Martensite heat-resistant steel with high creep strength and heat treatment method thereof
By utilizing a combination of nitrogen heating, vacuum rotation, and cooling media in the heat treatment of martensitic heat-resistant steel, the precipitation of the MX phase is increased, and the coarsening of the M23C6 phase is suppressed. This solves the creep strength problem of martensitic heat-resistant steel under high temperature and high pressure conditions and improves the high temperature creep resistance of the material.
Patent Information
- Application Number
- CN202411099171.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-08
AI Technical Summary
When existing martensitic heat-resistant steels are used in high-temperature and high-pressure environments, frequent temperature cycles and alternating loads lead to a decrease in creep strength, coarsening of the M23C6 carbide phase and Laves phase, and a reduction in the ability to hinder dislocation movement and grain boundary migration.
A heat treatment method is adopted, which includes heating and holding in a nitrogen-filled furnace, then evacuating and rotating, followed by spraying a cooling medium to cool to room temperature and tempering. The nitriding and cooling processes are optimized to increase the fine and dispersed distribution of the MX phase and suppress the coarsening of the M23C6 phase and the formation of δ ferrite.
It improves the high-temperature creep resistance of martensitic heat-resistant steel by pinning dislocations with fine and dispersed MX phases, hindering dislocation recovery, and enhancing the high-temperature creep performance of the material.
Smart Images

Figure CN118910373A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heat-resistant steel production, and in particular to a martensitic heat-resistant steel with high creep strength and a heat treatment method thereof. Background Art
[0002] Martensitic heat-resistant stainless steel has high thermal conductivity and low thermal expansion coefficient, good thermal fatigue resistance, good hot and cold processing performance, excellent welding performance, and high thermal strength. Therefore, martensitic heat-resistant stainless steel can be used to make important parts such as high-pressure compressor discs and rotor blades of aircraft engines. It is also often used to manufacture parts used in high-temperature environments in industrial fields such as boilers, steam turbines, power machinery, industrial furnaces, and petrochemicals. These parts not only need to have good high-temperature strength and high-temperature oxidation corrosion resistance, but also need to have sufficient toughness, good processability and weldability, and a certain degree of organizational stability to meet different uses.
[0003] Martensitic heat-resistant stainless steel mainly includes two types: oxidation-resistant steel (or high-temperature non-scaling steel) and heat-resistant steel. Oxidation-resistant steel generally requires good chemical stability, but the load it bears is low. Heat-resistant steel requires higher high-temperature strength and corresponding oxidation resistance. With the continuous adjustment and optimization of alloying components, the endurance strength of martensitic heat-resistant steel continues to improve. Cr is the basic alloying element in martensitic heat-resistant steel and belongs to the ferrite-forming element. The oxidation corrosion resistance of martensitic heat-resistant steel increases with the increase of Cr content. When the Cr content exceeds 11%, the corrosion performance of the material at 650°C can be significantly improved. Therefore, martensitic heat-resistant steel with a Cr content of 9%~12% is widely used. However, martensitic heat-resistant steel with a Cr content of 9%~12% often encounters frequent temperature cycle changes and withstands various alternating loads when serving in high temperature and high pressure environments, so it often produces high-temperature creep.
[0004] Martensitic heat-resistant steel with a Cr content of 9% to 12% is a lath-like structure rich in high-density dislocations. Various fine precipitation strengthening phases are widely and dispersedly distributed inside and at the boundary of the structure, such as M 23 C6 carbide phase, MX phase, Laves phase, etc. The complex interaction between these precipitated phases, dislocation structure, and grain boundary interface improves the high temperature creep resistance and thermal stability of martensitic heat-resistant steel. However, during the long-term service of this type of martensitic heat-resistant steel, M 23 The C6 carbide phase and Laves phase tend to coarsen significantly, which significantly weakens their ability to hinder dislocation movement and grain boundary migration, causing a significant deterioration in the high-temperature creep strength of this type of martensitic heat-resistant steel.
[0005] Therefore, how to improve the high temperature creep strength of martensitic heat-resistant steel is an urgent problem to be solved in this field. Summary of the invention
[0006] In view of the above problems existing in the prior art, the present invention provides a martensitic heat-resistant steel with high creep strength and a heat treatment method thereof.
[0007] According to one aspect of the present invention, there is provided a heat treatment method for martensitic heat-resistant steel, the method comprising the following steps: Step S1: placing the martensitic heat-resistant steel into a heating furnace filled with nitrogen for heating and heat preservation; Step S2: evacuate the heating furnace and rotate the martensitic heat-resistant steel in the heating furnace; Step S3: stopping heating, spraying cooling medium on the surface of the rotating martensitic heat-resistant steel to cool the martensitic heat-resistant steel to room temperature, and performing pressure relief operation; Step S4: Stop the rotation and the splashing, and perform a tempering treatment on the martensitic heat-resistant steel to obtain the martensitic heat-resistant steel with improved creep strength.
[0008] According to one embodiment of the present invention, the martensitic heat-resistant steel includes the following components in mass percentage: C: 0.07%~0.14%, Si≤0.2%, Mn: 0.4%~0.9%, Mo: 1.5%~2.0%, Cr: 11%~12.6%, Co: 1%~3%, Ni: 2%~3%, V: 0.2%~0.4%, N: 0.025%~0.04%, B: 0.001%~0.003%, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0009] According to one embodiment of the present invention, the martensitic heat-resistant steel includes the following components in mass percentage: C: 0.09%~0.12%, Si≤0.2%, Mn: 0.6%~0.8%, Mo: 1.65%~1.8%, Cr: 11.5%~12%, Co: 1.5%~2.5%, Ni: 2.3%~2.8%, V: 0.25%~0.35%, N: 0.03%~0.035%, B: 0.002%~0.003%, S≤0.02%, P≤0.02%, and the rest is Fe and unavoidable impurities.
