3D printing method of hydrogel orthokeratology lens capable of regulating and controlling mechanical properties
Through 3D printing technology, a finite element model is established and a hydrogel corneal resizing mirror that can regulate mechanical properties is prepared, which solves the problem of personalized design and uncontrollable mechanical properties of corneal resizing mirrors in the existing technology, and achieves a more accurate Corrective effect and biocompatibility.
Patent Information
- Application Number
- CN202411287858.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-08
AI Technical Summary
When existing corneal resizing lenses correct the middle and low myopia, individual differences lead to inconsistent correction effects, mainly because clinical fitting does not consider the differences in corneal biomechanical properties and the inability to regulate the mechanical properties of materials.
Using 3D printing method, a finite element model was established to obtain personalized geometric morphology and mechanical performance parameters of corneal reshaping mirrors, and a supporting object photocuring resin and a shaping mirror photocuring resin system were used to prepare hydrogel corneal plastic through ultraviolet curing technology. The shape mirror realizes the controllable design of its geometric structure and mechanical properties.
The personalized design of the corneal resizing lens is realized, accurately matches the target human body's corneal biomechanical properties, improves the correction effect and the biocompatibility of the material, and monitors corneal deformation and intraocular pressure changes.
Smart Images

Figure CN118906513A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of orthokeratology lens processing, and specifically relates to a 3D printing method of a hydrogel orthokeratology lens with adjustable mechanical properties. Background Art
[0002] As a medical device for scientific diagnosis and treatment of myopia in adolescents, orthokeratology lenses have a good effect on correcting low and moderate myopia and can effectively control and slow down the development of myopia in adolescents.
[0003] Currently, ophthalmologists perform personalized fitting based on the patient's myopia refractive power, corneal curvature, axial length and other test data. However, it is found that patients with the same conditions have different myopia correction effects after wearing glasses. The reasons can be attributed to the following three aspects: (1) During the clinical fitting process, the individual differences in the biomechanical properties of corneal materials are not taken into account, and no consistent conclusion has been reached on the changes in corneal biomechanical properties (corneal hysteresis and corneal resistance coefficient) after wearing orthokeratology lenses; (2) Commercial orthokeratology lenses used in clinical fitting mainly rely on traditional mechanical manufacturing methods, which make it difficult to achieve controllable molding of thickness and curvature radius; (3) The mechanical properties of commercial orthokeratology lens materials cannot be controlled, and the optimal matching of the force applied by the orthokeratology lens on the cornea and the corneal biomechanical properties cannot be achieved by adjusting the material properties.
[0004] Therefore, how to design and prepare corneal reshaping lenses that are "customized to the eye" based on the personalized characteristics of the human cornea and the composition and structure of the reshaping lens material itself is an urgent problem that needs to be solved. Summary of the invention
[0005] In order to address the deficiencies in the prior art, the present invention aims to provide a hydrogel corneal reshaping lens with adjustable mechanical properties, which has good optical properties, wettability, oxygen permeability, gas permeability and biocompatibility, and at the same time has adjustable geometric structure and mechanical properties and a stable structure. The present invention also provides a 3D printing method thereof.
[0006] The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties of the present invention comprises the following steps: (1) Establish a finite element model of the cornea wearing orthokeratology lenses to obtain the geometric parameters and mechanical performance parameters of orthokeratology lenses that match the target human cornea; (2) Based on the geometric parameters of the orthokeratology lens obtained by simulation, a 3D printing model consistent with the curvature of the posterior surface of the orthokeratology lens is established, and the support is printed using the support photocurable resin system as the support 3D printing ink; (3) Based on the geometric structure parameters and mechanical property parameters of the orthokeratology lens obtained by simulation, a 3D printing model was established and the formula of the photocurable resin system of the orthokeratology lens was adjusted. The photocurable resin system of the orthokeratology lens was used as the 3D printing ink for the orthokeratology lens. The hydrogel orthokeratology lens was printed on the surface of the support. After curing by ultraviolet light, the hydrogel orthokeratology lens was obtained.
[0007] In step (1), when establishing the finite element model of the cornea wearing orthokeratology lenses, it is necessary to consider the biomechanical properties of human corneal materials and corneal tissue structure, as well as the differences in biomechanical properties of human corneal materials before wearing lenses and the changes in biomechanical properties of human corneal materials after wearing lenses.
[0008] The biomechanical properties of the above-mentioned human corneal materials include the elastic modulus of the corneal stroma and the stiffness modulus of the collagen fibers, and the corneal tissue structure refers to the degree of dispersion of the collagen fibers.
