Polyethylene compositions, methods of making the same and films made
A linear low-density polyethylene composition with optimized melt index, density, and molecular structure was prepared by single-reactor solution polymerization using a polyvalent aryloxy ether metal complex catalyst system. This method solves the performance and cost-effectiveness problems in the prior art and realizes high-performance, low-cost membrane production.
Patent Information
- Application Number
- CN202410629804.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2016-03-03
- Filing Date
- 2017-03-03
- Publication Date
- 2024-11-12
AI Technical Summary
Existing linear low-density polyethylene compositions are difficult to simultaneously meet performance requirements and cost-effectiveness in film production, especially in terms of melt index, density, and molecular structure.
Linear low-density polyethylene compositions were prepared by solution polymerization in a single reactor using a catalyst system containing polyvalent aryloxy ether metal complexes, controlling their melt index, density, and molecular structure, specifically including the ratio and molecular weight distribution of ethylene and α-olefin comonomers.
It achieved a CEF fraction greater than 80% at 70-90℃, a melt index I2 of 0.8-1.5 g/10 min, a melt flow ratio I10/I2 of 7.0-8.0, and a density of 0.914-0.920 g/cm3, reducing processing energy consumption and cost while improving the mechanical properties of the membrane.
Smart Images

Figure CN118931018A_ABST
Abstract
Description
[0001] This application is a divisional application of Chinese patent application No. 201780011809.6 (application date: 2017 / 3 / 3, invention name: polyethylene composition, preparation method thereof and film made thereof). Field of the Invention
[0002] The present invention relates to a linear low density polyethylene composition, a method for preparing the composition, and a film prepared therefrom. Background of the Invention
[0004] It is generally known to use polyethylene compositions, such as linear low density polyethylene (LLDPE), in the manufacture of films. Such polyethylene compositions can be produced by any conventional process, such as a gas phase process, a slurry process or a solution process. In addition, such films can be produced by any conventional film process such as a blown film extrusion process.
[0005] Various polymerization techniques using different catalyst systems have been employed to produce such polyethylene compositions suitable for film production applications. Currently available polyethylene compositions fail to meet all desired film properties while providing additional cost benefits.
[0006] Despite research efforts in developing polyethylene compositions suitable for film production applications, there remains a need for low cost linear low density polyethylene compositions having improved properties. Summary of the invention
[0007] The present disclosure provides a linear low density polyethylene composition, a method for preparing the composition, a film prepared therefrom, and a method for preparing the film. In one embodiment, the present disclosure provides a linear low density polyethylene composition, which exhibits each of the following properties: (1) a CEF fraction at 70-90°C equal to or greater than 80% of the total CEF fraction; (2) a melt index I measured according to ASTM D 1238 (2.16 kg, 190°C); 2 The range is 0.8-1.5g / 10min; (3) melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0008] In an alternative embodiment, the present disclosure also provides a film layer comprising a linear low density polyethylene composition, the composition exhibiting each of the following properties: (1) a CEF fraction at 70-90°C equal to or greater than 80% of the total CEF fraction; (2) a melt index I measured according to ASTM D 1238 (2.16 kg, 190°C); 2 The range is 0.8-1.5g / 10min; (3) melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0009] In an alternative embodiment, the present disclosure also provides a method for preparing a film, comprising: (a) blow-extruding a linear low-density polyethylene composition, the composition exhibiting each of the following properties: (1) a CEF fraction at 70-90°C equal to or greater than 80% of the total CEF fraction; (2) a melt index I measured according to ASTM D 1238 (2.16 kg, 190°C); 2 The range is 0.8-1.5g / 10min; (3) melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0010] In an alternative embodiment, the present disclosure also provides a linear low-density polyethylene composition, a film and a method for preparing the same according to the aforementioned embodiment, except that the linear low-density polyethylene resin also has a molecular weight of from 0.914 to 0.920 g / cm 2 Density (measured according to ASTM D792).
[0011] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film and a method for preparing the same according to any of the preceding embodiments, except that the linear low density polyethylene comprises units derived from ethylene and units derived from one or more α-olefin comonomers.
[0012] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film and a method for preparing the same according to any of the preceding embodiments, except that the comonomer is 1-hexene.
[0013] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film and a method for preparing the same according to any of the preceding embodiments, except that the comonomer is 1-octene.
[0014] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film and a method for preparing the same according to any of the preceding embodiments, except that the comonomer is 1-butene.
[0015] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film, and a method for preparing the same according to any of the preceding embodiments, except that the linear low density polyethylene composition is prepared by a solution phase process using one reactor.
[0016] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film and a method for preparing the same according to any of the preceding embodiments, except that the linear low density polyethylene composition is prepared in a single loop solution polymerization reactor in the presence of hexene.
[0017] In an alternative embodiment, the present disclosure also provides a linear low density polyethylene composition, a film and a method for preparing the same according to any of the preceding embodiments, except that the film layer comprises the linear low density polyethylene composition and the low density polyethylene. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] For the purpose of illustrating the invention, there is shown in the drawings a form which is exemplary; it being understood, however, that the invention is not limited to the precise arrangements and instrumentalities shown.
[0019] Figure 1 is a graph illustrating the CEF results of each of Comparative Examples 1 and 2 and Inventive Example 1 (elution mass (dW T / dT) versus temperature).
[0020] Figure 2 is the corresponding integral of the unsaturation in the data processing of the double presaturation experiment (I 1,2-亚乙烯基 ,I 三取代的 ,I 乙烯基 and I 亚乙烯基 ) is a schematic diagram of the integration region. DETAILED DESCRIPTION
[0021] The present disclosure provides a linear low-density polyethylene composition, a film and a method for preparing the same. The linear low-density polyethylene composition according to the present disclosure exhibits each of the following properties: (1) a CEF fraction at 70-90°C equal to or greater than 80% of the total CEF fraction; (2) a melt index I measured according to ASTM D 1238 (2.16 kg, 190°C); 2 The range is 0.8-1.5g / 10min; (3) melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0022] The film layer according to the present disclosure comprises a linear low density polyethylene composition, which exhibits each of the following properties: (1) a CEF fraction at 70-90° C. equal to or greater than 80% of the total CEF fraction; (2) a melt index I measured according to ASTM D1238 (2.16 kg, 190° C.); 2 The range is 0.8-1.5g / 10min; (3) melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0023] The film layer according to the present disclosure may comprise the linear low density polyethylene composition and a low density polyethylene.The film layer may comprise less than 50 wt% of the low density polyethylene, such as 5 to 45 wt%, or 5 to 35 wt%, or 15 to 35 wt%.
[0024] Linear low density polyethylene
[0025] The linear low density polyethylene composition exhibits each of the following properties: (1) a CEF fraction at 70-90°C equal to or greater than 80% of the total CEF fraction; (2) a melt index I measured according to ASTM D 1238 (2.16 kg, 190°C); 2 The range is 0.8-1.5g / 10min; (3) melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0026] Linear low density polyethylene (LLDPE) comprises ethylene / α-olefin copolymers, which comprise (a) less than or equal to 100 wt%, such as at least 70 wt%, or at least 80 wt%, or at least 90 wt% of units derived from ethylene; and (b) less than 30 wt%, such as less than 25 wt%, or less than 20 wt%, or less than 10 wt% of units derived from one or more α-olefin comonomers. The term "ethylene / α-olefin copolymer" refers to a polymer containing greater than 50 mole % polymerized ethylene monomer (based on the total amount of polymerizable monomers) and at least one comonomer.
[0027] The alpha-olefin comonomers generally have no more than 20 carbon atoms. For example, the alpha-olefin comonomers may preferably have 3 to 8 carbon atoms, more preferably 3 to 6 carbon atoms. Exemplary alpha-olefin comonomers include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene and 4-methyl-1-pentene. One or more alpha-olefin comonomers may, for example, be selected from propylene, 1-butene, 1-hexene, or, selected from 1-butene and 1-hexene. In one embodiment, the linear low density polyethylene resin does not include units derived from 1-octene.
[0028] The CEF fraction of the LLDPE at 70 to 90°C is equal to or greater than 80% of the total CEF fraction, for example, the CEF fraction of the LLDPE at 70 to 90°C is equal to or greater than 85% of the total CEF fraction, or in the alternative, the CEF fraction of the LLDPE at 70 to 90°C is equal to or greater than 90% of the total CEF fraction.
