Preparation method of transition metal loaded mineral based flame-retardant silicone rubber

By combining the minerals of porous structure with transition metal salts, efficient and environmentally friendly mineral flame retardants are prepared, which solves the problems of limited resources, expensive prices and environmental pollution of traditional flame retardants, and achieves efficient and environmentally friendly flame retardants. Effects, suitable for other polymer flame retardant fields.

CN118931183AInactive Publication Date: 2024-11-12CHANGCHUN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310519855.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the preparation process, existing flame retardants have problems such as limited resources, expensive prices, complex processes and environmental pollution. Traditional flame retardants may release toxic gases during combustion, threatening human health and the environment.

Method used

Using the preparation method of transition metal-loaded mineral-based flame-retardant silicone rubber, the minerals with porous structures are combined with transition metal salts and chemical reactions to introduce inorganic ions into the mineral structure to prepare efficient and environmentally friendly mineral flame-retardant , achieve zero emission and environmentally friendly flame retardant effects.

Benefits of technology

Overcoming the limited resources, expensive prices and environmental pollution of traditional flame retardants, improving the efficiency of mineral flame retardant silicone rubber, achieving zero emission and environmentally friendly flame retardant effects, and is suitable for flame retardant fields of other types of polymers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004220497970000011
    Figure HDA0004220497970000011
  • Figure HDA0004220497970000021
    Figure HDA0004220497970000021
  • Figure HDA0004220497970000031
    Figure HDA0004220497970000031
Patent Text Reader

Abstract

The invention relates to a preparation method of transition metal loaded mineral based flame-retardant silicone rubber, which comprises the following steps: by taking a porous mineral material as a carrier, introducing inorganic ions into a mineral structure through chemical reaction among characteristic groups, and further preparing a transition metal loaded mineral flame retardant which is used for a flame-retardant silicone rubber material. Compared with a traditional flame retardant, the mineral flame retardant prepared by the invention overcomes the problems of limited source, high price, complex preparation process, phosphorus and halogen containing and the like of a halogen-free flame retardant, and fully utilizes the unique shielding capability of the mineral flame retardant and the catalytic char forming capability of transition metal; further, the efficiency of the mineral flame-retardant silicone rubber is effectively improved. The flame retardant prepared through the method has the advantages of being simple in method, wide in raw material source, low in manufacturing cost, excellent in performance, good in flame retardant effect and the like, is harmless to the environment and the human body, achieves effective utilization and conversion of natural resources, improves the additional value of natural minerals, and therefore has good application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant materials, and in particular relates to a method for preparing transition metal-loaded mineral-based flame retardant silicone rubber. Technical Background

[0002] Nowadays, the industrial field is growing and penetrating into people's lives. It is closely related to people's lives, and polymer materials occupy a pivotal position. However, there are still many safety hazards in the application of polymer materials. Polymer organic materials may be accompanied by the release of toxic gases during the combustion process. The burning speed is too fast to extinguish, and even threatens people's health and safety. Although some flame retardants can prevent these problems, there are various difficulties in their preparation, such as the difficulty of the production process, limited sources and inability to be widely used, high prices, and the emission of toxic gases; in addition, the treatment process of discarded flame retardant materials is also complicated, consuming manpower and material resources, and even seriously polluting the environment. In summary, for the safety of human life and the protection of the environment, it is an important task to develop efficient, environmentally friendly, low-carbon and non-toxic flame retardants.

[0003] Natural minerals are often used as functional fillers for polymers due to their high adsorption capacity, low density, green environmental protection and low price. As a low-cost filler, natural minerals have been widely used in rubber, coatings, medicine and other fields. In particular, natural minerals can be used as a kind of inorganic flame retardant. During use, the inorganic particles loaded inside play a major flame retardant effect. During the combustion process, a carbon layer is formed on the surface of the composite material composed of inorganic particles and polymers, and the released heat is isolated. In addition, the mineral pores are large and the adsorption capacity is strong, which reduces the concentration of CO to effectively reduce the risk of fire and smoke toxicity. The raw materials of traditional flame retardants are limited in source and cannot be over-developed to avoid waste of resources. The toxic gases formed during the treatment process harm the environment and threaten human health. Mineral flame retardants can effectively overcome the shortcomings of traditional flame retardants, such as limited sources, high prices, environmental pollution and halogen and phosphorus. Therefore, the new challenge at present is to develop mineral flame retardants that are low-carbon, environmentally friendly, widely available and low-priced.

