Hard mask composition, hard mask layer, and method of forming pattern

By using the hard mask layer formed by a specific hard mask composition, the problem of insufficient pattern fineness and etch resistance in lithography technology is solved, and efficient pattern transfer and etching effects are achieved.

CN118915386APending Publication Date: 2024-11-08SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410529694.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-04-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

It is difficult for the existing lithography techniques to form fine patterns with excellent profiles, especially in the small size range, and the etch resistance of the hard mask layer is not sufficient to withstand the etching process.

Method used

Using a hard mask composition containing a specific compound, a hard mask layer is formed by heat treatment and exposed and developed on the photoresist layer to form a pattern, selectively removing the hard mask layer to expose portions of the material layer, achieving Etching.

Benefits of technology

It achieves excellent etch resistance and heat resistance, ensures the fineness of pattern transfer and process reliability, and improves the accuracy and efficiency of lithography technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915386A_ABST
    Figure CN118915386A_ABST
Patent Text Reader

Abstract

The present invention provides a hard mask composition, a hard mask layer comprising a cured product of the hard mask composition, and a method for forming a pattern using the hard mask layer comprising the cured product of the hard mask composition, the hard mask composition comprising a compound represented by Chemical Formula 1 and a solvent, [Chemical Formula 1] # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0059327 filed in the Korean Intellectual Property Office on May 8, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] Embodiments relate to a hard mask composition, a hard mask layer, and a method of forming a pattern. Background Art

[0004] In recent years, the semiconductor industry has developed ultra-fine technology with patterns ranging from a few nanometers to tens of nanometers in size. This ultra-fine technology can utilize photolithography technology.

[0005] Some photolithography techniques may include: providing a material layer on a semiconductor substrate; coating a photoresist layer on the material layer; exposing and developing the photoresist layer to provide a photoresist pattern; and etching the material layer using the photoresist pattern as a mask.

[0006] Depending on the small size of the pattern to be formed, it may be difficult to provide a fine pattern with an excellent profile by using only some photolithography techniques. Therefore, an auxiliary layer called a hard mask layer may be formed between the material layer and the photoresist layer to provide a fine pattern. Summary of the invention

[0007] Embodiments may be implemented by providing a hard mask composition including a compound represented by Chemical Formula 1 and a solvent:

[0008] [Chemical formula 1]

[0009]

[0010] In chemical formula 1, Ar 1 To Ar 3 ,Ar 11 ,Ar 21 and Ar 31 Each is independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a substituted or unsubstituted C3 to C30 heteroaromatic hydrocarbon group, wherein two or more of the aromatic hydrocarbon group, heteroaromatic hydrocarbon group or a combination thereof are linked by a single bond or a substituted or unsubstituted C1 to C10 alkylene group, or a combination thereof,

[0011] R 1 To R 3each independently represents hydrogen, deuterium, substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, substituted or unsubstituted C1 to C30 saturated or unsaturated heteroaliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated heteroalicyclic hydrocarbon group, substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, substituted or unsubstituted C4 to C30 heteroaromatic hydrocarbon group, or a combination thereof,

[0012] R 11 , R 21 and R 31 are each independently hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group,

[0013] n is an integer from 0 to 2, and

[0014] m is an integer of 1 to 4.

[0015] Ar in Formula 1 1 To Ar 3 The substituted or unsubstituted groups which may each independently be moieties of Group 1 are:

[0016] [Group 1]

[0017]

[0018] In group 1, R a and R b Each may independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group.

[0019] Ar in Formula 1 1 To Ar 3 The substituted or unsubstituted groups which may each independently be part of Group 1-1 are:

[0020] [Group 1-1]

[0021]

[0022] Among them, in group 1-1, R a and R b Each may independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group.

[0023] Ar in Formula 1 11 ,Ar21 and Ar 31 Each independently may be a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group.

[0024] Ar in Formula 1 11 ,Ar 21 and Ar 31 Substituted or unsubstituted groups which may each independently be part of Group 2:

[0025] [Group 2]

[0026]

[0027] Ar in Formula 1 1 To Ar 3 may be independently a substituted or unsubstituted group of Group 1-2, and Ar 11 ,Ar 21 and Ar 31 Substituted or unsubstituted groups which may each independently be part of Group 2-1:

[0028] [Group 1-2]

[0029]

[0030] [Group 2-1]

[0031]

[0032] In Chemical Formula 1, R 1 To R 3 may each independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof, and R 11 , R 21 and R 31 They may each independently be hydrogen, deuterium, or a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group.

[0033] In Chemical Formula 1, R 1 To R 3 , R 11 , R 21 and R 31 Each may independently be hydrogen, deuterium, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof.

[0034] In Chemical Formula 1, Ar 1 with Ar 2 ,Ar 11 with Ar21 , R 1 With R 2 or R 11 With R 21 Can be the same as each other.

[0035] The compound represented by Chemical Formula 1 may be represented by one of Chemical Formulas 2 to 15:

[0036] [Chemical formula 2]

[0037]

[0038] [Chemical formula 3]

[0039]

[0040] [Chemical formula 4]

[0041]

[0042] [Chemical formula 5]

[0043]

[0044] [Chemical formula 6]

[0045]

[0046] [Chemical formula 7]

[0047]

[0048] [Chemical formula 8]

[0049]

[0050] [Chemical formula 9]

[0051]

[0052] [Chemical formula 10]

[0053]

[0054] [Chemical formula 11]

[0055]

[0056] [Chemical formula 12]

[0057]

[0058] [Chemical formula 13]

[0059]

[0060] [Chemical formula 14]

[0061]

[0062] [Chemical formula 15]

[0063]

[0064] The compound may have a molecular weight of about 500 g / mole to about 10,000 g / mole.

[0065] The compound may be included in an amount of about 0.1 wt % to about 30 wt % based on the total weight of the hardmask composition.

[0066] The solvent may include propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone or ethyl 3-ethoxypropionate.

[0067] Embodiments may be implemented by providing a hard mask layer including a cured product of the hard mask composition according to embodiments.

[0068] An embodiment can be implemented by providing a method for forming a pattern, the method comprising: providing a material layer on a substrate; applying a hard mask composition according to an embodiment to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; using the photoresist pattern to selectively remove the hard mask layer to expose a portion of the material layer; and etching the exposed portion of the material layer.

