Negative electrode protection liquid, negative electrode zinc paste and alkaline zinc-manganese battery

By using negative electrode protection liquid containing water, potassium hydroxide, zinc oxide and light liquid paraffin in alkaline zinc-manganese batteries, an oily protective film is formed, which solves the problem of corrosion of zinc alloy electrodes and significantly improves the storage cycle and discharge of the battery. performance.

CN118919723APending Publication Date: 2024-11-08GUANGDONG LIWANG NEW ENERGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410951998.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Zinc alloy electrodes are prone to corrosion under the action of potassium hydroxide, resulting in a shortened service life and a reduced storage cycle of alkaline zinc-manganese batteries.

Method used

A negative electrode protection liquid is used, including water, potassium hydroxide, zinc oxide and light liquid paraffin, to form an oily protective film, reduce the corrosion rate of zinc electrodes and gas production, and improve the electrochemical performance of the battery.

Benefits of technology

The storage cycle and discharge capacity of the battery were significantly improved. After 100 days of storage at 60℃, the discharge capacity of 3.9Ω and 1.5W increased by 7.70% and 12.7%, and the gas analysis volume in 30 days decreased by 33.3% year-on-year.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947485440000071
    Figure BDA0004947485440000071
  • Figure BDA0004947485440000081
    Figure BDA0004947485440000081
  • Figure BDA0004947485440000091
    Figure BDA0004947485440000091
Patent Text Reader

Abstract

The invention provides a negative electrode protection liquid, a negative electrode zinc paste and an alkaline zinc-manganese battery. The negative electrode protection liquid is prepared from the following components in parts by weight: 2500 to 3000 parts of water, 1800 to 2000 parts of potassium hydroxide, 200 to 300 parts of zinc oxide and 2 to 8 parts of light liquid paraffin. Wherein potassium hydroxide can be used as an electrolyte component to promote chemical reaction between the positive electrode and the negative electrode and provide stable voltage and current output; by adding zinc oxide, the capacity and the energy density of the battery can be improved, and meanwhile, the electrochemical activity and the conductivity of the zinc alloy are improved; the light liquid paraffin is insoluble in water and is added into the negative electrode protection liquid, so that the surface of the negative electrode zinc powder can be coated with a layer of oily protection film, the corrosion of the electrolyte to the zinc electrode is reduced, the passivation speed of the zinc electrode and the generation of gassing are slowed down, the reaction of active substances is more lasting, and the storage period of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alkaline batteries, and in particular relates to a negative electrode protection solution, a negative electrode zinc paste and an alkaline zinc-manganese battery. Background Art

[0002] Potassium hydroxide is used as the electrolyte in zinc-manganese batteries. When the battery is in use, potassium hydroxide reacts with the zinc alloy electrode to produce hydrogen and zincate. As the reaction proceeds, the zinc alloy electrode is gradually corroded and passivated by potassium hydroxide, losing its structural integrity and physical properties. At the same time, after zinc is oxidized by potassium hydroxide, the oxygen released forms water molecules, which in turn aggravates the corrosion of the zinc alloy electrode, shortening the battery's service life and reducing the storage cycle.

[0003] Therefore, providing a protective liquid to prevent the zinc alloy electrode from being corroded is a problem that needs to be solved urgently. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a negative electrode protection solution, a negative electrode zinc paste and an alkaline zinc-manganese battery. The negative electrode protection solution has a certain conductivity and is a grease-type protective agent, which can reduce the corrosion of the zinc electrode, slow down the passivation rate of the zinc electrode and the generation of gas evolution.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a negative electrode protection solution, which comprises, by weight: 2500-3000 parts of water, 1800-2000 parts of potassium hydroxide, 200-300 parts of zinc oxide, and 2-8 parts of light liquid paraffin.

[0007] Preferably, the light liquid paraffin has a purity greater than 96%, a boiling point of 280 to 300° C., a melting point of -20 to -24° C., a flash point of 164 to 228° C., and a viscosity of 110 to 230 mPa·s.

[0008] Preferably, the water is deionized water, and the conductivity of the deionized water is less than 5 μS / cm.

[0009] Preferably, the negative electrode protection solution comprises, by weight: 2500-3000 parts of water, 1800-2000 parts of potassium hydroxide, 200-300 parts of zinc oxide, and 2-8 parts of light liquid paraffin.