[0029] The melt index of LLDPE is measured according to ASTM D 1238 (2.16 kg, 190°C). 2 The range is 0.8-1.5 g / 10 min. All individual values and subranges from 0.8 to 1.5 g / 10 min are included and disclosed herein; for example, 2The range of can be 0.8, 1.0, 1.2 or 1.4 g / 10min lower limit to 0.9, 1.1, 1.3 or 1.5 g / 10min upper limit. For example, I 2 It may be 0.8 to 1.5 g / 10 min, or alternatively, 0.9 to 1.2 g / 10 min, or alternatively, 1.0 to 1.5 g / 10 min.
[0030] The LLDPE is characterized by having a zero shear viscosity ratio (ZSVR) in the range of 1.2 to 5. All individual values and subranges are disclosed and included herein; for example, the ZSVR can range from a lower limit of 1.2, 2.2, 3.2, or 4.2 to an upper limit of 1.5, 2.6, 3.5, 4.4, or 5. For example, the ZSVR can range from 1.2 to 5; or in the alternative, 1.5 to 4; or in the alternative, 1.2 to 3.1; or in the alternative, 3 to 5, or in the alternative, 2 to 4.
[0031] The density of LLDPE is about 0.914 to 0.920 g / cm 3 Range: 0.914 to 0.920 g / cm 3 All individual values and subranges of are included and disclosed herein. For example, the density can be from 0.914, 0.916, 0.918 g / cm 3 The lower limit is 0.920, 0.917 or 0.915 g / cm 3 For example, the density can range from 0.914 to 0.920 g / cm 3 , or alternatively, 0.914 to 0.918 g / cm 3 , or alternatively, 0.913 to 0.919 g / cm 3 , or alternatively, 0.918 to 0.920 g / cm 3 , or alternatively, 0.915 to 0.919 g / cm 3 .
[0032] The molecular weight distribution of LLDPE (M w / M n ) is in the range of 2.0 to 3.5. All individual values and subranges within the range of 2.0 to 3.5 are included and disclosed herein; for example, the molecular weight distribution (M w / M n ) can range from a lower limit of 2, 2.1, 2.2, 2.4, 2.5 or 2.6 to an upper limit of 2.2, 2.3, 2.4, 2.5, 2.7, 2.9, 3.2 or 3.5. For example, the molecular weight distribution (M w / M n) can be from 2.0 to 3.5, or in the alternative, from 2.0 to 2.4, or in the alternative, from 2.0 to 2.8, or in the alternative, from 2.8 to 3.5.
[0033] The molecular weight distribution of LLDPE (M z / M n ) is in the range of 3.5 to 6. All individual values and subranges within the range of 3.5 to 6 are included and disclosed herein; for example, the molecular weight distribution (M z / M n ) can be a lower limit of 3.5, 3.7, 3.9, 4.5 or 5 to an upper limit of 3.5, 4.0, 4.2, 4.4, 4.7, 5.0, 5.5 or 6.0. For example, the molecular weight distribution (M z / M n ) can range from 3.5 to 6; or in the alternative, 3.5 to 4.8; or in the alternative, 4.8 to 6; or in the alternative, 4 to 5; or in the alternative, 3.5 to 4.5.
[0034] LLDPE has a molecular weight distribution asymmetry [(M w / M n ) / (M z / M w )], that is, M w 2 / (M n *M z ). For example, the molecular weight distribution asymmetry M w 2 / (M n *M z ) can be from a lower limit of 1.0, 1.05, 1.10, 1.15 or 1.20 to an upper limit of 1.25, 1.30, 1.35 or 1.40. For example, the molecular weight distribution asymmetry M w 2 / (M n *M z ) can range from 1.00 to 1.40, or in the alternative, from 1.00 to 1.20, or in the alternative, from 1.20 to 1.40, or in the alternative, from 1.10 to 1.30.
[0035] The LLDPE has less than 0.15 vinyl groups / thousand carbon atoms of vinyl unsaturation present in the LLDPE backbone. All individual values of less than 0.15 vinyl groups / thousand carbon atoms are included and disclosed herein. For example, the LLDPE may have less than 0.15 vinyl groups / thousand carbon atoms of vinyl unsaturation, or alternatively, less than 0.12 vinyl groups / thousand carbon atoms, or alternatively, less than 0.09 vinyl groups / thousand carbon atoms, or alternatively, less than 0.06 vinyl groups / thousand carbon atoms.
[0036] In one embodiment, the LLDPE contains less than or equal to 100 parts by weight, such as less than 10 parts by weight, less than 8 parts by weight, less than 5 parts by weight, less than 4 parts by weight, less than 1 part by weight, less than 0.5 parts by weight or less than 0.1 parts by weight of metal complex residues remaining from a catalyst system comprising a metal complex of a polyvalent aryloxy ether per one million parts of LLDPE. The metal complex residues remaining from a catalyst system comprising a metal complex of a polyvalent aryloxy ether in the LLDPE can be measured by X-ray fluorescence (XRF), which is calibrated against a reference standard. In a preferred method, the polymer resin particles can be compression molded at an elevated temperature into a plaque having a thickness of about 3 / 8 inches for X-ray measurement. At very low metal complex concentrations, such as less than 0.1 ppm, ICP-AES would be a suitable method for determining the metal complex residues present in the LLDPE.
[0037] LLDPE may further contain other components, such as one or more other polymers and / or one or more additives. Such additives include, but are not limited to, antistatic agents, color enhancers, dyes, lubricants, fillers such as TiO 2 or CaCO 3 , opacifiers, nucleating agents, processing aids, pigments, primary antioxidants, secondary antioxidants, processing aids, UV stabilizers, anti-blocking agents, slip agents, tackifiers, flame retardants, antimicrobial agents, deodorants, antifungal agents and combinations thereof. Based on the weight of the LLDPE including such additives, the LLDPE may contain from about 0.1% to about 10% of such additives by combined weight.
[0038] The LLDPE may be prepared using any conventional ethylene (co)polymerization solution single reactor reaction process. One method for preparing the LLDPE disclosed herein is described in detail in US Pat. No. 5,977,251, the disclosure of which is incorporated herein by reference in its entirety.
[0039] In one embodiment, the LLDPE is prepared by a solution polymerization process in a single reactor, wherein the process comprises polymerizing ethylene and optionally one or more α-olefins in the presence of a catalyst system comprising a metal complex of a polyvalent aryloxyether corresponding to the formula:
[0040]
[0041] Among them, M 3 is Ti, Hf or Zr, preferably Zr;
[0042] Ar 4 In each occurrence, independently replace C 9-20 Aryl, wherein the substituents are independently selected at each occurrence from alkyl; cycloalkyl; and aryl; and halo-, trialkylsilyl-, and haloalkyl-substituted derivatives thereof, provided that at least one substituent lacks coplanarity with the aryl group to which it is attached;
[0043] T 4 C independently at each occurrence 2-20 Alkylene, cycloalkylene or cycloalkenylene, or inertly substituted derivatives thereof;
[0044] R 21 is independently at each occurrence hydrogen, halo, hydrocarbyl, trihydrocarbylsilyl, trihydrocarbylsilylhydrocarbyl, alkoxy or di(hydrocarbyl)amino, up to 50 atoms not counting hydrogen;
[0045] R 3 is independently at each occurrence hydrogen, halo, hydrocarbyl, trihydrocarbylsilyl, trihydrocarbylsilylhydrocarbyl, alkoxy, or amino, up to 50 atoms not counting hydrogen, or two R on the same arylene ring. 3 The groups together may be the same or different on the arylene ring R 3 and R 21 The groups together form a divalent ligand group that is attached to the arylene group at two positions or that connects two different arylene rings together; and
[0046] R D is independently at each occurrence halogenated or a hydrocarbon or trihydrocarbylsilyl group having up to 20 atoms, not counting hydrogen, or 2 R D The groups together are a hydrocarbylene, hydrocarbylene, diene or poly(hydrocarbyle)silylene.
[0047] The ethylene / α-olefin interpolymer composition can be prepared by solution polymerization according to the following exemplary method.
