Post consumer recovered colored polyethylene compositions, methods of making same, and articles made therefrom

The method for preparing polyethylene color blends solves the problems of benzene pollution and homogeneity in post-consumer recycled plastic materials, and produces high-purity, low-pollution, and color-consistent polyethylene blends suitable for packaging, rotational molding, automobiles, and wire and cable industries.

CN118922286APending Publication Date: 2024-11-08BOREALIS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028997.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-18
Filing Date
2023-03-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing technology, post-consumer recycled plastic materials have problems such as benzene pollution residue, poor homogeneity, inconsistent color, and insufficient mechanical properties, which limit their application in products with odor requirements and injection molding products.

Method used

A method for preparing polyethylene color-mixed blends includes steps such as sieving, near-infrared and optical sorting, aqueous cleaning, and drying, to produce high-purity, low-pollution, and uniformly colored polyethylene blends that meet the requirements of high mechanical properties and low-temperature toughness.

Benefits of technology

It achieves high purity, low pollution, color consistency and excellent mechanical properties in polyethylene blends, and is suitable for packaging, rotational molding, automotive and wire and cable industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051597420000071
    Figure BDA0005051597420000071
  • Figure BDA0005051597420000191
    Figure BDA0005051597420000191
  • Figure BDA0005051597420000192
    Figure BDA0005051597420000192
Patent Text Reader

Abstract

The present invention relates to a polyethylene color blend having: (i) a melt flow rate (ISO 1133, 5.0 kg) of from 0.1 g / 10 min to 10 g / 10 min; 190 DEG C), (ii) a density (ISO 1183) of from 950 kg / m3 to 990kg / m3; (iii) a C2 fraction having a content of at least 95.0 wt.-%, as measured by 13C-NMR of the soluble fraction of d2-tetrachloroethylene; (iv) a homopolymer fraction (HPF) content in the range of 73.0 wt.-% to 91.0 wt.-%, as determined according to the chemical composition analysis by cross fractionation chromatography (CFC); (v) a copolymer fraction (CPF) content in the range of from 10.0 wt.-% to 22.0 wt.-%, as determined according to the chemical composition analysis by cross fractionation chromatography (CFC); (vi) the total content of heavy metals selected from Cr, Cd, Hg and Pb, relative to the total polyethylene blend, which does not exceed 100 ppm, as measured by X-ray fluorescence (XRF); and (vii) a full notch creep test (FNCT) having a failure time of at least 3.0 h, as determined according to 16770-2019 at 50 DEG C and 6.0 MPa in 2 wt.-% Arkopal N100 wherein the polyethylene color blend has a CIELAB color space (L * a * b *) of L * from 30.0 to 73.0; a * from-10 to 25; b * from-5 to 20, as described herein, as measured according to DIN EN ISO 11664-4. The invention also relates to a process for recovering the polyethylene color blend material to obtain the aforementioned blend, and to articles made from the aforementioned polyethylene color blend.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to mixed color polyethylene blends derived from post-consumer recycle (PCR). Background Art

[0002] The challenges of accumulating plastic waste disposal and the corresponding environmental issues have received widespread attention from the public and the industry. Therefore, the recycling of plastic materials has become an important topic, in which plastic waste can be converted into a valuable resource for new plastic products. Therefore, recycling and reusing plastic materials can take into account both environmental and economic aspects.

[0003] Although the recycling of plastic materials has been started as early as the mid-1990s, through the implementation of collection systems that allow plastic materials to be collected and separated from other household waste in a more targeted manner, the reuse of plastic materials originating from plastic waste is still limited. Plastic materials from so-called post-consumer recycling (PCR) usually contain a mixture of different plastics and several contaminating materials. Methods have been developed to further purify plastic materials from post-consumer recycling (PCR).

[0004] Many attempts have been made to purify recycling streams derived from post-consumer plastic waste. Among them are washing, screening, aeration, distillation and other measures. For example, WO2018 / 046578A1 discloses a method for producing polyolefin recyclate from mixed-color polyolefin waste including packaging waste, the method comprising cold washing the waste with water, then washing with an alkaline medium at 60°C, and then flake color sorting to obtain a color-sorted fraction rich in monopolyolefins.

[0005] US 5,767,230A describes a process comprising contacting a PCR polyolefin sheet containing volatile impurities with a heated gas having a superficial velocity sufficient to significantly reduce the volatile impurities (e.g. odor active substances). However, contamination with residual benzene has been a problem to date. The source of residual benzene in post-consumer recyclate remains uncertain, but it poses an obstacle to end uses in areas such as medical packaging, food packaging, etc. Residual amounts, i.e. trace amounts, of benzene pose a particular problem, as odor testing by sniffing experiments is not possible. End uses with certain odor requirements are therefore hindered.

[0006] Another known problem is the moderate homogeneity found in recyclates, which is reflected in surface contamination occurring in injection molded products.

[0007] Therefore, there is still a strong need for recycled materials with properties as close as possible to the original resin. In particular, the present invention aims to provide PE-PCR materials that are superior to existing materials in terms of high product purity with respect to polyethylene content, low contaminant content, brighter grey shades, high color consistency, high homogeneity, improved mechanical properties such as toughness (even at low temperatures), good tensile and impact properties, and good processability. Summary of the invention

[0008] It is an object of the present invention to provide a post-consumer recycled polyethylene composition that addresses the above-mentioned needs and drawbacks.

[0009] These objects are achieved by providing a post-consumer recycled polyethylene composition that addresses the above-mentioned needs and drawbacks.

[0010] Therefore, the present invention provides a polyethylene mixed color blend having

[0011] (i) a melt flow rate of 0.1 g / 10 min to 10 g / 10 min (ISO 1133, 5.0 kg; 190° C.),

[0012] (ii) 950kg / m 3 Up to 990kg / m 3 Density (ISO1183);

[0013] (iii) a C2 fraction having a content of at least 95.0 wt.-%, as measured by 13C-NMR of the d2-tetrachloroethylene soluble fraction;

[0014] (iv) a homopolymer fraction (HPF) content in the range of 73.0 wt.-% to 91.0 wt.-%, determined according to chemical composition analysis by cross fractionation chromatography (CFC); and

[0015] (v) a copolymer fraction (CPF) content in the range of 10.0 wt.-% to 22.0 wt.-%, determined according to chemical composition analysis by cross fractionation chromatography (CFC);

[0016] (vi) a total content of heavy metals selected from Cr, Cd, Hg and Pb, relative to the total polyethylene blend, which does not exceed 100 ppm as measured by X-ray fluorescence (XRF) as described herein; and

[0017] (vii) full notch creep test environmental stress cracking resistance (FNCT) with a time to failure of at least 3.0 h, measured in 2 wt.-% Arkopal N100 at 50°C and 6.0 MPa in accordance with 16770-2019, as described herein;

[0018] The CIELAB color space (L*a*b*) of polyethylene mixed color blends is

[0019] L* from 30.0 to 73.0;

[0020] a* from -10 to 25;

[0021] b* from -5 to 20,

[0022] Measured according to DIN EN ISO 11664-4, as described herein.