[0010] In a second aspect, the present invention provides a negative electrode zinc paste, which comprises, by weight, 300 to 400 parts of zinc powder, 1 to 5 parts of a binder, 1 to 6 parts of a dispersant, and 2 to 5 parts of the negative electrode protection solution described in any one of claims 1 to 3.

[0011] Preferably, the binder is selected from polyacrylic acid and / or sodium polyacrylate.

[0012] Preferably, the dispersant is selected from sodium polyacrylate and / or polyacrylic acid.

[0013] Preferably, the zinc powder is alloy zinc powder.

[0014] Preferably, the purity of the alloy zinc powder is ≥99.9%.

[0015] In a third aspect, the present invention provides an alkaline zinc-manganese battery, which includes a positive electrode, a negative electrode, a separator and a steel shell; the negative electrode is made of the above-mentioned negative electrode zinc paste.

[0016] Preferably, the positive electrode comprises electrolytic manganese dioxide, a conductive agent, calcium stearate and potassium hydroxide.

[0017] Preferably, the separator comprises separator paper.

[0018] Preferably, the conductive agent is selected from graphite.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention provides a negative electrode protection liquid, which is a grease-type protective agent, and includes, by weight: 2500-3000 parts of water, 1800-2000 parts of potassium hydroxide, 200-300 parts of zinc oxide, and 2-8 parts of light liquid paraffin. Among them, potassium hydroxide can be used as an electrolyte component to promote the chemical reaction between the positive and negative electrodes and provide stable voltage and current output; zinc oxide can be used as a negative electrode catalyst in alkaline batteries to accelerate the hydroxide ion (OH - ) in the electrolyte, thereby increasing the power and energy density of the battery. In addition, zinc oxide can also be used as an electronic conductor to promote the flow of current inside the battery, reduce the internal resistance of the battery, improve the overall efficiency of the battery, and improve the electrochemical activity and conductivity of the zinc alloy; light liquid paraffin is insoluble in water. When added to the negative electrode protective solution, it can wrap the surface of the negative electrode zinc powder with an oily protective film, reduce the corrosion of the zinc electrode by the KOH electrolyte, slow down the passivation rate of the zinc electrode and the generation of gas evolution, make the active substance reaction more durable, and increase the storage cycle of the battery. In addition, light liquid paraffin can also increase the viscosity of the electrolyte and improve the wettability of the electrolyte, thereby improving the electrochemical performance of the battery.

[0021] After testing, the alkaline zinc-manganese battery with the negative electrode zinc paste made of the above-mentioned negative electrode protective solution as the negative electrode, compared with the alkaline zinc-manganese battery with the negative electrode zinc paste made of no negative electrode protective solution, after being stored at 60°C for 100 days, the 3.9Ω and 1.5W discharge capacities increased by 7.70% and 12.7% respectively, and the 30-day gas evolution volume decreased by 33.3% year-on-year. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Microscope images of corroded zinc alloy and normal zinc alloy;

[0023] Figure 2 This is a microscope image of the zinc alloy in the negative electrode zinc paste in Example 1;

[0024] Figure 3 This is an enlarged microscope image of the zinc alloy in the negative electrode zinc paste in Example 1. DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In view of the problem in the prior art that zinc alloy electrodes are easily corroded, resulting in a shortened battery life and a reduced storage period, the present invention provides a negative electrode protection solution, which comprises, by weight: 2500-3000 parts of water, 1800-2000 parts of potassium hydroxide, 200-300 parts of zinc oxide, and 2-8 parts of light liquid paraffin.

[0027] In the present invention, the negative electrode protection solution includes 2500-3000 parts of water by weight, preferably 2600-2800 parts, and more preferably 2650-2700 parts. The water as a solvent is preferably deionized water, and the conductivity of the deionized water is preferably <5μS / cm, and more preferably <4μS / cm. The present invention has no particular restrictions on the source of water, and it can be a general commercial product.

[0028] In the present invention, the negative electrode protection solution includes 1800 to 2000 parts of potassium hydroxide by weight, preferably 1800 to 1900 parts, and more preferably 1850 to 1880 parts. In the present invention, the potassium hydroxide can be used as a component of the electrolyte to promote the chemical reaction between the positive and negative electrodes and provide stable voltage and current output. Therefore, adding it to the negative electrode protection solution can improve the ionic conductivity and electrochemical performance of the electrolyte. The present invention has no particular restrictions on the source of potassium hydroxide, and it can be a general commercial product.