[0048] All raw materials (ethylene, 1-hexene) and process solvents (narrow boiling range high purity isoparaffin solvents commercially available from ExxonMobil Corporation under the trade name ISOPAR E) were purified with molecular sieves before introduction into the reaction environment. Hydrogen was supplied in high purity grades in pressurized cylinders without further purification. The reactor monomer feed (ethylene) stream was pressurized to a pressure above the reaction pressure, approaching 750 psig, by a mechanical compressor. The solvent and comonomer (1-hexene) feeds were pressurized to a pressure above the reaction pressure, approximately 750 psig, by a mechanical positive displacement pump. Each catalyst component was manually diluted in batches with a purified solvent (ISOPAR E) to a specified component concentration and pressurized to a pressure above the reaction pressure, approximately 750 psig. All reaction feed flows were measured with mass flow meters and independently controlled by a computer automatic valve control system.
[0049] By passing the feed stream through a heat exchanger, the combined feed of solvent, monomer, comonomer and hydrogen to the reactor is independently temperature controlled at any temperature between 5°C and 50°C, typically 40°C. The fresh comonomer feed entering the polymerization reactor is injected into the reactor. The catalyst component is injected into the polymerization reactor through a specially designed injection needle without contact time before the reactor. The main catalyst component feed is controlled by a computer to maintain the reactor monomer concentration at a specified target. Two cocatalyst components are added to the main catalyst component based on a calculated specified molar ratio. Immediately after each fresh injection position (feed or catalyst), the feed stream is mixed with the circulating polymerization reactor contents with a static mixing element. The contents of the reactor are continuously circulated through a heat exchanger, which is responsible for removing most of the reaction heat, and the temperature on the coolant side is responsible for maintaining an isothermal reaction environment at a specified temperature. The circulation of each reactor loop is provided by a screw pump. When the stream leaves the reactor, it contacts a deactivating agent such as water to stop the reaction. In addition, various additives, such as antioxidants, can be added at this time. The stream then passes through another set of static mixing elements to evenly disperse the catalyst kill agent and additives.
[0050] After the addition of additives, the effluent (containing solvent, monomer, comonomer, hydrogen, catalyst components and molten polymer) passes through a heat exchanger to raise the stream temperature in preparation for separating the polymer from other lower boiling reaction components. The stream then enters a two-stage separation and devolatilization system, where the polymer is removed from the solvent, hydrogen and unreacted monomer and comonomer. The recycled stream is purified before entering the reactor again. The separated and devolatilized polymer melt is pumped through a die specially designed for underwater pelletization, cut into uniform solid pellets, dried and transferred to a hopper.
[0051] In one embodiment, the LLDPE is prepared by a polymerization process in a single solution phase loop reactor system, wherein the catalyst system comprises (a) one or more procatalysts comprising a metal-ligand complex of formula (I):
[0052]
[0053] in:
[0054] M is titanium, zirconium or hafnium, each independently in a formal oxidation state of +2, +3 or +4; n is an integer from 0 to 3, and wherein when n is 0, X is absent; and
[0055] Each X is independently a monodentate ligand that is neutral, monoanionic or dianionic; or two X together form a neutral, monoanionic or dianionic bidentate ligand; X and n are selected so that the metal-ligand complex of formula (I) is neutral overall; and
[0056] Each Z is independently O, S, N(C1-C40)alkyl or P(C1-C40)alkyl; and
[0057] L is (C3-C40)alkylene or (C3-C40)heteroalkylene, wherein the (C3-C40)alkylene has a portion of a linker backbone comprising 3-carbon atoms to 10-carbon atoms that connects to the Z atom in formula (I) (to which L is bonded) and the (C3-C40)heteroalkylene has a portion of a linker backbone comprising 3-atoms to 10-atoms that connects to the Z atom in formula (I), wherein each of the 3 to 10 atoms of the 3-atoms to 10-atoms linker backbone of the (C3-C40)heteroalkylene is independently a carbon atom or a heteroatom, wherein each heteroatom is independently O, S, S(O), S(O)2, Si(R) C )2、Ge(R C 2. P(R P ) or N(R N ), where independently each R C is a (C1-C30) hydrocarbon group; each R P is a (C1-C30) hydrocarbon group; and each R N is (C1-C30)hydrocarbyl or is absent; and
[0058] R 1-26 Each independently selected from (C1-C40)alkyl, (C1-C40)heteroalkyl, Si(R C )3、Ge(R C ) 3 , P(R P )2、N(R N )2.OR C , SR C、NO2、CN、CF3、R C S(O)-、R C S(O)2-、(R C )2C=N-、R C C(O)O-、R C OC(O)-、R C C(O)N(R)-、(R C )2NC(O)-, halogen atoms, hydrogen atoms and any combination thereof, hydrocarbon groups, heteroalkyl groups, Si(R C ) 3 , Ge(R C ) 3 , P(R P ) 2 、N(R N ) 2 , OR C , SR C , R C S(O)-、R C S(O) 2 -、(R C ) 2 C=N-、R C C(O)O-、R C OC(O)-、R C C(O)N(R)-、(R C ) 2 Each of NC(O)-, alkylene and heteroalkylene is independently unsubstituted or substituted with one or more R S Substituent substitution, each R S are independently halogen atoms, polyfluorinated, perfluorinated, unsubstituted (C 1 -C 18 ) alkyl, F 3 C-、FCH 2 O-、F 2 HCO-、F 3 CO-、R 3 Si-、R 3 Ge-, RO-, RS-, RS(O)-, RS(O) 2 -、R 2 P-、R 2 N-、R 2 C=N-, NC-, RC(O)O-, ROC(O)-, RC(O)N(R)- or R 2 NC(O)-, or two R S Together they form unsubstituted (C 1 -C 18 )alkylene, wherein each R is independently unsubstituted (C 1 -C18 )alkyl;
[0059] When R 7 When H, R 8 For (C 1 -C 40 ) alkyl; (C 1 -C 40 ) heteroalkyl; Si(R C ) 3 , Ge(R C ) 3 , P(R P ) 2 ,N(R N ) 2 , OR C , SR C , NO 2 , CN, CF 3 , R C S(O)-,R C S(O) 2 -,(R C ) 2 C=N-,R C C(O)O-,R C OC(O)-,R C C(O)N(R)-,(R C ) 2 NC(O)- or a halogen atom; or when R 8 When H, R 7 For (C 1 -C 40 ) alkyl; (C 1 -C 40 ) heteroalkyl; Si(R C ) 3 , Ge(R C ) 3 , P(R P ) 2 ,N(R N ) 2 , OR C , SR C , NO 2 , CN, CF 3 , R C S(O)-,R C S(O)2-,(R C ) 2 C=N-,R C C(O)O-,R C OC(O)-,R C C(O)N(R)-,(R C ) 2NC(O)- or halogen atom;
[0060] Optionally, R 1-26 Two or more R groups of a group (e.g., from R 1-7 , R 8-14 , R 8-11 , R 1-3 , R 4-7 , R 15 -20 , R 21-26 ) may be combined together to form a ring structure having from 3 to 50 atoms in the ring, excluding any hydrogen atoms; and Y has the formula -T(R d ) b and contains four or more non-hydrogen atoms, wherein T is independently selected from C, Si, Ge, N, O, S, P or a combination thereof for each occurrence of Y, and wherein T is replaced by R d Substituents are substituted, and b is an integer from 1 to 3, depending on T and R d The valence of each R d is a substituent selected from hydrogen, (C 1 -C 40 ) alkyl; (C 1 -C 40 ) heteroalkyl; Si(R C ) 3 , Ge(R C ) 3 , P(R P ) 2 ,N(R N ) 2 , OR C , SR C , NO 2 , CN, CF 3 , R C S(O)-,R C S(O) 2 -,(R C ) 2 C=N-,R C C(O)O-,R C OC(O)-,R C C(O)N(R)-,(R C ) 2 NC(O)- or a halogen atom.
[0061] As used herein, the term “ 1 -C 40 )alkyl" refers to a hydrocarbon radical having 1 to 40 carbon atoms. 1 -C 40The term "alkylene" refers to a hydrocarbon diradical having 1 to 40 carbon atoms, wherein each hydrocarbon radical and diradical is independently aromatic (6 carbon atoms or more) or non-aromatic, saturated or unsaturated, straight chain or branched, cyclic (including monocyclic and polycyclic, fused and non-fused polycyclic, including bicyclic; 3 carbon atoms or more) or acyclic, or a combination of two or more thereof; and each hydrocarbon radical and diradical is independently the same as or different from another hydrocarbon radical and diradical, and is independently unsubstituted or substituted by one or more R S replace.