[0010] According to one embodiment of the present invention, the heating temperature in step S1 is 1000-1100° C., and the holding time is 0.5-1 h.
[0011] According to one embodiment of the present invention, in step S2, the martensitic heat-resistant steel is rotated to a rotation speed of 400-600 rpm.
[0012] According to one embodiment of the present invention, the cooling medium in step S3 is a mixture of argon and quenching oil or argon and liquid metal, the gas content of the mixture is controlled at 40% to 70%, and the injection intensity is greater than 5L / (min·m²).
[0013] According to one embodiment of the present invention, the liquid metal is selected from at least one of gallium-based liquid metal and bismuth-based liquid metal.
[0014] According to one embodiment of the present invention, the tempering process includes primary tempering and secondary tempering.
[0015] According to one embodiment of the present invention, the tempering temperature of the primary tempering is 500-600° C., and the tempering time is 0.5-1.5 h.
[0016] According to one embodiment of the present invention, the tempering temperature of the secondary tempering is 480-580° C., and the tempering time is 0.5-1.5 h.
[0017] According to another aspect of the present invention, there is provided a martensitic heat-resistant steel with high creep strength, wherein the martensitic heat-resistant steel with high creep strength is prepared by the heat treatment method described in any of the above embodiments.
[0018] In the technical solution of the present invention, the heat treatment method of the present invention performs nitriding treatment on martensitic heat-resistant steel, and by optimizing the processes of nitriding, cooling, tempering, etc., the fine and dispersed MX phase is fully precipitated in the martensitic heat-resistant steel, while reducing the amount of delta ferrite, thereby further improving the high-temperature creep resistance of the martensitic heat-resistant steel. Furthermore, by optimizing the chemical composition of the martensitic heat-resistant steel, the precipitation amount of the MX phase in the martensitic heat-resistant steel is increased, and the M 23 The creep strength of the material is improved by the coarsening and growth of the C6 phase and the inhibition of the formation of δ ferrite. The coarsening rate of the MX precipitate phase during high temperature creep is low, which can effectively pin dislocations, hinder the recovery of dislocations and martensite laths, and improve the high temperature creep resistance of martensitic heat-resistant steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0020] Figure 1 is a flow chart of a heat treatment method for martensitic heat-resistant steel according to one embodiment of the present invention; Figure 2 A schematic structural diagram of an apparatus for implementing the heat treatment method according to the present invention; Figure 3 This is a metallographic photograph of the martensitic heat-resistant steel prepared by the method of Example 5; Figure 4 This is a metallographic photograph of the martensitic heat-resistant steel prepared by the method of Comparative Example 4.
[0021] In the attached picture: 10. furnace body; 20. vacuum pump; 30. nitrogen source; 40. rotating mechanism; 50. cooling mechanism; W. workpiece. DETAILED DESCRIPTION
[0022] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0023] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0024] It should be understood that the embodiments of the present invention shown in the exemplary embodiments are only illustrative. Although only a few embodiments are described in detail in the present invention, it is easy for those skilled in the art to appreciate that multiple modifications are feasible without actually departing from the teaching of the subject matter of the present invention. Accordingly, all such modifications should be included within the scope of the present invention. Without departing from the gist of the present invention, other replacements, modifications, changes and deletions may be made to the design, operating conditions and parameters of the following exemplary embodiments.
[0025] As described in the background art, martensitic heat-resistant steel with a Cr content of 9% to 12% is a lath-like structure rich in high-density dislocations, and a variety of fine precipitation strengthening phases are widely and dispersedly distributed inside and in the boundary areas of the structure, such as M 23 C6 carbide phase, MX phase, Laves phase, etc., rely on the complex interaction between these precipitation phases and dislocation structure and grain boundary interface to improve the high temperature creep resistance and thermal stability of martensitic heat-resistant steel. However, during the long-term service of this type of martensitic heat-resistant steel, M 23 The C6 carbide phase and Laves phase tend to coarsen significantly, which significantly weakens their ability to hinder dislocation movement and grain boundary migration, which in turn leads to a significant deterioration in the high temperature creep strength of this type of martensitic heat-resistant steel.
[0026] In order to solve the above problems, according to one aspect of the present invention, a heat treatment method for martensitic heat-resistant steel is provided. Figure 1As shown, the method generally comprises the following steps: Step S1: placing the martensitic heat-resistant steel into a heating furnace filled with nitrogen for heating and heat preservation; Step S2: evacuate the heating furnace and rotate the martensitic heat-resistant steel in the heating furnace; Step S3: stopping heating, spraying cooling medium on the surface of the rotating martensitic heat-resistant steel to cool the martensitic heat-resistant steel to room temperature, and performing pressure relief operation; Step S4: Stop the rotation and the splashing, and perform a tempering treatment on the martensitic heat-resistant steel to obtain the martensitic heat-resistant steel with improved creep strength.
