Full-spectrum high-color-rendering-index fluorescent ceramic for solid-state illumination and preparation method thereof

By introducing Ce3+, Mn2+ and Pr3+ doping into fluorescent ceramics and adjusting the luminescence wavelength, the problem of low color rendering index of Ce:YAG fluorescent ceramics is solved, high color rendering index and red light supplementation are achieved, and the quality of solid-state lighting is improved and applicability.

CN118930239APending Publication Date: 2024-11-12XUZHOU NORMAL UNIVERSITY +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411151831.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing Ce:YAG fluorescent ceramics have a problem of low color rendering index in solid state illumination, lacking sufficient red light components and cyan light parts, resulting in a shift in emission color and a reduced sensory comfort of the human eye.

Method used

The full spectrum high finger fluorescent ceramic with the chemical formula (Ca1-x-zCexPrz)3(Sc1-yMny)2Si3O12 is used. Through the doping of Ce3+, Mn2+ and Pr3+, the luminescence wavelength covers the range of 525-750nm to improve the color rendering. and industrial production through sintering and annealing process optimization.

Benefits of technology

The color rendering index has been increased to 85~92, and the red light component is effectively supplemented, and the material has good thermal stability. It is suitable for high-quality light sources and adapts to lighting needs in different occasions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930239A_ABST
    Figure CN118930239A_ABST
Patent Text Reader

Abstract

The invention discloses full-spectrum high-color-rendering-index fluorescent ceramic for solid-state illumination and a preparation method of the full-spectrum high-color-rendering-index fluorescent ceramic. The general chemical formula of the fluorescent ceramic is (Ca1-x-zCexPrz) 3 (Sc1-yMny) 2Si3O12, in which x is the molar percentage of Ca < 2 + > substituted by Ce < 3 + >, and x is more than or equal to 0.001 and less than or equal to 0.005; y is the mole percent of Sc < 3 + > substituted by Mn < 2 + >, and y is more than or equal to 0.001 and less than or equal to Z is the molar percentage of Pr < 3 + > replacing Ca < 2 + >, and z is more than or equal to 0.0001 and less than or equal to 0.005 According to the fluorescent ceramic prepared by the invention, the luminescent wavelength of the material can be adjusted by properly doping Pr < 3 + > and Mn < 2 + >, so that the material has a wider application range. Under the excitation of a blue light LED chip with the wavelength of 450 nm, the fluorescent powder can emit fluorescence with the wavelength covering the range of 525-750 nm, and the color rendering index is 85-92. When the environment temperature is 150 DEG C, the luminous intensity of the fluorescent ceramic is kept at 75%-90%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to fluorescent ceramics, in particular to full-spectrum high-rendering index fluorescent ceramics for solid-state lighting and a preparation method thereof, belonging to the technical field of luminescent materials. Background Art

[0002] Solid-state lighting is a modern lighting technology, represented by LED, which has the advantages of energy saving, environmental protection, and long life. The current pcWLED often uses a combination of yellow-emitting Ce:YAG fluorescent ceramics and blue LEDs. Garnet-based ceramic phosphors have the advantages of good thermal stability, strong heat bearing capacity, high chemical composition designability, and stable fluorescence performance. 3+ There are two significant problems with doped garnet-based fluorescent ceramics, namely the lack of sufficient red light components and the absence of cyan light, which leads to a relatively low color rendering index (CRI of about 60). Therefore, there are many disadvantages such as emission color shift and reduced sensory comfort of the human eye. For example, the literature (X. Liu, H. Zhou, Z. Hu, et al. Transparent Ce: GdYAG ceramic color converters for high-brightness white LEDs and LDs, Opt. Mater. 2019, 88: 97-102.) reported that Gd 3+ Ion-doped YAG:Ce fluorescent ceramics have limitedly improved the color rendering index of ceramics, up to 67.2. Therefore, exploring a high color rendering index fluorescent ceramic material is crucial to achieving higher quality and practical light sources. Summary of the invention

[0003] One of the purposes of the present invention is to provide a full-spectrum high color rendering index fluorescent ceramic for solid-state lighting, which has the advantage of high color rendering index as a luminescent material.