[0062] Preferably, the (C1-C40)hydrocarbyl group is independently unsubstituted or substituted (C1-C40)alkyl, (C3-C40)cycloalkyl, (C3-C20)cycloalkyl-(C1-C20)alkylene, (C6-C40)aryl, or (C6-C20)aryl-(C1-C20)alkylene. More preferably, each of the aforementioned (C1-C40)hydrocarbyl groups independently has a maximum of 20 carbon atoms (i.e., a (C1-C20)hydrocarbyl group) and still more preferably a maximum of 12 carbon atoms.
[0063] The terms "(C1-C40) alkyl" and "(C1-C18) alkyl" refer to saturated straight or branched chain hydrocarbon groups of 1 to 40 carbon atoms or 1 to 18 carbon atoms, respectively, which are unsubstituted or substituted with one or more R S Examples of unsubstituted (C1-C40)alkyl are unsubstituted (C1-C20)alkyl; unsubstituted (C1-C10)alkyl; unsubstituted (C1-C5)alkyl; methyl; ethyl; 1-propyl; 2-propyl; 1-butyl; 2-butyl; 2-methylpropyl; 1,1-dimethylethyl; 1-pentyl; 1-hexyl; 1-heptyl; 1-nonyl; and 1-decyl. Examples of substituted (C1-C40)alkyl are substituted (C1-C20)alkyl, substituted (C1-C10)alkyl, trifluoromethyl, and (C45)alkyl. (C45)alkyl is, for example, replaced by one R S Substituted (C27-C40) alkyl, R S Preferably, each (C1-C5)alkyl group is independently methyl, trifluoromethyl, ethyl, 1-propyl, 1-methylethyl or 1,1-dimethylethyl.
[0064] The term "(C6-C40)aryl" refers to an unsubstituted or (substituted with one or more R S)substituted mono-, bi- or tricyclic aromatic hydrocarbon groups having 6 to 40 carbon atoms, wherein at least 6 to 14 carbon atoms are aromatic ring carbon atoms, and the mono-, bi- or tricyclic groups contain 1, 2 or 3 rings, respectively; wherein 1 of the rings is aromatic, the 2 or 3 rings are independently fused or non-fused and at least one of the 2 or 3 rings is aromatic. Examples of unsubstituted (C6-C40)aryl groups are unsubstituted (C6-C20)aryl groups; unsubstituted (C6-C18)aryl groups; 2-(C1-C5)alkyl-phenyl groups; 2,4-bis(C1-C5)alkyl-phenyl groups; phenyl groups; fluorenyl groups; tetrahydrofluorenyl groups; indacenyl groups; hexahydrodicyclopentadienylphenyl groups; indenyl groups; dihydroindenyl groups; naphthyl groups; tetrahydronaphthyl groups; and phenanthrene groups. Substituted (C6-C40)aryl groups are preferably substituted (C6-C20)aryl groups; 2-(C1-C5)alkyl-phenyl groups; 2,4-bis(C1-C5)alkyl-phenyl groups; phenyl groups; fluorenyl groups; tetrahydrofluorenyl groups; indacenyl groups; hexahydrodicyclopentadienylphenyl groups; indenyl groups; dihydroindenyl groups; naphthyl groups; tetrahydronaphthyl groups; and phenanthrene groups. 6 -C 40 Examples of )aryl groups are substituted (C6-C20)aryl groups; substituted (C6-C18)aryl groups; 2,4-bis[(C20)alkyl]-phenyl groups; polyfluorophenyl groups; pentafluorophenyl groups; and fluoren-9-on-1-yl groups.
[0065] The term "(C3-C40) cycloalkyl" refers to a saturated cyclic hydrocarbon group of 3 to 40 carbon atoms, which is unsubstituted or substituted with one or more R S The cycloalkyl radicals of (C3-C12) cycloalkyl radicals are substituted with cycloalkyl radicals of (C3-C20) cycloalkyl radicals, cycloalkyl radicals of (C3-C10) cycloalkyl radicals, cyclopropyl radicals, cyclobutyl radicals, cyclopentyl radicals, cyclohexyl radicals, cycloheptyl radicals, cyclooctyl radicals, cyclononyl radicals and cyclodecyl radicals. The cycloalkyl radicals of (C3-C40) cycloalkyl radicals are substituted with cycloalkyl radicals of (C3-C20) cycloalkyl radicals, substituted with cycloalkyl radicals, cyclopentane-2-yl radicals and 1-fluorocyclohexyl radicals.
[0066] Examples of (C1-C40)alkylene groups are unsubstituted or substituted (C6-C40)arylene groups, (C3-C40)cycloalkylene groups, and (C1-C40)alkylene groups (e.g., (C1-C20)alkylene groups). In some embodiments, the diradicals are on the same carbon atom (e.g., -CH2-) or on adjacent carbon atoms (i.e., 1,2-diradicals), or are separated by one, two, or more intervening carbon atoms (e.g., respective 1,3-diradicals, 1,4-diradicals, etc.). Preferred are 1,2-, 1,3-, 1,4-, or α,ω-diradicals, more preferably 1,2-diradicals. α,ω-diradicals are diradicals having the largest carbon backbone spacing between radical carbons. More preferred is a (C6-C18)arylene group, a (C3-C20)cycloalkylene group or a (C2-C20)alkylene group in the form of a 1,2-diradical, a 1,3-diradical or a 1,4-diradical.
[0067] The term "(C1-C40)alkylene" refers to a saturated straight or branched chain diradical (ie, the radical is not on a ring atom) of 1 to 40 carbon atoms, which is unsubstituted or substituted by one or more R S Examples of the unsubstituted (C1-C40)alkylene group are unsubstituted (C1-C20)alkylene groups, including unsubstituted 1,2-(C2-C10)alkylene groups; 1,3-(C3-C10)alkylene groups; 1,4-(C4-C10)alkylene groups; -CH2-, -CH2CH2-, -(CH2)3-, -(CH2)4-, -(CH2)5-, -(CH2)6-, -(CH2)7-, -(CH2)8-, and -(CH2)4C(H)(CH3)-. Examples of substituted (C1-C40)alkylene groups are substituted (C1-C20)alkylene groups, -CF2-, -C(O)-, and -(CH 2 ) 14 C(CH 3 ) 2 (CH 2 ) 5 - (i.e., 6,6-dimethyl-substituted n-1,20-eicosyl). As mentioned above, the two R S Examples of the substituted (C1-C40)alkylene groups that can be formed together include 1,2-bis(methylene)cyclopentane, 1,2-bis(methylene)cyclohexane, 2,3-bis(methylene)-7,7-dimethyl-bicyclo[2.2.1]heptane, and 2,3-bis(methylene)bicyclo[2.2.2]octane.
[0068] The term "(C3-C40)cycloalkylene" refers to a cyclic diradical (i.e., the radical is on a ring atom) of 3 to 40 carbon atoms, which is unsubstituted or substituted with one or more R S Substitution. Examples of unsubstituted (C3-C40)cycloalkylene groups are 1,3-cyclopropylene, 1,1-cyclopropylene, and 1,2-cyclohexylene. Examples of substituted (C3-C40)cycloalkylene groups are 2-oxo-1,3-cyclopropylene and 1,2-dimethyl-1,2-cyclohexylene.
[0069] The term "(C1-C40) heteroalkyl" refers to a heteroalkyl having 1 to 40 carbon atoms, and the term "(C1-C40) heteroalkylene" refers to a heteroalkyl diradical having 1 to 40 carbon atoms, and each heteroalkyl independently has one or more heteroatoms O; S; S(O); S(O)2; Si(R C )2;Ge(R C )2; P(R P ); and N(R N), where each R C is independently an unsubstituted (C1-C18) hydrocarbon group, each R P is an unsubstituted (C1-C18) hydrocarbon group; and each R N is an unsubstituted (C1-C18)alkyl or absent (e.g., absent when N comprises -N= or a tri-carbon substituted N). The heteroalkyl radical and each heteroalkyl diradical are independently on a carbon atom or a heteroatom thereof, but are preferably on a carbon atom when bonded to a heteroatom in formula (I) or to a heteroatom of another heteroalkyl or heteroalkylene radical. Each (C1-C40)heteroalkyl and (C1-C40)heteroalkylene radical independently may be unsubstituted or (substituted by one or more R S ) substituted, aromatic or non-aromatic, saturated or unsaturated, linear or branched, cyclic (including monocyclic and polycyclic, fused and non-fused polycyclic) or acyclic, or a combination of two or more thereof; and each is the same as or different from the other.
