Lock head structure and preparation method thereof, container locking mechanism and container transportation system
By applying a nitriding layer, transition layer and diamond-like layer on the lock head, the problem of lock head stuck in container transportation is solved, and the removal efficiency and stability of the lock box mechanism are improved.
Patent Information
- Application Number
- CN202411138136.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-19
AI Technical Summary
During transportation, the container is prone to vibration to cause the lock head to get stuck, which is difficult to release, resulting in waste of disassembly time and reduced stability of the lock box mechanism.
Using a locking structure including a nitriding layer, a transition layer and a diamond-like layer, the hardness and deformation resistance of the locking head are improved through ionic nitriding treatment and arc ion coating technology, reducing friction and friction coefficient, and reducing locking head and coordination. frictional moment between surfaces.
It effectively reduces the external force required for the lock box to be freed, reduces the probability of the lock head stuck, improves the wear resistance and stability of the lock head, and ensures the normal relief of the container.
Smart Images

Figure CN118933451A_ABST
Abstract
Description
Technical Field
[0001] The application relates to the field of automobile technology, and in particular to a locking structure, a preparation method, a locking mechanism and a container transportation system. Background Art
[0002] Containers play an extremely important role in modern logistics and trade. The container transportation method has the advantages of high transportation efficiency, safe and reliable transportation process, and simple loading and unloading.
[0003] The container and the base are connected by a lock box mechanism. The rotary lock box is one of the commonly used mechanisms. It is mainly composed of a lock head, a lock rod and a lock body. The lock head is generally round or oblate. The lock head cooperates with the container fixing device and tightens by rotating the lock head, thereby limiting the freedom of the container to move up and down.
[0004] However, due to the influence of vibration during transportation, the container is prone to slight radial movement, and the lock may be stuck in the container and difficult to release. At this time, manual assistance is required to open it, which wastes disassembly time and reduces the stability of the locking mechanism. Summary of the invention
[0005] The application provides a locking structure, a preparation method, a locking mechanism and a container transportation system, to solve the problem that existing locking containers are difficult to relieve from being stuck.
[0006] In a first aspect, the present application provides a locking structure, including a locking body and a protective layer disposed on the surface of the locking body, wherein the protective layer comprises sequentially arranged from the inside to the outside:
[0007] Nitriding layer;
[0008] a transition layer, the material of the transition layer includes at least one of Cr and CrN; and,
[0009] Diamond-like carbon layer.
[0010] The container and the base are connected by a lock mechanism, and the container is released by overcoming the friction torque formed between the lock and the mating surface. When the friction torque exceeds the lock driving torque, the container will be stuck and difficult to release. During transportation, the container is prone to slight radial movement, resulting in slight deformation of the connection lock, generating greater pressure at the contact surface with the lock, and then generating excessive friction, causing the lock to lock and unable to open normally. At the same time, the surface of the lock is prone to wear and tear after repeated use, further increasing the friction coefficient between the lock and the mating surface, resulting in locking.
[0011] The present application utilizes the characteristics of high hardness and low friction coefficient of the diamond-like carbon layer. On the one hand, it can strengthen the contact surface strength of the lock and reduce the wear caused by long-term friction; on the other hand, it can effectively reduce the friction force, thereby reducing the external force required to release the lock box, and reducing the excessive contact force on the contact surface due to local deformation, which leads to excessive friction torque for release and jamming. After the metal material is treated with ion nitriding, the hardness and elastic modulus of the nitrided layer formed on the surface will be improved compared to the matrix, so the deformation resistance of the surface will be improved. Under the same force, the surface deformation will be smaller after nitriding, so that the nitrided layer provides good support for the diamond-like layer, reduces the hardness mutation between the diamond-like layer and the matrix, and reduces the probability of the diamond-like layer deforming under extrusion and collapsing.
[0012] Diamond-like materials mainly refer to SP of C 2 Hybrid bonds and SP 3 Metastable materials formed by hybrid bonds.
[0013] In some embodiments, the thickness of the nitriding layer is 0.2-0.3 mm. Within this range, the thickness of the nitriding layer can further provide good support for the diamond-like carbon layer, reduce the hardness mutation between the diamond-like carbon layer and the substrate, and reduce the probability of the diamond-like carbon layer deforming and collapsing under extrusion; and / or,
[0014] The material of the lock body includes at least one of 35CrMnSi and 42CrMo. The lock body is made of the above-mentioned materials, which has good comprehensive mechanical properties, high strength and sufficient toughness.
[0015] In some embodiments, the transition layer includes a Cr layer and a CrN layer arranged sequentially from the inside to the outside, wherein:
[0016] The thickness of the Cr layer is 0.1 to 0.2 μm; the Cr single substance has good toughness and high bonding strength with the substrate, which can improve the bonding firmness between the diamond-like carbon layer and the lock body and reduce the shedding of the diamond-like carbon layer; and / or,
[0017] The thickness of the CrN layer is 0.5 to 1 μm. CrN has a higher hardness than single substance Cr. While providing bonding performance for the diamond-like carbon layer to reduce the shedding of the diamond-like carbon layer, it can also provide certain support for the diamond-like carbon layer, reduce the hardness mutation between the diamond-like carbon layer and the lock body, and reduce the probability of the diamond-like carbon layer deforming and collapsing under extrusion; and / or,
[0018] The thickness of the diamond-like layer is 1-2 μm. When the thickness of the diamond-like layer is within this range, the internal stress of the diamond-like coating is small, and natural cracking and falling off caused by excessive internal stress can be prevented.
