Modified polyimide binder and preparation method thereof, electrode plate and lithium ion battery
By introducing benzotriazole structures and long aliphatic side chains into polyimide binders, the problem of high expansion rate of silicon-based anodes is solved, thereby improving the cycle life and safety of lithium-ion batteries.
Patent Information
- Application Number
- CN202411069934.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
AI Technical Summary
Among existing lithium-ion battery anode materials, silicon-based anodes have a high expansion rate, which leads to the destruction of the active material layer and a decline in battery cycle performance. Traditional binders have weak adhesion and cannot effectively solve this problem.
A modified polyimide binder is used, which enhances the bonding force with the current collector and improves flexibility by introducing benzotriazole structure and long aliphatic side chains into its molecular structure, thereby improving the resistance to volume expansion of the silicon-based anode.
It improves the volume expansion resistance of silicon-based anodes, enhances the bonding force between the anode slurry and the current collector, and extends the cycle life and safety of lithium-ion batteries.
Smart Images

Figure CN118931473A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of batteries, and in particular to a modified polyimide binder and a preparation method thereof, an electrode sheet and a lithium ion battery. Background Art
[0002] At present, the negative electrode materials of lithium-ion batteries are mainly carbon-based negative electrodes, and the binders used are mainly oily binders such as polyvinylidene fluoride (PVDF) and water-based binders such as sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR). These traditional negative electrode binders have poor adhesion and poor bonding with metal current collectors, which will lead to a decrease in battery capacity and a shortened cycle life during repeated charge and discharge. Silicon-based negative electrodes are the main choice for the next generation of new negative electrode materials, with advantages such as high specific capacity and excellent fast charging performance. However, the expansion rate of silicon-based negative electrodes is extremely high, and the common negative electrode binders such as PVDF, SBR, and CMC have poor adhesion, which will cause the active material layer to be destroyed due to volume changes, resulting in a decrease in battery cycle performance.
[0003] Therefore, there is an urgent need to provide an adhesive that can alleviate the high expansion problem of silicon-based materials. Summary of the invention
[0004] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, the present invention provides a modified polyimide binder and a preparation method, an electrode sheet and a lithium ion battery. The modified polyimide binder has good thermal stability and flexibility, strong binding force with the current collector, and can improve the volume expansion resistance of the silicon-based negative electrode.
[0005] To this end, the first aspect of the present invention provides a modified polyimide binder, wherein the modified polyimide binder has a structure represented by formula (I) or a stereoisomer, nitrogen oxide, hydrate, solvate or salt thereof represented by formula (I);
[0006]
[0007] Among them, R 1 Selected from aromatic groups or fluorine-containing aromatic groups containing ether bonds, ester groups and / or carbonyl groups;
[0008] R 2 Selected from aromatic groups containing ether bonds and / or thioether bonds;
[0009] R 3 Selected from C 1 -C 10 Alkylene, C 3 -C 10 At least one of cycloalkyl groups;
[0010] R 4Select from single bonds or C 1 -C 5 Alkylene;
[0011] x:y=(40-450):(5-100).
[0012] In order to solve the deficiencies in the prior art, the present invention adopts a polyimide resin with high mechanical properties and high heat resistance as a binder, and modifies the polyimide resin to introduce a benzotriazole structure into its molecular structure. The benzotriazole structure can form covalent bonds and coordination bonds with metal atoms, and alternately form chain polymers, thereby increasing the binding force between the binder and the current collector, and improving the binding force between the negative electrode slurry and the current collector. While introducing the benzotriazole structure, a long aliphatic branch chain is also introduced into the polyimide molecular structure, thereby increasing the distance between the molecular chains, improving the flexibility of the polyimide molecular structure, and at the same time, the branched structure is wound on the surface of the negative electrode material, thereby improving the volume expansion resistance of the silicon-based negative electrode.
[0013] According to an embodiment of the present invention, R 1 Selected from
[0014] According to an embodiment of the present invention, R 2 Selected from
[0015]
[0016] According to an embodiment of the present invention, R 3 Selected from C 1 -C 10 Alkylene, C 4 -C 6 At least one of cycloalkyl.
[0017] According to an embodiment of the present invention, R 3 Selected from C 1 -C 10 Alkylene, C 4 Cycloalkyl,
[0018] According to an embodiment of the present invention, R 4 Select from single bonds or C 1 -C 2 Alkylene.
[0019] The second aspect of the present invention provides a method for preparing the modified polyimide binder according to the first aspect, comprising:
[0020] Performing a first mixing treatment on the dianhydride monomer and the diamine monomer to obtain a polyamic acid;
[0021] performing a second mixing process on the polyamic acid and the intermediate to obtain a modified polyamic acid;
[0022] The modified polyamic acid is subjected to imidization reaction to obtain the modified polyimide binder;
[0023] Wherein, the dianhydride monomer has a structure shown in formula (II):
[0024] R 1 As described in the first aspect;
[0025] The diamine monomer has a structure shown in formula (III):
[0026] H 2 NR 2 -NH 2 Formula (III), R 2 As described in the first aspect;
[0027] The intermediate has a structure shown in formula (IV):
[0028] R 3 , R 4 As described in the first aspect.
[0029] The modified polyimide binder can be obtained by the above method. The binder has good thermal stability and flexibility, strong bonding force with the current collector, and can improve the volume expansion resistance of the silicon-based negative electrode.
[0030] According to an embodiment of the present invention, the molar ratio of the dianhydride monomer to the diamine monomer is (0.9-1.01):1.
[0031] According to an embodiment of the present invention, the dianhydride monomer is selected from at least one of bisphenol A type diether dianhydride, p-phenylene-diphenyltrimethylol dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, hexafluoro dianhydride, diethylene glycol (4-tricarboxylic anhydride), and 5-isobenzofurancarboxylic acid 1,3-dihydro-1,3-dioxy-5,5'-[(1-methylethylidene)di-4,1-phenylene] ester.
[0032] According to an embodiment of the present invention, the dianhydride monomer is selected from at least one of 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 4,4'-diaminophenyl sulfone, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)diphenyl sulfone and 2,2-bis[4-(4-aminophenoxy)phenyl]propane.
[0033] According to an embodiment of the present invention, the temperature of the first mixing treatment is 0-20°C, preferably 5-10°C.
[0034] According to an embodiment of the present invention, the time of the first mixing treatment is 2-24 hours, preferably 6-18 hours.
[0035] According to an embodiment of the present invention, the molar ratio of the polyamic acid to the intermediate is 1:(0.1-0.2).
[0036] According to an embodiment of the present invention, the temperature of the second mixing treatment is 0-100°C, preferably 20-50°C.
[0037] According to an embodiment of the present invention, the time of the second mixing treatment is 1-24 hours, preferably 2-6 hours.
[0038] According to an embodiment of the present invention, the method further includes:
[0039] The polyamic acid and thionyl chloride are subjected to a third mixing treatment to obtain an intermediate compound, and the intermediate compound is mixed with the intermediate to obtain the modified polyamic acid.
[0040] According to an embodiment of the present invention, the molar ratio of the intermediate to thionyl chloride is 1:(1-1.1).
[0041] According to an embodiment of the present invention, the temperature of the third mixing treatment is 50-100°C, preferably 50-80°C.
[0042] According to an embodiment of the present invention, the time of the third mixing treatment is 2-24 hours, preferably 1-5 hours.
[0043] According to an embodiment of the present invention, the modified polyamic acid is subjected to imidization reaction under the action of a dehydrating agent and a catalyst.