[0069] Forming the hard mask layer may include performing a heat treatment at about 100°C to about 1,000°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Features will be readily apparent to those skilled in the art by describing exemplary embodiments in detail with reference to the accompanying drawings, in which:

[0071] Figure 1 Reference diagrams illustrating level differences of a hard mask layer to explain a method of evaluating planarization characteristics and calculation formulas for evaluating planarization characteristics are shown. DETAILED DESCRIPTION

[0072] Example embodiments will now be described more fully hereinafter with reference to the accompanying drawings; however, they may be embodied in different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and these embodiments will fully convey exemplary implementations to those skilled in the art.

[0073] In the various drawings, the dimensions of layers and regions may be exaggerated for clarity of illustration. It is also understood that when a layer or element is referred to as being "on" another layer or substrate, it may be directly on the other layer or substrate, or there may be intervening layers. Furthermore, it is understood that when a layer is referred to as being "below" another layer, it may be directly below, and there may also be one or more intervening layers. In addition, it is also understood that when a layer is referred to as being "between" two layers, it may be the only layer between the two layers, or there may also be one or more intervening layers. The same reference numerals refer to the same elements throughout.

[0074] As used herein, when no definition is otherwise provided, 'substituted' may refer to that a hydrogen atom of a compound is replaced by a substituent selected from the group consisting of a halogen atom (F, Br, Cl or I), a hydroxyl group, an alkoxy group, a nitro group, a cyano group, an amino group, an azido group, a carbamimido group, a hydrazine group, a hydrazo group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a vinyl group, a C1 to C20 alkyl group, a C2 to C20 alkenyl group, a C2 to C20 alkynyl group, a C6 to C30 aryl group, a C7 to C30 aralkyl group, a C9 to C30 allylaryl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroaralkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, a C3 to C30 heterocycloalkyl group, or a combination thereof. As used herein, hydrogen substitution (-H) may include deuterium substitution (-D) or tritium substitution (-T). For example, any hydrogen in any compound described herein may be protium, deuterium, or tritium (e.g., based on natural substitution or artificial substitution). As used herein, the term "or" is not necessarily an exclusive term, for example, "A or B" will include A, B, or A and B. As used herein, * is a point of attachment unless otherwise described.

[0075] In addition, two adjacent substituents of a substituted halogen atom (F, Br, Cl or I), a hydroxyl group, a nitro group, a cyano group, an amino group, an azido group, a carbamimido group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphate group or a salt thereof, a C1 to C30 alkyl group, a C2 to C30 alkenyl group, a C2 to C30 alkynyl group, a C6 to C30 aryl group, a C7 to C30 aralkyl group, a C1 to C30 alkoxy group, a C1 to C20 heteroalkyl group, a C3 to C20 heteroaralkyl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C15 cycloalkynyl group, or a C2 to C30 heterocyclyl group may be condensed to form a ring.

[0076] As used herein, when no definition is otherwise provided, "aromatic hydrocarbon group" refers to a group having one or more hydrocarbon aromatic moieties, including a form in which the hydrocarbon aromatic moieties are connected by a single bond, a non-aromatic condensed ring form in which the hydrocarbon aromatic moieties are directly or indirectly condensed, or a combination thereof, as well as a non-condensed aromatic hydrocarbon ring, a condensed aromatic hydrocarbon ring.

[0077] More specifically, the substituted or unsubstituted aromatic hydrocarbon group may be a substituted or unsubstituted phenyl group, a substituted or unsubstituted naphthyl group, a substituted or unsubstituted anthracenyl group, a substituted or unsubstituted phenanthrenyl group, a substituted or unsubstituted fused tetraphenyl group, a substituted or unsubstituted pyrenyl group, a substituted or unsubstituted biphenyl group, a substituted or unsubstituted terphenyl group, a substituted or unsubstituted quaterphenyl group, a substituted or unsubstituted chrysene group, a substituted or unsubstituted triphenylenyl group, a substituted or unsubstituted peryl group, a substituted or unsubstituted indenyl group, a combination thereof, or a combined fused ring of the foregoing groups, but is not limited thereto.

[0078] As used herein, when a definition is not otherwise provided, “hetero” refers to one containing 1 to 3 heteroatoms selected from N, O, S, Se and P.

[0079] As used herein, when no additional definition is provided, "heteroaromatic hydrocarbon group" is a concept including heteroaryl groups, and may contain at least one heteroatom selected from N, O, S, P and Si, rather than carbon (C) in a cyclic compound, such as an aromatic hydrocarbon ring group, a cycloalkyl group, a condensed ring thereof, or a combination thereof. When the heteroaromatic hydrocarbon group is a condensed ring, the entire ring or each ring of the heterocyclic group may contain one or more heteroatoms.

[0080] As used herein, when a specific definition is not otherwise provided, the term "combination" means mixing or copolymerization.

[0081] Unless otherwise specified in the specification, the "molecular weight" is measured by dissolving a powder sample in tetrahydrofuran (THF) and then using Agilent Technologies' 1200 series Gel Permeation Chromatography (GPC) (column: Shodex Company LF-804, standard sample: Showa Company polystyrene).

[0082] The hard mask composition according to some embodiments may include a compound represented by Chemical Formula 1 and a solvent.

[0083] [Chemical formula 1]

[0084]

[0085] In Chemical Formula 1, Ar 1 To Ar 3 ,Ar 11 ,Ar 21 and Ar 31 Each independently may be or include, for example, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a substituted or unsubstituted C3 to C30 heteroaromatic hydrocarbon group, a group in which two or more of the aromatic hydrocarbon rings, heteroaromatic hydrocarbon rings, or a combination thereof are linked by a single bond or a substituted or unsubstituted C1 to C10 alkylene group, or a combination thereof.

[0086] R 1 To R 3 Each independently may be or include, for example, hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, a substituted or unsubstituted C1 to C30 saturated or unsaturated heteroaliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated heteroaliphatic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a substituted or unsubstituted C4 to C30 heteroaromatic hydrocarbon group, or a combination thereof.

[0087] R 11 , R 21 and R 31 Each independently may be or include, for example, hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group.

[0088] n may be an integer from 0 to 2.

[0089] m may be an integer from 1 to 4.