[0019] Second, the present application provides a method for preparing a locking structure to prepare the locking structure of the first aspect, including the following steps:
[0020] Ion nitriding is performed on the surface of the lock body to obtain a nitriding layer;
[0021] The material of the transition layer is plated on the surface of the nitriding layer to obtain a transition layer;
[0022] Diamond-like material is plated on the surface of the transition layer to form a diamond-like layer, resulting in a locked structure.
[0023] The high hardness and low friction coefficient of the diamond-like carbon layer can, on the one hand, strengthen the contact surface strength of the lock and reduce the deterioration of surface roughness caused by long-term friction and wear; on the other hand, it can effectively reduce friction, thereby reducing the external force required to release the lock box, and reduce the excessive contact force on the contact surface due to local deformation, which leads to excessive friction torque and jamming. After the metal material is treated with ion nitriding, the surface hardness and elastic modulus will be improved, so the surface deformation resistance will be improved. Under the same force, the surface deformation will be smaller after nitriding, so that the nitrided layer provides good support for the diamond-like carbon layer, reduces the hardness mutation between the diamond-like carbon layer and the substrate, and reduces the probability of the diamond-like carbon layer deforming under extrusion and collapsing.
[0024] It should be noted that before forming the nitriding layer, the lock body can be sandblasted to remove impurities such as oil stains and rust on the lock surface, exposing the fresh metal activated surface; at the same time, the impact of the micro-shot during the sandblasting process can change the stress state of the lock surface from tensile stress to compressive stress, thereby improving the surface compressive resistance. Then, the sandblasted lock is ultrasonically cleaned with anhydrous ethanol or acetone to further remove surface impurities. Specifically, the sandblasting distance can be 20 to 30 cm, the sandblasting angle is 60° to 90°, the sandblasting pressure is 0.4 to 0.8 MPa, the sand particle diameter used is 320 to 500 mesh, and there is no rust and oil stains on the surface after sandblasting, and fresh metal is exposed. Subsequently, the surface is cleaned with anhydrous ethanol or acetone in an ultrasonic cleaning device for 20 to 30 minutes.
[0025] In some embodiments, the ionic nitriding treatment is performed on the surface of the lock body to obtain a nitriding layer:
[0026] The temperature of ion nitriding is 400-500°C; and / or,
[0027] The voltage of ion nitriding is -200 to -700V; and / or,
[0028] The pressure of ion nitridation is 250-300 Pa; and / or,
[0029] The time for ion nitriding is 5 to 8 hours.
[0030] It should be noted that the lock body can be pre-treated before the ion nitriding treatment. Specifically, the lock is placed in the ion nitriding furnace, and the furnace door is closed to evacuate. When the vacuum degree is 60-80Pa, arc cleaning is started, that is, the voltage difference between the workpiece and the furnace wall is increased, and the substrate voltage is -200--700V, so that the remaining air in the furnace is ionized to generate N + , H + The ions impact the surface impurities, thereby achieving the cleaning effect; after the cleaning is completed, H2 and N2 are introduced, and the flow rate is gradually increased as the temperature increases, maintaining the flow rate ratio of H2:N2=3:1, and gradually increasing the negative bias voltage of the substrate. When the heating temperature reaches 400-500°C, the insulation temperature, voltage, pressure and gas flow rate are set and then the insulation nitriding is started. The nitriding time is 5-8h. After the nitriding is completed, it is cooled with the furnace for standby use.
[0031] In some embodiments, the material of a transition layer is plated on the surface of the nitriding layer, and the transition layer comprises:
[0032] The Cr layer material is plated on the surface of the nitriding layer to obtain a Cr layer;
[0033] CrN is deposited on the surface of the Cr layer to form a CrN layer to obtain a transition layer.
[0034] Elemental Cr has good toughness and high adhesion with the substrate, which can improve the bonding strength between the diamond-like carbon layer and the lock body and reduce the shedding of the diamond-like carbon layer. CrN has higher hardness than elemental Cr. While providing bonding properties for the diamond-like carbon layer and reducing the shedding of the diamond-like carbon layer, it can also provide certain support for the diamond-like carbon layer, reduce the hardness mutation between it and the lock body, and reduce the probability of the diamond-like carbon layer deforming and collapsing under extrusion.
[0035] In some embodiments, the target voltage when the Cr layer is plating is 20 to 40 V; and / or,
[0036] The arc current of the target material when the Cr layer is plated is 80 to 120A; and / or,
[0037] The time for plating the Cr layer is 5 to 15 minutes; and / or,
[0038] The internal pressure of the furnace with the Cr layer plated is 1 to 2 Pa; and / or,
[0039] The temperature of the Cr coating is 450-470°C; and / or,
[0040] The time for forming the CrN layer is 30 to 50 minutes.
[0041] It should be noted that the method of forming the Cr layer and the CrN layer can be specifically: place the lock on the rotary frame in the arc ion coating machine, close the furnace door and turn on the automatic vacuum mode, and when the vacuum is pumped to 5×10 -3 Pa, turn on the auxiliary heating wire in the furnace for gradient heating. First, set the heating temperature to 270-300°C, wait for the temperature to rise to the set value, keep warm for 20-30 minutes, then set the heating temperature to 400-470°C, and wait for the temperature to rise to 450-470°C before plating Cr. First, introduce a mixed gas of Ar+H2 with a flow rate of 180-220sccm into the furnace, maintain the pressure in the furnace at 0.5-1Pa, turn on the Ti target arc to etch and clean the lock surface, set the substrate bias voltage to -30--150V, and turn off the target arc after the etching and cleaning is completed. Then, Ar is introduced alone, the pressure in the furnace is set to 1-2Pa, the Cr target arc is turned on, the target voltage is 20-40V, the current is 80-120A, and single Cr is plated on the surface of the workpiece for 5-15min; then, Ar is turned off, and N2 is introduced into the furnace at the same time, maintaining the pressure at 1-2Pa, and the CrN layer is continued to be prepared on the surface for 30-50min. After completion, the Cr target arc is turned off, and the N2 introduction is closed.
