Manufacturing method of bamboo winding pipeline
By wrapping the bamboo strip layer in an unsaturated resin gel state and reacting with the urea formaldehyde resin at high temperature to form a crosslinked structure, the problem of insufficient interface bonding force between the inner lining layer and the structural layer in the bamboo-wrapped pipe is solved, and the pipeline is improved Compression resistance and mechanical properties.
Patent Information
- Application Number
- CN202411144635.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
Smart Images

Figure CN118906505A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite pipe production technology, and in particular to a method for manufacturing a bamboo-wound pipe. Background Art
[0002] Bamboo wrapped pipe is a composite pipe, which can be divided into three layers from the inside to the outside, namely the inner lining layer, the structural layer and the outer protective layer. The inner lining layer is mainly made of unsaturated resin and fabric, which mainly plays a fixing role and resists internal pressure. The middle layer is the structural layer, which is mainly made of bamboo-based materials and adhesives continuously wound, and mainly plays a role in resisting internal and external pressure. The outermost layer is the outer protective layer. The appropriate resin or coating is selected according to the different usage scenarios of the pipeline, which mainly plays a protective role for the pipeline.
[0003] The existing bamboo winding pipe process is to first make the inner lining layer, and then wind the structural layer after the inner lining layer is completely cured at room temperature. After the structural layer is completely cured, the outer protective layer is finally made. The resin of the existing inner lining layer is oily resin, and the adhesive of the structural layer is water-based adhesive. Considering the compatibility issue, the winding of the existing structural layer is carried out after the inner lining layer is completely cured.
[0004] According to the existing bamboo winding pipe process, when the inner lining layer is completely cured, the inner lining layer is made of unsaturated resin and fabric, and the surface of the inner lining layer is very smooth. The smooth interface greatly affects the adhesion ability of the structural layer, thereby deteriorating the interface bonding performance between the two. The thickness of the inner lining layer of the bamboo composite pipe is about 1.2mm-2.0mm. If the interface process is not well controlled, the stress transfer of the two composite materials of the inner lining layer and the structural layer will be weakened. When there is internal pressure, the inner lining layer cannot use the force of the bamboo pieces of the structural layer to resist deformation, and eventually it cannot withstand the internal pressure and ruptures; at the same time, once the inner lining layer ruptures and water penetrates into the structural layer, the mechanical properties of the bamboo material will be greatly reduced after mildew, resulting in the pipe being unable to resist external pressure. Summary of the invention
[0005] In view of the above problems, the present invention provides a method for manufacturing a bamboo winding pipe.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A method for manufacturing a bamboo wound pipe, comprising:
[0008] The inner lining manufacturing process is as follows: a demoulding layer is arranged on the mold; a fabric impregnated with an unsaturated resin (which may be unsaturated polyester) is wound on the demoulding layer, and the fabric is pressed with a pressing roller to squeeze out bubbles on the surface of the fabric to obtain the inner lining;
[0009] Structural layer production process: when the unsaturated resin is in a gel state, the first bamboo strip layer is wound on the outside of the inner lining layer, and the first bamboo strip layer is completed before the unsaturated resin is completely cured. The bamboo strip layer is made of bamboo strips impregnated with urea-formaldehyde resin or amino resin and mesh cloth. After the first bamboo strip layer is wound, the inner lining layer and the first bamboo strip layer are heated until the unsaturated resin is cured. The temperature for heating the inner lining layer and the first bamboo strip layer is 60°C to 120°C; the bamboo strip layer is continued to be wound on the outside of the first bamboo strip layer to a set number of layers to obtain a structural layer, and the mold is placed in a curing furnace to heat and cure the structural layer. The heating and curing temperature is 60°C to 120°C;
[0010] Outer protective layer production process: After the structural layer is completely cured, the outer protective layer is produced on the outside of the structural layer, and the inner lining layer, structural layer and outer protective layer form a bamboo-wrapped composite pipe;
[0011] Demoulding process: After the outer protective layer is completely cured, the bamboo wrapped composite pipe is removed from the mould.
