Preparation method of porous coating textile and porous coating textile
By coating water-based base slurry, water-absorbent resin particles and surface slurry on textiles, the expansion of water-absorbent resin particles is used to form a porous structure, and the problem of flat surface of existing foam printed textiles is solved, thus achieving the formation of a porous coating, providing Decorative and protective effects.
Patent Information
- Application Number
- CN202411037499.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The bubble cell diameter of existing foam printed textiles is small, with flat surfaces and lacks a three-dimensional structure, making it difficult to provide a variety of decorative appearances and protective effects.
The water-based base slurry, water-absorbent resin particles and water-based surface slurry are successively coated on the textiles, and the porous structure is formed by the water-absorbent expansion of the water-absorbent resin particles to form a composite coating to achieve a porous coating with uneven surfaces.
The uneven porous structure of the textile surface is realized, providing different decorative appearances and enhanced protection, while ensuring the integrity and adhesion of the composite coating.
Smart Images

Figure CN118932733A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textiles, and relates to a preparation method of a porous coated textile and the porous coated textile. Background Art
[0002] In textiles, such as shoe materials, printing and forming prints have good aesthetic decoration and protective effects. Foaming technology can be used to form foaming prints. However, the diameter of the foaming pores in foaming prints is relatively small, generally at the micron level, and the surface is flat without an uneven appearance.
[0003] Therefore, it is urgent to provide a foaming printing with a three-dimensional structure to provide different decorative appearances and protective effects for textiles. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a porous coated textile and the porous coated textile.
[0005] The technical solution of the present invention is as follows:
[0006] A method for preparing a porous coated textile comprises the following steps:
[0007] Applying a water-based base paste on the textile to form a base paste layer;
[0008] Laying water-absorbing resin particles on the base slurry layer and drying for the first time to obtain an intermediate layer;
[0009] Applying water-based paste on the intermediate layer and drying it for a second time to obtain a pre-composite layer;
[0010] The pre-composite layer is soaked in water, the expanded water-absorbing resin particles are removed, and the porous coated textile is obtained by drying for a third time.
[0011] Preferably, the method of applying the water-based primer is screen printing.
[0012] Preferably, the area on the textile coated with the aqueous base slurry is a single-layer mesh structure or a single-layer cloth structure with mesh holes, and the mesh holes of the mesh structure and the mesh holes of the single-layer cloth structure have sizes of 0.5-5 mm, respectively.
[0013] More preferably, the size of the water absorbing resin particles does not exceed the mesh size.
[0014] Further preferably, the size of the water-absorbing resin particles does not exceed 1 / 2 of the mesh size.
[0015] Preferably, the method of applying the aqueous paste is hollow screen printing.
[0016] More preferably, the height of the hollow screen is not less than the size of the water-absorbing resin particles.
[0017] Preferably, the pre-composite layer is immersed in water for 0.5-12 hours at a temperature of 5-40°C.
[0018] Preferably, the removing of the expanded water-absorbing resin particles is removing from meshes of the textile.
[0019] A porous coated textile is prepared by the method for preparing a porous coated textile described in any one of the above embodiments.
[0020] The beneficial effects of the present invention are:
[0021] (1) The present invention forms a composite coating covering water-absorbent resin particles on the surface of the textile by coating a water-based base slurry, water-absorbent resin particles and a water-based surface slurry on the textile. The water-absorbent resin particles have a high swelling property when absorbing water. After the water-absorbent resin particles absorb water and swell and are removed, a porous structure is formed at the swelling position, and the composite coating forms a porous coating with an uneven surface.
[0022] (2) In the present invention, the water-absorbing resin particles can be removed from the outer surface of the composite coating or from the mesh of the textile. When removed from the mesh of the textile, the porous structure of the outer surface of the composite coating will not be destroyed. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a front view of the porous coated textile of Example 1.
[0024] Figure 2 This is a back view of the porous coated textile of Example 1.