[0042] In some embodiments, the diamond-like material is coated on the surface of the transition layer to form a diamond-like layer, resulting in a locked structure;
[0043] The plating temperature is 100-200°C; and / or,
[0044] The plating time is 30 to 50 minutes; and / or,
[0045] The bias voltage of the substrate attached is -200 to -300V; and / or,
[0046] The plated bias pulse frequency is 30-80kHz; and / or,
[0047] The pressure inside the plating furnace is 0.1~0.5Pa.
[0048] It should be noted that the above-mentioned plating diamond-like plating uses a pure C target with a purity of 99.99% as the raw material and is carried out under an inert gas.
[0049] In a third aspect, the present application provides a locking box mechanism, including a locking structure made of a locking structure of the first aspect or a locking structure of the second aspect.
[0050] It should be noted that the lock box mechanism also includes a lock body, an electric push rod or a pneumatic push rod, and a connecting ring. The lock head is installed inside the lock body. The connecting ring is connected to the lock head on one hand, and its extended part is connected to the drive rod. Its function is to convert the linear motion of the push rod into the rotational motion of the lock head.
[0051] In a fourth aspect, the present application provides a container transport system, including a locking mechanism of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0053] Figure 1 This is a structural diagram of the locking structure of an embodiment of this application.
[0054] Figure 2 It is a schematic axial cross-sectional view of a locking structure according to an embodiment of the present application.
[0055] Figure 3 It is a schematic axial cross-sectional view of a locking head structure according to another embodiment of the present application.
[0056] Figure 4 The friction coefficient diagram of the locking structure of the first embodiment of the present application is a diagram of the change over time.
[0057] Figure 5 The friction coefficient diagram of the locking structure of Comparative Example 1 of this application is a diagram of the change over time.
[0058] Figure 6 The friction coefficient diagram of the locking structure of Comparative Example 2 of this application is a graph of time change.
[0059] Figure 7 The friction coefficient diagram of the locking structure of Comparative Example 3 of this application is a diagram of the change over time.
[0060] Description of Figure Numbers:
[0061] 100 locking structure; 1 locking body; 2 protective layer; 21 nitriding layer; 22 transition layer; 221Cr layer; 222CrN layer; 23 diamond layer. DETAILED DESCRIPTION
[0062] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0063] Containers play an extremely important role in modern logistics and trade. The container transportation method has the advantages of high transportation efficiency, safe and reliable transportation process, and simple loading and unloading.
[0064] The container and the base are connected by a lock box mechanism. The rotary lock box is one of the commonly used mechanisms. It is mainly composed of a lock head, a lock rod and a lock body. The lock head is generally round or oblate. The lock head cooperates with the container fixing device and tightens by rotating the lock head, thereby limiting the freedom of the container to move up and down.
[0065] However, due to the influence of vibration during transportation, the container is prone to slight radial movement, and the lock may be stuck in the container and difficult to release. At this time, manual assistance is required to open it, which wastes disassembly time and reduces the stability of the locking mechanism.
[0066] In view of this, the present application provides a locking structure and a preparation method, a locking mechanism and a container transportation system to solve the problem that existing locking containers are difficult to relieve from being stuck.
[0067] like Figure 1 and Figure 2 In the first aspect, the present application provides a lock structure 100 including a lock body 1 and a protective layer 2 disposed on the surface of the lock body 1 , wherein the protective layer 2 comprises sequentially arranged from the inside to the outside:
[0068] Nitriding layer 21;
[0069] The transition layer 22, the material of which includes at least one of Cr and CrN; and,
[0070] The diamond-like carbon layer 23 .
[0071] The container and the base are connected by a lock mechanism, and the container is released by overcoming the friction torque formed between the lock and the mating surface. When the friction torque exceeds the lock driving torque, the container will be stuck and difficult to release. During transportation, the container is prone to slight radial movement, resulting in slight deformation of the connection lock, generating greater pressure at the contact surface with the lock, and then generating excessive friction, causing the lock to lock and unable to open normally. At the same time, the surface of the lock is prone to wear and tear after repeated use, further increasing the friction coefficient between the lock and the mating surface, resulting in locking.
[0072] The present application uses the characteristics of high hardness and low friction coefficient of the diamond-like carbon layer 23. On the one hand, it can strengthen the contact surface strength of the lock and reduce the wear caused by long-term friction; on the other hand, it can effectively reduce the friction force, thereby reducing the external force required for the lock box to release, and reduce the excessive contact force on the contact surface due to local deformation, which leads to excessive friction torque for release and jamming. After the metal material is treated with ion nitriding, the surface hardness and elastic modulus will be improved, so the surface deformation resistance will be improved. Under the same force, the surface deformation will be smaller after nitriding, so that the nitrided layer 21 provides good support for the diamond-like carbon layer 23, reduces the hardness mutation between the diamond-like carbon layer 23 and the substrate, reduces the probability of the diamond-like carbon layer 23 deforming under extrusion and collapsing, and reduces the probability of the lock getting stuck.
