bed fusion additive manufacturing that automatically collects powder material for reuse after a printing cycle.

[0263] Improved powder handling may be another aspect of the improved additive manufacturing system. The build platform supporting the powder bed can be tilted, inverted, and shaken to substantially separate the powder bed from the build platform in the hopper. The powder material forming the powder bed can be collected in the hopper for reuse in subsequent printing jobs. The powder collection method may be automated, and vacuum handling or gas injection systems may also be used to aid in powder movement and removal.

[0264] In practical implementations, the method and system according to the present disclosure may include a device for evaluating the purity of the powder 10 contained in the powder pool 730 and / or filtering the powder 10.

[0265] Fig.37 An apparatus 700 is shown as a non-limiting embodiment of an apparatus for evaluating purity and filtering a powder pool 730. The apparatus 700 includes a platform 722 as a powder bed and a plurality of walls 724. 1 To 724 W The apparatus 700 includes a sensor 742 to sense a property of the powder pool 730. In one embodiment, the sensor 742 may include a camera, and the property of the powder 10 may include a visual appearance of an upper surface 746 of the pool 730. In one embodiment, the visual appearance includes the size and color of the particles 20.

[0266] In this embodiment, the camera 742 is connected to a processing device 780 to automatically assess or allow an operator to assess the purity of the powder 10 contained in the powder pool 730. In some embodiments, the device 700 includes a processing device 780, while in other embodiments, the processing device 780 is a remote processing device. The processing device 780 may include an interface 782, a processing portion 788, and a memory portion 790 implemented by suitable hardware and / or software.

[0267] Interface 782 includes one or more inputs and outputs that enable processing device 780 to receive input signals from and send output signals to other components (including sensor 742 in this embodiment) that are connected (i.e., directly or indirectly, for example, via a network) to processing device 780. For example, in this embodiment, inputs to interface 782 are performed by a wireless receiver to receive sensor signals from sensor 742. Outputs to interface 782 are performed by a transmitter to transmit signals that may be indicative of a sensed characteristic or an assessment made by processing device 780.

[0268] The processing portion 788 includes one or more processors for executing processing operations that perform the functions of the processing device 780. The processor of the processing portion 788 may be a general-purpose processor that executes program code stored in the memory portion 790. Alternatively, the processor of the processing portion 788 may be a special-purpose processor including one or more pre-programmed hardware or firmware elements (e.g., an application-specific integrated circuit (ASIC), an electrically erasable programmable read-only memory (EEPROM), etc.) or other related elements.

[0269] The memory portion 790 includes one or more memories for storing program code executed by the processing portion 788 and / or data used during the operation of the processing portion 788. The memory portion 790 can also be used to store data (e.g., dimension readings, reference dimensions). The memory of the memory portion 790 can be a semiconductor medium (including, for example, solid-state memory), a magnetic storage medium, an optical storage medium, and / or any other suitable type of memory. The memory of the memory portion 790 can be, for example, a read-only memory (ROM) and / or a random access memory (RAM).

[0270] In some embodiments, two or more elements of the processing device 780 may be implemented by physically distinct devices from one another and may be connected to one another via a bus (e.g., one or more electrical conductors or any other suitable bus) or via a communication link that may be wired, wireless, or both. In other embodiments, two or more elements of the processing device 780 may be implemented by a single integrated device.

[0271] In this embodiment, the interface 782 may be configured to receive a signal from the camera 742 indicating the visual appearance of the upper portion of the powder pool 730. The processing device 786 may be configured to evaluate the purity of the powder 10 in the powder pool 730 by comparing the signal sensed by the camera 742 with reference data, or the processing device 786 may be configured to display an image of the powder pool to the operator to allow the operator to evaluate the purity of the powder 10 contained in the pool 730.

[0272] When the processing device 780 or the operator determines that the powder pool 730 contains impurities and / or aggregates, these impurities and / or aggregates can be removed from the powder pool 730 manually or automatically by the operator. For example, in this embodiment, the powder bed 722 can be a lifting powder bed that can be lifted and lowered by the actuator 726. The device 700 can also include a spreading tool 744 to flatten the upper surface of the powder pool 730. The actuator 726 and the spreading tool 744 can be connected to the processing device 780. When the powder pool 730 includes impurities and / or aggregates, the processing device 780 can send a signal to the actuator 726 to lift the powder pool 730, thereby pushing the top surface of the powder pool 730 to be higher than the wall 724 of the device 700. 1 To 724 W The top edge of the powder pool 700 is formed, and the upper portion of the powder 10 containing impurities and / or aggregates flows out of the building platform 720 of the device and is removed from the pool 730. To facilitate this process, the processing device 780 can send a signal to the spreading tool 744, which can trigger the spreading tool 744 to remove excess powder from the pool 730.

[0273] In some embodiments, vibration may facilitate separation of powder 10. When impurities and aggregates are subjected to vibration, they may separate at any suitable rate.

[0274] One or more steps of vibrating the powder pool 730 at a predetermined frequency for a predetermined duration may be added to the above method to evaluate the purity of the powder 10 in the powder pool 730 and / or to remove impurities and / or aggregates from the powder 10 in the powder pool 730. For example, Fig.38 As shown, the method for evaluating the purity of powder 10 in a powder pool 730 may include: step 810 of vibrating the powder pool 730 at a predetermined frequency for a predetermined duration; step 820 of sensing a characteristic (e.g., visual appearance) of the powder pool 730 using one or more sensors (e.g., a camera); step 830 of evaluating the presence of impurities and / or agglomerates based on the characteristics sensed in step 820; and step 840 of removing impurities and / or agglomerates from the powder pool 730.

[0275] For example, the device 700 may include a vibration actuator 760 connected to the processing device 780. When the processing device 780 sends a signal to the vibration actuator 760, the vibration actuator may vibrate at a predetermined frequency for a predetermined duration, thereby promoting the separation of impurities and / or aggregates to the top layer and / or bottom layer of the powder pool 730.

[0276] Other improvements in manufacturing methods

[0277] In some embodiments, powder 10 may also allow for other improvements to the manufacturing method and / or manufacturing apparatus 600, as described further below.

[0278] For example, in some embodiments, the improved flow properties of the powders 10 described herein can make the particles 20 more fluid-like, i.e., have more fluid-like behavior. This behavior can be used for new methods of additive manufacturing.

[0279] Therefore, refer to Fig. 27 and Fig.28 In some embodiments, the additive manufacturing 600 for powder bed fusion may be without a spreading tool (e.g., rollers, rakes, etc.). In this example, during the recoating step, instead of lowering the three-dimensional metal part 610 after melting each layer 646' into a new layer 612' and spreading the layer 646' of powder 10 on the three-dimensional metal part 610 using the spreading tool 644, the three-dimensional metal part 610 may be contained within the wall and the layers 612' may be formed into a new layer 612'. i After formation, the predetermined volume V P The particles 10 are introduced or spread on the three-dimensional metal part 610. Because the particles 10 are in a fluid state, the particles 10 can cover the final product horizontally, thereby producing a layer 646' of constant thickness. For example, in some embodiments, Fig.39 As shown, the additive manufacturing 600 may be provided with a vibration actuator 696 that generates vibrations, thereby providing energy to the powder 10 so that the particles move relative to each other to horizontally cover the final product, thereby generating a layer 646' when the vibration of the vibration actuator 696 ends.

[0280] In another example, additionally referring to Figure 29 to Figure 31 , the building portion 620 may include an actuator 680 located at the lower side of the powder pool 630 but offset from the three-dimensional metal component 610. In each re-coating step, the actuator 680 may be inserted into the powder pool 630 by a predetermined volume so that the upper surface of the powder pool 630 is higher than the dimension T relative to the three-dimensional metal component 610. L ,like Fig.30 As shown, and until it covers the three-dimensional metal part 610 with the same size, as shown Fig.31 shown.