[0027] In some embodiments, the martensitic heat-resistant steel includes the following components in mass percentage: C: 0.07%~0.14%, Si≤0.2%, Mn: 0.4%~0.9%, Mo: 1.5%~2.0%, Cr: 11%~12.6%, Co: 1%~3%, Ni: 2%~3%, V: 0.2%~0.4%, N: 0.025%~0.04%, B: 0.001%~0.003%, S≤0.02%, P≤0.02%, and the rest is Fe and unavoidable impurities.
[0028] C (carbon) is an important element for forming, stabilizing and expanding the austenite phase region, which can inhibit the formation of delta ferrite, which is not conducive to the high-temperature creep performance of the material. C can combine with metal elements Cr, Mo, V and other alloy elements in steel to form carbides. The higher the C content, the more carbides precipitate after tempering. With the increase of C content, the strength, hardness, wear resistance and hot hardness of martensitic heat-resistant steel increase, but the plasticity, toughness and weldability decrease. In addition, too high C content will promote the aggregation and growth of carbides, and reduce the creep strength of the material. Therefore, in the present invention, the C content is controlled at 0.07%~0.14%, and further, the C content is controlled at 0.09%~0.12%.
[0029] Si (silicon) can form a dense SiO2 or Si-containing spinel layer on the surface of the material, thereby improving the oxidation resistance of martensitic heat-resistant steel. However, excessive Si content will promote the precipitation of coarse Laves phase from the matrix, resulting in a significant weakening of the Laves phase's ability to hinder dislocation movement and grain boundary migration, thereby reducing the high-temperature creep strength of martensitic heat-resistant steel. Therefore, in the present invention, the Si content is controlled to be below 0.2%.
[0030] Mn (manganese) can expand the austenite phase area and infinitely dissolve with Fe, playing a role in solid solution strengthening. Mn can also significantly improve the hardenability of steel. However, Mn will promote the diffusion of atoms at high temperatures, accelerating the M 23The coarsening and growth of the C6 phase, and the addition of excessive Mn will reduce the creep strength of the steel and the thermal stability of the structure. Therefore, in the present invention, the Mn content is controlled at 0.4% to 0.9%, and further, the Mn content is controlled at 0.6% to 0.8%.
[0031] Mo (molybdenum) can improve the bonding force between atoms in heat-resistant steel, thereby reducing the self-diffusion coefficient of the matrix and improving the thermal stability and creep resistance of the heat-resistant steel. Mo can also improve A c1 Temperature, improve the impact toughness of steel. However, when the Mo addition is too high, it will shorten the time for the Laves phase to precipitate from the matrix, and vacancies will gather around the Laves phase to form creep holes. The risk of brittle fracture of the material during long-term service will increase. Therefore, in the present invention, the Mo content is controlled at 1.5% to 2.0%, and further, the Mo content is controlled at 1.65% to 1.8%.
[0032] Cr (chromium) can form a dense oxide film on the surface of martensitic heat-resistant steel, delaying the oxidation of Fe. The addition of Cr can improve the oxidation resistance and steam corrosion resistance of steel, and the higher the Cr content, the stronger the oxidation resistance and steam corrosion resistance. Cr can also form M with C. 23 C6 precipitation phase, which is an important precipitation phase in heat-resistant steel. In addition, Cr can also be dissolved in the matrix to form solid solution strengthening. However, with the increase of Cr content, the transformation of MX phase to Z phase is accelerated during high-temperature creep. Z phase is a complex nitride. Martensitic heat-resistant steel will precipitate coarse Z phase under long-term creep above 550°C, which is formed by consuming pre-existing fine carbonitrides, which will cause the creep strength to drop rapidly. In addition, when the Cr content is too high, δ ferrite will be formed, which is not conducive to the high-temperature creep performance of the material. Therefore, it is necessary to reasonably control the content of Cr element in martensitic heat-resistant steel. In the present invention, the Cr content is controlled at 11%~12.6%, and further, the Cr content is controlled at 11.5%~12%.
[0033] Co (cobalt) can improve the toughness of the material in heat-resistant steel. Co can also reduce the self-diffusion coefficient of the matrix and inhibit the M 23 The coarsening and growth of the C6 phase improves the creep strength of the material. Co is an austenite-forming element. Adding Co to steel can effectively inhibit the formation of delta ferrite, which is not conducive to the high-temperature creep performance of the material. However, Co is a rare metal element and is expensive. Adding a large amount of Co will greatly increase the production cost of heat-resistant steel. Therefore, in the present invention, the Co content is controlled at 1% to 3%, and further, the Co content is controlled at 1.5% to 2.5%.
[0034] Ni (nickel) is an austenite-forming element. Ni can significantly inhibit the formation of delta ferrite, which is not conducive to the high temperature creep performance of the material. However, adding excessive Ni will cause M 23 The thermal stability of the C6 phase is reduced, which causes it to transform into a coarse M6C phase. Therefore, in the present invention, the Ni content is controlled at 2% to 3%, and further, the Ni content is controlled at 2.3% to 2.8%.
[0035] V (vanadium) is a strong carbide and nitride forming element. V can combine with C and N in steel to form dispersed and fine MX carbonitrides to hinder the movement of dislocations. MX-type carbides belong to a face-centered cubic structure. During tempering, the MX phase is mainly precipitated at the boundaries of martensite laths and dislocation lines, and its size is small. During long-term aging or high-temperature creep, the MX phase has a low coarsening rate and little size change. It is finely dispersed in the matrix, which can effectively pin dislocations, hinder the recovery of dislocations and martensite laths, and improve the creep resistance of martensitic heat-resistant steel. However, too high a V content will increase the amount of δ ferrite, which is not conducive to the high-temperature creep performance of the material. Therefore, in the present invention, the V content is controlled at 0.2%~0.4%, and further, the V content is controlled at 0.25%~0.35%.