[0044] According to an embodiment of the present invention, the molar ratio of the modified polyamic acid to the dehydrating agent and the catalyst is 1:(1.8-1.9):(0.8-0.9).
[0045] According to an embodiment of the present invention, the dehydrating agent is selected from at least one of acetic anhydride, acetyl chloride and trifluoroacetic anhydride.
[0046] According to an embodiment of the present invention, the catalyst is selected from at least one of triethylamine and pyridine.
[0047] According to an embodiment of the present invention, the temperature of the imidization reaction is 50-100°C, preferably 50-80°C.
[0048] According to an embodiment of the present invention, the imidization reaction time is 4-24 hours, preferably 4-12 hours.
[0049] According to an embodiment of the present invention, the method further comprises preparing the intermediate;
[0050] The preparation of the intermediate comprises: performing a fourth mixing treatment on compound 1, compound 2 and a condensing agent to obtain the intermediate;
[0051] Wherein, the compound 1 has a structure shown in formula (V):
[0052] H 2 NR 3 -NH 2 Formula (V), R 3 As described in the first aspect;
[0053] The compound 2 has a structure shown in formula (VI):
[0054] R 4 As described in the first aspect.
[0055] According to an embodiment of the present invention, the molar ratio of compound 1, compound 2 and the condensing agent is 1:1:(1-1.1).
[0056] According to an embodiment of the present invention, the compound 1 is selected from at least one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,3-diaminocyclobutylamine, 2-methyl-1,3-propylenediamine, 1,3-diaminopentane, 1,4-butylenediamine, 1,5-pentanediamine, 2-methyl-1,5-pentanediamine, 4-aminomethylcyclohexylamine, 2-aminomethylcyclohexylamine, 1,3-cyclohexanedimethylamine, hexanediamine, 1,7-diaminoheptane, 1,8-octanediamine, 1,9-nonanediamine, and decanediamine.
[0057] According to an embodiment of the present invention, the compound 2 is selected from at least one of 5-benzotriazole carboxylate, 2-(1H-benzo[d][1,2,3]triazol-6-yl)acetic acid, 2-(1H-benzo[d][1,2,3]triazol-6-yl)propionic acid, 2-(1H-benzo[d][1,2,3]triazol-6-yl)isopropionic acid, 2-(1H-benzo[d][1,2,3]triazol-7-yl)acetic acid, and 4-benzotriazole carboxylate.
[0058] According to an embodiment of the present invention, the condensing agent is selected from at least one of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, carbonyldiimidazole, thionyl chloride, and N,N'-carbonyldiimidazole.
[0059] According to an embodiment of the present invention, the temperature of the fourth mixing treatment is 0-100°C, preferably 20-50°C.
[0060] According to an embodiment of the present invention, the fourth mixing treatment is performed for 1-24 hours, preferably 1-5 hours.
[0061] A third aspect of the present invention provides an electrode sheet, comprising an electrode active material and the modified polyimide binder described in the first aspect or the modified polyimide binder obtained according to the method described in the second aspect.
[0062] Therefore, the electrode sheet has a better ability to resist volume expansion.
[0063] A fourth aspect of the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the electrode sheet described in the third aspect.
[0064] Therefore, the lithium-ion battery has better safety and longer cycle life.
[0065] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. DETAILED DESCRIPTION
[0066] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be understood as limiting the present invention.
[0067] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of the present invention, unless otherwise specified, the meaning of "plurality" is two or more.
[0068] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0069] In order to make the present invention more easily understood, certain technical and scientific terms are specifically defined below. Unless otherwise clearly defined elsewhere in this document, all other technical and scientific terms used herein have the meanings commonly understood by those skilled in the art to which the present invention belongs.
[0070] In this document, the terms “include” or “comprising” are open expressions, that is, including the contents specified in the present invention but not excluding other contents.
[0071] As used herein, the terms "optionally", "optional" or "optionally" generally mean that the subsequently described event or circumstance may but need not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not.
[0072] Unless otherwise stated, conventional methods within the technical scope of the art, such as mass spectrometry, NMR, IR and UV / Vis spectroscopy and pharmacological methods, are used. Unless specifically defined, the terms used herein in the relevant descriptions of analytical chemistry, organic synthetic chemistry, and drugs and medicinal chemistry are known in the art. Standard techniques can be used in chemical synthesis, chemical analysis, drug preparation, formulation and delivery, and in the treatment of patients. For example, the manufacturer's instructions for the use of the kit can be used, or the reaction and purification can be carried out in a manner known in the art or in accordance with the description of this application. The above techniques and methods can usually be implemented according to conventional methods well known in the art, according to the descriptions in the multiple general and more specific documents cited and discussed in this specification. In this specification, groups and substituents thereof can be selected by those skilled in the art to provide stable structural parts and compounds. When a substituent is described by a conventional chemical formula written from left to right, the substituent also includes a chemically equivalent substituent obtained when the structural formula is written from right to left. For example, CH 2 O is equivalent to OCH 2 .
[0073] The compounds of the invention may contain unnatural proportions of atomic isotopes on one or more of the atoms that make up the compound. For example, the compounds may be labeled with radioactive isotopes, such as deuterium ( 2 H), tritium ( 3 H), iodine-125( 125 I) or C-14( 14 C) All isotopic variations of the compounds of the present invention, whether radioactive or not, are included within the scope of the present invention.
[0074] The term "C 1 -C 10 "Alkylene" is understood to mean a straight-chain or branched alkyl radical having 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms, which is linked to other radicals via two carbon atoms to form an alkylene radical. 1 -C 10 The alkylene group may be a methylene group (-CH 2 -), ethylene (-CH 2 CH 2 -), propylene (-CH 2 CH 2 CH 2 -、-CH(CH3 )CH 2 -)wait.
[0075] The term "C 3 -C 10 "Cycloalkyl" is understood to be a cyclic alkyl group containing 3 to 10 carbon atoms and which is linked to other radicals via two carbon atoms.
[0076] The term "single bond" is to be understood as a covalent bond formed by two atoms sharing a pair of electrons.
[0077] According to an embodiment of the present invention, a first aspect of the present invention provides a modified polyimide binder, wherein the modified polyimide binder has a structure represented by formula (I) or a stereoisomer, nitrogen oxide, hydrate, solvate or salt thereof of the structure represented by formula (I);
[0078]
[0079] Among them, R 1 Selected from aromatic groups or fluorine-containing aromatic groups containing ether bonds, ester groups and / or carbonyl groups;
[0080] R 2 Selected from aromatic groups containing ether bonds and / or thioether bonds;
[0081] R 3 Selected from C 1 -C 10 Alkylene, C 3 -C 10 At least one of cycloalkyl groups;
[0082] R 4 Select from single bonds or C 1 -C 5 Alkylene;
[0083] x:y=(40-450):(5-100).
[0084] Polyimide has high mechanical properties and high heat resistance. By modifying it and introducing a benzotriazole structure into its molecular structure, the benzotriazole structure can form covalent bonds and coordination bonds with metal atoms (such as copper atoms), alternating into chain polymers, increasing the binding force between the binder and the copper foil current collector, and improving the binding force between the negative electrode slurry and the current collector. In addition, long aliphatic side chains are introduced into the polyimide molecular structure to increase the distance between the molecular chains and improve the flexibility of the polyimide molecular structure. At the same time, the branched structure is entangled on the surface of the negative electrode material, which can improve the volume expansion resistance of the silicon-based negative electrode.
