Material for automotive trim rubber mat and preparation method thereof
By using specific proportioning and granulation processes of raw materials such as SEBS, white oil, thermoplastic polyester elastomer TPEE in automotive mobile pad materials, the existing materials have been solved by poor tactile comfort, scratch resistance and mechanical properties. The problem is that the excellent elasticity and mechanical properties of the materials are achieved, and the quality and brand image of the whole vehicle are improved.
Patent Information
- Application Number
- CN202310523441.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
AI Technical Summary
The existing automotive mobile phone pad materials have poor tactile comfort, scratch resistance and mechanical properties, which affect the quality of the whole vehicle and the brand image.
Using specific ratios of raw materials such as SEBS, white oil, thermoplastic polyester elastomer TPEE, heavy calcium carbonate, compatibility agent, lubricant, antioxidant and light stabilizer, it is formed through pre-filling oil and blending granulation process. Material for automotive interior glue pads with excellent elasticity and mechanical properties.
It improves the fluidity, machining performance and scratch resistance of the material, extends the service life, and improves the quality and brand image of the whole vehicle.
Smart Images

Figure BDA0004221918960000111 
Figure BDA0004221918960000121 
Figure BDA0004221918960000131
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical industry, and in particular to a material for automobile interior rubber pads and a preparation method thereof. Background Art
[0002] In the related technologies, the popularization of mobile phone wireless charging technology, in order to bring more convenience to people's lives, wireless charging configurations are gradually introduced in cars, and mobile phone pads often use thermoplastic elastomer TPE materials. There are many existing thermoplastic elastomer TPE materials. At present, the most common automotive mobile phone pads are fully dynamically vulcanized thermoplastic elastomer TPV and thermoplastic polystyrene elastomer TPS.
[0003] As an exposed component of car interior that is in direct contact with the mobile phone, the perceived quality and performance of the mobile phone pad are gradually becoming more prominent. However, the shortcomings of TPV or TPS materials such as poor tactile comfort, poor scratch resistance and poor mechanical properties will affect the quality of the entire vehicle and reduce the brand image after long-term use. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one object of the present invention is to provide a material for automotive interior rubber pads to overcome the shortcomings of the prior art rubber pad materials such as poor comfort, poor scratch resistance and poor mechanical properties.
[0005] Another object of the present invention is to provide a method for preparing a material for automobile interior rubber pads.
[0006] According to an embodiment of the first aspect of the present invention, the present invention proposes a material for automotive interior rubber pads, including raw materials and their weight parts as follows: 20-30 parts of SEBS, 10-30 parts of white oil, 10-40 parts of thermoplastic polyester elastomer TPEE, 10-15 parts of polypropylene resin, 5-10 parts of heavy calcium carbonate, 1-5 parts of compatibilizer, 0.1-0.5 parts of lubricant, 0.1-0.5 parts of antioxidant and 0.1-0.5 parts of light stabilizer.
[0007] According to the material for automotive interior rubber pads of a specific embodiment of the present invention, thermoplastic polyester elastomer TPEE, heavy calcium carbonate and various additives are added to SEBS, white oil and polypropylene resin, so that the soft phase component showing elasticity and the hard phase component showing strength cooperate with each other, which, on the one hand, gives the material excellent elasticity and fixed shape, and on the other hand, the material has excellent mechanical properties. Specifically, the specific weight parts of the raw materials cooperate with each other, for example, the addition of heavy calcium carbonate can increase the fluidity and mechanical processing properties of the material.
[0008] According to some embodiments of the present invention, the raw materials and their weight parts are as follows: 20 parts of SEBS, 10 parts of white oil, 30-40 parts of thermoplastic polyester elastomer TPEE, 10 parts of polypropylene resin, 10 parts of calcium carbonate, 5 parts of compatibilizer, 0.2 parts of lubricant, 0.3 parts of antioxidant and 0.5 parts of light stabilizer.
[0009] According to some embodiments of the present invention, the content of styrene chain sulfonate in the SEBS is m in mass percentage, wherein m satisfies: 25wt%≤m≤35wt%.
[0010] According to some embodiments of the present invention, the white oil is paraffin oil; and / or the kinematic viscosity of the white oil at 40° C. is 90 to 100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃.
[0011] According to some embodiments of the present invention, the hardness of the thermoplastic polyester elastomer TPEE is 80-90A, and the melt index is 40-50 g / min at 230° C. and 2.16 kg.
[0012] According to some embodiments of the present invention, the polypropylene is homopolymer polypropylene; and / or the melt index of the polypropylene is 40 to 50 g / min at 230° C. and 2.16 kg.