[0025] Figure 3 This is a front view of the porous coated textile of Example 5.
[0026] Figure 4 This is a back view of the porous coated textile of Example 5. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0028] In one aspect, the present invention provides a method for preparing a porous coated textile, comprising the following steps:
[0029] Applying a water-based base paste on the textile to form a base paste layer;
[0030] Laying water-absorbing resin particles on the base slurry layer and drying for the first time to obtain an intermediate layer;
[0031] Applying water-based paste on the middle layer and drying it for a second time to obtain a pre-composite layer;
[0032] The pre-composite layer is immersed in water to remove the expanded water-absorbing resin particles, and then dried for a third time to obtain the porous coated textile of the present invention.
[0033] The present invention forms a composite coating covering water-absorbent resin particles on the surface of the textile by sequentially arranging a base slurry layer, a water-absorbent resin particle layer and a surface slurry layer on the surface of the textile. After the water-absorbent resin particles absorb water and swell and are removed, the cavity formed inside the composite coating is a porous structure. Due to the high-multiple expansion of the water-absorbent resin particles, the outer surface of the composite coating forms an uneven structure, thereby achieving the purpose of the present invention-forming a porous coating with an uneven outer surface on the textile.
[0034] In a preferred embodiment of the present invention, the method of applying the aqueous primer is screen printing, and the aqueous primer cannot be dried and solidified after application, or does not need to be heated. After the aqueous primer is applied, a layer of water-absorbing particle resin can be directly laid on it. In the present invention, there are four main purposes for setting the aqueous primer: (1) as a bottom layer of water-absorbing resin particles, supporting the water-absorbing resin particles and preventing the water-absorbing resin particles from falling off from the mesh of the textile; (2) adsorbing and fixing the water-absorbing resin particles on the surface of the textile; (3) making the surface paste have a good bonding force with the textile, and forming a composite coating with good adhesion including the bottom layer, water-absorbing resin particles and the surface layer on the surface of the textile; (4) the thickness of the aqueous primer is relatively thin, 5μm-100μm, and this thickness of the aqueous primer can be achieved by screen printing, which is conducive to the detachment of the expanded water-absorbing resin particles from the mesh through the primer layer.
[0035] In the present invention, the source of the aqueous slurry is not particularly limited, and can be a commonly used aqueous slurry for textiles, can be directly obtained from the market, or can be prepared according to the prior art. Taking the aqueous PU slurry as an example, the composition of an aqueous slurry can be as follows: 70-85wt% aqueous PU resin (concentration is 20-50wt%), 5-12wt% slow-drying agent (such as ethylene glycol monomethyl ether, propylene glycol, etc.), 0.3-0.7wt% defoamer, 0.1-0.5wt% leveling agent, 0.5-2.0wt% thickener and 2-4wt% cross-linking agent (such as isocyanate cross-linking agent).