[0085] In the present invention, "*" indicates connection with an end-capping structure, and the end-capping structure is determined by an end-capping agent, and the end-capping agent is not limited.
[0086]
[0087] According to a specific embodiment of the present invention, x and y represent the degree of polymerization, that is, the number of each repeating unit, and the ratio of x to y may be (40-450): (5-100). Specifically, the values of x and y are not particularly limited, and those skilled in the art may select them according to actual needs. As some specific examples, x may be an integer of 40-450, such as 40, 100, 150, 200, 250, 300, 350, 400, 450, etc.; y may be an integer of 5-100, such as 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, etc.
[0088] According to a specific embodiment of the present invention, R 1 is selected from aromatic groups or fluorine-containing aromatic groups containing ether bonds, ester groups and / or carbonyl groups, wherein "R 1 "selected from aromatic groups containing ether bonds, ester groups and / or carbonyl groups" should be understood as: R 1 It may be an aromatic group containing only an ether bond, an ester group or a carbonyl group, or an aromatic group containing both an ether bond and an ester group, or an aromatic group containing both an ether bond and a carbonyl group, or an aromatic group containing both an ester group and a carbonyl group, or an aromatic group containing both an ether bond, an ester group and a carbonyl group.
[0089] According to a specific embodiment of the present invention, R 2 is selected from aromatic groups containing ether bonds and / or sulfone groups, i.e. R 2 It may be an aromatic group containing only an ether bond or a sulfone group, or an aromatic group containing both an ether bond and a sulfone group.
[0090]
[0091]
[0092] According to a specific embodiment of the present invention, R 3 Selected from C 1 -C 10 Alkylene, C 3 -C 10 At least one of the cycloalkyl groups, namely R 3 Can be C 1 -C 10 Alkylene, C 3 -C 10 Cycloalkyl or including C 1 -C 10 Alkylene and C 3 -C10 A mixed group of cycloalkyl. 3 Preferred C 1 -C 10 Alkylene, C 4 -C 6 At least one of cycloalkyl; more preferably C 1 -C 10 Alkylene, C 4 Cycloalkyl,
[0093]
[0094] According to a specific embodiment of the present invention, R 4 Select from single bonds or C 1 -C 5 Alkylene, preferably a single bond or C 1 -C 2 Alkylene.
[0095] According to an embodiment of the present invention, a second aspect of the present invention provides a method for preparing the modified polyimide binder according to the first aspect, comprising:
[0096] (1) subjecting a dianhydride monomer and a diamine monomer to a first mixing treatment to obtain a polyamic acid;
[0097] Wherein, the dianhydride monomer has a structure shown in formula (II):
[0098] R 1 As described in the first aspect;
[0099] The diamine monomer has a structure shown in formula (III):
[0100] H 2 NR 2 -NH 2 Formula (III), R 2 As described in the first aspect.
[0101] The reaction process of this step is as follows:
[0102]
[0103] Among them, n is an integer of 50-500, which can be selected according to actual needs. As some specific examples, it can be 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, etc.
[0104] According to a specific embodiment of the present invention, the molar ratio of the dianhydride monomer to the diamine monomer is (0.9-1.01):1, which can be selected according to actual needs. As some specific examples, 0.9:1, 1:1, 1.01:1, etc. can be selected to avoid excessive monomers.
[0105] According to a specific embodiment of the present invention, the type of the dianhydride monomer is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the dianhydride monomer includes but is not limited to bisphenol A diether dianhydride (BPADA), p-phenylene-diphenyltrimethylol dianhydride (TAHQ), 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride (BTDA), 4,4'-biphenyl ether dianhydride (ODPA), hexafluoro dianhydride (6FDA), diethylene glycol (4-tricarboxylic anhydride) (TMEG), 5-isobenzofurancarboxylic acid 1,3-dihydro-1,3-dioxy-5,5'-[(1-methylethylidene) di-4,1-phenylene] ester (BPEDA).
[0106] According to a specific embodiment of the present invention, the type of the diamine monomer is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, the diamine monomer includes but is not limited to 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 3,4'-diaminodiphenyl ether (3,4'-ODA), 4,4'-diaminodiphenyl ether (4,4'-ODA), 4,4'-diaminophenyl sulfone (4,4-DDS), 4,4'-bis(3-aminophenoxy)biphenyl (BAPB-M), 4,4'-bis(3-aminophenoxy)diphenyl sulfone (BAPS-M), and 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP).
[0107] According to a specific embodiment of the present invention, the temperature and time of the first mixing treatment can be selected according to actual needs. As some specific examples, the temperature of the first mixing treatment can be 0-20° C., such as 0° C., 5° C., 10° C., 15° C., 20° C., etc., preferably 5-10° C. The time of the first mixing treatment can be 2-24h, such as 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc., preferably 6-18h.
[0108] According to a specific embodiment of the present invention, this step may specifically include: in a protective gas atmosphere, dissolving the diamine monomer in solvent 1, and after the diamine monomer is completely dissolved, adding the dianhydride monomer, the dianhydride monomer is added three times, each time interval is more than 30 minutes, after the reaction is complete, the product polyamic acid solution is sealed and stored at 0-5°C for standby use.
[0109] Specifically, the protective gas may be nitrogen, and the solvent 1 may be N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or dimethyl sulfoxide.
[0110] (2) subjecting the polyamic acid to a second mixing treatment with an intermediate to obtain a modified polyamic acid;
[0111] Wherein, the intermediate has a structure shown in formula (IV):
[0112] R 3 , R 4 As described in the first aspect.
[0113] The reaction process of this step is as follows:
[0114]
[0115] The range of n is as described above.
[0116] According to a specific embodiment of the present invention, the molar ratio of the polyamic acid to the intermediate is 1:(0.1-0.2), which can be selected according to actual needs. As some specific examples, the molar ratio of the polyamic acid to the intermediate is 1:0.1, 1:0.15, 1:0.2, etc.
[0117] According to a specific embodiment of the present invention, the temperature and time of the second mixing treatment can be selected according to actual needs. As some specific examples, the temperature of the second mixing treatment can be 0-100° C., such as 0° C., 10° C., 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., 100° C., etc., preferably 20-50° C. The time of the second mixing treatment can be 1-24h, such as 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc., preferably 2-6h.
[0118] According to a specific embodiment of the present invention, the method further includes:
[0119] The polyamic acid and thionyl chloride are subjected to a third mixing treatment to obtain an intermediate compound, and the intermediate compound is mixed with the intermediate to obtain the modified polyamic acid.
[0120] Specifically, thionyl chloride can react with the carboxyl group in the polyamic acid structure to convert the carboxyl group into an acyl chloride group, and the acyl chloride group can react with the amino group in the intermediate structure to obtain the modified polyamic acid.
[0121] Specifically, the molar ratio of the intermediate to thionyl chloride is 1:(1-1.1), which can be selected according to actual needs. As some specific examples, the molar ratio of the intermediate to thionyl chloride can be 1:1, 1:1.1, etc.
[0122] Specifically, the temperature and time of the third mixing treatment are not particularly limited, and those skilled in the art can select according to actual needs. As some specific examples, the temperature of the third mixing treatment can be 50-100° C., such as 50° C., 60° C., 70° C., 80° C., 90° C., 100° C., etc., preferably 50-80° C. The time of the third mixing treatment can be 2-24h, such as 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc., preferably 1-5h.
