Method for evaluating formability of reversible crosslinking self-healing 3D printing ink
By constructing reversible cross-linked self-healing ink using materials such as gelatin nanoparticles, silk fibroin nanoparticles, and nanoclay, and combining rheological testing and printing scaffold parameters, the problem of insufficient self-healing properties of water-based gels was solved, and the effective evaluation and optimization of 3D printing formability was achieved.
Patent Information
- Application Number
- CN202410974565.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing water-based gel 3D printing inks have poor self-healing properties and lack effective reversible cross-linking mechanisms, resulting in insufficient self-repair capabilities. This leads to imperfect evaluation methods for printability and makes it difficult to accurately assess the printability of reversibly cross-linked self-healing inks.
A reversible cross-linked self-healing ink was constructed using materials such as gelatin nanoparticles, silk fibroin nanoparticles, and nanoclay. A new method for evaluating formability was established by testing rheological properties and parameters such as the roundness and area change rate of the printing template, and the impact of self-healing and viscoelasticity on printing was quantified.
This provides a widely applicable method for evaluating printability, which can accurately assess the printing performance of reversible crosslinked self-healing inks, guide the design of bio-inks and optimize rheological parameters, and improve printing accuracy and structural stability.
Smart Images

Figure CN118914522A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of 3D printing material evaluation methods, and specifically relates to a method for evaluating the formability of reversibly cross-linked self-healing 3D printing ink. Background Art
[0002] Extrusion 3D printing is a technology that melts or softens materials (such as plastics, metals, biogels, etc.), extrudes them layer by layer through a nozzle, and stacks them into shape. With its flexibility and diversity, extrusion 3D printing technology plays an important role in different industries and continues to promote technological innovation and application expansion. Extrusion 3D printing technology is widely used in manufacturing, construction, food processing, and biomedical engineering. In the biomedical field, extrusion 3D printing technology is widely used due to its simple operation, wide range of available materials, and easy cell printing. It can be used to print scaffolds with specific porosity and mechanical properties, which can be used in tissue engineering and drug testing.
[0003] The precision of extrusion 3D printing is jointly determined by equipment precision, extrusion parameters, material formability and nozzle design. The formability of the material is mainly determined by its rheological properties. The ideal bio-ink should have good shear thinning behavior and appropriate yield stress. Shear thinning behavior helps to reduce the shear force on cells during printing, thereby protecting cell activity; yield stress helps the printed structure maintain its shape and resist deformation caused by gravity or surface tension. In addition, the self-healing property of ink is particularly important for printing scaffolds with high shape fidelity. Self-healing hydrogels can restore their binding force and their initial structure, properties and functions after extrusion. Combined with the shear thinning properties, it can not only print cells safely, but also ensure the shape stability of the printed structure. However, the current research on the self-healing property of ink mainly tests the modulus recovery after high strain amplitude or high oscillation frequency, and there is no systematic self-healing evaluation method. The evaluation of the impact of self-healing on 3D printing formability also needs to be supplemented.
[0004] At present, the ink used for extrusion 3D printing is mainly water-based gel, which can be composed of polymers (such as PluronicF127), polysaccharides (such as chitosan and cellulose) and proteins (such as silk and gelatin), inorganic materials (such as hydroxyapatite, tricalcium phosphate, graphene, glass), etc. Most water-based gels have poor self-healing properties. The main reasons are as follows: First, there is a lack of reversible interactions, such as hydrogen bonds, hydrophobic interactions, etc., which account for a small proportion in hydrogels. At the same time, there is a lack of dynamically reversible chemical bonds, such as acylhydrazone bonds, imine bonds, disulfide bonds, etc.; second, the irreversibility of chemical cross-linking. Some hydrogels form a stable network structure through chemical cross-linking, but these cross-linking bonds (such as covalent bonds) are difficult to re-form after destruction, which limits the self-healing ability of hydrogels; third, a single cross-linking mechanism may limit the self-healing property of inks. A single cross-linking mechanism may not provide sufficient self-healing ability. In contrast, multiple action mechanisms combining physical and chemical cross-linking can improve self-healing properties. Based on the problem of low self-healing rate caused by lack of reversible crosslinking in the above hydrogel ink, the specific surface area can be increased, such as colloidal gels constructed based on nanoparticles; a large number of reversible interactions are introduced, such as hydrophilic polymers or protein surface interactions to produce abundant hydrogen bonds or van der Waals forces, etc. to construct 3D printing inks with reversible crosslinking self-healing properties. Due to the rich reversible crosslinking types and dynamically reorganized mechanical entanglements inside this ink, it exhibits different rheological properties, such as different viscoelasticity, strain rate dependence, flow characteristics, infinite chain flow relaxation time and finite relaxation time, as well as the self-healing properties of macroscopic modulus and viscosity exhibited by the above rheological properties. Due to the lack of evaluation methods for the effect of self-healing on 3D printing formability, the impact of self-healing on printing is still unclear.
