Structured liquid crystal box as well as preparation method and application thereof

By using ultraviolet ozone irradiation and photosensitizer coating technology in liquid crystal box preparation, combining the dispensing process of silicon ball spacer and ultraviolet thermal curing glue, the problems of uneven thickness and insufficient accuracy of the liquid crystal box are solved, and high uniformity is achieved and high-precision structured liquid crystal box, and improves the diffraction efficiency and service life of large wavelength light.

CN118915358AInactive Publication Date: 2024-11-08CHANGSHA LUBANG PHOTOELECTRIC TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411287763.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing liquid crystal box preparation process, the box thickness is uneven and the accuracy is insufficient, and the technology based on photosensitizer-induced liquid crystal orientation has problems of preparation complexity and optical damage.

Method used

After irradiating the ITO conductive glass with ultraviolet ozone, the photosensitizer is coated, and the silicon ball spacer is mixed with ultraviolet thermal curing glue. Structured liquid crystal box is prepared through the dispensing process, and the coordinated movement of small liquid crystal molecules is induced by ultraviolet light to achieve high uniformity. And high precision box thick.

Benefits of technology

High uniformity and high precision of the thickness of the liquid crystal box, small volume, and the diffraction efficiency of large wavelength light is improved through optical deflection technology and the service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915358A_ABST
    Figure CN118915358A_ABST
Patent Text Reader

Abstract

The invention provides a structured liquid crystal box and a preparation method and application thereof, and belongs to the technical field of liquid crystal box preparation. The preparation method of the structured liquid crystal box comprises the following steps: respectively carrying out ultraviolet ozone irradiation on two pieces of ITO glass to obtain two pieces of ITO glass with hydrophilic groups on the surfaces; respectively coating the two pieces of ITO glass with the hydrophilic groups on the surfaces by utilizing a photosensitizer to obtain two pieces of coated ITO glass; mixing the silicon ball spacers with an ultraviolet heat curing adhesive to obtain a spacer-curing adhesive mixture; and respectively dispensing the two pieces of coated ITO glass along the edges of the coated ITO glass by using the spacer-curing adhesive mixture, then folding the ITO glass subjected to dispensing, and curing to obtain the structured liquid crystal box. The internal size thickness of the structured liquid crystal box provided by the invention has high uniformity, the box thickness has the characteristic of high precision, and the preparation method provided by the invention is simple.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of liquid crystal box preparation, and in particular relates to a structured liquid crystal box and a preparation method and application thereof. Background Art

[0002] In thin film transistor liquid crystal displays (TFT-LCD) and traditional liquid crystal box preparation processes, most of them use friction induced orientation induced by PI (PI refers to polyimide, and friction alignment generally uses a spin-coated specific polyimide derivative component as an induced orientation layer) to promote the orderly arrangement of liquid crystals. However, pixelated induced orientation technology is rarely used in the market. The multi-pixelated orientation work based on photosensitizer-induced liquid crystal can well realize the arrangement of liquid crystals in different polarization states and achieve effective light modulation.

[0003] At present, most of the liquid crystal boxes used in photosensitizer-induced liquid crystal technology are prepared using tetrafluoroethylene films of different thicknesses. The thickness of the liquid crystal boxes usually prepared (excluding glass, referring to the interlayer between two pieces of glass) is more than 10μm, and the thickness of the internal dimensions of the prepared liquid crystal boxes is uneven. The preparation process is relatively complicated and the accuracy of the box thickness is insufficient. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a structured liquid crystal box and its preparation method and application. The structured liquid crystal box provided by the present invention has high uniformity of internal dimension thickness and high precision of the box thickness, and the preparation method provided by the present invention is simple.

[0005] In order to achieve the above object, the present invention provides the following scheme:

[0006] The present invention provides a method for preparing a structured liquid crystal cell, comprising the following steps:

[0007] The two pieces of ITO conductive glass are respectively irradiated with ultraviolet ozone to obtain two pieces of ITO conductive glass with hydrophilic groups on the surface;

[0008] Using a photosensitizer to coat the two pieces of ITO conductive glass having hydrophilic groups on the surface, respectively, to obtain two pieces of coated ITO conductive glass;

[0009] Mixing the silicon ball spacer and the ultraviolet heat curing adhesive to obtain a mixed adhesive;

[0010] The two pieces of ITO conductive glass after coating are respectively dispensed with the mixed adhesive along the edge of the ITO conductive glass after coating, and then the ITO conductive glasses after coating are matched and cured to obtain the structured liquid crystal box.