[0123] According to a specific embodiment of the present invention, the method further comprises preparing the intermediate;
[0124] The preparation of the intermediate comprises: performing a fourth mixing treatment on compound 1, compound 2 and a condensing agent to obtain the intermediate;
[0125] Wherein, the compound 1 has a structure shown in formula (V):
[0126] H 2 NR 3 -NH 2 Formula (V), R 3 As described in the first aspect;
[0127] The compound 2 has a structure shown in formula (VI):
[0128] R 4 As described in the first aspect.
[0129] The reaction process of this step is as follows:
[0130]
[0131] Specifically, the molar ratio of compound 1, compound 2 and the condensing agent is 1:1:(1-1.1), which can be selected according to actual needs. As some specific examples, the molar ratio of compound 1, compound 2 and the condensing agent can be 1:1:1, 1:1:1.1, etc.
[0132] Specifically, the compound 1 is selected from ethylenediamine (CAS: 107-15-3), 1,2-propylenediamine (CAS: 78-90-0), 1,3-propylenediamine (CAS: 109-76-2), 1,3-diaminocyclobutylamine (CAS: 91301-66-5), 2-methyl-1,3-propylenediamine (CAS: 2400-78-4), 1,3-diaminopentane (CAS: 589-37-7), 1,4-butanediamine (CAS: 110-60-1), 1,5-pentanediamine (CAS: 462-94-2), 2-methyl-1 ,5-pentanediamine (CAS: 15520-10-2), 4-aminomethylcyclohexylamine (CAS: 13338-82-4), 2-aminomethylcyclohexylamine (CAS: 40015-92-7), 1,3-cyclohexanedimethylamine (CAS: 2579-20-6), hexanediamine (CAS: 124-09-4), 1,7-diaminoheptane (CAS: 646-19-5), 1,8-octanediamine (CAS: 373-44-4), 1,9-nonanediamine (CAS: 646-24-2), and decanediamine (CAS: 646-25-3).
[0133] Specifically, the compound 2 is selected from 5-benzotriazole carboxylate (CAS: 23814-12-2), 2-(1H-benzo[d][1,2,3]triazol-6-yl)acetic acid (CAS: 491612-10-3), 2-(1H-benzo[d][1,2,3]triazol-6-yl)propionic acid (CAS: 159454-47-4), 2-(1H-benzo[d][1,2,3]triazol-6-yl)isopropionic acid (CAS: 1506049-30-4), 2-(1H-benzo[d][1,2,3]triazol-7-yl)acetic acid (CAS: 1552705-76-6), 4-benzotriazole carboxylate (CAS: 62972-61-6), etc.
[0134] Specifically, the type of the condensing agent is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, it includes but is not limited to dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, carbonyldiimidazole, thionyl chloride, and N,N'-carbonyldiimidazole.
[0135] Specifically, the temperature and time of the fourth mixing treatment are not particularly limited, and those skilled in the art can select according to actual needs. As some specific examples, the temperature of the fourth mixing treatment can be 0-100° C., such as 0° C., 10° C., 20° C., 30° C., 40° C., 50° C., 60° C., 70° C., 80° C., 90° C., 100° C., etc., preferably 20-50° C. The time of the fourth mixing treatment can be 1-24h, such as 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc., preferably 1-5h.
[0136] Specifically, the preparation of the intermediate can be specifically as follows: in an inert atmosphere, compound 2 is dissolved in solvent 2, a condensing agent is added to react, compound 1 is added to react, washed with water, dried, solvent 2 is removed, and separated to obtain the product intermediate.
[0137] The inert atmosphere may be nitrogen, and the solvent 2 may be tetrahydrofuran, acetone, acetonitrile, ethyl acetate, etc.
[0138] (3) subjecting the modified polyamic acid to an imidization reaction to obtain the modified polyimide binder.
[0139] The reaction process of this step is as follows:
[0140]
[0141] According to a specific embodiment of the present invention, the modified polyamic acid is subjected to imidization reaction under the action of a dehydrating agent and a catalyst.
[0142] Specifically, the molar ratio of the modified polyamic acid to the dehydrating agent and the catalyst is 1:(1.8-1.9):(0.8-0.9), which can be selected according to actual needs. As some specific examples, the molar ratio of the modified polyamic acid to the dehydrating agent and the catalyst can be 1:1.8:0.8, 1:1.8:0.9, 1:1.9:0.8, 1:1.9:0.9, etc.
[0143] Specifically, the dehydrating agent includes but is not limited to acetic anhydride, acetyl chloride, trifluoroacetic anhydride. The catalyst includes but is not limited to triethylamine and pyridine.
[0144] Specifically, the temperature and time of the imidization reaction are not particularly limited, and those skilled in the art can select according to actual needs. As some specific examples, the temperature of the imidization reaction is 50-100° C., such as 50° C., 60° C., 70° C., 80° C., 90° C., 100° C., etc., preferably 50-80° C. The time of the imidization reaction can be 4-24h, such as 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, etc., preferably 4-12h.
[0145] According to an embodiment of the present invention, a third aspect of the present invention provides an electrode sheet, wherein the electrode sheet comprises the modified polyimide binder described in the first aspect or the modified polyimide binder obtained according to the method described in the second aspect.
[0146] According to a specific embodiment of the present invention, the preparation of the electrode sheet is not particularly limited, and those skilled in the art can select according to actual needs. As some specific examples, it can specifically include: under nitrogen protection, weighing a binder (modified polyimide powder), a negative electrode active material, conductive carbon black and solvent 3 (such as N-methylpyrrolidone, NMP), placing them in a high-speed stirring disperser and stirring and mixing them evenly to obtain a negative electrode slurry. Using a scraper, the negative electrode slurry is coated on a copper foil, and then placed at 70-100°C to dry for 60-120 minutes to obtain a negative electrode sheet.
[0147] According to a specific embodiment of the present invention, the negative electrode active material is carbon powder, silicon powder, tin powder or alloy powder containing silicon or tin, preferably silicon powder or silicon alloy powder.
[0148] According to a specific embodiment of the present invention, the mass ratio of the binder, the negative electrode active material and the conductive carbon black is (1-4): (90-95): (1-9), for example, 1:90:9, 1:91:8, 2:92:6, 3:95:2, 4:95:1, etc., preferably 3:92:5.
[0149] According to a specific embodiment of the present invention, the solid content of the negative electrode slurry is not particularly limited. Those skilled in the art can choose according to actual needs. As some specific examples, 40%-50% can be selected, such as 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, preferably 45%.
[0150] According to a specific embodiment of the present invention, the coating thickness of the negative electrode slurry is not particularly limited, and those skilled in the art can select it according to actual needs. As some specific examples, 50-60 μm can be selected, such as 50 μm, 51 μm, 52 μm, 53 μm, 54 μm, 55 μm, 56 μm, 57 μm, 58 μm, 59 μm, 60 μm, etc., preferably 55 μm.
[0151] According to an embodiment of the present invention, a fourth aspect of the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the electrode sheet described in the third aspect.
[0152] According to a specific embodiment of the present invention, the battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte conducts ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet to prevent the positive and negative electrodes from short-circuiting while allowing ions to pass through.
[0153] According to a specific embodiment of the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active coating disposed on at least one side surface of the positive electrode current collector, and the positive electrode active coating includes a positive electrode active material.
[0154] According to a specific embodiment of the present invention, the positive electrode current collector may include a metal foil or a composite positive electrode current collector. For example, the metal foil may be aluminum foil. The composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the surface of the polymer material base. For example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene, PP; polyethylene terephthalate, PET; polybutylene terephthalate, PBT and other substrates).
