Single-component rigid polymer cement-based waterproof mortar and preparation method thereof
By using composite powder modified by silane coupling agent in polymer cement waterproof mortar to form a compact structure, the problem of cracking and deterioration in transportation of cement-based waterproof mortar is solved, and the problem of cement-based waterproof mortar cracking during curing and deterioration during transportation is achieved. The high compression resistance and waterproof performance are improved, and the tensile bonding strength requirements of ceramic tile adhesives are met, replacing the use of ceramic tile adhesives.
Patent Information
- Application Number
- CN202410982816.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polymer cement waterproof mortars are cracked and shedded due to cement shrinkage stress during the curing process, and the two-component products are easily freezed or microbial erosion and deterioration during transportation and storage, which affects their performance.
Using a single-component rigid polymer cement-based waterproof mortar, composite polymerization is carried out by amorphous SiO2-Al2O3 composite powder, cellulose ether, redispersible latex powder, defoaming agent and dispersant modified with silane coupling agent. The additives form a compact membrane structure and a crisscrossing mesh structure, improve compression, cracking and waterproofing properties, and reduce water absorption through hydrophobic agents.
It significantly improves the compressive strength and waterproof and crack resistance of the mortar, meets the standard requirements of JC/T984-2011 "Polymer Cement Waterproof Mortar", and can replace ceramic tile adhesives, and meets the provisions of JC/T547-2017 "Ceramic Tile Adhesives" The tensile bonding strength performance improves the construction efficiency and the application scope of materials.
Smart Images

Figure BDA0004956565690000021 
Figure BDA0004956565690000022 
Figure BDA0004956565690000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement-based waterproof mortar, and specifically relates to a single-component rigid polymer cement-based waterproof mortar and a preparation method thereof. Background Art
[0002] The surface of waterproof coating is relatively smooth after drying and forming a film, but rigid waterproof mortar is different from this. Rigid waterproof mortar can effectively resist the deformation of the system, and the surface is rough after forming a film, with greater strength and good adhesion with the subsequent processes. It is mainly suitable for roofing, exterior wall waterproofing, anti-seepage projects and underground (such as pile heads, garages, tunnels, etc.) waterproofing projects, which are continuous moisture-proof and indirect waterproofing areas. The new waterproofing regulations came into effect on April 1, 2023, and mandatory requirements were put forward for exterior wall waterproofing. According to market feedback, roofs, exterior walls and underground garages are all areas with serious leakage points, and the demand for waterproof materials has greatly increased.
[0003] Mortar is mainly made of a mixture of sand, cement, rubber powder, cellulose ether, etc. During the curing process, the mortar will crack and fall off due to the shrinkage stress of the cement itself, resulting in water seepage. Polymer cement-based mortar is a waterproof material made of polymers and additives as modified materials and mixed in a fine ratio.
[0004] At present, people usually use polymer emulsion modified mortar to treat waterproof parts. This method is called two-component polymer cement waterproof slurry / coating. Two-component products have difficulties in packaging, transportation and storage. Improper storage will affect the performance of the mortar, and the emulsion may also be frozen or microbially eroded and deteriorated. Single-component waterproof mortar only needs to be added with water and stirred before use, which greatly improves construction efficiency. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a one-component rigid polymer cement-based waterproof mortar and a preparation method thereof. The one-component rigid polymer cement-based waterproof mortar can significantly improve the compressive strength and waterproof and crack resistance of the mortar. While meeting and exceeding the requirements of the JC / T984-2011 "Polymer Cement Waterproof Mortar" standard, it can also meet the five tensile bonding strength properties of cement-based adhesives specified in JC / T547-2017 "Ceramic Tile Adhesives", and can be used as a cement-based adhesive instead of tile adhesives.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A one-component rigid polymer cement-based waterproof mortar, comprising the following raw materials in parts by weight:
[0008]
[0009] The active additive is amorphous SiO modified by a silane coupling agent. 2 -Al 2 O 3 Composite powder; amorphous SiO 2 -Al 2 O 3 SiO in composite powder 2 The weight percentage is more than 90%;
[0010] The composite polymer additive consists of cellulose ether, redispersible latex powder, defoamer and dispersant;
[0011] The dosage of the waste rock powder and active additives is not 0 at the same time.