[0073] Diamond-like materials mainly refer to SP of C 2 Hybrid bonds and SP 3 Metastable materials formed by hybrid bonds.
[0074] In combination with the first aspect, in some embodiments provided in the present application, the thickness of the nitriding layer 21 is 0.2 to 0.3 mm. The thickness of the nitriding layer 21 within this range can further provide good support for the diamond-like carbon layer 23, reduce the hardness mutation between the diamond-like carbon layer 23 and the substrate, and reduce the probability of the diamond-like carbon layer 23 deforming and collapsing under extrusion.
[0075] In combination with the first aspect, in some embodiments provided in the present application, the material of the lock body 1 includes at least one of 35CrMnSi and 42CrMo. The lock body 1 adopts the above-mentioned material, has good comprehensive mechanical properties, high strength and sufficient toughness.
[0076] like Figure 3 As shown, in combination with the first aspect, in some embodiments provided in the present application, the transition layer 22 includes a Cr layer 221 and a CrN layer 222 arranged sequentially from the inside to the outside, wherein: the thickness of the Cr layer 221 is 0.1 to 0.2 μm; the Cr element has good toughness and high adhesion to the substrate, which can improve the firmness of the bond between the diamond-like carbon layer 23 and the lock body and reduce the shedding of the diamond-like carbon layer 23.
[0077] In combination with the first aspect, in some embodiments provided in the present application, the transition layer 22 includes a Cr layer 221 and a CrN layer 222 arranged in sequence from the inside to the outside, wherein: the thickness of the CrN layer 222 is 0.5 to 1 μm; CrN has a higher hardness than single Cr, and while providing bonding properties for the diamond-like layer 23 to reduce the shedding of the diamond-like layer 23, it can also provide certain support for the diamond-like layer 23, reduce the hardness mutation between it and the lock body, and reduce the probability of the diamond-like layer 23 deforming and collapsing under extrusion.
[0078] In combination with the first aspect, in some embodiments provided in the present application, the transition layer 22 includes a Cr layer 221 and a CrN layer 222 arranged sequentially from the inside to the outside, wherein: the thickness of the diamond-like layer 23 is 1 to 2 μm. Within this range, the diamond-like coating 23 has a small internal stress, which can prevent natural cracking and falling off due to excessive internal stress.
[0079] Second, the present application provides a method for preparing a locking structure to prepare the locking structure of the first aspect, including the following steps:
[0080] Ion nitriding is performed on the surface of the lock body to obtain a nitriding layer;
[0081] The material of the transition layer is plated on the surface of the nitriding layer to obtain a transition layer;
[0082] Diamond-like material is plated on the surface of the transition layer to form a diamond-like layer, resulting in a locked structure.
[0083] The high hardness and low friction coefficient of the diamond-like carbon layer can, on the one hand, strengthen the contact surface strength of the lock and reduce the wear caused by long-term friction; on the other hand, it can effectively reduce the friction force, thereby reducing the external force required to release the lock box, and reduce the excessive contact force on the contact surface due to local deformation, which leads to excessive friction torque and jamming. After the metal material is treated with ion nitriding, the surface hardness and elastic modulus will be improved, so the surface deformation resistance will be improved. Under the same force, the surface deformation will be smaller after nitriding, so that the nitrided layer provides good support for the diamond-like carbon layer, reduces the hardness mutation between the diamond-like carbon layer and the substrate, and reduces the probability of the diamond-like carbon layer deforming under extrusion and collapsing.
[0084] It should be noted that before forming the nitriding layer, the lock body can be sandblasted to remove impurities such as oil stains and rust on the lock surface, exposing the fresh metal activated surface; at the same time, the impact of the micro-balls during the sandblasting process can change the stress state of the lock surface from tensile stress to compressive stress, thereby improving the surface compressive resistance. Then, ethylene glycol or acetone is used to ultrasonically clean the sandblasted lock to further remove surface impurities. Specifically, the sandblasting distance can be 20 to 30 cm, the sandblasting angle is 60° to 90°, the sandblasting pressure is 0.4 to 0.8 MPa, and the sand particle diameter used is 320 to 500 mesh. After sandblasting, there is no rust and oil stains on the surface, and fresh metal is exposed. Then, the surface is cleaned with anhydrous ethanol in an ultrasonic cleaning device for 20 to 30 minutes.
[0085] In combination with the second aspect, in some embodiments provided by the present application, the ion nitriding treatment is performed on the surface of the lock body to obtain that the ion nitriding temperature in the nitriding layer is 400 to 500°C.
[0086] In combination with the second aspect, in some embodiments provided by the present application, the ion nitriding treatment is performed on the surface of the lock body to obtain that the voltage of ion nitriding in the nitriding layer is -200 to -700V.
[0087] In combination with the second aspect, in some embodiments provided by the present application, the ion nitriding treatment is performed on the surface of the lock body to obtain that the ion nitriding pressure in the nitriding layer is 250 to 300 Pa.
[0088] In combination with the second aspect, in some embodiments provided by the present application, the ion nitriding treatment is performed on the surface of the lock body to obtain the nitriding layer: the ion nitriding time is 5 to 8 hours.
[0089] Within the above temperature, voltage, pressure and time range, a nitriding layer with substantially no white bright layer can be prepared. Although the white bright layer has higher hardness and better corrosion resistance, it is more brittle than the diffusion layer, which is not conducive to the adhesion and bonding of the coating.