[0004] The second object of the present invention is to provide a method for preparing full-spectrum high-rendering index fluorescent ceramics for solid-state lighting, which is easy to realize industrial production.

[0005] In order to achieve the above-mentioned object, the technical solution adopted by the present invention is as follows: a full-spectrum high-rendering index fluorescent ceramic for solid-state lighting, the chemical formula of the fluorescent ceramic is:

[0006] (Ca 1-x-z Ce x Pr z )3(Sc 1-y Mn y )2Si3O 12

[0007] Where x is Ce 3+ Replace Ca2+ The molar percentage of the position, 0.001≤x≤0.005; y is Mn 2+ Replace Sc 3+ The molar percentage of the position, 0.001≤y≤0.01; z is Pr 3+ Replace Ca 2+ The molar percentage of the position, 0.0001≤z≤0.005.

[0008] The full-spectrum high-ratio fluorescent ceramic provided by the present invention can emit fluorescence with a wavelength covering the range of 525 to 750 nm under the excitation of 450 nm blue light.

[0009] On the other hand, the present invention provides a method for preparing the above-mentioned full-spectrum high-rendering index fluorescent ceramic for solid-state lighting, which specifically comprises the following steps:

[0010] (1) According to the chemical formula (Ca 1-x-z Ce x Pr z )3(Sc 1-y Mn y )2Si3O 12 The chemical stoichiometric ratio of each element in the mixture is as follows: calcium oxide, scandium oxide, praseodymium oxide, manganese carbonate, silicon dioxide, and cerium oxide with a purity greater than 99.99% are weighed as raw material powders, wherein x is Ce. 3+ Replace Ca 2+ The molar percentage of Mn is 0.0001≤x≤0.005; y is Mn 2+ Replace Sc 3+ The molar percentage of the position, 0.001≤y≤0.01; z is Pr 3+ Replace Ca 2+ The molar percentage of the position is 0.0001≤z≤0.005; the raw material powder and the ball milling medium are mixed and ball milled in proportion to obtain a mixed slurry;

[0011] (2) drying the mixed slurry obtained in step (1) in a drying oven, and then sieving the dried mixed powder;

[0012] (3) placing the sieved powder in step (2) into a mold for dry pressing, and then performing cold isostatic pressing to obtain a green blank with a relative density of 50% to 55%;

[0013] (4) The green blank obtained in step (3) is placed in a vacuum furnace for sintering, firstly heated to 1450°C to 1550°C for sintering, then cooled to 1400°C to 1500°C at a rate of 5°C / min, and kept at this temperature for 8h to 24h. The sintering vacuum degree is not less than 10 -3 Pa, and obtain fluorescent ceramics;

[0014] (5) Annealing the fluorescent ceramic obtained in step (4) in air at a temperature of 1300 to 1450° C. for a holding time of 8 to 24 hours to obtain a fluorescent ceramic having a relative density of 99.5% to 99.9%.

[0015] Preferably, in step (1), the ball milling medium is anhydrous ethanol, and the mass volume ratio of the raw material powder to the ball milling medium is 1 g: (2-4) mL.

[0016] Preferably, in step (1), the ball milling speed is 180 r / min to 220 r / min, and the ball milling time is 12 h to 18 h.

[0017] Preferably, in step (2), the drying time is 20 h to 25 h, and the drying temperature is 75° C. to 85° C.

[0018] Preferably, in step (2), the mesh size of the sieving sieve is 50 to 200 meshes, and the sieving times are 1 to 3 times.

[0019] Preferably, in step (3), the cold isostatic pressing holding pressure is 150 to 200 MPa, and the holding time is 200 to 400 s.

[0020] Preferably, in step (4), the heating rate in the vacuum sintering stage is 1 to 10°C / min, and the cooling rate after sintering is 1 to 10°C / min.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The fluorescent ceramic prepared by the present invention can emit fluorescence with a wavelength covering the range of 525 to 750 nm under the excitation of a blue light LED chip with a wavelength of 450 nm, and its color rendering index is 85 to 92.