[0009] The finite element model of the cornea of the orthokeratology lens Figure 1 As shown, the orthokeratology lens includes a base curve area, a reverse curve area, a positioning curve area and a peripheral curve area. In step (1), the geometric parameters of the orthokeratology lens include curvature, base curve radius, positioning curve radius, diameter, and central zone thickness.
[0010] The method for obtaining the geometric parameters of orthokeratology lenses is as follows: a three-dimensional axisymmetric corneal model is established in the finite element simulation software (ABAQUS 2020). In the normal physiological state, the thickness of the cornea is uneven, and the curvature at different positions on the front and back surfaces of the cornea is different. For the convenience of modeling, the cornea is set to have uniform thickness and the curvature at different positions is the same. The geometric parameters of orthokeratology lenses corresponding to different corneal curvatures are as follows: When the corneal curvature is 40.25D, the geometric parameters of the orthokeratology lens are: curvature 40.25D, base curve radius 9.00mm, positioning arc radius 8.37mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 41.25D, the geometric parameters of the orthokeratology lens are: curvature 41.25D, base arc radius 8.77mm, positioning arc radius 8.17mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 42.25D, the geometric parameters of the orthokeratology lens are: curvature 42.25D, base arc radius 8.50mm, positioning arc radius 7.98mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 43.25D, the geometric parameters of the orthokeratology lens are: curvature 43.25D, base curve radius 8.33mm, positioning arc radius 7.79mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 44.25D, the geometric parameters of the orthokeratology lens are: curvature 44.25D, base arc radius 8.13mm, positioning arc radius 7.62mm, diameter 10.6mm, and central area thickness 0.22mm.
[0011] In step (1), the mechanical performance parameters of the orthokeratology lens include elastic modulus and breaking strength.
[0012] The method for obtaining the mechanical performance parameters of orthokeratology lenses is as follows: As a biological tissue, the human cornea is a viscoelastic, anisotropic and incompressible material in its natural physiological state. In the finite element simulation of the cornea, the cornea is regarded as a hyperelastic, anisotropic and incompressible material, and the mechanical performance parameters of the orthokeratology lens are obtained using the strain energy function HGO model proposed by Gasser, Holzapfel and Ogden (Hu Junqi et al., Numerical Simulation of Factors Influencing the Corrective Effect of Orthokeratology Lenses, Journal of Taiyuan University of Technology, Vol. 55, No. 2, 2024.3). Through the above modeling, the relationship between the shaping effect and the geometric morphological parameters and mechanical properties of the orthokeratology lens is obtained, and the overall and regional morphological structure and mechanical properties are optimized.
[0013] The elastic modulus of orthokeratology lenses is 250-500MPa and the breaking strength is 35-50MPa.
[0014] In step (2), the support light-curable resin system is composed of the following raw materials in percentage by mass: Polyethylene glycol diacrylate (PEGDA) 10-20%, Gelatin methacrylate (GelMA) 5-10%, Photoinitiator 0.25-0.5%, Orange pigment light absorber 0.05-0.1%, Water balance.
[0015] Preferably, in the support photocurable resin system, methacrylated gelatin can also be replaced by acrylic acid, acrylamide, and the like.
[0016] The photoinitiator is at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 2,4,6-trimethylbenzoyl phenylphosphonic acid ethyl ester, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, 2,4-diethylthioxanthone, and phenol-ethyl formate.
[0017] The orange pigment light absorber is an ultraviolet light absorber, preferably UV-0.
[0018] The preparation method of the support photocurable resin system is as follows: Polyethylene glycol diacrylate, methacrylated gelatin, photoinitiator, orange pigment light absorber, and water are placed in a brown container and maintained at 37-50°C until completely dissolved to serve as support 3D printing ink.
[0019] In step (2), UG software is used to establish a 3D printing model that is consistent with the curvature of the back surface of the orthokeratology lens, and the support 3D printing ink is placed in the 3D printer material tank for printing. The printing time is 30-120 minutes, and then ultraviolet light irradiation molding is performed. The ultraviolet light irradiation wavelength is 365nm or 405nm.
[0020] The present invention prints a support first, and then prints a reshaping lens on the support, which can ensure that the reshaping lens maintains a stable mechanical structure during the printing process and is not easily deformed.
[0021] In step (3), the shaping mirror light-curing resin system is composed of the following raw materials in percentage by mass: Methyl methacrylate (MMA) 20-30%, Hydroxyethyl methacrylate (HEMA) 60-80%, Polyethylene glycol diacrylate (PEGDA) 1.5-2%, 3-(Isopropylacryloyloxy)propyltrimethoxysilane (KH-570) 7.25-18.2%, Photoinitiator 0.3-0.75%.
[0022] The photoinitiator is at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 2,4,6-trimethylbenzoyl phenylphosphonic acid ethyl ester, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, 2,4-diethylthioxanthone, and phenol-ethyl formate.
