Polyester-based composite material
By using hybrid filling strategy of molybdenum disulfide and hydroxyl and amino-modified boron nitride in polyester-based composite materials, the problem of water vapor barrier properties deviation after boron nitride modification is solved, and the thermal conductivity of the material is improved and tensile strength, an efficient thermal conductivity and barrier structure is constructed.
Patent Information
- Application Number
- CN202411222306.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
Hydroxy-modified boron nitride leads to a deviation in water vapor barrier properties in polyester-based composite materials, and increases the difficulty of material processing and melt viscosity, affecting the thermal conductivity and construction of barrier structures.
Molybdenum disulfide, hydroxyl and amino modified boron nitride are used as hybrid fillers for polyester. Through the mixing and melt extrusion process, the melt viscosity is reduced and the dispersion of boron nitride is promoted to build an efficient thermal conductivity and barrier structure.
The thermal conductivity, tensile strength and water vapor barrier properties of the polyester-based composite materials are improved, and high-thermal conductivity and high-barrier packaging materials with excellent performance are prepared.
Smart Images

Figure BDA0005023382130000061
Abstract
Description
Technical Field
[0001] The invention relates to a polyester-based composite material, belonging to the technical field of packaging materials. Background Art
[0002] Packaging materials with both thermal conductivity and barrier properties have a wide range of uses in the electronic and electrical fields. They can not only achieve thermal management of electronic products and prevent overheating damage, but also block the entry of external moisture and oxygen, ensuring the durability and operational stability of electronic products. Polyester is a polymer material with excellent comprehensive performance and low cost, and is widely used in the packaging field. Similar to other polymer materials, the bulk thermal conductivity of polyester is low and the barrier performance is difficult to meet the use requirements, so it needs to be modified. Adding thermally conductive fillers to polyester is the simplest and most effective way to improve its thermal conductivity. In order to take into account the requirements of electronic and electrical insulation, insulating thermally conductive fillers are usually added to polyester. The bulk thermal conductivity of boron nitride can reach more than 260W / mK, which is the most significant insulating thermally conductive filler for enhancement. At the same time, the larger the aspect ratio of boron nitride itself (the ratio of plane size to thickness), the easier it is to form a thermal conductive path in the polymer, thereby having a better thermal conductivity enhancement effect (Composites Science and Technology, 2022, 222, 109346). However, boron nitride also has its own disadvantages, namely, its surface inertness is relatively high and its compatibility with the polymer matrix is relatively poor, resulting in its poor dispersibility in the polymer and weak interfacial interaction, making the mechanical properties and barrier properties of the polymer-based composite materials prepared therefrom relatively poor.
[0003] Surface modification of boron nitride is an effective method to improve its compatibility with polymers and the mechanical properties and thermal conductivity of composite materials (Composites Communications, 2023, 42, 101696). Among them, hydroxyl modification of boron nitride is one of the more mature and effective methods. However, when filling hydroxyl-modified boron nitride, the viscosity of the polymer melt will increase, which will increase the difficulty of material processing and molding. In addition, the high viscosity melt is not conducive to the construction of an efficient barrier structure during processing, resulting in deviations in the water vapor barrier performance of polymer composites. Summary of the invention
[0004] The object of the present invention is to provide a polyester-based composite material, which can solve the problem of deviation in water vapor barrier performance of the polyester-based composite material currently prepared by using hydroxyl-modified boron nitride.
[0005] In order to achieve the above objectives, the technical solution adopted by the polyester-based composite material of the present invention is:
[0006] A polyester-based composite material is composed of the following components in parts by mass: 40-60 parts of polyester, 20-30 parts of functional group-modified flaky boron nitride, and 20-30 parts of molybdenum disulfide; the functional groups are hydroxyl and amino groups; the flaky boron nitride modified with functional groups has a sheet diameter of 0.1-0.4 μm, a thickness of 30-100 nm, and a functional group content of 5%-15%; the particle size of molybdenum disulfide is 200-300 nm; and the polyester is polyethylene terephthalate or polybutylene terephthalate.
[0007] The polyester-based composite material of the present invention adopts molybdenum disulfide and hydroxyl- and amino-modified boron nitride as hybrid fillers of polyester, and the two can play a synergistic role to improve the thermal conductivity, tensile strength and water vapor barrier performance of the polyester-based composite material.
[0008] Preferably, the weight average molecular weight of the polyester is 30,000-50,000.