[0023] 2. The fluorescent ceramics of the present invention are added with Pr 3+ and Mn 2+ The luminescent properties of materials can be improved. Through appropriate doping, the luminescent wavelength of the material can be adjusted, making the material have a wider range of applications. The correlated color temperature of fluorescent materials can be effectively adjusted to obtain a high color rendering index, further improving the lighting quality.

[0024] 3. The fluorescent ceramics of the present invention are added with Pr 3+ and Mn 2+ Doping fluorescent ceramics can adjust the luminescent color of the material by changing the Pr 3+ and Mn 2+ The doping concentration enables the material to emit light of different colors, such as red, orange, etc., to meet the lighting requirements of different occasions and needs.

[0025] 4. The present invention uses Ca3Sc2Si3O 12 As the matrix structure, by introducing the transition metal Mn 2+ , Pr 3+ ions, successfully increased the red light emission at 580-700nm, effectively broadened the emission peak, effectively compensated for the red light component, and significantly improved the color rendering index of the fluorescent ceramic. When the ambient temperature is 150°C, the luminous intensity of the fluorescent ceramic is maintained at 75%-90%.

[0026] 5. The process steps of the present invention are few, the process conditions are not harsh and are easy to achieve; the obtained luminescent material is of high quality and can be widely used in the preparation of luminescent materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The XRD diagrams of the fluorescent ceramics prepared in Examples 1 to 3 of the present invention are shown in FIG.

[0028] Figure 2 The relative temperature-dependent emission intensity diagram of the fluorescent ceramics prepared in Examples 1 to 3 of the present invention.

[0029] Figure 3 This is the electroluminescence spectrum of the fluorescent ceramic prepared in Example 1 of the present invention.

[0030] Figure 4 This is the emission spectrum of the fluorescent ceramic prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] The raw material powders used in the following examples are all commercially available products, with a particle size of 60 to 80 nm and a purity of 99.99%.

[0033] Example 1: Preparation of chemical formula (Ca 0.9965 Ce 0.002 Pr 0.0015 )3(Sc 0.993 Mn 0.007 )2Si3O 12 Fluorescent ceramics.

[0034] (1) According to the chemical formula (Ca 0.9965 Ce 0.002 Pr 0.0015 )3(Sc 0.993 Mn 0.007 )2Si3O 12Calcium oxide, scandium oxide, praseodymium oxide, manganese carbonate, silicon dioxide, and cerium oxide were weighed as raw material powders in the stoichiometric ratio of each element, totaling 60 g, and the raw material powders and ball milling media were mixed in a ratio of 1:1 and ball milled for 15 h to obtain a mixed slurry;

[0035] (2) drying the mixed slurry obtained in step (1) in a drying oven at 80° C. for 20 h, and then sieving the dried mixed powder three times with a 100-mesh sieve;

[0036] (3) placing the sieved powder in step (2) into a mold for dry pressing, and then performing cold isostatic pressing at 200 MPa for 200 seconds;

[0037] (4) placing the green blank obtained in step (3) in a vacuum furnace for sintering, heating at a rate of 10°C / min to a sintering temperature of 1500°C, then cooling at a rate of 5°C / min to 1450°C, holding the temperature for 10 hours, and sintering with a vacuum degree of not less than 10Pa, to obtain a fluorescent ceramic;

[0038] (5) Annealing the fluorescent ceramic obtained in step (4) in air at a temperature of 1450° C. for 10 h.

[0039] like Figure 1 As shown in the XRD pattern, the prepared fluorescent ceramics have no impurity phase. Figure 2 As shown in the relative temperature-dependent emission intensity graph, the thermal stability of the prepared fluorescent ceramic at 150°C remains above 85%, which is higher than that of Ce:YAG. Figure 3 Electroluminescence spectrum, using blue LED to excite fluorescent ceramics, when the output power is 2W, the color rendering index is as high as 92. Figure 4 The emission spectrum shows that Pr 3+ The doping of Mn increases the red emission at 600nm. 2+ The doping increases the red light emission at 580nm and expands the half-width. The color rendering index is effectively improved from 80 to 92 by supplementing the red light from two places.