[0070] Co-catalyst component
[0071] In some embodiments, the procatalyst comprising a metal-ligand complex of formula (I) may be catalytically active by contacting it with an activating cocatalyst or in combination with an activating cocatalyst or by using known activation techniques, such as those known in the art for use with metal-based olefin polymerization reactions. Suitable activating cocatalysts for use in the present invention include alkylaluminums; polymeric or oligomeric aluminoxanes (also referred to as aluminoxanes); neutral Lewis acids; and non-polymeric, non-coordinating ion-forming compounds (including use of these compounds under oxidizing conditions). Suitable activation techniques are bulk electrolysis. Combinations of one or more of the foregoing activating cocatalysts and techniques are also contemplated. The term "alkylaluminum" refers to monoalkylaluminum dihydrides or monoalkylaluminum dihalides, dialkylaluminum hydrides or dialkylaluminum halides, or trialkylaluminums. Aluminoxanes and their preparations are known, for example, in U.S. Pat. No. (U.S. Pat. No.) 6,103,657. Examples of preferred polymeric or oligomeric aluminoxanes are methylaluminoxane, triisobutylaluminum-modified methylaluminoxane, and isobutylaluminoxane.
[0072] Exemplary Lewis acid activating cocatalysts are Group 13 metal compounds containing 1-3 hydrocarbyl substituents as described herein. In some embodiments, exemplary Group 13 metal compounds are tri(hydrocarbyl)-substituted-aluminum or tri(hydrocarbyl)-boron compounds. In some other embodiments, exemplary Group 13 metal compounds are tri(hydrocarbyl)-substituted-aluminum or tri(hydrocarbyl)-boron compounds are tri((C1-C10)alkyl)aluminum or tri((C6-C18)aryl)boron compounds and halogenated (including perhalogenated) derivatives. In some other embodiments, exemplary Group 13 metal compounds are tri(fluoro-substituted phenyl)borane, and in other embodiments, are tri(pentafluorophenyl)borane. In some embodiments, the activating co-catalyst is tri((C1-C20)alkyl)borate (e.g., trityl tetrafluoroborate) or tri((C1-C20)alkyl)ammoniumtetra((C1-C20)alkyl)borane (e.g., bis(octadecyl)methylammoniumtetra(pentafluorophenyl)borane). As used herein, the term "ammonium" refers to a nitrogen cation, which is a ((C1-C20)alkyl)4N + ,((C1-C20)alkyl)3N(H) + ,((C1-C20)alkyl)2N(H)2 + , (C1-C20)alkylN(H)3 + or N(H)4 + , wherein each (C1-C20) hydrocarbon group may be the same or different.
[0073] Exemplary combinations of neutral Lewis acid activating cocatalysts include mixtures comprising a combination of tri((C1-C4)alkyl)aluminum and a tri((C6-C18)aryl)boron halide compound, particularly tri(pentafluorophenyl)borane. Other exemplary embodiments are combinations of such neutral Lewis acid mixtures with polymeric or oligomeric aluminoxanes, and combinations of a single neutral Lewis acid, particularly tri(pentafluorophenyl)borane with polymeric or oligomeric aluminoxanes. Exemplary embodiments of the molar ratio of (metal-ligand complex):(tri(pentafluoro-phenylborane):(aluminoxane) [e.g., (Group 4 metal-ligand complex):(tri(pentafluoro-phenylborane):(aluminoxane)] are 1:1:1 to 1:10:30, and other exemplary embodiments are 1:1:1.5 to 1:5:10.
[0074] A number of activating cocatalysts and activation techniques have been previously taught for different metal-ligand complexes in the following U.S. patents: U.S. 5,064,802; U.S. 5,153,157; U.S. 5,296,433; U.S. 5,321,106; U.S. 5,350,723; U.S. 5,425,872; U.S. 5,625,087; U.S. 5,721,185; U.S. 5,783,512; U.S. 5,883,204; U.S. 5,919,983; U.S. 6,696,379; and U.S. 7,163,907. Examples of suitable alkoxides are disclosed in U.S. Patent 5,296,433. Examples of suitable Bronsted acid salts for addition polymerization catalysts are disclosed in U.S. Pat. Nos. 5,064,802; 5,919,983; 5,783,512. Examples of suitable salts of cationic oxidants and non-coordinating compatible anions for use as activating co-catalysts for addition polymerization catalysts are disclosed in U.S. Pat. No. 5,321,106. Examples of suitable carbocation salts for use as activating co-catalysts for addition polymerization catalysts are disclosed in U.S. Pat. No. 5,350,723. Examples of silylium salts for use as activating co-catalysts for addition polymerization catalysts are disclosed in U.S. Pat. No. 5,625,087. Examples of suitable complexes of alcohols, thiols, silanols and oximes with tris(pentafluorophenyl)borane are disclosed in U.S. Pat. No. 5,296,433. Some of these catalysts are also described in a portion of US Patent 6,515,155 Bl, beginning at column 50, line 39 and continuing through column 56, line 55, only this portion of which is incorporated herein by reference.
[0075] In some embodiments, the procatalyst comprising a metal-ligand complex of formula (I) can be activated to form an active catalyst composition by combining with one or more cocatalysts (e.g., a cation-forming cocatalyst, a strong Lewis acid, or a combination thereof). Suitable cocatalysts for use include polymeric or oligomeric aluminoxanes, particularly methylaluminoxane, and inert compatible non-coordinating ion-forming compounds. Exemplary suitable cocatalysts include, but are not limited to, modified methylaluminoxane (MMAO), bis(hydrogenated tallow alkyl) methyl, tetrakis(pentafluorophenyl)borate (1-)amine, triethylaluminum (TEA), and any combination thereof.
[0076] In some embodiments, one or more of the aforementioned activating cocatalysts are used in combination with each other. A particularly preferred combination is a mixture of tri((C1-C4)hydrocarbyl)aluminum, tri((C1-C4)hydrocarbyl)borane or ammonium borate with an oligomeric or polymeric aluminoxane compound.
[0077] The ratio of the total moles of one or more metal-ligand complexes of formula (I) to the total moles of one or more activating co-catalysts is 1:10,000 to 100:1. In some embodiments, the ratio is at least 1:5000, in some other embodiments at least 1:1000; and 10:1 or less, and in some other embodiments, 1:1 or less. When aluminoxane is used alone as an activating co-catalyst, the moles of aluminoxane preferably employed are at least 100 times the moles of the metal-ligand complex of formula (I). When tris(pentafluorophenyl)borane is used alone as an activating co-catalyst, in some other embodiments, the moles of tris(pentafluorophenyl)borane employed form 0.5:1 to 10:1 with the total moles of one or more metal-ligand complexes of formula (I), in some other embodiments 1:1 to 6:1, and in some other embodiments 1:1 to 5:1. The remaining activating co-catalysts are typically used in a molar amount approximately equal to the total molar amount of the one or more metal-ligand complexes of formula (I).
[0078] End-use applications
[0079] The LLDPE according to the present disclosure is suitable for use in blown film extrusion processes. The LLDPE according to the present disclosure can be extruded in pure form or in blends with other polymers, additives and fillers. The film can be a single layer or coextruded multilayer film obtained by various extrusions via a single or multiple die heads. The resulting film can be used as is, or can be laminated to other films or substrates, for example by heat, adhesive lamination or direct extrusion onto a substrate. The resulting films and laminates can be subjected to other forming operations, such as embossing, stretching, thermoforming. Surface treatments such as corona can be applied and the film can be printed.