[0281] In another example, additionally referring to Fig.40 , the manufacturing device 600 may include a bottom-up 3D printer. In this embodiment, the building platform 620 includes a wall 624 1 to 624 W and a bed 690, which in this example is a static platform. The fixed bed 690 may include an interface 692 that is at least partially transparent to at least a portion of the laser beam 652. In this embodiment, the powder pool 630 is contained in a wall 624. 1 to 624 Wand a cavity defined by the bed 690. In this embodiment, the bottom-up 3D printer includes a lifting platform 684 that can be lowered and / or raised by an actuator 626, and the lifting platform 684 may include a surface 693 at the lower side of the lifting platform 684 configured to interlock with the three-dimensional metal component 610 while manufacturing the three-dimensional metal component 610. The laser 650 and the scanner 660 may be located at the lower side of the powder pool 630. First, the lifting platform 684 may be positioned so that the distance between the surface 693 and the bed 690 corresponds to the dimension T L The laser beam 650 may then pass through the transparent interface 692 of the bed 690 to scan and melt particles of the powder pool 630 disposed in the gap between the bed 690 and the lifting platform 684, so that the molten material adheres to the surface 693 of the lifting platform 684. 1 Thereafter, the actuator 626 can move the platform 684 and the first layer 612 bonded thereto. 1 Increase size T L An actuator 696 , such as a vibration actuator, may be coupled to at least a portion of the build platform 620 of the bottom-up 3D printer to generate vibrations that will promote particle flow of the powder pool 630 , such that the particles flow evenly in the newly created gap between the platform 684 and the bed 690 .

[0282] It may be necessary to empty the amount of powder in the three-dimensional metal component 610. In this embodiment, a method for emptying the three-dimensional metal component 610 of the powder that is retained in the hollow space of the three-dimensional metal component 610 is provided, wherein the powder exhibits enhanced flowability characteristics of the powder 10, thereby being able to reduce the time and cost of post-manufacturing processing. For example, in this embodiment, the manufacturing device 600 may include an emptying device 830, the emptying device 830 including a connecting device 832 for clamping the three-dimensional metal 610 and an actuator 834 for moving the final product in the space so that the powder in the empty space of the three-dimensional metal component 610 flows out: the process may be repeated to produce the layer 612 1 to 612 L , and fuses them with their respective surrounding layers until three-dimensional metal part 610 is manufactured from the bottom up by build platform 620.

[0283] In another example, additionally referring to Figure 41 to Figure 44, powder 10 can speed up the post-manufacturing process. For example, in some embodiments, the three-dimensional metal part 610 can be a hollow part. After manufacturing the three-dimensional metal part 610, some powder remains in the hollow space of the final product. Although this method is time consuming for conventional prior art powders, in this embodiment, powder 10 can speed up the method by up to at least 25%, or at least 35%, or at least 45%, or at least 50% in terms of the time required to complete the method.

[0284] In another example, the powder 10 can cause the three-dimensional metal part 610 to have a new geometry. For example, in some embodiments, the three-dimensional metal part 610 can be a hollow part. After manufacturing the three-dimensional metal part 610, some powder remains in the hollow space of the three-dimensional metal part 610, so it may be necessary to empty the three-dimensional metal part 610 of this amount of powder. However, when the hollow space is difficult to reach (e.g., due to a narrow elongated shape, due to an elbow, etc.), it may not be possible to use conventional prior art powder additive manufacturing of the three-dimensional metal part 610. In this embodiment, a method of emptying the three-dimensional metal part 610 of the powder that remains in the hollow space of the three-dimensional metal part 610 is provided, wherein the three-dimensional metal part 610 includes a long, narrow, and complex hollow shape.

[0285] In another example, additionally referring to Fig.45 , the manufacturing apparatus 600 may be configured to sense the properties of the powder 10 and change at least one of its settings accordingly. In this embodiment, the manufacturing apparatus 600 may include a blower 656 and a camera 658 to ensure that the powder 10 is spread in layers 612 of the three-dimensional metal part 610 being manufactured by the spreading tool. 1 to 612 LAfter the powder 10 is evenly spread on one of the surfaces, the surface of the powder 10 is evenly spread and does not include agglomerates or voids, which may be generated by agglomerates and may create weak points in the three-dimensional metal part 610. When the camera 658 detects irregular features on the surface of the powder 10, the blower 656 may be directed toward the aggregates and generate an air flow to remove the aggregates. The spreading step may be repeated to ensure that the powder 10 is evenly spread before the powder 10 is scanned by the laser beam 652. In some embodiments, the operator can adjust the setting of the blower 656 to ensure that the blower 656 blows enough air to remove the aggregates, but not too much, because this may remove too much powder 10 and produce a cloud of suspended powder particles 20, which may reduce the efficiency of manufacturing. In this example, the operator can input one or more characteristics of the powder 10 used to manufacture the three-dimensional metal part 610 (e.g., the size of the particles 20, flowability, etc.). In other embodiments, this can be automatically achieved by the manufacturing device 600. For example, the manufacturing apparatus 600 may include sensors to determine the properties of the powder 10 (e.g., the size, flowability, etc. of the particles 20) and accordingly adjust the settings of the blower 656. The manufacturing apparatus 600 may also use a machine learning algorithm to determine the best working settings for different types of powders based on predetermined properties (e.g., the size, flowability, etc. of the particles 20).

[0286] In at least some of the embodiments described above, manufacturing apparatus 600 may include a processing device similar to processing device 780 of apparatus 700, and the processing device controls and / or communicates with the electromechanical components of manufacturing apparatus 600 described herein. An interface of the processing device of manufacturing apparatus 600 enables an operator to input commands and view data, for example, via a display of the interface.

[0287] In another example, additionally referring to Fig.45 , the manufacturing apparatus 600 can be configured to sense the properties of the powder 10 and change at least one of its settings accordingly. In particular, in this embodiment, the manufacturing apparatus 600 can include a processing device 880 that is configured to control the operation of at least some tools of the manufacturing apparatus 600 (e.g., laser 650, scanner 660, rake 644, actuators 626, 696, etc.) according to a set of predetermined settings 882. In practice, the processing device 880 can associate a setting value 886 with each predetermined setting 882, and the control of the tools of the manufacturing apparatus 600 can depend on the setting value 886 of the predetermined setting 882.

[0288] In this embodiment, additional reference is made to Figure 66 to Figure 69 , the processing device 880 may include a plurality of setting value sets 890 1 Up to 890 S, each set includes a specific setting value 886 for each predetermined setting 882. For example, in some embodiments, each setting value set 890 i This may include laser power settings, laser scan speed settings, layer thickness settings, rake speed settings, etc.

[0289] Each setting value set 890 1 Up to 890 S One or more characteristics 892 of the powder placed in the manufacturing device 600 1 To 892 C and / or one or more desired characteristics of the final product 610. For example, the processing device 880 may include a processor having a first characteristic 892 1 The first set of setting values ​​associated with the powder 890 1 and with the second characteristic 892 2 The second set of setting values ​​associated with the powder 890 2 .

[0290] Specifically, in this example, the first setting value set 890 1 is associated with higher powder flowability, and the second set of settings 890 2 Associated with lower powder flowability. Feature 892 1 To 892 C Other examples of may be related to the material composition of the powder particles, the PSD of the powder, the desired surface finish of the final product, the desired porosity of the final product, etc.

[0291] In this embodiment, the processing device 880 is configured to evaluate the characteristic 892 1 To 892 C And according to the characteristics 892 1 To 892 C Automatically select setting value set 892 1 To 892 S The determination of the properties 892 may be done automatically (e.g., using a sensor in the manufacturing apparatus 600 to sense the properties of the powder, using a computer readable file including the desired properties of the final product 610, etc.) or via user input. 1 To 892 C assessment.