[0023] The above object is also achieved by a method for recycling polyethylene mixed color material, the method comprising the following steps:

[0024] a) providing a mixed plastic waste stream (A);

[0025] b) screening the mixed plastic waste stream (A) to produce a screened mixed plastic waste stream (B), wherein the screened mixed plastic waste stream (B) has only items having a longest dimension in the range of 30 mm to 400 mm;

[0026] c) sorting the screened mixed plastic waste stream (B) by one or more sorting systems equipped with near infrared (NIR) and optical sensors, wherein the screened mixed plastic waste stream (B) is sorted at least according to polymer type and color and optionally article form, thereby producing a sorted mixed color polyethylene recycling stream (CM), and the sorted mixed color polyethylene recycling stream (CM) is subjected to step d) and subsequent steps separately;

[0027] d) crushing the classified mixed color polyethylene recycling stream (CM) to form a flake-shaped mixed color polyethylene recycling stream (D);

[0028] e) washing the flaky mixed-color polyethylene recovery stream (D) with a first aqueous washing liquid (W1) without inputting heat energy, thereby producing a first suspended polyethylene recovery stream (E);

[0029] f) removing at least a portion of the first aqueous washing liquid (W1) from the first suspended polyethylene recovery stream (E) to obtain a first washed polyethylene recovery stream (F);

[0030] g) washing the first washed polyethylene recovery stream (F) with a second aqueous washing liquid (W2) to produce a second suspended polyethylene recovery stream (G), wherein sufficient thermal energy is introduced into the second suspended polyethylene recovery stream (G) to provide a temperature in the range of 65° C. to 95° C. during washing;

[0031] h) removing the second aqueous washing liquid (W2) and any material not floating on the surface of the second aqueous washing liquid (W2) from the second suspended polyethylene recovery stream (G) to obtain a second washed polyethylene recovery stream (H);

[0032] i) drying said second washed polyethylene recycling stream (H) thereby obtaining a dry polyethylene recycling stream (I) comprising the polyethylene mixed color blend according to the present invention.

[0033] The polyethylene mixed colorant blend of the present invention can be obtained or can be obtained according to the above method.

[0034] The present invention also provides an article made from the polyethylene mixed color blend of the present invention or obtained according to the above method.

[0035] The present invention also provides the use of the polyethylene mixed color blend of the present invention in packaging applications, rotational molding applications, automotive applications or wire and cable applications. DETAILED DESCRIPTION

[0036] For the purposes of this specification and the claims that follow, the term "recycled stream" is used to refer to materials processed from post-consumer waste, rather than virgin polymers and / or materials. Post-consumer waste refers to objects that have completed at least their first use cycle (or life cycle), i.e., have reached their first use. The term "virgin" refers to newly produced materials and / or objects before their first use, which have not yet been recycled. The term "recycled material" as used herein refers to materials that are reprocessed from post-consumer waste or recycling streams.

[0037] A blend is a mixture of two or more components, at least one of which is a polymer. Typically, a blend can be prepared by mixing two or more components. Suitable mixing procedures are known in the art. If such a blend comprises virgin material, the virgin material is preferably polyethylene, the polyethylene comprising at least 90 wt.-% of a reactor-made polyethylene material and optionally carbon black. Virgin material is a polymer material that has not yet been recycled.

[0038] For the purposes of this specification and the claims that follow, the term "polyethylene mixed color blend" means a polymer material that mainly comprises units derived from ethylene and no other polymer components of any nature. Such other polymer components may be derived, for example, from monomer units derived from: α-olefins, such as propylene, butene, octene, etc.; styrene derivatives, such as vinyl styrene; substituted and unsubstituted acrylic acid esters; substituted and unsubstituted methacrylic acid esters.

[0039] The quantitative 13C{1H}NMR measurements identify the other polymeric materials in the polyethylene mixed color blends. The quantitative 13 In C{1H}NMR measurements, different units in the polymer chain can be distinguished and quantified. These units are ethylene units (C2 units) and units with 3, 4, 6 or 7 carbon atoms. Thus, units with 2 carbon atoms (C2 units) can be distinguished in the NMR spectrum as individual C2 units and continuous C2 units, which indicates that the polymer material contains vinyl polymers. The polyethylene mixed color blend according to the present invention usually includes a small amount of propylene-based polymer components, in particular a small amount of units derived from isotactic polyethylene (iPP), which can be detected by the soluble fraction. 13 The results were determined by C-NMR analysis as described in the Experimental section below.

[0040] The term "C2 fraction" refers to the presence of repeating -[C 2 H 4 ]-unit, such as by quantitative 13 C{ 1 H} measured by NMR spectroscopy, and is repeated here to represent at least two units.

[0041] The C2 fraction can be calculated as

[0042] wt C2馏分 =fC C2总和 *100 / (fC C2总和 +fC PP )

[0043] Here

[0044] f C2总和 =(Iddg–ItwoB4)+(IstarB1*6)+(IstarB2*7)+(ItwoB4*9)+(IthreeB5*10)+((IstarB4plus-ItwoB4-IthreeB5)*7)+(I3s*3)

[0045] and

[0046] f PP =Isαα*3

[0047] Details are given in the experimental section below.

[0048] HDPE, LDPE or LLDPE, homopolymer polyethylene and copolymer polyethylene may be present in the recycled blend of the present invention. Polyethylene can be characterized by analytical separation. A suitable method is chemical composition analysis by cross fractionation chromatography (CFC). The method is described and successfully implemented in Polymer Char, Valencia Technology Par, Gustave Eiffel 8, Paterna E-46980 Valencia, Spain. Chemical composition analysis by cross fractionation chromatography (CFC) can be fractionated into homopolymer fraction (HPF) and copolymer fraction (CPF) and possible iso-PP fraction (IPPF). The homopolymer fraction (HPF) is a fraction that includes polyethylene similar to homopolymer-HDPE. The copolymer fraction (CPF) is a fraction similar to polyethylene HDPE copolymer, but it may also include fractions of LDPE and LLDPE, respectively. The iso-PP fraction (IPPF) includes isotactic polypropylene and is defined as a polymer fraction eluted at 104°C and above. The homopolymer fraction (HPF), the copolymer fraction (CPF) and any iso-PP fraction (IPPF) add up to 100 wt.-%. It goes without saying that 100 wt.-% refers to the material which is soluble in a cross-fractionation chromatography (CFC) experiment.

[0049] Besides the chemical composition analysis by cross fractionation chromatography (CFC), the polyethylene blends of the present invention are characterized in that the content of C2 fraction is at least 95.0 wt.-%, preferably at least 97.0 wt.-%, as determined by the analysis of the d2-tetrachloroethylene soluble fraction. 13 C-NMR measurement. The percentages refer to the d2-tetrachloroethylene soluble fraction used for the NMR experiments. The term "C2 fraction" is equal to the fraction of polymers obtainable from ethylene monomer units, ie not from propylene monomer units.

[0050] The upper limit of the "C2 fraction" is 100 wt.-%.

[0051] Typically, other components may be present in the polyethylene mixed color blend of the present invention, such as fillers, including organic fillers and inorganic fillers, such as talc, chalk, carbon black, and other pigments, such as TiO 2 , as well as paper and cellulose.

[0052] The melt flow rate (ISO 1133, 5.0 kg; 190° C.) of the polyethylene mixed color blend according to the present invention is typically 0.1 g / 10 min to 10 g / 10 min. The melt flow rate can be influenced by diverting post-consumer plastic waste streams, such as but not limited to: originating from extended producer responsibility schemes such as the German DSD, or sorting out a large number of pre-sorted fractions from municipal solid waste and recombining them in an appropriate manner. Preferably, the MFR 5 The range of is 0.5 g / 10 min to 5.0 g / 10 min, more preferably 0.7 g / 10 min to 4.0 g / 10 min, and even more preferably 1.0 g / 10 min to 3.0 g / 10 min.

[0053] The density of the polyethylene mixed color blend according to the present invention is 950 kg / m 3 Up to 990kg / m 3 , preferably 955kg / m 3 Up to 987kg / m 3 , more preferably 957kg / m 3 Up to 985kg / m 3 , measured according to ISO1183.

[0054] The content of C2 fraction in the polyethylene blend according to the invention is at least 95.0 wt.-%, preferably at least 97.0 wt.-%, more preferably at least 98.0 wt.-%, as determined by the d2-tetrachloroethylene soluble fraction. 13 C-NMR measurement.