[0012] Unsaturated polyester can be copolymerized with double bonds in unsaturated polyester by initiating free radical copolymerization with polymerizable vinyl monomers such as styrene, vinyl acetate, methyl methacrylate, etc., so that the linear polyester molecular chains are cross-linked into three-dimensional network structures. The reaction formula is as follows:
[0013]
[0014] From the reaction process, although COOH- in unsaturated polyester does not participate in the curing reaction, under certain heating conditions, COOH- is active and can react. Urea-formaldehyde resin contains a large number of functional groups such as CH2OH- and NH2-, which are relatively active under acidic conditions. They can react with COOH- in unsaturated polyester to form a three-dimensional network structure product. Therefore, before adding curing agent and curing, urea-formaldehyde resin can react chemically with unsaturated polyester to form a complex network product, so that the two resins are bonded more firmly.
[0015] The present application combines the characteristics of unsaturated polyester and urea-formaldehyde resin, and improves the bamboo-wrapped composite pipe from a process perspective. Under high temperature, the unsaturated polyester in a gel state reacts with the urea-formaldehyde resin to form a cross-linked interpenetrating network structure, thereby making the interface bonding stronger. Compared with the existing unsaturated polyester structure layer wrapped after complete curing, the interface bonding problem between the inner lining layer and the structural layer and the bulging problem of the inner lining layer can be well solved.
[0016] In actual use, the prepared outer protective layer can be naturally cooled and cured or heated and cured. After curing, it can be placed for 12 hours to 36 hours before the demolding process.
[0017] The unsaturated polyester used in the inner lining is produced by reacting with a curing agent and an accelerator. In actual production, according to different temperatures and humidities, by controlling the amount of curing agent and accelerator, we can control the time from gelation to curing of the inner lining, that is, the structural layer must start to wrap the bamboo strip layer within this time, and the time from gelation to curing is generally about 10 to 25 minutes. If the inner lining is completely cured when the bamboo strips are wrapped, the urea-formaldehyde resin cannot directly bond with the macromolecular polymer, that is, the stress transfer between the inner lining and the structural layer is weakened, and the pipeline cannot withstand the internal pressure.
[0018] In one embodiment of the present invention, in the process of making the structural layer, when winding the first bamboo strip layer, a pressure roller is used to assist the winding, and the pressure roller is used to make the bamboo strip layer and the inner lining layer tightly wound; the radial force of the pressure roller on the mold is controlled so that the pressure roller can just rotate after pressing the bamboo strip layer.
[0019] Usually, a set proportion of hard fillers are heated in urea-formaldehyde resin to adjust the viscosity (such as biomass fillers such as walnut shell powder). If the force of the pressure roller is too great, the filler will enter the inner lining layer and destroy the structure of the resin (unsaturated polyester) of the inner lining layer, causing the local thickness of the inner lining layer to be too thin and to have tiny cracks, ultimately making the inner lining unable to withstand pressure. If the pressure roller is not used during winding, the contact area between the unsaturated polyester of the inner lining layer and the urea-formaldehyde resin of the first layer of bamboo strips is too small, which will result in insufficient tightness at the interface.
[0020] In one embodiment of the present invention, a pressure sensor is provided on the pressing roller for detecting the radial pressure of the pressing roller on the mold.
[0021] After debugging, the value range of the pressure sensor can be determined, which is convenient for automatically controlling the pressure of the pressure roller on the mold during subsequent processing and ensuring the product processing quality.
[0022] In one embodiment of the present invention, a heating element is provided on the inner side of the mold, and the heating element is used to heat the lining layer and the first bamboo strip layer.
[0023] The existing molds do not have heating elements, but the present invention can quickly and conveniently make the gel-state unsaturated polyester react with the urea-formaldehyde resin to form a cross-linked interpenetrating network structure by setting a heating element in the mold. The heating element can be a variety of different structures such as heating wires.