[0155] According to a specific embodiment of the present invention, the positive electrode active coating layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0156] According to a specific embodiment of the present invention, the positive electrode active coating may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin.
[0157] According to a specific embodiment of the present invention, the positive electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, and the binder are dispersed in a solvent 4 (such as N-methylpyrrolidone, NMP) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0158] According to a specific embodiment of the present invention, the electrode sheet described in the third aspect can be used as a negative electrode sheet in a lithium-ion battery.
[0159] According to a specific embodiment of the present invention, the present invention has no particular limitation on the type of the isolation membrane, and any known porous structure isolation membrane with good chemical stability and mechanical stability can be selected. In some embodiments of the present invention, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride.
[0160] According to a specific embodiment of the present invention, the positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly through a winding process or a lamination process.
[0161] According to a specific embodiment of the present invention, the battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0162] According to a specific embodiment of the present invention, the outer packaging of the battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and as the plastic, polypropylene, polybutylene terephthalate, polybutylene succinate, etc. can be listed.
[0163] The scheme of the present invention will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.
[0164] Example 1
[0165]
[0166] FTIR(KBr):ν=3005,1776,1714,1608,1458,1373,1240,1105,968,874,725m -1 .
[0167] (1) Under nitrogen protection, 10.7208 g (0.0367 mol) of 1,3-bis(4-aminophenoxy)benzene (TPE-R) was dissolved in 270 mL of N-methylpyrrolidone. After the mixture was completely dissolved, 19.2792 g (0.0370 mol) of bisphenol A diether dianhydride (BPADA) was added. The BPADA was added three times, each time with an interval of 30 min. After reacting for 12 h at 10° C., 300 g of a polyamic acid solution with a solid content of 10% was obtained, which was stored at 5° C. for later use.
[0168] The structure of polyamic acid is as follows:
[0169]
[0170] FTIR(KBr):ν=3261,2989,1720,1661,1542,1499,1240,1104,873,833m -1 .
[0171] (2) Under nitrogen protection, 4.5676 g (0.0280 mol) of 5-carboxylic acid benzotriazole was dissolved in 200 mL of acetone. After complete dissolution, 4.9942 g (0.0308 mol) of N,N'-carbonyldiimidazole was added. After stirring at room temperature for 5 h, 3.2537 g (0.0280 mol) of 1,6-hexanediamine was added. The mixture was stirred at room temperature for 5 h. The reaction solution was dried over anhydrous sodium sulfate, the solvent acetone was removed by rotary evaporation, and 5.6344 g of the product intermediate was obtained by column chromatography with a yield of 77%;
[0172] The intermediate structure is as follows:
[0173]
[0174] FTIR(KBr):ν=3075,2918,2850,1739,1605,1458,13378,1067,850,730m -1 .
[0175] (3) Under nitrogen protection, 0.9684 g (0.0081 mol) of thionyl chloride was added to 300 g of the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 6 h. Then, 1.9339 g (0.0074 mol) of the intermediate obtained in step (2) was added, and the mixture was stirred at room temperature for 5 h. The excess thionyl chloride was removed by rotary evaporation to obtain a polyamic acid solution grafted with benzotriazole groups;
[0176] The structure of polyamic acid grafted with benzotriazole groups is as follows:
[0177]
[0178] FTIR(KBr):ν=3250,2905,1730,1659,1605,1550,1460,1250,1110,863,732m -1 .
[0179] (4) Under nitrogen protection, 6.7787 g (0.0664 mol) of acetic anhydride and 2.3351 g (0.0295 mol) of pyridine were added to the modified polyamic acid solution obtained in step (3), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaking machine filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The obtained solid powder was washed and filtered with pure water for 6 times, and then placed in a 100° C. forced air drying oven to dry the water, thereby obtaining 24.5602 g of a polyimide powder ① grafted with benzotriazole groups.
[0180] Preparation of negative electrode for lithium battery:
[0181] Under nitrogen protection, 3 parts of binder (modified polyimide powder ①), 92 parts of silicon powder, and 5 parts of conductive carbon black were weighed by mass and placed in 100 parts of N-methylpyrrolidone (NMP), and the materials were stirred and mixed evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. The negative electrode slurry was coated on copper foil with a scraper, and then placed in an oven at 100℃ for 120min to dry, and then rolled to obtain negative electrode sheet ①.
[0182] Example 2
[0183]
[0184] FTIR(KBr):ν=2998,1770,1710,1610,1440,1365,1238,1110,994,865,743m -1 .
[0185] (1) Under nitrogen protection, 10.7208 g (0.0367 mol) of 1,3-bis(4-aminophenoxy)benzene (TPE-R) was dissolved in 270 mL of N-methylpyrrolidone. After complete dissolution, 19.2792 g (0.0370 mol) of BPADA was added. The BPADA was added three times, each time with an interval of 30 min. After reacting at 10° C. for 12 h, 300 g of a polyamic acid solution with a solid content of 10% was obtained, which was stored at 5° C. for later use;
[0186] (2) Under nitrogen protection, 4.5676 g (0.0280 mol) of 5-carboxylic acid benzotriazole was dissolved in 200 mL of acetone. After complete dissolution, 4.9942 g (0.0308 mol) of N,N'-carbonyldiimidazole was added. After stirring at room temperature for 5 h, 4.8247 g (0.0280 mol) of decanediamine was added. The mixture was stirred at room temperature for 5 h. The reaction solution was dried over anhydrous sodium sulfate, the solvent acetone was removed by rotary evaporation, and 6.6659 g of the product intermediate was obtained by column chromatography with a yield of 75%;
[0187] (3) Under nitrogen protection, 0.9684 g (0.0081 mol) of thionyl chloride was added to 300 g of the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 6 h. Then, 2.3490 g (0.0074 mol) of the intermediate obtained in step (2) was added, and the mixture was stirred at room temperature for 5 h. The excess thionyl chloride was removed by rotary evaporation to obtain a polyamic acid solution grafted with benzotriazole groups;
[0188] (4) Under nitrogen protection, 6.7787 g (0.0664 mol) of acetic anhydride and 2.3351 g (0.0295 mol) of pyridine were added to the modified polyamic acid solution obtained in step (3), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaker filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The solid powder was washed and filtered 6 times with pure water, and then placed in a 100° C. air drying oven to dry the water, to obtain 25.2137 g of a polyimide powder modified by grafting of benzotriazole groups②.
[0189] Preparation of negative electrode for lithium battery:
[0190] Under nitrogen protection, weigh 3 parts of binder (modified polyimide powder ②), 92 parts of silicon powder, and 5 parts of conductive carbon black in 100 parts of NMP, stir and mix the materials evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. Use a scraper to coat the negative electrode slurry on copper foil, then place it in an oven at 100℃ and dry it for 120min, and roll it to obtain a negative electrode sheet ②.
[0191] Example 3
[0192]
[0193] FTIR(KBr):ν=3010,1775,1718,1609,1460,1375,1293,1079,902,734m -1 .
[0194] (1) Under nitrogen protection, 10.7208 g (0.0367 mol) of 1,3-bis(4-aminophenoxy)benzene (TPE-R) was dissolved in 270 mL of N-methylpyrrolidone. After complete dissolution, 19.2792 g (0.0370 mol) of BPADA was added. The BPADA was added three times, each time with an interval of 30 min. After reacting at 10° C. for 12 h, 300 g of a polyamic acid solution with a solid content of 10% was obtained, which was stored at 5° C. for later use;
[0195] (2) Under nitrogen protection, 4.9605 g (0.0280 mol) of 2-(1H-benzo[d][1,2,3]triazol-6-yl)acetic acid was dissolved in 200 mL of acetone. After complete dissolution, 4.9942 g (0.0308 mol) of N,N'-carbonyldiimidazole was added. After stirring at room temperature for 5 h, 3.2537 g (0.0280 mol) of 1,6-hexanediamine was added. The mixture was stirred at room temperature for 5 h. The reaction solution was dried over anhydrous sodium sulfate, the solvent acetone was removed by rotary evaporation, and 6.0910 g of the product intermediate was obtained by column chromatography with a yield of 79%.