[0090] It should be noted that the lock body can be pre-treated before the ion nitriding treatment. Specifically, the lock is placed in the ion nitriding furnace, and the furnace door is closed to evacuate. When the vacuum degree is 60-80Pa, arc cleaning is started, that is, the voltage difference between the workpiece and the furnace wall is increased, and the substrate voltage is -200--700V, so that the remaining air in the furnace is ionized to generate N + , H +, ions collide with surface impurities, thereby achieving a cleaning effect; after cleaning is completed, H2 and N2 are introduced, and the flow rate is gradually increased as the temperature increases, maintaining the flow rate ratio of H2:N2=3:1, and gradually increasing the negative bias voltage of the substrate. When the heating temperature reaches 400-500°C, the insulation temperature, voltage, pressure and gas flow rate are set and then the insulation nitriding is started. The nitriding time is 5 to 8 hours. After the nitriding is completed, it is cooled with the furnace for standby use.
[0091] In connection with the second aspect, in some embodiments provided by the present application, the material of a transition layer is plated on the surface of the nitriding layer, so that the transition layer comprises:
[0092] The Cr layer material is plated on the surface of the nitriding layer to obtain a Cr layer;
[0093] CrN is deposited on the surface of the Cr layer to form a CrN layer.
[0094] Elemental Cr has good toughness and high adhesion to the substrate, which can improve the bonding strength between the coating and the lock body. The CrN layer has higher hardness than the elemental Cr layer, which can provide certain support for the diamond-like carbon layer, reduce the hardness mutation between it and the lock body, and reduce the probability of the diamond-like carbon layer deforming and collapsing under extrusion.
[0095] In connection with the second aspect, in some embodiments provided by the present application, the substrate bias of the Cr-plated layer is -20 to -40V.
[0096] In connection with the second aspect, in some embodiments provided by the present application, the target current of the Cr layer is 80 to 120 A.
[0097] In connection with the second aspect, in some embodiments provided by the present application, the coating time of the Cr layer is 5 to 15 minutes.
[0098] In connection with the second aspect, in some embodiments provided by the present application, the intra-fired pressure of the Cr-plated layer is 1 to 2 Pa.
[0099] In connection with the second aspect, in some embodiments provided by the present application, the temperature of the Cr-coated layer is 450 to 470°C.
[0100] In connection with the second aspect, in some embodiments provided by the present application, the time for forming the CrN layer is 30 to 50 min.
[0101] Under the above voltage, current, coating time, furnace pressure, temperature and N2 input time, the hardness of the prepared transition layer increases in a gradient manner, thereby reducing the hardness of the final functional layer and the substrate.
[0102] It should be noted that the method of forming the Cr layer and the CrN layer can be specifically: place the lock on the rotary frame in the arc ion coating machine, close the furnace door and turn on the automatic vacuum mode, and when the vacuum is pumped to 5×10 -3 Pa, turn on the auxiliary heating wire in the furnace for gradient heating. First, set the heating temperature to 270-300°C, wait for the temperature to rise to the set value, keep warm for 20-30 minutes, then set the heating temperature to 400-470°C, and wait for the temperature to rise to 450-470°C before plating Cr. First, introduce a mixed gas of Ar+H2 with a flow rate of 180-220sccm into the furnace, maintain the pressure in the furnace at 0.5-1Pa, turn on the Ti target arc to etch and clean the lock surface, set the substrate bias voltage to -30--150V, and turn off the target arc after the etching and cleaning is completed. Then, Ar is introduced alone, the pressure in the furnace is set to 1-2Pa, the Cr target arc is turned on, the target voltage is 20-40V, the current is 80-120A, and single-element Cr is plated on the surface of the workpiece for 5-15min. Then, N2 is introduced into the furnace, the pressure is maintained at 1-2Pa, and the CrN layer is continued to be prepared on the surface for 30-50min. After completion, the Cr target arc is turned off, and the N2 introduction is closed.
[0103] In combination with the second aspect, in some embodiments provided by the present application, the diamond-like material is plated on the surface of the transition layer to form a diamond-like layer to obtain a locking structure; the plating temperature is 100 to 200°C.
[0104] In combination with the second aspect, in some embodiments provided by the present application, the diamond-like material is plated on the surface of the transition layer to form a diamond-like layer, resulting in a locked structure; the plating time is 30-50 minutes.
[0105] In combination with the second aspect, in some embodiments provided in the present application, a diamond-like material is plated on the surface of the transition layer to form a diamond-like layer to obtain a lock structure; the bias voltage of the plated substrate is -200 to -300V.
[0106] In combination with the second aspect, in some embodiments provided in the present application, a diamond-like material is plated on the surface of the transition layer to form a diamond-like layer to obtain a lock structure; the bias pulse frequency of the plated material is 30 to 80 kHz.
[0107] In combination with the second aspect, in some embodiments provided in the present application, a diamond-like material is plated on the surface of the transition layer to form a diamond-like layer to obtain a lock structure; the pressure in the plating furnace is 0.1 to 0.5 Pa.
[0108] It should be noted that the above-mentioned diamond-like carbon material is plated with C target as raw material under inert gas. Under the above-mentioned temperature, time, bias voltage, pulse frequency and intracranial pressure, the prepared DLC coating has high bonding strength, and has good hardness and friction coefficient.
[0109] In a third aspect, the present application provides a locking box mechanism, including a locking structure made of a locking structure of the first aspect or a locking structure of the second aspect.