[0011] Preferably, the mass of the silicon ball spacer is 0.3-1.5% of the mass of the UV curing adhesive.

[0012] Preferably, the particle size of the silicon sphere spacer is 3 to 13 μm.

[0013] Preferably, when the particle size of the silicon ball spacer is 3 μm, the mass of the silicon ball spacer is 0.3% of the mass of the UV thermal curing adhesive; when the particle size of the silicon ball spacer is 13 μm, the mass of the silicon ball spacer is 1.5% of the mass of the UV thermal curing adhesive.

[0014] Preferably, the photosensitizer includes azo dye SD1.

[0015] Preferably, the width of the glue dispensing is 1 to 1.2 mm, the glue dispensing speed is 0.05 to 0.15 mL / s, and the glue dispensing speed is 1.0 to 1.2 mm / s.

[0016] Preferably, the sizes of the two pieces of ITO conductive glass are 15×10 mm respectively.

[0017] Preferably, the intensity of the UV light during curing is 60 to 90 mW / cm 2 , time is 3 to 5 minutes.

[0018] The present invention provides a structured liquid crystal box prepared by the preparation method described in the above scheme.

[0019] The present invention provides application of the structured liquid crystal box described in the above solution in a liquid crystal light beam scanner.

[0020] The present invention provides a method for preparing a structured liquid crystal box, comprising the following steps: irradiating two pieces of ITO glass with ultraviolet ozone respectively to obtain two pieces of ITO glass with hydrophilic groups on the surface; coating the two pieces of ITO glass with hydrophilic groups on the surface respectively with a photosensitizer to obtain two pieces of coated ITO glass; mixing a silicon ball spacer with an ultraviolet heat curing adhesive to obtain a spacer-curing adhesive mixture; dispensing the two pieces of coated ITO glass along the edge of the coated ITO glass with the spacer-curing adhesive mixture, and then aligning the dispensed ITO glass, and curing to obtain the structured liquid crystal box. The structured liquid crystal box prepared by the present invention has high uniformity in thickness of internal dimensions and high box thickness precision, and the preparation method provided by the present invention is simple. In the present invention, the high uniformity is reflected in that when the box thickness is detected by white light interferometry, the error of the calculation result of the entire in-plane test site is less than 0.1μm, and the high precision of the box thickness is reflected in that the box thickness error is only 0.25μm.

[0021] The existing mechanical beam polarization technology requires the use of a mechanical deflection device, which is relatively large (length, width, height of about tens of centimeters), and the ordinary grating beam deflection technology can only be used in a smaller band range during design. When the applicable band is exceeded, the grating diffraction efficiency will be seriously reduced, resulting in greater optical damage. The optical damage here refers to the loss of optical energy. If the traditional grating beam deflection technology uses light of a large wavelength, the diffraction efficiency will be reduced due to the limitations of the traditional design, and the diffracted light energy will decrease, while the liquid crystal beam deflection technology can achieve high diffraction efficiency at a large wavelength. In addition, the structured liquid crystal box prepared by the present invention is small in size (the sizes of the two glass plates are 15×10 mm respectively), which is about 100 times smaller than the existing technology.

[0022] The structured liquid crystal box provided by the present invention can induce the orientation of the photosensitizer through ultraviolet light, and based on the interaction force between the host and the guest, promote the coordinated movement of the liquid crystal small molecules at a line width of 1 to 2 μm, thereby realizing effective design and regulation of any special phase. The designed and prepared structured liquid crystal empty box has the characteristics of high transmittance, long service life, etc.