[0292] In this regard, processing device 880 may include an interface 912 , a processing portion 918 , and a memory portion 920 implemented by suitable hardware and / or software, and may be implemented in a manner similar to interface 782 , processing portion 788 , and memory portion 790 of processing device 780 .

[0293] In this embodiment, the interface 912 also includes a graphical user interface (GUI) 914 to interact with the operator, display information and enable user input. The interface 912 can be connected to sensors in the manufacturing device 600 to automatically evaluate the characteristics 892 1 To 892 C , and may be further connected to tools of the manufacturing apparatus 600 so that the processing apparatus 880 can control the above-mentioned tools.

[0294] The memory portion 920 may include computer readable files that include desired characteristics of the final product 610. The memory portion 920 may also include a set of settings 890. 1 Up to 890 S and a computer readable file including computer readable instructions to convert the characteristic 892 1 To 892 C With the set value collection 890 1 Up to 890 S Associated.

[0295] The processing portion 918 may process the input data to generate setting values ​​for operating a tool of the manufacturing apparatus 600 .

[0296] Atmosphere Control

[0297] In another example, manufacturing apparatus 600 can include a device for controlling the atmosphere within manufacturing apparatus 600 that takes into account one or more improved properties of the powders described herein.

[0298] In practice, debris (e.g., metal vapor, molten metal, or plasma) may sometimes be generated in an enclosed space (e.g., above a material bed). The debris may float in the atmosphere of the enclosed space. The floating debris may change at least one characteristic of the energy beam (e.g., its power per unit area) during its passage through the enclosed space toward the material bed. The debris may change (e.g., damage) various components of the 3D printing system (e.g., optical windows). Some existing 3D printers establish a lateral flow of gas to reduce debris in the atmosphere of the enclosed space. However, some of these lateral flow solutions may result in undesirable airflow structures (e.g., stagnation, recirculation of gas within the enclosed space, which may produce a stable state), which cannot completely solve the problem associated with debris. Therefore, it may be necessary to establish an airflow solution that can avoid undesirable airflow structures and be able to remove debris from the atmosphere of the enclosed space. Sometimes, during the 3D printing process, various material forms are transmitted by gas. The material form may include (e.g., fine) powder or carbon black. Some gas-transmitted materials may react easily with reactants (e.g., oxidants). Some gas propagation materials may react violently (e.g., when contacted with a reactant). Sometimes, it may be desirable to provide low leakage of a reactive agent (e.g., oxygen in an ambient atmosphere) in one or more segments of a 3D printer. Sometimes, it may be desirable to isolate the interior of one or more segments of a 3D printer from harmful (e.g., violently reactive) levels of a reactant (e.g., a reactant present in the atmosphere outside of one or more segments of a 3D printer). Sometimes, it may be desirable to maintain a non-reactive (e.g., inert) atmosphere in at least one segment of a 3D printer (e.g., before, during, and / or after 3D printing).

[0299] Sometimes, the gas-borne material may be collected within a filtration mechanism. The gas-borne material may react violently (e.g., ignite, catch fire, and / or burn) when exposed to an atmosphere containing reactive reagents (e.g., an ambient atmosphere containing oxygen). It is desirable to introduce a filtration mechanism that can be separated (e.g., isolated) from an external (e.g., ambient) atmosphere containing reactive reagents. It may be desirable to introduce such a filtration mechanism that maintains an inert internal atmosphere around the filter at least during the filtering operation and / or removal of the filter from the filtration mechanism. It may be further desirable, for example, to facilitate the uninterrupted replacement of filters in the filtration mechanism when the filter becomes clogged and needs to be replaced and / or refurbished, (e.g.) to facilitate the continuous separation of gas-borne materials from recirculating gases in at least one or more page sections of a 3D printer during a 3D printing process.

[0300] In some embodiments, as discussed further below, powder characteristics can impact the above issues.

[0301] For example, the apparatus 600 may include one or more gas inlets and outlets and suitable controllers for providing a gas flow within the enclosed space sufficient to melt the powder to form the layer 612 of the final product. 1 to 612 p The atmosphere within the enclosure is appropriately controlled before, during and / or after, while being less than a threshold value to avoid disturbing the powder bed and / or lifting powder particles within the enclosure, which would otherwise create a cloud of powder particles and hinder operation of the device 600.

[0302] In some embodiments, the device 600 may additionally or alternatively include a fan 666 for blowing or sucking gas to generate the above-mentioned airflow.

[0303] In some embodiments, an operator may input one or more properties of the powder 10 used to manufacture the three-dimensional metal part 610 (e.g., size, fluidity, etc. of the particles 20) to control the airflow properties. In other embodiments, this may be automatically implemented by the manufacturing device 600. For example, the manufacturing device 600 may include sensors to measure the properties of the powder 10 (e.g., size, fluidity, etc. of the particles 20) and adjust the settings that control the airflow properties. The manufacturing device 600 may also use a machine learning algorithm to determine the optimal working settings for different types of powders based on predetermined properties (e.g., size, fluidity, etc. of the particles 20).

[0304] Variants

[0305] Other additive manufacturing methods do not rely on a powder bed, such as directed energy deposition (DED) methods (CLAD, LFMT, BeaM). These also require precise control of the flow rate of the feed material. One of the foreseeable applications of DED is the design and manufacture of functionalized gradient materials, where the unprocessed material is alloyed in situ according to the optimal local mechanical properties of the component. This is an evolution of topology optimization, where the optimization not only evaluates the topology, but also the localized material properties, thereby achieving optimization levels that have not yet been observed. In this scheme, controlling the distribution of the unprocessed material needs to be even more precise. It should be understood that the present disclosure can be applicable to a wide range of unprocessed materials, and can be applicable to directed energy deposition, topology optimization and functional gradient methods of materials.

[0306] test

[0307] The following paragraphs describe illustrative and non-limiting experiments mentioned in this disclosure.

[0308] Angle of repose / Hall flowmeter

[0309] The angle of repose defined in ISO-4490 / ASTM B213 is the angle of inclination of the cone formed relative to the bottom plate when the powder flows freely through the funnel onto the flat plate, and is considered to be a measure of powder flowability. ASTM also recommends this method as a characterization method for metal powders used in additive manufacturing.

[0310] Alternatively, the time required to discharge the powder can be used as a measure of flowability. For free-flowing powders, a low angle (and short discharge time) can be expected because the avalanche can easily flow down the slope, while for cohesive powders, the angle will be large.

[0311] Avalanche Corner

[0312] The determination of the avalanche angle is a method that is closer to powder bed-based additive manufacturing (SLS, SLM) than other technologies. It usually consists of a rotating transparent drum filled with a certain amount of powder and a camera located in front of a backlight. The camera records a picture of the powder free surface inside the drum and the cross-sectional area of ​​the powder. The pictures can be analyzed for different values ​​associated with the flowability of the powder, for example, the avalanche flow index (AFI) and the cohesive interaction index (CoI) have been proposed to quantify the powder.

[0313] ASTM E11 mesh screening

[0314] The test procedure with a stack of ASTM E11 meshes consists in determining the proportion of powder 10 collected after each sieve relative to the initial amount of powder used in the test and comparing this result with the result obtained by sieving the comparative prior art powder on the same stack of ASTM E11 meshes with the corresponding sieving steps. The results can also be reported using the proportion of powder collected after the last ASTM E11625 mesh (i.e., the proportion of particles with a size <20 μm).

[0315] The sieving efficiency can provide information about the behavior of a powder and its tendency to agglomerate: the tendency to agglomerate generally tends to reduce the proportion of powder collected after a sieving step with a given mesh, and ultimately to reduce the proportion of powder collected after the last ASTM E11 625 mesh (i.e. the proportion of particles with a size <20 μm), due to the gradual clogging of the mesh holes by agglomerates of material. Thus, in a sieving efficiency test, the recovery of particles with a diameter of less than 20 μm will be reduced for a powder with a tendency to form agglomerates (e.g. 50%, 75% relative humidity), for example, at high ambient humidity. In contrast, when the powder has a lower cohesion and comprises fewer or no agglomerates of material, the individual particles of the powder are forced to pass through the mesh holes, and the powder on the mesh itself is less cohesive, so it is easier to remove particles from the blockage.