[0080] The thickness of the film according to the present invention is in the range of 20 to 120 microns. All individual values and subranges from 20 to 120 microns (μm) are disclosed and included herein. For example, the thickness of the film can be in the range of the lower limit of 20, 40, 60, 80 or 100 microns to the upper limit of 30, 50, 70, 90, 110 or 120 microns. For example, the thickness of the film can be in the range of 20 microns to 120 microns, or in the alternative, 20 microns to 60 microns, or in the alternative, 40 microns to 100 microns, or in the alternative, 20 microns to 70 microns.
[0081] In one particular embodiment, the film is made from the linear low density polyethylene composition of the present invention without other polymer components.
[0082] In another embodiment, the film is made of a blend of the linear low density polyethylene composition of the present invention blended with low density polyethylene (LDPE).
[0083] In a specific embodiment, a monolayer film having a thickness of 50 microns is prepared only from the linear low density polyethylene composition of the present invention and has a haze equal to or less than 30%.
[0084] In a specific embodiment, a monolayer film having a thickness of 50 microns is prepared solely from the linear low density polyethylene composition of the present invention and exhibits a dart impact equal to or greater than 1,000 grams (g). At the same time, the processability of the polyethylene of the present invention results in at least 8% lower melt pressure and at least 8% lower current consumption than conventional metallocene-LLDPE produced in a gas phase process at similar melt index and density values and equivalent processing hardware and conditions.
[0085] In yet another embodiment, 85 wt% of the linear low density polyethylene composition of the present invention and 15 wt% of LDPE (density 0.923 g / cm 3 and I 2 A single-layer film having a thickness of 50 μm was prepared using a prepreg (0.75 g / 10 min) and a haze of the film was equal to or less than 5%.
[0086] In a specific embodiment, 85 wt% of the linear low-density polyethylene composition of the present invention and 15 wt% of LDPE (density 0.923 g / cm 3 and I 2 A single layer film having a thickness of 50 microns was prepared (0.75 g / 10 min) and a dart impact of the film was equal to or greater than 450 grams (g).
[0087] Films made from the compositions of the present invention can be used for a variety of purposes, such as films for lamination, for frozen food packaging, for silage wrapping films, for stretch hood films, and many other agricultural, food packaging, and industrial packaging applications.
[0088] Examples
[0089] The following examples illustrate the invention but are not intended to limit the scope of the invention. The examples of the invention demonstrate that selection of the LLDPE of the present disclosure results in [improved properties] while maintaining the polymerization process at a low cost.
[0090] Comparative composition 1 is EXCEED 1018, which is an ethylene-hexene copolymer prepared by a gas phase polymerization process in the presence of a metallocene catalyst system, with a melt index (I 2 ) is about 1.0 g / 10 minutes, and the density is about 0.918 g / cm 3 , the CEF fraction from 70℃ to 90℃ was 61.9%, I 10 / I 2The MgO-T(R) is about 6.0 and is commercially available from ExxonMobil Chemical Company (Houston, Texas, USA).
[0091] Comparative composition 2 is DOWLEX 4056G, which is an ethylene-hexene copolymer with a melt index (I 2 ) is 1.3 g / 10 min, and the density is 0.916 g / cm 3 , CEF fraction at 70-90℃ was 50.3%, I 10 / I 2 The OD 2000 is 7.4 and is commercially available from The Dow Chemical Company (Midland, Michigan, USA).
[0092] Composition 1 of the present invention is an ethylene-hexene copolymer prepared in a single reactor by a solution polymerization process in the presence of a catalyst system comprising a metal complex of a polyvalent aryloxy ether, and the melt index (I 2 ) is 1.05g / 10min, and the density is 0.916g / cm 3 , CEF grade from 70 to 90°C was 90.3%, I 10 / I 2 The composition 1 of the present invention is prepared by solution polymerization in the presence of a zirconium-based catalyst system ("post-metallocene catalyst") in a single loop reactor system described in U.S. Pat. No. 5,977,251, wherein the catalyst system comprises [2,2"'-[1,3-propanediylbis(oxy-κO)]bis[3",5,5"-tris(1,1-dimethylethyl)-5'-methyl[1,1':3',1"-terphenyl]-2'-hydroxyolato-κO]]dimethyl-, (OC-6-33)-zirconium represented by the following formula:
[0093]
[0094] The polymerization conditions of the composition 1 of the present invention are listed in Tables 1 and 2. Referring to Tables 1 and 2, TEA is triethylaluminum, PETROSOLD 100 / 120 is a solvent, available from CEPSA (Madrid, Spain) The molecular weight properties of the inventive and comparative compositions were measured and are reported in Table 3.
[0095] Table 1
[0096]
[0097] Table 2
[0098]
[0099]
[0100] Table 3
[0101] <![CDATA[M n (g / mol)]]> <![CDATA[M w (g / mol)]]> <![CDATA[M z (g / mol)]]> <![CDATA[M w / M n ]]> <![CDATA[M z / M w <!-- 12 -->]]> Composition 1 of the present invention 43400 94000 178000 2.17 1.89 Comparative composition 1 39600 104100 185000 2.63 1.78 Comparative composition 2 28800 111500 320000 3.88 2.87
[0102] The inventive composition 1 and comparative compositions 1 and 2 were extruded on a COVEX 45 mm blown film line to produce monolayer films, forming inventive film 1, comparative film 1 and comparative film 2. The monolayer films were prepared according to the process conditions shown in Tables 4 and 5. For each of the extruder hopper blends of 85 wt% and 15 wt% LDPE 310E (commercially available from The Dow Chemical Company) of the inventive composition 1 and comparative compositions 1 and 2, additional monolayer films were prepared under the same conditions, as shown in Table 6.
[0103] Table 4
[0104] Die head gap (mm): 0.8 Line speed [m / min]: 7.5 Melt temperature (℃): 215 Output rate (Kg / h): 5 Thickness(μm):50
[0105] Table 5
[0106] Extruder conditions Blowing ratio 2.5:1 Corona treatment (dynes) 0 Die head gap (mm) 1.5 Output rate (Kg / h) 22.5 Screw speed (rpm) 60 Starting speed (m / min) 7 Frost White Line 33-34cm Flat folding 584mm Thickness(μm) 50
[0107] Table 6
[0108] Membrane Examples Made from the following extruder hopper blend: Film 2 of the present invention 85 wt% of Inventive Composition 1 and 15 wt% of LDPE 310E Comparison film 3 85 wt% Comparative Composition 1 and 15 wt% LDPE 310E Comparison Film 4 85 wt% Comparative Composition 2 and 15 wt% LDPE 310E
[0109] Tables 7 and 8 provide a number of properties for each of the Inventive Films 1 and 2 and Comparative Films 1-4.
[0110] Table 7
[0111]
[0112]
[0113]
[0114] Table 8
[0115]
[0116]
[0117]
[0118] Test Method
[0119] The test methods include the following:
[0120] Melt Index
[0121] Melt index (I) was measured at 190°C and under loads of 2.16 kg and 10 kg, respectively, according to ASTM D-1238. 2 and I 10 ). Its value is reported in g / 10min.
[0122] density
[0123] Samples for density measurement were prepared according to ASTM D4703. Measurements were made within one hour of pressing the sample using ASTM D792, Method B.
[0124] High temperature gel permeation chromatography
[0125] The gel permeation chromatography (GPC) system consisted of a Waters (Milford, Mass) 150C high temperature chromatograph (other suitable high temperature GPC instruments include Polymer Laboratories (Shropshire, UK) Model 210 and Model 220), equipped with an on-board differential refractometer (RI) (other suitable concentration detectors may include an IR4 infrared detector from Polymer ChAR (Valencia, Spain). Data collection was performed using Viscotek TriSEC software (Version 3) and a 4-channel Viscotek data manager DM400. The system was also equipped with an online solvent degasser from Polymer Laboratories (Shropshire, UK).
[0126] Suitable high temperature GPC columns can be used, such as four 30 cm long Shodex HT803 13 micron columns or four 30 cm Polymer Labs columns (MixA LS, Polymer Labs) of 20 micron mixed pore size fillers. The autosampler chamber is operated at 140 ° C, and the column chamber is operated at 150 ° C. The sample is prepared at a concentration of 0.1 grams of polymer in 50 ml of solvent. The chromatographic solvent and the sample preparation solvent contain 200 ppm of trichlorobenzene (TCB). Both solvents are bubbled with nitrogen. The polyethylene sample is gently stirred at 160 ° C for 4 hours. The injection volume is 200 microliters. The flow rate through GPC is set to 1 ml / min.