[0013] According to some embodiments of the present invention, the average particle size of the heavy calcium carbonate is 1000-1200.
[0014] According to some embodiments of the present invention, the compatibilizer is a maleic anhydride grafted polyolefin elastomer; the lubricant is at least one of a silicone masterbatch and erucic acid amide; the light stabilizer is a hindered amine light stabilizer; and / or the antioxidant includes at least one of antioxidant 1010, antioxidant 1076, antioxidant 1790, antioxidant 168, antioxidant DLTP and antioxidant 626; preferably, the antioxidant is a compound of antioxidant 1010 and antioxidant 1076; more preferably, the weight ratio of the antioxidant 1010 to the antioxidant 1076 is 1:1.
[0015] According to another embodiment of the present invention, the present invention provides a method for preparing the material for automotive interior rubber pad according to the embodiment of the first aspect of the present invention, comprising the following steps:
[0016] Step 1: Pre-filling oil, SEBS and white oil are uniformly mixed according to the above weight ratio so that SEBS can fully absorb the white oil, and then placed to obtain pre-filled oil SEBS;
[0017] Step 2: Mixing the raw materials: blending the TPEE elastomer, polypropylene resin, heavy calcium carbonate, compatibilizer, lubricant, antioxidant, light stabilizer and the pre-filled oil SEBS obtained in step 1;
[0018] Step 3: Granulation, putting the raw materials mixed in step 2 into a twin-screw extruder, heating, vacuuming, rotating the screws, extruding and granulating, and obtaining the material for the automotive interior rubber pad.
[0019] According to some embodiments of the present invention, in step one, the placement time is more than 24 hours; and / or in step three, the heating temperature is 190°C to 220°C; and / or the rotation speed of the rotating screw is 80 to 150 rpm; and / or the aspect ratio of the screw is 35 to 55; and / or the vacuum degree of the vacuum is not higher than -0.04Mpa.
[0020] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0021] The embodiments of the present invention are described in detail below.
[0022] The material for automotive interior rubber pads according to the first embodiment of the present invention is described in detail below, including raw materials and their weight parts as follows: 20-30 parts of SEBS, 10-30 parts of white oil, 10-40 parts of thermoplastic polyester elastomer TPEE, 10-15 parts of polypropylene resin, 5-10 parts of heavy calcium carbonate, 1-5 parts of compatibilizer, 0.1-0.5 parts of lubricant, 0.1-0.5 parts of antioxidant and 0.1-0.5 parts of light stabilizer.
[0023] According to the material for automotive interior rubber pads of a specific embodiment of the present invention, thermoplastic polyester elastomer TPEE, heavy calcium carbonate and various additives are added to SEBS, white oil and polypropylene resin, so that the soft phase component showing elasticity and the hard phase component showing strength cooperate with each other, which, on the one hand, gives the material excellent elasticity and fixed shape, and on the other hand, the material has excellent mechanical properties. Specifically, the specific weight parts of the raw materials cooperate with each other, for example, the addition of heavy calcium carbonate can increase the fluidity and mechanical processing properties of the material.
[0024] According to some embodiments of the present invention, the raw materials and their weight parts are as follows: 20 parts of SEBS, 10 parts of white oil, 30-40 parts of thermoplastic polyester elastomer TPEE, 10 parts of polypropylene resin, 10 parts of calcium carbonate, 5 parts of compatibilizer, 0.2 parts of lubricant, 0.3 parts of antioxidant and 0.5 parts of light stabilizer. With such a configuration, the raw material ratio of the material for automotive interior rubber pad is more suitable and the performance is better.
[0025] According to some embodiments of the present invention, the content of styrene chain in SEBS is m in mass percentage, wherein m satisfies: 25%≤m≤35wt%. In this way, if m is less than 25%, the fluidity of the material for automotive interior rubber pads will be affected, and if m is greater than 35%, the elasticity of the material for automotive interior rubber pads will be affected. By setting so that m satisfies 25%≤m≤35wt%, the fluidity and elasticity of the material for automotive interior rubber pads are excellent.
[0026] According to some embodiments of the present invention, the white oil is paraffin oil. In this way, the paraffin oil has a low aromatic content and low volatility, and the low aromatic content can improve the material's anti-oxidative degradation performance, and the low volatility helps prevent the material from aging and shrinking, and is beneficial to improving the poor appearance of the product (such as roughness, bubbles), thereby helping to extend the service life of the rubber product.
[0027] According to some embodiments of the present invention, the kinematic viscosity of the white oil at 40°C is 90-100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃. In this way, during the oil filling process of the material, the kinematic viscosity is appropriate, the flash point is high, and the pour point is low, thus ensuring the safe use of the material.