[0029] In the present invention, the negative electrode protection solution includes 200 to 300 parts by weight of zinc oxide, preferably 220 to 250 parts, and more preferably 230 to 250 parts. The present invention adds zinc oxide to the negative electrode electrolyte, which can improve the capacity and energy density of the prepared alkaline battery, and can also improve the electrochemical activity and conductivity of the zinc alloy. The present invention has no particular restrictions on the source of zinc oxide, and it can be a general commercial product.

[0030] In the present invention, the negative electrode protection solution includes 2 to 8 parts by weight of light liquid paraffin, preferably 3 to 6 parts, and more preferably 4 to 5 parts. In the present invention, the light liquid paraffin is insoluble in water and can act as a protective agent. When added to the negative electrode protection solution, the negative electrode zinc paste prepared can wrap the surface of the negative electrode zinc powder with an oily protective film, thereby reducing the corrosion of the zinc electrode by the KOH electrolyte, slowing down the passivation rate of the zinc electrode and the generation of gas evolution, making the active substance react more persistently, thereby increasing the storage period of the battery. At the same time, the light liquid paraffin can also increase the viscosity of the electrolyte, improve the wettability of the electrolyte, and thus improve the electrochemical performance of the alkaline battery.

[0031] It should be noted that the light liquid paraffin is a colorless, tasteless, odorless oily liquid, a mixture of saturated alkanes, and is liquid at room temperature. It is one of the products after petroleum distillation, and is mainly composed of compounds with carbon atoms within the range of normal alkanes. Liquid paraffin has the following physical and chemical properties:

[0032] (1) Appearance: Colorless transparent liquid

[0033] (2) Density: smaller than water, generally between 0.82 and 0.86 g / cm3;

[0034] (3) Boiling point: relatively high, usually above 300°C;

[0035] (4) Melting point: low, usually below room temperature;

[0036] (5) Flash point: relatively high, usually exceeding 100°C;

[0037] (6) Solubility: insoluble in water, miscible in many organic solvents;

[0038] (7) Stability: Stable at room temperature and not prone to react with other substances;

[0039] (8) High thermal stability: can withstand higher temperatures;

[0040] (9) Low toxicity: Oral toxicity is low, but long-term intake may be harmful;

[0041] (10) Viscosity: The viscosity of liquid paraffin varies with its composition and temperature. It is usually low and has a certain fluidity at a specific temperature.

[0042] The light liquid paraffin in the present invention is stable to light, heat and acid, has a high alkane content, has good oxidation resistance and thermal stability, and has a purity greater than 96%, a boiling point of 280 to 300°C, a melting point of -20 to -24°C, a flash point of 164 to 228°C, and a viscosity of 110 to 230 mPa·s.

[0043] The negative electrode protection liquid provided by the present invention is used to prepare negative electrode zinc paste. Therefore, the present invention also provides a negative electrode zinc paste, which includes 300-380 parts of zinc powder, 1-5 parts of binder, 1-6 parts of dispersant and 2-5 parts of the above-mentioned negative electrode protection liquid in parts by weight; preferably includes 320-350 parts of zinc powder, 2-4 parts of binder, 3-5 parts of dispersant and 3-4 parts of the above-mentioned negative electrode protection liquid.

[0044] In the present invention, the zinc powder is used as the negative electrode material, specifically, alloy zinc powder, wherein the alloy zinc powder is an alloy zinc powder with a zinc alloy purity ≥ 99.9%. In a specific embodiment of the present invention, the zinc powder is selected from C-9 zinc alloy (purity ≥ 99.9%) produced and sold by Ningbo Jinneng New Materials Co., Ltd.

[0045] In the present invention, the binder is used for the negative electrode, which can form a chemical bond with the negative electrode material to enhance the structural stability of the negative electrode material. Specifically, it can be selected from polyacrylic acid and / or sodium polyacrylate, preferably polyacrylic acid.

[0046] In the present invention, the dispersant is used for the negative electrode, which can increase the viscosity of the negative electrode material so that the negative electrode material and the water phase are stably combined together to prevent stratification. Specifically, it can be selected from polyacrylic acid and / or sodium polyacrylate, preferably sodium polyacrylate.

[0047] The present invention also provides a method for preparing the negative electrode zinc paste, comprising the following steps:

[0048] Zinc powder, a binder and a dispersant are mixed to obtain dry powder; the dry powder and a negative electrode protection liquid are mixed evenly, and then vacuum is drawn to remove bubbles to obtain a negative electrode zinc paste.

