Multilayer crystallizable shrinkable films and sheets

By using specific polyester compositions and recycled PET in multilayer films, the existing crystallizable films have been solved, and the low starting shrinkage temperature and recycled material are achieved. The shrinkage control characteristics improve the toughness of the membrane and the recycling performance of PET bottles.

CN118922305APending Publication Date: 2024-11-08EASTMAN CHEM CO
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202380027807.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When used in hot air tunnels, the existing crystallizable films are prone to high initial shrinkage temperature and high shrinkage rate, resulting in loose and wrinkle labels when labeling on HDPE containers, and the film properties containing recycled materials are poor, affecting the PET bottle sheets. Recycling process.

Method used

Polyester compositions using a multi-layer crystallizable film of specific composition, including terephthalic acid residues, ethylene glycol residues and other glycol residues, designed as an amorphous but crystallizable structure for making multi-layered Layer the film, ensuring low initial shrinkage temperature and controlled shrinkage characteristics, and adding recycled PET to the core layer to improve the recyclability of the film.

Benefits of technology

The toughness and shrinkage force of the film under high temperature conditions is achieved, and the label is avoided loosening and wrinkled, while the shrinkage characteristics of the film containing the recycled material and the recirculation performance of the PET bottle sheet are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043177430000401
    Figure BDA0005043177430000401
  • Figure BDA0005043177430000402
    Figure BDA0005043177430000402
  • Figure BDA0005043177430000403
    Figure BDA0005043177430000403
Patent Text Reader

Abstract

Multi-layer crystallizable heat-shrinkable films and sheets comprising an amorphous copolyester composition and a crystallizable copolyester composition having certain advantages and improved properties, including recyclability, the composition comprising terephthalic acid residues, neopentyl glycol (NPG) residues, 1, 3, 4-trimethyl-1, 3-pentanediol residues, 1, 3, 4-trimethyl-1, 3-pentanediol residues, 1, 3, 4-trimethyl-1, 3-pentanediol residues, 1, 3, 4-trimethyl-1, 3-pentanediol residues, 1, 3, 4-trimethyl-1, 3- The present invention relates to a composition comprising 1, 4-cyclohexanedimethanol (CHDM) residues, ethylene glycol (EG) residues, and diethylene glycol (DEG) residues and comprising recycled PET.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The present disclosure relates to multi-layer crystallizable shrinkable films and / or sheets comprising an amorphous copolyester composition and a crystallizable copolyester composition having certain advantages and improved properties, including recyclability, wherein the composition comprises terephthalic acid residues, neopentyl glycol (NPG) residues, 1,4-cyclohexanedimethanol (CHDM) residues, ethylene glycol (EG) residues, and diethylene glycol (DEG) residues within a specific composition range and comprises recycled PET. Background of the Invention

[0003] There is a commercial need for multilayer shrink films having at least one of the following desirable shrink film properties: (1) a low initial shrink temperature, (2) a shrinkage percentage that increases gradually and in a controlled manner with increasing temperature over the temperature range in which shrinkage occurs, (3) a shrink force that is sufficiently low to prevent crushing of an underlying container, (4) a high ultimate shrinkage (shrinkage at maximum temperature), such as 50% or more in the principal shrink direction at 95°C, (5) a low shrinkage in a direction perpendicular to the direction of high shrinkage, (6) improved film toughness to prevent unwanted film cracking, rupture, tearing, splitting, blistering or wrinkling during the manufacturing process and before and after shrinking, (7) made from recycle content, and (8) recyclability. SUMMARY OF THE INVENTION

[0005] It has been found that certain combinations of diol monomers in shrink film resin compositions can be made into multilayer films that have good shrink film properties and can also be crystallized so that they do not negatively affect the recycling of PET bottle flakes during the recycling process. These multilayer crystallizable shrink films can be processed with PET bottles and eventually become components in recyclable PET bottle flakes that leave the recycling process. It has also been found that the selection and amount of a specific combination of diol monomers are important for producing multilayer films with good shrink film properties and producing crystallizable multilayer films. The optimized polyester resin compositions and blends disclosed herein are amorphous but crystallizable. Therefore, they exhibit good properties in film applications including as shrink films, but they have a high strain-induced crystallization melting point, so they provide compatibility in the recycling process. The multilayer shrink film labels disclosed herein do not have to be removed during the recycling process, and they do not affect the process.

[0006] In the past, some crystallizable films may present processing challenges. In some cases, crystallizable films may exhibit high onset shrink temperatures and high shrinkage rates. Due to these characteristics, crystallizable films are often incompatible in some applications; for example, labeling HDPE containers in a hot air tunnel. The high onset shrink temperature prevents the crystallizable film from shrinking before the HDPE container expands, and the label may loosen after the bottle leaves the shrink tunnel. In addition, the high shrinkage rate often causes wrinkles during the shrinking process in the hot air tunnel.

[0007] In other cases, crystallizable films may have high shrinkage. Therefore, if they are used as container labels in an application, the high shrinkage may cause wrinkles in the film and distort the shape of the container, depending on its design, especially in applications with thin bottles or bottles with differential modulus. The multilayer crystallizable films of the present disclosure provide solutions to these processing challenges of high onset shrinkage temperature and high shrinkage.

[0008] The multilayer crystallizable films of the present disclosure also address some sustainability issues and the desire to incorporate recycled materials into heat shrink films. Recycled PET (rPET) is directly incorporated into the multilayer crystallizable films of the present disclosure. In the past, films containing large amounts of rPET material tended to have inferior film properties compared to films without any rPET. However, in the present disclosure, optimized blending ratios and multilayer constructions provide the benefits of including rPET and including crystallizable resins. Even with the inclusion of rPET, the multilayer crystallizable films of the present disclosure have improved shrink properties, and they are also compatible with PET recycle streams.

[0009] Furthermore, the multi-layer crystallizable films of the present disclosure provide additional advantages such as lower shrink forces and incorporation of rPET without affecting other properties.

[0010] Multilayer films must meet various suitability criteria to be used in this application. The multilayer films must be strong, must shrink in a controlled manner, and must provide sufficient shrink force to hold themselves to the bottle without crushing the contents. In addition, when these labels are applied to polyester containers, the multilayer polyester shrink film labels must not interfere with the recycling process of the bottles. The multilayer shrink films of the present disclosure are advantageous because the labels can be recycled with the bottles or containers. Thus, the entire bottle, including the label, can be recycled and converted into new products without incurring additional handling requirements or creating new environmental issues. Heat shrinkable films have been made from a variety of raw materials to meet a range of material requirements. The present disclosure describes unique and unexpected effects measured with certain monomer combinations for shrink film resin compositions.

[0011] Polyester shrink film compositions have been used commercially as shrink film labels for food, beverages, personal care, household products, and the like. Typically, these shrink films are used in combination with clear polyethylene terephthalate (PET) bottles or containers. The entire package (bottle plus label) is then put into the recycling process. In a typical recycling center, the PET and shrink film materials are usually finally combined together at the end of the process due to the similarity in composition and density. The PET bottle flakes need to be dried to remove residual water left in the PET by the recycling process. Typically, PET is dried at temperatures above 150°C, and in some cases above 200°C. At these temperatures, typical polyester shrink film resins soften and become sticky, often forming lumps with the PET bottle flakes. These lumps must be removed before further processing. These lumps reduce the yield of PET bottle flakes from the process and result in additional operating steps.

[0012] It has also been found that certain combinations of diol monomers in film or sheet resin compositions can be made into films or sheets that have good performance properties and can also be crystallized so that they do not affect the recycling of PET bottle flakes. These crystallizable film or sheet resins can be processed with recycled PET and eventually become components in recyclable PET bottle flakes that leave the recycling process. It has also been found that the selection and amount of a specific combination of diol monomers are important for producing films or sheets with good performance properties and producing crystallizable films or sheets. The optimized polyester resin compositions of the present disclosure are amorphous but crystallizable. Therefore, they exhibit good properties in film or sheet applications, including as molded, thermoformed or formed parts and / or articles, but they have a high strain-induced crystallization melting point, so they can be recycled with PET. The films or sheets of the present disclosure do not have to be removed during the recycling process, and they do not affect the recycling process.

[0013] One embodiment of the present disclosure is a multilayer crystallizable film comprising at least one skin layer (A), the skin layer (A) comprising a polyester composition comprising: at least one polyester comprising:

[0014] (a) a dicarboxylic acid component comprising:

[0015] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0016] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0017] (b) a diol component comprising:

[0018] About 75 mol % or more of ethylene glycol residues and

[0019] About 25 mole % or less of other diols, the other diols comprising one or more of:

[0020] (i) from about 0 to less than about 24 mole percent neopentyl glycol residues;

[0021] (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues;

[0022] (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0023] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0024] At least one core layer (B), said core layer (B) comprising a blend of:

[0025] 30 to 95 weight percent of at least one polyester composition comprising:

[0026] At least one polyester comprising:

[0027] (a) a dicarboxylic acid component comprising:

[0028] (i) from about 90 to about 100 mole percent terephthalic acid residues;

[0029] (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0030] (b) a diol component comprising:

[0031] About 60 mol % or more of ethylene glycol residues and

[0032] About 40 mole % or less of other diols, the other diols comprising one or more of:

[0033] (i) from 15 mole % to less than about 30 mole % of 1,4-cyclohexanedimethanol residues;

[0034] (ii) from about 7 mole % to less than about 15 mole % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0035] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %;

[0036] and 5 to 70 wt. % of at least one polyester composition comprising:

[0037] At least one polyester comprising:

[0038] (a) a dicarboxylic acid component comprising:

[0039] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0040] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0041] (b) a diol component comprising:

[0042] About 50 mol % or more of ethylene glycol residues and

[0043] About 50 mole % or less of other diols, the other diols comprising one or more of:

[0044] (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues;

[0045] (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0046] The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

[0047] One embodiment of the present disclosure is a multilayer crystallizable film comprising at least one skin layer (A), the skin layer (A) comprising a blend of 50-99.9 wt. % of at least one polyester composition (1) and 0.1-50 wt. % of at least one polyester composition (2), the polyester composition (1) comprising: at least one polyester comprising:

[0048] (a) a dicarboxylic acid component comprising:

[0049] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0050] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0051] (b) a diol component comprising:

[0052] About 75 mol % or more of ethylene glycol residues and

[0053] About 25 mole % or less of other diols, the other diols comprising one or more of:

[0054] (i) from about 0 to less than about 24 mole percent neopentyl glycol residues;

[0055] (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues;

[0056] (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0057] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0058] The polyester composition (2) comprises: at least one polyester comprising:

[0059] (a) a dicarboxylic acid component comprising:

[0060] (i) from about 90 to about 100 mole percent terephthalic acid residues;

[0061] (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0062] (b) a diol component comprising:

[0063] About 60 mol % or more of ethylene glycol residues and

[0064] About 40 mole % or less of other diols, the other diols comprising one or more of:

[0065] (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues;

[0066] (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0067] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0068] at least one core layer (B), said core layer (B) comprising a blend of 30-95 wt. % of at least one polyester composition (1) and 5-70 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising:

[0069] (a) a dicarboxylic acid component comprising:

[0070] (i) from about 90 to about 100 mole percent terephthalic acid residues;

[0071] (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0072] (b) a diol component comprising:

[0073] About 60 mol % or more of ethylene glycol residues and

[0074] About 40 mole % or less of other diols, the other diols comprising one or more of:

[0075] (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues;

[0076] (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0077] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0078] The polyester composition (2) comprises: at least one polyester comprising:

[0079] (a) a dicarboxylic acid component comprising:

[0080] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0081] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0082] (b) a diol component comprising:

[0083] About 50 mol % or more of ethylene glycol residues and

[0084] About 50 mole % or less of other diols, the other diols comprising one or more of:

[0085] (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues;

[0086] (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0087] The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

[0088] One embodiment of the present disclosure is a multilayer crystallizable film comprising at least one skin layer (A), the skin layer (A) comprising a blend of 50-99.9 wt. % of at least one polyester composition (1) and 0.1-50 wt. % of at least one polyester composition (2), the polyester composition (1) comprising: at least one polyester comprising:

[0089] (a) a dicarboxylic acid component comprising:

[0090] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0091] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0092] (b) a diol component comprising:

[0093] About 75 mol % or more of ethylene glycol residues and

[0094] About 25 mole % or less of other diols, the other diols comprising one or more of:

[0095] (i) from about 0 to less than about 24 mole percent neopentyl glycol residues;

[0096] (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues;

[0097] (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0098] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0099] The polyester composition (2) comprises: at least one polyester comprising:

[0100] (a) a dicarboxylic acid component comprising:

[0101] (i) from about 90 to about 100 mole percent terephthalic acid residues;

[0102] (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0103] (b) a diol component comprising:

[0104] About 60 mol % or more of ethylene glycol residues and

[0105] About 40 mole % or less of other diols, the other diols comprising one or more of:

[0106] (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues;

[0107] (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0108] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0109] at least one core layer (B), said core layer (B) comprising a blend of 20-30 wt. % of at least one polyester composition (1) and 40-60 wt. % of at least one polyester composition (2) and 20-30 wt. % of at least one polyester composition (3), said polyester composition (1) comprising: at least one polyester comprising:

[0110] (a) a dicarboxylic acid component comprising:

[0111] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0112] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0113] (b) a diol component comprising:

[0114] About 75 mol % or more of ethylene glycol residues and

[0115] About 25 mole % or less of other diols, the other diols comprising one or more of:

[0116] (i) from about 0 to less than about 24 mole percent neopentyl glycol residues;

[0117] (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues;

[0118] (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0119] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0120] The polyester composition (2) comprises: at least one polyester comprising:

[0121] (a) a dicarboxylic acid component comprising:

[0122] (i) from about 90 to about 100 mole percent terephthalic acid residues;

[0123] (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0124] (b) a diol component comprising:

[0125] About 60 mol % or more of ethylene glycol residues and

[0126] About 40 mole % or less of other diols, the other diols comprising one or more of:

[0127] (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues;

[0128] (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0129] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0130] The polyester composition (3) comprises: at least one polyester comprising:

[0131] (a) a dicarboxylic acid component comprising:

[0132] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0133] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0134] (b) a diol component comprising:

[0135] About 50 mol % or more of ethylene glycol residues and

[0136] About 50 mole % or less of other diols, the other diols comprising one or more of:

[0137] (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues;

[0138] (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0139] The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

[0140] One embodiment of the present disclosure is a multilayer crystallizable film comprising at least one skin layer (A), the skin layer (A) comprising a blend of 50-70 wt. % of at least one polyester composition (1) and 30-50 wt. % of at least one polyester composition (2), the polyester composition (1) comprising: at least one polyester comprising:

[0141] (a) a dicarboxylic acid component comprising:

[0142] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0143] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0144] (b) a diol component comprising:

[0145] About 75 mol % or more of ethylene glycol residues and

[0146] About 25 mole % or less of other diols, the other diols comprising one or more of:

[0147] (i) from about 0 to less than about 24 mole percent neopentyl glycol residues;

[0148] (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues;

[0149] (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0150] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0151] The polyester composition (2) comprises: at least one polyester comprising:

[0152] (a) a dicarboxylic acid component comprising:

[0153] (i) from about 90 to about 100 mole percent terephthalic acid residues;

[0154] (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0155] (b) a diol component comprising:

[0156] About 60 mol % or more of ethylene glycol residues and

[0157] About 40 mole % or less of other diols, the other diols comprising one or more of:

[0158] (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues;

[0159] (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0160] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0161] at least one core layer (B), said core layer (B) comprising a blend of 30-50 wt. % of at least one polyester composition (1) and 50-70 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising:

[0162] (a) a dicarboxylic acid component comprising:

[0163] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0164] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0165] (b) a diol component comprising:

[0166] About 75 mol % or more of ethylene glycol residues and

[0167] About 25 mole % or less of other diols, the other diols comprising one or more of:

[0168] (i) from about 0 to less than about 24 mole percent neopentyl glycol residues;

[0169] (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues;

[0170] (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0171] wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and

[0172] The polyester composition (2) comprises: at least one polyester comprising:

[0173] (a) a dicarboxylic acid component comprising:

[0174] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0175] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0176] (b) a diol component comprising:

[0177] About 50 mol % or more of ethylene glycol residues and

[0178] About 50 mole % or less of other diols, the other diols comprising one or more of:

[0179] (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues;

[0180] (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0181] The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

[0182] One embodiment of the present disclosure is the multilayer crystallizable film of the preceding embodiment, wherein the polyester composition comprises:

[0183] At least one polyester comprising:

[0184] (a) a dicarboxylic acid component comprising:

[0185] (i) from about 70 to about 100 mole percent of terephthalic acid residues;

[0186] (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and

[0187] (b) a diol component comprising:

[0188] About 80 mol % or more of ethylene glycol residues and

[0189] About 20 mole % or less of other diols, the other diols comprising one or more of:

[0190] (i) from about 5 to less than about 17 mole percent neopentyl glycol residues;

[0191] (ii) from about 2 to less than about 10 mole percent of 1,4-cyclohexanedimethanol residues;

[0192] (iii) from about 1 to less than about 10 mole percent of the total diethylene glycol residues and / or butanediol residues in the final polyester composition;

[0193] The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

[0194] One embodiment of the present disclosure is a multi-layer crystallizable film using 10 wt% to 50 wt% recycled polyethylene terephthalate (rPET) bottle flakes blended with an amorphous copolyester resin in the core layer and a blended crystallizable copolyester resin and an amorphous copolyester resin in the skin layer.

[0195] One embodiment of the present disclosure is a multi-layer crystallizable film using 30-50 wt% recycled polyethylene terephthalate (rPET) bottle flakes blended with an amorphous copolyester resin in the core layer and a blended crystallizable copolyester resin and an amorphous copolyester resin in the skin layer.

[0196] In one embodiment, the multilayer crystallizable film has an ABA configuration.

[0197] In another embodiment, the multi-layer crystallizable shrinkable film of the present disclosure is composed of three layers having an ABA configuration, the skin layer (layer A) being composed of a blend of a crystallizable resin and a copolyester resin, and the core layer (layer B) being arranged between the first and second skin layers and being composed of a blend of a copolyester resin and rPET within a certain optimized range.

[0198] In one embodiment, the multi-layer crystallizable shrinkable film of the present disclosure is composed of two layers having an AB or BA configuration, the skin layer (layer A) is composed of a blend of a crystallizable resin and a copolyester resin, and the core layer (layer B) is composed of a blend of a copolyester resin and rPET within certain optimized ranges.

[0199] In one embodiment, the multi-layer crystallizable shrinkable film of the present disclosure consists of five layers having an ABABA configuration, the skin layer (layer A) consists of a blend of a crystallizable copolyester resin and an amorphous copolyester resin, the core layer (layer B) is arranged between the first, third and fifth skin layers, and the core layer consists of a blend of an amorphous copolyester resin and rPET within certain optimized ranges.

[0200] In one embodiment, the multi-layer crystallizable shrinkable film of the present disclosure consists of five layers having an AABAA configuration, the skin layer (layer A) consists of a blend of a crystallizable copolyester resin and an amorphous copolyester resin, the core layer (layer B) is arranged between the skin layers, and the core layer consists of a blend of an amorphous copolyester resin and rPET within certain optimized ranges.

[0201] In one embodiment, the multi-layer crystallizable shrinkable film of the present disclosure consists of five layers having an ABCBA configuration, the skin layers (layer A) consisting of a blend of a crystallizable copolyester resin and an amorphous copolyester resin, the core layer (layer B) being arranged between the skin layers, and the core layer consisting of a blend of an amorphous copolyester resin and rPET within certain optimized ranges.

[0202] Alternatively, in some embodiments, in an ABA or ABCBA configuration, the layer consists of, within certain optimized ranges:

[0203] Layer A is a blend of at least one amorphous copolyester resin and rPET,

[0204] Layer B is a blend of at least one crystallizable copolyester resin and an amorphous copolyester resin and rPET, and

[0205] Optionally, layer C is a blend of at least one amorphous copolyester resin and rPET; or

[0206] Layer A is a blend of at least one amorphous copolyester resin and rPET,

[0207] Layer B is a blend of at least one crystallizable copolyester resin and / or rPET, and

[0208] Optionally, layer C is a blend of at least one amorphous copolyester resin and rPET; or

[0209] Layer A is a blend of at least one amorphous copolyester resin and / or at least one crystallizable copolyester resin and / or rPET,

[0210] Layer B is a blend of at least one amorphous copolyester resin and / or at least one crystallizable copolyester resin and / or rPET, and

[0211] Optionally, layer C is a blend of at least one amorphous copolyester resin and / or at least one crystallizable copolyester resin and / or rPET.

[0212] In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 200°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 195°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 190°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 180°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 175°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 170°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 165°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 160°C or higher. In one embodiment of the present disclosure, the multilayer crystallizable film has a strain-induced crystalline melting point of 150°C or higher.

[0213] In one embodiment, the multi-layer crystallizable film of the present disclosure has a shrinkage in a primary shrinkage direction of 60% or greater when immersed in 85°C water for 10 seconds.

[0214] In one embodiment, the multi-layer crystallizable film of the present disclosure has a shrinkage in a primary shrinkage direction of 50% or greater when immersed in 85°C water for 10 seconds.

[0215] In one embodiment, the multi-layer crystallizable film of the present disclosure has a shrink force of 5 MPa or greater.

[0216] In one embodiment of the present disclosure, the multilayer crystallizable film may be recycled in the PET recycle stream.

[0217] Details

[0218] The present disclosure is more easily understood with reference to the following detailed description of certain embodiments and examples of the present disclosure. According to the purpose of the present disclosure, certain embodiments of the present disclosure are described in the summary of the invention and further described below. Other embodiments of the present disclosure are also described herein.

[0219] Heat shrinkable plastic films are used as covers to hold objects together and as outer packaging for bottles, cans and other types of containers. For example, such films are used to cover the cap, neck, shoulder or ridge of a bottle or the entire bottle; to label, protect, wrap or add value to a product; and for other reasons. In addition, such films can be used as covers to package objects such as boxes, bottles, boards, sticks or notebooks together in groups, and such films can also be tightly attached as packaging materials. The above uses take advantage of the shrinkability and internal shrinkage stress of the film.

[0220] In the past, poly(vinyl chloride) (PVC) films dominated the shrink film market. However, polyester films have become an important alternative because polyester films do not have the environmental issues associated with PVC films. Polyester shrink films ideally have properties very similar to PVC films so that polyester films can serve as a "drop-in" replacement film and can be processed in existing shrink tunnel equipment. The properties of PVC films that are desired to be replicated include the following: (1) a relatively low shrinkage initiation temperature, (2) a total shrinkage that increases gradually and in a controlled manner as the temperature rises, (3) a low shrink force that prevents the underlying container from breaking, (4) a high total shrinkage (e.g., 50% or greater), (5) inherent film toughness to prevent unwanted film tearing and splitting before and after shrinking, and (6) a high strain-induced crystalline melting temperature.

[0221] The present disclosure describes unique and unexpected effects measured with certain monomer combinations that improve the recyclability of multilayer polyester shrink film labels.

[0222] Shrink film compositions are used commercially as shrink film labels for food, beverages, personal care, household products, etc. Typically, these shrink films are used in combination with clear polyethylene terephthalate (PET) bottles or containers. The entire package (bottle plus label) is then put into the recycling process. In a typical recycling center, the PET and shrink film materials are usually finally combined together at the end of the process due to the similarity of composition and density. The PET bottle flakes need to be dried to remove residual water left in the PET by the recycling process. Typically, PET is dried at temperatures above 150°C, and in some cases above 200°C. At these temperatures, typical polyester shrink film resins soften and become sticky, often forming lumps with the PET bottle flakes. These lumps must be removed before further processing. These lumps reduce the yield of PET bottle flakes from the process and result in additional operating steps.

[0223] It has been found that certain combinations of diol monomers in shrink film resin compositions can produce films that have good shrink film properties and can also be crystallized so that they do not affect the recycling of PET bottle flakes during the recycling process. These crystallizable shrink film resins can be processed with PET bottles and eventually become a component in the recycled PET bottle flakes leaving the recycling process. It has also been found that the selection and amount of a specific combination of diol monomers is important for producing films with good shrink film properties and producing crystallizable films.

[0224] There is no limitation on the recycled polyethylene terephthalate (rPET) that can be used in the blend compositions of the present disclosure. In one embodiment, the rPET is mechanically recycled. In one embodiment, the rPET is made from chemically recycled monomers (made by any known depolymerization method). In one embodiment, the rPET may have slight modifications, such as modification with up to 5 mol % of isophthalic acid and / or up to 5 mol % of CHDM or other diols. In one embodiment, the recycled PET (rPET) can be almost any "waste" industrial or post-consumer PET. In one embodiment, the rPET that can be used in the blend compositions of the present disclosure can be post-consumer recycled PET. In one embodiment, the rPET is post-industrial recycled PET. In one embodiment, the rPET is post-consumer PET from soft drink bottles. In one embodiment, waste PET fibers, waste PET films, and low-quality PET polymers are also suitable sources of rPET. In one embodiment, recycled PET substantially comprises PET, although other copolyesters may also be used, particularly when they have a structure similar to PET, such as PET copolymers, etc. In one embodiment, the rPET is clean. In one embodiment, the rPET is substantially free of contaminants. In one embodiment, the rPET may be in the form of bottle flakes.

[0225] In one embodiment, up to about 50% by weight rPET may be incorporated into the blend composition of the present disclosure. In one embodiment, up to about 40% by weight rPET may be incorporated into the blend composition of the present disclosure. In one embodiment, up to about 30% by weight rPET may be incorporated into the blend composition of the present disclosure. In one embodiment, up to about 20% by weight rPET may be incorporated into the blend composition of the present disclosure. In one embodiment, the rPET / copolyester blend is 0.1-50% by weight rPET. In one embodiment, the rPET / copolyester blend is 1-50% by weight recycled polyethylene terephthalate (rPET). In one embodiment, the rPET / copolyester blend is 10-50% by weight recycled polyethylene terephthalate (rPET). In one embodiment, the rPET / copolyester blend is 15-50% by weight recycled polyethylene terephthalate (rPET). In one embodiment, the rPET / copolyester blend is 20-50 wt% recycled polyethylene terephthalate (rPET). In one embodiment, the rPET / copolyester blend is 20-30 wt% recycled polyethylene terephthalate (rPET). In one embodiment, the rPET / copolyester blend is 20-40 wt% recycled polyethylene terephthalate (rPET) and 30-40 wt% of at least one copolyester. In one embodiment, the rPET / copolyester blend is 1-50 wt% recycled polyethylene terephthalate (rPET) and 50-99 wt% of at least one copolyester.