[0036] N (nitrogen) is an element that expands the austenite phase region. N can form VN-type MX phase with V in steel and is dispersed in the matrix. During long-term aging or high-temperature creep, the MX phase has a low coarsening rate and little size change. It is finely dispersed in the matrix and can effectively pin dislocations, hinder the recovery of dislocations and martensitic laths, and improve the creep resistance of martensitic heat-resistant steel. However, too high a N content will lead to the formation and coarsening of the Z phase in the creep stage, and the formed Z phase consumes the MX phase at the expense of the high-temperature creep performance of the steel. Therefore, in the present invention, the N content is controlled at 0.025% to 0.04%, and further, the N content is controlled at 0.03% to 0.035%.
[0037] The atomic radius of B (boron) is larger than that of C and N. When it is dissolved in the matrix, it will cause strong lattice distortion. In order to reduce the energy of the system, B will automatically concentrate at the interface and other defects in the matrix. 23 The vacancies on the interface between the C6 phase and the matrix block the Cr, Fe, C and other elements from absorbing into the M 23 The diffusion of C6 phase inhibits the 23The coarsening and growth of C6 phase improves the long-term creep performance of heat-resistant steel. However, when the B content is too high, B is easy to combine with N in the steel to form hard and brittle BN inclusions. On the one hand, the formation of this inclusion is extremely unfavorable to the toughness of the steel. On the other hand, the formation of BN inclusions consumes N elements and causes the loss of MX phase, which is unfavorable to the creep performance of the steel. Therefore, in the present invention, the B content is controlled at 0.001% to 0.003%, and further, the B content is controlled at 0.002% to 0.003%.
[0038] S (sulfur) easily reacts with alloying elements such as Cr, affecting the formation and stability of the passive film on the surface of stainless steel, thereby reducing its ability to resist chemical corrosion. Therefore, in the present invention, the S content is controlled to be below 0.02%.
[0039] P (phosphorus) has a strong solid solution strengthening effect on martensitic heat-resistant steel and can increase the hardness of steel. However, P will also significantly reduce the toughness of steel, especially low-temperature toughness. This may cause martensitic stainless steel to easily undergo brittle fracture at low temperatures or under impact loads. Therefore, in the present invention, the P content is controlled to be below 0.02%.
[0040] The martensitic heat-resistant steel according to the present invention increases the precipitation amount of the MX phase in the martensitic heat-resistant steel, suppresses the 23 The high-temperature creep resistance of martensitic heat-resistant steel is improved by coarsening and growing the C6 phase and inhibiting the formation of δ-ferrite, among which the most critical is the precipitation control of the MX phase. Based on the above description, it can be seen that there are many elements that affect the precipitation amount of the MX phase, including elements that directly participate in the formation of the MX phase, such as C, N, V, Mo and other elements, and other elements that may consume the elements that form the MX phase, such as B elements that consume N elements, or elements that promote or inhibit the formation of other phases (such as Z phases) that consume the MX phase during high-temperature service. Therefore, there is an interaction between the various components of the martensitic heat-resistant steel according to the present invention, and they need to cooperate with each other to achieve the improvement of high-temperature creep resistance.
[0041] Furthermore, it is particularly necessary to comprehensively control the contents of V, N, and B. The martensitic heat-resistant steel of the present invention includes a relatively low content of B, which can avoid the formation of hard and brittle BN inclusions in the martensite, while reducing the consumption of B on N, which is conducive to the formation of VN-type MX phase. However, due to the low B content, for M 23 The coarsening inhibition effect of C6 phase is weak. Therefore, an appropriate amount of Co is added to the heat-resistant steel to inhibit the growth of M 23 The coarsening and growth of the C6 phase improves the creep strength of the material.
[0042] In order to facilitate the understanding of the above heat treatment method, Figure 2A simplified structural diagram of a device for implementing a heat treatment method is shown, which can provide multiple functions such as heating, heat preservation, specific atmosphere, spraying cooling medium, workpiece rotation, vacuuming, etc.
[0043] like Figure 2 As shown, the apparatus generally includes a sealable furnace body 10 , a heating mechanism (not shown), a vacuum pump 20 , a nitrogen source 30 , a rotating mechanism 40 and a cooling mechanism 50 .
[0044] A heating chamber is provided in the furnace body 10, and a heating mechanism heats the heating chamber in a controllable temperature. The heating chamber is connected to a vacuum pump 20 and a nitrogen source 30 outside the furnace body 10 via pipelines, so that vacuuming and / or nitrogen filling operations can be performed in the heating chamber. A rotating mechanism 40 is installed on the side wall of the heating chamber, and the rotating mechanism 40 may include a driver, a rotating shaft and a clamp. The driver may be a motor and is arranged outside the heating chamber, and the rotating shaft is connected to the driver by transmission and inserted into the heating chamber. The clamp is fixed to the end of the rotating shaft and can clamp the workpiece W in the heating chamber. The cooling mechanism 50 may include a plurality of nozzles arranged on a plurality of side walls of the heating chamber and a cooling medium source connected to each nozzle via a pipeline.