[0009] Preferably, the polyester-based composite material is prepared by a method comprising the following steps: mixing the formulated amount of polyester, molybdenum disulfide and functional group-modified flake boron nitride and then melt-extruding to obtain the polyester-based composite material. The preparation method of the polyester-based composite material of the present invention uses molybdenum disulfide and hydroxyl- and amino-modified boron nitride as hybrid fillers of polyester. After hybrid filling, molybdenum disulfide can reduce the viscosity of the melt, further promote the dispersion of hydroxyl- and amino-modified boron nitride and its orientation during the molding process, thereby constructing an efficient thermal conductive and barrier structure, and then preparing a polyester-based composite material for high thermal conductivity and high barrier packaging with excellent performance.
[0010] Preferably, the temperature of melt extrusion is 240-270°C.
[0011] Preferably, the mixing method is as follows: after mixing the polyester and molybdenum disulfide in the formulated amount, a mixed base material is obtained, and then the mixed base material and the flake boron nitride modified with the functional group are mixed.
[0012] Preferably, the mixing of the polyester and molybdenum disulfide is carried out using a kneader.
[0013] Preferably, the temperature for mixing the polyester and molybdenum disulfide is 70 to 90° C. and the time is 10 to 30 minutes.
[0014] Preferably, a kneader is used to mix the mixed base material and the functional group-modified flake boron nitride.
[0015] Preferably, mixing the mixed base material and the functional group-modified flake boron nitride includes a first mixing stage and a second mixing stage performed sequentially, the temperature used in the first mixing stage is 70-90°C and the time is 10-30 minutes, and the temperature used in the second mixing stage is 150-160°C and the time is 2-5 hours.
[0016] Preferably, the method for preparing the polyester-based composite material further comprises the following steps: uniformly mixing the formulated amounts of polyester, molybdenum disulfide and functional group-modified flaky boron nitride, cooling to room temperature, and then crushing to obtain a crushed material, and then melt-extruding the crushed material.
[0017] In order to obtain a polyester-based composite material of a specific shape, the material after melt extrusion can be injection molded at a temperature of 250 to 280°C. DETAILED DESCRIPTION
[0018] The polyester-based composite material of the present invention is a pioneering invention. The polyester-based composite material of the present invention is composed of the following components in parts by mass: 40 to 60 parts of polyester, 20 to 30 parts of functional group-modified flake boron nitride, and 20 to 30 parts of molybdenum disulfide; the functional groups are hydroxyl and amino groups. The present invention adopts a hybrid filling strategy of molybdenum disulfide and hydroxyl and amino-modified boron nitride. Molybdenum disulfide and hydroxyl and amino-modified boron nitride can play a synergistic role to improve the thermal conductivity, tensile strength and water vapor barrier properties of the polyester-based composite material; wherein, molybdenum disulfide is a new type of two-dimensional filler, which itself has good self-lubricity and barrier properties. Therefore, after hybrid filling, molybdenum disulfide can reduce the viscosity of the melt, further promote the dispersion of hydroxyl and amino-modified boron nitride and its orientation during the molding process, thereby constructing an efficient thermal conductive and barrier structure, and then preparing a polyester-based composite material for high thermal conductivity and high barrier packaging with excellent performance.
[0019] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0020] Example 1
[0021] The polyester-based composite material of this embodiment is composed of the following components in parts by mass: 60 parts of polyester, 20 parts of hydroxyl-modified flaky boron nitride, and 20 parts of molybdenum disulfide; the polyester is polybutylene terephthalate (PBT), produced by Changchun Chemical Jiangsu Co., Ltd., and has a weight-average molecular weight of 30,000 to 50,000; the manufacturer of molybdenum disulfide is Shanghai Yingfeng Ruihuang Metal Materials Co., Ltd., and has a particle size of 200 to 300 nm; the manufacturer of hydroxyl-modified flaky boron nitride is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a sheet diameter of 0.1 to 0.4 μm, a thickness of 30 to 100 nm, and a hydroxyl content of 5% to 15% (obtained by thermogravimetric measurement).