[0226] The term "polyester" as used herein is intended to include "copolyesters" and is understood to refer to synthetic polymers made by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxyl compounds and / or polyfunctional hydroxyl compounds, such as branching agents. Typically, the difunctional carboxylic acid can be a dicarboxylic acid, and the difunctional hydroxyl compound can be a dihydric alcohol (dihydricalcoh01), such as glycols and diols. The term "glycol" as used herein includes, but is not limited to, diols, glycols and / or polyfunctional hydroxyl compounds, such as branching agents. Alternatively, the difunctional carboxylic acid can be a hydroxycarboxylic acid, such as p-hydroxybenzoic acid, and the difunctional hydroxyl compound can have an aromatic core with 2 hydroxyl substituents, such as hydroquinone. The term "residue" as used herein refers to any organic structure incorporated into a polymer from the corresponding monomer by polycondensation and / or esterification reactions. The term "repeat unit" as used herein refers to an organic structure having a dicarboxylic acid residue and a diol residue bonded via an ester group. Thus, for example, a dicarboxylic acid residue may be derived from a dicarboxylic acid monomer or its associated acyl halides, esters, salts, anhydrides and / or mixtures thereof. In addition, the term "diacid" as used herein includes polyfunctional acids, such as branching agents. Thus, the term "dicarboxylic acid" as used herein is intended to include dicarboxylic acids and any derivatives of dicarboxylic acids that can be used in the process of reacting with a diol to make a polyester, including its associated acyl halides, esters, half-esters, salts, half-salts, anhydrides, mixed anhydrides and / or mixtures thereof. The term "terephthalic acid" as used herein is intended to include terephthalic acid itself and its residues that can be used in the process of reacting with a diol to make a polyester, as well as any derivatives of terephthalic acid, including its associated acyl halides, esters, half-esters, salts, half-salts, anhydrides, mixed anhydrides and / or mixtures thereof or residues thereof.

[0227] The polyesters used in the present disclosure can generally be prepared from dicarboxylic acids and diols that react in substantially equal proportions and are incorporated into the polyester polymer as their corresponding residues. The polyesters of the present disclosure may therefore contain substantially equal molar proportions of acid residues (100 mole %) and diol (and / or polyfunctional hydroxy compound) residues (100 mole %) to make the total mole number of repeating units equal to 100 mole %. Therefore, the mole percentages provided in the present disclosure may be based on the total mole number of acid residues, the total mole number of diol residues, or the total mole number of repeating units. For example, a polyester containing 10 mole % of isophthalic acid based on the total acid residues means that the polyester contains 10 mole % of isophthalic acid residues in a total of 100 mole % of acid residues. Therefore, there are 10 moles of isophthalic acid residues in every 100 moles of acid residues. In another example, a polyester containing 25 mole % of 1,4-cyclohexanedimethanol based on the total diol residues means that the polyester contains 25 mole % of 1,4-cyclohexanedimethanol residues in a total of 100 mole % of diol residues. Thus, there are 25 moles of 1,4-cyclohexanedimethanol residues for every 100 moles of diol residues.

[0228] In certain embodiments, terephthalic acid or its esters, such as dimethyl terephthalate or a mixture of terephthalic acid residues and their esters may constitute part or all of the dicarboxylic acid component used to form the polyesters that can be used in the present disclosure. In certain embodiments, terephthalic acid residues may constitute part or all of the dicarboxylic acid component used to form the polyesters that can be used in the present disclosure. For the purposes of the present disclosure, the terms "terephthalic acid" and "dimethyl terephthalate" are used interchangeably herein. In one embodiment, dimethyl terephthalate is part or all of the dicarboxylic acid component used to prepare the polyesters that can be used in the present disclosure. In embodiments, 70 to 100 mol%; or 80 to 100 mol%; or 90 to 100 mol%; or 95 to 100 mol%; or 99 to 100 mol%; or 99.9 to 100 mol%; or 100 mol% terephthalic acid and / or dimethyl terephthalate and / or mixtures thereof may be used.

[0229] In addition to terephthalic acid, the dicarboxylic acid component of the polyester that can be used in the present disclosure may also include up to 30 mol%, up to 20 mol%, up to 10 mol%, up to 5 mol%, or up to 1 mol% of one or more modified aromatic dicarboxylic acids. Another embodiment contains 0 mol% modified aromatic dicarboxylic acids. Therefore, if present, it is expected that the amount of one or more modified aromatic dicarboxylic acids can be the range of any of these aforementioned endpoint values, including, for example, 0.01 to 10 mol%, 0.01 to 5 mol%, and 0.01 to 1 mol%. In one embodiment, modified aromatic dicarboxylic acids that can be used in the present disclosure include, but are not limited to, those with up to 20 carbon atoms, which can be linear, para-oriented, or symmetrical. Examples of modified aromatic dicarboxylic acids that can be used in the present disclosure include, but are not limited to, isophthalic acid, 4,4′-biphenyl dicarboxylic acid, 1,4-, 1,5-, 2,6-, 2,7-naphthalene dicarboxylic acid, and trans-4,4′-stilbene dicarboxylic acid, and their esters. In one embodiment, the modifying aromatic dicarboxylic acid is isophthalic acid.

[0230] The carboxylic acid component of the polyester that can be used for the present disclosure can be further modified with up to 10 mol %, such as up to 5 mol % or up to 1 mol % of one or more aliphatic dicarboxylic acids containing 2-16 carbon atoms, such as cyclohexanedicarboxylic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and / or dodecanedicarboxylic acid. Certain embodiments can also include 0.01 to 10 mol %, such as 0.1 to 10 mol %, 1 to 10 mol %, 5 to 10 mol % of one or more modified aliphatic dicarboxylic acids. Another embodiment contains 0 mol % modified aliphatic dicarboxylic acids. The total mole % of the dicarboxylic acid component is 100 mol %. In one embodiment, adipic acid and / or glutaric acid are provided in the modified aliphatic dicarboxylic acid component of the polyester and it can be used for the present disclosure.

[0231] Can use esters of terephthalic acid and other modified dicarboxylic acids or their corresponding esters and / or salts to replace dicarboxylic acids. Suitable examples of dicarboxylic acid esters include but are not limited to dimethyl ester, diethyl ester, dipropyl ester, diisopropyl ester, dibutyl ester and diphenyl ester. In one embodiment, the ester is selected from at least one of the following: methyl ester, ethyl ester, propyl ester, isopropyl ester and phenyl ester.

[0232] In another embodiment, at least a portion of the residues derived from dicarboxylic acids and diols as described herein are derived from recycled monomer species, such as recycled dimethyl terephthalate (rDMT), recycled terephthalic acid (rTPA), recycled dimethyl isophthalate (rDMI), recycled ethylene glycol (rEG), recycled cyclohexanedimethanol (rCHDM), recycled neopentyl glycol (rNPG), recycled 2,2,4,4-tetramethyl-1,3-cyclobutanediol (rTMCD), and recycled diethylene glycol (rDEG). Such recycled monomer species can be obtained from known methanolysis or glycolysis reactions for depolymerization of various post-consumer recycled polyesters and copolyesters. Similarly, recycled poly(ethylene terephthalate) (rPET) can be used as a raw material (for the dicarboxylic acid and diol components) in the manufacture of polyesters with regrind of the present invention. Thus, in another embodiment, the polyester composition of the present invention comprises at least a portion of dicarboxylic acid residues and / or diol residues derived from (i) a recycled monomer species selected from rDMT, rTPA, rDMI, rEG, rCHDM, rDEG, rTMCD, rNPG and (ii) rPET.

[0233] In one embodiment, the diol component useful for the polyester composition of the present disclosure may include 1,4-cyclohexanedimethanol. In another embodiment, the diol component useful for the polyester composition of the present disclosure includes 1,4-cyclohexanedimethanol and 1,3-cyclohexanedimethanol. The molar ratio of cis / trans 1,4-cyclohexanedimethanol may range from 50 / 50 to 0 / 100, for example, from 40 / 60 to 20 / 80.

[0234] The diol component useful in the polyester compositions and crystallizable copolyester compositions of the present disclosure may include, but are not limited to, those wherein the sum of the residues of 1,4-cyclohexanedimethanol and the residues of neopentyl glycol in the final polyester composition is 0 to 30 mol%, or 1 to 30 mol%, or 1 to 25 mol%, 1 to 20 mol%, or 1 to 15 mol%, or 1 to 10 mol%, or 2 to 30 mol%, or 2 to 25 mol%, or 2 to 20 mol%, or 2 to 15 mol%, or 2 to 10 mol%, or 3 to 30 mol%, or 3 to 25 mol%, or 3 to 20 mol%, or 3 to 15 mol%, or 3 to 10 mol%, 4 to 30 mol%, or 4 to 25 mol%, 4 to 20 mol%, or 4 to 15 mol%, or 4 to 10 mol%, 5 to 30 mol%, or 5 to 25 mol%, 5 to 20 mol%, or 5 to 15 mol%, or 5 to 10 mol%, 6 to 30 mol%, or 6 to 25 mol%, 6 to 20 mol%, or 6 to 15 mol%, or 6 to 10 mol%, 7 to 30 mol%, or 7 to 25 mol%, 7 to 20 mol%, or 7 to 15 mol%, or 7 to 10 mol%, 8 to 30 mol%, or 8 to 25 mol%, 8 to 20 mol%, or 8 to 15 mol%, or 8 to 10 mol%, 9 to 30 mol%, or 9 to 25 mol%, 9 to 20 mol%, or 9 to 15 mol% %, or 9 to 10 mol%, 10 to 30 mol%, or 10 to 25 mol%, 10 to 20 mol%, or 10 to 15 mol%, or 11 to 30 mol%, 11 to 30 mol%, or 11 to 25 mol%, 11 to 20 mol%, or 11 to 15 mol%, or 12 to 30 mol%, 12 to 25 mol%, or 12 to 20 mol%, 12 to 15 mol%, or 13 to 30 mol%, or 13 to 25 mol%, 13 to 20 mol%, or 13 to 15 mol%, 14 to 30 mol%, or 14 to 25 mol%, or 14 to 20 mol%, 14 to 15 mol%, or 15 to 30 mol%, 15 to 25 mol%, or %, or 11 to 29 mol%, or 12 to 29 mol%, or 13 to 29 mol%, or 14 to 29 mol%, or 15 to 29 mol%, or 10 to 28 mol%, or 11 to 28 mol%, or 12 to 28 mol%, or 13 to 28 mol%, or 14 to 28 mol%, or 15 to 28 mol% of the composition.In one embodiment, the sum of the residues of 1,4-cyclohexanedimethanol and the residues of neopentyl glycol in the final polyester composition may be 4 to 15 mol%, or 2 to 21 mol%, or 2 to less than 20 mol%, or 4 to 20 mol%, or 5 to 18 mol%, or 10 to 21 mol%, or 12 to 21 mol%, wherein the total mol% of the diol components is 100 mol%.

[0235] In one embodiment, the diol component of the polyester composition that can be used in the present disclosure may contain 0 to 30 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition that can be used in the present disclosure may contain 0 to 25 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 0 to 20 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 0 to 17 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component of the polyester composition and the polyester blend composition that can be used in the present disclosure may contain 5 to 20 mol% of neopentyl glycol based on the total mole % of the diol component as 100 mol%. In one embodiment, the diol component that can be used in the polyester composition and the polyester blend composition of the present disclosure may contain 10 to 20 mol% of neopentyl glycol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used in the polyester composition and the polyester blend composition of the present disclosure may contain 10 to 15 mol% of neopentyl glycol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used in the polyester composition and the polyester blend composition of the present disclosure may contain 15 to 25 mol% of neopentyl glycol based on the total mol% of the diol component being 100 mol%.

[0236] In one embodiment, the diol component useful in the polyester composition of the present disclosure may contain 0 to 50 mol%, or 0.01 to 50 mol%, 0 to 40 mol%, or 0.01 to 40 mol%, 0 to 30 mol%, or 0.01 to 30 mol%, or 0 to 25 mol%, or 0.1 to 25 mol%, or 0 to 20 mol%, or 0.1 to 20 mol%, or 2 to 20 mol%, or 0.01 to 15 mol%, or 0.01 to 14 mol%, or 0.01 to 13 mol%, or 0.01 to 12 mol%, or 0.01 to 11 mol%, or 0.01 to 10 mol%, or 0.01 to 9 mol%. %, or 0.01 to 8 mol%, or 0.01 to 7 mol%, or 0.01 to 6 mol%, or 0.01 to 5 mol%, or 3 to 15 mol%, or 3 to 14 mol%, or 3 to 13 mol%, or 3 to 12 mol%, or 3 to 11 mol%, or 3 to 10 mol%, or 3 to 9 mol%, or 3 to 8 mol%, or 3 to 7 mol%, or 2 to 10 mol%, or 2 to 9 mol%, or 2 to 8 mol%, or 2 to 7 mol%, or 2 to 5 mol%, or 1 to 7 mol%, or 1 to 5 mol%, or 1 to 3 mol%, or 15 to 30 mol%, or 15 to 20 mol%, or 10 to 30 mol%, or 10 to 20 mol% of 1,4-cyclohexanedimethanol residues.