[0023] At least one of polyvinyl alcohol, polyvinyl pyrrolidone, and polyethylene glycol can be added to the above-mentioned photocurable resin system to replace MMA, with a mass percentage of 2-6wt.%; at least one of polypyrrole, polyaniline, Mxene, and poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid can also be added to replace part of HEMA, with a mass percentage of 2-6%.
[0024] In the photocurable resin system, the percentage of raw materials has an important influence on the performance of the product. For the photoinitiator, when its content is less than 0.3%, the number of free radicals generated is insufficient to start and maintain the polymerization reaction, resulting in the inability of the monomer to polymerize; with the increase of the photoinitiator content, the polymerization reaction rate increases, and the tensile strength and elastic modulus of the hydrogel both show an upward trend. When the photoinitiator content reaches 0.75%, the mechanical properties of the hydrogel reach the highest; when the photoinitiator content is higher than 0.75%, the polymerization reaction rate is too fast, and rapid polymerization will lead to insufficient growth of the polymer chain, the molecular weight of the generated polymer is low and the molecular chain is irregularly arranged, thereby affecting the mechanical properties of the hydrogel, causing its mechanical properties to decrease instead of increase. For methyl methacrylate (MMA), as its content increases, the tensile strength of the hydrogel increases, but the elastic modulus decreases. In order to make the hydrogel have good tensile strength and elastic modulus, its content is kept between 20-30%.
[0025] The preparation method of the shaping mirror light-curing resin system is as follows: Methyl methacrylate, hydroxyethyl methacrylate, polyethylene glycol diacrylate, and 3-(isobutyleneoxy)propyltrimethoxysilane are placed in a brown container, stirred evenly, and then a photoinitiator is added. Prepolymerization is carried out by ultraviolet light irradiation until the viscosity of the system is 3000-3600 mPa·s at 25°C, which is used as 3D printing ink for orthopedic lenses.
[0026] Preferably, the wavelength of ultraviolet light irradiation is 365 nm or 405 nm, and the prepolymerization time is 90-200 s.
[0027] The present invention first prepolymerizes the shaping mirror photocurable resin system to increase the viscosity of the system and keep its viscosity within the above range. If the viscosity of the ink is too low, it is difficult to form during the printing process, and if the viscosity is too high, it is not easy to print.
[0028] In step (3), the orthokeratology lens 3D printing ink is placed in the 3D printer extrusion printing barrel, and the orthokeratology lens is printed on the support. The printing time is 15-30 minutes, and the UV light curing time is 5-8 hours.
[0029] Compared with the prior art, the present invention has the following beneficial effects: (1) The geometric morphology and material mechanical performance parameters of the hydrogel corneal reshaping lens of the present invention are obtained through finite element modeling simulation, which fully considers the differences in biomechanical properties of the human cornea before wearing the lens and the changes in biomechanical properties of the human cornea after wearing the lens. It can more accurately predict the relationship between the mechanical properties and morphological indicators of the cornea and the reshaping effect of the reshaping lens materials, and realize the personalized design of the geometric morphology and mechanical properties of the reshaping lens in a true sense; (2) The hydrogel orthokeratology lens of the present invention is precisely formed by photocuring 3D printing. By establishing a finite element model of the cornea of the orthokeratology lens wearer, the geometric morphological parameters and mechanical performance parameters of the orthokeratology lens matching the target human body are obtained. The type of monomer and copolymerization ratio, prepolymerization time, printing time and ultraviolet irradiation time are determined and regulated according to the mechanical performance parameters, so as to realize the controllable design of the geometric structure and mechanical properties of the orthokeratology lens, achieve the best match between the force state of the orthokeratology lens on the cornea and the biomechanical properties of the cornea, and realize the "custom-made" orthokeratology lens; (3) The hydrogel orthokeratology lens prepared by the present invention has adjustable mechanical strength and good biocompatibility, and can monitor corneal deformation and intraocular pressure changes during the orthokeratology process. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The finite element model diagram of the cornea of the orthokeratology lens of the present invention; Figure 2 This is an optical image of the hydrogel orthokeratology lens printed in Example 1; Figure 3 This is an infrared spectrum of the hydrogel corneal reshaping lens printed in Example 1; Figure 4 This is a water contact angle diagram of the hydrogel corneal reshaping lens printed in Example 1; Figure 5 This is a scanning electron microscope image of the inner surface of the hydrogel orthokeratology lens printed in Example 1; Figure 6 This is a scanning electron microscope image of the outer surface of the hydrogel corneal reshaping lens printed in Example 1; Figure 7 This is a tensile performance diagram of the hydrogel orthokeratology lens printed in Example 1; Figure 8 This is the biocompatibility test image of the hydrogel corneal refractive therapy lens printed in Example 1. DETAILED DESCRIPTION
[0031] The present invention is further described below with reference to the examples and drawings. The raw materials used in the examples, unless otherwise specified, are all commercially available conventional raw materials; the process methods used in the examples, unless otherwise specified, are all conventional methods in the art.