[0049] Among them, the present invention preferably mixes zinc powder, a binder and a dispersant, and the mixing is carried out in a mixer under stirring conditions, the stirring time is 5 to 10 minutes, and the stirring speed is 40 to 60 r / min to obtain dry powder.

[0050] The negative electrode protection solution is preferably prepared according to the following method: potassium hydroxide is mixed with water, and after the potassium hydroxide is completely dissolved, the mixture is mixed with zinc oxide and light liquid paraffin. The mixing is preferably carried out under stirring conditions, the stirring time is 5 to 10 minutes, the stirring speed is 30 to 50 r / min, and the zinc oxide, light liquid paraffin and potassium hydroxide solution are fully mixed to obtain the negative electrode protection solution.

[0051] Then, according to the present invention, the negative electrode protection liquid is preferably mixed with the dry powder and wet-mixed for 20 to 40 minutes, and the speed of the wet-mixing is 60 to 70 r / min. After the two are fully mixed, vacuum is drawn to remove bubbles to obtain the negative electrode zinc paste.

[0052] It should be noted that in the present invention, the negative electrode protection solution is in a suspended state in the potassium hydroxide solution.

[0053] The present invention also provides an alkaline zinc-manganese battery, which includes a positive electrode, a negative electrode, a separator and a steel shell. The positive electrode includes electrolytic manganese dioxide, a conductive agent, calcium stearate and potassium hydroxide; the negative electrode is made of the negative electrode zinc paste; the separator includes a diaphragm paper (generally commercial products are sufficient); the steel shell is used to load the positive and negative electrode materials of the alkaline zinc-manganese battery, which can be general commercial products.

[0054] After testing, the alkaline zinc-manganese battery with the negative electrode zinc paste made of the above-mentioned negative electrode protective solution as the negative electrode, compared with the alkaline zinc-manganese battery with the negative electrode zinc paste made of no negative electrode protective solution, after being stored at 60°C for 100 days, the 3.9Ω and 1.5W discharge capacities increased by 7.30% and 12.7% respectively, and the 30-day gas evolution volume decreased by 33.3% year-on-year.

[0055] In order to further illustrate the present invention, the following examples are used to provide a detailed description. The polyacrylic acid used in the following examples of the present invention was purchased from Fujian Jinyang Technology Co., Ltd., model PA940; sodium polyacrylate was purchased from Shenzhen Yuhualong Industrial Development Co., Ltd., model DK500; and light liquid paraffin was purchased from Guangzhou Chemical Reagent Factory.

[0056] Example 1

[0057] Weigh 300 kg of zinc alloy, 2520 kg of deionized water, 1800 kg of potassium hydroxide, 175 kg of zinc oxide, 1.2 kg of polyacrylic acid, 1.9 kg of sodium polyacrylate, and 2.0 kg of light liquid paraffin.

[0058] First, put zinc powder, polyacrylic acid and sodium polyacrylate into the mixer for 10 minutes at a stirring speed of 50r / min. Stir evenly to make dry powder. Then prepare the protective liquid with potassium hydroxide, zinc oxide, deionized water and light liquid paraffin. Then put the dry powder and protective liquid into the zinc paste mixer for 30 minutes at a stirring speed of 60r / min. Stir evenly, evacuate, remove bubbles, and put into barrels for later use.

[0059] The present invention uses the surface morphology of the corroded zinc alloy and the normal zinc alloy as a comparison ( Figure 1 ), it can be seen that in the negative electrode zinc paste obtained in Example 1, an oily protective film is formed on the surface of the zinc alloy, thereby slowing down the corrosion of the electrolyte ( Figures 2-3 ).

[0060] Example 2

[0061] Weigh 350 kg of zinc alloy, 2700 kg of deionized water, 1900 kg of potassium hydroxide, 200 kg of zinc oxide, 1.5 kg of polyacrylic acid, 2.1 kg of sodium polyacrylate, and 3.5 kg of light liquid paraffin.

[0062] First, put zinc powder, polyacrylic acid and sodium polyacrylate into the mixer for 10 minutes at a stirring speed of 50r / min. Stir evenly to make dry powder. Then prepare the protective liquid with potassium hydroxide, zinc oxide, deionized water and light liquid paraffin. Then put the dry powder and protective liquid into the zinc paste mixer for 30 minutes at a stirring speed of 60r / min. Stir evenly, evacuate, remove bubbles, and put into barrels for later use.