[0023] Taking the structured liquid crystal cell prepared by the present invention for preparing a liquid crystal beam scanner as an example, the deflection process is as follows: by controlling the voltage applied to the liquid crystal variable retarder so that the delay amount of the liquid crystal variable retarder is one quarter of the wavelength of the incident light, controlling the voltage applied to N active liquid crystal polarization gratings so that the delay amount of the N active liquid crystal polarization gratings is one half of the wavelength of the incident light, when the incident light passes through the optical polarizer and the liquid crystal variable retarder, the polarization state of the incident light will be modulated into left-handed circularly polarized light or right-handed circularly polarized light. When left-handed circularly polarized light (right-handed circularly polarized light) passes through the first active liquid crystal polarization grating, since the delay amount of the active liquid crystal polarization grating is adjusted to half of the wavelength of the incident light, the left-handed circularly polarized light (right-handed circularly polarized light) will be completely converted into right-handed circularly polarized light (left-handed circularly polarized light), and deviate from the original incident direction, and the deflection angle is θ1, θ1=arcsin(λ / P1), λ is the wavelength of the incident light, P1 is the period of the first active liquid crystal polarization grating, when the right-handed circularly polarized light (left-handed circularly polarized light) When passing through the second active liquid crystal polarization grating, since the grating lines of the two adjacent active liquid crystal polarization gratings are parallel, the azimuth angles of the liquid crystal molecules change in the opposite order, and the right-handed circularly polarized light (left-handed circularly polarized light) will be polarized again along the original polarization direction, and the deflection angle is θ1+θ2, θ2=arcsin(λ / P2), P2 is the period of the second active liquid crystal polarization grating, and the right-handed circularly polarized light (left-handed circularly polarized light) will be converted into left-handed circularly polarized light (right-handed circularly polarized light) again, and so on. The whole process The main light intensity loss comes from the reflection between different active liquid crystal polarization grating glass substrates; the voltages applied to the N active liquid crystal polarization gratings are different. When the voltages applied to the N active liquid crystal polarization gratings reach the saturation voltage, each active liquid crystal polarization grating is equivalent to a window plate, and the incident light will not be deflected. By independently controlling the voltages applied to the N active liquid crystal polarization gratings, the deflection of the incident light within 0~θ1+θ2+...θN can be achieved. The specific deflection process diagram is shown in Figure 7 shown. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0025] Figure 1 The test results of Demo-A in Example 1 of the present invention are as follows;

[0026] Figure 2 This is the test result of Demo-B in Example 1 of the present invention;

[0027] Figure 3 The test results of Demo-C in Example 1 of the present invention are as follows;

[0028] Figure 4 This is a physical picture of Demo-A in Example 1 of the present invention;

[0029] Figure 5 The test results of comparative example 1 of the present invention are as follows;

[0030] Figure 6 It is a top view, a front view and a left view of two ITO conductive glasses after being joined together according to embodiments 1 to 3 of the present invention;

[0031] Figure 7 Schematic diagram of the incident light deflection process in a liquid crystal beam scanner. DETAILED DESCRIPTION

[0032] The present invention provides a method for preparing a structured liquid crystal cell, comprising the following steps:

[0033] The two pieces of ITO conductive glass are respectively irradiated with ultraviolet ozone to obtain two pieces of ITO conductive glass with hydrophilic groups on the surface;

[0034] Using a photosensitizer to coat the two pieces of ITO conductive glass having hydrophilic groups on the surface, respectively, to obtain two pieces of coated ITO conductive glass;

[0035] Mixing the silicon ball spacer and the ultraviolet heat curing adhesive to obtain a mixed adhesive;

[0036] The two pieces of ITO conductive glass after coating are respectively dispensed with the mixed adhesive along the edge of the ITO conductive glass after coating, and then the ITO conductive glasses after coating are matched and cured to obtain the structured liquid crystal box.

[0037] Unless otherwise specified, the materials and equipment used in the present invention are commercially available products.

[0038] The invention irradiates two pieces of ITO conductive glass with ultraviolet ozone respectively to obtain two pieces of ITO conductive glass with hydrophilic groups on the surface.

[0039] In the present invention, the sizes of the two pieces of ITO conductive glass are preferably 15×10 mm respectively.

[0040] In the present invention, before the ultraviolet ozone irradiation, the two ITO conductive glasses are preferably cleaned; the cleaning preferably includes: soaking the two ITO conductive glasses in acetone, placing them in an ultrasonic cleaning machine for 5 minutes, taking them out and then placing them in anhydrous ethanol for 5 minutes, then taking them out and placing them in ultrapure water for cleaning and ultrasonication for 5 minutes, and then placing them in a 60°C oven for drying. The present invention can clean the inorganic impurities and organic impurities on the ITO conductive glass by acetone cleaning.