[0055] Typically, the polyethylene blend according to the invention is a recycled material.

[0056] Typically, recycling properties can be assessed by the presence of one or more of the following:

[0057] (1) Inorganic residue content (measured by TGA) higher than 0.1 wt.-%;

[0058] Or, or in combination

[0059] (2) The content of limonene is 1 mg / m 3 or higher, as measured using a static headspace sampler coupled with gas chromatography and mass spectrometry (HS-GC-MS);

[0060] It will be appreciated that option (2) is preferred.

[0061] It goes without saying that the amount of inorganic residues, gels and limonene should be as low as possible.

[0062] The homopolymer fraction (HPF) content of the polyethylene mixed color blend of the present invention is in the range of 73.0 wt.-% to 91.0 wt.-%, preferably in the range of 75.0 wt.-% to 90.0 wt.-%, more preferably in the range of 77.0 wt.-% to 89.0 wt.-%, even more preferably in the range of 79.0 wt.-% to 88.0 wt.-%, as determined by chemical composition analysis by cross fractionation chromatography (CFC).

[0063] In addition, the copolymer fraction (CPF) content of the polyethylene mixed color blend of the present invention is in the range of 10.0 wt-% to 22.0 wt-%, preferably in the range of 12.0 wt-% to 22.0 wt-%, more preferably in the range of 13.0 wt-% to 21.0 wt-%, and more preferably in the range of 14.0 wt-% to 20.0 wt-%, as determined by chemical composition analysis by cross fractionation chromatography (CFC).

[0064] Furthermore, the total content of heavy metals selected from Cr, Cd, Hg and Pb of the polyethylene mixed color blend of the present invention does not exceed 100 ppm, preferably does not exceed 80 ppm, more preferably does not exceed 50 ppm relative to the total polyethylene blend, as measured by X-ray fluorescence (XRF) as described in the experimental part below.

[0065] The polyethylene mixed color blends of the present invention also exhibit a full notch creep test environmental stress cracking resistance (FNCT) failure time of at least 3.0 h, preferably at least 3.5 h, more preferably at least 4.0 h, and even more preferably at least 5.0 h, as measured in 2 wt% Arkopal N100 at 50°C and 6.0 MPa according to ISO 16770-2019, as described in the experimental part below.

[0066] In addition, the CIELAB color space (L*a*b*) of the polyethylene mixed color blend of the present invention is

[0067] L* from 30.0 to 73.0;

[0068] a* from -10 to 25;

[0069] b* from -5 to 20,

[0070] Measured according to DIN EN ISO 11664-4, as described in the experimental part below.

[0071] Preferably, the CIELAB color space (L*a*b*) is defined as

[0072] L* from 32.0 to 71.0;

[0073] a* from -9 to 23;

[0074] b* ranges from -5 to 18.

[0075] More preferably, the CIELAB color space (L*a*b*) is defined as

[0076] L* from 35.0 to 70.0;

[0077] a* from -7 to 20;

[0078] b* from -5 to 15.

[0079] The polyethylene mixed color blend of the present invention is characterized by having a higher chemical purity than traditional recycled materials, in particular a lower content of C3 units (propylene units), such as isotactic polypropylene (iPP). Preferably, the polyethylene mixed color blend according to the present invention contains units derived from isotactic polypropylene (iPP) in an amount not exceeding 0.1 wt.% to 3.0 wt.%, preferably 0.1 wt.% to 2.5 wt.%, more preferably 0.2 wt.% to 2.0 wt.%, by the soluble fraction. 13 C-NMR analysis was performed as described in the experimental section below.

[0080] The Large Amplitude Oscillatory Shear-Non-Linear Factor (LAOS-NLF) of the polyethylene mixed color blends according to the present invention is preferably in the range of 2.0 to 4.0, measured at 190°C, angular frequency of 0.628 rad / s and strain of 1000%, as described in the experimental part below.

[0081] LAOS-NLF is a rheological measure of the long-chain branching content and is defined as

[0082]

[0083] Here

[0084] G1' is the first order Fourier coefficient

[0085] G3' is the third-order Fourier coefficient

[0086] LAOS–NLF further indicates a nonlinear polymer structure. Higher LAOS-NLF values ​​indicate higher long-chain branching content.

[0087] The polyethylene mixed color blend according to the present invention preferably has a shear thinning factor (STF) value in the range of 30 to 60, more preferably in the range of 32 to 57, even more preferably in the range of 33 to 55, the shear thinning factor (STF) value being defined as the ratio of the complex viscosity eta (0.05) and eta (300) at 190° C. in the frequency range of 0.01 rad / s to 600 rad / s according to ISO 6721-1 and 6721-10, as determined as described in the experimental part below. The shear thinning factor (STF) indicates the processability of the polyethylene material.

[0088] The benzene content of the polyethylene mixed color blends according to the invention is preferably below the detection limit, determined according to static head space chromatography mass spectrometry (HS / GC-MS) at 100°C / 2h, as described in the experimental part below.

[0089] The odor (VDA270-B3) of the polyethylene mixed color blend according to the present invention is preferably 5.0 or lower, more preferably 4.0 or lower. It should be understood that many commercial recycled grades that do not report odor are actually even worse because odor testing according to VDA270 is prohibited due to the presence of problematic substances.

[0090] The Charpy notched impact strength of the polyethylene mixed color blend according to the present invention is preferably at least 5.0 kJ / m 2 , more preferably at least 5.5 kJ / m 2 , even more preferably at least 6.0 kJ / m 2 , measured according to ISO 179-1eA at -20°C on 80 x 10 x 4 mm injection moulded specimens prepared according to EN ISO 1873-2.

[0091] The tensile modulus of the polyethylene mixed color blends according to the invention is preferably in the range of 600 to 1300 MPa, more preferably in the range of 700 to 1200 MPa, measured according to ISO 527-2, as described in the experimental part below.

[0092] The flexural modulus of the polyethylene mixed color blends according to the invention is preferably in the range of 600 to 1300 MPa, more preferably in the range of 700 to 1100 MPa, measured according to ISO 178, as described in the experimental part below.

[0093] The impact strength of the polyethylene mixed color blend according to the present invention in a 1 l bottle drop test at 0°C is preferably at least 3.0 m, more preferably at least 3.5 m, even more preferably at least 4.0 m average drop height, as determined as described in the experimental part below, wherein the production of the bottle is also described in the experimental part below.

[0094] The polyethylene mixed color blend according to the present invention is preferably obtained from post-consumer recycle (PCR), preferably 100% PCR material. Such PCR material is typically obtained from consumer waste streams, such as waste streams originating from traditional collection systems, such as those implemented by the European Union (e.g., Extended Producer Responsibility Scheme, EPR Scheme). PCR material can also be derived from municipal solid waste originating from outside the EPR collection system.

[0095] The raw materials for obtaining the polyethylene mixed color blend according to the present invention can be selected from a wide range of fractions generated from municipal solid waste (MSW, also commonly referred to as residual waste, black box waste) to raw materials based on the Extended Producer Responsibility Program (EPR), such as the ARA402 fraction from AltstoffRecycling in Austria or the DSD 329 fraction from German producer responsibility organizations (such as DSD-Duales System Holding, Interzero, Reclay).

[0096] Preferably, the polyethylene mixed color blend according to the present invention comprises at least 95.0 wt.-%, more preferably at least 96 wt.-%, even more preferably at least 97 wt.-% derived from post-consumer waste.

[0097] The above object can also be achieved by the above method for recycling polyethylene mixed color materials, which comprises steps a) to i). In other words, the polyethylene mixed color blend according to the present invention is preferably obtainable or obtained by the above method or the following preferred method.