[0036] In a preferred embodiment of the present invention, the area on the textile coated with water-based slurry is a single-layer mesh structure or a single-layer cloth structure with meshes, and the mesh size of the mesh structure and the mesh size of the single-layer cloth structure are 0.5-5mm respectively. In the present invention, the size of the mesh refers to the shortest part of the mesh diameter, such as the mesh is circular, the mesh size is the diameter of the mesh, the mesh is square, the mesh size is the side length of the square, the mesh is rectangular, and the mesh size is the width of the rectangle. The single-layer mesh structure or the single-layer cloth structure with mesh is conducive to the subsequent expansion of the water-absorbing resin particles from the mesh of the mesh or the single-layer cloth after the composite coating is separated and removed. If the area coated with water-based slurry is a multi-layer mesh structure or multi-layer cloth with two or more layers, there may be intersections between the meshes of adjacent layers, resulting in the actual size of the mesh becoming lower, which is not conducive to the separation and removal of the water-absorbing resin particles. If the mesh is two or more layers or a multi-layer cloth is used, but the mesh size is large enough, such as 1-5 mm, and the meshes are highly aligned, that is, there is less cross-over between the meshes, it will also be less likely to affect the separation of the water-swellable resin particles in the present invention. However, the mesh size of the mesh and the single-layer cloth cannot be too large, otherwise when the water-based slurry is applied, it is likely that the water-based slurry will flow from the mesh, or block the mesh of the mesh or the single-layer cloth, and the slurry layer cannot be formed. The mesh size of the mesh and the single-layer cloth cannot be too small, otherwise it will cause the expanded water-absorbing resin particles to be unable to be separated and removed. For example, the mesh sizes of the mesh and the single-layer cloth can be any value among 0.5mm, 0.8mm, 1mm, 1.2mm, 1.3mm, 1.5mm, 1.8mm, 2mm, 2.3mm, 2.5mm, 2.8mm, 3mm, 3.2mm, 3.3mm, 3.5mm, 3.7mm, 4mm, 4.3mm, 4.5mm, 4.7mm, 4.8mm, 5mm, etc., but are not limited to those listed above.
[0037] On the other hand, considering the smoothness of removing the expanded water-absorbent resin particles from the mesh holes, laying the water-absorbent resin particles on the bottom slurry layer at the mesh holes of the gauze structure or the mesh holes of the single-layer cloth structure, that is, the water-absorbent resin particles correspond to the mesh holes, is obviously more conducive to the removal of the water-absorbent resin particles. However, when the positions of the water-absorbent resin particles and the mesh holes are not very corresponding or there is a misalignment, the expanded water-absorbent resin particles can still be removed from the mesh holes due to the thin thickness of the bottom slurry layer.
[0038] In a more preferred embodiment of the present invention, the size of the water-absorbing resin particles does not exceed the mesh size. In the present invention, the size of the water-absorbing resin particles refers to the size of the smallest sieve hole that the particles can pass through in the most favorable posture. The size of the water-absorbing resin particles exceeds the size of the mesh, which is not conducive to the removal of the water-absorbing resin particles from the mesh. Further, the size of the water-absorbing resin particles does not exceed 1 / 2 of the mesh size, so that the expanded water-absorbing resin particles can be removed from the mesh after falling off from the composite coating. For example, the size of the water-absorbing resin particles can be any value of 1 / 40, 1 / 35, 1 / 30, 1 / 27, 1 / 25, 1 / 22, 1 / 20, 1 / 16, 1 / 15, 1 / 13, 1 / 10, 1 / 8, 1 / 6, 1 / 5, 1 / 4, 1 / 3, 1 / 2, etc. of the mesh size, but is not limited to the above-mentioned ones. For example, if the mesh size is 4mm, the size of the water-absorbent resin particles can be 3mm, 2mm, 1mm, 0.5mm, 0.2mm, 0.1mm, etc.; for example, if the mesh size is 2mm, the size of the water-absorbent resin particles can be 2mm, 1mm, 0.5mm, 0.2mm, 0.1mm, etc.; for example, if the mesh size is 1mm, the size of the water-absorbent resin particles can be 1mm, 0.5mm, 0.3mm, 0.2mm, 0.1mm, etc.
[0039] In the present invention, the water-absorbing resin particles are polymer resin particles with a certain degree of crosslinking, which can absorb water and swell, and the water absorption weight can reach several to several hundred times the weight of the resin particles themselves, such as crosslinked polyacrylamide, crosslinked polyacrylic acid salt, crosslinked polyvinyl alcohol, or copolymers or modified products of these polymers, such as starch grafted modified polyacrylic acid salt. The water-absorbing resin particles can be directly obtained from the market, such as the commercially available Ocean Baby.