[0237] In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0.01 to 15 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0 to less than 15 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0.01 to 10 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0 to less than 10 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component that can be used for the polyester composition of the present disclosure may contain 0.01 to 5 mol% of 1,4-cyclohexanedimethanol based on the total mol% of the diol component being 100 mol%. In one embodiment, the diol component useful in the polyester composition of the present disclosure may contain 0 to less than 5 mole % of 1,4-cyclohexanedimethanol based on the total mole % of the diol component being 100 mole %.

[0238] It should be understood that some other diol residues may be formed in situ during processing. The total amount of diethylene glycol residues may be present in the polyesters useful for the present disclosure, whether formed in situ during processing or intentionally added, or both, for example, in any amount of 0.1 to 15 mol%, or 1 to 15 mol%, or 2 to 15 mol%, or 5 to 15 mol%, or 7 to 15 mol%, or 2 to 12 mol%, or 2 to 11 mol%, or 2 to 10 mol%, or 2 to 9 mol%, or 3 to 12 mol%, or 3 to 11 mol%, or 3 to 10 mol%, or 3 to 9 mol%, or 4 to 12 mol%, or 4 to 11 mol%, or 4 to 10 mol%, or 4 to 9 mol%, or 5 to 12 mol%, or 5 to 11 mol%, or 5 to 10 mol%, or 5 to 9 mol% of diethylene glycol residues, based on the total mol% of the diol component being 100 mol%.

[0239] In one embodiment, the total amount of diethylene glycol residues present in the polyesters useful in the present disclosure, whether formed in situ during processing or intentionally added, or both, can be 4 mol% or less, or 3.5 mol% or less, or 3.0 mol% or less, or 2.5 mol% or less, or 2.0 mol% or less, or 1.5 mol% or less, or 1.0 mol% or less, or 1 to 4 mol%, or 1 to 3 mol%, or 1 to 2 mol% of diethylene glycol residues, or 2 to 8 mol%, or 2 to 7 mol%, or 2 to 6 mol%, or 2 to 5 mol%, or 3 to 8 mol%, or 3 to 7 mol%, or 3 to 6 mol%, or 3 to 5 mol%, or in some embodiments, no intentionally added diethylene glycol residues, based on the total mol% of the diol component being 100 mol%. In certain embodiments, the polyester contains no added modifying glycol.

[0240] For all embodiments, the remaining diol component can contain any amount of ethylene glycol residues based on the total mole % of the diol component being 100 mole %. In one embodiment, the polyester portion of the polyester composition useful in the present disclosure can contain 50 mole % or more, or 55 mole % or more, or 60 mole % or more, or 65 mole % or more, or 70 mole % or more, or 75 mole % or more, or 80 mole % or more, or 85 mole % or more, or 90 mole % or more, or 95 mole % or more, or 50 to 80 mole %, or 55 to 80 mole %, or 60 to 80 mole %, or 50 to 75 mole %, or 55 to 75 mole %, or 60 to 75 mole %, or 65 to 75 mole % of ethylene glycol residues based on the total mole % of the diol component being 100 mole %.

[0241] In one embodiment, the diol component of the polyester composition useful in the present disclosure may contain up to 20 mol%, or up to 19 mol%, or up to 18 mol%, or up to 17 mol%, or up to 16 mol%, or up to 15 mol%, or up to 14 mol%, or up to 13 mol%, or up to 12 mol%, or up to 11 mol%, or up to 10 mol%, or up to 9 mol%, or up to 8 mol%, or up to 7 mol%, or up to 6 mol%, or up to 5 mol%, or up to 4 mol%, or up to 3 mol%, or up to 2 mol%, or up to 1 mol% or less of one or more modified diols (modified diols are defined as diols that are not ethylene glycol, diethylene glycol, neopentyl glycol, or 1,4-cyclohexanedimethanol). In certain embodiments, the polyesters useful in the present disclosure may contain 10 mol% or less of one or more modified diols. In certain embodiments, the polyesters useful in the present disclosure may contain 5 mol% or less of one or more modified diols. In certain embodiments, the polyesters useful in the present disclosure may contain 3 mol % or less of one or more modifying diols. In another embodiment, the polyesters useful in the present disclosure may contain 0 mol % of modifying diols. However, it is expected that some other diol residues may be formed in situ so that residual amounts formed in situ are also an embodiment of the present disclosure.

[0242] In an embodiment, if used, the modified glycol suitable for polyester as defined herein contains 2 to 16 carbon atoms. Examples of modified glycols include, but are not limited to, 1,2-propylene glycol, 1,3-propylene glycol, isosorbide, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol (p-xylene glycol), polytetramethylene glycol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) and mixtures thereof. In one embodiment, isosorbide is a modified glycol. In another embodiment, the modified glycol includes, but is not limited to, at least one of 1,3-propylene glycol and 1,4-butylene glycol. In one embodiment, 1,3-propylene glycol and / or 1,4-butylene glycol can be excluded. If 1,4- or 1,3-butylene glycol is used, greater than 4 mol % or greater than 5 mol % can be provided in one embodiment. In one embodiment, at least one modified glycol is 1,4-butylene glycol present in an amount of 0 to 25 mol %. In one embodiment, the at least one modifying diol is 1,4-butanediol present in an amount of 5 to 25 mole percent.

[0243] In one embodiment, a multilayer shrink film is provided, comprising a polyester composition, the polyester composition further comprising: 1,4-cyclohexanedimethanol residues present in an amount of 0.01 to about 10 mol %, diethylene glycol residues present in an amount of 2 to 9 mol %, neopentyl glycol residues present in an amount of 5 to 30 mol %, and ethylene glycol residues present in an amount of 60 mol % or greater, based on the total mol % of the diol component being 100 mol %.

[0244] In one embodiment, a multilayer shrink film is provided, comprising a polyester composition, the polyester composition further comprising: 1,4-cyclohexanedimethanol residues present in an amount of 0.01 to about 30 mol %, diethylene glycol residues present in an amount of 2 to 15 mol %, neopentyl glycol residues present in an amount of 0 to 30 mol %, and ethylene glycol residues present in an amount of 60 mol % or greater, based on the total mol % of the diol component being 100 mol %.

[0245] In some embodiments, polyesters according to the present disclosure may contain 0 to 10 mol%, e.g., 0.01 to 5 mol%, 0.01 to 1 mol%, 0.05 to 5 mol%, 0.05 to 1 mol%, or 0.1 to 0.7 mol% of one or more branching monomers (also referred to herein as branching agents) having 3 or more carboxyl substituents, hydroxyl substituents, or combinations thereof, based on the total mole percentage of diol or diacid residues, respectively. In certain embodiments, branching monomers or branching agents may be added before and / or during and / or after polymerization of the polyester. In some embodiments, one or more polyesters useful in the present disclosure may therefore be linear or branched.

[0246] Examples of branching monomers include, but are not limited to, polyfunctional acids or polyfunctional alcohols such as trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerol, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid, etc. In one embodiment, the branching monomer residues may contain 0.1 to 0.7 mole % of one or more residues selected from at least one of the following: trimellitic anhydride, pyromellitic dianhydride, glycerol, sorbitol, 1,2,6-hexanetriol, pentaerythritol, trimethylolethane and / or trimesic acid. The branching monomers may be added to the polyester reaction mixture or blended with the polyester as described in, for example, U.S. Patent Nos. 5,654,347 and 5,696,176 (their disclosures on branching monomers are incorporated herein by reference) in the form of a concentrate.

[0247] The polyesters useful in the present disclosure may include at least one chain extender. Suitable chain extenders include, but are not limited to, multifunctional (including but not limited to difunctional) isocyanates, multifunctional epoxides, including, for example, epoxidized novolac resins and phenoxy resins. In certain embodiments, the chain extender may be added at the end of the polymerization process or after the polymerization process. If added after the polymerization process, the chain extender may be incorporated by compounding or by addition during a conversion process, such as injection molding or extrusion.

[0248] The amount of chain extender used may vary depending upon the particular monomer composition used and the physical properties desired, but is typically from about 0.1 to about 10 weight percent, such as from about 0.1 to about 5 weight percent, based on the total weight of the polyester.

[0249] Unless otherwise stated, it is contemplated that the polyester compositions useful in the present disclosure may have at least one inherent viscosity range described herein and at least one monomer range for the polyester compositions described herein. Unless otherwise stated, it is also contemplated that the polyester compositions useful in the present disclosure may have at least one Tg range described herein and at least one monomer range for the polyester compositions described herein. Unless otherwise stated, it is also contemplated that the polyester compositions useful in the present disclosure may have at least one inherent viscosity range described herein, at least one Tg range described herein, and at least one monomer range for the polyester compositions described herein.

[0250] For embodiments of the present disclosure, the polyesters useful for the present disclosure may exhibit at least one of the following inherent viscosities measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.25 g / 50 ml at 25° C.: 0.50 to 1.2 dL / g; 0.50 to 1.0 dL / g; 0.50 to 0.90 dL / g; 0.50 to 0.80 dL / g; 0.55 to 0.80 dL / g; 0.60 to 0.80 dL / g; 0.65 to 0.80 dL / g; 0.70 to 0.80 dL / g; 0.50 to 0.75 dL / g; 0.55 to 0.75 dL / g; or 0.60 to 0.75 dL / g.

[0251] The glass transition temperature (Tg) of the polyesters was determined using a TA DSC 2920 from Thermal Analyst Instrument at a scanning rate of 20°C / min.

[0252] In certain embodiments, the multilayer oriented films or multilayer shrink films of the present disclosure comprise a polyester / polyester composition wherein the polyester has a Tg of 60 to 80° C.; 70 to 80° C.; or 65 to 80° C.; or 65 to 75° C. In certain embodiments, these Tg ranges may be met with or without the addition of at least one plasticizer during the polymerization process.

[0253] In embodiments of the present disclosure, certain multilayer oriented films and / or multilayer shrinkable films comprising the polyesters and / or polyester compositions useful in the present disclosure may have a unique combination of all of the following properties: good stretchability, controlled shrinkage properties, certain toughness, certain inherent viscosity, certain glass transition temperature (Tg), certain strain induced crystalline melting point, certain flexural modulus, certain density, certain tensile modulus, certain surface tension, good melt viscosity, good clarity, good color and recyclability.

[0254] In one embodiment, certain polyester compositions useful in the present disclosure may be visually clear.The term "visually clear" is defined herein as the apparent absence of cloudiness, haziness, and / or muddiness upon visual inspection.

[0255] The polyester portion of the polyester composition useful in the present disclosure can be made by methods known in the literature, such as by a process in a homogeneous solution, by a transesterification process in a melt, and by a two-phase interface process. Suitable methods include, but are not limited to, a step of reacting one or more dicarboxylic acids with one or more diols at a temperature of 100° C. to 315° C. and a pressure of 0.1 to 760 mm Hg for a time sufficient to form a polyester. For methods of producing polyesters, see U.S. Pat. No. 3,772,405, the disclosure of which is incorporated herein by reference for such methods.

[0256] As described in more detail in U.S. Pat. No. 2,720,507, which is incorporated herein by reference, polyesters can generally be prepared by condensing a dicarboxylic acid or a dicarboxylic acid ester with a diol in an inert atmosphere in the presence of a catalyst at elevated temperature (which gradually increases to a temperature of about 225° C. to 310° C. during the condensation process) and conducting the condensation under reduced pressure in the later stages of the condensation.

[0257] In some embodiments, in the process of making the method for polyesters that can be used in the present disclosure, certain reagents that color the polymer, including toners or dyes, can be added to the melt. In one embodiment, a bluing toner is added to the melt to reduce the b* of the resulting polyester polymer melt phase product. Such bluing agents include one or more blue inorganic and organic toners and / or dyes. In addition, one or more red toners and / or dyes can also be used to adjust the a* color. One or more organic toners can be used, such as one or more blue and red organic toners, such as those described in U.S. Patent Nos. 5,372,864 and 5,384,377, which are incorporated herein by reference in their entirety. One or more organic toners can be fed in as a premixed composition. The premixed composition can be a pure blend of red and blue compounds, or the composition can be pre-dissolved or pulped in one of the raw materials of the polyester, such as ethylene glycol.

[0258] The total amount of toner components added may depend on the amount of yellow inherent in the base polyester and the effectiveness of the toner. In one embodiment, a total organic toner component concentration of up to about 15 ppm may be used, and a minimum concentration of about 0.5 ppm. In one embodiment, the total amount of bluing additives may be 0.5 to 10 ppm. In one embodiment, one or more toners may be added to the esterification zone or the polycondensation zone. Preferably, one or more toners are added to the esterification zone or to the early stages of the polycondensation zone, such as in a prepolymer reactor.

[0259] The present disclosure further relates to polymer blends. In one embodiment, the polymer blend comprises:

[0260] (a) 5 to 95 weight percent of a polyester composition of the present disclosure as described herein; and

[0261] (b) 5 to 95 weight percent of at least one polymer component.