[0040] Example 2: Preparation of chemical formula (Ca 0.995 Ce 0.003 Pr 0.002 )3(Sc 0.992 Mn 0.008 )2Si3O 12 Fluorescent ceramics.

[0041] (1) According to the chemical formula (Ca 0.995 Ce 0.003 Pr 0.002 )3(Sc 0.992 Mn 0.008 )2Si3O 12Calcium oxide, scandium oxide, praseodymium oxide, manganese carbonate, silicon dioxide, and cerium oxide were weighed as raw material powders in the stoichiometric ratio of each element, totaling 60 g, and the raw material powders and ball milling media were mixed in a ratio of 1:1 and ball milled for 15 h to obtain a mixed slurry;

[0042] (2) drying the mixed slurry obtained in step (1) in a drying oven at 80° C. for 20 h, and then sieving the dried mixed powder three times with a 100-mesh sieve;

[0043] (3) placing the sieved powder in step (2) into a mold for dry pressing, and then performing cold isostatic pressing at 200 MPa for 200 seconds;

[0044] (4) placing the green blank obtained in step (3) in a vacuum furnace for sintering, heating at a rate of 10°C / min, the sintering temperature is 1550°C, then cooling at a rate of 5°C / min to 1500°C, keeping the temperature for 10 hours, and the sintering vacuum degree is not less than 10Pa, to obtain a fluorescent ceramic;

[0045] (5) Annealing the fluorescent ceramic obtained in step (4) in air at a temperature of 1450° C. for 10 h.

[0046] like Figure 1 As shown in the XRD diagram, the prepared fluorescent ceramics have no impurity phase; Figure 2 As shown in the relative temperature-dependent emission intensity graph, the thermal stability of the prepared fluorescent ceramic is maintained above 80% at 150°C, which is higher than Ce:YAG. When the fluorescent ceramic is excited by a blue light LED, the color rendering index is as high as 87 when the output power is 2W.

[0047] Example 3: Preparation of chemical formula (Ca 0.992 Ce 0.004 Pr 0.004 )3(Sc 0.99 Mn 0.01 )2Si3O 12 Fluorescent ceramics.

[0048] (1) According to the chemical formula (Ca 0.992 Ce 0.004 Pr 0.004 )3(Sc 0.99 Mn 0.01 )2Si3O 12 Calcium oxide, scandium oxide, praseodymium oxide, manganese carbonate, silicon dioxide, and cerium oxide were weighed as raw material powders in the stoichiometric ratio of each element, totaling 60 g, and the raw material powders and ball milling media were mixed in a ratio of 1:1 and ball milled for 15 h to obtain a mixed slurry;

[0049] (2) drying the mixed slurry obtained in step (1) in a drying oven at 80° C. for 20 h, and then sieving the dried mixed powder three times with a 100-mesh sieve;

[0050] (3) placing the sieved powder in step (2) into a mold for dry pressing, and then performing cold isostatic pressing at 200 MPa for 200 seconds;

[0051] (4) placing the green blank obtained in step (3) in a vacuum furnace for sintering, heating at a rate of 10°C / min, the sintering temperature is 1450°C, then cooling at a rate of 5°C / min to 1400°C, keeping the temperature for 10 hours, and the sintering vacuum degree is not less than 10Pa, to obtain a fluorescent ceramic;

[0052] (5) Annealing the fluorescent ceramic obtained in step (4) in air at a temperature of 1450° C. for 10 h.

[0053] like Figure 1 As shown in the XRD diagram, the prepared fluorescent ceramics have no impurity phase; Figure 2 As shown in the relative temperature-dependent emission intensity graph, the thermal stability of the prepared fluorescent ceramic is maintained at 70% at 150°C; when the fluorescent ceramic is excited by a blue light LED, the color rendering index is as high as 89 when the output power is 2W.