[0045] Combine the following Figure 1 and Figure 2 To illustrate the heat treatment method according to some embodiments of the present invention. First, the chemical composition of the martensitic heat-resistant steel with high creep strength designed by the present invention is smelted and processed to obtain the martensitic heat-resistant steel with the chemical composition defined in the above embodiments. Among them, the vacuum induction VIM and vacuum consumable VAR processes can be used to smelt to obtain an ingot with qualified composition, and then the ingot is forged into shape. For example, the ingot is heated to 1100~1250℃ for forging, and the deformation of each pass is controlled at 30%~50%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 300~400℃, and kept warm for at least 5h for annealing. The workpiece is then polished and then heat-treated.
[0046] In step S1, the workpiece is fixed on Figure 2 In the processing equipment shown, the heating furnace is evacuated and filled with nitrogen, and then heated and kept warm. For example, the workpiece can be mounted on a fixture, and the vacuum pump 20 is turned on to evacuate the vacuum. After reaching the set vacuum degree, the vacuum pump 20 is turned off. The nitrogen source 30 is turned on and nitrogen is filled into the heating chamber. The heating mechanism is then turned on to heat the workpiece. In some embodiments, the heating temperature is 1000~1100℃, and the insulation time is 0.5~1h. By using this operation, on the one hand, the martensitic workpiece can be solid solution strengthened, and on the other hand, N infiltrates into the martensite, which is beneficial to supplement the N in the matrix so that the VN-type MX phase is formed, further improving the creep resistance of the material.
[0047] In step S2, the heating furnace is evacuated and the martensitic heat-resistant steel is rotated in the heating furnace. For example, when the set insulation time is reached, the nitrogen source 30 is turned off. The vacuum pump 20 is turned on to evacuate, and after the set vacuum degree is reached, the vacuum pump 20 is turned off. While evacuating, the rotating mechanism 40 can be turned on synchronously to increase the rotation speed of the workpiece to the set speed. The set rotation speed of the martensitic heat-resistant steel is 400~600rpm. In this operation, extracting the gas in the heating chamber can prevent the gas from hindering heat transfer during subsequent quenching, and the air film is not easy to gather under vacuum, thereby suppressing the generation of steam film in the later quenching process, so that the workpiece dissipates heat faster. The air film is not easy to adhere to the surface of the workpiece under high-speed rotation, which is beneficial to the heat dissipation of the workpiece.
[0048] In step S3, the heating is stopped, and a cooling medium is sprayed on the surface of the rotating martensitic heat-resistant steel to cool the martensitic heat-resistant steel to room temperature, and a pressure relief operation is performed. In some embodiments, the cooling medium can be a mixture of argon and quenching oil or a mixture of argon and liquid metal, the gas content of the mixture is controlled at 40%~70%, and the spray intensity is>5L / (min·m²). In this operation, a mixture of argon and quenching oil or argon and liquid metal is used as a cooling medium, and the cooling medium is evenly sprayed onto the surface of the workpiece through a nozzle, so that the entire workpiece can be evenly cooled and its organizational structure is more uniform. Moreover, quenching oil and liquid metal are easy to volatilize, which makes it easier to take away heat, which is conducive to rapid cooling. In some embodiments, the liquid metal is selected from at least one of gallium-based liquid metal and bismuth-based liquid metal. Room temperature refers to an ambient temperature of 20~30℃.
[0049] In step S4, the rotation and splashing operations are stopped, and the martensitic heat-resistant steel is tempered to obtain martensitic heat-resistant steel with improved creep strength. In some embodiments, the tempering treatment may include primary tempering and secondary tempering. Among them, the tempering temperature of the primary tempering can be set to 500~600℃, and the tempering time is 0.5~1.5h. The tempering operation can make the carbides and nitrogen-containing vanadium-molybdenum MX phases in the matrix fully precipitate, further improving the high temperature creep resistance. The tempering temperature of the secondary tempering can be set to 480~580℃, and the tempering time is 0.5~1.5h. This operation can reduce the residual austenite of the material and improve the mechanical properties of the martensitic heat-resistant steel.
[0050] The technical solution of the present invention will be further described below through specific examples. Unless otherwise specified, the raw materials, equipment, consumables, etc. used in the following examples can be obtained by conventional commercial means.
[0051] Example 1 The martensitic heat-resistant steel in this embodiment includes the following components in mass percentage: 0.07% C, 0.2% Si, 0.4% Mn, 1.5% Mo, 11% Cr, 1% Co, 2% Ni, 0.2% V, 0.025% N, 0.003% B, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0052] The ingot with the above composition is smelted by vacuum induction VIM and vacuum consumable VAR process, and then the ingot is forged. The ingot is heated to 1100℃ for forging, and the deformation of each pass is controlled at 30%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 300℃ and kept warm for 5 hours for annealing.
[0053] The martensitic heat-resistant steel obtained in this embodiment was tested, and the ferrite content was 12.75×10 -3 %, the retained austenite content is 1.5%, and the total plastic strain is 0.18% based on the national standard GB2038-80 experimental temperature of 450℃, stress of 465Mpa and time of 100h.
[0054] Example 2 The martensitic heat-resistant steel in this embodiment includes the following components in mass percentage: 0.11% C, 0.18% Si, 0.7% Mn, 1.7% Mo, 11.8% Cr, 2% Co, 2.5% Ni, 0.35% V, 0.032% N, 0.002% B, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0055] The ingot with the above composition is smelted by vacuum induction VIM and vacuum consumable VAR process, and then the ingot is forged. The ingot is heated to 1150℃ for forging, and the deformation of each pass is controlled at 35%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 350℃ and kept warm for 6 hours for annealing.