[0110] It should be noted that the lock box mechanism also includes a driving device (electric push rod or pneumatic push rod), a connecting rod and a lock head matching flange. The lock head is connected to the driving device through the connecting rod, and the linear motion of the driving device is converted into the rotational motion of the lock head. During the locking process, the lock head cooperates with the lock head matching flange to achieve the locking action.
[0111] In a fourth aspect, the present application provides a container transport system, including a locking mechanism of the third aspect.
[0112] The technical solutions provided in this application will be described in detail below in connection with the examples and the accompanying drawings.
[0113] Example 1
[0114] Example 1 of this application provides a locking structure and a preparation method.
[0115] A locking structure includes a locking body of 42CrMo material and a protective layer disposed on the surface of the locking body, wherein the protective layer includes sequentially arranged from the inside to the outside:
[0116] Nitriding layer, thickness is 0.25mm;
[0117] The transition layer has a thickness of 0.8 μm, and the material of the transition layer is Cr; and,
[0118] Diamond-like carbon layer, thickness is 1.5 μm.
[0119] A method for preparing a locking structure, including the following steps:
[0120] The heat-treated lock surface was sandblasted with a sandblasting machine, with a sandblasting distance of 25 cm, a sandblasting angle of 75°, a sandblasting pressure of 0.5 MPa, and a sand particle diameter of 400 mesh. After sandblasting, there was no rust or oil stain on the surface, and fresh metal was exposed. The surface was then cleaned with anhydrous ethanol in an ultrasonic cleaning device for 25 minutes.
[0121] Place the lock in the ion nitriding furnace, close the furnace door and evacuate. When the vacuum degree reaches 70Pa, start arc cleaning, that is, increase the voltage difference between the workpiece and the furnace wall, the substrate voltage is -500V, and the remaining air in the furnace is ionized to produce N + , H + , ions impact the surface impurities, thus achieving the cleaning effect; after the cleaning is completed, H2 and N2 are introduced, and the flow rate is gradually increased as the temperature increases, maintaining the flow rate ratio of H2:N2=3:1, and gradually increasing the negative bias voltage of the substrate. When the heating temperature reaches 450°C, the insulation temperature, voltage, pressure and gas flow rate are set and then the insulation nitriding is started. The nitriding time is 6 hours. After the nitriding is completed, it is cooled with the furnace for standby use;
[0122] Place the lock on the rotary rack in the arc ion coating machine, close the furnace door and turn on the automatic vacuum mode, when the vacuum is pumped to 5×10 -3 Pa, turn on the auxiliary heating wire in the furnace for gradient heating. First, set the heating temperature to 280°C, wait for the temperature to rise to the set value, keep warm for 25 minutes, then set the heating temperature to 450°C, and start the coating process after the temperature rises to 450°C. Coating process: First, introduce a mixed gas of Ar+H2 with a flow rate of 200sccm into the furnace, maintain the pressure in the furnace at 0.8Pa, start the etching Ti target arc to etch and clean the surface of the lock head, and set the substrate bias voltage to -100V. After the etching and cleaning is completed, turn off the etching target arc. Then introduce Ar alone, set the pressure in the furnace to 1.5Pa, turn on the Cr target arc, the target voltage is 30V, the current is 100A, and plate single Cr on the surface of the workpiece for 10 minutes;
[0123] Reduce the temperature in the furnace to 150℃, turn on the inlet of Ar, control the pressure in the furnace by 0.4Pa, turn on the C target arc, base bias voltage -250V, bias pulse frequency 50kHz, prepare diamond-like coating, and coating time 40min.
[0124] Example 2
[0125] Example 2 of this application provides a locking structure and a preparation method.
[0126] A locking structure includes a locking body of 42CrMo material and a protective layer disposed on the surface of the locking body, wherein the protective layer includes sequentially arranged from the inside to the outside:
[0127] Nitriding layer, thickness is 0.25mm;
[0128] Cr layer, 0.15 μm;
[0129] CrN layer, 0.65 μm; and
[0130] Diamond-like carbon layer, thickness is 1.5 μm.
[0131] A method for preparing a locking structure, including the following steps:
[0132] The heat-treated lock surface was sandblasted with a sandblasting machine, with a sandblasting distance of 25 cm, a sandblasting angle of 75°, a sandblasting pressure of 0.5 MPa, and a sand particle diameter of 400 mesh. After sandblasting, there was no rust or oil stain on the surface, and fresh metal was exposed. The surface was then cleaned with anhydrous ethanol in an ultrasonic cleaning device for 25 minutes.