[0098] According to step c), the screened mixed plastic waste stream (B) can preferably be further sorted by article form. In this case, an artificial intelligence sorting system (commercially available from, for example, Tomra Systems) can also be used for sorting according to application type (MFR) or specific objects. In the sorting step c), white and natural waste are preferably sorted out, so that essentially only non-white and / or non-natural colored waste remains in one or more sorted mixed color polyethylene recycling streams (CM).

[0099] By the sorting step c), one or more sorted mixed color polyethylene recycling streams (CM) are preferably produced. This can preferably be achieved by removing white and natural polyethylene objects and non-polyethylene objects. In this article, "natural" means that the object has a natural color. This means that essentially no pigment (including carbon black) or colorant (such as dye or ink) is included in the object. On the other hand, "white" means that white pigment is included in the object. The same logic applies to the flake sorting described in step k) below. The term "mixed color" means that a given material contains all colors, except that white and natural colors have been intentionally removed as much as possible.

[0100] In step f), preferably substantially all of the first aqueous wash liquid (W1) is removed from the first suspended polyethylene polyolefin recovery stream (E) to obtain the first washed polyethylene recovery stream (F).

[0101] In step h), the second aqueous cleaning liquid (W2) and any material not floating on the surface of the second aqueous cleaning liquid are preferably removed by a density separation step.

[0102] The method of the present invention may further comprise at least one of the following steps:

[0103] j) separating the dried polyethylene recovery stream (I) obtained in step i) into a light fraction and a heavy fraction polyethylene recovery stream (J);

[0104] k) further classifying the heavy fraction polyethylene recovery stream (J) by one or more optical classifiers with NIR and / or optical sensors, or, in the absence of step j), classifying the dry polyethylene recovery stream (I), classifying the one or more target polyethylenes by removing any flakes containing materials other than the one or more target polyethylenes or flakes of undesirable colors (e.g., black, etc.), to obtain a purified polyethylene recovery stream (K);

[0105] l) melt-extruding, preferably pelletizing, said purified polyethylene recovery stream (K), preferably wherein the additive (Ad) is added in a molten state, to form an extruded, preferably pelletized, recovered polyethylene product (L);

[0106] m) aerating the recycled polyethylene product (L) or, in the absence of step l), aerating the purified polyethylene recycling stream (K) to remove volatile organic compounds, thereby producing an aerated recycled polyethylene product (M), which may be an aerated extruded, preferably granular, recycled polyethylene product (M1), or an aerated recycled polyethylene flake (M2),

[0107] The order of steps l) and m) can be interchanged, so that the purified polyethylene recovery stream (K) is first inflated to form an inflated recycled polyethylene sheet (M2), which is then extruded, preferably with the additive (Ad) added in a molten state, to form an extruded, preferably granular, inflated recycled polyethylene product (M3), which is a polyethylene mixed color blend according to the present invention.

[0108] In step j), the separation is preferably performed by air sieving. The separation can also be performed based on the aerodynamic properties of the particles (eg flakes), for example separating thin, light, flexible flakes from heavy, thick, rigid flakes.

[0109] After the above step j), a screening step j1) may be performed, wherein the dried polyethylene recovery stream (I) is screened to remove fine particles, producing a screened polyethylene recovery stream (J1), which may then be subjected to the above optional step k). In this screening step j1), fine particles having a size of 2.5 mm or less are preferably removed.

[0110] The present invention also relates to an article made of the above polyethylene mixed color blend. Preferably, the polyethylene mixed color blend according to the present invention accounts for at least 85wt.%, more preferably at least 90wt.%, and even more preferably at least 93wt.% of the total composition used to make the article. The remaining components may include additives such as antioxidants, stabilizers, carbon black (optionally in the form of masterbatches), pigments, colorants (such as dyes or inks).

[0111] The article is preferably a bottle or an article for other packaging applications. The blend of the present invention can also be used for rotational molding applications, automotive applications or wire and cable applications. In a preferred aspect, the polyethylene blend according to the present invention accounts for 95wt.-% to 98wt.-% of the total composition for making the article. Preferably, the article is made only of the polyethylene blend according to the present invention and additives. The additive can preferably be selected from the group consisting of UV stabilizers, antioxidants and / or acid scavengers.

[0112] The polyethylene mixed color blend of the present invention can also be blended with at least one virgin polyolefin and / or recycled polyolefin. For example, virgin ethylene homopolymer or copolymer can be blended.

[0113] Measurement method

[0114] The following definitions of terms and measurement methods apply to the above general description of the invention as well as to the following examples, unless otherwise defined.

[0115] a) Melt flow rate

[0116] The melt flow rate (MFR) is determined in accordance with ISO 1133 and is expressed in g / 10 min. The MFR indicates the flowability and therefore also the processability of a polymer. The higher the melt flow rate, the lower the viscosity of the polymer. Here, the MFR is determined at a temperature of 190° C. and under a load of 2.16 kg, 5.0 kg or 21.6 kg.

[0117] b) Density

[0118] Density is determined according to ISO 1183-1.

[0119] c) C2 fraction and general microstructure by NMR spectroscopy, including “continuous C3” and short chain branches

[0120] Quantitative measurements were recorded in solution using a Bruker AVNEO 400 MHz NMR spectrometer. 13 C{ 1 H}NMR spectrum, for 1 H and 13 C operates at 400.15MHz and 100.62MHz respectively. Used at 125℃ 13 C optimized 10mm extended temperature probe, all pneumatics use nitrogen, all pops are recorded. About 200mg of material is dissolved in about 3ml with about 3mg of BHT (2,6-di-tert-butyl-4-methylphenol CAS 128-37-0) and chromium-(III)-acetylacetonate (Cr(acac) 3 1,2-Tetrachloroethane-d 2 (TCE-d 2 ) to obtain a 60 mM solution of the relaxant in the solvent {singh09}. To ensure a homogeneous solution, the NMR tube was further heated in a rotary oven for at least 1 hour after the initial sample preparation in the heating block. After insertion into the magnet, the tube was rotated at 10 Hz. Standard single pulse excitation was employed with no NOEs, using an optimized tip angle, 1 s recycle delay, and a double-layer WALTZ16 decoupling scheme {zhou07,busico07}. A total of 6144 (6k) transient signals were collected per pop.

[0121] Quantitative 13 C{ 1 The H} NMR spectra were processed and integrated, and the relevant quantitative properties were determined from the integration using a proprietary computer program. All chemical shifts were indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. Characteristic signals corresponding to polyethylenes with different short chain branches (B1, B2, B4, B5, B6plus) and polyethylene {randall89, brandolini00} were observed.

[0122] Characteristic signals of polyethylene containing isolated B1 branches (starB1 33.3 ppm), isolated B2 branches (starB2 39.8 ppm), isolated B4 branches (twoB4 23.4 ppm), isolated B5 branches (threeB5 32.8 ppm), all branches longer than 4 carbons (starB4plus 38.3 ppm) and the third carbon from the end of the saturated aliphatic chain (3s 32.2 ppm) were observed. If one or the other structural element was not observable, it was excluded from the equation. The intensity of the combined ethylene backbone methine carbons (dd 30.0 ppm), gamma-carbons (g 29.6 ppm), 4s and threeB4 carbons (which will be compensated later) was taken between 30.9 ppm and 29.3 ppm, excluding Tββ from polyethylene. All mentioned signals were used to quantify the amount of C2 related carbons according to the following equation:

[0123] f C2总和 =(Iddg–ItwoB4)+(IstarB1*6)+(IstarB2*7)+(ItwoB4*9)+(IthreeB5*10)+((IstarB4plus-ItwoB4-IthreeB5)*7)+(I3s*3)

[0124] When characteristic signals corresponding to the presence of polyethylene (PP, continuous C3) were observed at 46.7 ppm, 29.0 ppm, and 22.0 ppm, the Sαα integral at 46.6 ppm was used to quantify the amount of PP-related carbon: fC PP =Isαα*3