[0196] (3) Under nitrogen protection, 0.9684 g (0.0081 mol) of thionyl chloride was added to 300 g of the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 6 h. Then, 2.0377 g (0.0074 mol) of the intermediate obtained in step (2) was added, and the mixture was stirred at room temperature for 5 h. The excess thionyl chloride was removed by rotary evaporation to obtain a polyamic acid solution grafted with benzotriazole groups;
[0197] (4) Under nitrogen protection, 6.7787 g (0.0664 mol) of acetic anhydride and 2.3351 g (0.0295 mol) of pyridine were added to the modified polyamic acid solution obtained in step (3), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaking machine filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The obtained solid powder was washed and filtered with pure water for 6 times, and then placed in a 100° C. forced air drying oven to dry the water, to obtain 24.8314 g of a polyimide powder modified by grafting of benzotriazole groups③.
[0198] Preparation of negative electrode for lithium battery:
[0199] Under nitrogen protection, 3 parts of binder (modified polyimide powder ③), 92 parts of silicon powder, and 5 parts of conductive carbon black were weighed by mass and placed in 100 parts of NMP, and the materials were stirred and mixed evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. The negative electrode slurry was coated on copper foil using a scraper, and then placed in an oven at 100℃ for 120min and rolled to obtain a negative electrode sheet ③.
[0200] Example 4
[0201]
[0202] FTIR(KBr):ν=3002,1765,1708,1607,1454,1366,1252,1135,968,845,742m -1 .
[0203] (1) Under nitrogen protection, 14.4802 g (0.0495 mol) of 1,3-bis(4-aminophenoxy)benzene (TPE-R) was dissolved in 270 mL of N-methylpyrrolidone. After it was completely dissolved, 15.5198 g (0.0500 mol) of 4,4'-biphenyl ether dianhydride (ODPA) was added. ODPA was added three times, each time with an interval of 30 min. After reacting for 12 h at 10° C., 300 g of a polyamic acid solution with a solid content of 10% was obtained, which was stored at 5° C. for later use.
[0204] (2) Under nitrogen protection, 4.5676 g (0.0280 mol) of 5-carboxylic acid benzotriazole was dissolved in 200 mL of acetone. After complete dissolution, 4.9942 g (0.0308 mol) of N,N'-carbonyldiimidazole was added. After stirring at room temperature for 5 h, 3.2537 g (0.0280 mol) of 1,6-hexanediamine was added. The mixture was stirred at room temperature for 5 h. The reaction solution was dried over anhydrous sodium sulfate, the solvent acetone was removed by rotary evaporation, and 5.6344 g of the product intermediate was obtained by column chromatography with a yield of 77%;
[0205] (3) Under nitrogen protection, 1.3087 g (0.0110 mol) of thionyl chloride was added to 300 g of the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 6 h. Then, 2.6134 g (0.0100 mol) of the intermediate obtained in step (2) was added, and the mixture was stirred at room temperature for 5 h. The excess thionyl chloride was removed by rotary evaporation to obtain a polyamic acid solution grafted with benzotriazole groups;
[0206] (4) Under nitrogen protection, 9.1473 g (0.0896 mol) of acetic anhydride and 3.1482 g (0.0398 mol) of pyridine were added to the modified polyamic acid solution obtained in step (3), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaking machine filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The solid powder was washed and filtered with pure water for 6 times, and then placed in a 100° C. air drying oven to dry the water, to obtain 24.7330 g of a polyimide powder modified by grafting of benzotriazole groups④.
[0207] Preparation of negative electrode for lithium battery:
[0208] Under nitrogen protection, 3 parts of binder (modified polyimide powder ④), 92 parts of silicon powder, and 5 parts of conductive carbon black were weighed by mass and placed in 100 parts of NMP, and the materials were stirred and mixed evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. The negative electrode slurry was coated on copper foil using a scraper, and then placed in an oven at 100℃ for 120min and rolled to obtain a negative electrode sheet ④.
[0209] Example 5
[0210]
[0211] FTIR(KBr):ν=3005,1776,1714,1615,1449,1370,1240,1105,970,863,732m -1 .
[0212] (1) Under nitrogen protection, 8.2751 g (0.0413 mol) of 3,4'-diaminodiphenyl ether (3,4'-ODA) was dissolved in 270 mL of N-methylpyrrolidone. After the mixture was completely dissolved, 21.7249 g (0.0417 mol) of BPADA was added. The BPADA was added three times, each time with an interval of 30 min. After reacting for 12 h at 10° C., 300 g of a polyamic acid solution with a solid content of 10% was obtained, which was stored at 5° C. for later use.
[0213] (2) Under nitrogen protection, 4.5676 g (0.0280 mol) of 5-carboxylic acid benzotriazole was dissolved in 200 mL of acetone. After complete dissolution, 4.9942 g (0.0308 mol) of N,N'-carbonyldiimidazole was added. After stirring at room temperature for 5 h, 3.2537 g (0.0280 mol) of 1,6-hexanediamine was added. The mixture was stirred at room temperature for 5 h. The reaction solution was dried over anhydrous sodium sulfate, the solvent acetone was removed by rotary evaporation, and 5.6344 g of the product intermediate was obtained by column chromatography with a yield of 77%.
[0214] (3) Under nitrogen protection, 1.0862 g (0.0091 mol) of thionyl chloride was added to 300 g of the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 6 h. Then, 2.1691 g (0.0083 mol) of the intermediate obtained in step (2) was added, and the mixture was stirred at room temperature for 5 h. The excess thionyl chloride was removed by rotary evaporation to obtain a polyamic acid solution grafted with benzotriazole groups;
[0215] (4) Under nitrogen protection, 7.6490 g (0.0749 mol) of acetic anhydride and 2.6340 g (0.0333 mol) of pyridine were added to the modified polyamic acid solution obtained in step (3), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaking machine filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The solid powder was washed and filtered 6 times with pure water, and then placed in a 100° C. air drying oven to dry the water, to obtain 24.8705 g of a polyimide powder modified by grafting of benzotriazole groups⑤.
[0216] Preparation of negative electrode for lithium battery:
[0217] Under nitrogen protection, 3 parts of binder (modified polyimide powder ⑤), 92 parts of silicon powder, and 5 parts of conductive carbon black were weighed by mass and placed in 100 parts of NMP, and the materials were stirred and mixed evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. The negative electrode slurry was coated on copper foil using a scraper, and then placed in an oven at 100°C for 120 minutes, and rolled to obtain a negative electrode sheet ⑤.
[0218] Comparative Example 1
[0219]
[0220] FTIR(KBr):ν=3005,1770,1720,1500,1380,1240,1105,954,844,730m -1 .
[0221] (1) Under nitrogen protection, 10.7208 g (0.0367 mol) of 1,3-bis(4-aminophenoxy)benzene (TPE-R) was dissolved in 270 mL of N-methylpyrrolidone. After the mixture was completely dissolved, 19.2792 g (0.0370 mol) of BPADA was added. The BPADA was added three times, each time with an interval of 30 min. After reacting for 12 h at 10° C., 300 g of a polyamic acid solution with a solid content of 10% was obtained, which was stored at 5° C. for later use.