[0316] Surface roughness

[0317] The surface roughness of a part can be measured using a surface roughness tester (e.g., Elcometer 7061, Elcometer Inc., USA), which mechanically maps the surface to record an "image" of the surface roughness over a predefined sample length. This measurement technique provides a number of measurement parameters, including: Ra, which is the average roughness over the sample length; Rz, which is the average distance between the highest peak and the lowest valley over multiple sample lengths; Rt, which is the distance between the highest peak and the lowest valley within any given sample length; and Rmax, which is the maximum distance between the highest peak and the lowest valley over the sample length (see, for example, ASTM D7127).

[0318] Other ASTM Standards

[0319] The following ASTM standards may be used in the context of the present disclosure:

[0320] B213 Test Methods for Flow Rate of Metal Powders Using the Hall Flowmeter Funnel

[0321] B214 Test Method for Sieve Analysis of Metal Powders

[0322] B243 Terminology of Powder Metallurgy

[0323] B311 Test Method for Density of Powder Metallurgy (PM) Materials Containing Less Than Two Percent Porosity

[0324] B348 Specification for Titanium and Titanium Alloy Bars and Billets

[0325] B600 Guide for Descaling and Cleaning Titanium and Titanium Alloy Surfaces

[0326] B769 Test Method for Shear Testing of Aluminum Alloys

[0327] B822 Test Method for Particle Size Distribution of Metal Powders and Related Compounds by Light Scattering

[0328] B855 Test Method for Volumetric Flow Rate of Metal Powders Using the Arnold Meter and Hall Flowmeter Funnel

[0329] B964 Test Methods for Flow Rate of Metal Powders Using the Carney Funnel

[0330] D3951 Practice for Commercial Packaging

[0331] D7127-17 Standard Test Method for Measurement of Surface Roughness of Abrasive Blast Cleaned Metal Surfaces Using a Portable Stylus Instrument

[0332] E3 Guide for Preparation of Metallographic Specimens

[0333] E8 / E8M Test Methods for Tension Testing of Metallic Materials

[0334] E9 Test Methods of Compression Testing of Metallic Materials at Room Temperature

[0335] E10 Test Method for Brinell Hardness of Metallic Materials

[0336] E11 Specification for Woven Wire Test Sieve Cloth and Test Sieves

[0337] E18 Test Methods for Rockwell Hardness of Metallic Materials

[0338] E21 Test Methods for Elevated Temperature Tension Tests of Metallic Materials

[0339] E23 Test Methods for Notched Bar Impact Testing of Metallic Materials

[0340] E29 Practice for Using Significant Digits in Test Data to Determine Conformance with Specifications

[0341] E238 Test Method for Pin-Type Bearing Test of Metallic Materials

[0342] E384 Test Method for Microindentation Hardness of Materials

[0343] E399 Test Method for Linear-Elastic Plane-Strain Fracture Toughness KIc of Metallic Materials

[0344] E407 Practice for Microetching Metals and Alloys

[0345] E466 Practice for Conducting Force Controlled Constant Amplitude Axial Fatigue Tests of Metallic Materials

[0346] E539 Test Method for Analysis of Titanium Alloys by X-Ray Fluorescence Spectrometry

[0347] E606 Test Method for Strain-Controlled Fatigue Testing

[0348] E647 Test Method for Measurement of Fatigue Crack Growth Rates

[0349] E1409 Test Method for Determination of Oxygen and Nitrogen in Titanium and Titanium Alloys by Inert Gas Fusion

[0350] E1417 Practice for Liquid Penetrant Testing

[0351] E1447 Test Method for Determination of Hydrogen in Titanium and TitaniumAlloys by Inert Gas Fusion Thermal Conductivity / Infrared Detection Method

[0352] E1450 Test Method for Tension Testing of Structural Alloys in Liquid Helium

[0353] E1742 Practice for Radiographic Examination

[0354] E1820 Test Method for Measurement of Fracture Toughness

[0355] E1941 Test Method for Determination of Carbon in Refractory and Reactive Metals and Their Alloys by Combustion Analysis

[0356] E2368 Practice for StrainControlled Thermomechanical Fatigue Testing

[0357] E2371 Test Method for Analysis of Titanium and Titanium Alloys by Direct Current Plasma and Inductively Coupled Plasma Atomic Emission Spectrometry (Performance-Based Test Methodology)

[0358] E2626 Guide for Spectrometric Analysis of Reactive and Refractory Metals

[0359] F136 Specification for Wrought Titanium-6Aluminum-4Vanadium ELI (ExtraLow ​​Interstitial) Alloy for Surgical Implant Applications (UNS R56401)

[0360] F1472 Specification for Wrought Titanium-6 Aluminum-4 Vanadium Alloy for Surgical Implant Applications (UNS R56400)

[0361] F2971 Practice for Reporting Data for Test Specimens Prepared by Additive Manufacturing

[0362] F3049 Guide for Characterizing Properties of Metal Powders Used for Additive Manufacturing Processes

[0363] F3122 Guide for Evaluating Mechanical Properties of Metal Materials Made via Additive Manufacturing Processes

[0364] definition

[0365] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. As used herein, unless otherwise specified or the context requires otherwise, each of the following terms shall have the definition set forth below.

[0366] As used herein, the term "powder" and the like refers to a number of particles. The particles may be of any configuration, shape or size as long as they are suitable for improving its flowability and / or spreadability.

[0367] As used herein, the term "average particle size" refers to the average value of particle sizes. In some embodiments, the average particle size refers to D50, ie, the particle diameter at the 50% point on the particle size distribution curve when the total volume is 100%.

[0368] As used herein, the term "substantially" refers to a deviation that is small enough not to significantly degrade the identified property (eg, sphericity). In some cases, the exact degree of deviation that is allowable may depend on the specific circumstances.

[0369] As used herein, the term "plasma" refers to a state of matter in which ionized gaseous matter becomes highly conductive to the extent that long-range electric and magnetic fields dominate the behavior of the matter. Plasma is typically artificially created by heating a neutral gas or by subjecting the gas to strong electromagnetic fields.

[0370] The expressions "plasma torch," "plasma arc," "plasma gun," and "plasma cutter" are used interchangeably herein and refer to a device for generating direct current plasma.

[0371] As used herein, the abbreviation "μm" means micrometer, and the abbreviation "nm" means nanometer.

[0372] As used herein, the expression "particle size distribution" or "PSD" defines the relative amount of particles present according to size. The most easily understood determination method is sieve analysis, in which a powder is separated on sieves of different sizes. Thus, the PSD is defined according to discrete size ranges: for example, when a sieve of size between 45 μm and 53 μm is used, the PSD is between 45 μm and 53 μm. The PSD is usually determined by a list of size ranges covering nearly all sizes present in the sample.

[0373] As used herein, the expression "comparative prior art powder" generally refers to a powder that has not been surface modified (eg, a powder that has been atomized and optionally sieved).

[0374] As used herein, the expression "additive manufacturing" (AM) refers to various methods by which materials are joined or solidified under computer control to produce three-dimensional objects, wherein materials are added together (e.g., liquid molecules or powder particles are fused together), typically layer by layer (also referred to in the art as 3D printing). Currently, ISO / ASTM 52900-15 defines seven categories of additive manufacturing methods within its meaning: binder jetting, directed energy deposition, material extrusion, material jetting, powder bed fusion, sheet lamination, and VAT photopolymerization.