[0024] In one embodiment of the present invention, the inner lining layer and the first bamboo strip layer are heated by infrared heating.
[0025] In one embodiment of the present invention, the inner lining layer and the first bamboo strip layer are heated for 10 minutes to 40 minutes.
[0026] In one embodiment of the present invention, in the process of manufacturing the outer protective layer, the outer protective layer is formed by coating the selected resin on the outer side of the structural layer.
[0027] In one embodiment of the present invention, in the process of manufacturing the outer protective layer, the protective layer is formed by winding a fabric soaked in resin around the outer side of the structural layer.
[0028] In one embodiment of the present invention, the release layer is a polyester film wrapped around the surface of the mold.
[0029] In one embodiment of the present invention, the release layer is a release agent coated on the surface of the mold.
[0030] In one embodiment of the present invention, a filler with a weight percentage of 5% to 20% is added to the urea-formaldehyde resin or amino resin of the bamboo strip layer, and the viscosity of the urea-formaldehyde resin or amino resin is 400 c.p to 800 c.p.
[0031] The beneficial effects of the present invention are as follows: the present application combines the characteristics of unsaturated polyester and urea-formaldehyde resin, improves the bamboo-wrapped composite pipe from a process perspective, and under high temperature, the unsaturated polyester in a gel state reacts with the urea-formaldehyde resin to form a cross-linked interpenetrating network structure, thereby making the interface bonding stronger. Compared with the existing unsaturated polyester structure layer wrapped after complete curing, the interface bonding problem between the inner lining layer and the structure layer and the bulging problem of the inner lining layer can be well solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a cross-sectional view of a bamboo-wrapped pipe;
[0033] Figure 2 This is a picture of the E plate after 10 cycles of testing;
[0034] Figure 3 This is a picture of the F board after 10 cycles of testing.
[0035] The reference numerals in the figures are:
[0036] 1. Inner lining layer; 2. Structural layer; 3. Outer protective layer. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0038] In the description of this application, it should be noted that the terms "inside", "outside", etc. indicate the orientation or positional relationship based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship in which the product of the application is usually placed when in use, which is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application. In addition, the terms "first", "second", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0039] In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "disposed" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0040] The present invention is described in detail below in conjunction with the accompanying drawings.
[0041] like Figure 1 As shown, a bamboo-wound pipe comprises, from inside to outside, an inner lining layer 1, a structural layer 2 and an outer protective layer 3. The manufacturing method of the bamboo-wound pipe comprises:
[0042] The inner lining manufacturing process includes: setting a demoulding layer on the mold; winding a fabric impregnated with unsaturated polyester on the demoulding layer to obtain the inner lining; when manufacturing the inner lining, pressing the fabric with a pressing roller to squeeze out bubbles on the surface of the fabric;
[0043] Structural layer production process: when the unsaturated polyester is in a gel state, the first bamboo strip layer is wound on the outside of the inner lining layer, and the first bamboo strip layer is completed before the unsaturated polyester is completely cured. The bamboo strip layer is made of bamboo strips impregnated with urea-formaldehyde resin and mesh cloth. After the first bamboo strip layer is wound, the inner lining layer and the first bamboo strip layer are heated until the unsaturated polyester is cured. The temperature for heating the inner lining layer and the first bamboo strip layer is 60°C to 120°C; the bamboo strip layer is continued to be wound on the outside of the first bamboo strip layer to a set number of layers to obtain a structural layer, and the mold is placed in a curing furnace to heat and cure the structural layer. The heating and curing temperature is 60°C to 120°C;
[0044] Outer protective layer production process: After the structural layer is completely cured, the outer protective layer is produced on the outside of the structural layer, and the inner lining layer, structural layer and outer protective layer form a bamboo-wrapped composite pipe;
[0045] Demoulding process: After the outer protective layer is completely cured, the bamboo wrapped composite pipe is removed from the mould.