[0041] In the present invention, the light intensity of the ultraviolet ozone irradiation is preferably 28 to 32 mW / cm 2 , in the specific embodiment of the present invention, it can be 28mW / cm 2 、29mW / cm 2 、30mW / cm 2 、31mW / cm 2 or 32mW / cm 2 The present invention can increase the proportion of hydrophilic groups on the surface of ITO conductive glass by ultraviolet ozone irradiation, and maintain a certain degree of hydrophilicity on the surface of ITO conductive glass. In the present invention, the hydrophilic group is a hydroxyl group. The present invention can increase the uniformity of the photosensitizer on the conductive glass by adding hydrophilic groups on the conductive glass.

[0042] After obtaining the two pieces of ITO conductive glasses with hydrophilic groups on the surfaces, the present invention uses a photosensitizer to respectively plate the two pieces of ITO conductive glasses with hydrophilic groups on the surfaces to obtain two pieces of plated ITO conductive glasses.

[0043] In the present invention, the photosensitizer preferably includes azo dye SD1.

[0044] In the present invention, the coating preferably includes: placing two pieces of ITO conductive glass with hydrophilic groups on the surface on a spin coating machine, vacuum adsorption, then sucking the photosensitizer solution with a syringe, dropping 0.1 mL on the ITO conductive glass, and spin coating. After the spin coating is completed, place it on a 100°C hot stage to remove excess solvent for 3 minutes, and then place the two pieces of ITO conductive glass in a constant temperature nitrogen cabinet for storage until use.

[0045] In the present invention, the photosensitizer solution is preferably obtained by dissolving a photosensitizer in an organic solvent; the organic solvent preferably includes N,N-dimethylformamide (DMF); and the mass concentration of the photosensitizer solution is preferably 30%.

[0046] In the present invention, the rotation speed of the spin coating is preferably 3000 rpm, and the time is preferably 30 seconds. In the present invention, the constant temperature is preferably 25°C.

[0047] The present invention mixes the silicon ball spacer and the ultraviolet heat curing adhesive to obtain the mixed adhesive.

[0048] In the present invention, the particle size of the silicon ball spacer is preferably 3 to 13 μm, and specifically can be 3 μm, 5 μm, 7 μm, 9 μm, 11 μm or 13 μm.

[0049] In the present invention, the mass of the silicon ball spacer is preferably 0.3-1.5% of the mass of the UV curing adhesive, and in a specific embodiment of the present invention, it can be 0.3%, 0.5%, 0.8%, 1.0%, 1.2% or 1.5%. In the present invention, when the particle size of the silicon ball spacer is 3 μm, the mass of the silicon ball spacer is preferably 0.3% of the mass of the UV curing adhesive; when the particle size of the silicon ball spacer is 13 μm, the mass of the silicon ball spacer is preferably 1.5% of the mass of the UV curing adhesive.

[0050] In the present invention, the mixing is preferably carried out under stirring conditions, the stirring speed is preferably 500 rpm, and the stirring time is preferably 10 min.

[0051] The present invention preferably places the mixed glue in a glue cylinder of a glue dispensing machine for standby use.

[0052] In the process of preparing the mixed glue of the present invention, the content (mass percentage) of the added silicon ball spacer is related to its size (particle size). The smaller the size of the silicon ball spacer, the lower the content of the added silicon ball spacer. Because for the same mass of silicon ball spacers, the surface area of ​​small-sized silicon ball spacers is larger than that of large-sized silicon ball spacers, and it is easier to cause silicon balls to agglomerate due to the effect of surface tension. Therefore, in the present invention, the best effect is achieved when the proportion of 13μm silicon ball spacers in the cured glue is 1.5wt%, and the best effect is achieved when the proportion of small-sized 3μm silicon ball spacers in the cured glue is 0.3wt%.

[0053] After obtaining the mixed glue and two pieces of coated ITO conductive glass, the present invention uses the mixed glue to dispense glue on the two pieces of coated ITO conductive glass along the edges of the coated ITO conductive glass, and then aligns the dispensed ITO conductive glasses, and obtains the structured liquid crystal box after curing.