[0004] Mineral materials in nature are inexhaustible. These mineral materials are mainly inorganic salts, with the characteristics of wide sources, green environmental protection, and low price. In addition, most of these mineral materials have porous structures and can be used as carriers or surface modified, so they can be widely used as a new type of flame retardant. Therefore, combining natural minerals with high-performance flame retardant technology to prepare efficient and clean mineral flame retardants will inevitably achieve the goal of sustainable development and be beneficial and harmless to human society. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing transition metal-loaded mineral-based flame-retardant silicone rubber.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] 1. A method for preparing a transition metal-loaded mineral-based flame-retardant silicone rubber, comprising the following sequence and steps: --- Preparation process of a transition metal-loaded mineral flame retardant:

[0008] a. Weigh 3g of minerals and place them in a 500mL three-necked flask, add 100mL of deionized water, and mechanically stir for about 30min at room temperature to obtain a uniformly dispersed viscous liquid A;

[0009] b. Weigh 1.69 g of transition metal salt into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0010] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0011] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is the transition metal-loaded mineral flame retardant;

[0012] -Preparation of mineral flame retardant silicone rubber:

[0013] a. Weigh 97g of silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of silicone rubber component B, and continue stirring for 5min;

[0014] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0015] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0016] 2. The method for preparing transition metal-loaded mineral flame-retardant silicone rubber according to claim 1, characterized in that the mineral is one of diatomaceous earth, mica, kaolin, tourmaline, attapulgite, hydrotalcite, hydromagnesite and montmorillonite;

[0017] 3. The method for preparing a transition metal-loaded mineral-based flame-retardant silicone rubber according to claim 1, characterized in that the transition metal salt is one of transition metal salts such as manganese sulfate, nickel sulfate, manganese acetate, nickel acetate, manganese nitrate, nickel nitrate, iron nitrate, copper nitrate, cobalt nitrate, copper acetate and cobalt acetate; 4. The method for preparing a transition metal-loaded mineral-based flame-retardant silicone rubber according to claim 1, characterized in that the silicone rubber is one of room temperature vulcanized silicone rubber, dimethyl silicone rubber, methyl vinyl and methylphenyl vinyl silicone rubber;

[0018] Preferably, in the process of loading the transition metal with the mineral flame retardant, 3 g of the mineral flame retardant is dissolved in 100 mL of deionized water, and 1.69 g of the transition metal salt is added in 45 mL of deionized water;

[0019] Preferably, the addition ratio of transition metal-loaded mineral flame retardant and silicone rubber is 30:100;

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] Using porous mineral materials as carriers, inorganic ions are introduced into the mineral structure through chemical reactions between characteristic groups, thereby preparing mineral flame retardants. Compared with traditional flame retardants, the mineral flame retardants prepared by this patent overcome the problems of limited sources, high prices, complex processes, and phosphorus and halogen content of halogen-free flame retardants, and make full use of the unique shielding ability of mineral flame retardants and the catalytic carbonization ability of transition metals, thereby effectively improving the efficiency of mineral flame retardant silicone rubber materials. The scheme designed by the present invention achieves zero emissions of VOCs from the preparation process to the composition of the flame retardant, reduces the pollution and damage to the environment caused by the preparation and use of flame retardants, and is expected to achieve the replacement of traditional flame retardants and expand applications in other types of polymer flame retardant fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Provided for Example 1 are the particle size test results of the flame retardants before and after modification: (a) diatomaceous earth flame retardant, (b) transition metal loaded diatomaceous earth flame retardant;

[0023] Figure 2 Provided for Example 1 are the residue effect diagrams of different vulcanized silicone rubber samples at 600° C.: (a) the residue of a diatomaceous earth flame retardant silicone rubber sample, (b) the residue of a transition metal loaded diatomaceous earth flame retardant silicone rubber sample;

[0024] Figure 3 Provided for Example 1 are the mechanical property test results of different vulcanized silicone rubber samples;

[0025] Figure 4Provided for Example 1 are the limiting oxygen index test results of different vulcanized silicone rubber samples;

[0026] Figure 5 Provided for Example 1 are the infrared spectrogram test results before and after the flame retardant is modified; DETAILED DESCRIPTION

[0027] The following is further described in detail in conjunction with the embodiments:

[0028] Embodiment 1:

[0029] -Preparation process of transition metal loaded mineral-based flame retardant:

[0030] a. Weigh 3 g of diatomaceous earth and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir for about 30 min at room temperature to obtain a uniformly dispersed viscous liquid A;

[0031] b. Weigh 1.69 g of manganese sulfate and place it in a 100 mL beaker. Add 45 mL of deionized water and stir with a glass rod until it is completely dissolved to obtain solution B.