[0056] The martensitic heat-resistant steel obtained in this embodiment was tested, and the ferrite content was 10.15×10 -3 %, the retained austenite content is 1.2%, and the total plastic strain is 0.15% based on the national standard GB2038-80 experimental temperature of 450℃, stress of 465Mpa and time of 100h.
[0057] Example 3 The martensitic heat-resistant steel in this embodiment includes the following components in mass percentage: 0.14% C, 0.12% Si, 0.9% Mn, 2.0% Mo, 12.6% Cr, 3% Co, 3% Ni, 0.4% V, 0.04% N, 0.001% B, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0058] The ingot with the above composition is smelted by vacuum induction VIM and vacuum consumable VAR process, and then the ingot is forged. The ingot is heated to 1250℃ for forging, and the deformation of each pass is controlled at 50%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 400℃ and kept at this temperature for 7 hours for annealing.
[0059] The martensitic heat-resistant steel obtained in this embodiment was tested, and the ferrite content was 11.25×10 -3 %, the retained austenite content is 0.9%, and the total plastic strain is 0.17% based on the national standard GB2038-80 experimental temperature of 450℃, stress of 465Mpa and time of 100h.
[0060] Example 4 This embodiment heat treats the martensitic heat-resistant steel workpiece prepared in Example 2. Specifically, the following steps are included: placing the martensitic heat-resistant steel workpiece in a heating furnace filled with nitrogen, heating it to 1000°C, and keeping it warm for 1 hour; evacuating the heating furnace, and rotating the martensitic heat-resistant steel in the heating furnace until the speed is 400rpm; stopping heating, spraying a cooling medium on the surface of the rotating martensitic heat-resistant steel, cooling the martensitic heat-resistant steel to room temperature, and performing a pressure relief operation, wherein the cooling medium is a mixture of argon and quenching oil, the gas content of the mixture is controlled at 40%, and the spray intensity is 8L / (min·m²); stopping rotation and spraying, tempering the martensitic heat-resistant steel, first keeping it warm at 500°C for 1.5 hours, air cooling the workpiece to room temperature, then heating it to 480°C and keeping it warm for 1.5 hours, cooling it to room temperature, and obtaining a martensitic heat-resistant steel with improved creep strength.
[0061] The martensitic heat-resistant steel obtained in this example was tested, and the ferrite content was 3.25×10 -3 %, the retained austenite content is 0.6%, and the total plastic strain is 0.13% based on the national standard GB2038-80 experimental temperature of 450℃, stress of 465Mpa and time of 100h.
[0062] Example 5 This embodiment heat treats the martensitic heat-resistant steel workpiece prepared in Example 2. Specifically, the following steps are included: placing the martensitic heat-resistant steel workpiece in a heating furnace filled with nitrogen, heating it to 1050°C, and keeping it warm for 45 minutes; evacuating the heating furnace, and rotating the martensitic heat-resistant steel in the heating furnace until the speed is 500rpm; stopping heating, spraying a cooling medium on the surface of the rotating martensitic heat-resistant steel, cooling the martensitic heat-resistant steel to room temperature, and performing a pressure relief operation, wherein the cooling medium is a mixture of argon and gallium-based liquid metal, the gas content of the mixture is controlled at 60%, and the spray intensity is 5L / (min·m²); stopping rotation and spraying, tempering the martensitic heat-resistant steel, first keeping it warm at 550°C for 45 minutes, air cooling the workpiece to room temperature, then heating it to 530°C and keeping it warm for 45 minutes, cooling it to room temperature, and obtaining a martensitic heat-resistant steel with improved creep strength.
[0063] The martensitic heat-resistant steel obtained in this embodiment was tested, and the ferrite content was 2.75×10 -3 %, the retained austenite content is 0.5%, and the total plastic strain is 0.11% based on the national standard GB2038-80 experimental temperature of 450℃, stress of 465Mpa and time of 100h.
[0064] Example 6 This embodiment heat treats the martensitic heat-resistant steel workpiece prepared in Example 2. Specifically, the following steps are included: placing the martensitic heat-resistant steel workpiece in a heating furnace filled with nitrogen, heating it to 1100°C, and keeping it warm for 0.5h; evacuating the heating furnace, and rotating the martensitic heat-resistant steel in the heating furnace until the speed is 600rpm; stopping heating, spraying a cooling medium on the surface of the rotating martensitic heat-resistant steel, cooling the martensitic heat-resistant steel to room temperature, and performing a pressure relief operation, wherein the cooling medium is a mixture of argon and bismuth-based liquid metal, the gas content of the mixture is controlled at 70%, and the spray intensity is 5.2L / (min·m²); stopping rotation and spraying, tempering the martensitic heat-resistant steel, first keeping it warm at 600°C for 0.5h, air cooling the workpiece to room temperature, then heating it to 580°C and keeping it warm for 0.5h, cooling it to room temperature, and obtaining a martensitic heat-resistant steel with improved creep strength.
[0065] The martensitic heat-resistant steel obtained in this example was tested, and the ferrite content was 2.95×10 -3 %, the retained austenite content is 0.6%, and the total plastic strain is 0.14% based on the national standard GB2038-80 experimental temperature of 450℃, stress of 465Mpa and time of 100h.