[0090] The compound according to some embodiments may include an aromatic hydrocarbon group or a heteroaromatic hydrocarbon group as shown in Chemical Formula 1, and may include a tertiary carbon or a quaternary carbon connected thereto, thereby increasing the carbon content of the composition. In addition, a portion of the linking group connecting the aromatic hydrocarbon group or the heteroaromatic hydrocarbon group may include a nitrogen (N) atom, so that the cross-linking characteristics during curing of the composition can be improved, and the hard mask layer formed therefrom can have excellent etching resistance.

[0091] In addition, Chemical Formula 1 may include a tertiary carbon or a quaternary carbon and a 11 、-OR 21 OR 31 The substituent represented by , makes it possible to improve the solubility of the compound in a solvent, and the hard mask composition containing such a compound can be effectively applied to a spin coating process. In addition, since the compound can be cross-linked into a high molecular weight polymer form in a short period of time during heat treatment, a hard mask layer formed therefrom can have excellent heat resistance and excellent etching resistance.

[0092] Ar in Formula 1 1 To Ar 3 The groups which may each independently be part of Group 1 are substituted or unsubstituted.

[0093] [Group 1]

[0094]

[0095] In group 1, R a and R b Each independently may be, for example, hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group.

[0096] In an embodiment, Ar in Formula 1 1 To Ar 3 Each may independently be a substituted or unsubstituted group such as a part of Group 1-1.

[0097] [Group 1-1]

[0098]

[0099] In group 1-1, R a and R b Each independently may be, for example, hydrogen, deuterium, a substituted or unsubstituted C1 to C10 alkyl group, or a substituted or unsubstituted C6 to C20 aryl group.

[0100] In an embodiment, Ar in Formula 1 1 To Ar 3Each may independently be a substituted or unsubstituted group such as a part of Group 1-2.

[0101] [Group 1-2]

[0102]

[0103] In an embodiment, in Chemical Formula 1, Ar 11 ,Ar 21 and Ar 31 Each of Ar and Ar in Formula 1 may be independently, for example, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group. 11 ,Ar 21 and Ar 31 may each independently be a substituted or unsubstituted group of a part of Group 2. In an embodiment, Ar in Formula 1 11 ,Ar 21 and Ar 31 Each may be independently a substituted or unsubstituted group of the group 2-1.

[0104] [Group 2]

[0105]

[0106] [Group 2-1]

[0107]

[0108] In an embodiment, Ar in Formula 1 1 To Ar 3 may be independently a substituted or unsubstituted group of Group 1-2, and Ar 11 ,Ar 21 and Ar 31 Each may be independently a substituted or unsubstituted group of the group 2-1.

[0109] In an embodiment, R in Chemical Formula 1 1 To R 3 Each independently may be, for example, hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof.

[0110] In an embodiment, R in Chemical Formula 1 11 , R 21 and R 31 They may each independently be, for example, hydrogen, deuterium, or a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group.

[0111] In an embodiment, R in Chemical Formula 1 1 To R 3 , R 11 , R 21 and R 31 Each of R and R in Formula 1 may be independently, for example, hydrogen, deuterium, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof. 1 To R 3 , R 11 , R 21 and R 31 Each of R in Formula 1 may be independently, for example, hydrogen, deuterium, methyl, ethyl, propyl, butyl, phenyl, naphthyl, anthracenyl, phenanthryl, or a combination thereof. 1 To R 3 , R 11 , R 21 and R 31 Each can independently be, for example, hydrogen, deuterium, methyl, phenyl, or a combination thereof.

[0112] In an embodiment, in Chemical Formula 1, n may be an integer of 0 to 2, for example, 0 or 1.

[0113] In an embodiment, in Chemical Formula 1, m may be an integer of 1 to 4. In an embodiment, in Chemical Formula 1, m may be an integer of 1 to 3, for example, 1 or 2.

[0114] In an embodiment, in Chemical Formula 1, Ar 1 with Ar 2 ,Ar 11 with Ar 21 , R 1 With R 2 or R 11 With R 21 Each of the may be the same, only some of them may be the same, or each may be different from each other. 1 with Ar 2 ,Ar 11 with Ar 21 , R 1 With R 2 or R 11 With R 21 Can be the same as each other can mean Ar 1 with Ar 2 Can be the same, Ar 11 with Ar 21 Can be the same, R 1 With R 2 can be the same, and R 11 With R 21 Can be the same.

[0115] In an embodiment, in Chemical Formula 1, Ar 3 Can be used with Ar 1 or Ar 2 Same or different.

[0116] In an embodiment, if n in Chemical Formula 1 is 1 or greater than 1, then Ar 31 Can be used with Ar 11 or Ar 21 Same, R 3 Can be used with R 1 or R 2 The same, and R 31 Can be used with R 11 or R 21 same.

[0117] In an embodiment, if m in Chemical Formula 1 is 2 or greater than 2, then Ar 1 ,Ar 2 ,Ar 11 ,Ar 21 , R 1 , R 2 , R 11 and R 21 Each of can be the same as or different from each other.

[0118] In the embodiment, the compound represented by Chemical Formula 1 may be represented by one of Chemical Formulas 2 to 15.

[0119] [Chemical formula 2]

[0120]

[0121] [Chemical formula 3]

[0122]

[0123] [Chemical formula 4]

[0124]

[0125] [Chemical formula 5]

[0126]

[0127] [Chemical formula 6]

[0128]

[0129] [Chemical formula 7]

[0130]

[0131] [Chemical formula 8]

[0132]

[0133] [Chemical formula 9]

[0134]

[0135] [Chemical formula 10]

[0136]

[0137] [Chemical formula 11]

[0138]

[0139] [Chemical formula 12]

[0140]

[0141] [Chemical formula 13]

[0142]

[0143] [Chemical formula 14]

[0144]

[0145] [Chemical formula 15]

[0146]

[0147] The compound may have a molecular weight of, for example, about 500 g / mol to about 10,000 g / mol. In an embodiment, the molecular weight of the compound may be, for example, about 500 g / mol to about 9,500 g / mol, about 500 g / mol to about 9,000 g / mol, about 600 g / mol to about 8,500 g / mol, about 600 g / mol to about 8,000 g / mol, about 700 g / mol to about 7,500 g / mol, or about 700 g / mol to about 7,000 g / mol. By having a molecular weight within the above range, the carbon content and solubility in a solvent of a hard mask composition containing the above compound can be adjusted and optimized.