[0028] According to some embodiments of the present invention, the hardness of the thermoplastic polyester elastomer TPEE is 80-90A, and the melt index is 40-50g / min at 230°C and 2.16kg. In this way, the thermoplastic polyester elastomer TPEE has a high hardness and good meltability, so that when the thermoplastic polyester elastomer TPEE is mixed with SEBS, white oil, etc., it can not only increase the elastic properties of the material, but also optimize the mechanical properties of the material.
[0029] According to some embodiments of the present invention, the polypropylene is homopolymer polypropylene. In this way, the homopolymer polypropylene has high mechanical properties, transparency and processing fluidity, which is beneficial to improving the mechanical properties and processing properties of the material for automotive interior rubber pads.
[0030] According to some embodiments of the present invention, the melt index of polypropylene is 40-50 g / min at 230°C and 2.16 kg. In this way, polypropylene has a suitable kinematic viscosity, a high flash point and a low pour point at the normal working temperature of the material for the vehicle interior rubber pad, thereby ensuring the safe use of the material. In addition, the melt index of polypropylene is equivalent to that of white oil, which is more conducive to the processing and molding of the material.
[0031] According to some embodiments of the present invention, the average particle size of heavy calcium carbonate is 1000-1200. The volume effect, surface effect and quantum size effect of heavy calcium carbonate with an average particle size of 1000-1200 make it have a strong interface bonding force with SEBS / polypropylene thermoplastic elastomer, which has a good reinforcement effect. At the same time, it can also improve the heat resistance and dimensional stability of the thermoplastic elastomer, control the viscosity, thermal expansion coefficient and shrinkage of the thermoplastic elastomer, improve processing and molding, and many other good properties. In this way, the particle size of heavy calcium carbonate is appropriate, which is more conducive to the processing and molding of the material and improves the mechanical properties of the material.
[0032] According to some embodiments of the present invention, the compatibilizer is a maleic anhydride grafted polyolefin elastomer. The addition of the maleic anhydride compatibilizer can well reduce the agglomeration of SEBS, improve the dispersion performance of polypropylene resin and thermoplastic polyester elastomer TPEE, form a more uniformly dispersed phase structure, enhance the interface effect between the rubber and plastic phases, effectively transfer stress to the low modulus rubber, and make full use of the elasticity of the rubber phase. Therefore, it is ensured that the material has high mechanical strength and toughness.
[0033] According to some embodiments of the present invention, the lubricant is at least one of silicone masterbatch and erucic acid amide. In this way, the addition of the lubricant can reduce the friction between the polymer and the processing equipment during the processing, thereby ensuring the reduced fluidity of the polymer melt and the processing performance.
[0034] According to some embodiments of the present invention, the light stabilizer is a hindered amine light stabilizer. Optionally, the hindered amine light stabilizer includes at least one of hindered amine light stabilizer 944, hindered amine light stabilizer 788 and hindered amine light stabilizer 622. But not limited to this. Light, heat and oxygen in the environment are external factors that induce material aging. Ultraviolet light with a wavelength of 290nm to 400nm is the main reason affecting material aging. The wavelength of ultraviolet light sensitivity of the material for automotive interior rubber pads in the specific embodiment of the present invention is 310nm, and its chemical bond energy just corresponds to the energy of this wavelength in ultraviolet light, so the material will absorb the corresponding ultraviolet light, resulting in chemical bond breakage, which further leads to material aging and degradation. The addition of hindered amine light stabilizers can improve the light stability and mechanical property retention rate of polypropylene.
[0035] According to some embodiments of the present invention, the antioxidant includes at least one of antioxidant 1010, antioxidant 1076, antioxidant 1790, antioxidant 168, antioxidant DLTP and antioxidant 626. The thermal oxidation degradation of the high molecular polymer RH is mainly caused by the chain free radical reaction triggered by the free radicals generated by the hydroperoxide ROOH when heated. Therefore, the self-oxidation chain reaction process of RH can be prevented by capturing the generated free radicals and decomposing the generated hydroperoxide ROOH, thereby inhibiting the thermal oxidation degradation of the polymer. Since the phenolic antioxidant has an active hydroxyl group, it is easier for it to provide protons to the peroxide free radicals than the high molecular polymer RH, so that it is converted into a stable peroxide, thereby terminating the free radical reaction and preventing the polymer from further oxidation.