[0046] Unsaturated polyester can be copolymerized with double bonds in unsaturated polyester by initiating free radical copolymerization with polymerizable vinyl monomers such as styrene, vinyl acetate, methyl methacrylate, etc., so that the linear polyester molecular chains are cross-linked into three-dimensional network structures. The reaction formula is as follows:
[0047] From the reaction process, although COOH- in unsaturated polyester does not participate in the curing reaction, under certain heating conditions (60℃~120℃), COOH- is active and can react. Urea-formaldehyde resin contains a large number of functional groups such as CH2OH- and NH2-, which are relatively active under acidic conditions. They can react with COOH- in unsaturated polyester to form a three-dimensional network structure product. Therefore, before adding curing agent and curing, urea-formaldehyde resin can react chemically with unsaturated polyester to form a complex network product, so that the two resins are bonded more firmly.
[0048] The present application combines the characteristics of unsaturated polyester and urea-formaldehyde resin, and improves the bamboo-wrapped composite pipe from a process perspective. Under high temperature, the unsaturated polyester in a gel state reacts with the urea-formaldehyde resin to form a cross-linked interpenetrating network structure, thereby making the interface bonding stronger. Compared with the existing unsaturated polyester structure layer wrapped after complete curing, the interface bonding problem between the inner lining layer and the structural layer and the bulging problem of the inner lining layer can be well solved.
[0049] In actual use, the prepared outer protective layer can be naturally cooled and cured or heated and cured. After curing, it can be placed for 12 hours to 36 hours before the demolding process.
[0050] In this embodiment, in the process of making the structural layer, when winding the first bamboo strip layer, a pressure roller is used to assist the winding, and the pressure roller is used to make the bamboo strip layer and the inner lining layer tightly wound; the radial force of the pressure roller on the mold is controlled so that the pressure roller can just rotate after pressing the bamboo strip layer.
[0051] Usually, a set proportion of hard fillers are heated in urea-formaldehyde resin to adjust the viscosity (such as biomass fillers such as walnut shell powder). If the force of the pressure roller is too great, the filler will enter the inner lining layer and destroy the structure of the resin (unsaturated polyester) of the inner lining layer, causing the local thickness of the inner lining layer to be too thin and to have tiny cracks, ultimately making the inner lining unable to withstand pressure. If the pressure roller is not used during winding, the contact area between the unsaturated polyester of the inner lining layer and the urea-formaldehyde resin of the first layer of bamboo strips is too small, which will result in insufficient tightness at the interface.
[0052] In actual use, the pressure roller is equipped with a pressure sensor to detect the radial pressure of the pressure roller on the mold. After debugging, the value range of the pressure sensor can be determined, which is convenient for automatically controlling the pressure of the pressure roller on the mold during subsequent processing and ensuring the processing quality of the product.
[0053] In this embodiment, a heating element is provided inside the mold, and the heating element is used to heat the inner lining layer and the first bamboo strip layer. No heating element is provided in the existing molds. The present application can quickly and conveniently make the gel-state unsaturated polyester react with the urea-formaldehyde resin and form a cross-linked interpenetrating mesh structure by providing a heating element in the mold. The heating element can be a variety of different structures such as heating wires.
[0054] In actual use, the inner lining layer and the first bamboo strip layer can also be heated by infrared heating.
[0055] In this embodiment, the inner lining layer and the first bamboo strip layer are heated for 10 minutes to 40 minutes.
[0056] In actual use, in the process of making the outer protective layer, the outer protective layer is formed by brushing the selected resin on the outer side of the structural layer; or, in the process of making the outer protective layer, the protective layer is formed by winding a fabric impregnated with resin on the outer side of the structural layer.
[0057] In this embodiment, the demoulding layer is a polyester film wrapped around the surface of the mold. In actual use, the demoulding layer can also be a demoulding agent coated on the surface of the mold.
[0058] In actual application, the urea-formaldehyde resin of the bamboo strip layer can also be replaced by amino resins such as melamine formaldehyde resin.