[0040] In a preferred embodiment of the present invention, the method for applying the water-based paste is hollow screen printing. Since the thickness of the water-absorbing resin particles laid on the middle layer is relatively large, although only one layer of water-absorbing resin particles is laid on the bottom paste layer, that is, the water-absorbing resin particles do not cover each other from top to bottom, the thickness of the water-based paste is at least not less than the size of the water-absorbing resin particles. For example, if the size of the water-absorbing resin particles is 0.1 mm, the screen height can be 0.1 mm, 0.2 mm, 0.5 mm, 1 mm, 1.5 mm, 2 mm, etc., so that the water-based paste can completely cover and envelop the water-absorbing resin particles. Therefore, the coating thickness of the water-based paste is relatively thick. If screen printing is used, it takes several or even dozens of printings to achieve it, but it can be achieved by one printing by hollow screen printing.
[0041] In the present invention, the source of the aqueous paste is not particularly limited, and can be the aqueous paste commonly used for textiles, can be directly obtained from the market, or can be prepared according to the prior art. Taking the aqueous PU paste as an example, the composition of an aqueous paste can be as follows: 70-80wt% aqueous silicone modified PU resin, 2-10wt% water, 0.3-0.6wt% defoamer, 0.5-2.0wt% thickener, 2.0-4.0wt% propylene glycol, 4-8wt% aqueous isocyanate crosslinker.
[0042] In a more preferred embodiment of the present invention, the height of the hollow screen is not less than the size of the water-absorbing resin particles. The height of the hollow screen is not less than the size of the water-absorbing resin particles, so that the dough can completely cover and envelop the water-absorbing resin particles. For example, the height of the hollow screen can be any value of 1 times, 1.1 times, 1.2 times, 1.3 times, 1.4 times, 1.5 times, 1.6 times, 1.7 times, 1.8 times, 1.9 times, 2 times, etc., the size of the water-absorbing resin particles, but is not limited to the above-mentioned values.
[0043] In a preferred embodiment of the present invention, the pre-composite layer is immersed in water for 0.5-12 hours and the temperature is 5-40°C, or further, the pre-composite layer is immersed in water for 0.5-6 hours. By adjusting the time and water temperature of the pre-composite layer immersed in water, the expansion multiple of the water-absorbing resin particles can be adjusted, and then the pore size of the porous structure can be adjusted. The higher the expansion multiple, the larger the pore size of the porous structure. Generally speaking, the longer the immersion time and the higher the water temperature, the higher the expansion multiple of the water-absorbing resin particles. For example, the water temperature can be 5°C, the immersion time can be 1h, 2h, 3h, 4h, 6h, etc., the water temperature can be 20°C, the immersion time can be 1h, 1.5h, 2h, 3h, etc., the water temperature can be 35°C, and the immersion time can be 0.5h, 1h, 1.5h, 2h, etc.
[0044] In a preferred embodiment of the present invention, the expanded water-absorbing resin particles are removed from the mesh of the textile. Since the base slurry layer is very thin, it is easy to be squeezed and broken at the mesh, and the expanded water-absorbing resin particles are separated from the squeezed and broken places and further separated from the mesh, and even the water-absorbing resin particles can actively squeeze and break the base slurry layer when swelling by absorbing water, so that the outer surface of the porous coating can be prevented from being damaged or broken, and the outer surface of the formed porous coating is intact.
[0045] In the present invention, by setting the structure and mesh size of the textile covering composite layer, the expanded water-absorbing resin particles can be removed from the mesh of the textile, which can achieve the following: (1) due to the presence of the base slurry layer, the porous coating and the textile still maintain good bonding; (2) the porous coating remains intact when viewed from the outer surface; (3) the porous structure of part or all of the porous coating is connected to the mesh opening of the textile.
[0046] In the present invention, there is no particular limitation on the drying conditions for the first drying, the second drying and the third drying. For example, the first drying may be baked at 50-70°C for 10-30 min; the second drying may be placed at room temperature for 1-12 h (placed at room temperature first, the curing may proceed slowly, the moisture may evaporate slowly or be partially absorbed by the water-absorbing resin particles, and the dough layer may still cover the water-absorbing resin particles during the drying and curing process to form a surface coating layer), and then baked at 50-70°C for 8-12 h; the third drying may be dried at 50-70°C for 24-60 h.