[0125] The weight percentages of C2 fraction and polyethylene can be quantified according to the following equations:

[0126] wt C2馏分 =fC C2总和 *100 / (fC C2总和 +fC PP )

[0127] wt PP =fC PP *100 / (fC C2总和 +fC PP )

[0128] Characteristic signals corresponding to various short chain branches were observed and their weight percentages were quantified as the relevant branch would be an alpha olefin, first quantifying the weight fraction of each branch:

[0129] fwtC2=fC C2总和–(IstarB1*3)–(IstarB2*4)–(ItwoB4*6)–(IthreeB5*7)

[0130] fwtC3(separated C3)=IstarB1*3

[0131] fwtC4=IstarB2*4

[0132] fwtC6=ItwoB4*6

[0133] fwtC7=IthreeB5*7

[0134] Normalization of all weight fractions yields the amount of weight percentage of all relevant branches:

[0135] fsum wt%总和 =fwtC2+fwtC3+fwtC4+fwtC6+fwtC7+fC PP

[0136] wtC2 sum = fwtC2*100 / fsum wt%总和

[0137] wtC3 sum = fwtC3*100 / fsum wt%总和

[0138] wtC4 sum = fwtC4*100 / fsum wt%总和

[0139] wtC6 total = fwtC6*100 / fsum wt%总和

[0140] wtC7 sum = fwtC7*100 / fsum wt%总和

[0141] zhou07

[0142] Zhou,Z.,Kuemmerle,R.,Qiu,X.,Redwine,D.,Cong,R.,Taha,A.,Baugh,D.Winniford,B.,J.Mag.Reson.187(2007)225

[0143] busico07

[0144] Busico,V.,Carbonniere,P.,Cipullo,R.,Pellecchia,R.,Severn,J.,Talarico,G.,Macromol.Rapid Commun.2007,28,1128

[0145] singh09

[0146] Singh,G.,Kothari,A.,Gupta,V.,PolymerTesting 285(2009),475

[0147] randall89

[0148] J. Randall, Macromol. Sci., Rev. Macromol. Chem. Phys. 1989, C29, 201.

[0149] brandolini00

[0150] AJBrandolini,DDHills,NMR Spectra ofPolymers and PolymerAdditives,Marcel DekkerInc.,2000c)Crystex analysis,crystalline fraction(CF)and solublefraction(SF)

[0151] d) Cross-fractionation chromatography

[0152] The chemical composition distribution as well as the determination of the molecular weight distribution and the corresponding average molecular weights (Mn, Mw and Mv) at a specific elution temperature (polymer crystallinity in solution) were determined by fully automated cross fractionation chromatography (CFC) as described in Ortin A., Monrabal B., Sancho-Tello J., Macromol. Symp., 2007, 257, 13-28.

[0153] Cross fractionation chromatography (TREF×SEC) was performed using a CFC instrument (PolymerChar, Valencia, Spain). The concentration was monitored using a quad band IR5 infrared detector (PolymerChar, Valencia, Spain). The polymer was dissolved at 160°C for 150 minutes at a concentration of approximately 1 mg / ml.

[0154] To avoid injection of possible gels and polymers (which do not dissolve in TCB at 160°C, such as PET and PA), the weighed samples were loaded into a stainless steel mesh MW 0.077 / D 0.05 mmm.

[0155] After the sample was completely dissolved, a 0.5 ml aliquot was loaded into the TREF column and stabilized for a period of time at 110° C. By using a constant cooling rate of 0.1° C. / min, the polymer crystallized and precipitated when the temperature reached 30° C. The following temperature steps were used for the discontinuous elution procedure: (35, 40, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 103, 106, 109, 112, 115, 117, 119, 121, 123, 125, 127, 130, 135 and 140).

[0156] In the second dimension, GPC analysis used 3PL Olexis columns and 1× Olexis Guard columns from Agilent (Chess Stretton, UK) as stationary phases. 1,2,4-Trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-di-tert-butyl-4-methylphenol) was used as eluent at a constant flow rate of 1 mL / min at 150 °C. The column set was calibrated using universal calibration (according to ISO 16014-2:2003) with at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11500 kg / mol. PS molecular weights were converted to PP molecular weight equivalents using the following Mark Houwink constants.

[0157] K PS =19×10 -3 mL / g,α PS =0.655

[0158] K PP =19×10 -3 mL / g,α PP =0.725

[0159] A third order polynomial fit was used to fit the calibration data. Data processing was performed using the software provided by PolymerChar and the CFC instrument.

[0160] e) Environmental stress crack resistance (FNCT)

[0161] Environmental stress cracking resistance was evaluated by full notch creep test (FNCT). The FNCT failure time was measured at 50°C according to the full notch creep test method (FNCT) ISO 16770-2019, with a notch depth of 1 mm and a specimen size of 6 mm × 6 mm × 90 mm (4 mm x 4 mm). The solvent used was 2 wt% Arkopal N100 in deionized water. Sample preparation was carried out in accordance with ISO16670-2019 (compression molding and annealing).

[0162] The test specimens were compressed at a stress of 6.0 MPa in aqueous solution. For each sample, 3 to 4 specimens were tested. The average time to failure value of all measurements was used to report the time to failure in hours.

[0163] f) Bottle drop test

[0164] 1L bottle with an outer diameter of 90 mm, a wall thickness of 0.6 mm, an overall height of 204 mm, and a cylindrical shell height of 185 mm, produced by extrusion blow molding with a single screw extruder on a B&W machine, using a melt temperature of 190°C and a mold temperature of 15°C as described in WO 2020 / 148319A1.

[0165] A progressive drop test was performed as described in WO 2020 / 148319 A1. Each bottle as defined above was dropped several times from increasing heights in succession. The test was stopped when each bottle broke.

[0166] The drop test was conducted on a 1 L bottle extrusion blow molded as described above. The bottle was filled with water up to the shoulder of the bottle.

[0167] For each test series, at least 12 bottles are required. 4 bottles are dropped simultaneously from a starting height selected according to the following table, where the expected rupture drop height has been determined in a preliminary test or selected empirically:

[0168] Expected rupture drop height (m) 0.3-1-0 1.0-2.5 2.5-5.0 Initial drop height (m) 0.2 0.5 2.0

[0169] Discard the broken bottles and continue the test with the remaining bottles at increasing heights. The step length of the height increase depends on the starting height. When the starting height is below 0.5m, the step length is 0.1m, while when the starting height is equal to or above 0.5m, the step length is 0.25m. Record the break drop height of each bottle and calculate the average break drop height based on the individual values ​​according to the following formula:

[0170] h p =∑(h i ) / n g

[0171] in,

[0172] h p = Average rupture drop height

[0173] h i = Single rupture drop height

[0174] n g = Total number of containers dropped

[0175] g) Tensile modulus and tensile strain at break

[0176] The tensile modulus and tensile strain at break were measured according to ISO 527-2 (crosshead speed = 1 mm / min; test speed 50 mm / min, 23° C.) using injection molded specimens as described in EN ISO 1873-2 (dog bone shape, 4 mm thickness). The measurements were performed after a conditioning time of 96 h for the specimens.

[0177] h) Flexural modulus

[0178] The flexural modulus was determined according to ISO 178 method A (3-point bending test) on 80 mm x 10 mm x 4 mm. According to the standard, a test speed of 2 mm / min and a span length of 16 x thickness were used. The test temperature was 23 ± 2 °C. Injection molding was performed according to ISO 17855-2.

[0179] i) Impact strength (Charpy NIS)

[0180] Impact strength was determined as notched Charpy impact strength (1eA) (non-instrumented, ISO 179-1, 0°C) according to ISO 179-1eA at +23°C and -20°C on 80x10x4 mm injection moulded specimens prepared according to EN ISO 1873-2.