[0032] In the embodiment, the index testing method of the hydrogel orthokeratology lens is as follows: (1) Water contact angle test: The water contact angle test was carried out at room temperature using a HARKE-SPCAX3 contact angle tester. The droplet size was 3.0 μL, and the average value was taken after five measurements.
[0033] (2) Equilibrium water content (EWC) and oxygen permeability (DK) test: After freeze-drying, soak the orthokeratology lens in deionized water at room temperature and measure it every 2 hours until the mass no longer changes. Record the weight before soaking and the weight at water absorption equilibrium, then the equilibrium water content. The DK value depends on the equilibrium water content of the orthokeratology lens saturated with water, and the data used are the average of 5 independent tests.
[0034] (3) Elastic modulus and breaking strength test: The tensile properties of hydrogel orthokeratology lenses were tested using a universal testing machine (INSTRON 3343). The geometry of the test specimen was dumbbell-shaped and the loading rate was 10 mm / min.
[0035] (4) Fourier transform infrared spectroscopy analysis: First, the prepared hydrogel orthokeratology lens was soaked in water for 2 hours, then placed in a flat polytetrafluoroethylene mold, and quickly transferred to a vacuum freeze dryer for 24 hours after being frozen in a refrigerator for 48 hours. The samples were tested at room temperature using attenuated total reflection infrared spectroscopy (ATR-FTIR, Thermo Scientific Nicolet iS50) with a wavelength range of 4000-400 cm -1 , the scanning speed is 0.25Hz-125kHz.
[0036] (5) Biocompatibility test method: Rabbit corneal epithelial cells (rCECs) were used as culture cells. The hydrogel corneal reshaping lenses were immersed in culture medium for 24 hours, and then the cells were cultured with culture medium without hydrogel extract (control group) and culture medium containing hydrogel extract (experimental group), respectively. The cells in the culture medium were subjected to live-dead staining experiments on 1 day and 3 days, respectively, and stained with acridine orange (AO) green dye (10 mg / mL, 1µL) and propidium iodide (PI) red dye (1 mg / mL, 10µL). The stained samples were observed using a fluorescence microscope (EVOSM5000, ThermoFisher Scientific), and the images of green-stained live cells and red-stained dead cells were captured, respectively, to study the relative survival rate of cells co-cultured with hydrogels. If the relative survival rate of cells is greater than 1, it means that the hydrogel has good biocompatibility.
[0037] Example 1 A 3D printing method for a hydrogel orthokeratology lens comprises the following steps: (1) The finite element method was used to simulate the effect of wearing orthokeratology lenses on the cornea. A finite element model of the cornea wearing orthokeratology lenses was established. The cornea was regarded as a hyperelastic, anisotropic material. The hyperelastic constitutive equation of the material used the strain energy function proposed by Gasser, Holzapfel, and Ogden, namely the HGO model, in which the elastic modulus of the corneal stroma was 0.02 MPa, the stiffness modulus of the collagen fibers was 50 MPa, and the dispersion range of the collagen fibers was 1 / 3. The orthokeratology lenses were regarded as elastic materials. The curvature, thickness, and mechanical properties of the orthokeratology lenses were changed (the corneal curvature was 40.2 5D, 41.25D, 42.25D, 43.25D, 44.25D, thicknesses of 200μm, 500μm, 525μm, 550μm, 575μm, and elastic modulus of 50MPa-1GPa), and calculated the biomechanical response of the cornea after wearing the lens. Finally, the geometric parameters of the adapted orthokeratology lens were obtained as follows: thickness 200μm, curvature 40.25D, base curve radius 9.00mm, positioning curve radius 8.37mm, diameter 10.6mm, central area thickness 0.22mm; the mechanical performance parameters are: elastic modulus 260MPa.
[0038] (2) In terms of mass percentage, 20% of polyethylene glycol diacrylate, 5% of methacrylated gelatin, 0.25% of phenyl-2,4,6-trimethylbenzoyl lithium phosphinate, 0.05% of orange pigment light absorber, and 74.7% of water were placed in a brown container and maintained at 37°C until completely dissolved to obtain a support photocurable resin system as a support 3D printing ink. Based on the geometric morphological parameters of the orthokeratology lens obtained by simulation, a 3D printing model consistent with the curvature of the posterior surface of the orthokeratology lens was established using UG software, and the support 3D printing ink was placed in the trough of the 3D printer for printing and curing. The printing time was 40 minutes and the ultraviolet light wavelength was 405 nm.