[0262] Suitable examples of polymer components include, but are not limited to, nylon; polyesters other than those described herein; polyamides, such as those from DuPont; Polystyrene; polystyrene copolymers; styrene acrylonitrile copolymers; acrylonitrile butadiene styrene copolymers; poly(methyl methacrylate); acrylic copolymers; poly(ether-imides), such as (poly(ether-imide) from General Electric); polyphenylene ethers, such as poly(2,6-dimethylphenylene ether) or poly(phenylene ether) / polystyrene blends, such as NORYL (a blend of poly(2,6-dimethylphenylene oxide) and polystyrene resin from General Electric); polyphenylene sulfide; polyphenylene sulfide / sulfone; poly(ester-carbonate); polycarbonates such as (polycarbonate from General Electric); polysulfone; polysulfone ether; and poly(ether-ketone) of an aromatic dihydroxy compound; or a mixture of any of the foregoing polymers. In one embodiment, aliphatic-aromatic polyesters may be excluded from the polyester compositions useful in the present disclosure. The following polyesters that may be blended to make the polyester compositions of the present disclosure may be excluded as polymer components for additional blending—if such blending is outside the compositional scope of the present disclosure: polyethylene terephthalate (PET), glycol-modified PET (PETG), glycol-modified poly(cyclohexylene dimethylene terephthalate) (PCTG), poly(cyclohexylene dimethylene terephthalate) (PCT), acid-modified poly(cyclohexylene dimethylene terephthalate) (PCTA), poly(butylene terephthalate) and / or diethylene glycol-modified PET (EASTOBOND TM copolyester).

[0263] The blends can be prepared by conventional processing techniques known in the art, such as melt blending or solution blending.

[0264] In embodiments, the polyester composition and polymer blend composition may also contain 0.01 to 25 wt % of the total composition of commonly used additives such as colorants, one or more toners, dyes, mold release agents, flame retardants, plasticizers, glass bubbles, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers and / or reaction products thereof, fillers and impact modifiers. Examples of commercially available impact modifiers include but are not limited to ethylene / propylene terpolymers, functionalized polyolefins such as those containing methyl acrylate and / or glycidyl methacrylate, styrene-based block copolymer impact modifiers, and various acrylic core-shell impact modifiers. Residues of these additives are also expected to be part of the polyester composition.

[0265] Reinforcement materials can be added to compositions useful for the present disclosure. Reinforcement materials may include, but are not limited to, carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof. In one embodiment, the reinforcement material comprises glass, such as a mixture of fiberglass filaments, glass and talc, a mixture of glass and mica, and a mixture of glass and polymer fibers.

[0266] In one embodiment, the multilayer films and multilayer shrink films according to the present disclosure may contain 0.01 to 10 weight percent of a polyester plasticizer. In one embodiment, the multilayer shrink film may contain 0.1 to 5 weight percent of a polyester plasticizer. Typically, the multilayer shrink film may contain 90 to 99.99 weight percent of a copolyester. In certain embodiments, the multilayer shrink film may contain 95 to 99.9 weight percent of a copolyester.

[0267] In one aspect, the present disclosure relates to one or more multilayer shrink films and one or more molded articles of the present disclosure comprising polyester compositions and / or polymer blends that can be used for the present disclosure. The method of molding polyester and / or blends into one or more films and / or one or more sheets is well known in the art. Examples of one or more films and / or one or more sheets that can be used for the present disclosure include, but are not limited to, one or more extruded films and / or sheets, one or more compression molded films, one or more calendered films and / or one or more sheets, one or more solution cast films and / or sheets. In one aspect, the method of manufacturing films and / or sheets that can be used for producing shrink films of the present disclosure includes, but is not limited to, extrusion, compression molding, calendering, and solution casting.

[0268] In one embodiment, the polyester compositions useful in the present disclosure are made into films using any method known in the art for producing films from polyesters, such as solution casting, extrusion, compression molding, or calendaring.

[0269] In one embodiment, the as-formed film is subsequently oriented in one or more directions (e.g., a uniaxially and / or biaxially oriented film). Such orientation of the film can be performed by any method known in the art using standard orientation conditions. For example, the oriented film of the present disclosure can be made from a film having a thickness of approximately 100 to 400 microns, such as an extruded, cast, or calendered film, which can be oriented at a ratio of 5:1 to 3:1 at a temperature of Tg to Tg+55°C or 70°C to 125°C, for example, at a ratio of 5:1 or 3:1 at a temperature of 70°C to 100°C, and can be oriented to a thickness of 20 to 80 microns. In one embodiment, the orientation of the initial pre-shrinkage film can be performed on a tenter frame according to these orientation conditions.

[0270] The shrink film of the present disclosure may have a shrinkage initiation temperature of about 55 to about 80° C., or about 55 to about 75° C., or about 55 to about 70° C. The shrinkage initiation temperature is a temperature at which shrinkage begins to occur.

[0271] In certain embodiments, the polyester compositions useful in the present disclosure may have a density of 1.6 g / cc or less, or 1.5 g / cc or less, or 1.4 g / cc or less, or 1.1 g / cc to 1.5 g / cc, or 1.2 g / cc to 1.4 g / cc, or 1.2 g / cc to 1.35 g / cc.

[0272] In one embodiment, the density of the film is reduced by introducing many small voids or holes into the film or shaped article. This method is called "voiding", which may also be called "cavitating" or "microvoiding". The voids are obtained by incorporating about 1 to about 50 weight percent of small organic or inorganic particles (including glass microspheres) or "inclusions" (referred to in the art as "pore-forming" or "cavitating" agents) into the matrix polymer and stretching it in at least one direction to orient the polymer. During the stretching process, small holes or voids are formed around the pore-forming agent. When voids are introduced into the polymer film, the resulting void-containing film not only has a lower density than a void-free film, but also becomes opaque and forms a paper-like surface. This surface also has the advantage of improved printability; that is, the surface can accept a lot of ink with a significantly higher capacity than a void-free film. Typical examples of void-containing membranes are described in U.S. Pat. Nos. 3,426,754; 3,944,699; 4,138,459; 4,582,752; 4,632,869; 4,770,931; 5,176,954; 5,435,955; 5,843,578; 6,004,664; 6,287,680; 6,500,533; 6, 720,085; U.S. Patent Application Publication Nos. 2001 / 0036545; 2003 / 0068453; 2003 / 0165671; 2003 / 0170427; Japanese Patent Application Nos. 61-037827; 63-193822; 2004-181863; European Patent No. 0581970B1 and European Patent Application No. 0214859A2.

[0273] In certain embodiments, the extruded multilayer film is oriented while being stretched. Oriented multilayer films or multilayer shrinkable films of the present disclosure can be made of films with any thickness, depending on the desired end use. In one embodiment, the ideal condition is that the oriented film and / or shrinkable film can be printed with ink for use in applications including labels, photographic films that can be attached to substrates such as paper, and / or other applications that may be useful. It may be desirable to coextrude polyesters that can be used for the present disclosure with another polymer, such as PET, to make films that can be used for making oriented films and / or shrink films of the present disclosure. An advantage of the latter approach is that a bonding layer may not be required in some embodiments.

[0274] In one embodiment, the uniaxial and biaxially oriented films of the present disclosure may be made from films having a thickness of about 100 to 400 microns, such as extruded, cast or calendered films, which may be stretched at a ratio of 6.5:1 to 3:1 at a temperature of the film's Tg to Tg+55°C, and may be stretched to a thickness of 20 to 80 microns. In one embodiment, the orientation of the initial as-extruded film may be performed on a tenter according to these orientation conditions. The shrink film of the present disclosure may be made from the oriented film of the present disclosure.

[0275] In certain embodiments, the shrink films of the present disclosure shrink gradually with little to no wrinkling. In certain embodiments, the shrink films of the present disclosure have a transverse direction shrinkage of no greater than 40% per 5°C temperature increment.

[0276] In certain embodiments of the present disclosure, when immersed in 65°C water for 10 seconds, the shrink film of the present disclosure has a longitudinal shrinkage of 10% or less, or 5% or less, or 3% or less, or 2% or less, or no shrinkage. In certain embodiments of the present disclosure, when immersed in 65°C water for 10 seconds, the shrink film of the present disclosure has a longitudinal shrinkage of -10% to 10%, -5% to 5%, or -5% to 3%, or -5% to 2%, or -4% to 4%, or -3% to 4%, or -2% to 4%, or -2% to 2.5%, or -2% to 2%, or 0 to 2%, or no shrinkage. Negative longitudinal shrinkage percentages refer to longitudinal growth here. Positive longitudinal shrinkage refers to longitudinal shrinkage.

[0277] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure has a shrinkage in a major shrinking direction of 50% or more, or 60% or more, or 70% or more when immersed in 95°C water for 10 seconds.

[0278] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure has a shrinkage in the main shrinking direction in an amount of 50 to 90% and a longitudinal shrinkage of 10% or less, or -10% to 10%, when immersed in 95°C water for 10 seconds.

[0279] In one embodiment, the polyester useful in the present disclosure is made into a film using any method known in the art for producing films from polyesters, such as solution casting, extrusion, compression molding, or calendaring. The as-extruded (or as-formed) film is subsequently oriented in one or more directions (e.g., a uniaxially and / or biaxially oriented film). Such orientation of the film can be performed using standard orientation conditions by any method known in the art. For example, the uniaxially oriented film of the present disclosure can be made from a film having a thickness of approximately 100 to 400 microns, such as an extruded, cast, or calendared film, which can be stretched at a ratio of 6.5:1 to 3:1 at a temperature of the film's Tg to Tg+55°C, and can be stretched to a thickness of 20 to 80 microns. In one embodiment, the orientation of the initial as-extruded film can be performed on a tenter frame according to these orientation conditions.

[0280] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure has a transverse direction shrinkage of no greater than 40% per 5°C temperature increment.

[0281] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure may have a shrink initiation temperature of about 55 to about 80° C., or about 55 to about 75° C., or 55 to about 70° C. The shrink initiation temperature is the temperature at which shrinkage begins to occur.

[0282] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure may have a shrink initiation temperature of 55°C to 70°C.

[0283] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure may have a percent strain at break greater than 100% at a stretching speed of 300 mm / min in a direction perpendicular to the primary shrinking direction according to ASTM method D882.

[0284] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure may have a percent strain at break greater than 300% at a stretching speed of 300 mm / min in a direction perpendicular to the primary shrinking direction according to ASTM method D882.

[0285] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure may have a tensile stress at break (break stress) of 20 to 400 MPa; or 40 to 260 MPa; or 42 to 260 MPa, as measured according to ASTM method D882.

[0286] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure may have a shrink force of 2 to 18 MPa, or 4 to 15 MPa, measured by ISO method 14616, depending on the stretching conditions and the desired end use. For example, certain labels made for plastic bottles may have a shrink force of 4 to 8 MPa, and certain labels made for glass bottles may have a shrink force of 10 to 14 MPa measured by ISO method 14616 at 80°C using a Shrink Force Tester manufactured by LabThink.

[0287] In one embodiment of the present disclosure, the polyester composition may be formed by reacting monomers in a known process for making polyesters, which is generally referred to as a reactor grade composition.

[0288] In one embodiment of the present disclosure, the polyester composition of the present disclosure can be prepared by mixing polyesters such as polyethylene terephthalate (PET), glycol-modified PET (PETG), glycol-modified poly(cyclohexylene dimethylene terephthalate) (PCTG), poly(cyclohexylene dimethylene terephthalate) (PCT), acid-modified poly(cyclohexylene dimethylene terephthalate) (PCTA), poly(butylene terephthalate) and / or diethylene glycol-modified PET (EASTOBOND TM Copolyesters) are blended to achieve the monomer ranges for these compositions.

[0289] In certain embodiments, the polyester composition and polymer blend composition may also contain 0.01 to 25 weight % of common additives of the total composition, such as colorants, one or more toners, dyes, release agents, flame retardants, plasticizers, glass bubbles, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers and / or their reaction products, fillers and impact modifiers. Examples of commercially available impact modifiers include but are not limited to ethylene / propylene terpolymers, functionalized polyolefins, such as those containing methyl acrylate and / or glycidyl methacrylate, styrene-based block copolymer impact modifiers, and various acrylic core-shell impact modifiers. Residues of these additives are also expected to be part of the polyester composition.

[0290] Reinforcement materials can be added to the polyester compositions useful in the present disclosure. Reinforcement materials can include, but are not limited to, carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof. In one embodiment, the reinforcement material comprises glass, such as fiberglass filaments, a mixture of glass and talc, a mixture of glass and mica, and a mixture of glass and polymer fibers.

[0291] Molded articles, which may or may not consist of or contain a shrink film, may also be made from any of the polyester compositions disclosed herein and are included within the scope of the present disclosure.

[0292] Typically, the multilayer shrink film according to the present disclosure may contain 0.01 to 10 weight percent of a polyester plasticizer. In one embodiment, the multilayer shrink film may contain 0.1 to 5 weight percent of a polyester plasticizer. Typically, the multilayer shrink film may contain 90 to 99.99 weight percent of a copolyester. In certain embodiments, the multilayer shrink film may contain 95 to 99.9 weight percent of a copolyester.