[0036] According to some embodiments of the present invention, the antioxidant is a compound of antioxidant 1010 and antioxidant 1076. Antioxidant 1010 is an auxiliary agent with high thermal stability and is very suitable for use under high temperature conditions, which can extend the service life of the product, and antioxidant 1076 has the characteristics of good antioxidant properties, low volatility, and washing resistance. The combination of the two can provide a more excellent antioxidant effect, achieving the effect of 1+1>2.
[0037] According to some embodiments of the present invention, the weight ratio of the antioxidant 1010 to the antioxidant 1076 is 1: 1. With this configuration, the antioxidant has a better antioxidant effect.
[0038] According to an embodiment of the second aspect of the present invention, the present invention provides a method for preparing a material for an automotive interior rubber pad according to an embodiment of the first aspect of the present invention, comprising the following steps:
[0039] Step 1: pre-filling with oil, uniformly mixing SEBS and white oil according to the above weight ratio so that SEBS can fully absorb the white oil, and leaving it to obtain pre-filled with oil SEBS; in this way, SEBS is plasticized by pre-filling with oil, and the material and performance of SEBS are adjusted, which can overcome the defect of SEBS being difficult to process due to its large relative molecular weight and reduce material costs.
[0040] Step 2: Mixing the raw materials: blending the TPEE elastomer, polypropylene resin, heavy calcium carbonate, compatibilizer, lubricant, antioxidant, light stabilizer and the pre-filled oil SEBS obtained in step 1;
[0041] Step 3: Granulation, put the raw materials mixed in step 2 into a twin-screw extruder, heat, evacuate, rotate the screw, extrude and granulate to obtain the material for automotive interior rubber pads.
[0042] According to the method for preparing the material for automobile interior rubber pads of a specific embodiment of the present invention, the material for automobile interior rubber pads of a specific embodiment of the present invention is prepared through the steps of pre-filling oil, mixing raw materials and granulating, and the material has excellent mechanical properties and elastic properties.
[0043] According to some embodiments of the present invention, the storage time in step 1 is more than 24 hours. Such a setting is conducive to SEBS fully absorbing the white oil to form a uniform premixed oil.
[0044] According to some embodiments of the present invention, in step 3, the heating temperature is 190° C. to 220° C. This arrangement allows the raw materials for the automotive interior rubber pad to be fully melted, which is beneficial to the molding and granulation of the material.
[0045] According to some embodiments of the present invention, the speed of the rotating screw is 80 to 150 rpm. With this arrangement, the speed of the rotating screw is appropriate, which facilitates the sufficient stirring and mixing of the raw materials.
[0046] According to some embodiments of the present invention, the aspect ratio of the screw is 35 to 45. In this way, the aspect ratio of the screw is appropriate, the stirring force is strong, and it is conducive to the full mixing of the raw materials.
[0047] According to some embodiments of the present invention, the vacuum degree of the vacuum is not higher than -0.04Mpa. In this way, the vacuum degree of the system is maintained during the granulation process, and the interference of oxygen in the air on the material during the material preparation process can be avoided, thereby ensuring the performance of the material.
[0048] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.
[0049] The lubricating oil and the preparation method thereof of the present invention are described below by means of specific examples.
[0050] Example 1
[0051] A material for automobile interior rubber pads, comprising raw materials and their weight parts as follows: 20 parts of SEBS (Kateng G1642), 10 parts of white oil (Sinopec Karamay Refining Company 30#), 10 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008), 10 parts of polypropylene resin (Lanzhou Petrochemical H9018), 5 parts of heavy calcium carbonate, 1 part of compatibilizer, 0.1 part of lubricant, 0.1 part of antioxidant and 0.1 part of light stabilizer;
[0052] The content of styrene chain in SEBS is expressed as m in mass percentage, wherein m satisfies: m = 25wt%;
[0053] White oil is paraffin oil;
[0054] The kinematic viscosity of white oil at 40°C is 90-100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃;
[0055] The hardness of thermoplastic polyester elastomer TPEE is 80-90A, and the melt index is 40-50g / min at 230℃ and 2.16kg.
[0056] The polypropylene is homopolymer polypropylene;
[0057] The melt index of polypropylene is 40-50 g / min at 230°C and 2.16 kg;
[0058] The average particle size of heavy calcium carbonate is 1000;
[0059] The compatibilizer is maleic anhydride grafted polyolefin elastomer;
[0060] The lubricant is silicone masterbatch;
[0061] The light stabilizer is hindered amine light stabilizer 944;
[0062] The antioxidant is a compound of antioxidant 1010 and antioxidant 1076; the weight ratio of antioxidant 1010 to antioxidant 1076 is 1:3.