[0375] Example

[0376] The following examples are given to illustrate the practice of various embodiments of the present disclosure. These examples are not intended to limit or define the entire scope of the present disclosure. It should be understood that the present disclosure is not limited to the specific embodiments described and shown herein, but includes all modifications and changes within the scope of the present disclosure as defined in the attached embodiments.

[0377] Unless otherwise stated, the PSD of the powders used in these examples ranged from 0 microns to 1000 microns.

[0378] Example 1

[0379] In this non-limiting working example, a plasma atomized Ti64 powder having a PSD of about 15 μm to about 45 μm was processed according to embodiments of the present disclosure to obtain a powder having improved physical properties, i.e., flowability, that was insensitive to relative humidity. In this example, the flowability of the treated powder was less than 30 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213.

[0380] After argon purging, 15 kg of the plasma-atomized Ti64 powder thus prepared was introduced into a V-type mixer with an 8-liter working capacity. Three solutions were prepared. First, 9 g of ammonium hydroxide (30% aqueous solution) was dissolved in 400 ml of ethanol (95%, denatured) (solution 1). Then 4.05 g of methyltrimethoxysilane was dissolved in 400 ml of ethanol (95%, denatured) (solution 2). The third solution contained only an ethanol solution (95%, denatured) (solution 3). The V-type mixer was started to rotate, and the injection mechanism with an enhancement rod was started. The solutions were then injected in sequence: solution 1, then solution 2, and then solution 3. The container was then pressurized and hermetically sealed. The mixture was reacted for 4 hours, at which time a 12 standard liters / minute (slpm) argon flow was created through the container, and the temperature was raised to 50°C for drying. The mixture was dried for 4 hours with the mixer rotating. The powder was then transferred to a tank and sieved.

[0381] Sieving has two main purposes. The first is to separate the powder into smaller subsets according to the target particle size distribution. The second is to break up and disperse any agglomerates that may have formed during processing. Fig.12 As shown, the fluidity curve obtained according to ASTM B213 shows that: as the relative humidity increases, the Hall flow result decreases (i.e., indicating an increase in fluidity); the Hall flow result is less than 28 seconds; and the change in the Hall flow result between 10% relative humidity and 75% relative humidity is less than 3 seconds, or 7%.

[0382] Similar results were obtained with variations of this method in which, for example, the concentration of ammonium hydroxide in the total alcohol ranged from 5 g / L to 120 g / L.

[0383] Example 2

[0384] In this non-limiting working example, the metal powder of Example 1, as well as various other metal powders, were treated using an anhydrous process to obtain powders having improved physical properties in accordance with embodiments of the present disclosure.

[0385] 120 g of metal powder (Ti64 with a PSD of about 15 μm to about 45 μm, AlSi10Mg with a PSD of about 30 μm to about 70 μm, AlSi7Mg with a PSD of about 30 μm to about 70 μm, and Ni718 with a PSD of about 15 μm to about 45 μm) was impregnated into 200 mL of a solvent (Hydrocabon). The suspension was stirred with a magnetic stirrer. Then, 5 mL of silane was added, and the suspension was heated to reflux for 3 hours. The mixture was vacuum filtered using a Buchner funnel, washed with ethanol, and then subjected to a drying step.

[0386] Table 4 describes the different powders obtained, as well as the solvents and silanes used according to the method:

[0387] Table 4

[0388]

[0389] Example 3

[0390] In this non-limiting working example, the metal powder of Example 2 was treated with other coupling agents for surface modification via chelate bonding to obtain a powder with improved physical properties, according to embodiments of the present disclosure.

[0391] 120 g of metal powder (Ti64 with a PSD of about 15 μm to about 45 μm, AlSi10Mg with a PSD of about 30 μm to about 70 μm, AlSi7Mg with a PSD of about 30 μm to about 70 μm, and Ni718 with a PSD of about 15 μm to about 45 μm) is impregnated into 200 mL of ethanol. The suspension is stirred with a magnetic stirrer. Then, 1 mL of a coupling agent (di-(2-ethylhexyl) phosphoric acid or oleic acid or sodium dodecyl sulfate) is added, and the suspension is heated at 50°C for 4 hours. The mixture is vacuum filtered using a Buchner funnel, washed with ethanol, and then a drying step is performed. Figure 1 The hydrophobic character of the treated powder 10 is shown, where the water added to the powder forms cohesive droplets 35 on top of the powder.

[0392] Example 4

[0393] In this non-limiting working example, the metal powder of Example 1 was treated according to an embodiment of the present disclosure using a variation of the method described in Example 1 to obtain a powder with improved physical properties. In this example, the flowability of the treated powder was less than 35 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213.

[0394] After argon purging, 15 kg of the plasma atomized Ti64 powder thus produced with a PSD of about 15 μm to about 45 μm was introduced into a V-type mixer with a working capacity of 8 liters. Three solutions were prepared. First, 9 g of ammonium hydroxide (30% aqueous solution) was dissolved in 200 ml of ethanol (95%, denatured) (solution 1). Then 4.05 g of methyltrimethoxysilane was dissolved in 200 ml of ethanol (95%, denatured) (solution 2). The third solution contained only ethanol solution (solution 3, 200 mL).

[0395] The solutions were then injected sequentially: Solution 1, then Solution 2, then Solution 3. The vessel was then pressurized and hermetically sealed. The mixture was allowed to react for 4 hours, at which time a 12 slpm argon flow was established through the vessel and the temperature was raised to 50°C for drying. The mixture was allowed to dry for 2 hours with the mixer rotating. The powder was then transferred to a jar and sieved. Fig.13 As shown, the fluidity curve obtained according to ASTM B213 shows that: as the relative humidity increases, the Hall Flow result decreases (i.e., indicating an increase in fluidity); the Hall Flow result is less than 34 seconds; and the change in the Hall Flow result between 10% relative humidity and 75% relative humidity is less than 14 seconds, or 42%.

[0396] Example 5

[0397] In this non-limiting working example, the metal powder of Example 1 was treated according to an embodiment of the present disclosure using a variation of the method described in Example 1 to obtain a powder with improved physical properties. In this example, the flowability of the treated powder was less than 30 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213.

[0398] After argon purging, 15 kg of the plasma atomized Ti64 powder thus produced with a PSD of about 15 μm to about 45 μm was introduced into a V-type mixer with a working capacity of 8 liters. Three solutions were prepared. First, 9 g of ammonium hydroxide (30% aqueous solution) was dissolved in 50 ml of ethanol (95%, denatured) (solution 1). Then 4.05 g of methyltrimethoxysilane was dissolved in 50 ml of ethanol (95%, denatured) (solution 2). The third solution contained only ethanol solution (solution 3, 50 mL). The solutions were then injected in sequence: solution 1, then solution 2, and then solution 3. The container was then pressurized and hermetically sealed. The mixture was allowed to react for 2 hours, at which time a 12 slpm argon flow was created through the container and the temperature was raised to 50°C for drying. The mixture was allowed to dry for 2 hours with the mixer rotating. The powder was then transferred to a jar and sieved. As Fig.14 As shown, the flow curves obtained according to ASTM B213 indicate that: the Hall Flow results generally decrease as the relative humidity increases (i.e., indicating an increase in flow); the Hall Flow results are less than 27 seconds; and the change in the Hall Flow results between 10% relative humidity and 75% relative humidity is less than 5 seconds, or 19%.

[0399] Example 6

[0400] In this non-limiting working example, the metal powder of Example 1 was treated according to an embodiment of the present disclosure using a variation of the method described in Example 1 to obtain a powder with improved physical properties. In this example, the flowability of the treated powder was less than 25 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213.