[0039] (3) Based on the mechanical properties of orthokeratology lenses obtained by simulation, the monomer type and copolymerization ratio, prepolymerization time, printing time and UV irradiation time of the materials were regulated. In terms of mass percentage, 30% of methyl methacrylate, 60% of hydroxyethyl methacrylate, 1.2% of polyethylene glycol diacrylate, and 8.2% of 3-(isobutyleneoxy)propyltrimethoxysilane were placed in a brown container, stirred evenly, and then 0.6% of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide was added. The mixture was irradiated with ultraviolet light at a wavelength of 405 nm for 100 seconds for prepolymerization to obtain an orthokeratology lens photocurable resin system as orthokeratology lens 3D printing ink. Based on the geometric structure parameters of the orthokeratology lens obtained by simulation, a 3D printing model was established, and the orthokeratology lens 3D printing ink was placed in the extrusion printing barrel of the 3D printer. The orthokeratology lens was printed on the surface of the support for 15 minutes. After that, it was irradiated with ultraviolet light at a wavelength of 405nm for 5 hours to obtain the hydrogel orthokeratology lens.
[0040] The optical morphology of the hydrogel orthokeratology lens is as follows Figure 2 As shown, from Figure 2 It can be seen that the 3D printed hydrogel corneal reshaping lens of the present invention can maintain its shape.
[0041] The infrared spectrum test results of the hydrogel orthokeratology lens are as follows: Figure 3 As shown, Figure 3 As shown in Figure 2, the absorption peaks of hydroxyl and ester carbonyl appear at 3419 cm -1 and 1714cm -1 Nearby, 2943cm -1 The absorption peak at 1234 cm corresponds to the stretching of n-alkanes (-CH), (-CH2-), and (-CH3). -1 The peak at 1200-1000 cm-1 is assigned to the bending vibration of -CH3, while the peak at 1200-1000 cm-1 is assigned to the bending vibration of -CH3. -1 The double peaks appearing in the interval correspond to Si-O bonds.
[0042] The water contact angle test results of the hydrogel corneal reshaping lens are as follows: Figure 4 As shown, from Figure 4 It can be seen that the water contact angle of the surface of the hydrogel orthokeratology lens is 73°, indicating that it has good hydrophilicity.
[0043] The scanning electron microscopy results of the hydrogel corneal reshaping lens are as follows Figure 5-6 As shown, from Figure 5-6 It can be seen that the surfaces of different areas of the inner and outer surfaces of the hydrogel orthokeratology lens are smooth and free of particles.
[0044] The tensile properties test results of the hydrogel corneal reshaping lens are as follows: Figure 7 As shown, from Figure 7It can be seen that the stress of the hydrogel orthokeratology lens increases linearly with strain. When the strain reaches 0.11, the sample is destroyed, indicating that it has a high elastic modulus.
[0045] The biocompatibility test results of the hydrogel orthokeratology lens are as follows: Figure 8 As shown, from Figure 8 It can be seen that rabbit corneal epithelial cells (rCECs) were cultured in a culture medium without hydrogel extract (control group) and a culture medium containing hydrogel extract (experimental group), and live-dead staining experiments were performed on the cells in the culture medium on the 1st and 3rd days. The number of live cells stained green increased significantly, indicating that the extract of the hydrogel corneal reshaping lens has good biocompatibility.
[0046] Example 2 A 3D printing method for a hydrogel orthokeratology lens comprises the following steps: (1) The finite element method was used to simulate the effect of wearing orthokeratology lenses on the cornea. A finite element model of the cornea wearing orthokeratology lenses was established. The cornea was regarded as a hyperelastic, anisotropic material. The hyperelastic constitutive equation of the material used the strain energy function proposed by Gasser, Holzapfel, and Ogden, namely the HGO model, in which the elastic modulus of the corneal stroma was 1.5 MPa, the stiffness modulus of the collagen fibers was 150 MPa, and the dispersion range of the collagen fibers was 1 / 3. The orthokeratology lenses were regarded as elastic materials, and the curvature, thickness, and mechanical properties of the orthokeratology lenses were changed (the corneal curvature was selected as 40.2 5D, 41.25D, 42.25D, 43.25D, 44.25D, thicknesses of 200μm, 500μm, 525μm, 550μm, 575μm, and elastic modulus of 50MPa-1GPa), and calculated the biomechanical response of the cornea after wearing the lens. Finally, the geometric parameters of the adapted orthokeratology lens were obtained as follows: thickness 300μm, curvature 44.25D, base curve radius 8.13mm, positioning curve radius 7.62mm, diameter 10.6mm, central area thickness 0.22mm; the mechanical performance parameters are: elastic modulus 400MPa.