[0222] (2) Under nitrogen protection, 3.4194 g (0.0280 mol) of benzoic acid was dissolved in 200 mL of acetone. After complete dissolution, 4.9942 g (0.0308 mol) of N,N'-carbonyldiimidazole was added. After stirring at room temperature for 5 h, 3.2537 g (0.0280 mol) of 1,6-hexanediamine was added. The mixture was stirred at room temperature for 5 h. The reaction solution was dried over anhydrous sodium sulfate, the solvent acetone was removed by rotary evaporation, and 4.9969 g of the product intermediate was obtained by column chromatography with a yield of 81%;
[0223] (3) Under nitrogen protection, 0.9684 g (0.0081 mol) of thionyl chloride was added to 300 g of the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 6 h. Then, 1.6304 g (0.0074 mol) of the intermediate obtained in step (2) was added, and the mixture was stirred at room temperature for 5 h. The excess thionyl chloride was removed by rotary evaporation to obtain a polyamic acid solution grafted with benzotriazole groups;
[0224] (4) Under nitrogen protection, 6.7787 g (0.0664 mol) of acetic anhydride and 2.3351 g (0.0295 mol) of pyridine were added to the modified polyamic acid solution obtained in step (3), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaking machine filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The obtained solid powder was washed and filtered with pure water for 6 times, and then placed in a 100° C. air drying oven to dry the water, to obtain 24.7316 g of graft-modified polyimide powder⑥.
[0225] Preparation of negative electrode for lithium battery:
[0226] Under nitrogen protection, 3 parts of binder (modified polyimide powder ⑥), 92 parts of silicon powder, and 5 parts of conductive carbon black were weighed by weight and placed in 100 parts of NMP, and the materials were stirred and mixed evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. The negative electrode slurry was coated on copper foil using a scraper, and then placed in an oven at 100°C for 120 minutes, and rolled to obtain a negative electrode sheet ⑥.
[0227] Comparative Example 2
[0228]
[0229] FTIR(KBr):ν=3005,1776,1714,1373,1260,1100,960,831,740m -1 .
[0230] (1) Under nitrogen protection, 10.7208 g (0.0367 mol) of 1,3-bis(4-aminophenoxy)benzene (TPE-R) was dissolved in 270 mL of N-methylpyrrolidone. After the mixture was completely dissolved, 19.2792 g (0.0370 mol) of BPADA was added. The BPADA was added three times, each time with an interval of 30 min. After reacting for 12 h at 10° C., 300 g of a polyamic acid solution with a solid content of 10% was obtained.
[0231] (2) Under nitrogen protection, 7.5342 g (0.0738 mol) of acetic anhydride and 2.9188 g (0.0369 mol) of pyridine were added to the polyamic acid solution obtained in step (1), and the mixture was stirred at 60° C. for 12 h. The product was pulped using a wall breaking machine filled with pure water to obtain a solid-liquid mixture, and then filtered under reduced pressure using a Buchner funnel to separate a solid powder. The obtained solid powder was washed and filtered 6 times with pure water, and then placed in a 100° C. air drying oven to dry the water to obtain 23.6827 g of polyimide powder⑦.
[0232] Preparation of negative electrode for lithium battery:
[0233] Under nitrogen protection, 3 parts of binder (polyimide powder⑦), 92 parts of silicon powder, and 5 parts of conductive carbon black were weighed by mass and placed in 100 parts of NMP, and the materials were stirred and mixed evenly at a stirring speed of 3000r / min to obtain negative electrode slurry. The negative electrode slurry was coated on copper foil using a scraper, and then placed in an oven at 100℃ for 120min and rolled to obtain a negative electrode sheet⑦.
[0234] Battery preparation: The rolled negative electrode sheets ①-⑦ and the positive electrode sheet were cut into 14 mm diameter discs using a punching machine. 2 O<0.01ppm, O 2 <0.01ppm) assemble CR2032 button batteries, assemble the negative electrode shell, negative electrode sheet, diaphragm, positive electrode sheet, nickel foam, spring sheet, and positive electrode shell in sequence, and drip 1mL of electrolyte at both ends of the diaphragm. The electrolyte is 1.0mol / L LiPF 6 The assembled battery was dissolved in a mixed solution of EC and DMC (EC:DMC=1:1, volume ratio), and the packaging pressure was 75MPa. After standing for 24h, the corresponding electrochemical performance test was carried out.
[0235] Test Case
[0236] The following tests were performed on the polyimide binders ①-⑦, negative electrode sheets ①-⑦ and the corresponding assembled batteries ①-⑦ prepared in Examples 1-5 and Comparative Examples 1-2 respectively:
[0237] (1) Molecular weight Mw of polyimide material;
[0238] (2) Glass transition temperature Tg of polyimide material;
[0239] (3) Thermal weight loss temperature of polyimide material:
[0240] The temperature at which the thermal weight loss reaches 5 wt% in an inert gas atmosphere;
[0241] (4) Lithium battery negative electrode peel strength test:
[0242] Use INSTRON tensile testing machine to test the peel strength. Use the tensile testing machine to test the 180° peeling of the pole piece. The peel strength test uses a sample made of 2.5cm wide and about 10cm long, and the pulling speed is 2mm / s.
[0243] (5) Battery cycle life test:
[0244] Carry out cycle test at 25℃ for N cycles, record the battery discharge capacity of the Nth time and the first time, and calculate the discharge retention rate.
[0245] Discharge retention rate = Nth discharge capacity / 1st discharge capacity*100%. When the cycle discharge retention rate reaches 80%, the cycle test is terminated and the number of cycles is recorded.
[0246] (6) Battery expansion rate:
[0247] After 100 cycles of charge and discharge, the battery is fully charged or fully discharged, respectively, to obtain the negative electrode sheets in the charge and discharge states, and the thickness difference between the two is measured.
[0248] Test Results
[0249] 1. The molecular weight test and thermal stability test results of the polyimide adhesive are shown in Table 1.
[0250] Examples 1-5 and Comparative Example 1 are polyimides modified by grafting with flexible side chains, and Comparative Example 2 is a polyimide without grafting with side chains. It can be seen from the glass ring transition temperature test data that the Tg of the polyimide modified by grafting with flexible side chains is lower than that of the polyimide without grafting modification, indicating that after the polyimide is grafted with flexible side chains, its flexibility is significantly improved and the chain segments are easier to move; it can be seen from the thermal weight loss temperature data that even after the flexible side chain grafting modification, the temperature of thermal weight loss of 5% of the obtained polyimide is above 350°C, indicating that the grafted polyimide still has good thermal stability.
[0251] 2. The test results of negative electrode are shown in Table 2.
[0252] Examples 1-5 are polyimides grafted with benzotriazole groups, Comparative Example 1 is a grafted polyimide, but the modified group does not contain benzotriazole groups, and Comparative Example 2 is an unmodified polyimide. The benzotriazole groups can form covalent bonds and coordination bonds with copper atoms, alternating with each other to form chain polymers. Therefore, the coating peel strength of Examples 1-5 is significantly greater than that of Comparative Examples 1 and 2.
[0253] 3. The test results of the electrochemical properties of lithium-ion batteries are shown in Table 3.