[0063] Example 3

[0064] Weigh 380 kg of zinc alloy, 2600 kg of deionized water, 1900 kg of potassium hydroxide, 260 kg of zinc oxide, 3.5 kg of polyacrylic acid, 4.0 kg of sodium polyacrylate, and 5.0 kg of light liquid paraffin.

[0065] First, put zinc powder, polyacrylic acid and sodium polyacrylate into the mixer for 10 minutes at a stirring speed of 50r / min. Stir evenly to make dry powder. Then prepare the protective liquid with potassium hydroxide, zinc oxide, deionized water and light liquid paraffin. Then put the dry powder and protective liquid into the zinc paste mixer for 30 minutes at a stirring speed of 60r / min. Stir evenly, evacuate, remove bubbles, and put into barrels for later use.

[0066] The surface of the negative zinc paste prepared in Examples 2 to 3 also has an oily protective film, which will not be illustrated one by one to avoid complexity.

[0067] Comparative Example 1

[0068] Compared with Example 1, the only difference is that the liquid paraffin is replaced by an equal amount of a fluorine-containing active agent, and the other steps and parameters are consistent with those of Example 1.

[0069] Comparative Example 2

[0070] Compared with Example 2, the only difference is that the liquid paraffin is replaced by an equal amount of a fluorine-containing active agent, and the other steps and parameters are consistent with those of Example 2.

[0071] Comparative Example 3

[0072] Compared with Example 3, the only difference is that the liquid paraffin is replaced with an equal amount of a fluorine-containing active agent (purchased from Shengtian Chemical Co., Ltd., Quzhou City, Zhejiang Province), and the remaining steps and parameters are consistent with Example 3.

[0073] Performance Testing

[0074] Test method:

[0075] 1. 3.9Ω continuous discharge test; Testing instrument: DM-3000 three-in-one battery automatic discharge detection system (V4.69); Testing environment: 20±2℃, RH60±15%; Discharge mode: 24h / d; End voltage: 0.800V.

[0076] 2. 1.5w continuous discharge test: Testing instrument: DMP-1 battery constant power discharge analyzer (V2.84); Testing environment: 20±2℃, RH60±15%; Discharge conditions: 10T / h, 24h / d; End voltage: 1.05V.

[0077] 3. Storage at 60℃: Storage instrument: EB-KX-210K incubator; Power supply: 220V; Power: 2KW; Range: room temperature ~ 250℃±2℃; Adjustment accuracy: 0.5℃; Detection environment: -5℃ ~ +30℃, RH≤85%.

[0078] 4. Discharge test, the specific method is shown in Table 1 below:

[0079] Table 1

[0080]

[0081]

[0082] The alkaline battery preparation process is as follows:

[0083] 1. Provide raw materials:

[0084] Electrolytic manganese dioxide; MnO2 content ≥ 92.0%; purchased from Guangxi Huiyuan Manganese Industry Co., Ltd.; graphite powder is high-purity flake graphite, purchased from Qingdao Zhongdong Graphite Co., Ltd.; calcium stearate; Ca content 6.5% to 7.5%; purchased from Dongguan Hanwei Technology Co., Ltd.; potassium hydroxide; KOH content ≥ 90.0%; purchased from Uni-T (Jiangsu) Chemical Co., Ltd.; zinc alloy Zn content ≥ 99.9%, purchased from Ningbo Jinneng New Materials Co., Ltd., model C-9; potassium hydroxide KOH content ≥ 90.0%; purchased from Uni-T (Jiangsu) Chemical Co., Ltd.; zinc oxide ZnO content ≥ 99.7%; purchased from Changzhou Zhiyi Zinc Industry Co., Ltd.; Polyacrylic acid was purchased from Fujian Jinyang Technology Co., Ltd., model PA940; sodium polyacrylate was purchased from Shenzhen Yuhualong Industrial Development Co., Ltd., model DK500; light liquid paraffin; purchased from Guangzhou Chemical Reagent Factory; zinc negative electrode bottom; surface nickel plating thickness ≥0.25um, purchased from Ningbo Yunbo Hardware Co., Ltd.; copper needle; surface indium plating thickness ≥0.1um, purchased from Ningbo Shuangbai Electronics Co., Ltd.; sealing ring, the main material is nylon, purchased from Shanghai Liushi Electronic Technology Co., Ltd.; diaphragm paper, the main material is synthetic fiber; purchased from Wanbang Special Materials Co., Ltd.; steel shell; surface nickel plating thickness ≥0.25um, purchased from Xinxiang Zhixin Electronic Accessories Co., Ltd.