[0047] (2) In terms of mass percentage, 20% of polyethylene glycol diacrylate, 5% of methacrylated gelatin, 0.25% of phenyl-2,4,6-trimethylbenzoyl lithium phosphinate, 0.05% of orange pigment light absorber, and 74.7% of water were placed in a brown container and maintained at 37°C until completely dissolved to obtain a support photocurable resin system as a support 3D printing ink. Based on the geometric morphological parameters of the orthokeratology lens obtained by simulation, a 3D printing model consistent with the curvature of the posterior surface of the orthokeratology lens was established using UG software, and the support 3D printing ink was placed in the trough of the 3D printer for printing and curing. The printing time was 40 minutes and the ultraviolet light wavelength was 405 nm.
[0048] (3) Based on the mechanical properties of orthokeratology lenses obtained by simulation, the monomer type and copolymerization ratio, prepolymerization time, printing time and UV irradiation time of the materials were regulated. In terms of mass percentage, 30% of methyl methacrylate, 60% of hydroxyethyl methacrylate, 1.2% of polyethylene glycol diacrylate, and 8.2% of 3-(isobutyleneoxy)propyltrimethoxysilane were placed in a brown container, stirred evenly, and then 0.75% of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide was added. The mixture was irradiated with ultraviolet light at a wavelength of 405 nm for 140 seconds for prepolymerization to obtain an orthokeratology lens photocurable resin system as orthokeratology lens 3D printing ink. Based on the geometric structure parameters of the orthokeratology lens obtained by simulation, a 3D printing model was established, and the orthokeratology lens 3D printing ink was placed in the extrusion printing barrel of the 3D printer. The orthokeratology lens was printed on the surface of the support for 20 minutes. After that, it was irradiated with ultraviolet light at a wavelength of 405nm for 6 hours to obtain the hydrogel orthokeratology lens.
[0049] Example 3 A 3D printing method for a hydrogel orthokeratology lens comprises the following steps: (1) The finite element method was used to simulate the effect of wearing orthokeratology lenses on the cornea. A finite element model of the cornea wearing orthokeratology lenses was established. The cornea was regarded as a hyperelastic, anisotropic material. The hyperelastic constitutive equation of the material used the strain energy function proposed by Gasser, Holzapfel, and Ogden, namely the HGO model, in which the elastic modulus of the corneal stroma was 1 MPa, the stiffness modulus of the collagen fibers was 100 MPa, and the dispersion range of the collagen fibers was 1 / 3. The orthokeratology lenses were regarded as elastic materials, and the curvature, thickness, and mechanical properties of the orthokeratology lenses were changed (the corneal curvature was selected as 40.25 D, 41.25D, 42.25D, 43.25D, 44.25D, thicknesses of 200μm, 500μm, 525μm, 550μm, 575μm, and elastic modulus of 50MPa-1GPa), the biomechanical response of the cornea after wearing the lens was calculated, and the final geometric parameters of the adapted orthokeratology lens were: thickness 200μm, curvature 43.25D, base curve radius 8.33mm, positioning arc radius 7.79mm, diameter 10.6mm, central area thickness 0.22mm; the mechanical performance parameters are: elastic modulus 500MPa.
[0050] (2) In terms of mass percentage, 20% polyethylene glycol diacrylate, 5% methacrylated gelatin, 0.25% phenyl-2,4,6-trimethylbenzoyl lithium phosphinate, 0.05% orange pigment light absorber, and 74.7% water were placed in a brown container and maintained at 37°C until completely dissolved to obtain a support photocurable resin system as a support 3D printing ink. Based on the geometric morphological parameters of the orthokeratology lens obtained by simulation, a 3D printing model consistent with the curvature of the posterior surface of the orthokeratology lens was established using UG software, and the support 3D printing ink was placed in the trough of the 3D printer for printing and curing. The printing time was 120 minutes and the ultraviolet light wavelength was 405 nm.
[0051] (3) Based on the mechanical properties of orthokeratology lenses obtained by simulation, the monomer type and copolymerization ratio, prepolymerization time, printing time and UV irradiation time of the materials were regulated. In terms of mass percentage, 30% of methyl methacrylate, 60% of hydroxyethyl methacrylate, 1.2% of polyethylene glycol diacrylate, and 8.2% of 3-(isobutyleneoxy)propyltrimethoxysilane were placed in a brown container, stirred evenly, and then 0.75% of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide was added. The mixture was irradiated with ultraviolet light at a wavelength of 405 nm for 200 seconds for prepolymerization to obtain an orthokeratology lens photocurable resin system as orthokeratology lens 3D printing ink. Based on the geometric structure parameters of the orthokeratology lens obtained by simulation, a 3D printing model was established, and the 3D printing ink of the orthokeratology lens was placed in the extrusion printing barrel of the 3D printer. The orthokeratology lens was printed on the surface of the support for 30 minutes. After that, it was irradiated with ultraviolet light of a wavelength of 405nm for 8 hours to obtain the hydrogel orthokeratology lens.