[0148] The compound may be included, for example, in an amount of about 0.1 wt % to about 30 wt % based on the total weight of the hard mask composition. In an embodiment, the compound may be included, for example, in an amount of about 0.2 wt % to about 30 wt %, about 0.5 wt % to about 30 wt %, about 1 wt % to about 30 wt %, about 1 wt % to about 25 wt %, or about 1 wt % to about 20 wt %. By including the compound within the above range, the thickness, surface roughness, and planarization degree of the hard mask may be easily adjusted.

[0149] The hardmask composition may include a solvent. In an embodiment, the solvent may include, for example, propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone, ethyl 3-ethoxypropionate, or the like. In an embodiment, the solvent may be a suitable solvent having sufficient solubility or dispersibility for the compound.

[0150] In an embodiment, the hardmask composition may further include additives such as a surfactant, a crosslinking agent, a thermal acid generator, or a plasticizer.

[0151] The surfactant may include, for example, fluoroalkyl compounds, alkylbenzene sulfonates, alkylpyridinium salts, polyethylene glycol, quaternary ammonium salts, and the like.

[0152] The crosslinking agent may be, for example, melamine, a substituted urea or a polymer crosslinking agent. In an embodiment, it may be a crosslinking agent having at least two crosslinking substituents, such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea or butoxymethylated thiourea.

[0153] In the embodiment, as the crosslinking agent, a crosslinking agent having high heat resistance may be used. The crosslinking agent having high heat resistance may include a compound having a crosslinking substituent having an aromatic ring (eg, a benzene ring or a naphthalene ring) in a molecule.

[0154] In an embodiment, the thermal acid generator may be, for example, an acid compound such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate, salicylic acid, sulfosalicylic acid, citric acid, benzoic acid, hydroxybenzoic acid, naphthoic acid or 2,4,4,6-tetrabromocyclohexadienonone, benzoin tosylate, 2-nitrobenzyl tosylate, or other organic sulfonic acid alkyl esters.

[0155] According to some embodiments, a hard mask layer including a cured product of the foregoing hard mask composition may be provided.

[0156] Hereinafter, a method of forming a pattern using the aforementioned hard mask composition may be described.

[0157] According to some embodiments, the method of forming a pattern may include: providing a material layer on a substrate; applying a hard mask composition including the aforementioned compound and a solvent to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; and etching the exposed portion of the material layer.

[0158] The substrate may be, for example, a silicon wafer, a glass substrate, or a polymer substrate. The material layer may be a material to be finally patterned, such as a metal layer (e.g., an aluminum layer or a copper layer), a semiconductor layer (e.g., a silicon layer), or an insulating layer (e.g., a silicon oxide layer or a silicon nitride layer). The material layer may be formed by a method such as a chemical vapor deposition (CVD) process.

[0159] The hard mask composition may be the same as described above and may be applied by spin coating in solution form. In an embodiment, the coating thickness of the hard mask composition may be, for example, about to about 200,000 angstroms.

[0160] The heat treatment of the hard mask composition may be performed, for example, at about 100° C. to about 1,000° C. for about 10 seconds to about 1 hour. In an embodiment, the heat treatment of the hard mask composition may include a plurality of heat treatment processes, such as a first heat treatment process and a second heat treatment process.

[0161] In an embodiment, heat treatment of the hard mask composition may include, for example, a heat treatment process at about 100° C. to about 1,000° C. for about 10 seconds to about 1 hour, and the heat treatment may be performed, for example, in an atmosphere of air or nitrogen, or an atmosphere having an oxygen concentration of 1 wt % or less.

[0162] In an embodiment, heat treatment of the hard mask composition may include a first heat treatment process, for example, at about 100°C to about 1,000°C, about 100°C to about 800°C, about 100°C to about 500°C, or about 150°C to about 400°C for about 30 seconds to about 1 hour, e.g., about 30 seconds to about 30 minutes, about 30 seconds to about 10 minutes, or about 30 seconds to about 5 minutes.

[0163] In an embodiment, the heat treatment of the hard mask composition may include, for example, a second heat treatment process continuously performed at about 100° C. to about 1,000° C., about 300° C. to about 1,000° C., about 500° C. to about 1,000° C., or about 500° C. to about 600° C. for about 30 seconds to about 1 hour, for example, about 30 seconds to about 30 minutes, about 30 seconds to about 10 minutes, or about 30 seconds to about 5 minutes. In an embodiment, the first heat treatment process and the second heat treatment process may be performed in an air or nitrogen atmosphere, or may be performed in an atmosphere having an oxygen concentration of 1 wt % or less.

[0164] By performing at least one of the steps of heat-treating the hard mask composition at a high temperature, for example, 200° C. or higher, high etching resistance capable of withstanding etching gas and chemical liquid exposed in a subsequent process including an etching process may be exhibited.

[0165] In an embodiment, forming the hard mask layer may include a UV / Vis curing process or a near IR curing process.

[0166] In an embodiment, forming the hard mask layer may include a first heat treatment process, a second heat treatment process, a UV / Vis curing process, or a near IR curing process, or may include two or more processes in succession.

[0167] In an embodiment, the method may further include forming a silicon-containing thin layer on the hard mask layer. The silicon-containing thin layer may include, for example, SiCN, SiOC, SiON, SiOCN, SiC, SiO, SiN, or the like.

[0168] In an embodiment, the method may further include forming a bottom antireflective coating (BARC) on the silicon-containing thin layer or on the hard mask layer before forming the photoresist layer.

[0169] In an embodiment, the exposure of the photoresist layer may be performed using, for example, ArF, KrF, or EUV. After the exposure, a heat treatment may be performed at about 100° C. to about 700° C.

[0170] In an embodiment, the etching process of the exposed portion of the material layer may be performed by a dry etching process using an etching gas, and the etching gas may be, for example, N2 / O2, CHF3, CF4, Cl2, BCl3 or a mixed gas thereof.

[0171] The etched material layer may be formed in a plurality of patterns, and the plurality of patterns may be metal patterns, semiconductor patterns, insulating patterns, or the like, such as different patterns of a semiconductor integrated circuit device.

[0172] The following examples and comparative examples are provided to highlight the features of one or more embodiments, but it should be understood that the examples and comparative examples should not be interpreted as limiting the scope of the embodiments, and the comparative examples should not be interpreted as being outside the scope of the embodiments. In addition, it should be understood that the embodiments are not limited to the specific details described in the examples and comparative examples.