[0181] j) CIELAB color space (L*a*b*)

[0182] In the CIEL*a*b* uniform color space, the color coordinates are: L*—lightness coordinate; a*—red / green coordinate, where +a* represents red and -a* represents green; and b*—yellow / blue coordinate, where +b* represents yellow and -b* represents blue. The L*, a*, and b* coordinate axes define the three-dimensional CIE color space. Standard Konica / Minolta colorimeter CM-3700A.

[0183] k) Heavy metal content

[0184] The contents of heavy metals including Cr, Cd, Hg and Pb were determined by X-ray fluorescence (XRF).

[0185] The instrument used for the XRF measurements was a wavelength dispersive Zetium (2,4 kW) from Malvern Panalytical. The instrument was calibrated using a polyolefin based standard set (i.e. Toxel) from Malvern Panalytical.

[0186] The analysis was performed under vacuum on blocks with a diameter of 40 mm and a thickness of 2 mm.

[0187] This method is used to determine the quantitative content of Cr, Cd, Hg and Pb in polyolefin matrices within the specified range of this standard.

[0188] l) Headspace gas chromatography / mass spectrometry (HS-GC-MS)

[0189] The determination of benzene and limonene is based on the static headspace (HS) method. The analysis uses a HS sampler in combination with a gas chromatograph (GC) and a mass spectrometer (MS) for screening purposes.

[0190] The samples were delivered to the laboratory in sealed aluminized polyethylene (PE) bags. Prior to analysis, the samples were cryogenically ground and portions of 2.000 ± 0.100 g were weighed in 20 ml HS bottles and sealed. For each sample, duplicate determinations were performed.

[0191] 1.1 HS / GC / MS parameters

[0192] HS parameters (Agilent G1888 headspace sampler)

[0193] Bottle equilibration time: 120min (sample), 5min (standard)

[0194] Column box temperature: 100℃ (sample), 200℃ (standard)

[0195] Ring temperature: 110℃(sample), 205℃(standard)

[0196] Transfer line temperature: 120℃ (sample), 210℃ (standard)

[0197] Low vibration

[0198] GC parameters (Agilent 7890AGC system)

[0199] Column: ZB-WAX 7HG-G007-22 (30m×250μm×1μm)

[0200] Carrier gas: Helium 5.0

[0201] Flow rate: 2ml / min

[0202] Split: 5:1

[0203] GC column oven program: 35℃ for 0.1min

[0204] 10℃ / min up to 250℃

[0205] 250℃ for 1min

[0206] MS parameters (Agilent 5975C Inert XLMSD)

[0207] Acquisition Mode: Scan

[0208] Scan parameters:

[0209] Low Quality: 20

[0210] High quality: 200

[0211] Threshold: 10

[0212] Software / data evaluation

[0213] MSD ChemStation E.02.02.1431

[0214] MassHunter GC / MS AcquisitionB.07.05.2479

[0215] AMDIS GC / MS Analysis Version 2.71

[0216] NIST / EPA / NIH Mass Spectral Library (2011 version)

[0217] NIST Mass Spectral Search Program Version 2.0g

[0218] AMDIS deconvolution parameters

[0219] Minimum match factor: 80

[0220] Threshold: Low

[0221] Scan direction: high to low

[0222] Data file format: Agilent file

[0223] Instrument Type: Quadrupole

[0224] Component width: 20

[0225] The difference between adjacent peaks minus 2

[0226] High resolution

[0227] Sensitivity: Very high

[0228] Peak shape requirements: Medium

[0229] Solvent tailing: 91m / z

[0230] Column bleed: 207m / z

[0231] Minimum model peak: 2

[0232] Min. S / N: 10

[0233] Minimum specific peak: 0.5

[0234] · MSD ChemStation Integration Parameters

[0235] Integrator: ChemStation

[0236] Initial area reject: 0

[0237] Initial peak width: 0.005

[0238] Shoulder peak detection: Off

[0239] Initial threshold: 10.5

[0240] In this study, the expression "below the detection limit (<LOD)" describes the situation where the matching factor is below 80 (AMDIS) or the signal-to-noise ratio of the peak in the sample run (Pk-pk S / N = corrected signal / Pk-pk noise, MSD ChemStation signal-to-noise ratio report) is below 3. The results only refer to the measured sample, measurement time, and applied parameters.

[0241] 1.2. Standard Solutions

[0242] For positive identification and comparison with the (lowest) odor detection threshold (ODT), benzene standard and limonene standard were used respectively (see Table 1).

[0243] For HS / GC / MS analysis, 5 μl of various standards were injected into a 20 ml HS vial, sealed and measured.

[0244] Assuming complete evaporation of the standard substance, the concentration of benzene (or limonene in another case) in HSc G is estimated as shown in Table 1.

[0245] Table 1: Calibration Standards and ODT

[0246]

[0247] 1.3 Data Evaluation

[0248] By considering the amount of substance m G and the available HS volume V G to calculate the concentration of the analyte in HSc G (Equation 1).

[0249]

[0250] To estimate the concentration of the analyte in the HS above the polymer sample, the response factor Rf for single-point calibration is required (Equation 2). By integrating the extracted ion chromatogram (EIC), the peak area of the analyte can be obtained. The corresponding target ions are listed in

[0251]

[0252] Calculate the concentration of the analyte in the HS above the polymer sample by multiplying the response factor with the EIC peak area of ​​the sample (Equation 3).

[0253]

[0254] In addition, the odor relevance of the analytes in the HS above the polymer samples was evaluated by the odor activity value (OAV). Comparison is made with the (lowest) odor detection threshold (ODT) found in the literature (Equation 4) [1]. Values ​​greater than 1 indicate a strong association of the analyte with the odor at a given HS temperature.

[0255]

[0257] 1.4 Notes and Limitations

[0258] It has to be taken into account that the ODT of some substances is below the limit of detection (LOD) of the method. Therefore, components below the LOD may be missed, although they are still relevant to the overall odor.

[0259] OAV is based on the assumption that HS parameters are to some extent related to the measurement conditions of the ODT assay. Of course, this is not entirely true, as a temperature setting of 100 °C is not necessarily chosen for such experiments, and is therefore of limited practical value. Nevertheless, this approach can at least indicate the odor relevance of the marker substances being defined.

[0260] Taking into account all mentioned assumptions and limitations, the concentrations and odor activity values ​​determined in the HS above the samples must be regarded only as rough assessments.

[0261] 1.5 References

[0262] [1]Van Gemert LJ, Odour Thresholds: Compilations of odour threshold values ​​in air, water and other media, Utrecht, Oliemans Punter & Partners BV, 2011.

[0263] n) Odor (VDA270-B3)

[0264] VDA 270 is a determination of the odor characteristics of automotive trim materials. In this study, the odor was determined according to VDA 270 (2018) variant B3. Each assessor evaluated the odor of each sample according to the VDA 270 scale after opening the can lid as little as possible. The six-level scale consists of the following levels: Level 1: Imperceptible, Level 2: Perceptible, not disturbing, Level 3: Clearly perceptible, but not disturbing, Level 4: Disturbing, Level 5: Strongly disturbing, Level 6: Unacceptable. The assessors remained calm during the assessment and were not allowed to bias each other by discussing personal results during the test. They were also not allowed to adjust the assessment after testing another sample. For statistical reasons (and as accepted by VDA 270), the assessors had to use the entire step in the assessment. Therefore, the odor level is based on the average of all individual assessments and is rounded to an integer.