[0047] In another aspect, the present invention provides a porous coated textile, which is prepared by the method for preparing a porous coated textile according to any one of the above embodiments.
[0048] The porous coated textile of the present invention can be applied to clothing, shoes, curtains and the like, and has the functions of buffering, decoration, protection and the like.
[0049] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.
[0050] In the following embodiments and comparative examples, the composition of the aqueous base paste is: 85wt% aqueous PU resin (concentration is 35wt%), 9wt% slow-drying agent (ethylene glycol monomethyl ether), 0.5wt% defoamer, 0.4wt% leveling agent, 1.1wt% aqueous associative polyurethane thickener and 4wt% aqueous isocyanate crosslinker; the composition of the aqueous surface paste is: 79.3wt% aqueous silicone modified PU resin (concentration is 40wt%), 10wt% water, 0.5wt% defoamer, 1.2wt% aqueous associative polyurethane thickener, 3wt% propylene glycol, 6wt% aqueous isocyanate crosslinker. Those skilled in the art know that the above-mentioned aqueous base paste and aqueous surface paste are only examples and are not limitations of the present invention. Those skilled in the art can directly obtain the aqueous base paste and / or aqueous surface paste from the market, or they can prepare them according to the prior art.
[0051] Example 1
[0052] A single layer of mesh (mesh size 2mm) was fixed on the printing plate, and a water-based base paste was printed on the mesh with a 300-mesh screen, with a thickness of 30μm. A layer of water-absorbent resin particles (commercially available Ocean Baby, size 0.5mm) was laid, and the water-absorbent resin particles corresponded to the mesh of the mesh. The water-absorbent resin particles that were not adhered by the water-based base paste were removed and baked in a 60°C oven for 20min. The water-based surface paste was printed on the water-absorbent resin particles by hollow printing. The height of the hollow screen was 1.5mm. The surface paste layer covered and wrapped the water-absorbent resin particles. It was dried at 25°C for 8h, then transferred to 60°C for drying for 10h, cooled to room temperature, and left for 24h to obtain a pre-composite layer. The pre-composite layer was immersed in 25°C water for 2 hours and taken out. It was found that the water-absorbing resin particles expanded, the bottom slurry layer at about 30% of the mesh holes was squeezed out, and the outer surface of the coating was not damaged. The expanded water-absorbing resin particles were squeezed out from the mesh holes, and then the printed fabric was placed in a 70°C environment and continued to dry for 40 hours, taken out and cooled, to obtain a porous coated mesh.
[0053] Attached Figure 1 This is a front view of the porous coating mesh of this embodiment. It can be seen that the outer surface of the porous coating presents obvious bubble protrusions and is not damaged.
[0054] Attached Figure 2 This is a back view of the porous coated mesh of this embodiment. It can be seen that the base slurry layer at the mesh holes is damaged and the water-absorbing resin particles fall off from these damaged parts.
[0055] Example 2
[0056] The difference between this embodiment and embodiment 1 is that in embodiment 1, the height of the hollow screen is adjusted from 1.5 mm to 1 mm. The other steps remain unchanged. The result is similar to that of embodiment 1.
[0057] Example 3
[0058] The difference between this embodiment and embodiment 1 is that in embodiment 1, the water-absorbing resin particles are changed to sea babies with a size of 1 mm. The other steps remain unchanged.
[0059] The results showed that the bottom slurry layer was squeezed out at about 20% of the mesh holes, the outer surface of the coating was not damaged, and the expanded water-absorbing resin particles could be squeezed out from the mesh holes.