[0059] In order to detect the difference in product performance between the present application method and the traditional process, the following experiments were conducted for comparison:
[0060] 1. Interface plate experiment
[0061] Experimental process ①: Wind a layer of bamboo fiber felt soaked in unsaturated polyester, a layer of knitted felt and a layer of mesh cloth on the mold in sequence to obtain an inner lining layer; after the inner lining layer is completely cured, wind four layers of bamboo strips (the bamboo strips in the four layers of bamboo strips are circumferential) to obtain a structural layer; the structural layer is cured at 80°C for 3 hours, and after cooling, it is cut into the size required for the test to obtain sample A (length and width are 260mm×190mm respectively).
[0062] Experimental process ②: A layer of bamboo fiber felt soaked with unsaturated polyester, a layer of knitted felt and a layer of mesh cloth are wound on the mold in sequence to obtain an inner lining layer; when the unsaturated polyester of the inner lining layer is in a gel state, the first layer of bamboo strips is wound first, and the inner lining layer and the first layer of bamboo strips are heated at 80°C for 30 minutes, and then three layers of bamboo strips are wound (the bamboo strips in the four layers of bamboo strips are circumferential) to obtain a structural layer; the structural layer is cured at 80°C for 3 hours, and after cooling, it is cut into the size required for the test to obtain sample B (length and width are 260 mm×190 mm, respectively).
[0063] (i) Conduct an interface 180° peel strength test (where the lining tensile strength is 27.68 MPa).
[0064] In sample A, at 23.74 MPa, the interface between the lining layer and the structural layer separated. In sample B, the lining layer was pulled apart, but the interface between the lining layer and the structural layer did not separate.
[0065] It can be seen that the connection strength of the interface in experimental process ② is greater than the strength of the lining layer matrix, which meets the interface theoretical design requirements.
[0066] (II) Plate hot and cold alternating test
[0067] Experimental steps: Place the test sample in an 80℃ oven for 2 hours, take it out and immediately put it in a -40℃ freezer, and observe the interface adhesion until it comes off.
[0068] Sample A: At the 17th cycle, the interface was slightly detached, and the detachment gradually worsened in subsequent cycles; it was completely detached at the 32nd cycle, and the experiment was terminated.
[0069] Sample B: At the 88th cycle, the interface was slightly detached, and the detachment gradually worsened in subsequent cycles; it was completely detached at the 112th cycle, and the experiment was terminated.
[0070] It can be seen that the interface performance of sample B is significantly higher than that of sample A.
[0071] 2. DN300 pipeline pilot test
[0072] Experimental process ③: A layer of bamboo fiber felt soaked in unsaturated polyester, a layer of knitted felt and a layer of mesh cloth are wound on the mold in sequence to obtain an inner lining layer; after the inner lining layer is completely cured, four layers of bamboo strips are wound (the bamboo strips in the four layers of bamboo strips are circumferential) to obtain a structural layer (pressed at 1.0MPa, 10KN / m 2 The structural layer is cured at 80°C for 3 hours and, after cooling, is cut to obtain a pipe section C of the required length for the test.
[0073] Experimental process ④: A layer of bamboo fiber felt soaked with unsaturated polyester, a layer of knitted felt and a layer of mesh cloth are wound on the mold in sequence to obtain an inner lining layer; when the unsaturated polyester of the inner lining layer is in a gel state, the first layer of bamboo strips is wound first, and the inner lining layer and the first layer of bamboo strips are heated at a temperature of 80°C for 30 minutes, and then three layers of bamboo strips are wound (the bamboo strips in the four layers of bamboo strips are circumferential) to obtain a structural layer (at 1.0MPa, 10KN / m 2 The structural layer is cured at 80°C for 3 hours and, after cooling, is cut to obtain a pipe section D of the required length for the test.
[0074] The circumferential tensile test, axial tensile test, ring stiffness test and hydraulic bursting test were performed on pipe section C and pipe section D, and the results are shown in Table 1.