[0022] The preparation method of the polyester-based composite material of this embodiment specifically includes the following steps: first, start a kneading machine, add PBT particles thereto and heat it to 50°C, when the temperature reaches 50°C and stabilizes, add molybdenum disulfide to the kneading machine, and at the same time raise the temperature of the kneading machine to 70°C, stir at a constant temperature for 10 minutes, add hydroxyl-modified flake boron nitride, and continue stirring for 30 minutes, then close the kneading machine, introduce circulating nitrogen, gradually heat up to 150°C, continue stirring for 4 hours, crush and discharge the material to obtain a crushed material; dry the crushed material in a vacuum oven at 80°C for 12 hours, then melt-extrude it at 240°C, and injection mold it at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0023] Example 2
[0024] The polyester-based composite material of this embodiment is composed of the following components in parts by mass: 60 parts of polyester, 30 parts of hydroxyl-modified flaky boron nitride, and 20 parts of molybdenum disulfide; the polyester is polybutylene terephthalate (PBT), produced by Changchun Chemical Jiangsu Co., Ltd., and has a weight-average molecular weight of 30,000 to 50,000; the manufacturer of molybdenum disulfide is Shanghai Yingfeng Ruihuang Metal Materials Co., Ltd., and has a particle size of 200 to 300 nm; the manufacturer of hydroxyl-modified flaky boron nitride is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a sheet diameter of 0.1 to 0.4 μm, a thickness of 30 to 100 nm, and a hydroxyl content of 5% to 15% (obtained by thermogravimetric measurement).
[0025] The preparation method of the polyester-based composite material of this embodiment specifically includes the following steps: first, start a kneading machine, add PBT particles thereto and heat it to 50°C, when the temperature reaches 50°C and stabilizes, add molybdenum disulfide to the kneading machine, and at the same time raise the temperature of the kneading machine to 70°C, stir at a constant temperature for 10 minutes, add hydroxyl-modified flake boron nitride, and continue stirring for 30 minutes, then close the kneading machine, introduce circulating nitrogen, gradually heat up to 150°C, continue stirring for 4 hours, crush and discharge the material to obtain a crushed material; dry the crushed material in a vacuum oven at 80°C for 12 hours, then melt-extrude it at 240°C, and injection mold it at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0026] Example 3
[0027] The polyester-based composite material of this embodiment is composed of the following components in parts by mass: 60 parts of polyester, 30 parts of hydroxyl-modified flaky boron nitride, and 30 parts of molybdenum disulfide; the polyester is polybutylene terephthalate (PBT), produced by Changchun Chemical Jiangsu Co., Ltd., and has a weight-average molecular weight of 30,000 to 50,000; the manufacturer of molybdenum disulfide is Shanghai Yingfeng Ruihuang Metal Materials Co., Ltd., and has a particle size of 200 to 300 nm; the manufacturer of hydroxyl-modified flaky boron nitride is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a sheet diameter of 0.1 to 0.4 μm, a thickness of 30 to 100 nm, and a hydroxyl content of 5% to 15% (obtained by thermogravimetric measurement).
[0028] The preparation method of the polyester-based composite material of this embodiment specifically includes the following steps: first, start a kneading machine, add PBT particles thereto and heat it to 50°C, when the temperature reaches 50°C and stabilizes, add molybdenum disulfide to the kneading machine, and at the same time raise the temperature of the kneading machine to 70°C, stir at a constant temperature for 10 minutes, add hydroxyl-modified flake boron nitride, and continue stirring for 30 minutes, then close the kneading machine, introduce circulating nitrogen, gradually heat up to 150°C, continue stirring for 4 hours, crush and discharge the material to obtain a crushed material; dry the crushed material in a vacuum oven at 80°C for 12 hours, then melt-extrude it at 240°C, and injection mold it at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0029] Example 4
[0030] The polyester-based composite material of this embodiment is composed of the following components in parts by mass: 60 parts of polyester, 20 parts of hydroxyl-modified flaky boron nitride, and 30 parts of molybdenum disulfide; the polyester is polybutylene terephthalate (PBT), produced by Changchun Chemical Jiangsu Co., Ltd., and has a weight-average molecular weight of 30,000 to 50,000; the manufacturer of molybdenum disulfide is Shanghai Yingfeng Ruihuang Metal Materials Co., Ltd., and has a particle size of 200 to 300 nm; the manufacturer of hydroxyl-modified flaky boron nitride is Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a sheet diameter of 0.1 to 0.4 μm, a thickness of 30 to 100 nm, and a hydroxyl content of 5% to 15% (obtained by thermogravimetric measurement).