[0173] Synthesis of compounds

[0174] Synthesis Example 1

[0175] 9.94 grams of triphenylamine, 17.37 grams of benzoyl chloride and 132.93 grams of 1,2-dichloroethane were added to a flask to prepare a mixed solution. 19.77 grams of aluminum chloride were slowly added to the mixed solution and stirred for 10 hours at ambient temperature. When the reaction was complete, the reaction mixture was washed with water and concentrated under reduced pressure, and n-hexane was added thereto. The solid produced at this time was filtered out and dried under reduced pressure to obtain an intermediate product A-1 represented by chemical formula A-1.

[0176] [Chemical formula A-1]

[0177]

[0178] In a flask, 25.15 grams of intermediate product A-1 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 10.24 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product A-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, and washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and dried under reduced pressure to obtain compound 1 represented by chemical formula A.

[0179] [Chemical formula A]

[0180]

[0181] Synthesis Example 2

[0182] In a flask, 9.21 grams of triphenylamine, 19.54 grams of 4-methoxybenzoyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. 18.32 grams of aluminum chloride were slowly added to the mixed solution at ambient temperature, and then stirred for 10 hours. When the reaction was complete, the obtained product was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and dried under reduced pressure to obtain an intermediate product B-1 represented by chemical formula B-1.

[0183] [Chemical formula B-1]

[0184]

[0185] In a flask, 13.00 grams of intermediate product B-1, 16.25 grams of 1-dodecyl mercaptan, 6.76 grams of potassium hydroxide and 144.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. The mixed solution was heated to 90 ° C and stirred until the intermediate product B-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain the intermediate product B-2 represented by chemical formula B-2.

[0186] [Chemical formula B-2]

[0187]

[0188] In a flask, 25.15 grams of intermediate product B-2 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 10.24 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product B-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 2 represented by chemical formula B.

[0189] [Chemical formula B]

[0190]

[0191] Synthesis Example 3

[0192] In a flask, 15.49 grams of the intermediate product B-2 of Synthesis Example 2 and 93.74 grams of tetrahydrofuran were added to prepare a mixed solution. 90.77 grams of 27% phenylmagnesium chloride tetrahydrofuran solution was slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product B-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 3 represented by chemical formula C.

[0193] [Chemical formula C]

[0194]

[0195] Synthesis Example 4

[0196] In a flask, 8.78 grams of triphenylamine, 20.82 grams of 2-naphthoyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 17.47 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product D-1 represented by chemical formula D-1.

[0197] [Chemical formula D-1]

[0198]

[0199] In a flask, 26.79 grams of intermediate product D-1 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 8.59 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated and stirred at 60°C until the intermediate product D-1 was completely used up. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 4 represented by chemical formula D.

[0200] [Chemical formula D]

[0201]

[0202] Synthesis Example 5

[0203] In a flask, 7.46 grams of triphenylamine, 24.76 grams of 1-pyrenecarbonyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 14.85 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product E-1 represented by chemical formula E-1.

[0204] [Chemical formula E-1]

[0205]

[0206] In a flask, 28.44 grams of intermediate product E-1 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 6.94 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product E-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 5 represented by chemical formula E.

[0207] [Chemical formula E]

[0208]

[0209] Synthesis Example 6

[0210] In a flask, 10.88 grams of triphenylamine, 26.03 grams of 1-pyrenecarbonyl chloride and 147.70 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 15.38 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product F-1 represented by chemical formula F-1.

[0211] [Chemical formula F-1]

[0212]

[0213] In a flask, 15.11 grams of intermediate product F-1 and 80.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. 4.89 grams of aluminum borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product F-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 6 represented by chemical formula F.

[0214] [Chemical formula F]

[0215]

[0216] Synthesis Example 7

[0217] In a flask, 7.46 grams of triphenylamine, 10.66 grams of N, N-diphenyl-2-naphthylamine, 18.79 grams of 4-methoxybenzoyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 17.62 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product G-1 represented by chemical formula G-1.

[0218] [Chemical formula G-1]

[0219]

[0220] In a flask, 7.46 grams of triphenylamine, 9.27 grams of intermediate product G-1, 18.88 grams of 1-dodecyl mercaptan, 7.85 grams of potassium hydroxide and 144.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. The mixed solution was heated to 90 ° C and then stirred until the intermediate product G-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using a 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product G-2 represented by chemical formula G-2.

[0221] [Chemical formula G-2]

[0222]

[0223] In a flask, 7.46 grams of triphenylamine, 25.20 grams of intermediate product G-2 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 10.18 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product G-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 7 represented by chemical formula G.

[0224] [Chemical formula G]

[0225]

[0226] Synthesis Example 8

[0227] In a flask, 7.46 grams of triphenylamine, 8.71 grams of N, N-diphenyl-2-naphthylamine, 23.98 grams of 1-pyrenecarbonyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 14.38 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product H-1 represented by chemical formula H-1.

[0228] [Chemical formula H-1]

[0229]

[0230] In a flask, 7.46 grams of triphenylamine, 28.73 grams of intermediate product H-1 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 6.65 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C until the intermediate product H-1 was fully reacted. After stirring, the resulting product was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 8.

[0231] [Chemical formula H]

[0232]

[0233] Synthesis Example 9

[0234] In a flask, 15.43 g of tris[4-(2-thienyl)phenyl]amine, 16.33 g of 4-methoxybenzoyl chloride and 132.93 g of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 15.31 g of aluminum chloride was slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. Herein, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product I-1 represented by chemical formula I-1.

[0235] [Chemical Formula I-1]

[0236]

[0237] In a flask, 7.46 grams of triphenylamine, 15.78 grams of intermediate product I-1, 14.28 grams of 1-dodecyl mercaptan, 5.94 grams of potassium hydroxide and 144.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. The mixed solution was heated to 90 ° C and stirred until the intermediate product I-1 was completely used up. After stirring, the resultant was neutralized to pH 7 by using a 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product I-2 represented by chemical formula I-2.

[0238] [Chemical Formula I-2]

[0239]

[0240] In a flask, 26.99 grams of intermediate product I-2 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 8.39 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product I-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 9 represented by chemical formula I.

[0241] [Chemical Formula I]

[0242]

[0243] Synthesis Example 10

[0244] In a flask, 7.46 g of triphenylamine, 12.91 g of tri[4-(2-thienyl)phenyl]amine, 21.35 g of 1-pyrenecarbonyl chloride and 132.93 g of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 12.81 g of aluminum chloride was slowly added at ambient temperature. When the reaction was completed, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. Herein, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product J-1 represented by chemical formula J-1.