[0127] The GPC column set is calibrated by running 21 polystyrene standards with narrow molecular weight distributions. The molecular weight (MW) range of the standards is between 580 and 8,400,000, and the standards are included in 6 "cocktail" mixtures. There is at least a ten-fold interval between the individual molecular weights in each standard mixture. The standard mixture is purchased from Polymer Laboratories. For molecular weights equal to or greater than 1,000,000, polystyrene standards are prepared with 0.025g in 50mL solvent, and for molecular weights less than 1,000,000, 0.05g is prepared in 50mL solvent. Under gentle stirring, the polystyrene standards are dissolved at 80°C for 30 minutes. The narrow standard mixture is operated first, and in the order of decreasing the highest molecular weight component to minimize degradation. Polystyrene standard peak molecular weights were converted to polyethylene molecular weights using the following equation (as described in Williams and Ward, J. Polym. Sci., Polym. Letters, 6, 621 (1968)):
[0128] M 聚乙烯 =A×(M 聚苯乙烯 ) B ,
[0129] Where M is the molecular weight of polyethylene or polystyrene (as indicated by the label), and B is equal to 1.0. It is known to those of ordinary skill in the art that A can range from about 0.38 to about 0.44 and is determined using a broad polyethylene standard during calibration. Using this polyethylene calibration method to obtain molecular weight values, such as molecular weight distribution (MWD or M w / M n ), and related statistics (usually referred to as conventional GPC or cc-GPC results), are defined herein as the modified Williams and Ward method.
[0130] Crystallization Elution Fractionation (CEF) Method
[0131] The crystallization elution fractionation (CEF) method is described according to Monrabal et al., Macromol. Symp. 257, 71-79 (2007), which is incorporated herein by reference. The CEF instrument is equipped with an IR-4 detector (such as those commercially sold by PolymerChar, Spain) and a dual-angle light scattering detector model 2040 (such as those commercially sold by Precision Detectors). The IR-4 detector is operated in a composition mode with two filters: C006 and B057. A 50mm×4.6mm 10-micron guard column (such as those commercially sold by PolymerLabs) is installed in front of the IR-4 detector in the detector oven. Obtain o-dichlorobenzene (ODCB, 99% anhydrous grade) and 2,5-di-tert-butyl-4-methylphenol (BHT) (such as available from Sigma-Aldrich). Silica gel 40 (particle size 0.2-0.5mm) (such as available from EMD Chemicals) is also obtained. The silica gel was dried in a vacuum oven at 160°C for about two hours before use. Eight hundred milligrams of BHT and five grams of silica gel were added to two liters of ODCB. The ODCB containing BHT and silica gel is hereinafter referred to as "ODCB-m". ODBC-m was dried with dry nitrogen (N 2 ) was bubbled for one hour. By passing nitrogen at <90 psig through the CaCO 3 and Molecular sieves are used to obtain dry nitrogen. The sample solution is prepared by dissolving the polymer sample in ODCB-m at 4 mg / ml under shaking at 160°C for 2 hours using an automatic sampler. 300 μL of the sample solution is injected into the column. The temperature profile of CEF is: crystallization: from 110°C to 25°C at 3°C / min; thermal equilibrium: at 30°C for 5 minutes (including the soluble fraction elution time set to 2 minutes); and elution: from 25°C to 140°C at 3°C / min. The flow rate during crystallization is 0.052 mL / min. The flow rate during elution is 0.50 mL / min. IR-4 signal data is collected at one data point / second.
[0132] According to US2011 / 0015346 A1, the CEF column was filled with glass beads (such as those available from MO-SCI Specialty Products) at 125 μm ± 6% with 1 / 8 inch stainless steel tubing. The internal liquid volume of the CEF column was between 2.1 ml and 2.3 ml. Temperature calibration was performed using a mixture of NIST standard reference materials linear polyethylene 1475a (1.0 mg / ml) and eicosane (2 mg / ml) in ODCB-m. The calibration consisted of the following four steps: (1) calculation of the delay volume defined as the temperature offset between the measured eicosane peak elution temperature minus 30.00°C; (2) CEF raw temperature data minus the temperature offset of the elution temperature. It should be noted that this temperature shift is a function of experimental conditions such as elution temperature, elution flow rate, etc.; (3) a linear calibration line was generated that translates elution temperatures between 25.00°C and 140.00°C, such that NIST linear polyethylene 1475a has a peak temperature at 101.00°C and eicosane has a peak temperature of 30.00°C, (4) for the soluble fraction measured isothermally at 30°C, the elution temperature was linearly extrapolated by using an elution heating rate of 3°C / min. The reported elution peak temperatures were obtained such that the observed comonomer content calibration curves were consistent with those previously reported in US 8,372,931.
[0133] The CEF fraction from 70 to 90°C is defined as the integral of the IR-4 chromatogram (baseline minus measurement channel) with an elution temperature range of 70.0 to 90.0°C divided by the total integral from 25 to 140.0°C, according to the following equation:
[0134]
[0135] where T is the elution temperature (from the calibration discussed above).
[0136] The linear baseline was calculated by selecting two data points: one before polymer elution, typically at a temperature of 25.5° C., and the other after polymer elution, typically at 118° C. For each data point, the detector signal was subtracted from the pre-integration baseline.
[0137] Creep Zero Shear Viscosity Measurement Method
[0138] Zero shear viscosity was obtained by creep testing, which was performed at 190°C using 25 mm diameter parallel plates on an AR-G2 stress-controlled rheometer (TA Instruments; New Castle, Del.). The rheometer oven was set to the test temperature for at least 30 minutes before the fixture was zeroed. The compression molded sample disk was inserted between the plates and allowed to equilibrate for 5 minutes at the test temperature. The upper plate was then lowered to 50 μm above the desired test gap (1.5 mm). Any excess material was trimmed off and the upper plate was lowered to the desired gap. Measurements were performed at a flow rate of 5 L / min under a nitrogen purge. The default creep time was set to 2 hours.
[0139] A constant low shear stress of 20 Pa was applied to all samples to ensure that the steady-state shear rate was low enough to be in the Newtonian region. For the samples in this study, the steady-state shear rate obtained was between 10 -3 Up to 10 -4 s -1 The steady state is determined by performing a linear regression of all data points in the last 10% time window of the log(J(t)) versus log(t) plot, where J(t) is the creep compliance and t is the creep time. If the slope of the linear regression is greater than 0.97, steady state is considered to be reached and the creep test is stopped. In all cases in this study, the slope met the criterion within 2 hours. The steady-state shear rate is determined by the slope of the linear regression of all data points in the last 10% time window of the ε versus t curve, where ε is the strain. The zero shear viscosity is determined by the ratio of the applied stress to the steady-state shear rate.
[0140] To determine if the sample has degraded during the creep test, a small amplitude oscillatory shear test from 0.1 to 100 rad / s is performed on the same specimen before and after the creep test. The complex viscosity values of the two tests are compared. If the difference in the viscosity value at 0.1 rad / s is greater than 5%, the sample is considered to have degraded during the creep test and the result is discarded.
[0141] The zero shear viscosity ratio (ZSVR) is defined as the ratio of the zero shear viscosity (ZSV) of the branched polyethylene material to the ZSV of the linear polyethylene material at equivalent weight average molecular weight (Mw-gpc), according to the following equation:
[0142]
[0143] The ZSV value is obtained by creep testing at 190°C using the method described above. The Mw-gpc value is determined by conventional GPC methods. A correlation between the ZSV of linear polyethylene and its Mw-gpc is established based on a series of linear polyethylene reference materials. A description of the ZSV-Mw relationship can be found in the ANTEC program: Karjala, Teresa P.; Sammler, Robert L.; Mangnus, Marc A.; Hazlitt, Lonnie G.; Johnson, Mark S.; Hagen, Charles M., Jr.; Huang, Joe WL; Reichek, Kenneth N. Detection of low levels of long chain branching in polyolefins. Annual Technical Conference-Society of Plastics Engineers (2008), 66, 887-891.