[0012] The one-component rigid polymer cement-based waterproof mortar preferably comprises the following raw materials in parts by weight:
[0013]
[0014]
[0015] Furthermore, the composite polymer additive is composed of cellulose ether, redispersible latex powder, defoamer and dispersant in a mass ratio of 0.05-0.15:1.5-2.5:0.05-0.15:8-12, preferably in a mass ratio of 0.1:2:0.1:10.
[0016] Furthermore, the cellulose ether is hydroxypropyl methylcellulose ether; the defoamer is polyether defoamer AGITAN RP803 type, and the dispersant is limestone powder below 200 meshes.
[0017] The redispersible latex powder is ethylene-vinyl acetate copolymer rubber powder.
[0018] The silicate cement is 42.5 ordinary silicate cement.
[0019] The machine-made sand is limestone machine-made sand, and 0.075-0.15 mm limestone fine sand, 0.15-0.3 mm limestone fine sand and 0.3-0.6 mm limestone fine sand are used in combination.
[0020] The waste rock powder is recycled powder produced by the machine-made sand production line, and the particle size of the waste rock powder is less than 200 meshes.
[0021] The water repellent is a powdered silane-based water repellent, preferably a 200-mesh SEAL80 powdered silane-based water repellent, model SYLCOP TM 50 / 50;
[0022] The water reducing agent is a polycarboxylic acid water reducing powder, and the water reducing rate is ≥25%.
[0023] The silane coupling agent modified fiber is a silane coupling agent modified polypropylene fiber, wherein the length of the polypropylene fiber is 3-6 mm.
[0024] When used, the one-component rigid polymer cement-based waterproof mortar is mixed according to a mass ratio of powder: water = 1: 0.15-0.23.
[0025] The present invention also provides a method for preparing the single-component rigid polymer cement-based waterproof mortar, wherein the raw materials in the formula are stirred and mixed uniformly, and when used, they are mixed according to a mass ratio of powder: water = 1: 0.15-0.23.
[0026] The shrinkage of mortar mainly comes from the deformation of cement stone, which produces voids, while the aggregate of mortar can inhibit the shrinkage and deformation of mortar to a certain extent. The present invention fills the pores of mortar by adding inert micro-aggregate waste stone powder or active micro-aggregate active additives, eliminates harmful macropores, optimizes pore size distribution, destroys connected channels, makes mortar more compact, and improves strength and waterproof performance. Cellulose ether, rubber powder, defoamer and dispersant are compounded as composite polymer additives. With the help of dispersant, the rubber powder disperses into film when it meets water or distributes in the middle of cement particles or hydration products as latex particles. The carboxyl groups on the surface of the polymer cross-link with the siloxy groups on the surface of the cement particles to form a membrane structure, thereby improving the density, tensile strength and fracture toughness of the cement material. The fiber modified by the silane coupling agent can overlap with the polymer film structure and the cement hydration product to form a criss-cross network structure, improve the microstructure and aggregate interface structure of the cement mortar, thereby improving the mortar's anti-seepage, compression resistance, flexural resistance and other properties. The addition of the hydrophobic agent can effectively reduce the water absorption rate.
[0027] In the present invention, a silane coupling agent is grafted onto the surface of the active additive and the polypropylene fiber. The hydrophilicity of the silane coupling agent enables the active additive and the polypropylene fiber to be better dispersed in the mortar system, accelerates the secondary hydration reaction rate, generates a hydration product with a denser structure to fill the capillary channels, reduces the mortar porosity and optimizes the pore size distribution. The surface of the unmodified polypropylene fiber is relatively smooth and no other substances are attached. There are tiny gaps at the interface with the polymer cement waterproof mortar, and the degree to which the two are tightly combined is low. The polypropylene fiber modified by the silane coupling agent has attachments on the surface that can appropriately increase its surface roughness, and the number of surrounding hydration products is large, which improves the bonding performance of the interface between the modified polypropylene fiber and the polymer cement waterproof mortar, and plays a role in filling and optimizing the interface transition zone. Therefore, the modified active additive and polypropylene fiber greatly improve the working performance, mechanical properties and impermeability of the mortar.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The one-component rigid polymer cement-based waterproof mortar provided by the present invention not only meets and exceeds the requirements of the JC / T984-2011 "Polymer Cement Waterproof Mortar" standard, but can also meet the five tensile bonding strength properties of cement-based adhesives specified in JC / T547-2017 "Ceramic Tile Adhesives". Therefore, the one-component rigid polymer cement-based waterproof mortar provided by the present invention can be used as a cement-based adhesive instead of tile adhesive. DETAILED DESCRIPTION
[0030] The present invention provides a one-component rigid polymer cement-based waterproof mortar, comprising the following raw materials in parts by weight:
[0031]
[0032] The active additive is amorphous SiO modified by a silane coupling agent. 2 -Al 2 O 3 Composite powder; amorphous SiO 2 -Al 2 O 3 SiO in composite powder 2 The weight percentage is more than 90%.