[0060] Example 4
[0061] The difference between this embodiment and embodiment 1 is that in embodiment 1, the single-layer mesh is changed to a double-layer mesh consisting of two layers of single-layer mesh, the mesh size is 2 mm, and the two layers of mesh are aligned at the mesh, and the meshes of the two layers of mesh are less crossed. The other steps remain unchanged.
[0062] The results showed that the bottom slurry layer was squeezed out at about 30% of the mesh holes, the outer surface of the coating was not damaged, and the water-absorbing resin particles that swelled after absorbing water could be squeezed out from the mesh holes.
[0063] Comparative Example 1
[0064] The difference between this comparative example and Example 1 is that the mesh is not printed with water-based slurry, but a layer of water-absorbing resin particles is directly laid on the mesh. The other steps remain unchanged.
[0065] The results showed that (1) during laying, the water-absorbent resin particles would fall off directly from the mesh holes, and it was not easy to lay only one layer of water-absorbent resin particles, as the water-absorbent resin particles would easily overlap up and down; (2) the adhesion between the surface slurry layer and the mesh was very low. After being soaked in water for 2 hours, it was found that part of the surface slurry layer had detached from the mesh.
[0066] Comparative Example 2
[0067] The difference between this comparative example and comparative example 1 is that the mesh size of the mesh is adjusted from 2 mm to 0.3 mm. The other steps remain unchanged.
[0068] The results showed that (1) during laying, the water-absorbent resin particles would not fall off directly from the mesh holes, but it was not easy to lay only one layer of water-absorbent resin particles, and the water-absorbent resin particles were prone to overlap; (2) the adhesion between the surface slurry layer and the mesh was very low. After being soaked in water for 2 hours, it was found that part of the surface slurry layer had detached from the mesh; (3) the expanded water-absorbent resin particles could not detach from the mesh holes of the mesh, and could only damage the outer surface of the coating and detach from the outer surface.
[0069] Example 5
[0070] A single layer of cloth (mesh size 0.5mm) was fixed on the printing plate, and a water-based base paste was printed on the mesh with a 250-mesh screen, with a thickness of 25μm. A layer of loose water-absorbent resin particles (cross-linked sodium polyacrylate, size 0.1mm, water absorption rate 120 times, for water absorption test at 25°C for 24h) was laid, and the water-absorbent resin particles not adhered by the water-based base paste were removed, and baked in a 70°C oven for 12min. The water-based surface paste was printed on the water-absorbent resin particles by hollow printing, and the height of the hollow screen was 0.2mm. The surface paste layer covered and wrapped the water-absorbent resin particles, dried at 25°C for 6h, then transferred to 60°C for drying for 8h, cooled to room temperature, and left for 24h to obtain a pre-composite layer. The pre-composite layer was immersed in 25°C water for 0.5h and taken out. The water-absorbing resin particles expanded, the bottom slurry layer at less than 5% of the mesh openings was squeezed out, and the outer surface of the coating was intact. The expanded water-absorbing resin particles were squeezed out from the mesh openings, and then the printed fabric was placed in a 70°C environment and continued to dry for 36h, taken out and cooled, to obtain a porous coated fabric.
[0071] Attached Figure 3This is a front view of the porous coated cloth of this embodiment. It can be seen that the outer surface of the porous coating presents obvious pore protrusions and is not damaged.
[0072] Attached Figure 4 This is a back view of the porous coated cloth of this embodiment. It can be seen that the base slurry layer is damaged at the mesh openings and the water-absorbing resin particles fall off from these damaged portions.
[0073] Example 6
[0074] The difference between this embodiment and embodiment 5 is that in embodiment 5, the pre-composite layer is immersed in 25° C. water for 1 hour instead of 0.5 hours. The other steps remain unchanged.
[0075] The results showed that the water-absorbing resin particles expanded, the bottom slurry layer at about 40% of the mesh openings was squeezed and broken, and the outer surface of the coating was not damaged.