[0052] Comparative Example 1 In this comparative example, the finite element method is not used to simulate the effect of wearing orthokeratology lenses. The geometric parameters of orthokeratology lenses are designed directly according to the corneal topography: thickness 220 μm, curvature 42.25D, base arc radius 8.23 mm, positioning arc radius 7.69 mm, diameter 10.5 mm, and central area thickness 0.21 mm. Then, printing is performed according to the methods of step (2) and step (3) of Example 1.
[0053] Comparative Example 2 The difference between this comparative example and Example 3 is that the formula of the orthokeratology lens 3D printing ink in step (3) is adjusted. In terms of mass percentage, this comparative example places 35% of methyl methacrylate, 55% of hydroxyethyl methacrylate, 2.5% of polyethylene glycol diacrylate, and 7.3% of 3-(isobutyleneoxy)propyltrimethoxysilane in a brown container, stirs evenly, adds 0.2% of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and irradiates with ultraviolet light at a wavelength of 405nm for 200s to use as the orthokeratology lens 3D printing ink; based on the simulated geometric structure parameters of the orthokeratology lens, a 3D printing model is established, the orthokeratology lens 3D printing ink is placed in the extrusion printing barrel of the 3D printer, and the orthokeratology lens is printed on the surface of the support for 30 minutes. After irradiation with ultraviolet light at a wavelength of 405nm for 12 hours, it still fails to form because the photoinitiator content is too low and the number of free radicals generated is insufficient to initiate the polymerization reaction.
[0054] Comparative Example 3 The difference between this comparative example and Example 1 is that the formula of the orthokeratology lens 3D printing ink in step (3) is adjusted. In terms of mass percentage, this comparative example places 5% of methyl methacrylate, 85% of hydroxyethyl methacrylate, 1.2% of polyethylene glycol diacrylate, and 8.2% of 3-(isobutyleneoxy)propyltrimethoxysilane in a brown container, stirs evenly, adds 0.6% of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and irradiates with ultraviolet light of a wavelength of 405nm for 100s to perform prepolymerization to obtain a photocurable resin system for orthokeratology lenses as 3D printing ink for orthokeratology lenses. Based on the geometric structure parameters of the orthokeratology lens obtained by simulation, a 3D printing model is established, and the orthokeratology lens 3D printing ink is placed in the extrusion printing barrel of a 3D printer, and the orthokeratology lens is printed on the surface of the support for 15 minutes, and then irradiated with ultraviolet light of a wavelength of 405nm for 5 hours to obtain a hydrogel orthokeratology lens.
[0055] The performance of the hydrogel corneal reshaping lenses prepared in the embodiments and comparative examples was tested, and the test results are shown in Table 1.
[0056] As can be seen from Table 1, Comparative Example 1 did not build a model based on the biomechanical properties of the cornea and predict and correct the geometric parameters of the orthokeratology lens. Although Comparative Example 3 predicted and corrected the geometric parameters of the orthokeratology lens, it did not consider the influence of the mechanical performance parameters of the orthokeratology lens. The above two comparative examples ignored the relationship between the mechanical properties and morphological indicators of the orthokeratology lens materials and the shaping effect, resulting in a decrease in the vertex displacement and a deterioration in the shaping effect. This shows that the orthokeratology lens optimized by finite element modeling in the present invention has a better shaping effect.
Claims
1. A 3D printing method for a hydrogel orthokeratology lens with adjustable mechanical properties, characterized in that: The following steps are involved: (1) Establish a finite element model of the cornea wearing orthokeratology lenses to obtain the geometric parameters and mechanical performance parameters of orthokeratology lenses that match the target human cornea; (2) Based on the geometric parameters of the orthokeratology lens obtained by simulation, a 3D printing model consistent with the curvature of the posterior surface of the orthokeratology lens is established, and the support is printed using the support photocurable resin system as the support 3D printing ink; (3) Based on the geometric structure parameters and mechanical property parameters of the orthokeratology lens obtained by simulation, a 3D printing model was established and the formula of the photocurable resin system of the orthokeratology lens was adjusted. The photocurable resin system of the orthokeratology lens was used as the 3D printing ink for the orthokeratology lens, and the hydrogel orthokeratology lens was printed on the surface of the support. After curing by ultraviolet light, the hydrogel orthokeratology lens was obtained. In step (3), the shaping mirror light-curing resin system is composed of the following raw materials in percentage by mass: Methyl methacrylate 20-30%, Hydroxyethyl methacrylate 60-80%, Polyethylene glycol diacrylate 1.5-2%, 3-(Isopropylacryloyloxy)propyltrimethoxysilane 7.25-18.2%, Photoinitiator 0.3-0.75%.
2. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1, characterized in that: In step (1), the geometric parameters of the orthokeratology lens include thickness, curvature, base arc radius, positioning arc radius, diameter, and central zone thickness; The method for obtaining the geometric parameters of orthokeratology lenses is as follows: assuming that the cornea has uniform thickness and the curvature at different positions is the same, the geometric parameters of orthokeratology lenses corresponding to different corneal curvatures are as follows: When the corneal curvature is 40.25D, the geometric parameters of the orthokeratology lens are: curvature 40.25D, base curve radius 9.00mm, positioning arc radius 8.37mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 41.25D, the geometric parameters of the orthokeratology lens are: curvature 41.25D, base arc radius 8.77mm, positioning arc radius 8.17mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 42.25D, the geometric parameters of the orthokeratology lens are: curvature 42.25D, base arc radius 8.50mm, positioning arc radius 7.98mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 43.25D, the geometric parameters of the orthokeratology lens are: curvature 43.25D, base curve radius 8.33mm, positioning arc radius 7.79mm, diameter 10.6mm, central zone thickness 0.22mm; When the corneal curvature is 44.25D, the geometric parameters of the orthokeratology lens are: curvature 44.25D, base arc radius 8.13mm, positioning arc radius 7.62mm, diameter 10.6mm, and central area thickness 0.22mm.
3. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1, characterized in that: In step (1), the mechanical performance parameters of the orthokeratology lens include elastic modulus and fracture strength; The method for obtaining the mechanical performance parameters of orthokeratology lenses is as follows: the cornea is regarded as a hyperelastic, anisotropic and incompressible material, and the strain energy function HGO model proposed by Gasser, Holzapfel and Ogden is used to obtain the mechanical performance parameters of orthokeratology lenses. The elastic modulus of orthokeratology lenses is 250-500MPa, and the fracture strength is 35-50MPa.
4. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1, characterized in that: In step (2), the support light-curable resin system is composed of the following raw materials in percentage by mass: Polyethylene glycol diacrylate 10-20%, Methacrylated gelatin 5-10%, Photoinitiator 0.25-0.5%, Orange pigment light absorber 0.05-0.1%, Water balance.
5. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1 or 4, characterized in that: The photoinitiator is at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 2,4,6-trimethylbenzoyl phenylphosphonic acid ethyl ester, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, 2,4-diethylthioxanthone, and phenol-ethyl formate.
6. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 4, characterized in that: The preparation method of the support light-curable resin system is as follows: Polyethylene glycol diacrylate, methacrylated gelatin, photoinitiator, orange pigment light absorber, and water are placed in a brown container and maintained at 37-50°C until completely dissolved to serve as support 3D printing ink.
7. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1, characterized in that: In step (2), UG software is used to establish a 3D printing model that is consistent with the curvature of the back surface of the orthokeratology lens, and the support 3D printing ink is placed in the 3D printer material tank for printing. The printing time is 30-120 minutes, and then ultraviolet light irradiation molding is performed. The ultraviolet light irradiation wavelength is 365nm or 405nm.
8. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1, characterized in that: The preparation method of the shaping mirror light-curing resin system is as follows: Methyl methacrylate, hydroxyethyl methacrylate, polyethylene glycol diacrylate, and 3-(isobutyleneoxy)propyltrimethoxysilane are placed in a brown container, stirred evenly, and then a photoinitiator is added. Prepolymerization is carried out by ultraviolet light irradiation until the viscosity of the system is 3000-3600 mPa·s at 25°C, which is used as 3D printing ink for orthopedic lenses.
9. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 8, characterized in that: The wavelength of ultraviolet light irradiation is 365nm or 405nm, and the prepolymerization time is 90-200s.
10. The 3D printing method of the hydrogel orthokeratology lens with adjustable mechanical properties according to claim 1, characterized in that: In step (3), the orthokeratology lens 3D printing ink is placed in the 3D printer extrusion printing barrel, and the orthokeratology lens is printed on the support. The printing time is 15-30 minutes, and the UV light curing time is 5-8 hours.
Citation Information
Cited By
3D printing hydrogel material, preparation method thereof and application of 3D printing hydrogel material in preparation of intelligent contact lenses
CN121895496A
3D-printed hydrogel materials, methods of making the same, and applications thereof in the preparation of smart contact lenses
CN121895496B