[0063] The preparation method thereof comprises the following steps:
[0064] Step 1: Pre-filling oil, SEBS and white oil are uniformly mixed according to the above weight ratio so that SEBS can fully absorb the white oil, and then placed to obtain pre-filled oil SEBS;
[0065] Step 2: Mixing the raw materials: blending the TPEE elastomer, polypropylene resin, heavy calcium carbonate, compatibilizer, lubricant, antioxidant, light stabilizer and the pre-filled oil SEBS obtained in step 1;
[0066] Step 3: Granulation, putting the mixed raw materials in step 2 into a twin-screw extruder, heating, vacuuming, rotating the screws, extruding and granulating, and obtaining the material for automotive interior rubber pads;
[0067] In step 1, the storage time is more than 24 hours;
[0068] In step 3, the heating temperature is 205°C;
[0069] The speed of the rotating screw was 120 rpm;
[0070] The aspect ratio of the screw is 45;
[0071] The vacuum degree of the vacuum is not higher than -0.04Mpa.
[0072] Example 2
[0073] A material for automobile interior rubber pads includes raw materials and their weight parts are as follows: 30 parts of SEBS (Kraton A1536), 30 parts of white oil (30# from Sinopec Karamay Refinery), 40 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008), 15 parts of polypropylene resin (Lanzhou Petrochemical H9018), 10 parts of heavy calcium carbonate, 5 parts of compatibilizer, 0.5 parts of lubricant, 0.5 parts of antioxidant and 0.5 parts of light stabilizer.
[0074] The content of styrene chain in SEBS is expressed as m in mass percentage, wherein m satisfies: m=35wt%;
[0075] White oil is paraffin oil;
[0076] The kinematic viscosity of white oil at 40°C is 90-100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃;
[0077] The hardness of thermoplastic polyester elastomer TPEE is 80-90A, and the melt index is 40-50g / min at 230℃ and 2.16kg.
[0078] The polypropylene is homopolymer polypropylene;
[0079] The melt index of polypropylene is 40-50 g / min at 230°C and 2.16 kg;
[0080] The average particle size of heavy calcium carbonate is 1200;
[0081] The compatibilizer is maleic anhydride grafted polyolefin elastomer;
[0082] The lubricant is erucamide;
[0083] The light stabilizer is hindered amine light stabilizer 788;
[0084] The antioxidant is a compound of antioxidant 1010 and antioxidant 1076; the weight ratio of antioxidant 1010 to antioxidant 1076 is 3:1.
[0085] The preparation method is basically the same as that in Example 1.
[0086] Example 3
[0087] A material for automobile interior rubber pads, characterized in that it includes raw materials and their weight parts are as follows: 25 parts of SEBS (Kateng G1654), 20 parts of white oil (Sinopec Karamay Refinery Company 30#), 25 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008), 13 parts of polypropylene resin (Lanzhou Petrochemical H9018), 7 parts of heavy calcium carbonate, 3 parts of compatibilizer, 0.3 parts of lubricant, 0.3 parts of antioxidant and 0.3 parts of light stabilizer.
[0088] The content of styrene chain in SEBS is expressed as m in mass percentage, wherein m satisfies: m=30wt%.
[0089] White oil is paraffin oil;
[0090] The kinematic viscosity of white oil at 40°C is 90-100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃;
[0091] The hardness of thermoplastic polyester elastomer TPEE is 80-90A, and the melt index is 40-50g / min at 230℃ and 2.16kg.
[0092] The polypropylene is homopolymer polypropylene;
[0093] The melt index of polypropylene is 40-50 g / min at 230°C and 2.16 kg;
[0094] The average particle size of heavy calcium carbonate is 1100;
[0095] The compatibilizer is maleic anhydride grafted polyolefin elastomer;
[0096] The lubricant is a mixture of silicone masterbatch and erucic acid amide in equal weight ratio;
[0097] The light stabilizer is hindered amine light stabilizer 622;
[0098] The antioxidant is a compound of antioxidant 1010 and antioxidant 1076; the weight ratio of antioxidant 1010 to antioxidant 1076 is 1:1.
[0099] The preparation method is basically the same as that in Example 1.
[0100] Example 4
[0101] A material for automobile interior rubber pads includes raw materials and their weight parts are as follows: 20 parts of SEBS (Kateng G1654), 10 parts of white oil (30# from Sinopec Karamay Refinery), 30 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008), 10 parts of polypropylene resin (Lanzhou Petrochemical H9018), 10 parts of heavy calcium carbonate, 5 parts of compatibilizer, 0.2 parts of lubricant, 0.3 parts of antioxidant and 0.5 parts of light stabilizer.
[0102] The content of styrene chain in SEBS is expressed as m in mass percentage, wherein m satisfies: m=30wt%.