[0401] After argon purging, 15 kg of the plasma-atomized Ti64 powder thus produced with a PSD of about 15 μm to about 45 μm was introduced into a V-type mixer with an 8-liter working capacity. Three solutions were prepared. First, 3 g of ammonium hydroxide (30% aqueous solution) was dissolved in 25 ml of ethanol (95%, denatured) (solution 1). Then 0.675 g of methyltrimethoxysilane was dissolved in 25 ml of ethanol (95%, denatured) (solution 2). The third solution contained only ethanol solution (solution 3, 25 mL). The solutions were then injected in sequence: solution 1, then solution 2, and then solution 3. The container was then pressurized and hermetically sealed. The mixture was allowed to react for 30 min, at which time a 12 slpm argon flow was created through the container and the temperature was raised to 50°C for drying. The mixture was allowed to dry for 1 hour with the mixer rotating. The powder was then transferred to a jar and sieved. As Fig.15As shown, the flow curves obtained according to ASTM B213 indicate that: the Hall Flow result generally decreases slightly (i.e., indicating an increase in flow) as the relative humidity increases; the Hall Flow result is less than 25 seconds; and the change in the Hall Flow result between 10% relative humidity and 75% relative humidity is less than 3 seconds, or 11%.

[0402] Example 7

[0403] In this non-limiting working example, the metal powder of Example 1 was treated according to an embodiment of the present disclosure using a variation of the method described in Example 1 to obtain a powder with improved physical properties. In this example, the flowability of the treated powder was less than 35 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213.

[0404] After argon purging, 15 kg of pre-screened plasma-atomized Ti64 powder with a PSD of about 15 μm to about 45 μm was introduced into a V-type mixer with an 8 liter working capacity. Three solutions were prepared. First, 9 g of ammonium hydroxide (30% aqueous solution) was dissolved in 50 ml of ethanol (95%, denatured) (solution 1). Then 2.9 g of methyltrimethoxysilane was dissolved in 50 ml of ethanol (95%, denatured) (solution 2). The third solution contained only ethanol solution (solution 3, 50 mL). The solutions were then injected in sequence: solution 1, then solution 2, and then solution 3. The container was then pressurized and hermetically sealed. The mixture was allowed to react for 1 hour, at which time a 12 slpm argon flow was created through the container and the temperature was raised to 50°C for drying. The mixture was allowed to dry for 2 hours with the mixer rotating. The powder was then transferred to a can and sieved again. As Fig.16 As shown, the fluidity curves obtained according to ASTM B213 indicate that: the Hall Flow results generally decrease as the relative humidity increases (i.e., indicating an increase in fluidity); the Hall Flow results are less than 33 seconds; and the change in the Hall Flow results between 10% relative humidity and 75% relative humidity is less than 5 seconds, or 15%.

[0405] Example 8

[0406] In this non-limiting working example, another metal powder was produced according to embodiments of the present disclosure to obtain a powder with improved physical properties that is insensitive to relative humidity.

[0407] 1 kg of unprocessed AlSi10Mg powder with a PSD of about 30 μm to about 70 μm was obtained by plasma atomization and suspended in 2 L of toluene. 50 g of dimethyldiethoxysilane was added to the mixture while stirring. The mixture was stirred under reflux for 3 hours, and the powder was filtered out of the solution and washed with ethanol. The powder was dried at ambient temperature and atmosphere.

[0408] Example 9

[0409] In this non-limiting working example, another metal powder was made according to an embodiment of the present disclosure to obtain a powder with improved physical properties that is insensitive to relative humidity. In this example, the flowability of the treated powder was less than 45 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213, and the Hall flow results varied by less than 3 seconds, or 7%, between 10% relative humidity and 75% relative humidity.

[0410] 300 g of AlSi10Mg powder with a PSD of about 30 μm to about 70 μm was added to a polyethylene container. Methyltrimethoxysilane (0.2 g) was dissolved in ethanol (25 ml), and in a second container an aqueous ammonium hydroxide solution (30%, 0.3 ml) was mixed with ethanol (25 ml). The ammonium hydroxide solution was added to the container first, and the contents were mixed thoroughly.

[0411] The silane solution was then added to the container and the contents of the container were mixed thoroughly. The container was placed in a rotating mixer. The mixer was then rotated at 0.5 RPM for 4 hours.

[0412] like Fig.17 As shown, the flow curves obtained according to ASTM B213 indicate that: the Hall Flow result is generally stable (i.e., indicating an increase in flow); the Hall Flow result is less than 43 seconds; and the change in the Hall Flow result between 10% relative humidity and 75% relative humidity is less than 2 seconds, or 5%.

[0413] Example 10

[0414] In this non-limiting working example, another metal powder was produced according to an embodiment of the present disclosure to obtain a powder with improved physical properties that is insensitive to relative humidity. In this example, the flowability of the treated powder was less than 15 seconds at 10% relative humidity up to 75% relative humidity according to ASTM B213.

[0415] 500 g of unprocessed atomized Ni718 powder was added to a polyethylene jar. Methyltrimethoxysilane (0.053 g) was dissolved in ethanol (12.5 ml), and in a second container, an aqueous ammonium hydroxide solution (30%, 0.15 ml) was mixed with ethanol (12.5 ml). First, the ammonium hydroxide solution was added to the container and the contents were mixed thoroughly. Then the silane solution was added to the container and the contents of the container were mixed thoroughly. The container was placed in a rotating mixer. The mixer was then rotated at 0.5 RPM for 4 hours. Fig.18 As shown, the flow curve obtained according to ASTM B213 shows that: the Hall Flow result is less than 14 seconds; and the change in the Hall Flow result between 10% relative humidity and 75% relative humidity is less than 3 seconds, or 21%.

[0416] Other examples of implementations will become apparent to the reader in view of the teachings of this specification.While various embodiments of the present disclosure have been described and illustrated, it will be apparent to those skilled in the art from this specification that many modifications and variations may be made.

[0417] For example, the mixer described herein may be a V-type, a double cone type, a spiral type, or any type of mixer capable of blending metal powders.

[0418] For example, all reactants may be added in a single solution or in at least two different solutions and / or in any order.

[0419] For example, the concentration of the aqueous ammonium hydroxide solution in the total alcohol can range from about 0.01 g / L to about 500 g / L, for example, in the range of 5 g / L to 120 g / L.

[0420] For example, the alcohol solution may be ethanol, methanol, isopropanol, or mixtures thereof with or without residual water.

[0421] For example, the solution may be injected into the mixer simultaneously with or prior to blending or in multiple steps.

[0422] The reaction time can range from about 10 min to about 12 h, for example, about 20 min to about 12 h, about 30 min to about 12 h, about 40 min to about 12 h, about 50 min to about 12 h, about 60 min to about 12 h, about 10 min to about 11 h, about 20 min to about 11 h, about 30 min to about 11 h, about 40 min to about 11 h, about 50 min to about 11 h, about 60 min to about 11 h, about 10 min to about 10 h, about 20 min to about 10 h, about 30 min to about 10 h, about 40 min to about 10 h, about 50 min to about 10 h, about 60 min to about 10 h, about 10 min to about 9 h, about 20 min to about 9 h, about 30 min to about 9 h, about 40 min to about 9 h, about 50 min to about 9 h, about 60 min to about 9 h, or any time within any of these ranges.

[0423] The reaction temperature may range from about 20°C to about 250°C, for example, from about 30°C to about 250°C, from about 40°C to about 250°C, from about 50°C to about 250°C, from about 60°C to about 250°C, from about 20°C to about 200°C, from about 30°C to about 200°C, from about 40°C to about 200°C, from about 50°C to about 200°C, from about 60°C to about 200°C, from about 20°C to about 150°C, from about 30°C to about 150°C, from about 40°C to about 150°C, from about 50°C to about 150°C, from about 60°C to about 150°C, from about 20°C to about 100°C, from about 30°C to about 100°C, from about 40°C to about 100°C, from about 50°C to about 100°C, from about 60°C to about 100°C, or any temperature within these ranges.