[0075] Table 1 Performance test comparison of two pipe sections
[0076] It can be seen from Table 1 that the hoop tensile strength, hoop stiffness and water pressure bursting strength of pipe section C are all unqualified, while those of pipe section D are all qualified.
[0077] In order to verify the effect of temperature on unsaturated polyester and urea-formaldehyde resin, the following experiments were conducted for comparison:
[0078] Experimental steps: Make E plate and F plate respectively (using two interface processes), and examine the bonding strength of the interface through hot-cold alternating experiment; then, make 3 more groups of samples in parallel.
[0079] The E plate is obtained by the first process, specifically:
[0080] (1) Preparation of the inner lining layer: a fabric soaked in unsaturated polyester (the amount of unsaturated polyester is 100 g) is wound on the polyester film of the mold, and the fabric includes a layer of bamboo fiber felt, a layer of knitted felt and a layer of mesh cloth arranged in sequence from the inside to the outside;
[0081] (2) Interface preparation: When the unsaturated polyester is in a gel state, a layer of urea-formaldehyde resin (30 g) is poured on the surface of the mesh cloth, and then immediately placed in an 80° C. oven for curing for 30 minutes and then taken out, wherein the urea-formaldehyde resin contains 5% to 20% filler by weight, and the viscosity of the urea-formaldehyde resin is 400 c.p. to 800 c.p.; the urea-formaldehyde resin on the outside of the mesh cloth forms an interface with the unsaturated polyester;
[0082] (3) Fabrication of the structural layer: 3 layers of circumferential bamboo strips and 3 layers of mesh cloth are sequentially laid on the outside of the interface, and the circumferential bamboo strips and the mesh cloth are both impregnated with urea-formaldehyde resin, wherein the two inner layers of mesh cloth are respectively between the two adjacent layers of circumferential bamboo strips, and the third layer of mesh cloth is located at the outermost layer;
[0083] (4) Curing process: Place in an oven at 80°C for 2 hours and take out. After cooling, cut into the set size to obtain an E-plate.
[0084] The F plate is obtained by the second process, specifically:
[0085] (1) Preparation of the inner lining layer: a fabric soaked in unsaturated polyester (the amount of unsaturated polyester is 100 g) is wound on the polyester film of the mold, and the fabric includes a layer of bamboo fiber felt, a layer of knitted felt and a layer of mesh cloth arranged in sequence from the inside to the outside;
[0086] (2) Interface preparation: When the unsaturated polyester is in a gel state, a layer of urea-formaldehyde resin (30 g) is poured on the surface of the mesh cloth and cured at room temperature (15° C.) for 2 hours, wherein the urea-formaldehyde resin contains 5% to 20% filler by weight and has a viscosity of 400 c.p to 800 c.p; the urea-formaldehyde resin on the outside of the mesh cloth forms an interface with the unsaturated polyester;
[0087] (3) Fabrication of the structural layer: 3 layers of circumferential bamboo strips and 3 layers of mesh cloth are sequentially laid on the outside of the interface, and the circumferential bamboo strips and the mesh cloth are both impregnated with urea-formaldehyde resin, wherein the two inner layers of mesh cloth are respectively between the two adjacent layers of circumferential bamboo strips, and the third layer of mesh cloth is located at the outermost layer;
[0088] (4) Curing process: Place in an oven at 80°C for 2 hours and take out. After cooling, cut into the set size to obtain an E-plate.
[0089] Among them, in the first process and the second process, the structures, materials and proportions are the same. The difference is that in the first process, the interface is placed in an 80°C oven for curing for 30 minutes during interface production, while in the second process, the interface is placed at room temperature (15°C) for curing for 2 hours during interface production.
[0090] Experimental process: Put the E plate and F plate of the same size into an 80℃ oven for 0.5h, and then put them into a -40℃ freezer for 0.5h. This is counted as one cycle. Observe whether the interface cracks after 10 cycles. The experimental results are shown in Table 2 and Figure 2 and Figure 3 .