[0033] The composite polymer additive consists of cellulose ether, redispersible latex powder, defoamer and dispersant;
[0034] The amounts of the waste rock powder and active additives are not all 0 at the same time.
[0035] Furthermore, the composite polymer additive is composed of cellulose ether, rubber powder, defoamer and dispersant in a mass ratio of 0.05-0.15:1.5-2.5:0.05-0.15:8-12, preferably in a mass ratio of 0.1:2:0.1:10.
[0036] Furthermore, the cellulose ether is hydroxypropyl methylcellulose ether; the defoamer is polyether defoamer AGITAN RP803 type, and the dispersant is limestone powder below 200 meshes.
[0037] The redispersible latex powder is ethylene-vinyl acetate copolymer powder.
[0038] The silicate cement is 42.5 ordinary silicate cement.
[0039] The machine-made sand is limestone machine-made sand, and 0.075-0.15 mm limestone fine sand, 0.15-0.3 mm limestone fine sand and 0.3-0.6 mm limestone fine sand are used in combination.
[0040] The waste rock powder is recycled powder produced by the machine-made sand production line, and the particle size of the waste rock powder is less than 200 meshes.
[0041] The water repellent is a powdered silane-based water repellent, preferably a 200-mesh SEAL80 powdered silane-based water repellent, model SYLCOP TM 50 / 50;
[0042] The water reducing agent is a polycarboxylic acid water reducing powder, and the water reducing rate is ≥25%.
[0043] The silane coupling agent modified fiber is a silane coupling agent modified polypropylene fiber, wherein the length of the polypropylene fiber is 3-6 mm.
[0044] When used, the one-component rigid polymer cement-based waterproof mortar is mixed according to a mass ratio of powder: water = 1: 0.15-0.23.
[0045] The present invention is described in detail below with reference to the embodiments.
[0046] The sources of the raw materials used in each embodiment and comparative example are as follows:
[0047] Portland cement from Conch P · O42.5 cement.
[0048] The machine-made sand in Examples 1-8 and Comparative Examples 2 and 3 is selected from the 0.075-0.15 mm, 0.015-0.3 mm and 0.3-0.6 mm grades of Hailong machine-made sand in a mass ratio of 1:3:1.
[0049] Waste rock powder is the recycled dust from the machine-made sand production line, with a particle size of less than 200 mesh.
[0050] The water repellent is selected from Zhongwei High-tech SEAL80 powdered silane-based water repellent, model SYLCOP TM 50 / 50 + .
[0051] The water reducing agent is polycarboxylate water reducing powder (PCE) with a water reducing rate of ≥25%.
[0052] The composite polymer additive is composed of cellulose ether, redispersible latex powder, defoamer and dispersant in a mass ratio of 0.1:2:0.1:10; wherein the hydroxypropyl methylcellulose ether is MH4019P with a Brookfield viscosity of 4W; the redispersible latex powder is ethylene-vinyl acetate copolymer powder, which is commercially available; the defoamer is a polyether defoamer AGITAN RP803; and the dispersant is limestone powder with a particle size of less than 200 meshes.
[0053] Amorphous SiO modified by silane coupling agent 2 -Al 2O 3 The preparation method of the composite powder is as follows: 100 parts of amorphous SiO 2 -Al 2 O 3 The composite powder and 9 parts of silane coupling agent KH560 were dispersed in 100 parts of anhydrous ethanol, HCl was added to adjust the solution pH to 4-5, ultrasonic stirring was performed at 30°C for 3 hours, filtered, and then placed in an oven at 85°C for 24 hours; then placed in a ball mill and ground for 60 minutes. 2 -Al 2 O 3 The source of the composite powder is Gongyi Chenyi Wear-Resistant Materials Co., Ltd., and the fineness is 800 mesh.