[0054] In the present invention, the width of the dispensing is preferably 1-1.2 mm, and in a specific embodiment of the present invention, it can be 1 mm, 1.1 mm or 1.2 mm; the dispensing speed of the dispensing is preferably 0.05-0.15 mL / s, and in a specific embodiment of the present invention, it can be 0.05 mL / s, 0.08 mL / s, 0.10 mL / s, 0.12 mL / s, 0.14 mL / s or 0.15 mL / s; the dispensing speed is preferably 1.0-1.2 mm / s, and in a specific embodiment of the present invention, it can be 1.0 mm / s, 1.1 mm / s or 1.2 mm / s.

[0055] The present invention has no special requirements for the alignment, and the implementation process known in the art can be used. In the embodiment of the present invention, the alignment is preferably performed in a fixture, and the alignment is shown in FIG. Figure 6 As shown, there are top view, front view and left view in sequence, and the unit of the values ​​in the figure is mm.

[0056] In the present invention, the intensity of the UV light for curing is preferably 60 to 90 mW / cm 2 , in the specific embodiment of the present invention, it can be 60mW / cm 2 、70mW / cm 2 、80mW / cm 2 or 90mW / cm 2 The curing time is preferably 3 to 5 minutes, and in a specific embodiment of the present invention it can be 3 minutes, 4 minutes or 5 minutes.

[0057] The present invention provides a structured liquid crystal box prepared by the preparation method described in the above scheme.

[0058] The structured liquid crystal box provided by the present invention can induce the orientation of the photosensitizer through ultraviolet light, and based on the interaction force between the host and the guest, promote the coordinated movement of the liquid crystal small molecules at a line width of 1 to 2 μm, thereby realizing effective design and regulation of any special phase. The designed and prepared structured liquid crystal empty box has the characteristics of high transmittance, long service life, etc.

[0059] The present invention provides application of the structured liquid crystal box described in the above solution in a liquid crystal light beam scanner.

[0060] Taking the structured liquid crystal cell prepared by the present invention for preparing a liquid crystal beam scanner as an example, the deflection process is as follows: by controlling the voltage applied to the liquid crystal variable retarder so that the delay amount of the liquid crystal variable retarder is one quarter of the wavelength of the incident light, controlling the voltage applied to N active liquid crystal polarization gratings so that the delay amount of the N active liquid crystal polarization gratings is one half of the wavelength of the incident light, when the incident light passes through the optical polarizer and the liquid crystal variable retarder, the polarization state of the incident light will be modulated into left-handed circularly polarized light or right-handed circularly polarized light. When left-handed circularly polarized light (right-handed circularly polarized light) passes through the first active liquid crystal polarization grating, since the delay amount of the active liquid crystal polarization grating is adjusted to half of the wavelength of the incident light, the left-handed circularly polarized light (right-handed circularly polarized light) will be completely converted into right-handed circularly polarized light (left-handed circularly polarized light), and deviate from the original incident direction, and the deflection angle is θ1, θ1=arcsin(λ / P1), λ is the wavelength of the incident light, P1 is the period of the first active liquid crystal polarization grating, when the right-handed circularly polarized light (left-handed circularly polarized light) When passing through the second active liquid crystal polarization grating, since the grating lines of the two adjacent active liquid crystal polarization gratings are parallel, the azimuth angles of the liquid crystal molecules change in the opposite order, and the right-handed circularly polarized light (left-handed circularly polarized light) will be polarized again along the original polarization direction, and the deflection angle is θ1+θ2, θ2=arcsin(λ / P2), P2 is the period of the second active liquid crystal polarization grating, and the right-handed circularly polarized light (left-handed circularly polarized light) will be converted into left-handed circularly polarized light (right-handed circularly polarized light) again, and so on. The whole process The main light intensity loss comes from the reflection between different active liquid crystal polarization grating glass substrates; the voltages applied to the N active liquid crystal polarization gratings are different. When the voltages applied to the N active liquid crystal polarization gratings reach the saturation voltage, each active liquid crystal polarization grating is equivalent to a window plate, and the incident light will not be deflected. By independently controlling the voltages applied to the N active liquid crystal polarization gratings, the deflection of the incident light within 0~θ1+θ2+...θN can be achieved. The specific deflection process diagram is shown in Figure 7 shown.