[0054] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A full-spectrum high-ratio fluorescent ceramic for solid-state lighting, characterized in that: The general chemical formula of the fluorescent ceramic is: (That 1-x-z What x Fr. z )3(Sc 1-y min y )2Si3O 12 Where x is Ce 3+ Replace Ca 2+ The molar percentage of the position, 0.001≤x≤0.005; y is Mn 2+ Replace Sc 3+ The molar percentage of the position, 0.001≤y≤0.01; z is Pr 3+ Replace Ca 2+ The molar percentage of the position, 0.0001≤z≤0.

005.

2. A method for preparing the full-spectrum high-rendering index fluorescent ceramic for solid-state lighting according to claim 1, characterized in that: The following steps are involved: (1) According to the chemical formula (Ca 1-x-z Ce x Pr z )3(Sc 1-y Mn y )2Si3O 12 The stoichiometric ratio of each element in the mixture is as follows: calcium oxide, scandium oxide, praseodymium oxide, manganese carbonate, silicon dioxide, and cerium oxide with a purity greater than 99.99% are weighed as raw material powders, wherein x is Ce. 3+ Replace Ca 2+ The molar percentage of Mn is 0.0001≤x≤0.005; y is Mn 2+ Replace Sc 3+ The molar percentage of the position, 0.001≤y≤0.01; z is Pr 3+ Replace Ca 2+ The molar percentage of the position is 0.0001≤z≤0.005; the raw material powder and the ball milling medium are mixed and ball milled in proportion to obtain a mixed slurry; (2) drying the mixed slurry obtained in step (1) in a drying oven, and then sieving the dried mixed powder; (3) placing the sieved powder in step (2) into a mold for dry pressing, and then performing cold isostatic pressing to obtain a green blank with a relative density of 50% to 55%; (4) The green blank obtained in step (3) is placed in a vacuum furnace for sintering, firstly heated to 1450°C to 1550°C for sintering, then cooled to 1400°C to 1500°C at a rate of 5°C / min, and kept at this temperature for 8h to 24h. The sintering vacuum degree is not less than 10 -3 Pa, and obtain fluorescent ceramics; (5) Annealing the fluorescent ceramic obtained in step (4) in air at a temperature of 1300 to 1450° C. for a holding time of 8 to 24 hours to obtain a fluorescent ceramic having a relative density of 99.5% to 99.9%.

3. The method for preparing the full-spectrum high-rendering index fluorescent ceramic for solid-state lighting according to claim 2, characterized in that: In step (1), the ball milling medium is anhydrous ethanol, and the mass volume ratio of the raw material powder to the ball milling medium is 1 g: (2-4) mL.

4. The method for preparing the full-spectrum high-CRI fluorescent ceramic for solid-state lighting according to claim 2, characterized in that: In step (1), the ball milling speed is 180 r / min to 220 r / min, and the ball milling time is 12 h to 18 h.

5. The method for preparing the full-spectrum high-CRI fluorescent ceramic for solid-state lighting according to claim 2, characterized in that: In step (2), the drying time is 20 hours to 25 hours, and the drying temperature is 75° C. to 85° C.

6. The method for preparing the full-spectrum high-rendering index fluorescent ceramic for solid-state lighting according to claim 2, characterized in that: In step (2), the mesh size of the sieve is 50 to 200 meshes, and the sieving times are 1 to 3 times.

7. The method for preparing the full-spectrum high-CRI fluorescent ceramic for solid-state lighting according to claim 2, characterized in that: In step (3), the cold isostatic pressing holding pressure is 150 to 200 MPa, and the holding time is 200 to 400 s.

8. The method for preparing full-spectrum high-CRI fluorescent ceramics for solid-state lighting according to claim 2, characterized in that: In step (4), the heating rate in the vacuum sintering stage is 1 to 10°C / min, and the cooling rate after sintering is 1 to 10°C / min.

Citation Information

Patent Citations

  • Blue-light-matrix single fluorescent powder and application thereof in preparation of white light LED (light-emitting diode)

    CN102719250A

  • High-color-rendering-index and high-quantum-efficiency fluorescence conversion composite material for laser illumination and preparation method thereof

    CN117777996A

  • Ceramic composition

    US20200063029A1