[0133] Place the lock in the ion nitriding furnace, close the furnace door and evacuate. When the vacuum degree reaches 70Pa, start arc cleaning, that is, increase the voltage difference between the workpiece and the furnace wall, the substrate voltage is -500V, and the remaining air in the furnace is ionized to produce N + , H + , ions collide with surface impurities, thus achieving the cleaning effect; after the cleaning is completed, H2 and N2 are introduced, and the flow rate is gradually increased as the temperature increases, maintaining the flow rate ratio of N2:H2=3:1, and gradually increasing the negative bias voltage of the substrate. When the heating temperature reaches 450°C, the insulation temperature, voltage, pressure and gas flow rate are set and then the insulation nitriding is started. The nitriding time is 6 hours. After the nitriding is completed, it is cooled with the furnace for standby use;
[0134] Place the lock on the rotary rack in the arc ion coating machine, close the furnace door and turn on the automatic vacuum mode, when the vacuum is pumped to 5×10 -3 Pa, turn on the auxiliary heating wire in the furnace for gradient heating. First, set the heating temperature to 280℃, wait for the temperature to rise to the set value, keep warm for 25 minutes, then set the heating temperature to 450℃, and start the coating process after the temperature rises to 450℃. Coating process: First, introduce a mixed gas of Ar+H2 with a flow rate of 200sccm into the furnace, maintain the pressure in the furnace at 0.8Pa, start the etching Ti target arc to etch and clean the surface of the lock head, and set the substrate bias voltage to -100V. After the etching and cleaning is completed, turn off the etching target arc. Then introduce Ar alone, set the pressure in the furnace to 1.5Pa, turn on the Cr target arc, the target voltage is 30V, the current is 100A, and plate single Cr on the surface of the workpiece for 10 minutes. Then introduce N2 into the furnace, maintain the pressure at 1.5Pa, and continue to prepare the CrN transition layer on the surface for 40 minutes. After completion, turn off the Cr target arc and close the N2 channel;
[0135] Reduce the temperature in the furnace to 150℃, turn on the inlet of Ar, control the pressure in the furnace by 0.4Pa, turn on the C target arc, base bias voltage -250V, bias pulse frequency 50kHz, prepare diamond-like coating, and coating time 40min.
[0136] Example 3
[0137] Example 3 of this application provides a locking structure and a preparation method.
[0138] A locking structure includes a locking body of 35CrMnSi material and a protective layer disposed on the surface of the locking body, wherein the protective layer includes sequentially arranged from the inside to the outside:
[0139] Nitriding layer, thickness is 0.2mm;
[0140] Cr layer, 0.1 μm;
[0141] CrN layer, 1.0 μm; and
[0142] Diamond-like carbon layer, thickness is 1.0 μm.
[0143] A method for preparing a locking structure, including the following steps:
[0144] The heat-treated lock surface was sandblasted with a sandblasting machine, with a sandblasting distance of 20 cm, a sandblasting angle of 60°, a sandblasting pressure of 0.4 MPa, and a sand particle diameter of 320 mesh. After sandblasting, there was no rust or oil stain on the surface, and fresh metal was exposed. The surface was then cleaned with anhydrous ethanol in an ultrasonic cleaning device for 20 minutes.
[0145] Place the lock in the ion nitriding furnace, close the furnace door and evacuate. When the vacuum degree reaches 60Pa, start arc cleaning, that is, increase the voltage difference between the workpiece and the furnace wall, the substrate voltage is -200V, so that the remaining air in the furnace is ionized to produce N + , H + , ions impact the surface impurities, thus achieving the cleaning effect; after the cleaning is completed, H2 and N2 are introduced, and the flow rate is gradually increased as the temperature increases, maintaining the flow rate ratio of N2:H2=3:1, and gradually increasing the negative bias voltage of the substrate. When the heating temperature reaches 400°C, the insulation temperature, voltage, pressure and gas flow rate are set and then the insulation nitriding is started. The nitriding time is 5h. After the nitriding is completed, it is cooled with the furnace for standby use;
[0146] Place the lock on the rotary rack in the arc ion coating machine, close the furnace door and turn on the automatic vacuum mode, when the vacuum is pumped to 5×10 -3Pa, turn on the auxiliary heating wire in the furnace for gradient heating. First, set the heating temperature to 270℃, wait for the temperature to rise to the set value, keep warm for 20 minutes, then set the heating temperature to 400℃, and wait for the temperature to rise to 460℃ before the coating process. Coating process: First, introduce a mixed gas of Ar+H2 with a flow rate of 180sccm into the furnace, maintain the pressure in the furnace at 0.5Pa, start the etching Ti target arc to etch and clean the surface of the lock head, and set the substrate bias voltage to -30V. After the etching and cleaning is completed, turn off the etching target arc. Then introduce Ar alone, set the pressure in the furnace to 1.0Pa, turn on the Cr target arc, the target voltage is 20V, the current is 80A, and plate single Cr on the surface of the workpiece for 15 minutes. Then introduce N2 into the furnace, maintain the pressure at 1.0Pa, and continue to prepare the CrN transition layer on the surface for 50 minutes. After completion, turn off the Cr target arc and close the N2 channel;
[0147] Reduce the temperature in the furnace to 100℃, turn on the inlet of Ar, control the pressure in the furnace by 0.1Pa, turn on the C target arc, base bias voltage -200V, bias pulse frequency 30kHz, prepare diamond-like coating, and coating time 30min.
[0148] Example 4
[0149] Example 4 of this application provides a locking structure and a preparation method.
[0150] A locking structure includes a locking body of 35CrMnSi material and a protective layer disposed on the surface of the locking body, wherein the protective layer includes sequentially arranged from the inside to the outside:
[0151] Nitriding layer, thickness is 0.3mm;
[0152] Cr layer, 0.2 μm;
[0153] CrN layer, 0.5 μm; and
[0154] Diamond-like carbon layer, thickness is 2 μm.
[0155] A method for preparing a locking structure, including the following steps:
[0156] The heat-treated lock surface was sandblasted with a sandblasting machine, with a sandblasting distance of 30 cm, a sandblasting angle of 90°, a sandblasting pressure of 0.8 MPa, and a sand particle diameter of 500 mesh. After sandblasting, there was no rust or oil stain on the surface, and fresh metal was exposed. The surface was then cleaned with anhydrous ethanol in an ultrasonic cleaning device for 30 minutes.