[0054] The preparation method of silane coupling agent modified fiber is as follows: 50 parts of polypropylene fiber with a length of 3-6 mm and 9 parts of silane coupling agent KH560 are dispersed in 100 parts of anhydrous ethanol, HCl is added to adjust the solution pH to 4-5, ultrasonic stirring and dispersion at 30°C for 3h, filtered, and then placed in a 65°C oven to dry for 24h.
[0055] Other raw materials are commercially available unless otherwise specified.
[0056] Example 1
[0057] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0058]
[0059]
[0060] When in use, the amount of water added is the mass ratio of powder to water being 1:0.22.
[0061] Example 2
[0062] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0063] When in use, the amount of water added is the mass ratio of powder to water being 1:0.22.
[0064] Example 3
[0065] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0066] When in use, the amount of water added is the mass ratio of powder to water being 1:0.18.
[0067] Example 4
[0068] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0069] When in use, the amount of water added is the mass ratio of powder to water being 1:0.17.
[0070] Example 5
[0071] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0072] When in use, the amount of water added is the mass ratio of powder to water being 1:0.17.
[0073] Example 6
[0074] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0075]
[0076]
[0077] When in use, the amount of water added is the mass ratio of powder to water being 1:0.19.
[0078] Example 7
[0079] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0080] When in use, the amount of water added is the mass ratio of powder to water being 1:0.19.
[0081] Example 8
[0082] A single-component rigid polymer cement-based waterproof mortar, composed of the following raw materials in parts by weight:
[0083]
[0084]
[0085] When in use, the amount of water added is the mass ratio of powder to water being 1:0.19.
[0086] Comparative Example 1
[0087] The other parts are the same as in Example 1, except that the machine-made sand used is 0.6-0.3 mm machine-made sand. That is, the single-component rigid polymer cement-based waterproof mortar is composed of the following raw materials in parts by weight:
[0088]
[0089] When in use, the amount of water added is the mass ratio of powder to water being 1:0.22.
[0090] Comparative Example 2
[0091] The other parts are the same as those in Example 1, except that the amount of machine-made sand in the formula is 400 parts, and it also contains 200 parts of waste stone powder, that is, the single-component rigid polymer cement-based waterproof mortar is composed of the following raw materials in parts by weight:
[0092]
[0093] When in use, the amount of water added is the mass ratio of powder to water being 1:0.23.
[0094] Comparative Example 3
[0095] The rest is the same as in Example 3, except that the silane coupling agent modified fiber is replaced by a polypropylene fiber with a length of 3-6 mm.
[0096] Test Example 1
[0097] The waterproof mortars prepared in the above-mentioned embodiments and comparative examples were stirred and tested for related performance in accordance with the standard JC / T984-2011 "Polymer Cement Waterproof Mortar".
[0098] Table 1 JC / T984-2011 "Polymer cement waterproof mortar" related performance indicators.
[0099]
[0100] Table 2 Test results of Example 1, Example 2 and Example 3
[0101]
[0102] Table 3 is the test results of Example 4 and Example 5
[0103]
[0104]
[0105] Table 4 shows the test results of Example 6, Example 7 and Example 8
[0106]
[0107]
[0108] Table 5 is the test results of Comparative Example 1, Comparative Example 2 and Comparative Example 3
[0109]
[0110] It can be seen from Table 2 that the polymer waterproof mortar prepared by the present invention has excellent mechanical properties such as compressive strength and flexural strength and waterproof and impermeability. By comparing Example 1 with Example 2, it can be seen that compared with the inert waste stone powder which only has the function of filling pores, the active aluminum and active silicon rich in the active additive can react with the cement hydration product CH to generate gel substances such as CSH and CASH, promote cement hydration, improve pore structure, and reduce porosity, thereby improving the strength, impermeability and corrosion resistance of the mortar. By comparing Example 2 with Example 3, it can be seen that the compressive strength, flexural strength, bonding strength and impermeability of the polypropylene fiber reinforced polymer cement waterproof mortar obtained by modification with a silane coupling agent have obvious advantages.
[0111] In order to expand the application scope of the material, it can be seen from the test results in Table 2 that when the ratio of cementitious materials and machine-made sand is adjusted, the active additives and composite polymer additives can still meet the index requirements of JC / T984-2011 "Polymer Cement Waterproof Mortar" after appropriate adjustment.