[0061] In order to further illustrate the present invention, a structured liquid crystal box and a preparation method thereof provided by the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0062] In the embodiments of the present invention, the materials and equipment used are: 15×10 mm ITO conductive glass (Luoyang Guluo), Spacer silicon ball spacers (3 / 5 / 7 / 9 / 11 / 13 μm, Japan Hayakawa Company - Japan Hayakawa powder - 3DS), UV thermal curing glue (Japan Sekisui Company - Japan Sekisui Photolec-S), glue dispenser (Xiaomao Automation Technology Co., Ltd.), small stainless steel cantilever vertical mixer (Lichen Technology Co., Ltd.), vacuum pressing machine (Triangle Iron Technology Co., Ltd.), ultrasonic cleaning machine (Shangyi Technology Co., Ltd.), heating table (Bangyuan Technology Co., Ltd.), 50 mL beaker, laser direct writing equipment, spin coating machine (Suzhou Wenhao Microfluidic WH-SC-01 model glue spreader), photosensitizer (azo dye SD1).

[0063] Example 1

[0064] ITO glass cleaning: soak two pieces of 15×10 mm ITO conductive glass in acetone, put them in an ultrasonic cleaner for 5 minutes, take them out and put them in anhydrous ethanol for 5 minutes, then take them out and put them in ultrapure water for cleaning and ultrasonic for 5 minutes, then put them in a 60℃ oven for drying, and irradiate the two pieces of ITO conductive glass with ultraviolet ozone (28-32 mW / cm 2 ), maintaining a certain degree of hydrophilicity on the surface.

[0065] Coating: Place the two treated ITO conductive glasses on the spin coating machine, vacuum adsorb, then use a syringe to absorb an appropriate amount of photosensitizer solution (the mass concentration of the photosensitizer solution is 30%), drop 0.1mL on the ITO conductive glass, adjust the speed to 3000rpm and spin coat for 30s. After the spin coating is completed, place it on a 100℃ hot plate to remove excess solvent for 3min. Then place the two ITO conductive glasses coated with photosensitizer molecules in a constant temperature (25℃) nitrogen cabinet for storage until use.

[0066] Preparation of Spacer / cured glue: Select Spacer silicon ball spacers with a size of 3μm and mix them with the curing glue (the silicon ball spacers are 0.3wt% of the curing glue), place them in a 50mL beaker, and then stir them on a mechanical stirring table for 10 minutes at a speed of 500rpm. After the curing glue and the Spacer silicon ball spacers are fully mixed, place the resulting mixed glue in the glue barrel of the glue dispensing machine for later use.

[0067] Dispensing / curing: Place two ITO conductive glasses coated with photosensitizer molecules on the displacement stage of the dispensing machine, and dispense glue along the 1.0mm width at the edge of the ITO conductive glass. The glue flow rate is 0.05mL / s, and the dispensing speed is 1.0mm / s. After dispensing, place the two ITO conductive glasses according to Figure 6Precise alignment is performed in the fixture and then cured with a UV lamp. The UV lamp irradiation energy is 90mw / cm 2 , curing time 3 minutes, to obtain the structured liquid crystal box.

[0068] According to the above test steps, three parallel tests were carried out, and the obtained structured liquid crystal cell samples were respectively recorded as Demo-A, Demo-B and Demo-C. The actual picture of Demo-A is shown in Figure 4 shown.

[0069] Laser direct writing: The photosensitizer molecules provided by the present invention can be oriented vertically along the direction of polarized blue light. Therefore, the above-mentioned ITO conductive glass coated with photosensitizer molecules is placed on a laser direct writing platform for phase replication. The step length of the laser spot is 1 to 2 μm. Therefore, multiple polarization state pixels can be written within the range of 10 mm of the aperture, thereby preparing a structured liquid crystal box that can induce an orderly arrangement of liquid crystal molecules with different orientation angles.

[0070] Cell thickness test: In order to verify the success of the preparation of the structured liquid crystal cell and verify the cell thickness of the liquid crystal cell, the present invention uses white light interferometry to test the above three samples respectively. The test results of Demo-A, Demo-B and Demo-C are as follows: Figures 1 to 3 As shown, the horizontal axis is wavelength nm and the vertical axis is intensity. The blue line represents the fitting graph, and the red line represents the test graph, i.e., the sample graph. The wavelength results of adjacent interference peaks and the box thickness (spacing d) are shown in Table 1.