[0005] There are two main evaluation methods currently applicable to extrusion 3D printing. One is roundness (Pr). Ideally, the fusion of ink should not occur on an orthogonal path. Under the influence of gravity and the low mechanical strength of the ink, fusion is inevitable, so Pr is usually less than 1. If the ink is difficult to extrude, when Pr exceeds 1, it may cause jagged filaments. The second is the area change rate (Ar), which is the ratio of the actual printing gap to the ideal gap. The printing gap is usually smaller than the theoretical area without deformation, extrusion expansion, fusion, etc. However, when evaluating the formability of high-strength materials, Ar and Pr may not reflect the significant difference between the two inks in low-strength materials. In addition, self-healing inks based on reversible cross-linking usually have complex rheological properties, and different inks may have similar formability. It is difficult for Ar and Pr to accurately evaluate reversibly cross-linked self-healing inks. This is because Ar is more significantly affected by ink viscosity, while Pr is more significantly affected by modulus. In essence, Pr is suitable for the evaluation of the formability of medium and high-strength inks, while Ar is more obvious for the formability of medium and low-strength inks.
[0006] In summary, although there is a consensus on the effect of ink strength on printing, the effect of ink self-healing on 3D printing, especially on formability, is still unclear. This has prompted researchers engaged in additive manufacturing to study the quantitative method of self-healing and its effect on formability. At present, most hydrogel inks have poor self-healing properties and insufficient viscoelastic controllability, making them difficult to use in the construction of inks with various rheological properties. Based on this, nanoscale particles are prepared based on hydrogel components. The larger specific surface area of nanoparticles increases surface interactions, and the shear thinning properties required for extrusion printing can be easily achieved by the movement and repetition of the particle structure under high amplitude or shear. In addition, reversibly cross-linked ink construction can be achieved by using natural polymers such as gelatin and silk, or hydrophilic inorganic substances such as hydroxyapatite and nanoclay, which have rich reversible interaction groups on the surface. This reversible interaction promotes the reorganization of the colloidal network after the shear action is removed, thereby achieving self-healing of the ink, which is an ideal material for rheological research and 3D printing. With the help of the rich surface interactions and diverse self-assembly structures of reversibly cross-linked self-healing inks, the viscoelasticity of the ink can be controlled, which can be used to study the rationality of different printing evaluation methods. Analyzing the disadvantages of existing evaluation methods and constructing new widely applicable moldability evaluation parameters are of great significance for guiding the construction and extrusion parameters of 3D printing inks. Summary of the invention
[0007] In view of this, the purpose of the present invention is to provide a method for evaluating the formability of reversibly cross-linked self-healing 3D printing ink. The present invention is based on the quantitative characterization of the self-healing property of particle cross-linked self-healing ink, analyzes the effect of viscoelasticity on the formability of extrusion 3D printing, and constructs a method for evaluating the formability of ink with wide applicability.
[0008] The object of the present invention is achieved by the following methods:
[0009] The present invention provides a method for evaluating the formability of a reversibly cross-linked self-healing 3D printing ink, comprising the following steps:
[0010] (1) preparing reversibly cross-linked self-healing ink: mixing the reversibly cross-linked self-healing material with deionized water to prepare colloidal inks with different volume fractions;
[0011] (2) Testing the rheological properties of the reversibly cross-linked self-healing ink: Take 0.35 ml of the reversibly cross-linked self-healing ink and apply it to the bottom plate of the rheometer. Then select a 20 mm parallel plate for testing, set the working distance to 1 mm, and set the axial force to about 0.1 N.