[0245] [Chemical formula J-1]

[0246]

[0247] In a flask, 31.35 grams of intermediate product J-1, 24.76 grams of 1-pyrenecarbonyl chloride and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 4.03 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product J-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 10 represented by chemical formula J.

[0248] [Chemical formula J]

[0249]

[0250] Synthesis Example 11

[0251] In a flask, 12.40 grams of N,N,N,N-tetraphenylbenzidine, 7.75 grams of 4-methoxybenzoyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 16.92 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product K-1 represented by chemical formula K-1.

[0252] [Chemical formula K-1]

[0253]

[0254] In a flask, 7.46 grams of triphenylamine, 15.55 grams of intermediate product K-1, 15.35 grams of 1-dodecyl mercaptan, 5.11 grams of potassium hydroxide and 144.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. The mixed solution was heated to 90 ° C and stirred until the intermediate product K-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain the intermediate product K-2 represented by chemical formula K-2.

[0255] [Chemical formula K-2]

[0256]

[0257] In a flask, 26.18 grams of intermediate product K-2 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 9.20 grams of sodium borohydride were added to the mixed solution, and then heated to 60 ° C and stirred until the intermediate product K-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 11 represented by chemical formula K.

[0258] [Chemical formula K]

[0259]

[0260] Synthesis Example 12

[0261] In a flask, 10.23 grams of N,N,N,N-tetraphenylbenzidine, 22.89 grams of 1-pyrenecarbonyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours, while 13.95 grams of aluminum chloride were slowly added thereto at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product L-1 represented by chemical formula L-1.

[0262] [Chemical formula L-1]

[0263]

[0264] In a flask, 31.17 grams of intermediate product L-1 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 4.21 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product L-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 12 represented by chemical formula L.

[0265] [Chemical formula L]

[0266]

[0267] Synthesis Example 13

[0268] In a flask, 10.92 grams of N,N,N,N-tetraphenyl-1,4-phenylenediamine, 18.51 grams of 4-methoxybenzoyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours, while 17.64 grams of aluminum chloride were slowly added thereto at ambient temperature. When the reaction was complete, the obtained product was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product M-1 represented by chemical formula M-1.

[0269] [Chemical formula M-1]

[0270]

[0271] In a flask, 14.87 grams of intermediate product M-1, 15.86 grams of 1-dodecyl mercaptan, 5.27 grams of potassium hydroxide and 144.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. The mixed solution was heated to 90 ° C and stirred until the intermediate product M-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain the intermediate product M-2 represented by chemical formula M-2.

[0272] [Chemical formula M-2]

[0273]

[0274] In a flask, 29.20 grams of intermediate product M-2 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 6.18 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product M-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 13 represented by chemical formula M.

[0275] [Chemical formula M]

[0276]

[0277] Synthesis Example 14

[0278] In a flask, 8.94 grams of N,N,N,N-tetraphenyl-1,4-phenylenediamine, 23.69 grams of 1-pyrenecarbonyl chloride and 132.93 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 14.44 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the obtained product was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product N-1 represented by chemical formula N-1.

[0279] [Chemical formula N-1]

[0280]

[0281] In a flask, 30.96 grams of intermediate product N-1 and 150.84 grams of N-methylpyrrolidone were added to prepare a mixed solution. 14.85 grams of aluminum chloride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product N-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain compound 14 represented by chemical formula N.

[0282] [Chemical formula 14]

[0283]

[0284] Comparative Synthesis Examples

[0285] In a flask, 21.68 grams of terephthaloyl chloride, 49.37 grams of 1-methoxypyrene and 399.89 grams of 1,2-dichloroethane were added to prepare a mixed solution. The mixed solution was stirred for 10 hours while 29.05 grams of aluminum chloride were slowly added at ambient temperature. When the reaction was complete, the resultant was washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain an intermediate product P-1 represented by the chemical formula P-1.

[0286] [Chemical formula P-1]

[0287]

[0288] In a flask, 25.02 grams of intermediate product P-1, 18.88 grams of 1-dodecyl mercaptan, 9.44 grams of potassium hydroxide and 240.00 grams of N-methylpyrrolidone were added to prepare a mixed solution. The mixed solution was heated to 90 ° C and stirred until the intermediate product P-1 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain the intermediate product P-2 represented by chemical formula P-2.

[0289] [Chemical formula P-2]

[0290]

[0291] In a flask, 16.22 grams of intermediate product P-2 and 125.63 grams of N-methylpyrrolidone were added to prepare a mixed solution. 8.67 grams of sodium borohydride were slowly added to the mixed solution at ambient temperature, and then heated to 60 ° C and stirred until the intermediate product P-2 was fully reacted. After stirring, the resultant was neutralized to pH 7 by using 1% hydrochloric acid solution, washed and concentrated under reduced pressure, and n-hexane was added thereto. In this article, the solid produced therein was filtered and then dried under reduced pressure to obtain a compound P represented by chemical formula P.

[0292] [Chemical formula P]

[0293]

[0294] Preparation of hard mask composition

[0295] Examples and Comparative Examples

[0296] Each of the compounds and comparative compounds of Synthesis Examples 1 to 14 and Comparative Synthesis Examples was dissolved in cyclohexanone, and then filtered with a membrane filter having a diameter of 0.1 μm to prepare a hard mask composition in which each compound content was 10.0 wt %.

[0297] Assessment 1: Heat resistance

[0298] Each of the hard mask compositions of Examples 1 to 14 and Comparative Examples was spin-coated on a silicon wafer and then heat-treated on a hot plate at 160°C for 1 minute to form a hard mask layer. The thickness of the hard mask layer was measured by using a film thickness meter manufactured by K-MAC Co., Ltd. Subsequently, the hard mask layer was heat-treated again at 400°C for 2 minutes to re-measure the thickness of the hard mask layer. If the thickness change ratio of the hard mask layer before and after the re-heat treatment at 400°C for 2 minutes is less than 5%, "A" (excellent) is given, if greater than or equal to 5% and less than 10%, "B" (good) is given, and if greater than or equal to 10%, "C" (poor) is given. The results are shown in Table 1.