[0254] Examples 1-5 are polyimides grafted with benzotriazole groups, Comparative Example 1 is a grafted polyimide, but the modified group does not contain a benzotriazole group, and Comparative Example 2 is an unmodified polyimide. The introduction of the benzotriazole group improves the bonding strength between the negative electrode coating and the electrode sheet, increases the flexibility of the silicon-based negative electrode, and makes the silicon-based negative electrode more stable. The cycle life and volume expansion resistance of the prepared battery are better than those of the comparative example.
[0255] Table 1
[0256]
[0257] Table 2
[0258] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Peel strength / N / m 19.86 21.47 20.53 18.62 18.87 14.31 10.05
[0259] Table 3
[0260]
[0261]
[0262] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0263] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A modified polyimide binder, characterized in that: The modified polyimide binder has a structure represented by formula (I) or a stereoisomer, nitrogen oxide, hydrate, solvate or salt thereof; Wherein, R1 is selected from aromatic groups or fluorine-containing aromatic groups containing ether bonds, ester groups and / or carbonyl groups; R2 is selected from aromatic groups containing ether bonds and / or sulfone groups; R3 is selected from C1-C 10 Alkylene, C3-C 10 At least one of cycloalkyl groups; R4 is selected from a single bond or a C1-C5 alkylene group; x:y=(40-450):(5-100).
2. The modified polyimide adhesive according to claim 1, characterized in that: R1 is selected from 3. The modified polyimide adhesive according to claim 1, characterized in that: R2 is selected from 4. The modified polyimide adhesive according to claim 1, characterized in that: R3 is selected from C1-C 10 At least one of an alkylene group and a C4-C6 cycloalkyl group; Optionally, R3 is selected from C1-C 10 Alkylene, C4 cycloalkyl, 5. The modified polyimide adhesive according to claim 1, characterized in that: R4 is selected from a single bond or a C1-C2 alkylene group.
6. A method for preparing the modified polyimide binder according to any one of claims 1 to 5, characterized in that: include: Performing a first mixing treatment on the dianhydride monomer and the diamine monomer to obtain a polyamic acid; performing a second mixing process on the polyamic acid and the intermediate to obtain a modified polyamic acid; The modified polyamic acid is subjected to imidization reaction to obtain the modified polyimide binder; Wherein, the dianhydride monomer has a structure shown in formula (II): R1 is as claimed in any one of claims 1 or 2; The diamine monomer has a structure shown in formula (III): H2N-R2-NH2 formula (III), R2 as described in any one of claims 1 or 3; The intermediate has a structure shown in formula (IV): R3, R4 are as described in any one of claims 1, 4 or 5.
7. The method according to claim 6, characterized in that The molar ratio of the dianhydride monomer to the diamine monomer is (0.9-1.01):1; Optionally, the dianhydride monomer is selected from at least one of bisphenol A type diether dianhydride, p-phenylene-diphenyltrimethylol dianhydride, 3,3',4,4'-dibenzophenone tetracarboxylic dianhydride, 4,4'-biphenyl ether dianhydride, hexafluoro dianhydride, diethylene glycol (4-tricarboxylic anhydride), and 5-isobenzofurancarboxylic acid 1,3-dihydro-1,3-dioxy-5,5'-[(1-methylethylidene)di-4,1-phenylene] ester; Optionally, the dianhydride monomer is selected from at least one of 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 4,4'-diaminophenyl sulfone, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)diphenyl sulfone, and 2,2-bis[4-(4-aminophenoxy)phenyl]propane; Optionally, the temperature of the first mixing treatment is 0-20°C, preferably 5-10°C; Optionally, the first mixing treatment is performed for 2-24 hours, preferably 6-18 hours.
8. The method according to claim 6, characterized in that The molar ratio of the polyamic acid to the intermediate is 1:(0.1-0.2); Optionally, the temperature of the second mixing treatment is 0-100°C, preferably 20-50°C; Optionally, the second mixing treatment is performed for 1-24 hours, preferably 2-6 hours.
9. The method according to claim 6, characterized in that The method further comprises: The polyamic acid and thionyl chloride are subjected to a third mixing treatment to obtain an intermediate compound, and the intermediate compound is mixed with the intermediate to obtain the modified polyamic acid; Optionally, the molar ratio of the intermediate to thionyl chloride is 1:(1-1.1); Optionally, the temperature of the third mixing treatment is 50-100°C, preferably 50-80°C; Optionally, the third mixing treatment lasts for 2-24 hours, preferably 1-5 hours.
10. The method according to claim 6, characterized in that The modified polyamic acid is subjected to imidization reaction under the action of a dehydrating agent and a catalyst; Optionally, the molar ratio of the modified polyamic acid to the dehydrating agent and the catalyst is 1:(1.8-1.9):(0.8-0.9); Optionally, the dehydrating agent is selected from at least one of acetic anhydride, acetyl chloride and trifluoroacetic anhydride; Optionally, the catalyst is selected from at least one of triethylamine and pyridine; Optionally, the temperature of the imidization reaction is 50-100°C, preferably 50-80°C; Optionally, the imidization reaction time is 4-24 hours, preferably 4-12 hours.
11. The method according to claim 6, characterized in that The method further comprises preparing the intermediate; The preparation of the intermediate comprises: performing a fourth mixing treatment on compound 1, compound 2 and a condensing agent to obtain the intermediate; Wherein, the compound 1 has a structure shown in formula (V): H2N-R3-NH2 formula (V), R3 as described in any one of claims 1 or 4; The compound 2 has a structure shown in formula (VI): R4 as claimed in any one of claims 1 or 5; Optionally, the molar ratio of compound 1, compound 2 and condensing agent is 1:1:(1-1.1); Optionally, the compound 1 is selected from at least one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,3-diaminocyclobutylamine, 2-methyl-1,3-propylenediamine, 1,3-diaminopentane, 1,4-butylenediamine, 1,5-pentanediamine, 2-methyl-1,5-pentanediamine, 4-aminomethylcyclohexylamine, 2-aminomethylcyclohexylamine, 1,3-cyclohexanedimethylamine, hexanediamine, 1,7-diaminoheptane, 1,8-octanediamine, 1,9-nonanediamine, and decanediamine; Optionally, the compound 2 is selected from at least one of 5-benzotriazole carboxylate, 2-(1H-benzo[d][1,2,3]triazol-6-yl)acetic acid, 2-(1H-benzo[d][1,2,3]triazol-6-yl)propionic acid, 2-(1H-benzo[d][1,2,3]triazol-6-yl)isopropionic acid, 2-(1H-benzo[d][1,2,3]triazol-7-yl)acetic acid, and 4-benzotriazole carboxylate; Optionally, the condensing agent is selected from at least one of dicyclohexylcarbodiimide, diisopropylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide, carbonyldiimidazole, thionyl chloride, and N,N'-carbonyldiimidazole; Optionally, the temperature of the fourth mixing treatment is 0-100°C, preferably 20-50°C; Optionally, the fourth mixing treatment is performed for 1-24 hours, preferably 1-5 hours.
12. An electrode sheet, characterized in that: The electrode sheet comprises the modified polyimide binder according to any one of claims 1 to 5 or the modified polyimide binder obtained by the method according to any one of claims 6 to 11.
13. A lithium ion battery, characterized in that: The lithium-ion battery comprises the electrode sheet according to claim 12.
Citation Information
Cited By
Modified polyimide as well as preparation method and application thereof
CN120944107A
Polyol-modified soluble polyimide adhesive and preparation method therefor
WO2026179882A1
Polyimide binder, electrode sheet, battery, battery pack, and electric device