[0012] (3) Using reversibly cross-linked self-healing ink to print single-layer and eight-layer stents, wait for 20 to 60 minutes to ensure that the stent relaxation is completely completed, and calculate the roundness Pr of the orthogonal unit area of the printed stent. The calculation method is Pr = L 2 / 16A, where L is the perimeter of the area and A is the area of the area; calculate the area change rate Ar of the unit area orthogonal to the printed stent, and the calculation method is Ar=A / A0, where A is the actual detection area area and A0 is the ideal area when the stent does not fuse or collapse; assign equivalent values to Ar and Pr, and calculate the formability index Fid, and the calculation method is:
[0013]
[0014] Where D P and D A are the standard deviations of Pr and Ar, U P and U A are the average values of Pr and Ar respectively, and e is a natural constant.
[0015] (4) The storage modulus, complex viscosity, modulus self-repair rate and viscosity self-repair rate measured by the rheometer are taken as variables, and their relationship with Ar, Pr and Fid is fitted.
[0016] Based on the above technical solution, further, the reversibly cross-linked self-healing material described in step (1) includes gelatin nanoparticles, silk nanoparticles and nanoclay.
[0017] Based on the above technical solution, further, the volume fractions described in step (1) are 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45 and 0.5 respectively.
[0018] Based on the above technical solution, further, the test described in step (2) mainly includes two consecutive step tests, which need to be tested after sample preparation respectively:
[0019] A. At a fixed frequency of 1 Hz / s, continuous tests of time scan 1, amplitude scan 1 and time scan 2 are performed, where the test time of time scan 1 and time scan 2 is 60 minutes, and the strain is controlled to 0.1%; the time of amplitude scan 1 is determined by the actual test of the rheometer, and it is only necessary to control the strain to change nonlinearly from 0.1% to 100%; the three tests are performed in sequence, and the average storage modulus G of time scan 1 and time scan 2 is calculated from the last 60s of time scan 1 and the first 60s of time scan 2 ’ 1 and G ’ 2. The modulus self-repair rate is G ’ 2 / G ’ 1;
[0020] B. At a fixed frequency of 1 Hz / s, perform continuous tests of time scan 3, peak hold 1 and time scan 4, where the test time of time scan 3 and time scan 4 is 60 minutes, and the strain rate is controlled to 0.1s -1 ; The peak value is maintained for 60 seconds, and the strain rate is controlled at 30 seconds -1 The three tests were performed in sequence, and the average composite viscosity V of time scan 3 and time scan 4 was calculated from the last 60s of time scan 3 and the first 60s of time scan 4. ’ 1 and V ’ 2. The viscosity self-repair rate is G ’ 2 / G ’ 1.
[0021] Based on the above technical solution, further, the outer side of the bracket described in step (3) is a cylindrical structure with a diameter of 20 mm, and the inner side is a rectangular structure formed by six equally spaced paths arranged orthogonally in the horizontal and vertical directions, and the length of each path is 14.14 mm; the bracket is composed of 8 layers of the above structure, and the thickness of each layer is 0.4 mm.
[0022] Based on the above technical solution, further, in step (3), the value range of the formability index Fid is 0-1, and the larger the value, the better the formability.
[0023] Based on the above technical solution, further, the fitting in step (4) uses the fourth-order polynomial fitting in Origin.
[0024] The beneficial effects of the present invention compared with the prior art are as follows:
[0025] This paper demonstrates the feasibility of Ar and Pr of gelatin nanoparticles, silk nanoparticles and nanoclay materials, establishes a new parameter to quantify the fidelity (Fid), which is suitable for the evaluation of reversibly cross-linked self-healing gel formability, and by comparing the fidelity of different colloidal gels, the relationship between good and bad printing performance and rheological properties of the materials is obtained, thereby guiding the rheological parameters of bio-ink design. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0027] Figure 1 8-layer orthogonal scaffolds printed with gelatin, nanoclay, and silk inks;
[0028] Figure 2 The rheological test results of gelatin (frequency sweep, shear thinning, modulus self-repair and viscosity self-repair);
[0029] Figure 3The rheological test results of silk fibroin (frequency sweep, shear thinning, modulus self-repairing and viscosity self-repairing);
[0030] Figure 4 The rheological test results of nanoclay (frequency sweep, shear thinning, modulus self-repairing and viscosity self-repairing);
[0031] Figure 5 The local fusion of gelatin, silk and nanoclay inks with different volume fractions after printing;
[0032] Figure 6 The significance analysis of the three evaluation parameters Ar, Pr and Fid for the colloidal inks with different volume fractions and components, where a is the Ar evaluation parameter, b is the Pr evaluation parameter, and c is the Fid evaluation parameter. DETAILED DESCRIPTION
[0033] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0034] Example 1
[0035] In this example, the self-healing property and viscoelasticity of colloidal particles are controlled by different surface interactions, and a quantitative analysis is performed based on this. Subsequently, a 3D printed stent with an eight-layer structure and uniform orthogonal distribution is constructed. After printing with different self-healing inks, a visual analysis of stent collapse and fusion is performed, and the relationship between the existing evaluation parameters Pr and Ar and the ink self-healing type and viscoelasticity is calculated. It is found that the existing evaluation parameters are only applicable within a limited range of rheological characteristics. Therefore, we combine the two evaluation parameters to construct an evaluation method with wider applicability.