[0031] The preparation method of the polyester-based composite material of this embodiment specifically includes the following steps: first, start a kneading machine, add PBT particles thereto and heat it to 50°C, when the temperature reaches 50°C and stabilizes, add molybdenum disulfide to the kneading machine, and at the same time raise the temperature of the kneading machine to 70°C, stir at a constant temperature for 10 minutes, add hydroxyl-modified flake boron nitride, and continue stirring for 30 minutes, then close the kneading machine, introduce circulating nitrogen, gradually heat up to 150°C, continue stirring for 4 hours, crush and discharge the material to obtain a crushed material; dry the crushed material in a vacuum oven at 80°C for 12 hours, then melt-extrude it at 240°C, and injection mold it at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0032] Comparative Example 1
[0033] The polyester-based composite material of this comparative example is composed of the following components in parts by mass: 60 parts of polyester and 40 parts of molybdenum disulfide; the polyester is the same as the polyester used in Example 1, and the molybdenum disulfide is the same as the molybdenum disulfide used in Example 1.
[0034] The preparation method of the polyester-based composite material of the present comparative example specifically comprises the following steps: firstly, a kneading machine is opened, PBT particles are added thereto and the temperature is raised to 50°C; when the temperature reaches 50°C and stabilizes, molybdenum disulfide is added to the kneading machine, and the temperature of the kneading machine is raised to 70°C, and the mixture is stirred at a constant temperature for 40 minutes; then, the kneading machine is sealed, circulating nitrogen is introduced, the temperature is gradually raised to 150°C, stirring is continued for 4 hours, and the material is crushed to obtain a crushed material; the crushed material is dried in a vacuum oven at 80°C for 12 hours, and then melt-extruded at 240°C, and injection molded at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0035] Comparative Example 2
[0036] The polyester-based composite material of this comparative example is composed of the following components in parts by mass: 60 parts of polyester and 60 parts of molybdenum disulfide; the polyester is the same as the polyester used in Example 3, and the molybdenum disulfide is the same as the molybdenum disulfide used in Example 3.
[0037] The preparation method of the polyester-based composite material of the present comparative example specifically comprises the following steps: firstly, a kneading machine is opened, PBT particles are added thereto and the temperature is raised to 50°C; when the temperature reaches 50°C and stabilizes, molybdenum disulfide is added to the kneading machine, and the temperature of the kneading machine is raised to 70°C, and the mixture is stirred at a constant temperature for 40 minutes; then, the kneading machine is sealed, circulating nitrogen is introduced, the temperature is gradually raised to 150°C, stirring is continued for 4 hours, and the material is crushed to obtain a crushed material; the crushed material is dried in a vacuum oven at 80°C for 12 hours, and then melt-extruded at 240°C, and injection molded at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0038] Comparative Example 3
[0039] The polyester-based composite material of this comparative example is composed of the following components in parts by mass: 60 parts of polyester and 40 parts of hydroxyl-modified flaky boron nitride; the polyester is the same as the polyester used in Example 1, and the molybdenum disulfide is the same as the molybdenum disulfide used in Example 1.
[0040] The preparation method of the polyester-based composite material of this embodiment specifically includes the following steps: first, start the kneading machine, add PBT particles thereto and heat it to 50°C, when the temperature reaches 50°C and stabilizes, raise the temperature of the kneading machine to 70°C, stir at a constant temperature for 10 minutes, add hydroxyl-modified flake boron nitride, and continue stirring for 30 minutes, then close the kneading machine, introduce circulating nitrogen, gradually heat up to 150°C, continue stirring for 4 hours, crush and discharge the material to obtain a crushed material; dry the crushed material in a vacuum oven at 80°C for 12 hours, then melt-extrude it at 240°C, and injection mold it at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0041] Comparative Example 4
[0042] The polyester-based composite material of this comparative example is composed of the following components in parts by mass: 60 parts of polyester and 60 parts of hydroxyl-modified flaky boron nitride; the polyester is the same as the polyester used in Example 3, and the molybdenum disulfide is the same as the molybdenum disulfide used in Example 3.
[0043] The preparation method of the polyester-based composite material of this embodiment specifically includes the following steps: first, start the kneading machine, add PBT particles thereto and heat it to 50°C, when the temperature reaches 50°C and stabilizes, raise the temperature of the kneading machine to 70°C, stir at a constant temperature for 10 minutes, add hydroxyl-modified flake boron nitride, and continue stirring for 30 minutes, then close the kneading machine, introduce circulating nitrogen, gradually heat up to 150°C, continue stirring for 4 hours, crush and discharge the material to obtain a crushed material; dry the crushed material in a vacuum oven at 80°C for 12 hours, then melt-extrude it at 240°C, and injection mold it at 250°C to prepare dumbbell-shaped and round polyester-based composite material samples for subsequent mechanical, thermal conductivity and barrier property tests.