[0265] o) Dynamic rheological measurements

[0266] Characterization of polymer melts by dynamic shear measurements complies with ISO standards 6721-1 and 6721-10. Measurements were performed on an Anton Paar MCR501 stress-controlled rotational rheometer equipped with 25 mm parallel plate geometry. Measurements were performed on compression molded plates, using a nitrogen atmosphere and setting the strain in the linear viscoelastic range. Oscillatory shear tests were performed at 190 °C for PE and 200 °C for PP, respectively, using a frequency range of 0.01 rad / s to 600 rad / s with a gap setting of 1.3 mm.

[0267] In dynamic shear experiments, the probe is subjected to uniform deformation under sinusoidally varying shear strain or shear stress (strain and stress controlled modes, respectively). In controlled strain experiments, the probe is subjected to a sinusoidal strain that can be expressed as

[0268] (t) = γ 0 sin(ωt) (1)

[0269] If the applied strain is in the linear viscoelastic range, the resulting sinusoidal stress response can be given by:

[0270] (t) = σ 0 sin(ωt+δ) (2)

[0271] in

[0272] σ 0 and γ 0 are stress amplitude and strain amplitude respectively

[0273] ω is the angular frequency

[0274] δ is the phase shift (loss angle between applied strain and stress response)

[0275] t is the time.

[0276] Dynamic test results are usually expressed by several different rheological functions, namely shear storage modulus G', shear loss modulus G", complex shear modulus G*, complex shear viscosity η*, dynamic shear viscosity η', heterogeneous component of complex shear viscosity η", and loss tangent tanδ, which can be expressed as follows:

[0277]

[0278] G * =G′+iG″[Pa] (5)

[0279] η * =η′-iη″[Pa.s] (6)

[0280]

[0281] The so-called shear thinning factor (STF) is determined as described in Equation 9.

[0282]

[0283] These values ​​were determined by a one-point interpolation procedure as defined in the Rheoplus software. In cases where a given G* value was not experimentally reached, this value was determined by extrapolation to 10 using the same procedure as before. In both cases (interpolation or extrapolation), the options "-Interpolate y values ​​to x values ​​from parameters" and "Logarithmic interpolation type" from Rheoplus were used.

[0284] The tests were performed on compression-molded discs made from cryogenically ground powders.

[0285] p) LAOS nonlinear viscoelastic ratio

[0286] The nonlinear viscoelastic behavior under shear flow has been investigated with the aid of large-amplitude oscillatory shear. The method requires a sinusoidal strain amplitude γ0 applied for a given time t at a given angular frequency ω. As long as the applied sinusoidal strain is high enough, a nonlinear response will occur. In this case, the stress σ is a 20 function of the applied strain amplitude, time, and angular frequency. Under these conditions, the nonlinear stress response is still a periodic function; however, it can no longer be represented by a single harmonic sine wave. The stress [0-0] resulting from the nonlinear viscoelastic response can be represented by a Fourier series, which includes higher harmonic contributions:

[0287] σ(t,ω,γ 0 )=γ 0 .∑ n [G′ n (ω,γ 0).sin(nωt)+G″ n (ω,γ 0 ).cos(nωt)]

[0288] Where, σ-stress response

[0289] t-time

[0290] ω-Frequency

[0291] γ0-strain amplitude

[0292] n - number of harmonics

[0293] G′ n -nth order elastic Fourier coefficient

[0294] G″ n -nth order viscosity Fourier coefficient

[0295] The nonlinear viscoelastic response was analyzed using large amplitude oscillatory shear (LAOS) [4-6]. Time sweep measurements were performed on an RPA 2000 rheometer from Alpha Technologies equipped with a standard double cone die. During the measurements, the test chamber was sealed and a pressure of approximately 6 MPa was applied. LAOS tests were performed using a temperature of 190°C, an angular frequency of 0.628 rad / s and a strain of 1000%. To ensure that steady-state conditions were achieved, the nonlinear response was determined only after at least 20 cycles had been completed for each measurement. The large amplitude oscillatory shear nonlinear factor (LAOS NLF) is defined as:

[0296]

[0297] Where G′1-first order Fourier coefficient

[0298] G'3 - third order Fourier coefficient

[0299] The tests were performed on cryogenically ground powders.

[0300] [1]JMDealy, KFWissbrun, Melt Rheology and Its Role in PlasticsProcessing: Theory and Applications; edited by Van Nostrand Reinhold, New York (1990)

[0301] [2]S.Filipe, Non-Linear Rheology of Polymer Melts, AIP Conference Proceedings 1152, pp.168-174(2009)

[0302] [3]M.Wilhelm, Macromol.Mat.Eng.287, 83-105(2002)

[0303] [4]S.Filipe, K.Hofstadler, K.Klimke, A.T.Tran, Non-Linear Rheological Parameters for Characterisation of Molecular Structural Properties in Polyolefins, Proceedings of Annual European Rheology Conference, 135(2010)

[0304] [5]S.Filipe, K.Klimke, A.T.Tran, J.Reussner, Proceedings of Novel Non-Linear Rheological Parameters for Molecular Structural Characterisation of Polyolefins, Novel Trends in Rheology IV, Zlin, Check Republik(2011)

[0305] [6]K.Klimke, S.Filipe, A.T.Tran, Non-linear rheological parameters for characterization of molecular structural properties in polyolefins, Proceedings of European Polymer Conference, Granada, Spain(2011)

[0306] q) Inorganic residues

[0307] Inorganic residues were measured by TGA using a Perkin Elmer TGA 8000 according to DIN ISO 1172:1996. About 10-20 mg of material was placed in a platinum pan. The temperature was equilibrated at 50°C for 10 minutes and then raised to 950°C at a heating rate of 20°C / min under nitrogen. The ash content was calculated as weight percent at 850°C.

[0308] Example

[0309] The raw material for IE1 is mixed plastic fractions sorted from municipal solid waste (MSW) in Greece and Poland.

[0310] The feedstock for IE2 is polyethylene sorted from post-consumer waste (PCW) multilayer milk bottle feedstock commercially available on the French and Swiss markets.

[0311] CE1 is a commercial product of HDPE recyclate. It is based on a feedstock of post-consumer waste (PCW), which mainly consists of pre-sorted community waste.

[0312] A HDPE mixed recyclate of IE1 and IE2 composition is obtained by a recycling method, the method comprising the following steps:

[0313] a) providing the post-consumer plastic waste fraction (as described above) in bale form;

[0314] b) screening the material to remove the undersized fraction (and, if necessary, the oversized fraction),

[0315] c) White and clear / natural colors (e.g. white bottles, clear shampoo bottles, yogurt cups) are sorted out through a color sorting step, and other polymer types (PP, PS, PA) as well as contaminants (e.g. paper, wood, etc.) are sorted out through near infrared (NIR) and optical sensors.

[0316] d) grinding the remaining fraction consisting of colored HDPE objects, washing with various detergents in an alkaline aqueous solution, and then drying, air separation and screening;

[0317] e) further sorting the resulting plastic flake material to eliminate non-polyolefin flakes;

[0318] f) Extruding the material and obtaining the HDPE blend according to the invention in the form of pellets.

[0319] The properties of the resulting recycled polyethylene mixed color blend are shown in Table 1 below.

[0320] Table 1

[0321]

[0322]

[0323]

[0324]

[0325] nd - not determined

[0326] Using the above IE1, IE2 and CE1 samples, environmental stress crack resistance according to FNCT was performed in 2 wt% Arkopal N100 at 50°C and 6.0 MPa according to ISO 16770-2019, and impact strength was performed according to the bottle drop test described in the experimental part. The results are shown in Table 2 below.

[0327] Table 2

[0328]

[0329] The above results show that the polyethylene mixed color blends according to IE1 and IE2 have been improved in various properties, reaching commercial recyclates, such as:

[0330] - rHDPE mixed recyclates of (very) high purity (low iPP content);

[0331] - Benzene was not detected by HS GC-MS;

[0332] - Heavy metal (Cr, Cd, Pb, Hg) pollution level is (very) low;

[0333] - Good toughness properties, even at low temperatures (Charpy notched impact strength);

[0334] - The mechanical properties of the bottle are good (e.g. bottle drop test).