[0036] Extrusion 3D printing is a technology widely used in tissue engineering and biomedical fields. It constructs three-dimensional complex structures by precisely controlling the extrusion and assembly of biological inks. The following is a detailed description of the ink preparation and operation steps for extrusion 3D printing:
[0037] Preparation of bio-ink: Bio-ink is a key material in 3D printing and needs to have appropriate rheological properties to ensure a smooth printing process.
[0038] The surface of gelatin nanoparticles is rich in amino and carboxyl groups, making them more hydrophilic and easier to swell. The thickening of the hydration layer increases the volume fraction and inter-particle chain entanglement, further fixing the colloidal structure. Therefore, the colloidal gel formed by gelatin nanoparticles has high strength, low volume and good self-healing properties. Soft gelatin nanoparticles can be deformed under injection, which makes injection easier.
[0039] Nanoclay is a flaky montmorillonite. After absorbing water, the positively charged edges and negatively charged surfaces combine through electrostatic interactions, thus forming a "house of cards" structure and gel. This structure can be modified after injection and exhibits self-healing properties.
[0040] Silk nanoparticles are less hydrophilic than gelatin nanoparticles and nanoclays, which are affected by β-folding to form nanoparticles. This results in almost no free chains on the surface, so the stiffness is higher than that of gelatin nanoparticles. The gelation of silk nanoparticles is mainly achieved by weak van der Waals forces, hydrophobic interactions and dense stacking. Due to the different compositions and interactions of the above three materials, they form different rheological properties. It is applicable to compare the fidelity of various colloidal materials.
[0041] Gelatin nanoparticles (approximately 100 nanometers in a dry state) were synthesized according to existing studies (Hathout RM, Metwally A A. Gelatin nanoparticles [J]. Pharmaceutical Nanotechnology: Basic Protocols, 2019: 71-78.). 10g of gelatin was dissolved in 200ml of deionized water, kept at a constant temperature of 50 degrees Celsius, and the magnetic stirring speed was 400rpm. The reaction lasted for 30 minutes until the gelatin was completely dissolved. Acetone was then slowly added using a peristaltic pump to form an emulsion at a flow rate of 20ml / min and a total amount of 800ml. When the solution was emulsified, glutaraldehyde as a cross-linking agent was added to fix the shape of the gelatin nanoparticles, and the volume of glutaraldehyde added was 1ml. After 8 hours of reaction, 50ml of 5M glycine solution was added to consume unreacted glutaraldehyde, and the reaction was carried out for 2 hours. The fixed nanoparticles were washed with ethanol, ethanol-water mixture and water.
[0042] Silk nanoparticles (approximately 115 nm in dry state) were provided by Huanova Biotech (Shenzhen, China). Ethanol was added dropwise to the silk solution until it was fully emulsified. Then, the nanoparticles were washed three times with ethanol and water.
[0043] Laponite XLS(Lap,SiO2:MgO:Li2O:Na2O:P2O5=54.5:26:0.8:5.6:4.1)
[0044] It was purchased from BYK (Germany).
[0045] At room temperature, gelatin nanoparticles, silk nanoparticles and Laponite XLS nanoparticles were dissolved in 5mM HEPES solution to form a 5mg / mL suspension, and the pH was adjusted to 7±0.1. After the suspension was stabilized for 60 seconds, the diameter and surface zeta potential of the nanoparticles were measured using dynamic light scattering (DLS), with 60 data points taken for each measurement and 1 second interval between each measurement. A total of three measurements were performed and the results were averaged.