[0299] (Table 1)

[0300] Heat resistance Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Example 7 A Example 8 A Example 9 A Example 10 A Example 11 A Example 12 A Example 13 A Example 14 A Comparative Example C

[0301] Referring to Table 1, the hard mask layers formed of the compositions of Examples 1 to 14 exhibited a thickness change ratio of less than 5% before and after reheat treatment, and the hard mask layers formed of the compositions according to the comparative examples exhibited a thickness change ratio of greater than or equal to 10% before and after reheat treatment. In other words, the hard mask layers formed of the compositions of Examples 1 to 14 exhibited excellent heat resistance compared to the hard mask layers formed of the compositions according to the comparative examples.

[0302] Assessment 2: Gap Filling Features

[0303] Each of the hard mask compositions of Examples 1 to 14 and the comparative example was spin-coated on a patterned silicon wafer and then heat-treated at 400° C. for 60 seconds to form a hard mask layer. A cross-sectional image of the pattern of the hard mask layer was examined with a field emission scanning electron microscope (FE-SEM) to check whether voids occurred. The results are shown in Table 2.

[0304] (Table 2)

[0305] Is there a gap? Example 1 No gaps appear Example 2 No gaps appear Example 3 No gaps appear Example 4 No gaps appear Example 5 No gaps appear Example 6 No gaps appear Example 7 No gaps appear Example 8 No gaps appear Example 9 No gaps appear Example 10 No gaps appear Example 11 No gaps appear Example 12 No gaps appear Example 13 No gaps appear Example 14 No gaps appear Comparative Example No gaps appear

[0306] Referring to Table 2, voids were not generated in the hard mask layers formed of the hard mask compositions according to Examples 1 to 14, and the gap-fill characteristics of the hard mask layers formed of the hard mask compositions according to Examples were improved.

[0307] Evaluation 3: Flattening Features

[0308] Each of the hard mask compositions of Examples 1 to 14 and the comparative example was spin-coated on a patterned silicon wafer and heat-treated at 400° C. for 60 seconds, and its pattern cross-sectional image was detected by a field emission scanning electron microscope (FE-SEM). The thickness of the hard mask layer shown in the pattern cross-sectional image was measured, which was used to calculate the thickness of the hard mask layer according to the method described in the embodiment of the present invention. Figure 1 The calculation equation for the degree of digital flattening is Figure 1 In the table, h1 refers to the average value of the thickness of the hard mask layer measured at three arbitrary points where no pattern is formed, and h2 refers to the average value of the thickness of the hard mask layer measured at three arbitrary points where a pattern is formed. If the numerical result of the flattening degree is less than 5, "A" (excellent) is given, if it is between 5 and 10, "B" (good) is given, and if it exceeds 10, "C" (poor) is given. The results are shown in Table 3.

[0309] (Table 3)

[0310] Flattening feature Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Example 7 A Example 8 A Example 9 A Example 10 A Example 11 A Example 12 A Example 13 A Example 14 A Comparative Example C

[0311] Referring to Table 3, the hard mask layers formed of the hard mask compositions according to Examples 1 to 14 had excellent planarization degrees, whereas the hard mask layers formed of the composition according to the comparative example had deteriorated planarization degrees.

[0312] Evaluation 4: Etching resistance

[0313] Each of the hard mask compositions of Examples 1 to 14 and Comparative Examples was spin-coated on a silicon wafer, and then heat treated on a hot plate at 160° C. for 1 minute to form a hard mask layer. The hard mask layer was dry-etched for 30 seconds using a CF4 / Ar mixed gas, and then before and after etching, the film thickness meter manufactured by Komei Co., Ltd. was measured relative to the hard mask thickness to calculate the etching rate (bulk etching rate, BER) according to calculation equation 2. Etching resistance was evaluated as the ratio of the etching rate of the hard mask layer formed by the composition according to Examples 1 to 14 to the etching rate of the hard mask layer formed by the composition according to the comparative example. If the ratio is less than 0.95, it is evaluated as "A" (excellent), if it is between 0.95 and less than 1.00, it is evaluated as "B" (good), and if it is 1.00 or more than 1.00, it is evaluated as "C" (poor). The results are shown in Table 4.

[0314] [Calculation equation 2]

[0315] Etching rate (angstroms / second) = (initial film thickness - film thickness after etching) / etching time (seconds)

[0316] (Table 4)

[0317] Etching resistance Example 1 A Example 2 A Example 3 A Example 4 A Example 5 A Example 6 A Example 7 A Example 8 A Example 9 A Example 10 A Example 11 A Example 12 A Example 13 A Example 14 A

[0318] Referring to Table 4, the etch rate of the hard mask layer formed by the compositions according to Examples 1 to 14 was less than 0.95 compared to the etch rate of the hard mask layer formed by the composition according to the comparative example, indicating that the etch resistance of the hard mask layer formed by the compositions according to Examples 1 to 14 was better than that of the hard mask layer formed by the composition according to the comparative example.

[0319] In summary, there is a constant trend in the semiconductor industry to reduce the size of wafers. In response to this, the line width of the patterned resist in photolithography can have a size of tens of nanometers. Therefore, the height of the line width that can withstand the resist pattern can be limited, and there may be situations where the resist may not have sufficient resistance to withstand the etching step. In order to compensate for this, an auxiliary layer called a hard mask layer can be used between the etched material layer and the photoresist layer. This hard mask layer can act as an interlayer for the fine pattern of the photoresist transferred by selective etching. Therefore, it may be necessary for the hard mask layer to have sufficient etching resistance to withstand the etching process during pattern transfer.

[0320] Some hard mask layers may be formed in chemical or physical deposition methods, and may have low economic efficiency due to large-scale equipment and high process costs. Therefore, spin coating techniques for forming hard mask layers have recently been developed. Spin coating techniques may be a process that is easier to perform than conventional methods, and hard mask layers formed therefrom may exhibit more excellent gap filling characteristics and planarization characteristics. However, hard mask layers formed using spin coating techniques may have slightly reduced desired etch resistance. Therefore, it may be desirable for a hard mask composition to be applied to a spin coating technique and to ensure an etch resistance comparable to that of a hard mask layer formed in a chemical or physical deposition method.

[0321] In order to improve the etching resistance of the hard mask layer, research on maximizing the carbon content of the hard mask composition is being conducted. However, when the carbon content of the compound included in the hard mask composition is maximized, the solubility of the compound in the solvent may be reduced. The carbon content of the compound included in the hard mask composition may be maximized to improve the etching resistance of the hard mask layer formed therefrom, while the compound may be sufficiently soluble in the solvent.