[0076] Example 7
[0077] The difference between this embodiment and embodiment 5 is that in embodiment 5, the pre-composite layer is immersed in 25° C. water for 3 hours instead of 0.5 hours. The other steps remain unchanged.
[0078] The results showed that the water-absorbing resin particles expanded, the bottom slurry layer at about 75% of the mesh openings was squeezed and the outer surface of the coating was not damaged.
[0079] Example 8
[0080] The difference between this embodiment and embodiment 5 is that in embodiment 5, the pre-composite layer is immersed in 25° C. water for 0.5 h, which is adjusted to be immersed in 5° C. water for 2 h. The other steps remain unchanged.
[0081] The results showed that the water-absorbing resin particles expanded, the bottom slurry layer at about 30% of the mesh openings was squeezed and broken, and the outer surface of the coating was not damaged.
[0082] Example 9
[0083] The difference between this embodiment and embodiment 5 is that in embodiment 5, the pre-composite layer is immersed in 25° C. water for 0.5 h, which is adjusted to be immersed in 5° C. water for 6 h. The other steps remain unchanged.
[0084] The results showed that the water-absorbing resin particles expanded, the bottom slurry layer was squeezed and broken at about 80% of the mesh openings, and the outer surface of the coating was not damaged.
[0085] Comparative Example 3
[0086] The water-absorbing resin particles in the pre-composite layer in Example 5 were directly squeezed and found to be difficult to separate from the mesh. This may be because the water-absorbing resin particles did not absorb water and swell, and had a high bonding force with the base slurry layer and / or the surface slurry layer.
[0087] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a porous coated textile, characterized in that: The following steps are involved: Applying a water-based base paste on the textile to form a base paste layer; Laying water-absorbing resin particles on the base slurry layer and drying for the first time to obtain an intermediate layer; Applying water-based paste on the intermediate layer and drying it for a second time to obtain a pre-composite layer; The pre-composite layer is soaked in water, the expanded water-absorbing resin particles are removed, and the porous coated textile is obtained by drying for a third time.
2. The method for preparing a porous coated textile according to claim 1, characterized in that: The method for applying the water-based base paste is screen printing.
3. The method for preparing a porous coated textile according to claim 1, characterized in that: The area on the textile coated with the aqueous base slurry is a single-layer mesh structure or a single-layer cloth structure with mesh holes, and the sizes of the mesh holes of the mesh structure and the mesh holes of the single-layer cloth structure are 0.5-5 mm respectively.
4. The method for preparing a porous coated textile according to claim 3, characterized in that: The size of the water absorbing resin particles does not exceed the mesh size.
5. The method for preparing a porous coated textile according to claim 4, characterized in that: The size of the water absorbing resin particles does not exceed 1 / 2 of the mesh size.
6. The method for preparing a porous coated textile according to claim 1, characterized in that: The method for applying the water-based paste is hollow screen printing.
7. The method for preparing a porous coated textile according to claim 6, characterized in that: The height of the hollow screen is not less than the size of the water-absorbing resin particles.
8. The method for preparing a porous coated textile according to claim 1, characterized in that: The pre-composite layer is immersed in water for 0.5-12 hours at a temperature of 5-40°C.
9. The method for preparing a porous coated textile according to claim 1, characterized in that: The removing of the expanded water absorbing resin particles is removing from the mesh of the textile.
10. A porous coated textile, characterized in that: The porous coated textile is prepared by the preparation method of any one of claims 1 to 9.
Citation Information
Patent Citations
Composite absorption core
CN104367418A
Long-life super-hydrophobic composite coating and preparation method thereof
CN117363111A
Building surface anticorrosive paint near water
CN204727832U
Low-volatility quick-drying high-solid-content water-based paint coating structure
CN212737316U
hartsbestrykningskomposition SOM SVAELLER I VATTEN OCH EN OPTISK KAPEL I VILKEN DENNA ANVAENDS.
FI923859A0