[0424] The drying time may range from about 10 min to 12 h, for example, from about 20 min to about 12 h, from about 30 min to about 12 h, from about 40 min to about 12 h, from about 50 min to about 12 h, from about 60 min to about 12 h, from about 10 min to about 11 h, from about 20 min to about 11 h, from about 30 min to about 11 h, from about 40 min to about 11 h, from about 50 min to about 11 h, from about 60 min to about 11 h, from about 10 min to about 10 h, from about 20 min to about 10 h, from about 30 min to about 10 h, from about 40 min to about 10 h, from about 50 min to about 10 h, from about 60 min to about 10 h, from about 10 min to about 9 h, from about 20 min to about 9 h, from about 30 min to about 9 h, from about 40 min to about 9 h, from about 50 min to about 9 h, from about 60 min to about 9 h, or any time within any of these ranges.

[0425] It should be noted that for the convenience of the reader, headings or subheadings may be used throughout this disclosure, but these should not limit the scope of the invention. In addition, certain theories may be proposed and disclosed herein; however, whether these theories are correct or incorrect, they should never limit the scope of the invention, as long as the invention can be practiced according to this disclosure without considering any particular theory or course of action.

[0426] All references cited throughout this specification are intended to be incorporated herein by reference in their entirety.

[0427] References to "some embodiments" and the like throughout the specification refer to specific elements (e.g., features, structures, and / or characteristics) described in conjunction with the present invention that are included in at least one embodiment described herein, and may or may not be present in other embodiments. Furthermore, it should be understood that the described inventive features may be combined in different embodiments in any suitable manner.

[0428] Those skilled in the art will appreciate that, throughout this specification, the term "a" used before a term encompasses embodiments that include one or more of the things to which the term refers. Those skilled in the art will also appreciate that, throughout this specification, the term "comprising" (which is synonymous with "including," "containing," or "characterized by") is inclusive or open-ended, and does not exclude additional unlisted elements or method steps.

[0429] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. In the event of a conflict, the present document, including definitions, will control.

[0430] As used in this disclosure, the terms "approximately", "about" or "close to" should generally mean within the error range generally accepted in the art. Therefore, the numerical amounts given herein generally include such error ranges, so that if not explicitly stated, the terms "approximately", "about" or "close to" can be inferred.

[0431] The scope of the invention is more particularly defined in the appended claims.

Claims

1. An additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm and an apparent density of ≥ 2.440 g / cm2 at 30% relative humidity determined according to ASTM B212 3 .

2. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 0 μm to 25 μm.

3. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 5 μm to 25 μm.

4. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 10 μm to 45 μm.

5. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 15 μm to 45 μm.

6. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 20 μm to 53 μm.

7. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 15 μm to 63 μm.

8. The additive manufacturing powder according to claim 1, comprising particles having a PSD of 45 μm to 90 μm.

9. The additive manufacturing powder of claim 1, comprising particles having a PSD of 45 μm to 177 μm.

10. The additive manufacturing powder of claim 1, comprising particles having a PSD of 45 μm to 106 μm.

11. The additive manufacturing powder of claim 1, comprising particles having a PSD of 45 μm to 105 μm.

12. The additive manufacturing powder of claim 1, comprising particles having a PSD of 75 μm to 150 μm.

13. The additive manufacturing powder of claim 1, comprising particles having a PSD of 90 μm to 250 μm.

14. The additive manufacturing powder according to any one of claims 1 to 13, wherein the oxygen content of the particles is less than 2000 ppm, or less than 1000 ppm, or less than 400 ppm, or less than 300 ppm, or less than 150 ppm.

15. The additive manufacturing powder of any one of claims 1 to 14, wherein the particles have a hydrogen content of less than 200 ppm, or less than 150 ppm, or less than 100 ppm.

16. The additive manufacturing powder of any one of claims 1 to 15, wherein the particles have a carbon content of less than 1000 ppm, or less than 500 ppm, or less than 300 ppm, or less than 100 ppm.

17. The additive manufacturing powder of any one of claims 1 to 16, wherein the particles have a nitrogen content of less than 500 ppm, or less than 400 ppm, or less than 300 ppm.

18. The additive manufacturing powder according to any one of claims 1 to 17, wherein the particles are pure metal-based particles, alloy-based particles, ceramic-based particles or composite-based particles.

19. The additive manufacturing powder of claim 18, wherein the particles are titanium-based particles, zirconium-based particles, nickel-based particles, platinum-based particles, or gold-based particles.

20. The additive manufacturing powder of claim 18, wherein the particles are aluminum alloy-based particles, steel-based particles, stainless steel-based particles, copper alloy-based particles, nickel alloy-based particles, superalloy-based particles, palladium-based particles, silver-based particles, tungsten-based particles, refractory metal-based particles, ceramic-based particles, polyamide-based particles, or polystyrene-based particles.

21. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of Al-10Si-0.35Mg.

22. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of Al-10Si-Mg.

23. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of Al-7Si-Mg.

24. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of 62Ni-21.5Cr-9.0Mo-3.65Nb.

25. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of Ti-6Al-4Va.

26. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of Ti-6Al-2Sn-4Zr-2Mo.

27. The additive manufacturing powder of claim 18, wherein the particles have a chemical formula of Ti-5Al-5V-5Mo-3Cr.

28. The additive manufacturing powder of claim 18, wherein the particles are Ni alloy 625 based particles.

29. The additive manufacturing powder of claim 18, wherein the particles are Ni alloy 718 based particles.

30. The additive manufacturing powder of claim 18, wherein the particles are pure titanium-based particles.

31. An additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm and an apparent density of ≥ 2.400 g / cm2 at 75% relative humidity determined according to ASTM B212 3 .

32. The additive manufacturing powder of claim 31, comprising particles having a PSD of 0 μm to 25 μm.

33. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 5 μm to 25 μm.

34. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 10 μm to 45 μm.

35. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 15 μm to 45 μm.

36. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 20 μm to 53 μm.

37. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 15 μm to 63 μm.

38. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 45 μm to 90 μm.

39. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 45 μm to 177 μm.

40. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 45 μm to 106 μm.

41. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 45 μm to 105 μm.

42. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 75 μm to 150 μm.

43. The additive manufacturing powder of claim 31 , comprising particles having a PSD of 90 μm to 250 μm.

44. The additive manufacturing powder of any one of claims 31 to 43, wherein the particles have an oxygen content of less than 2000 ppm, or less than 1000 ppm, or less than 400 ppm, or less than 300 ppm, or less than 150 ppm.

45. The additive manufacturing powder of any one of claims 31 to 44, wherein the particles have a hydrogen content of less than 200 ppm, or less than 150 ppm, or less than 100 ppm.

46. ​​The additive manufacturing powder of any one of claims 31 to 45, wherein the particles have a carbon content of less than 1000 ppm, or less than 500 ppm, or less than 300 ppm, or less than 100 ppm.

47. The additive manufacturing powder of any one of claims 31 to 46, wherein the particles have a nitrogen content of less than 500 ppm, or less than 400 ppm, or less than 300 ppm.

48. The additive manufacturing powder of any one of claims 31 to 47, wherein the particles are pure metal-based particles, alloy-based particles, ceramic-based particles, or composite-based particles.

49. The additive manufacturing powder of claim 48, wherein the particles are titanium-based particles, zirconium-based particles, nickel-based particles, platinum-based particles, or gold-based particles.

50. The additive manufacturing powder of claim 48, wherein the particles are aluminum alloy-based particles, steel-based particles, stainless steel-based particles, copper alloy-based particles, nickel alloy-based particles, superalloy-based particles, palladium-based particles, silver-based particles, tungsten-based particles, refractory metal-based particles, ceramic-based particles, polyamide-based particles, or polystyrene-based particles.

51. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of Al-10Si-0.35Mg.

52. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of Al-10Si-Mg.

53. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of Al-7Si-Mg.

54. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of 62Ni-21.5Cr-9.0Mo-3.65Nb.

55. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of Ti-6Al-4Va.

56. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of Ti-6Al-2Sn-4Zr-2Mo.

57. The additive manufacturing powder of claim 48, wherein the particles have a chemical formula of Ti-5Al-5V-5Mo-3Cr.

58. The additive manufacturing powder of claim 48, wherein the particles are Ni alloy 625 based particles.

59. The additive manufacturing powder of claim 48, wherein the particles are Ni alloy 718 based particles.

60. The additive manufacturing powder of claim 48, wherein the particles are pure titanium-based particles.

61. An additive manufacturing powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, and having a first apparent density determined according to ASTM B212 at 30% relative humidity, and a second apparent density determined according to ASTM B212 at 75% relative humidity, wherein the second apparent density shows a loss of ≤ 2% relative to the first apparent density.

62. The additive manufacturing powder of claim 61, wherein the loss is ≤ 1.5%.

63. The additive manufacturing powder of claim 61, wherein the loss is ≤ 1.0%.

64. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 0 μm to 25 μm.

65. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 5 μm to 25 μm.

66. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 10 μm to 45 μm.

67. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 15 μm to 45 μm.

68. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 20 μm to 53 μm.

69. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 15 μm to 63 μm.

70. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 45 μm to 90 μm.

71. The additive manufacturing powder of any one of claims 61 to 63, comprising particles having a PSD of 45 μm to 177 μm.

72. The additive manufacturing powder of any one of claims 61 to 63, comprising particles having a PSD of 45 μm to 106 μm.

73. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 45 μm to 105 μm.

74. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 75 μm to 150 μm.

75. An additive manufacturing powder according to any one of claims 61 to 63, comprising particles having a PSD of 90 μm to 250 μm.

76. The additive manufacturing powder of any one of claims 61 to 75, wherein the particles have an oxygen content of less than 2000 ppm, or less than 1000 ppm, or less than 400 ppm, or less than 300 ppm, or less than 150 ppm.

77. The additive manufacturing powder of any one of claims 61 to 76, wherein the particles have a hydrogen content of less than 200 ppm, or less than 150 ppm, or less than 100 ppm.

78. The additive manufacturing powder of any one of claims 61 to 77, wherein the particles have a carbon content of less than 1000 ppm, or less than 500 ppm, or less than 300 ppm, or less than 100 ppm.

79. The additive manufacturing powder of any one of claims 61 to 78, wherein the particles have a nitrogen content of less than 500 ppm, or less than 400 ppm, or less than 300 ppm.

80. The additive manufacturing powder of any one of claims 61 to 79, wherein the particles are pure metal-based particles, alloy-based particles, ceramic-based particles, or composite-based particles.

81. The additive manufacturing powder of claim 80, wherein the particles are titanium-based particles, zirconium-based particles, nickel-based particles, platinum-based particles, or gold-based particles.

82. The additive manufacturing powder of claim 80, wherein the particles are aluminum alloy-based particles, steel-based particles, stainless steel-based particles, copper alloy-based particles, nickel alloy-based particles, superalloy-based particles, palladium-based particles, silver-based particles, tungsten-based particles, refractory metal-based particles, ceramic-based particles, polyamide-based particles, or polystyrene-based particles.

83. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of Al-10Si-0.35Mg.

84. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of Al-10Si-Mg.

85. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of Al-7Si-Mg.

86. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of 62Ni-21.5Cr-9.0Mo-3.65Nb.

87. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of Ti-6Al-4Va.

88. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of Ti-6Al-2Sn-4Zr-2Mo.

89. The additive manufacturing powder of claim 80, wherein the particles have a chemical formula of Ti-5Al-5V-5Mo-3Cr.

90. The additive manufacturing powder of claim 80, wherein the particles are Ni alloy 625 based particles.

91. The additive manufacturing powder of claim 80, wherein the particles are Ni alloy 718 based particles.

92. The additive manufacturing powder of claim 80, wherein the particles are pure titanium-based particles.

93. A shipping container comprising additive manufacturing powder, the powder comprising spherical particles having a particle size distribution (PSD) of about 0 micrometers (μm) to about 1000 μm, wherein the shipping container comprises a top layer of the powder having a first D50, and a bottom layer of the powder having a second D50, wherein the first D50>the second D50.

94. The shipping container of claim 93 wherein the powder is in an atmosphere having a relative humidity of up to 75%.

95. The shipping container of claim 93 wherein said powder is in a nitrogen atmosphere.

96. A sea container as claimed in any one of claims 93 to 95, said powder comprising particles having a PSD of from 0 μm to 25 μm.

97. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 5 μm to 25 μm.

98. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 10 μm to 45 μm.

99. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 15 μm to 45 μm.

100. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 20 μm to 53 μm.

101. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 15 μm to 63 μm.

102. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of 45 μm to 90 μm.

103. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 45 μm to 177 μm.

104. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 45 μm to 106 μm.

105. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of from 45 μm to 105 μm.

106. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of 75 μm to 150 μm.

107. A sea container as claimed in any one of claims 93 to 95 comprising particles having a PSD of 90 μm to 250 μm.

108. The sea container of any one of claims 93 to 107 wherein the particles have an oxygen content of less than 2000 ppm, or less than 1000 ppm, or less than 400 ppm, or less than 300 ppm, or less than 150 ppm.

109. The marine container of any one of claims 93 to 108 wherein the particles have a hydrogen content of less than 200 ppm, or less than 150 ppm, or less than 100 ppm.

110. A sea container according to any one of claims 93 to 109 wherein the particles have a carbon content of less than 1000 ppm, or less than 500 ppm, or less than 300 ppm, or less than 100 ppm.

111. A sea container according to any one of claims 93 to 110 wherein the particles have a nitrogen content of less than 500 ppm, or less than 400 ppm, or less than 300 ppm.

112. A shipping container according to any one of claims 93 to 111 wherein the particles are pure metal based particles, alloy based particles, ceramic based particles or composite based particles.

113. The marine container of claim 112, wherein the particles are titanium-based particles, zirconium-based particles, nickel-based particles, platinum-based particles or gold-based particles.

114. The marine container of claim 112, wherein the particles are aluminum alloys, aluminum alloy based particles, steel based particles, stainless steel based particles, copper alloy based particles, nickel alloy based particles, superalloy based particles, palladium based particles, silver based particles, tungsten based particles, refractory metal based particles, ceramic based particles, polyamide based particles, or polystyrene based particles.

115. The marine container of claim 112 wherein the particles have a chemical formula of Al-10Si-0.35Mg.

116. The marine container of claim 112 wherein the particles have a chemical formula of Al-10Si-Mg.

117. The marine container of claim 112 wherein the particles have the chemical formula Al-7Si-Mg.

118. The marine container of claim 112, wherein the particles have a chemical formula of 62Ni-21.5Cr-9.0Mo-3.65Nb.

119. The marine container of claim 112, wherein the particles have the chemical formula Ti-6Al-4Va.

120. The marine container of claim 112, wherein the particles have the chemical formula Ti-6Al-2Sn-4Zr-2Mo.

121. The marine container of claim 112, wherein the particles have the chemical formula Ti-5Al-5V-5Mo-3Cr.

122. The marine container of claim 112, wherein the particles are Ni alloy 625 based particles.

123. The marine container of claim 112, wherein the particles are Ni alloy 718 based particles.

124. The marine container of claim 112, wherein the particles are pure titanium based particles.

125. A powder for additive manufacturing, the powder comprising powder particles, the powder particles comprising a metal material having a certain density, the powder having a particle size distribution (PSD) of about 0 microns (μm) to about 1000 μm, the powder having an apparent density, wherein the ratio of the apparent density of the powder to the minimum density of the metal material is at least 57.5%.