[0293] In one embodiment, when having a pre-orientation thickness of about 100 to 400 microns and subsequently oriented on a tenter frame at a temperature of Tg to Tg+55°C at a ratio of 6.5:1 to 3:1 to a thickness of about 20 to about 80 microns, the multilayer shrink film of the present disclosure may have one or more of the following properties:

[0294] (1) when immersed in 95°C water for 10 seconds, a shrinkage in the main shrinkage direction or transverse direction of greater than 50% (or greater than 60% or greater than 70%), and a shrinkage in the longitudinal direction of 10% or less (or -5% to 4%); (2) a shrinkage initiation temperature of about 55°C to about 70°C; (3) a percent strain at break of greater than 100%, or 200 to 600%, or 200 to 500%, or 226 to 449%, or 250 to 455% in the transverse direction or in the longitudinal direction or in both directions at a stretching speed of 300 mm / min according to ASTM method D882; (4) a shrinkage of no more than 40% per 5°C temperature increment; and / or (5) a strain-induced crystalline melting point greater than 200°C. Any combination of these properties or all of these properties may be present in the shrink film of the present disclosure. The shrink film of the present disclosure may have a combination of two or more of the above shrink film properties. The shrink film of the present disclosure may have a combination of three or more of the above shrink film properties. The shrink film of the present disclosure may have a combination of four or more of the above shrink film properties. In certain embodiments, properties (1)-(2) are present. In certain embodiments, properties (1)-(5) are present. In certain embodiments, properties (1)-(3) are present, and so on.

[0295] The shrinkage percentages herein are based on an initially as-formed film having a thickness of about 20 to 80 microns that has been oriented on a tenter frame at a temperature of Tg to Tg+55° C. at a ratio of 6.5:1 to 3:1, such as oriented at a ratio of 5:1 at a temperature of 70° C. to 85° C. In one embodiment, the shrinkage properties of the oriented film used to make the shrink film of the present disclosure are not adjusted by annealing the film at a temperature above its orientation temperature.

[0296] The shape of the film that can be used to make the oriented multilayer film or multilayer shrink film of the present disclosure is not limited in any way. For example, it can be a flat film or a film that has been formed into a tube. In order to produce the multilayer shrink film that can be used in the present disclosure, the polyester is first formed into a flat film and then "uniaxially stretched", which means that the polyester film is oriented in one direction. The film can also be "biaxially oriented", which means that the polyester film is oriented in two different directions; for example, the film is stretched in the machine direction and in a direction different from the machine direction. Usually, but not always, the two directions are substantially perpendicular. For example, in one embodiment, the two directions are the longitudinal or machine direction ("MD") of the film (the direction in which the film is produced on the film making machine) and the transverse direction ("TD") of the film (the direction perpendicular to the MD of the film). The biaxially oriented film can be sequentially oriented, simultaneously oriented, or oriented by some combination of simultaneous and sequential stretching.

[0297] The multilayer film can be oriented by any common method, such as roller stretching, long gap stretching, tenter stretching and tubular stretching. By using any of these methods, it is possible to carry out sequential biaxial stretching, simultaneous biaxial stretching, uniaxial stretching or a combination of these. For the biaxial stretching mentioned above, longitudinal and transverse stretching can be carried out simultaneously. Stretching can also be carried out first in one direction and then in the other direction to produce effective biaxial stretching. In one embodiment, the film is stretched by preheating the film to 5°C to 80°C above its glass transition temperature (Tg). In one embodiment, the film can be preheated to 10°C to 30°C above its Tg. In one embodiment, the stretching rate is 5 to 20 inches (12.7 to 50.8 cm) / second. Then, the multilayer film can be oriented to 2 to 6 times the original measured value, for example, in the longitudinal, transverse or two directions. The multilayer film can be oriented as a single film layer, or it can be coextruded into a multilayer film with another polyester, such as PET (polyethylene terephthalate), and then oriented.

[0298] In one embodiment, the present disclosure includes a manufactured or shaped article comprising a multilayer shrink film of any multilayer shrink film embodiment of the present disclosure. In another embodiment, the present disclosure includes a manufactured or shaped article comprising a multilayer oriented film of any multilayer oriented film embodiment of the present disclosure.

[0299] In certain embodiments, the present disclosure includes, but is not limited to, multilayer shrink films applied to containers, plastic bottles, glass bottles, packaging, battery packs, hot-fill containers, and / or industrial articles, or other applications. In one embodiment, the present disclosure includes, but is not limited to, oriented films applied to containers, packaging, plastic bottles, glass bottles, photo substrates such as paper, battery packs, hot-fill containers, and / or industrial articles, or other applications.

[0300] In certain embodiments of the present disclosure, the multilayer shrink film of the present disclosure can be formed into a label or sleeve. The label or sleeve can then be applied to a finished product, such as a container wall, a battery pack, or applied to a sheet or film.

[0301] The multilayer oriented films or multilayer shrink films of the present disclosure can be applied to shaped articles, such as sheets, films, tubes, bottles, and are commonly used in various packaging applications. For example, films and sheets made from polymers such as polyolefins, polystyrenes, poly(vinyl chloride), polyesters, polylactic acid (PLA) are often used to make shrink labels for plastic beverage or food containers. For example, the multilayer shrink films of the present disclosure can be used in many packaging applications, wherein the multilayer shrink films applied to shaped articles exhibit properties such as good printability, high opacity, higher shrink force, good texture, and good stiffness.

[0302] The combination of improved shrink properties and improved toughness provides new commercial options including, but not limited to, multilayer shrink films for containers, plastic bottles, glass bottles, packaging, battery packs, hot fill containers and / or industrial articles or other applications.

[0303] In one aspect of the present disclosure, the disclosed polyester compositions can be used as thermoformed and / or thermoformable films or sheets. The present disclosure also relates to manufactured articles comprising one or more thermoformed films and / or sheets of the present disclosure. In one embodiment, the polyester compositions of the present disclosure can be used as films and sheets that are easily formed into shaped articles or molded articles. In one embodiment, one or more films and / or sheets of the present disclosure can be processed into molded articles or parts by thermoforming. The polyester compositions of the present disclosure can be used in various molding and extrusion applications.

[0304] In addition, in one embodiment, the polyester composition and polyester blend composition useful for one or more thermoformable sheets of the present disclosure may also contain 0.1 to 25 weight percent of the total composition of commonly used additives such as colorants, mold release agents, flame retardants, plasticizers, nucleating agents, stabilizers, including but not limited to UV stabilizers, heat stabilizers, fillers, and impact modifiers.

[0305] In one embodiment, reinforcing materials may be included in one or more thermoformed films or sheets comprising the polyester composition of the present disclosure. For example, suitable reinforcing materials may include carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, and polymer fibers and combinations thereof.

[0306] In one embodiment, the thermoformed film or sheet is a multilayer film or sheet.In one embodiment, at least one layer of the multilayer film or sheet is a foam or expanded polymer or polyester layer.

[0307] One aspect of the present disclosure is a method of making molded or formed parts and articles using thermoforming.Any thermoforming technique or method known to those skilled in the art can be used to produce the molded or formed articles of the present disclosure.

[0308] In one embodiment, the thermoforming process can be carried out in several ways, such as taught in "Technology of Thermoforming"; Throne, James; Hanser Publishers; 1996; pages 16-29, which is incorporated herein by reference. In some embodiments, it is a positive thermoforming process in which gas or air pressure is applied to the softened sheet, and the sheet is then stretched and drawn out like a bubble, and a male mold is introduced into the bubble from the inside. A vacuum is then applied to further pull the part and make the part follow the surface of the male mold. In this thermoforming process, biaxial stretching / orientation is mainly completed in one step when gas or air pressure is applied to the softened sheet. The molding step is then completed with the help of vacuum and male mold to fix the orientation into the sheet to achieve a good balance of physical and appearance properties. In other embodiments, it is a negative thermoforming process in which a vacuum or physical plug is applied to the heat softened sheet and stretches and pulls the sheet to approximately the final part dimensions, then positive air pressure from the inside or further external vacuum from the outside pulls the sheet and conforms the sheet to an external negative mold, fixing the orientation into the polymer and forming the sheet into the article.

[0309] In some embodiments, the generated bubbles are further shaped, sometimes with the aid of a plug, after which the sheet is covered and shaped on the rising male mold, and then the corners and shelf guides, etc., are pulled into the mold by applying a vacuum. In some embodiments, the molded parts or articles may be trimmed, punched, and chamfered as desired after removal from the mold.

[0310] In other embodiments, thermoforming is a process in which a film or sheet of the polyester composition of the present disclosure is heated to a temperature sufficient to deform it, and then the heated film or sheet is made to follow the contours of the mold by means such as vacuum assist, gas pressure assist, and matched mold assist. In another embodiment, the heated film or sheet is placed in a mold and forced to follow the contours of the mold by, for example, applying gas pressure, applying a vacuum, plunger assist, or applying a matched mold. In some embodiments, thermoforming produces thin-walled articles.

[0311] In one embodiment, thermoforming is molded into a desired shape by pressing a male mold into a heated film or sheet. In this embodiment, thermoforming involves supporting the male mold of the article between surfaces or countertops equipped with a vacuum. In this embodiment, the heat from an external heat source, such as a hot air blower, a heat lamp or other radiant heat source, is directed to the film or sheet. In this embodiment, the film or sheet is heated to a softening point. In this embodiment, a vacuum is then applied to the countertop and below the countertop and around the mold, and the heat-softened film or sheet is pulled toward the countertop, so that the softened film or sheet is contacted with the mold surface. In this embodiment, the vacuum pulls the softened film or sheet to a close contact and conformal with the profile of the mold surface. Therefore, the film or sheet then presents the shape of the mold. In this embodiment, after the film or sheet cools, it hardens, and the resulting article or component can be removed from the mold.

[0312] In one embodiment, the thermoforming process comprises: forming a film or sheet from the polyester composition of the present disclosure; heating the film or sheet until it softens and positioning it over a mold; drawing the preheated film or sheet onto the heated mold surface; cooling the film or sheet; and then removing the molded article or part from the mold cavity, or optionally, heat setting the formed film or sheet by maintaining the film or sheet in contact with the heated mold for a time sufficient to partially crystallize the film or sheet.

[0313] In one embodiment, the thermoforming process comprises: forming a film or sheet from the polyester composition of the present disclosure; heating the film or sheet to a temperature at or above the Tg of the polyester; applying gas, vacuum and / or physical pressure to the heat softened film or sheet and stretching the film or sheet to approximately the final part dimensions; causing the sheet to conform to the shape of the mold by the vacuum or pressure; cooling the film or sheet to a temperature below the Tg of the polyester; and then removing the thermoformed article or part from the mold.

[0314] Films and sheets for thermoforming can be made by any conventional method known to those skilled in the art. In one embodiment, the film or sheet is formed by extrusion. In one embodiment, the film or sheet is formed by calendaring. In one embodiment, during the thermoforming process, the film or sheet is heated to a temperature at or above the Tg of the polyester. In one embodiment, the temperature is about 10°C to about 60°C higher than the Tg of the polyester. In one embodiment, in order to achieve a shorter molding time, the heating of the film or sheet before being positioned above the thermoforming mold is necessary. In one embodiment, the sheet must be heated to a temperature above its Tg and below that at which it sags excessively during positioning above the mold cavity. In one embodiment, before removing the molded film or sheet from the mold, it is cooled to a temperature below the Tg of the polyester. In one embodiment, the thermoforming process may include vacuum assistance, air assistance, mechanical plunger assistance or matching molds. In some embodiments, the mold is heated to a temperature at or above the Tg of the film or sheet. The selection of the optimal mold temperature depends on the type of thermoforming equipment, the configuration and wall thickness of the molded article, and other factors.

[0315] In some embodiments, the heated film or sheet is stretched by establishing and withdrawing a vacuum.

[0316] In one embodiment, heat setting is a process of heat-inducing partial crystallization of a polyester film or sheet without significant orientation. In one embodiment, heat setting is achieved by maintaining the film or sheet in contact with a heated mold surface for a sufficient time to achieve a level of crystallinity that provides adequate physical properties for the finished part. In one embodiment, the level of crystallinity should be from about 10% to about 30%.

[0317] In one embodiment, the heat-set component can be removed from the mold cavity by known removal means. For example, in one embodiment, backblowing is used and involves breaking the vacuum established between the mold and the formed film or sheet by introducing compressed air. In some embodiments, the molded article or component is then trimmed and the waste is ground and recycled.

[0318] In some embodiments, the addition of nucleating agents provides faster crystallization during the thermoforming process, and therefore provides faster molding. In one embodiment, nucleating agents such as fine-grained inorganic or organic materials can be used. For example, in one embodiment, suitable nucleating agents include talc, titanium dioxide, calcium carbonate, and immiscible or cross-linked polymers. In one embodiment, the amount of nucleating agent is about 0.01% to about 20% of the weight of the article. In one embodiment, other conventional additives such as pigments, dyes, plasticizers, anti-cracking agents, and stabilizers can be used according to the needs of thermoforming. In some embodiments, anti-cracking agents improve impact strength, and nucleating agents provide faster crystallization. In some embodiments, crystallization is necessary to achieve high temperature stability.

[0319] In one embodiment, the polyester composition of the present disclosure is foamed by chemical and / or physical foaming agents, the foamed polyester is extruded into a sheet or film, and the foamed polyester film or sheet is thermoformed to make a foamed polyester film or sheet. Before foaming, additives for providing enhanced properties for the foamed polyester film can be added to the polyester. Some examples of additives include slip agents, anti-blocking agents, plasticizers, fluorescent whitening agents, and ultraviolet inhibitors. In one embodiment, the foamed polyester film can be extruded or laminated on one or both sides using conventional techniques to enhance its properties. In one embodiment, the coating material can be a printed surface providing a product label, rather than the foam film itself.