[0144] 1 H NMR methods
[0145] 3.26 g of the stock solution was added to 0.133 g of the polyolefin sample in a 10 mm NMR tube. The stock solution was tetrachloroethane-d 2 (TCE) and perchloroethylene (50:50, w:w) with 0.001M Cr 3+ The solution in the tube was heated with N 2 Purge for 5 minutes to reduce the amount of oxygen. Leave the capped sample tube at room temperature overnight to swell the polymer sample. Shake the sample at 110°C to dissolve. The sample does not contain additives that may cause unsaturation, for example, slip agents such as erucamide.
[0146] 1 H NMR was performed on a Bruker AVANCE 400 MHz spectrometer at 120 °C with a 10 mm cryoprobe.
[0147] Two experiments were performed to obtain the degree of unsaturation: a control and a double presaturation experiment.
[0148] For control experiments, data were processed with an exponential window function, LB = 1 Hz, and baseline correction from 7 to -2 ppm. 1 The H signal was set to 100, and the integral I was between -0.5 and 3 ppm. 总 Used as the signal from the entire polymer in control experiments. CH 2 Number of groups NCH 2 The calculation is as follows:
[0149] NCH2 =I 总 / 2
[0150] For the double presaturation experiments, the data were processed with an exponential window function, LB = 1 Hz, and the baseline was corrected from 6.6 to 4.5 ppm. 1 The signal of H is set to 100, and the corresponding integral of unsaturation (I 1,2-亚乙烯基 ,I 三取代的 ,I 乙烯基 and I 亚乙烯基 ) Based on the attached Figure 2 The area shown is integrated.
[0151] Calculate the number of unsaturated units for vinylidene, trisubstituted, vinyl, and vinylidene:
[0152] N 1,2-亚乙烯基 =I 1,2-亚乙烯基 / 2
[0153] N 三取代的 =I 三取代的
[0154] N 乙烯基 =I 乙烯基 / 2
[0155] N 亚乙烯基 =I 亚乙烯基 / 2
[0156] Unsaturated units / 1,000,000 carbons are calculated as follows:
[0157] N 1,2-亚乙烯基 / 1,000,000C=(N 1,2-亚乙烯基 / NCH 2 )*1,000,000
[0158] N 三取代的 / 1,000,000C=(N 三取代的 / NCH 2 )*1,000,000
[0159] N 乙烯基 / 1,000,000C=(N 乙烯基 / NCH 2 )*1,000,000
[0160] N 亚乙烯基 / 1,000,000C=(N 亚乙烯基 / NCH 2 )*1,000,000
[0161] The requirements for the unsaturation NMR analysis included: a quantitative level of 0.47 ± 0.02 / 1,000,000 carbons for Vd2, 200 scans (data acquisition time less than 1 hour, including time for control experiments), a sample weight of 3.9% (for Vd2 structure, see Macromolecules, vol. 38, 6988, 2005), and a 10 mm high temperature cryoprobe. The quantitative level was defined as a signal-to-noise ratio of 10.
[0162] For the residual protons from TCT-d2 1 H signal, chemical shift reference set to 6.0ppm. Controls were run using ZG pulses, TD 32768, NS 4, DS12, SWH 10,000Hz, AQ 1.64s, D1 14s. Double presaturation experiments were run using a modified pulse sequence, O1P 1.354ppm, O2P 0.960ppm, PL9 57db, PL21 70db, TD 32768, NS200, DS4, SWH 10,000Hz, AQ 1.64s, D1 1s, D13 13s. The modified unsaturated pulse sequence using a Bruker AVANCE 400MHz spectrometer is shown below:
[0163]
[0164] Membrane test conditions
[0165] The following physical properties were measured on the produced films:
[0166] Dart impact: ISO 7765-1 / 1998
[0167] Tensile strength: ASTM 527-3
[0168] Shrinkage ASTM D2732
[0169] Puncture: ASTM D-5748-95
[0170] Elmendorf Tear: ASTM D1922-09
[0171] Gloss at 45 degrees: ASTM D2457-08
[0172] Haze: ASTM D1003-11
[0173] Hot Adhesive CD: ASTM F1921-98
[0174] Seal strength CD: ASTM F2029-00
[0175] The present invention may be embodied in other forms without departing from the spirit and essential attributes thereof, and, accordingly, reference should be made to the appended claims rather than to the foregoing specification as indicating the scope of the invention.
[0176] In summary, the present invention includes but is not limited to the following items:
[0177] 1. A linear low density polyethylene composition having each of the following properties:
[0178] (1) The CEF fraction at 70 to 90°C is equal to or greater than 80% of the total CEF fraction;
[0179] (2) Melt index I measured according to ASTM D 1238 (2.16 kg, 190° C.) 2 range of 0.8-1.5 g / 10 minutes; and
[0180] (3) Melt flow ratio I 10 / I 2 The range is 7.0-8.0.
[0181] 2. The linear low density polyethylene composition according to claim 1, further having a molecular weight of 0.914 to 0.920 g / cm 3 Density (measured according to ASTM D792).
[0182] 3. The linear low density polyethylene composition according to any one of the preceding items, wherein the polyethylene comprises units derived from ethylene and units derived from one or more comonomers selected from butene, hexene and octene.
[0183] 4. The linear low density polyethylene composition according to any one of the preceding items, wherein the polyethylene comprises units derived from ethylene and units derived from hexene.
[0184] 5. The linear low density polyethylene composition according to any of the preceding items, wherein the polyethylene is produced in a single loop solution polymerization reactor.
[0185] 6. The linear low density polyethylene composition according to any one of the preceding items, wherein a film layer having a thickness of 50 microns prepared from a blend of 85 wt% of the linear low density polyethylene composition and 15 wt% of a low density polyethylene has a density of 0.923 g / cm 3 , I 2 0.75g / 10min, with one or more of the following properties:
[0186] (i) a haze of less than 5%; and
[0187] (ii) Dart impact strength greater than 450 g.
[0188] 7. The linear low density polyethylene composition according to any one of the preceding items, wherein a film layer prepared only from the linear low density polyethylene composition exhibits a dart drop impact strength equal to or greater than 1,000 g.
[0189] 8. An article comprising at least one component prepared from the linear low-density polyethylene composition according to any one of items 1 to 5.
[0190] 9. The article of claim 8, wherein the article is a stand-up bag.
Claims
1. A film layer prepared from a linear low density polyethylene composition, the linear low density polyethylene composition having each of the following properties: (1) The CEF fraction of 70 to 90°C is equal to or greater than 80% of the total CEF fraction; (2) a melt index I2 range of 0.8-1.5 g / 10 min measured according to ASTM D 1238 (2.16 kg, 190° C.); (3) Melt flow ratio I 10 / I2 ranges from 7.0-8.0; and (4) Molecular weight distribution asymmetry [(M w / M n ) / (M z / M w )] ranges from 1.00 to 1.15; (5) Density measured according to ASTM D792 is 0.914 to 0.920 g / cm 3 ;and The linear low density polyethylene composition is composed of linear low density polyethylene, optionally one or more other polymers and optionally one or more additives, wherein the additives are selected from antistatic agents, color enhancers, dyes, lubricants, fillers, pigments, primary antioxidants, secondary antioxidants, UV stabilizers, anti-blocking agents, slip agents, tackifiers, flame retardants, antimicrobial agents, deodorants, antifungal agents and combinations thereof.
2. The film layer according to any one of the preceding claims, wherein the linear low density polyethylene composition comprises units derived from ethylene and units derived from one or more comonomers selected from butene, hexene and octene.
3. The film layer according to any one of the preceding claims, wherein the linear low density polyethylene composition comprises units derived from ethylene and units derived from hexene.
4. The film layer according to any one of the preceding claims, wherein the linear low density polyethylene composition is produced in a single loop solution polymerization reactor.
5. The film layer according to any one of the preceding claims, wherein a film layer having a thickness of 50 microns prepared from a blend of 85 wt% of the linear low density polyethylene composition and 15 wt% of a low density polyethylene has a density of 0.923 g / cm 3 , I2 is 0.75g / 10min, and has one or more of the following properties: (i) a haze of less than 5%; and (ii) Dart impact strength greater than 450 g.
6. An article comprising at least one component prepared from the film layer according to any one of claims 1 to 4.
7. The article of claim 6, wherein the article is a stand-up bag.