[0112] The present application also sets up three control groups. Compared with Example 1, in Example 1, the machine-made sand selects single-grade fine sand of 0.6-0.3mm. It can be seen from the test results that when the content of fine powder particles decreases, the water demand decreases, the porosity increases, and the compression, flexural and impermeability properties are reduced. Compared with Example 1, when the inert fillers such as waste stone powder continue to increase, that is, when they are added too much, it can be seen that the excessive increase in the content of fine powder particles will lead to an increase in the water demand of the mortar, poor working performance, increased water absorption, and affected water retention. By adjusting the content of the water reducer, the density can be improved while reducing the water consumption, thereby improving the density of the waterproof mortar. Compared with Example 3, in Example 3, the fiber uses unmodified fiber. It can be seen from the test results that the fiber surface is relatively smooth, and the modified fiber surface has a rough interface, and the compression, flexural and impermeability properties are relatively reduced.
[0113] Further tests in Examples 6, 7 and 8 show that when the amounts of various raw materials in the waterproof mortar are controlled within the scope of the present invention, various indicators can meet the product standards.
[0114] Test Example 2
[0115] The waterproof mortars prepared in the above embodiments and comparative example 3 were subjected to five tests of tensile bond strength, including tensile bond strength after immersion in water, tensile bond strength after heat aging, tensile bond strength after freeze-thaw cycles and cooling time ≥ 20 min, with reference to JC / T547-2017 "Ceramic Tile Adhesive".
[0116] Table 6 shows the technical requirements for cement-based adhesives (C)
[0117]
[0118] Table 7 Test results of Examples 1-4
[0119]
[0120] Table 8 Test results of Examples 5-8 and Comparative Example 3
[0121]
[0122] As can be seen from the table, the waterproof mortar provided by the present invention can meet the five tensile bond strength properties of cement-based adhesives specified in JC / T 547-2017 "Ceramic Tile Adhesives", and can be used instead of tile adhesives. While the waterproof mortar provided in Comparative Example 3 can meet the requirements of JC / T984-2011 "Polymer Cement Waterproof Mortar", it cannot meet the five tensile bond strength properties of cement-based adhesives specified in JC / T 547-2017 "Ceramic Tile Adhesives", and cannot be used instead of tile adhesives.
[0123] The detailed description of a one-component rigid polymer cement-based waterproof mortar and its preparation method with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A one-component rigid polymer cement-based waterproof mortar, characterized in that: The invention comprises the following raw materials in parts by weight: The active additive is an amorphous SiO2-Al2O3 composite powder modified by a silane coupling agent; The composite polymer additive consists of cellulose ether, redispersible latex powder, defoamer and dispersant; The amounts of the waste rock powder and active additives are not all 0 at the same time.
2. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: The composite polymer additive is composed of cellulose ether, rubber powder, defoamer and dispersant in a mass ratio of 0.05-0.15:1.5-2.5:0.05-0.15:8-12.
3. The one-component rigid polymer cement-based waterproof mortar according to claim 2, characterized in that: The redispersible latex powder is ethylene-vinyl acetate copolymer rubber powder.
4. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: The weight percentage of SiO2 in the amorphous SiO2-Al2O3 composite powder is more than 90%.
5. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: The silicate cement is 42.5 ordinary silicate cement.
6. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: The machine-made sand is selected from the 0.075-0.15mm, 0.015-0.3mm and 0.3-0.6mm grades of Hailong machine-made sand in a mass ratio of 1:3:
1.
7. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: The waste rock powder is recycled powder produced by the machine-made sand production line, and the particle size is below 200 meshes.
8. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: The water repellent is a powdered silane-based water repellent; and the water reducing agent is a polycarboxylic acid water reducing powder.
9. The one-component rigid polymer cement-based waterproof mortar according to claim 1, characterized in that: When used, the one-component rigid polymer cement-based waterproof mortar is mixed according to a mass ratio of powder: water = 1: 0.15-0.
23.
10. The method for preparing the one-component rigid polymer cement-based waterproof mortar according to any one of claims 1 to 8, characterized in that: Stir and mix the raw materials in the formula evenly, and mix them according to the mass ratio of powder: water = 1: 0.15-0.23 when using.
Citation Information
Patent Citations
Polymer waterproofing dry mixed mortar
CN106892612A
One-component polymer cement waterproof mortar and preparation method thereof
CN110330286A
Waterproofing cement mortar composition
KR101325879B1