[0032] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0033] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0034] -Preparation of mineral-based flame-retardant silicone rubber:

[0035] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0036] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0037] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0038] Embodiment 2:

[0039] -Preparation process of transition metal loaded mineral-based flame retardant:

[0040] a. Weigh 3 g of mica stone and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0041] b. Weigh 1.69 g of nickel sulfate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0042] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0043] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0044] -Preparation of mineral-based flame-retardant silicone rubber:

[0045] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0046] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0047] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0048] Embodiment 3:

[0049] -Preparation process of transition metal loaded mineral-based flame retardant:

[0050] a. Weigh 3 g of kaolin and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0051] b. Weigh 1.69 g of manganese nitrate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0052] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0053] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0054] -Preparation of mineral-based flame-retardant silicone rubber:

[0055] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0056] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0057] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0058] Embodiment 4:

[0059] -Preparation process of transition metal loaded mineral-based flame retardant:

[0060] a. Weigh 3 g of diatomaceous earth and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir for about 30 min at room temperature to obtain a uniformly dispersed viscous liquid A;

[0061] b. Weigh 1.69 g of manganese acetate and place it in a 100 mL beaker. Add 45 mL of deionized water and stir with a glass rod until it is completely dissolved to obtain solution B.

[0062] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0063] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0064] -Preparation of mineral-based flame-retardant silicone rubber:

[0065] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0066] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0067] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0068] Embodiment 5:

[0069] -Preparation process of transition metal loaded mineral-based flame retardant:

[0070] a. Weigh 3 g of mica stone and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0071] b. Weigh 1.69 g of manganese sulfate and place it in a 100 mL beaker. Add 45 mL of deionized water and stir with a glass rod until it is completely dissolved to obtain solution B.

[0072] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0073] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0074] -Preparation of mineral-based flame-retardant silicone rubber:

[0075] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0076] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0077] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0078] Embodiment 6:

[0079] -Preparation process of transition metal loaded mineral-based flame retardant:

[0080] a. Weigh 3 g of kaolin and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0081] b. Weigh 1.69 g of manganese sulfate and place it in a 100 mL beaker. Add 45 mL of deionized water and stir with a glass rod until it is completely dissolved to obtain solution B.

[0082] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0083] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0084] -Preparation of mineral-based flame-retardant silicone rubber:

[0085] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0086] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0087] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0088] Embodiment 7:

[0089] -Preparation process of transition metal loaded mineral-based flame retardant:

[0090] a. Weigh 3 g of diatomaceous earth and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir for about 30 min at room temperature to obtain a uniformly dispersed viscous liquid A;

[0091] b. Weigh 1.69 g of manganese nitrate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0092] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0093] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0094] -Preparation of mineral-based flame-retardant silicone rubber:

[0095] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0096] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0097] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0098] Embodiment 8:

[0099] -Preparation process of transition metal loaded mineral-based flame retardant:

[0100] a. Weigh 3 g of mica stone and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0101] b. Weigh 1.69 g of manganese acetate and place it in a 100 mL beaker. Add 45 mL of deionized water and stir with a glass rod until it is completely dissolved to obtain solution B.

[0102] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0103] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0104] -Preparation of mineral-based flame-retardant silicone rubber:

[0105] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0106] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0107] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0108] Embodiment 9:

[0109] -Preparation process of transition metal loaded mineral-based flame retardant:

[0110] a. Weigh 3 g of kaolin and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0111] b. Weigh 1.69 g of nickel nitrate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0112] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0113] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0114] -Preparation of mineral-based flame-retardant silicone rubber:

[0115] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0116] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0117] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0118] Embodiment 10:

[0119] -Preparation process of transition metal loaded mineral-based flame retardant:

[0120] a. Weigh 3 g of diatomaceous earth and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir for about 30 min at room temperature to obtain a uniformly dispersed viscous liquid A;

[0121] b. Weigh 1.69 g of nickel sulfate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0122] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0123] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0124] -Preparation of mineral-based flame-retardant silicone rubber:

[0125] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0126] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0127] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0128] Embodiment 11:

[0129] -Preparation process of transition metal loaded mineral-based flame retardant:

[0130] a. Weigh 3 g of diatomaceous earth and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir for about 30 min at room temperature to obtain a uniformly dispersed viscous liquid A;

[0131] b. Weigh 1.69 g of nickel acetate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0132] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0133] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0134] -Preparation of mineral-based flame-retardant silicone rubber:

[0135] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0136] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0137] d. Take the fully cured RTV silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the RTV silicone rubber sample into strips of the size required for the flame retardant test;

[0138] Embodiment 12:

[0139] -Preparation process of transition metal loaded mineral-based flame retardant:

[0140] a. Weigh 3 g of mica stone and place it in a 100 mL three-necked flask, add 100 mL of deionized water, and mechanically stir at room temperature for about 30 min to obtain a uniformly dispersed viscous liquid A;

[0141] b. Weigh 1.69 g of manganese nitrate into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B;

[0142] c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours;

[0143] d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water for 3-5 times to collect the filter cake; e. Dry the filter cake in a 60°C vacuum drying oven for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral-based flame retardant;

[0144] -Preparation of mineral-based flame-retardant silicone rubber:

[0145] a. Weigh 97g of room temperature vulcanized silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of room temperature vulcanized silicone rubber component B, and continue stirring for 5min;

[0146] c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours;

[0147] d. Take the fully cured room temperature vulcanized silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the room temperature vulcanized silicone rubber sample into strips of the size required for the flame retardant test.

Claims

1. A method for preparing a transition metal-loaded mineral-based flame-retardant silicone rubber, comprising the following sequence and steps: ---Preparation process of transition metal loaded mineral flame retardant: a. Weigh 3g of minerals and place them in a 500mL three-necked flask, add 100mL of deionized water, and mechanically stir for about 30min at room temperature to obtain a uniformly dispersed viscous liquid A; b. Weigh 1.69 g of transition metal salt into a 100 mL beaker, add 45 mL of deionized water, and stir with a glass rod until completely dissolved to obtain solution B; c. Under mechanical stirring, use a constant flow pump to add solution B dropwise into liquid A, maintain the temperature at 40°C, continue stirring for 30 minutes after the addition is completed, adjust the pH to 8-9 with ammonia water, and continue stirring for 12 hours; d. When the system cools to room temperature, vacuum filter and rinse repeatedly with deionized water 3-5 times to collect the filter cake; e. Place the filter cake in a vacuum drying oven at 60°C and dry for 12 hours, take it out, grind it, and the obtained product is a transition metal-loaded mineral flame retardant; -Preparation of mineral flame retardant silicone rubber: a. Weigh 97g of silicone rubber component A, place it in a 200mL polytetrafluoroethylene container, stir it mechanically at a rate of 5000r / min, add 30g of transition metal-loaded mineral-based flame retardant, and continue stirring for 30min. Then, increase the mechanical stirring rate to 6000r / min, add 3g of silicone rubber component B, and continue stirring for 5min; c. Inject the room temperature vulcanized silicone rubber mixture into a polytetrafluoroethylene mold, then place it in a vacuum drying oven for evacuation and cure at room temperature for 24 hours; d. Take the fully cured room temperature vulcanized silicone rubber out of the mold, cut off the excess edge, and use a cutting machine to cut the room temperature vulcanized silicone rubber sample into strips of the size required for the flame retardant test.

2. The method for preparing the transition metal-loaded mineral flame-retardant silicone rubber according to claim 1, Features The mineral is one of diatomaceous earth, mica, kaolin, tourmaline, attapulgite, hydrotalcite, hydromagnesite and montmorillonite.

3. The method for preparing the transition metal-loaded mineral flame-retardant silicone rubber according to claim 1, Features The transition metal salt is one of transition metal salts such as manganese sulfate, nickel sulfate, manganese acetate, nickel acetate, manganese nitrate, nickel nitrate, iron nitrate, copper nitrate, cobalt nitrate, copper acetate and cobalt acetate.

4. The method for preparing the transition metal-loaded mineral flame-retardant silicone rubber according to claim 1, Features The silicone rubber is one of room temperature vulcanized silicone rubber, dimethyl silicone rubber, methyl vinyl and methyl phenyl vinyl silicone rubber.