[0046] Table 1 Surface zeta potential and hydrated average particle size of gelatin, nanoclay and silk nanoparticles
[0047]
[0048] Preparation of reversibly cross-linked self-healing ink: reversibly cross-linked self-healing materials (gelatin nanoparticles, silk nanoparticles and nanoclay) were mixed with deionized water to prepare colloidal inks with different volume fractions, which were 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45 and 0.5 respectively;
[0049] Rheological testing: The rheological properties of different colloidal systems were measured by a DHR-2 rheometer (DHR, TA Instruments) at room temperature with 20 mm parallel plates and an operating gap of 1000 μm. This example was subjected to strain-controlled testing: the frequency and strain were set to 1 Hz / s and 0.1%. The viscoelasticity was measured by frequency sweeping from 100 Hz / s to 0.1 Hz / s. The self-healing ability of the modulus was measured by amplitude sweeping, applying a slight strain (0.1%) within 20 seconds. After the material properties stabilized, a strain (100%) sufficient to destroy the material structure was applied for 20 seconds, and then quickly recovered to a strain of 0.1%. The self-healing ability of the viscosity was measured by peak holding, with the same period as the modulus. The shear rates were set to 0.1 and 30s, respectively. -1 The modulus and viscosity were averaged over the first five seconds of each cycle. The flow scan measured the shear thinning behavior of the three materials at shear rates ranging from 0.1 to 30 s -1 changes, and then record the change in viscosity.
[0050] The ink was loaded into a 10 ml syringe with a 260 μm needle. During printing, the extrusion speed was 5 mm / s and the extrusion volume was controlled to 60%, 80% and 100% of the volume required to fill the needle. The height of the first layer was 0.7 mm and the height of the second layer was 0.22 mm. The double-layer orthogonal scaffold with a diameter of 20 mm × 20 mm was printed using eight-row paths. Each sample was printed three times to evaluate its printability ( Figure 5 ), Figure 5 , 1-1 represents the first single-layer scaffold printed when the volume fraction is 10%, 2-1 represents the first single-layer scaffold printed when the volume fraction is 15%, 3-1 represents the first single-layer scaffold printed when the volume fraction is 20%, and 4-1 represents the first single-layer scaffold printed when the volume fraction is 25%.
[0051] The ink samples were printed using a 400 micron needle, which was used to calculate the collapse rate. The extrusion speed was 5 mm / s and the needle filling ratio was 80%. The first layer was printed at a height of 0.95 mm, and each subsequent layer was printed at a height of 0.4 mm, forming a cylinder with a diameter of 20 mm, with a total of eight layers; six rows of paths formed the orthogonal structure inside. The scaffolds were photographed 30 minutes after printing.
[0052] The printed brackets were sampled using an equidistant sampling method, with eight grid spaces selected for each bracket, and 24 points of each sample were photographed using a 4x microscope. MATLAB captured the spatial images taken by the optical microscope. Using contrast differences, the boundaries were automatically found, and the boundary length and spacing area were exported in the form of pixels, which were then converted using the fixed resolution and scale of the optical microscope.
[0053] Pr (roundness) is calculated by Pr = L 2 / 16A, where L is the perimeter and A is the area; Ar (area collapse ratio) is calculated by Ar=A / A0, where A0 is the area when the filament does not expand or collapse in an ideal situation. Based on the combination of Ar and Pr, and taking into account the instability of the results at lower concentrations, which leads to a larger standard deviation, a new printability evaluation algorithm Fid (fidelity) was established:
[0054]
[0055] Among them, D P and D A are the standard deviations of Pr and Ar, U P and U A are the average values of Pr and Ar respectively, and e is a natural constant. The value range of the formability index Fid is 0-1, and the larger the value, the better the formability.
[0056] The storage modulus, complex viscosity, modulus self-repair rate and viscosity self-repair rate measured by the rheometer were used as variables to fit their relationship with Ar, Pr and Fid. The fitting was done using the fourth-order polynomial fitting in Origin, and the formula is y=a0+a1x+a2x 2 +a3x 3 +a4x 4 , coefficient of determination R 2 The calculation of is based on the ratio of the regression sum of squares (SSR) to the total sum of squares (SST), i.e., R 2 =SSR / SST. Where SSR is the variance explained by the regression model and SST is the total variance of the dependent variable. The coefficient of determination R2 ranges from 0 to 1.