[0103] White oil is paraffin oil;
[0104] The kinematic viscosity of white oil at 40°C is 90-100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃;
[0105] The hardness of thermoplastic polyester elastomer TPEE is 80-90A, and the melt index is 40-50g / min at 230℃ and 2.16kg.
[0106] The polypropylene is homopolymer polypropylene;
[0107] The melt index of polypropylene is 40-50 g / min at 230°C and 2.16 kg;
[0108] The average particle size of heavy calcium carbonate is 1100;
[0109] The compatibilizer is maleic anhydride grafted polyolefin elastomer;
[0110] The lubricant is a mixture of silicone masterbatch and erucic acid amide in equal weight ratio;
[0111] The light stabilizer is a mixture of hindered amine light stabilizer 944, hindered amine light stabilizer 788 and hindered amine light stabilizer 622 in equal weight ratios;
[0112] The antioxidant is a compound of antioxidant 1010 and antioxidant 1076; the weight ratio of antioxidant 1010 to antioxidant 1076 is 1:1.
[0113] The preparation method is basically the same as that in Example 1.
[0114] Example 5
[0115] Example 5 is substantially the same as Example 4, except that 40 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008) are used.
[0116] Example 6
[0117] Example 6 is substantially the same as Example 4, except that:
[0118] A material for automobile interior rubber pads, characterized in that it includes raw materials and their weight parts are as follows: 30 parts of SEBS (Kraton G1654), 30 parts of white oil (Sinopec Karamay Refining Company 30#), 10 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008), 15 parts of polypropylene resin, 10 parts of heavy calcium carbonate, 5 parts of compatibilizer, 0.2 parts of lubricant, 0.3 parts of antioxidant and 0.5 parts of light stabilizer.
[0119] Example 7
[0120] Example 7 is substantially the same as Example 4, except that:
[0121] A material for automobile interior rubber pads, characterized in that it includes raw materials and their weight parts are as follows: 25 parts of SEBS (Kraton G1654), 20 parts of white oil (Sinopec Karamay Refinery Company 30#), 20 parts of thermoplastic polyester elastomer TPEE (DSM Arnitel EL25008), 12 parts of polypropylene resin, 10 parts of heavy calcium carbonate, 5 parts of compatibilizer, 0.2 parts of lubricant, 0.3 parts of antioxidant and 0.5 parts of light stabilizer.
[0122] Example 8
[0123] Example 8 is substantially the same as Example 4, except that the polypropylene is copolymerized polypropylene (Total BL9600).
[0124] Example 9
[0125] Example 9 is substantially the same as Example 4, except that the content of styrene chain styrene in SEBS (Kraton A1536) is m in mass percentage, wherein m satisfies: m=15wt%.
[0126] Example 10
[0127] Example 10 is substantially the same as Example 4, except that the content of styrene chain sulfonate in SEBS (Asahi Kasei H1050) is m in mass percentage, wherein m satisfies: m=45wt%.
[0128] Embodiment 11
[0129] Example 11 is substantially the same as Example 4, except that the compatibilizer is an imide-modified acrylic resin.
[0130] Example 12
[0131] Example 12 is substantially the same as Example 4, except that the lubricant is silicate.
[0132] Embodiment 13
[0133] Example 13 is substantially the same as Example 4, except that the antioxidant is antioxidant 1010.
[0134] Embodiment 14
[0135] Example 14 is substantially the same as Example 4, except that the light stabilizer is a benzophenone light stabilizer.
[0136] Embodiment 15
[0137] Example 15 is substantially the same as Example 4, except that the antioxidant is antioxidant DLTP.
[0138] Example 16
[0139] Example 16 is basically the same as Example 4, except that the preparation method is different. In step three, the heating temperature is 190° C. and the screw rotation speed is 80 rpm.
[0140] Embodiment 17
[0141] Example 17 is basically the same as Example 4, except that the preparation method is different. In step three, the heating temperature is 220° C. and the speed of the rotating screw is 150 rpm.
[0142] Embodiment 18
[0143] Example 18 is basically the same as Example 4, except that in step three, the heating temperature is 200° C. and the speed of the rotating screw is 130 rpm.
[0144] Comparative Example 1
[0145] Comparative Example 1 is substantially the same as Example 4, except that the heavy calcium carbonate is replaced by an equal weight of light calcium carbonate.
[0146] Comparative Example 2
[0147] Comparative Example 2 is substantially the same as Example 4, except that the thermoplastic polyester elastomer TPEE is deleted.