[0071] Table 1 White light interferometry sample test data

[0072]

[0073] The results in Table 1 show that the cell thickness error of the present invention is only 0.25 μm (standard value 3.0 μm), indicating that the cell thickness of the structured liquid crystal cell prepared by the present invention has high precision.

[0074] In addition, Demo-C took five different test locations within the 10mm aperture range, and the error range of the samples tested by white light interferometry did not exceed 0.1μm.

[0075] The above data indicate that the structured liquid crystal cells obtained by the present invention have excellent properties such as high uniformity and high precision.

[0076] Comparative Example 1

[0077] The preparation steps are the same as those in Example 1, except that the comparative example 1 adopts wet dispensing. Specifically, wet dispensing: 3 μm spacer silicon ball spacers are dissolved in trimethylbenzene solution to prepare a mixed solution (the spacer accounts for 0.3 wt%), and the mixed solution is sprayed onto the ITO glass with photosensitizer at room temperature. Figure 5 shown.

[0078] like Figure 5 As shown in the test results, the calculation results show that the sample prepared by the 3μm Spacer silicon ball spacer is tested by white light interferometry and the result spacing is 4.9μm. At the same time, the interference light peak intensity is greatly reduced, which is greatly related to the light loss caused by wet dispensing (the wet dispensing process is easy to cause a certain degree of light scattering in the aperture due to the spacer in the light transmission range, causing light loss, resulting in reduced transmittance and decreased box thickness accuracy). The dry dispensing of the present invention (without adding any solvent) is to dispense at the edge of the conductive glass, so it can avoid the above problems in the wet dispensing process and will not cause light loss.

[0079] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a structured liquid crystal cell, characterized in that: The following steps are involved: The two pieces of ITO conductive glass are respectively irradiated with ultraviolet ozone to obtain two pieces of ITO conductive glass with hydrophilic groups on the surface; Using a photosensitizer to coat the two pieces of ITO conductive glass having hydrophilic groups on the surface, respectively, to obtain two pieces of coated ITO conductive glass; Mixing the silicon ball spacer and the ultraviolet heat curing adhesive to obtain a mixed adhesive; The two pieces of ITO conductive glass after coating are respectively dispensed with the mixed adhesive along the edge of the ITO conductive glass after coating, and then the ITO conductive glasses after coating are matched and cured to obtain the structured liquid crystal box.

2. The preparation method according to claim 1, characterized in that: The mass of the silicon ball spacer is 0.3-1.5% of the mass of the ultraviolet heat curing adhesive.

3. The preparation method according to claim 1 or 2, characterized in that: The particle size of the silicon ball spacer is 3 to 13 μm.

4. The preparation method according to claim 3, characterized in that: When the particle size of the silicon ball spacer is 3 μm, the mass of the silicon ball spacer is 0.3% of the mass of the UV thermal curing adhesive; when the particle size of the silicon ball spacer is 13 μm, the mass of the silicon ball spacer is 1.5% of the mass of the UV thermal curing adhesive.

5. The preparation method according to claim 1, characterized in that: The photosensitizer includes azo dye SD1.

6. The preparation method according to claim 1, characterized in that: The width of the glue dispensing is 1 to 1.2 mm, the glue dispensing speed is 0.05 to 0.15 mL / s, and the glue dispensing speed is 1.0 to 1.2 mm / s.

7. The preparation method according to claim 1, characterized in that: The sizes of the two pieces of ITO conductive glass are 15×10 mm respectively.

8. The preparation method according to claim 1, characterized in that: The intensity of the UV light for curing is 60-90 mW / cm 2 , time is 3 to 5 minutes.

9. The structured liquid crystal box prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the structured liquid crystal cell according to claim 9 in a liquid crystal beam scanner.

Citation Information

Patent Citations

  • Preparation method of liquid crystal box

    CN113031334A

  • Method for eliminating liquid crystal misalignment

    CN115542615A

  • Device for generating annular structured light and preparation method thereof

    CN115685566A

  • Polarization-independent silicon-based liquid crystal spatial light modulator and preparation method thereof

    CN117850101A

  • Production of low-voltage-driven liquid-crystal refractive-index grating

    CN1896779A