[0320] The composition of the present disclosure can be used as molded or formed plastic parts or as solid plastic objects. The composition of the present disclosure can be used as thermoformed parts or products. The composition is suitable for any application requiring clear hard plastics. Examples of such parts include disposable knives, forks, spoons, plates, cups, straws and eyeglass frames, toothbrush handles, toys, car decorations, tool handles, camera parts, parts of electronic devices, razor parts, ink pen holders, disposable syringes, bottles, etc. In one embodiment, the composition of the present disclosure can be used as plastics, films, fibers and sheets. In one embodiment, the composition can be used as the plastics for making bottles, bottle caps, eyeglass frames, cutlery, disposable cutlery, cutlery handles, shelves, shelf dividers, electronic housings, electronic equipment housings, computer monitors, printers, keyboards, pipelines, automotive parts, automotive interior parts, automotive decorations, logos, thermoformed letters, sidings, toys, thermally conductive plastics, ophthalmic lenses, tools, tool handles and utensils. In another embodiment, the compositions of the present disclosure are suitable for use as films, sheets, fibers, molded articles, formed articles, molded parts, formed parts, medical devices, dental trays, dental appliances, containers, food containers, shipping containers, packaging, bottles, bottle caps, eyeglass frames, cutlery, disposable cutlery, cutlery handles, shelves, shelf dividers, furniture components, electronic housings, electronic equipment housings, computer monitors, printers, keyboards, pipes, toothbrush handles, automotive parts, automotive interior parts, automotive decoration, signs, outdoor signs, skylights, multi-wall films, multi-layer films, insulation parts, insulation articles, insulation containers, thermoformed letters, siding, toys, toy parts, trays, food trays, dental trays, thermally conductive plastics, ophthalmic lenses and frames, tools, tool handles and utensils, health care products, commercial food service products, boxes, films for graphic arts applications, plastic films for plastic glass laminates, end-of-sale displays, skylights, smoke vents, laminated cards, fenestrations, glazing, partitions, ceilings, lighting, machine covers guards, graphic arts, lenses, extruded laminated sheets or films, decorative laminates, office furniture, face masks, medical packaging, point of sale shelf sign holders and shelf price holds.

[0321] The present thermoformable or thermoformable compositions can be used to form films, molded articles, molded parts, shaped articles, formed parts and sheets. The method of making the thermoformable or thermoformable compositions into films, molded articles, molded parts, shaped articles, formed parts and sheets can be according to any method known in the art. Examples of molded articles include, but are not limited to, medical devices, medical packaging, health care products, commercial food service products, such as trays, containers, food trays, tumblers, storage boxes, bottles, food processors, blenders and mixer bowls, utensils, water bottles, crisper trays, washing machine parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses and frames and toys.

[0322] One embodiment of the present disclosure is a method for making a thermoformed film or sheet, comprising: A. heating a polyester film or sheet; B. applying air pressure, vacuum and / or physical pressure to the heat-softened film or sheet; C. causing the sheet to conform to the shape of a mold by vacuum or pressure; and D. removing the thermoformed part or article from the mold.

[0323] The present disclosure further relates to manufactured articles comprising one or more films and / or sheets comprising the polyester compositions described herein.In embodiments, the films and / or sheets of the present disclosure may be any thickness desired for the intended application.

[0324] The present disclosure further relates to one or more films and / or sheets as described herein. The method of molding the polyester composition into one or more films and / or sheets includes any method known in the art. The examples of one or more films and / or sheets disclosed herein include, but are not limited to, one or more extruded films and / or sheets, one or more calendered films and / or sheets, one or more compression molded films and / or sheets, one or more solution cast films and / or sheets. The method of manufacturing films and / or sheets includes, but is not limited to, extrusion, calendering, compression molding, wet block processing, dry block processing, and solution casting.

[0325] The present disclosure further relates to molded or shaped articles as described herein. Methods for molding the polyester composition into molded or shaped articles include any known methods in the art. Examples of molded or shaped articles of the present disclosure include, but are not limited to, thermoformed or thermoformable articles, injection molded articles, extrusion molded articles, injection blow molded articles, injection stretch blow molded articles, and extrusion blow molded articles. Methods for making molded articles include, but are not limited to, thermoforming, injection molding, extrusion, injection blow molding, injection stretch blow molding, and extrusion blow molding. The methods of the present disclosure may include any thermoforming method known in the art. The methods of the present disclosure may include any blow molding method known in the art, including, but not limited to, extrusion blow molding, extrusion stretch blow molding, injection blow molding, and injection stretch blow molding.

[0326] The present disclosure includes any injection blow molding manufacturing method known in the art. Although not limited thereto, a typical description of an injection blow molding (IBM) manufacturing method includes: 1) melting a composition in a reciprocating screw extruder; 2) injecting the molten composition into an injection mold to form a partially cooled tube (i.e., a preform) closed at one end; 3) moving the preform into a blow mold having a desired finished shape around the preform, and closing the blow mold around the preform; 4) blowing air into the preform to stretch and expand the preform to fill the mold; 5) cooling the molded product; 6) ejecting the product from the mold.

[0327] The present disclosure includes any injection stretch blow molding manufacturing method known in the art. Although not limited thereto, a typical description of the injection stretch blow molding (ISBM) manufacturing method includes: 1) melting a composition in a reciprocating screw extruder; 2) injecting the molten composition into an injection mold to form a partially cooled tube (i.e., a preform) closed at one end; 3) moving the preform into a blow mold having a desired finished shape around the preform, and closing the blow mold around the preform; 4) stretching the preform using an internal stretch rod, and blowing air into the preform to stretch and expand the preform to fill the mold; 5) cooling the molded product; 6) ejecting the product from the mold.

[0328] The present disclosure includes any extrusion blow molding manufacturing method known in the art. Although not limited thereto, a typical description of the extrusion blow molding manufacturing method includes: 1) melting a composition in an extruder; 2) extruding the molten composition through a die to form a tube (i.e., a parison) of molten polymer; 3) locking a mold having a desired finished shape around the parison; 4) blowing air into the parison to stretch and expand the extrudate to fill the mold; 5) cooling the molded article; 6) ejecting the article from the mold; and 7) removing excess plastic (commonly referred to as flash) from the article.

[0329] The following examples further illustrate how the polyesters of the present disclosure can be made and evaluated, and they are intended to be exemplary only and not intended to limit the scope thereof. Unless otherwise indicated, parts are parts by weight, temperatures are in ° C (Celsius) or at room temperature, and pressures are at or near atmospheric pressure.

[0330] The following examples further illustrate how the polyesters of the present disclosure can be made and evaluated, and they are intended to be exemplary only and not intended to limit the scope thereof. Unless otherwise indicated, parts are parts by weight, temperatures are in ° C (Celsius) or at room temperature, and pressures are at or near atmospheric pressure. Example

[0331] The present disclosure may be further illustrated by the following examples of embodiments, but it is to be understood that these examples are included for illustration purposes only and are not intended to limit the scope of the present disclosure unless expressly specified otherwise.

[0332] Description of general multilayer film manufacturing methods and property test

[0333] The multilayer heat-shrinkable polyester films in the examples were prepared and evaluated by a method comprising the following steps:

[0334] (a) melting and extruding a random copolymer resin in a specific layer structure to obtain an unstretched A|B|A three-layer film;

[0335] (b) stretching the unstretched multilayer film in one direction;

[0336] (c) evaluation of various film properties (including glass transition temperature (Tg), strain-induced melting point (Tm), shrinkage with temperature (shrinkage curve), tensile test, and shrinkage force (SF)), and

[0337] (d) The recyclability of the membranes was evaluated by clump testing.

[0338] Multilayer structure / composition range

[0339] A multilayer film comprising three layers - an ABA structure - is shown in Scheme 1.

[0340] The first and second skin layers (layer A) contain a blend of amorphous copolyester resin 1 and crystallizable resin 2.

[0341] The weight ratio (wt %) of the resin 1 and the resin 2 is 0 / 100 to 30 / 70.

[0342] The composition of the copolyester blend in layer A comprises the following residues:

[0343] (A) a diacid component containing at least 70 mole % of terephthalic acid residues

[0344] (B) a diol component comprising

[0345] (i) about 50 to about 90 mole % EG residues,

[0346] (ii) about 1-35 mol % CHDM residues,

[0347] (iii) 0-30 mol% NPG residues, and

[0348] (iv) 0.1-15 mol% of DEG residues,

[0349] The final polymer contains substantially equal molar proportions of acid equivalents (100 mole %) and diol equivalents (100 mole %), with all reactants totaling 200 mole %.

[0350] The core layer (layer B) disposed between the first and second skin layers is composed of a blend of amorphous copolyester resin 1 and crystallizable copolyester resin 3 .

[0351] The weight ratio of resin 1 to resin 3 in the core layer is 80 / 20-40 / 60.

[0352] The composition of the copolyester blend in layer B comprises the following residues:

[0353] (C) a diacid component containing at least 70 mole % of terephthalic acid residues

[0354] (D) a diol component comprising

[0355] (i) about 50 to about 95 mole % EG residues,

[0356] (ii) 0 to 25 mol% CHDM residues, more preferably 5 to 15 mol%, and

[0357] (iii) 0.1-15 mol% of DEG residues, more preferably 5-12 mol%

[0358] The final polymer contains substantially equal molar proportions of acid equivalents (100 mole %) and diol equivalents (100 mole %), with all reactants totaling 200 mole %.

[0359]

[0360] Table 1. Resins used in multilayer films

[0361]

[0362] Table 2. Multilayer structure

[0363]

[0364] Membrane property range

[0365] With respect to thermal properties in each layer, the first and second skin layers (layer A) contain at least 50% by weight of a crystallizable resin 2 having a Tm ≥ 190° C., more preferably a Tm ≥ 200° C., as measured by differential scanning calorimetry (DSC) in the second scan at a scan rate of 20° C. / min. The third layer (layer B) disposed between the first and second layers preferably has no more than 95% by weight, more preferably no more than 80% by weight of an amorphous copolyester resin 1 having a Tg ≤ 78° C., as measured by DSC.

[0366] The third layer (Layer B) disposed between the first and second layers has rPET (Resin 3) of 0.1-90 wt% rPET, with a preferred range of 10 wt%-70 wt%; a more preferred range of 20 wt%-60 wt%.

[0367] With respect to the film thickness in each layer, if measured, prior to stretching, the first and second skin layers (layer A) preferably have a thickness in the range of 1-4 mils and the third layer (layer B) preferably has a thickness in the range of 2-8 mils.

[0368] The desired properties of the shrink film made with this multilayer structure include: (a) an ultimate shrinkage rate of at least 50%, preferably 70% or more in the main shrinking direction (transverse direction, TD), which gradually increases with increasing temperature; (b) the shrinkage rate in the direction perpendicular to the main shrinking direction at 80°C should be negative (i.e., increasing) or no shrinkage; (c) the final shrink film should also have a shrink force of less than 10 MPa measured at 80°C; (d) a break strain percentage greater than 100% at a tensile speed of 300 mm / min in the longitudinal direction (MD, the direction perpendicular to the main shrinking direction).

[0369] Film Recyclability. Shrink films heated together with rPET bottle flakes (with 3 wt% shrink film) at 208°C for 90 minutes exhibited <5% blocking, more preferably <1% blocking as measured by the blocking test described in the experimental section.

[0370] For good film physical properties and film processability, the film preferably has an inherent viscosity (IV) of 0.5-0.9 dL / g, more preferably 0.55-0.7 dL / g.

[0371] Film manufacturing method

[0372] The method for preparing the multilayer film comprises drying the polymer pellets at 135°F for 4-6 hours, melt extruding at 220°C-300°C, more preferably 240°C-260°C in a B230 via a 1" Killion extruder to obtain an unstretched film. The unstretched film is stretched about 3-6 times of the original size in one direction at 70°C-100°C, more preferably about 3-5 times at 70°C-90°C using a Bruckner Karo machine. The thickness of the heat-shrinkable polyester film prepared according to the present invention may be 20 μm to 80 μm, preferably 30 μm to 50 μm. Various film properties of the stretched film are evaluated, including glass transition temperature (Tg), strain induced melting point (Tm), shrinkage with temperature (shrinkage curve), tensile test and shrinkage force (SF) and (e) the recyclability of the film is evaluated by a blocking test.

[0373] Analytical test

[0374] Inherent Viscosity (IV) - IV was measured in a 60 / 40 parts by weight solution of phenol / tetrachloroethane at 250°C and at a concentration of approximately 0.5 grams of polymer per 100 milliliters of the solvent.

[0375] Film Glass Transition Temperature (Tg) and Melting Temperature (Tm) All thermal testing of the pellets and stretched films was done under standard Differential Scanning Calorimetry (DSC) scans at a scan rate of 20°C / min.

[0376] Shrinkage force (SF) - Shrinkage force was determined using a Labthink FST-02 Shrinkage Force Tester. Shrinkage force measurements were performed at the same temperature conditions as the stretching temperature (80°C) used to stretch the film on a Bruckner and kept in a heated chamber for 60 seconds - to determine the maximum shrinkage force value for each film.