[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for evaluating the formability of a reversibly cross-linked self-healing 3D printing ink, characterized in that: The steps include: (1) preparing reversibly cross-linked self-healing ink: mixing the reversibly cross-linked self-healing material with deionized water to prepare colloidal inks with different volume fractions; (2) Testing the rheological properties of the reversibly cross-linked self-healing ink: Take 0.35 ml of the reversibly cross-linked self-healing ink and apply it to the bottom plate of the rheometer. Then select a 20 mm parallel plate for testing, set the working distance to 1 mm, and set the axial force to about 0.1 N. (3) Using reversibly cross-linked self-healing ink to print single-layer and eight-layer stents, wait for 20 to 60 minutes to ensure that the stent relaxation is completely completed, and calculate the roundness Pr of the orthogonal unit area of the printed stent. The calculation method is Pr = L 2 / 16A, where L is the perimeter of the area and A is the area of the area; calculate the area change rate Ar of the unit area orthogonal to the printed stent, and the calculation method is Ar=A / A0, where A is the actual detection area area and A0 is the ideal area when the stent does not fuse or collapse; assign equivalent values to Ar and Pr, and calculate the formability index Fid, and the calculation method is: Where D P and D A are the standard deviations of Pr and Ar, U P and U A are the average values of Pr and Ar respectively, and e is a natural constant. (4) The storage modulus, complex viscosity, modulus self-repair rate and viscosity self-repair rate measured by the rheometer are taken as variables, and their relationship with Ar, Pr and Fid is fitted.
2. The evaluation method according to claim 1, characterized in that: The reversibly cross-linked self-healing material described in step (1) comprises gelatin nanoparticles, silk nanoparticles and nanoclay.
3. The evaluation method according to claim 1, characterized in that: The volume fractions described in step (1) are 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45 and 0.5 respectively.
4. The evaluation method according to claim 1, characterized in that: The test described in step (2) mainly includes two consecutive steps of testing, which need to be tested after sample preparation: A. At a fixed frequency of 1Hz / s, perform continuous tests of time scan 1, amplitude scan 1 and time scan 2, where the test time of time scan 1 and time scan 2 is 60 minutes, and the strain is controlled to 0.1%; the time of amplitude scan 1 is determined by the actual test of the rheometer, and only the strain needs to be controlled to change nonlinearly from 0.1% to 100%; The three tests were performed sequentially, and the average storage modulus G of time scan 1 and time scan 2 was calculated from the last 60s of time scan 1 and the first 60s of time scan 2. ’ 1 and G ’ 2. The modulus self-repair rate is G ’ 2 / G ’ 1; B. At a fixed frequency of 1 Hz / s, perform continuous tests of time scan 3, peak hold 1 and time scan 4, where the test time of time scan 3 and time scan 4 is 60 minutes, and the strain rate is controlled to 0.1s -1 ; The peak value is maintained for 60 seconds, and the strain rate is controlled at 30 seconds -1 The three tests were performed in sequence, and the average composite viscosity V of time scan 3 and time scan 4 was calculated from the last 60s of time scan 3 and the first 60s of time scan 4. ’ 1 and V ’ 2. The viscosity self-repair rate is G ’ 2 / G ’ 1.
5. The evaluation method according to claim 1, characterized in that: The outer side of the stent described in step (3) is a cylindrical structure with a diameter of 20 mm, and the inner side is a rectangular structure formed by six equally spaced paths arranged orthogonally in the horizontal and vertical directions, and the length of each path is 14.14 mm; the stent is composed of 8 layers of the above structure, and the thickness of each layer is 0.4 mm.
6. The evaluation method according to claim 1, characterized in that: The value range of the formability index Fid in step (3) is 0-1, and the larger the value, the better the formability.
7. The evaluation method according to claim 1, characterized in that: The fitting in step (4) uses the fourth-order polynomial fitting in Origin.
Citation Information
Patent Citations
Collagen gel formulation
CN115003321A
Structural protein / hyaluronic acid composite micro-nano particle, particle hydrogel material and application
CN115521627A
Enhanced 3D printing ink based on yeast protein and quantitative evaluation method of 3D printing performance of enhanced 3D printing ink
CN117310134A
Numerical simulation method for fused deposition modeling 3D printing process aided design
CN117951931A
Two-field coupling crosslinked, injectable, moldable and printable granular hydrogel material, preparation method thereof and application thereof
US20240100224A1