[0044] Experimental example
[0045] In order to investigate the use effect of the polyester-based composite materials of each embodiment and comparative example as electronic packaging materials, the polyester-based composite materials of each embodiment and comparative example and pure PBT resin were tested for thermal conductivity, tensile strength and water vapor barrier performance (water vapor transmission rate), and the results are shown in Table 1. The test standard for thermal conductivity is ISO 22007-4, the test standard for tensile strength is GB / T 1040.2-2006, and the thickness of the sample used in the water vapor transmission rate test is 100μm, and the test standard is GB / T 1037-1988. The water vapor barrier performance (water vapor transmission rate) in Table 1 means the water vapor transmission rate per m within the test time of 24h. 2 The total mass of water vapor transmitted by polyester material.
[0046] Table 1 Test results of thermal conductivity, tensile strength and barrier properties of pure PBT resin, polyester-based composite materials of various embodiments and comparative examples
[0047]
[0048] In order to investigate the influence of process parameters on the experimental results, the experiment was repeated according to the preparation method of the polyester-based composite material in Example 1, with the difference that the hydroxy-modified flaky boron nitride was replaced by commercially available amino-modified flaky boron nitride (flaky diameter of 0.1-0.4 μm, thickness of 30-100 nm, amino content of 5%-15%), or polybutylene terephthalate was replaced by commercially available polyethylene terephthalate with a weight average molecular weight of 30,000-50,000, or the melt extrusion temperature was adjusted from 240°C to 270°C, or the injection molding temperature was adjusted from 250°C to 280°C, and then the polyester-based composite material prepared after adjusting the parameters was tested for thermal conductivity, tensile strength and barrier properties according to the method of the experimental example. The results showed that the thermal conductivity, tensile strength and barrier properties of the polyester-based composite material prepared after adjusting the parameters were close to those of the polyester-based composite material in Example 1.
Claims
1. A polyester-based composite material, characterized in that: The invention is composed of the following components in parts by mass: 40-60 parts of polyester, 20-30 parts of functional group-modified flaky boron nitride, and 20-30 parts of molybdenum disulfide; the functional groups are hydroxyl and amino groups; the flaky boron nitride modified with functional groups has a sheet diameter of 0.1-0.4 μm, a thickness of 30-100 nm, and a functional group content of 5%-15%; the particle size of molybdenum disulfide is 200-300 nm; and the polyester is polyethylene terephthalate or polybutylene terephthalate.
2. The polyester-based composite material according to claim 1, characterized in that: The weight average molecular weight of the polyester is 30,000 to 50,000.
3. The polyester-based composite material according to claim 1 or 2, characterized in that: The polyester-based composite material is prepared by a method comprising the following steps: mixing a formulated amount of polyester, molybdenum disulfide and functional group-modified flake boron nitride and then melt-extruding the mixture to obtain the polyester-based composite material.
4. The polyester-based composite material according to claim 3, characterized in that: The temperature of melt extrusion is 240 to 270°C.
5. The polyester-based composite material according to claim 3, characterized in that: The mixing method is as follows: After mixing the polyester and molybdenum disulfide in the formula amount, a mixed base material is obtained, and then the mixed base material and the flake boron nitride modified with the functional group are mixed.
6. The polyester-based composite material according to claim 5, characterized in that: The polyester and molybdenum disulfide are mixed by a kneader.
7. The polyester-based composite material according to claim 5, characterized in that: The temperature of mixing polyester and molybdenum disulfide is 70-90°C and the time is 10-30 minutes.
8. The polyester-based composite material according to claim 5, characterized in that: The mixed base material and the functional group-modified flake boron nitride are mixed by using a kneader.
9. The polyester-based composite material according to claim 8, characterized in that: The mixing of the mixed base material and the functional group-modified flake boron nitride includes a first mixing stage and a second mixing stage, the first mixing stage adopts a temperature of 70-90°C and a time of 10-30 minutes, and the second mixing stage adopts a temperature of 150-160°C and a time of 2-5 hours.
10. The polyester-based composite material according to claim 3, characterized in that: The preparation method of polyester-based composite material is also The method comprises the following steps: uniformly mixing the polyester, molybdenum disulfide and functional group-modified flake boron nitride in a prescribed amount, cooling to room temperature, and then crushing to obtain crushed material, and then melt-extruding the crushed material.