[0148] Comparative Example 3
[0149] Comparative Example 3 is substantially the same as Example 4, except that an equal weight portion of polyurethane elastomer is used to replace the thermoplastic polyester elastomer TPEE.
[0150] Comparative Example 4
[0151] Comparative Example 4 is substantially the same as Example 4, except that the weight portion of the thermoplastic polyester elastomer TPEE is 60 parts.
[0152] Comparative Example 5
[0153] Comparative Example 5 is substantially the same as Example 4, except that the weight portion of the thermoplastic polyester elastomer TPEE is 5 parts.
[0154] The raw materials of the automotive interior rubber pad materials of Examples 1-18 of the present invention and Comparative Examples 1-5 are shown in Table 1 below.
[0155] Table 1.
[0156]
[0157]
[0158]
[0159] The raw material dosages of the materials for the automotive interior rubber pads of Examples 1 to 18 of the present invention and Comparative Examples 1 to 5 are shown in Table 2 below.
[0160] Table 2.
[0161]
[0162] Performance Testing
[0163] The materials for automotive interior rubber pads obtained in Examples 1 to 18 and Comparative Examples 1 to 5 were injection molded into 2 mm test pieces according to the standard for mechanical properties and scratch resistance tests, wherein the test methods are as follows: the hardness test is carried out in accordance with GB / T531.1-2019, the tensile strength and elongation at break are tested in accordance with GB / T 528-2009, the hot air aging test is carried out in accordance with GB / T 3512-2014, the xenon lamp aging test is carried out in accordance with GB / T32088-2015, the gray card grade test is carried out in accordance with GB / T 250-2008, and the friction coefficient test method is carried out in accordance with GB 10006-88.
[0164] The scratch resistance test is carried out according to the internal standard experimental method of Great Wall. The test method is as follows: at room temperature, a scratch head with a diameter of 1mm is used to scratch the material surface once at a speed of 1000mm / min under a load of 5N. After the test, a colorimeter is used to evaluate the color difference change at the scratch point, and the degree of color difference change is used to characterize the scratch resistance of the material. The smaller the color difference value, the better the scratch resistance of the material, and vice versa.
[0165] The correlation between the performance parameters of the above tests and the materials for automotive interior rubber pads of the specific embodiments and comparative examples of the present invention is as follows:
[0166] Hardness (HA): The hardness (HA) of the material for the automotive interior rubber pad of the specific embodiment of the present invention will directly affect the comfort of the material's touch. When the hardness of the material is low, the touch comfort is good; if the hardness of the material is too high, the touch comfort is poor. However, if the hardness of the material is too low, it will affect the surface scratch resistance.
[0167] Tensile strength: The tensile strength of a material can reflect the mechanical properties of the material. Low tensile strength means poor tear resistance.
[0168] Elongation at break (%): The elongation at break of a material is a parameter that measures the elongation of the material.
[0169] Hot air aging: The ability of aging test to obtain results similar to those of natural aging or aging in the use environment. These aging refers to the changes in materials during the thermal aging process. These changes may be mechanical or appearance changes, or chemical changes.
[0170] Xenon lamp aging: Xenon lamp aging is to test the material's ability to maintain appearance and performance after UV resistance. After xenon lamp aging, a gray card is used to determine the degree of discoloration of the product.
[0171] Dynamic friction coefficient: The dynamic friction coefficient of the material directly affects the touch comfort. The lower the dynamic friction coefficient, the better the touch comfort of the material. However, the mobile phone pad in the car must also have friction to prevent the phone from sliding. The best performance is when it is greater than or equal to 0.3.
[0172] Scratch resistance: Use a colorimeter to evaluate the color difference change at the scratch, and use the degree of color difference change to characterize the scratch resistance of the material. The smaller the color difference value, the better the scratch resistance of the material. Conversely, the worse the scratch resistance of the material.
[0173] The lubricating oil performance test of Example 1 to Example 18 and Comparative Example 1 to Comparative Example 5 is shown in Table 3 below:
[0174] Table 3.