[0085] 2. Preparation process of positive electrode materials:

[0086] 2.1 Put electrolytic manganese dioxide, graphite powder and calcium stearate into a mixer and dry mix them into mixed powder;

[0087] 2.2 Dissolve potassium hydroxide in pure water to make an electrolyte;

[0088] 2.3 Inject the mixed dry powder described in 2.1 into the electrolyte described in 2.2, and wet mix them to prepare a wet mixed powder;

[0089] 2.4 The wet mixed powder described in 2.3 is subjected to processes such as granulation, tableting, and ring making to complete the preparation of the positive electrode material.

[0090] 3. Negative electrode material preparation process:

[0091] Prepared according to the methods of the above examples and comparative examples.

[0092] 4. Current collector preparation process:

[0093] 4.1: Weld the copper needle onto the concave surface of the zinc negative electrode;

[0094] 4.2: The sealing ring is combined with the welded copper needle and zinc negative electrode bottom described in 4.1 to complete the current collector.

[0095] 5. Assemble the battery according to the steps known to those skilled in the art.

[0096] The test results are shown in Tables 2 to 5 below:

[0097] Table 2 Comparison of 60℃ storage for 100 days, 3.9Ω continuous discharge data

[0098]

[0099] Table 3 Comparison of data at 60℃ for 100 days and 1.5W continuous discharge

[0100]

[0101]

[0102] Table 4 Comparison of gas evolution after storage at 60℃ for 30 days

[0103]

[0104] Table 5 Discharge performance comparison

[0105]

[0106] From the data in Tables 2 to 5, it can be seen that the negative electrode zinc paste obtained by using the negative electrode protection solution provided by the present application can be used in alkaline batteries to significantly improve the discharge performance and storage performance of alkaline batteries, and the various discharge times and discharge times are significantly increased compared with the control ratio. Among them, after being stored at 60°C for 100 days, the 3.9Ω and 1.5W discharge capacities increased by 7.30% and 12.7% respectively, and the gas evolution amount after being stored at 60°C for 30 days decreased by 33.3% year-on-year.

[0107] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A negative electrode protection solution, characterized in that: The invention comprises, by weight: 2500-3000 parts of water, 1800-2000 parts of potassium hydroxide, 200-300 parts of zinc oxide and 2-8 parts of light liquid paraffin.

2. The negative electrode protection solution according to claim 1, characterized in that: The light liquid paraffin has a purity greater than 96%, a boiling point of 280 to 300° C., a melting point of -20 to -24° C., a flash point of 164 to 228° C., and a viscosity of 110 to 230 mPa·s; The water is deionized water, and the conductivity of the deionized water is less than 5 μS / cm.

3. The negative electrode protection solution according to claim 1 or 2, characterized in that: The negative electrode protection solution comprises, by weight, 2500 to 3000 parts of water, 1800 to 2000 parts of potassium hydroxide, 200 to 300 parts of zinc oxide, and 2 to 8 parts of light liquid paraffin.

4. A negative electrode zinc paste, characterized in that: The invention comprises, by weight, 300 to 400 parts of zinc powder, 1 to 5 parts of a binder, 1 to 6 parts of a dispersant, and 2 to 5 parts of the negative electrode protection solution according to any one of claims 1 to 3.

5. The negative electrode zinc paste according to claim 4, characterized in that: The binder is selected from polyacrylic acid and / or sodium polyacrylate.

6. The negative electrode zinc paste according to claim 4 or 5, characterized in that: The dispersant is selected from sodium polyacrylate and / or polyacrylic acid.

7. The negative electrode zinc paste according to any one of claims 4 to 6, characterized in that: The zinc powder is alloy zinc powder; The purity of the alloy zinc powder is ≥99.9%.

8. An alkaline zinc-manganese battery, characterized in that: It includes positive electrode, negative electrode, separator and steel shell; The negative electrode is made of the negative electrode zinc paste according to any one of claims 4 to 7.

9. The alkaline zinc-manganese battery according to claim 8, characterized in that: The positive electrode comprises electrolytic manganese dioxide, a conductive agent, calcium stearate and potassium hydroxide; The separator includes separator paper.

10. The alkaline zinc-manganese battery according to claim 8 or 9, characterized in that: The conductive agent is selected from graphite.