[0091] Table 2 Experimental results of alternating hot and cold cycles of two plates
[0092]
[0093] Repeat the above experimental steps, and produce three parallel samples of E1 board, E2 board, and E3 board through the first process, and produce three parallel samples of F1 board, F2 board, and F3 board through the second process. Perform hot and cold alternating experiments on the six samples. The results are shown in Table 3.
[0094] Table 3 Parallel sample fast hot and cold alternating test results
[0095]
[0096] Experimental conclusion: From the alternating experiment, it can be seen that unsaturated polyester and urea-formaldehyde resin will hardly react without temperature conditions, so the two are not well bonded; but if they react at 80°C, they will form a cross-linked interpenetrating network structure, making the interface bonding stronger.
[0097] The above description is only a preferred embodiment of the present invention, and does not limit the patent protection scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention and the drawings, directly or indirectly used in other related technical fields, is also included in the protection scope of the present invention.
Claims
1. A method for manufacturing a bamboo-wrapped pipe, characterized in that: include: The inner lining manufacturing process is as follows: a demoulding layer is provided on the mold; a fabric impregnated with unsaturated resin is wound on the demoulding layer to obtain the inner lining; Structural layer production process: when the unsaturated resin is in a gel state, the first bamboo strip layer is wound on the outside of the inner lining layer, and the first bamboo strip layer is completed before the unsaturated resin is completely cured. The bamboo strip layer is made of bamboo strips impregnated with urea-formaldehyde resin or amino resin and mesh cloth. After the first bamboo strip layer is wound, the inner lining layer and the first bamboo strip layer are heated until the unsaturated resin is cured. The temperature for heating the inner lining layer and the first bamboo strip layer is 60°C to 120°C; the bamboo strip layer is continued to be wound on the outside of the first bamboo strip layer to a set number of layers to obtain a structural layer, and the mold is placed in a curing furnace to heat and cure the structural layer. The heating and curing temperature is 60°C to 120°C; Outer protective layer production process: After the structural layer is completely cured, the outer protective layer is produced on the outside of the structural layer, and the inner lining layer, structural layer and outer protective layer form a bamboo-wrapped composite pipe; Demoulding process: After the outer protective layer is completely cured, the bamboo wrapped composite pipe is removed from the mould.
2. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: In the process of making the structural layer, when winding the first bamboo strip layer, a pressure roller is used to assist the winding, and the pressure roller is used to make the bamboo strip layer and the inner lining layer tightly wound; the radial force of the pressure roller on the mold is controlled so that the pressure roller can just rotate after pressing the bamboo strip layer.
3. The method for manufacturing a bamboo-wrapped pipe according to claim 2, characterized in that: The pressure roller is provided with a pressure sensor for detecting the radial pressure of the pressure roller on the mold.
4. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: The inner side of the mold is provided with a heating element, and the heating element is used to heat the inner lining layer and the first bamboo strip layer.
5. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: The inner lining layer and the first bamboo strip layer are heated by infrared heating.
6. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: The time for heating the inner lining layer and the first bamboo strip layer is 10 minutes to 40 minutes.
7. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: In the process of making the outer protective layer, the outer protective layer is formed by brushing a selected resin on the outer side of the structural layer, or, in the process of making the outer protective layer, the protective layer is formed by winding a fabric soaked in resin on the outer side of the structural layer.
8. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: In the process of making the inner lining layer, the fabric is pressed with a pressure roller to squeeze out the bubbles on the fabric surface.
9. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: The demoulding layer is a polyester film wound on the surface of the mold, or the demoulding layer is a demoulding agent coated on the surface of the mold.
10. The method for manufacturing a bamboo-wrapped pipe according to claim 1, characterized in that: A filler with a weight percentage of 5% to 20% is added to the urea-formaldehyde resin or amino resin of the bamboo strip layer, and the viscosity of the urea-formaldehyde resin or amino resin is 400 c.p to 800 c.p.
Citation Information
Cited By
Bamboo winding pipe structure and production method thereof
CN122606900A