[0377] Shrinkage - Shrinkage is measured by placing a 50mm x 50mm square film sample in water at a temperature of 60°C to 95°C for 10 seconds without restraining the shrinkage in any direction. The % shrinkage is then calculated using the following equation

[0378] % Shrinkage rate = [(50mm-length after shrinkage) / 50mm] x 100%

[0379] Shrinkage is measured in the direction perpendicular to the main shrinkage direction (machine direction, MD) and also in the main shrinkage direction (transverse direction, TD).

[0380] Negative contraction rate indicates growth

[0381] Tensile Properties - The MD strain at break of the films was tested using ASTM method D 882. The films were prepared by cutting them into 3.5" x 0.5" strips and tested at a tensile speed of 300 mm / min.

[0382] PET Blocking - Blocking testing of these compositions was conducted by first shrinking the stretched film at 85°C for 10 seconds and chopping the shrunk material to make shrunk bottle flakes. 18 grams of the shrunk bottle flakes were then combined with 582 grams of PET bottle flakes and spread evenly into an aluminum cooking pan, ensuring that the material depth was 1.5". The pan was placed in a forced air oven set at 208°C for 90 minutes and allowed to cool, then the percentage of blocking was evaluated using the following formula.

[0383] [(remaining material + weight of pot) - (weight of pot) / (600g)] x 100 = degree of caking (%)

[0384] Comparative Example

[0385] Note: Notes on shrink film properties in the table below

[0386] Good: Desirable properties of shrink films made with this multilayer structure include:

[0387] • An ultimate shrinkage in the main shrinkage direction (transverse direction, TD) of at least 50%, preferably 70% or more, which gradually increases with increasing temperature.

[0388] • A shrinkage at 70°C in the main shrinkage direction of at least 5%.

[0389] The shrinkage at 80°C in the direction perpendicular to the main shrinkage direction should be negative (i.e. growth) or no shrinkage;

[0390] The final shrink film should also have a shrink force of less than 10 MPa measured at 80°C;

[0391] • A percent strain at break greater than 100% at a tensile speed of 300 mm / min in the machine direction (MD, the direction perpendicular to the main shrinkage direction).

[0392] Shrink film dried with PET bottle flakes in an oven at 208°C for 90 minutes showed <1% blocking.

[0393] Not good: Shrink film performance does not meet the criteria for "good"

[0394] Comparative Example

[0395] The compositions and film properties of the comparative examples are shown in Table 3 below.

[0396] Table 3

[0397]

[0398]

[0399] Table 4 - Example 1-2: Resin 1 / Resin 2 Blend | Resin 1 / Resin 2 Blend | Resin 1 / Resin 2 Blend

[0400]

[0401]

[0402] Table 5 - Examples 3-6: Resin 1 / Resin 2 Blends | Resin 1 / rPET Blends | Resin 1 / Resin 2 Blends

[0403]

[0404]

[0405] The disclosure has been described in detail with particular reference to preferred embodiments thereof, but it will be understood that variations and modifications can be effected within the spirit and scope of the disclosure.

Claims

1. A multilayer crystallizable film comprising at least one skin layer (A), wherein the skin layer (A) comprises a polyester composition, wherein the polyester composition comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 75 mol % or more of ethylene glycol residues and About 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole percent neopentyl glycol residues; (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and At least one core layer (B), said core layer (B) comprising a blend of: 30 to 100 wt. % of at least one polyester composition comprising: At least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 90 to about 100 mole percent terephthalic acid residues; (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 60 mol % or more of ethylene glycol residues and About 40 mole % or less of other diols, the other diols comprising one or more of: (i) from 15 mole % to less than about 30 mole % of 1,4-cyclohexanedimethanol residues; (ii) from about 7 mole % to less than about 15 mole % of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and 0-70 wt. % of at least one polyester composition comprising: At least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 50 mol % or more of ethylene glycol residues and About 50 mole % or less of other diols, the other diols comprising one or more of: (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues; (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues or butanediol residues in the final polyester composition; The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

2. A multilayer crystallizable film comprising at least one skin layer (A), said skin layer (A) comprising a blend of 50-99.9 wt. % of at least one polyester composition (1) and 0.1-50 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 75 mol % or more of ethylene glycol residues and About 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole percent neopentyl glycol residues; (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (2) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 90 to about 100 mole percent terephthalic acid residues; (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 60 mol % or more of ethylene glycol residues and About 40 mole % or less of other diols, the other diols comprising one or more of: (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues; (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and at least one core layer (B), said core layer (B) comprising a blend of 30-95 wt. % of at least one polyester composition (1) and 5-70 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 90 to about 100 mole percent terephthalic acid residues; (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 60 mol % or more of ethylene glycol residues and About 40 mole % or less of other diols, the other diols comprising one or more of: (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues; (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (2) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 50 mole % or more of ethylene glycol residues and about 50 mole % or less of other glycols, the other glycols comprising one or more of: (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues; (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues or butanediol residues in the final polyester composition; The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

3. A multilayer crystallizable film comprising at least one skin layer (A), said skin layer (A) comprising a blend of 50-99.9 wt. % of at least one polyester composition (1) and 0.1-50 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 75 mol % or more of ethylene glycol residues and About 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole percent neopentyl glycol residues; (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (2) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 90 to about 100 mole percent terephthalic acid residues; (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 60 mol % or more of ethylene glycol residues and About 40 mole % or less of other diols, the other diols comprising one or more of: (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues; (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and at least one core layer (B), said core layer (B) comprising a blend of 20-30 wt. % of at least one polyester composition (1) and 40-60 wt. % of at least one polyester composition (2) and 20-30 wt. % of at least one polyester composition (3), said polyester composition (1) comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 75 mol % or more of ethylene glycol residues and About 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole percent neopentyl glycol residues; (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (2) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 90 to about 100 mole percent terephthalic acid residues; (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 60 mol % or more of ethylene glycol residues and About 40 mole % or less of other diols, the other diols comprising one or more of: (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues; (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (3) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 50 mol % or more of ethylene glycol residues and About 50 mole % or less of other diols, the other diols comprising one or more of: (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues; (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues or butanediol residues in the final polyester composition; The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

4. A multilayer crystallizable film comprising at least one skin layer (A), said skin layer (A) comprising a blend of 50-70 wt. % of at least one polyester composition (1) and 30-50 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 75 mol % or more of ethylene glycol residues and About 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole percent neopentyl glycol residues; (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (2) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 90 to about 100 mole percent terephthalic acid residues; (ii) from about 0 to about 10 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 60 mol % or more of ethylene glycol residues and About 40 mole % or less of other diols, the other diols comprising one or more of: (i) 15 mol % to less than 30 mol % of 1,4-cyclohexanedimethanol residues; (ii) 7 mol % to less than 15 mol % of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and at least one core layer (B), said core layer (B) comprising a blend of 30-50 wt. % of at least one polyester composition (1) and 50-70 wt. % of at least one polyester composition (2), said polyester composition (1) comprising: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 75 mol % or more of ethylene glycol residues and About 25 mole % or less of other diols, the other diols comprising one or more of: (i) from about 0 to less than about 24 mole percent neopentyl glycol residues; (ii) 0 to less than about 24 mole % of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 15 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; wherein the total mole % of the dicarboxylic acid components is 100 mole %, and wherein the total mole % of the diol components is 100 mole %; and The polyester composition (2) comprises: at least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 50 mol % or more of ethylene glycol residues and About 50 mole % or less of other diols, the other diols comprising one or more of: (i) 0 mole % to less than about 50 mole % of 1,4-cyclohexanedimethanol residues; (ii) from about 0.1 mole % to less than about 15 mole % of the total diethylene glycol residues or butanediol residues in the final polyester composition; The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

5. The multilayer crystallizable film of claim 1, wherein the polyester composition comprises: At least one polyester comprising: (a) a dicarboxylic acid component comprising: (i) from about 70 to about 100 mole percent of terephthalic acid residues; (ii) from about 0 to about 30 mole % of aromatic and / or aliphatic dicarboxylic acid residues having up to 20 carbon atoms; and (b) a diol component comprising: About 80 mol % or more of ethylene glycol residues and About 20 mole % or less of other diols, the other diols comprising one or more of: (i) from about 5 to less than about 17 mole percent neopentyl glycol residues; (ii) from about 2 to less than about 10 mole percent of 1,4-cyclohexanedimethanol residues; (iii) from about 1 to less than about 10 mole percent of the total diethylene glycol residues or butanediol residues in the final polyester composition; The total mol % of the dicarboxylic acid components therein is 100 mol %, and the total mol % of the diol components therein is 100 mol %.

6. The multilayer crystallizable film according to any one of claims 1 to 5, wherein the film has an ABA configuration.

7. The multilayer crystallizable film of any one of claims 1-6, wherein the film is a heat shrinkable film; or wherein the film is stretched in at least one direction; or wherein the film is oriented in one or more directions; or wherein the film is stretched and oriented in at least one direction; or wherein the film is annealed; or wherein the film is annealed at a temperature of about 75°C to about 110°C.

8. The multilayer crystallizable film of any one of claims 1-7, wherein the film has a crystalline melting point of 190°C to 225°C, or 190°C to 245°C, or 150°C to 245°C; or wherein the film is stretched in at least one direction and the stretched film has a strain-induced crystalline melting point of 200°C or higher; or 195°C or higher; or 180°C or higher; or 150°C or higher.

9. The multilayer crystallizable film according to any one of claims 1 to 8, wherein when immersed in 85°C water for 10 seconds, the film has a shrinkage in the main shrinkage direction of 60% or more; or wherein when immersed in 85°C water for 10 seconds, the film has a shrinkage in the main shrinkage direction of 50% or more; or wherein when immersed in 95°C water for 10 seconds, the film has a shrinkage in the main shrinkage direction of 50 to 90% and a shrinkage in a direction perpendicular to the main shrinkage direction of 10% or less.

10. The multilayer crystallizable film of any one of claims 1-9, wherein the film has a shrink force of 5 MPa or greater; or wherein the film has a shrink force of less than 10 MPa; or wherein the film has a percent strain at break greater than 100%.

11. The multilayer crystallizable film according to any one of claims 1 to 10, further comprising at least one pore former.

12. A lidding film, an extrusion blow molded container, an extruded sheet, a thermoformed sheet, a flexible packaging film for a stand-up pouch, comprising the multilayer crystallizable film according to any one of claims 1 to 11.

13. A manufactured article, shaped article, container, plastic bottle, glass bottle, package, battery, hot fill container or industrial article having applied thereto a label or sleeve comprising the multilayer crystallizable film according to any one of claims 1 to 12.

14. The multilayer crystallizable film of any one of claims 1 to 12, wherein the film is used in an application selected from the group consisting of medical device packaging, medical packaging, pharmaceutical supplies, pharmaceutical packaging, blister packaging, healthcare supply packaging, commercial food service products, trays, containers, food trays, tumblers, storage bins, bottles, food processors, blender and mixer bowls, utensils, water bottles, crisper containers, washing machine parts, refrigerator parts, vacuum cleaner parts, ophthalmic lenses and frames, or toys.

15. The multilayer crystallizable film according to any one of claims 1 to 14, wherein the film is recyclable in a PET recycle stream.

16. A polyester recycle stream comprising recycled poly(ethylene terephthalate) bottle flakes and admixed therewith at least about 0.1 wt. % of recycled multilayer crystallizable film according to any one of claims 1 to 15.

17. The polyester recycle stream of claim 16, comprising recycled polyethylene terephthalate bottle flakes and at least about 0.1 weight percent of a multilayer crystallizable recycled shrink film mixed therewith, wherein the stream passes the "Critical Guidance Protocol for Clear PET Articles with Labels and Closures", File No. PET-CG-02, dated April 11, 2019.

18. The multilayer crystallizable film according to any one of claims 1 to 5, further comprising at least one polyester composition having recycled content; or wherein the polyester composition comprises recycled PET; or wherein the EG of the polyester composition is recycled EG (rEG); or wherein the CHDM of the polyester composition is recycled CHDM (rCHDM) or the CHDM is made from recycled DMT (rDMT); or wherein at least a portion of the dicarboxylic acid residues and / or diol residues are derived from (i) recycled monomer species selected from rDMT, rTPA, rDMI, rEG, rDEG and rCHDM and (ii) rPET.

19. The multilayer crystallizable film according to any one of claims 1 to 5, wherein the inherent viscosity of the film measured at 25°C at a concentration of 0.5 g / dL in 60 / 40 (wt / wt) phenol / tetrachloroethane is from 0.50 to 0.80 dL / g, and / or wherein the film has a Tg of 65°C to 80°C measured using a TA DSC 2920 from Thermal Analyst Instrument at a scan rate of 20°C / min.

20. The multilayer crystallizable film of any one of claims 1-5, wherein the film has less than 1% PET agglomeration as measured in accordance with "Critical Guidance Protocol for Clear PET Articles with Labels and Closures", File No. PET-CG-02, dated April 11, 2019.

Citation Information

Patent Citations

  • Crystallizable shrinkable and thermoformable sheets made from reactor grade resins

    CN112789155A

  • Crystallizable shrinkable films and thermoformable sheets made from resin blends

    CN112789156A

  • Recyclable molded articles from blends of copolyesters and recycled pet

    CN113785002A

  • Porous polyester film

    US20010036545A1

  • Thermoformable Copolyester Laminate

    US20130236612A1