[0066] Comparative Example 1 The martensitic heat-resistant steel in this comparative example includes the following components in mass percentage: 0.11% C, 0.18% Si, 0.7% Mn, 1.7% Mo, 11.8% Cr, 2% Co, 2.5% Ni, 0.35% V, 0.032% N, 0.006% B, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0067] The ingot with the above composition is smelted by vacuum induction VIM and vacuum consumable VAR process, and then the ingot is forged. The ingot is heated to 1150℃ for forging, and the deformation of each pass is controlled at 35%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 350℃ and kept warm for 6 hours for annealing.
[0068] The martensitic heat-resistant steel obtained in this comparative example was tested, and the ferrite content was 15.15×10 -3 %, the retained austenite content is 3.2%, and the total plastic strain is 0.85% under the national standard GB2038-80 test temperature of 450℃, stress of 465Mpa, and time of 100h. In this comparative example, due to the high B content, it is easy to combine with N, consuming the N in the matrix, resulting in less VN type MX phase and insufficient high temperature creep resistance of the steel.
[0069] Comparative Example 2 The martensitic heat-resistant steel in this comparative example includes the following components in mass percentage: 0.11% C, 0.18% Si, 0.7% Mn, 1.7% Mo, 11.8% Cr, 2% Co, 2.5% Ni, 0.35% V, 0.012% N, 0.002% B, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0070] The ingot with the above composition is smelted by vacuum induction VIM and vacuum consumable VAR process, and then the ingot is forged. The ingot is heated to 1150℃ for forging, and the deformation of each pass is controlled at 35%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 350℃ and kept warm for 6 hours for annealing.
[0071] The martensitic heat-resistant steel obtained in this comparative example was tested, and the ferrite content was 13.15×10 -3 %, the retained austenite content is 2.8%, and the total plastic strain is 0.55% under the experimental temperature of 450℃, stress of 465Mpa, and time of 100h based on the national standard GB2038-80. In this comparative example, due to the low N content, the amount of VN type MX phase is small, and the high temperature creep resistance of the steel is insufficient.
[0072] Comparative Example 3 The martensitic heat-resistant steel in this comparative example includes the following components in mass percentage: 0.11% C, 0.18% Si, 0.7% Mn, 0.2% Mo, 11.8% Cr, 2% Co, 2.5% Ni, 0.1% V, 0.032% N, 0.002% B, S≤0.02%, P≤0.02%, and the rest are Fe and unavoidable impurities.
[0073] The ingot with the above composition is smelted by vacuum induction VIM and vacuum consumable VAR process, and then the ingot is forged. The ingot is heated to 1150℃ for forging, and the deformation of each pass is controlled at 35%. After forging, the formed workpiece is air-cooled to room temperature, and then heated to 350℃ and kept warm for 6 hours for annealing.
[0074] The martensitic heat-resistant steel obtained in this comparative example was tested, and the ferrite content was 12.15×10 -3 %, the retained austenite content is 3.5%, and the total plastic strain is 0.95% under the experimental temperature of 450℃, stress of 465Mpa and time of 100h based on the national standard GB2038-80. In this comparative example, due to the low content of Mo and V, the amount of MX phase is small, and the high temperature creep resistance of the steel is insufficient.
[0075] Comparative Example 4 This comparative example adopts the martensitic heat-resistant steel workpiece prepared in Example 2 to perform heat treatment on the workpiece. Specifically, the following steps are included: placing the martensitic heat-resistant steel workpiece in a common heating furnace, heating it to 1050°C, and keeping it warm for 45 minutes; rotating the martensitic heat-resistant steel in the heating furnace until the rotation speed is 500rpm; stopping heating, spraying a cooling medium on the surface of the rotating martensitic heat-resistant steel, and cooling the martensitic heat-resistant steel to room temperature, wherein the cooling medium is a mixture of argon and gallium-based liquid metal, the gas content of the mixture is controlled at 60%, and the spray intensity is 5L / (min·m²); stopping rotation and spraying, tempering the martensitic heat-resistant steel, first keeping it warm at 550°C for 45 minutes, air cooling the workpiece to room temperature, then heating it to 530°C and keeping it warm for 45 minutes, cooling it to room temperature, and obtaining the treated martensitic heat-resistant steel.
[0076] The martensitic heat-resistant steel obtained in this comparative example was tested, and the ferrite content was 3.5×10 -3%, the retained austenite content is 0.8%, and the total plastic strain is 0.22% under the national standard GB2038-80 test temperature of 450℃, stress of 465Mpa, and time of 100h. Due to the lack of nitrogen filling, the nitriding link is missing, which leads to a small amount of VN-type MX phase in the creep-resistant nano-precipitation phase. At the same time, due to the lack of vacuum, the heat dissipation capacity is weak during the cooling process, and the content of ferrite and retained austenite is slightly increased, resulting in poor creep resistance.