[0335] - Better environmental stress crack resistance (FNCT).

[0336] The iPP content of IE1 is only 0.8 wt.-%, indicating an improvement in chemical purity, while the impurity content of the conventional recyclate according to CE1 is 12.1 wt.-%. At the same time, both examples IE1 and IE2 have low heavy metal levels and benzene content below the detection limit, while CE1 does not meet this requirement.

[0337] The mixed color blends according to IE1 and IE2 have further improvements in mechanical properties over the blends according to CE1. Both inventive examples show excellent Charpy notched impact strength (Table 1), excellent ESCR (FNCT) and toughness in the bottle drop test (Table 2).

Claims

1. A polyethylene mixed color blend having: (i) a melt flow rate of 0.1 g / 10 min to 10 g / 10 min (ISO 1133, 5.0 kg; 190° C.), (ii) 950kg / m 3 Up to 990kg / m 3 Density (ISO1183); (iii) a C2 fraction containing at least 95.0 wt.-%, e.g. 13 C-NMR measurement; (iv) a homopolymer fraction (HPF) content in the range of 73.0 wt.-% to 91.0 wt.-%, determined according to chemical composition analysis by cross fractionation chromatography (CFC); and (v) a copolymer fraction (CPF) content in the range of 10.0 wt.-% to 22.0 wt.-%, determined according to chemical composition analysis by cross fractionation chromatography (CFC); (vi) a total content of heavy metals selected from Cr, Cd, Hg and Pb, relative to the total polyethylene blend, which does not exceed 100 ppm as measured by X-ray fluorescence (XRF) as described herein; and (vii) Full Notch Creep Test (FNCT) with a time to failure of at least 3.0 h, measured in 2 wt.-% Arkopal N100 at 50°C and 6.0 MPa according to 16770-2019, as described herein; The CIELAB color space (L*a*b*) of the polyethylene mixed color blend is L* from 30.0 to 73.0; a* from -10 to 25; b* from -5 to 20, Measured according to DIN EN ISO 11664-4, as described herein.

2. The polyethylene mixed color blend according to claim 1, which has units derived from isotactic polypropylene (iPP) in an amount of 0.1 wt.% to 3.0 wt.%, through the soluble fraction 13 C-NMR analysis was performed as described herein.

3. The polyethylene mixed color blend according to any one of the preceding claims, having a Large Amplitude Oscillatory Shear-Non-Linear Factor (LAOS-NLF) in the range of 2.0 to 4.0, measured at 190°C, an angular frequency of 0.628 rad / s and a strain of 1000%, as described herein: Here G1' is the first-order Fourier coefficient G3' is the third-order Fourier coefficient.

4. The polyethylene mixed color blend according to any one of the preceding claims, having a shear thinning factor (STF) value in the range of 30 to 60, wherein the shear thinning factor (STF) value is defined as the ratio of the complex viscosity eta (0.05) and eta (300) in the frequency range of 0.01 rad / s to 600 rad / s at 190°C according to ISO 6721-1 and 6721-10, determined as described herein.

5. A polyethylene mixed color blend according to any one of the preceding claims having a benzene content below the detection limit as determined by static head space chromatography mass spectrometry (HS / GC-MS) at 100°C / 2h as described herein.

6. The polyethylene mixed color blend according to any one of the preceding claims, having a Charpy notched impact strength of at least 5.0 kJ / m 2 , measured according to ISO 179-1eA at -20°C on 80 x 10 x 4 mm injection moulded specimens prepared according to EN ISO 1873-2.

7. A polyethylene mixed color blend as claimed in any preceding claim having an impact strength of at least 3.0 m average drop height at 0°C in the 1 L bottle drop test as described herein, wherein the bottle is produced as described herein.

8. A method for recycling polyethylene mixed color material, the method comprising the following steps: a) providing a mixed plastic waste stream (A); b) screening the mixed plastic waste stream (A) to produce a screened mixed plastic waste stream (B), wherein the screened mixed plastic waste stream (B) has only items having a longest dimension in the range of 30 mm to 400 mm; c) sorting the screened mixed plastic waste stream (B) by one or more sorting systems equipped with near infrared (NIR) and optical sensors, wherein the screened mixed plastic waste stream (B) is sorted at least according to polymer type and color and optionally article form, thereby producing a sorted mixed color polyethylene recycling stream (CM), and the sorted mixed color polyethylene recycling stream (CM) is subjected to step d) and subsequent steps separately; d) crushing the classified mixed color polyethylene recycling stream (CM) to form a flake-shaped mixed color polyethylene recycling stream (D); e) washing the flaky mixed-color polyethylene recovery stream (D) with a first aqueous washing liquid (W1) without inputting heat energy, thereby producing a first suspended polyethylene recovery stream (E); f) removing at least a portion of the first aqueous washing liquid (W1) from the first suspended polyethylene recovery stream (E) to obtain a first washed polyethylene recovery stream (F); g) washing the first washed polyethylene recovery stream (F) with a second aqueous washing liquid (W2) to produce a second suspended polyethylene recovery stream (G), wherein sufficient thermal energy is introduced into the second suspended polyethylene recovery stream (G) to provide a temperature in the range of 65° C. to 95° C. during washing; h) removing the second aqueous washing liquid (W2) and any material not floating on the surface of the second aqueous washing liquid (W2) from the second suspended polyethylene recovery stream (G) to obtain a second washed polyethylene recovery stream (H); i) drying said second washed polyethylene recovery stream (H) thereby obtaining a dried polyethylene recovery stream (I) comprising the polyethylene mixed color blend according to any one of the preceding claims.

9. The method according to claim 8, further comprising at least one of the following steps: j) separating the dried polyethylene recovery stream (I) obtained in step i) into a light fraction and a heavy fraction polyethylene recovery stream (J); k) further classifying the heavy fraction polyethylene recovery stream (J) by one or more optical classifiers, or, in the absence of step j), classifying the dry polyethylene recovery stream (I), classifying the one or more target polyethylenes by removing any flakes containing materials other than the one or more target polyethylenes, to obtain a purified polyethylene recovery stream (K); l) melt-extruding, preferably pelletizing, said purified polyethylene recovery stream (K), preferably wherein the additive (Ad) is added in a molten state, to form an extruded, preferably pelletized, recovered polyethylene product (L); and m) aerating the recycled polyethylene product (L) or, in the absence of step l), the purified polyethylene recycling stream (K) to remove volatile organic compounds, thereby producing an aerated recycled polyethylene product (M), which is an aerated extruded, preferably granular recycled polyethylene product (M1), or an aerated recycled polyethylene flake (M2), in, The order of steps l) and m) can be interchanged so that the purified polyethylene recovery stream (K) is first aerated to form an aerated recycled polyethylene sheet (M2), which is then extruded, preferably with the additive (Ad) added in a molten state, to form an extruded, preferably granular, aerated recycled polyethylene product (M3), which is a polyethylene mixed color blend according to any one of the preceding claims 1 to 7.

10. The polyethylene mixed color blend according to any one of the preceding claims 1 to 7, obtainable by or obtained according to the process of claim 8 or 9.

11. An article made from the polyethylene mixed color blend according to any one of claims 1 to 7 or 10.

12. The article according to claim 11 which is a bottle.

13. A blend comprising the polyethylene mixed color blend according to any one of claims 1 to 7 or 10 and at least one virgin polyolefin and / or recycled polyolefin.

14. Use of the polyethylene mixed color blend according to any one of claims 1 to 7 or 10 for packaging applications, rotomolding applications, automotive applications or wire and cable applications.