[0322] The hard mask composition according to some embodiments may include a compound having an aromatic hydrocarbon group or a heteroaromatic hydrocarbon group, thereby increasing the carbon content of the composition. Therefore, the hard mask layer obtained from the composition can ensure excellent etching resistance. In addition, the compound may include a specific functional group, thereby increasing the carbon content of the composition and ensuring excellent solubility in a solvent.

[0323] One or more embodiments may provide a hard mask composition that may be effectively applied to a hard mask layer.

[0324] One or more embodiments may provide a hard mask layer including a cured product of a hard mask composition.

[0325] One or more embodiments may provide a method of forming a pattern using a hard mask composition.

[0326] The hard mask composition according to some embodiments may have excellent solubility in a solvent and may be effectively applied to a hard mask layer.

[0327] The hard mask composition according to some embodiments may have excellent cross-linking characteristics when cured, and a hard mask layer formed therefrom may ensure excellent heat resistance and excellent etching resistance.

[0328] Example embodiments have been disclosed herein, and although specific terms are employed, the terms are used and interpreted in a generic and descriptive sense only and not for purposes of limitation. In some cases, as would be apparent to one of ordinary skill in the art (as of the time of filing this application), features, characteristics, and / or elements described with respect to a particular embodiment may be used alone or in combination with features, characteristics, and / or elements described with respect to other embodiments, unless specifically noted otherwise. Accordingly, it should be understood by those skilled in the art that various changes in form and details may be made without departing from the spirit and scope of the present invention as set forth in the claims above.

Claims

1. A hard mask composition, include: A compound represented by Chemical Formula 1; and solvent, [Chemical formula 1] Wherein, in Chemical Formula 1, Ar 1 To Ar 3 ,Ar 11 ,Ar 21 and Ar 31 Each is independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a substituted or unsubstituted C3 to C30 heteroaromatic hydrocarbon group, wherein two or more of the aromatic hydrocarbon group, heteroaromatic hydrocarbon group or a combination thereof are linked by a single bond or a substituted or unsubstituted C1 to C10 alkylene group, or a combination thereof, R 1 To R 3 each independently represents hydrogen, deuterium, substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, substituted or unsubstituted C1 to C30 saturated or unsaturated heteroaliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated heteroalicyclic hydrocarbon group, substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, substituted or unsubstituted C4 to C30 heteroaromatic hydrocarbon group, or a combination thereof, R 11 , R 21 and R 31 are each independently hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, n is an integer from 0 to 2, and m is an integer of 1 to 4.

2. The hard mask composition according to claim 1, in: In Chemical Formula 1, Ar 1 To Ar 3 Substituted or unsubstituted groups each independently being part of Group 1: [Group 1] In group 1, R a and R b Each is independently hydrogen, deuterium, substituted or unsubstituted C1-C10 alkyl, or substituted or unsubstituted C6-C20 aryl.

3. The hard mask composition according to claim 1, in: In Chemical Formula 1, Ar 1 To Ar 3 Each independently a substituted or unsubstituted group that is part of Group 1-1: [Group 1-1] In group 1-1, R a and R b Each is independently hydrogen, deuterium, substituted or unsubstituted C1-C10 alkyl, or substituted or unsubstituted C6-C20 aryl.

4. The hard mask composition according to claim 1, wherein in Chemical Formula 1, Ar 11 ,Ar 21 and Ar 31 Each is independently a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group.

5. The hard mask composition according to claim 1, wherein in Chemical Formula 1, Ar 11 ,Ar 21 and Ar 31 Substituted or unsubstituted groups each independently being part of Group 2: [Group 2] 6. The hard mask composition according to claim 1, wherein in Chemical Formula 1, Ar 1 To Ar 3 are each independently a substituted or unsubstituted group of a part of Group 1-2, and Ar 11 ,Ar 21 and Ar 31 Substituted or unsubstituted groups each independently being part of Group 2-1: [Group 1-2] [Group 2-1] 7. The hard mask composition according to claim 1, wherein in Chemical Formula 1, R 1 To R 3 are each independently hydrogen, deuterium, a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, or a combination thereof, and R 11 , R 21 and R 31 Each is independently hydrogen, deuterium or a substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group.

8. The hard mask composition according to claim 1, wherein in Chemical Formula 1, R 1 To R 3 , R 11 , R 21 and R 31 Each is independently hydrogen, deuterium, a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C6 to C20 aromatic hydrocarbon group, or a combination thereof.

9. The hard mask composition according to claim 1, wherein in Chemical Formula 1, Ar 1 with Ar 2 Same, Ar 11 with Ar 21 Same, R 1 With R 2 Same, or R 11 With R 21 same.

10. The hard mask composition according to claim 1, wherein the compound represented by Chemical Formula 1 is represented by one of Chemical Formulas 2 to 15: [Chemical formula 2] [Chemical formula 3] [Chemical formula 4] [Chemical formula 5] [Chemical formula 6] [Chemical formula 7] [Chemical formula 8] [Chemical formula 9] [Chemical formula 10] [Chemical formula 11] [Chemical formula 12] [Chemical formula 13] [Chemical formula 14] [Chemical formula 15] 11 . The hardmask composition of claim 1 , wherein the compound has a molecular weight of 500 to 10,000 g / mol. 12 . The hardmask composition of claim 1 , wherein the compound is included in an amount of 0.1 wt % to 30 wt % based on the total weight of the hardmask composition.

13. The hardmask composition according to claim 1, wherein the solvent comprises propylene glycol, propylene glycol diacetate, methoxypropylene glycol, diethylene glycol, diethylene glycol butyl ether, tri(ethylene glycol) monomethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, cyclohexanone, ethyl lactate, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, methylpyrrolidone, acetylacetone or ethyl 3-ethoxypropionate. 14 . A hard mask layer comprising a cured product of the hard mask composition according to claim 1 .

15. A method for forming a pattern, the method comprising: include: providing a material layer on a substrate; applying the hard mask composition according to claim 1 to the material layer; thermally treating the hard mask composition to form a hard mask layer; forming a photoresist layer on the hard mask layer; exposing and developing the photoresist layer to form a photoresist pattern; selectively removing the hard mask layer using the photoresist pattern to expose a portion of the material layer; as well as The exposed portion of the material layer is etched. 16 . The method of forming a pattern according to claim 15 , wherein forming the hard mask layer comprises performing a heat treatment at 100° C. to 1,000° C.