[0077] Comparative Example 5 This comparative example adopts the martensitic heat-resistant steel workpiece prepared in Example 2 to perform heat treatment on the workpiece. Specifically, the following steps are included: placing the martensitic heat-resistant steel workpiece into a heating furnace filled with nitrogen, heating it to 1050°C, and keeping it warm for 45 minutes; evacuating the heating furnace, spraying a cooling medium on the surface of the martensitic heat-resistant steel, cooling the martensitic heat-resistant steel to room temperature, and performing a pressure relief operation, wherein the cooling medium is a mixture of argon and gallium-based liquid metal, the gas content of the mixture is controlled at 60%, and the spray intensity is 5L / (min·m²); stopping the spraying, tempering the martensitic heat-resistant steel, first keeping it warm at 550°C for 45 minutes, air cooling the workpiece to room temperature, then heating it to 530°C and keeping it warm for 45 minutes, cooling it to room temperature, and obtaining the treated martensitic heat-resistant steel The martensitic heat-resistant steel obtained in this comparative example was tested, and the ferrite content was 8.34×10 -3 %, the retained austenite content is 3.3%, and the total plastic strain is 0.33% under the national standard GB2038-80 test temperature of 450℃, stress of 465Mpa, and time of 100h. Due to the lack of rotation, the heat dissipation capacity is greatly reduced during the cooling process, and the ferrite and retained austenite content are significantly increased, resulting in a significant increase in creep.
[0078] Comparative Example 6 This comparative example adopts the martensitic heat-resistant steel workpiece prepared in Example 2 to perform heat treatment on the workpiece. Specifically, the following steps are included: placing the martensitic heat-resistant steel workpiece in a heating furnace filled with nitrogen, heating it to 1050°C, and keeping it warm for 45 minutes; evacuating the heating furnace, and rotating the martensitic heat-resistant steel in the heating furnace until the speed is 500rpm; stopping heating, spraying a cooling medium on the surface of the rotating martensitic heat-resistant steel, cooling the martensitic heat-resistant steel to room temperature, and performing a pressure relief operation, wherein the cooling medium is water, and the spraying intensity is 5L / (min·m²); stopping rotation and spraying, tempering the martensitic heat-resistant steel, first keeping it warm at 550°C for 45 minutes, air cooling the workpiece to room temperature, then heating it to 530°C and keeping it warm for 45 minutes, cooling it to room temperature, and obtaining the treated martensitic heat-resistant steel.
[0079] The martensitic heat-resistant steel obtained in this comparative example was tested, and the ferrite content was 4.12×10-3 %, the retained austenite content is 1.6%, and the total plastic strain is 0.18% under the national standard GB2038-80 test temperature of 450℃, stress of 465Mpa, and time of 100h. Due to the lack of a cooling medium with good cooling capacity, the heat dissipation capacity is reduced during the cooling process, and the content of ferrite and retained austenite is increased, resulting in an increase in creep.
[0080] Figure 3 The metallographic photograph of the martensitic heat-resistant steel prepared by the method of Example 5 is shown. Figure 4 The metallographic photograph of the martensitic heat-resistant steel prepared by the method of comparative example 4 is shown. By comparing the two, it can be seen that Figure 4 The bright white ferrite content in the matrix phase is relatively high. Since ferrite is a soft phase, the material is easily deformed under stress, which will reduce the high temperature creep resistance of the steel. Figure 3 The bright white ferrite in the matrix is significantly reduced, and the total plastic strain of the steel in Example 5 is significantly lower than that in Comparative Example 4, which indicates that the creep resistance of the heat-resistant steel treated by the method of the present invention is improved.
[0081] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention is limited to these examples; under the idea of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A heat treatment method for martensitic heat-resistant steel, characterized in that: The following steps are involved: Step S1: placing the martensitic heat-resistant steel into a heating furnace filled with nitrogen for heating and heat preservation; Step S2: evacuating the heating furnace and rotating the martensitic heat-resistant steel in the heating furnace; Step S3: stopping the heating, spraying a cooling medium on the surface of the rotating martensitic heat-resistant steel to cool the martensitic heat-resistant steel to room temperature, and performing a pressure relief operation; Step S4: stopping the rotation and the splashing, and subjecting the martensitic heat-resistant steel to tempering to obtain martensitic heat-resistant steel with improved creep strength.
2. The heat treatment method according to claim 1, characterized in that The martensitic heat-resistant steel includes the following components in mass percentage: C: 0.07%~0.14%, Si≤0.2%, Mn: 0.4%~0.9%, Mo: 1.5%~2.0%, Cr: 11%~12.6%, Co: 1%~3%, Ni: 2%~3%, V: 0.2%~0.4%, N: 0.025%~0.04%, B: 0.001%~0.003%, S≤0.02%, P≤0.02%, and the rest is Fe and unavoidable impurities.
3. The heat treatment method according to claim 1, characterized in that The heating temperature in step S1 is 1000-1100° C., and the holding time is 0.5-1 h.
4. The heat treatment method according to claim 1, characterized in that: In step S2, the martensitic heat-resistant steel is rotated to a rotation speed of 400-600 rpm.
5. The heat treatment method according to claim 1, characterized in that: The cooling medium in step S3 is a mixture of argon and quenching oil or argon and liquid metal, the gas content of the mixture is controlled at 40% to 70%, and the injection intensity is greater than 5L / (min·m²).
6. The heat treatment method according to claim 5, characterized in that: The liquid metal is selected from at least one of gallium-based liquid metal and bismuth-based liquid metal.
7. The heat treatment method according to claim 1, characterized in that: The tempering treatment includes primary tempering and secondary tempering.
8. The heat treatment method according to claim 7, characterized in that: The tempering temperature of the primary tempering is 500-600° C., and the tempering time is 0.5-1.5 h.
9. The heat treatment method according to claim 7, characterized in that: The secondary tempering has a tempering temperature of 480-580° C. and a tempering time of 0.5-1.5 h.
10. A martensitic heat-resistant steel with high creep strength, characterized in that: The martensitic heat-resistant steel with high creep strength is prepared by the heat treatment method according to any one of claims 1 to 9.