[0175]
[0176]
[0177] From Example 1 to Example 18 and Comparative Example 1 to Comparative Example 5, combined with the test results of Table 3, it can be seen that the introduction of polyester elastomer TPEE will significantly improve the tactile comfort and over-rubbing resistance of the material for automotive interior rubber pads, but when the addition ratio is too high or too low, it will affect the hardness and anti-aging properties of the material. The introduction of compatibilizers, lubricants, antioxidants and photo-oxidants can improve the mechanical properties of the material. Among them, the introduction of antioxidants can significantly improve the anti-aging properties of the material, and the compound use effect is the best. In addition, SEBS and white oil are compounded in the material for automotive interior rubber pads of the present invention. If the amount of white oil added is too much, it exceeds the oil absorption capacity of SEBS, which is easy to cause oil precipitation. If the amount of white oil added is too little, the plasticizing property of SEBS will be weak. Further, if the amount of SEBS and white oil added accounts for too high a proportion of the total amount of all raw materials, it is also easy to cause oil precipitation. Comparing Example 4 and Comparative Example 1, it can be seen that in the present invention, if light calcium carbonate is used instead of heavy calcium carbonate, the material will have white matter precipitation. Since light calcium carbonate has a large specific surface area, a high oil absorption value, and a light weight, it is difficult to dissolve and mix with the raw materials such as SEBS, white oil, and polypropylene resin of the present invention after adding it. Therefore, during the preparation process, the raw materials are easy to agglomerate, resulting in the precipitation of white matter in the material.
[0178] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0179] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A material for automobile interior rubber pads, characterized in that: The raw materials and their weight parts are as follows: 20-30 parts of SEBS, 10-30 parts of white oil, 10-40 parts of thermoplastic polyester elastomer TPEE, 10-15 parts of polypropylene resin, 5-10 parts of heavy calcium carbonate, 1-5 parts of compatibilizer, 0.1-0.5 parts of lubricant, 0.1-0.5 parts of antioxidant and 0.1-0.5 parts of light stabilizer.
2. The material for automotive interior rubber pad according to claim 1, characterized in that: The raw materials and their weight parts are as follows: 20 parts of SEBS, 10 parts of white oil, 30-40 parts of thermoplastic polyester elastomer TPEE, 10 parts of polypropylene resin, 10 parts of calcium carbonate, 5 parts of compatibilizer, 0.2 parts of lubricant, 0.3 parts of antioxidant and 0.5 parts of light stabilizer.
3. The material for automotive interior rubber pad according to claim 1 or 2, characterized in that: The content of styrene chain in the SEBS is m in mass percentage, wherein m satisfies: 25wt%≤m≤35wt%.
4. The material for automotive interior rubber pad according to claim 1 or 2, characterized in that: The white oil is paraffin oil; and / or The kinematic viscosity of the white oil at 40°C is 90-100 mm 2 / s, flash point ≥200℃, pour point ≤-15℃.
5. The material for automotive interior rubber pad according to claim 1 or 2, characterized in that: The thermoplastic polyester elastomer TPEE has a hardness of 80-90A and a melt index of 40-50 g / min under the conditions of 230° C. and 2.16 kg.
6. The material for automotive interior rubber pad according to claim 1 or 2, characterized in that: The polypropylene is homopolypropylene; and / or The melt index of the polypropylene is 40-50 g / min at 230° C. and 2.16 kg.
7. The automotive interior rubber pad material according to claim 1 or 2, characterized in that: The average particle size of the heavy calcium carbonate is 1000-1200.
8. The material for automotive interior rubber pad according to claim 1 or 2, characterized in that: The compatibilizer is maleic anhydride grafted polyolefin elastomer; and / or The lubricant is at least one of silicone masterbatch and erucamide; and / or The light stabilizer is a hindered amine light stabilizer; and / or The antioxidant includes at least one of antioxidant 1010, antioxidant 1076, antioxidant 1790, antioxidant 168, antioxidant DLTP and antioxidant 626; preferably, the antioxidant is a compound of antioxidant 1010 and antioxidant 1076; more preferably, the weight ratio of the antioxidant 1010 to the antioxidant 1076 is 1:
1.
9. A method for preparing the material for automobile interior rubber pad according to any one of claims 1 to 8, characterized in that: The steps include: Step 1: Pre-filling oil, SEBS and white oil are uniformly mixed according to the above weight ratio so that SEBS can fully absorb the white oil, and then placed to obtain pre-filled oil SEBS; Step 2: Mixing the raw materials: blending the TPEE elastomer, polypropylene resin, heavy calcium carbonate, compatibilizer, lubricant, antioxidant, light stabilizer and the pre-filled oil SEBS obtained in step 1; Step 3: Granulation, putting the raw materials mixed in step 2 into a twin-screw extruder, heating, vacuuming, rotating the screws, extruding and granulating, and obtaining the material for the automotive interior rubber pad.
10. The method for preparing lubricating oil according to claim 9, characterized in that: In step 1, the placement time is more than 24 hours; and / or In step 3, the heating temperature is 190° C. to 220° C.; and / or The rotating speed of the rotating screw is 80 to 150 rpm; and / or The aspect ratio of the screw is 35 to 55; and / or The vacuum degree of the vacuum is not higher than -0.04Mpa.