[0157] Place the lock in the ion nitriding furnace, close the furnace door and evacuate. When the vacuum degree reaches 80Pa, start arc cleaning, that is, increase the voltage difference between the workpiece and the furnace wall, the substrate voltage is -700V, and the remaining air in the furnace is ionized to produce N + , H + , ions impact the surface impurities, thus achieving the cleaning effect; after the cleaning is completed, H2 and N2 are introduced, and the flow rate is gradually increased as the temperature increases, maintaining the flow rate ratio of H2:N2=3:1, and gradually increasing the negative bias voltage of the substrate. When the heating temperature reaches 500°C, the insulation temperature, voltage, pressure and gas flow rate are set and then the insulation nitriding is started. The nitriding time is 8h. After the nitriding is completed, it is cooled with the furnace for standby use;
[0158] Place the lock on the rotary rack in the arc ion coating machine, close the furnace door and turn on the automatic vacuum mode, when the vacuum is pumped to 5×10 -3 Pa, turn on the auxiliary heating wire in the furnace for gradient heating. First, set the heating temperature to 300℃, wait for the temperature to rise to the set value, keep warm for 30 minutes, then set the heating temperature to 470℃, and start the coating process after the temperature rises to 470℃. Coating process: First, introduce a mixed gas of Ar+H2 with a flow rate of 220sccm into the furnace, maintain the pressure in the furnace at 1.0Pa, start the etching Ti target arc to etch and clean the surface of the lock head, and set the substrate bias voltage to -150V. After the etching and cleaning is completed, turn off the etching target arc. Then introduce Ar alone, set the pressure in the furnace to 2.0Pa, turn on the Cr target arc, the target voltage is 40V, the current is 120A, and plate single Cr on the surface of the workpiece for 5 minutes. Then introduce N2 into the furnace, maintain the pressure at 2Pa, and continue to prepare the CrN transition layer on the surface for 30 minutes. After completion, turn off the Cr target arc and close the N2 channel;
[0159] Reduce the temperature in the furnace to 200℃, turn on the inlet of Ar, control the pressure in the furnace by 0.5Pa, turn on the C target arc, base bias voltage -300V, bias pulse frequency 80kHz, prepare diamond-like coating, and coating time 50min.
[0160] Comparative Example 1
[0161] Comparative Example 1 of the present application provides a locking structure similar to Example 1, with the difference being free of nitriding and transition layers.
[0162] Comparative Example 2
[0163] Comparative Example 2 of this application provides a locking structure similar to Example 1, with the difference not containing a diamond-like layer.
[0164] Comparative Example 3
[0165] Comparative Example 3 of this application provides a locking structure containing only the locking body.
[0166] The hardness and friction coefficient of the lock structures of Examples 1 to 4 and Comparative Examples 1 to 4 were tested, and the results are shown in Table 1, where the hardness was tested using the Vickers hardness test method, and the friction coefficient was tested using a friction wear tester. Figure 4 As shown, the friction coefficient of comparative example 1 is shown in FIG. Figure 5 As shown, the friction coefficient of comparative example 2 is shown in FIG. Figure 6 As shown, the friction coefficient of comparative example 3 is shown in FIG. Figure 7 shown.
[0167] Table 1 Performance of locking structures in Examples 1 to 4 and Comparative Examples 1 to 3
[0168] Hardness (HV) Average friction coefficient Example 1 2235 0.20 Example 2 2194 0.22 Example 3 2157 0.20 Example 4 2203 0.21 Comparative Example 1 2204 0.25 Comparative Example 2 1800 0.49 Comparative Example 3 612 0.63
[0169] Since Comparative Example 1 does not contain a nitriding layer and a transition layer, the tested hardness is close to that of the example, but the friction coefficient is larger than that of Example 1. This is because there is no transition layer, the DLC functional layer has low bonding strength, and it is easy to wear during the wear process, resulting in coating failure. The change in the friction coefficient of Comparative Example 1 also reflects this point. When the friction time is about 5 minutes, the friction coefficient rises sharply, which is caused by coating damage.
[0170] Comparative Example 2 Since there is no diamond-like layer, the lock head friction coefficient is smaller than that of the lock head without the protective layer, but it is larger than that of all DLC coatings.
[0171] Since Comparative Example 3 does not contain a protective layer, its hardness is low, the friction coefficient is high, and the friction coefficient fluctuates greatly, and has a tendency to gradually increase, indicating that as the friction test proceeds, the surface condition gradually deteriorates; in actual working conditions, as the number of uses increases, the friction coefficient increases, which is more unfavorable for the release of the lock box mechanism.
[0172] In summary, the high hardness and low friction coefficient of the diamond-like carbon layer can, on the one hand, strengthen the contact surface strength of the lock and reduce the wear caused by long-term friction; on the other hand, it can effectively reduce the friction force, thereby reducing the external force required to release the lock box, and reducing the excessive contact force on the contact surface due to local deformation, which leads to excessive friction torque and jamming. After the metal material is treated with ion nitriding, the surface hardness and elastic modulus will be improved, so the surface deformation resistance will be improved. Under the same force, the surface deformation will be smaller after nitriding, so that the nitrided layer provides good support for the diamond-like carbon layer, reduces the hardness mutation between the diamond-like carbon layer and the substrate, reduces the probability of the diamond-like carbon layer deforming under extrusion and collapsing, and reduces the probability of the lock getting stuck.
[0173] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0174] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.
[0175] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A lock structure, It is characterized in that The invention comprises a lock body and a protective layer arranged on the surface of the lock body, wherein the protective layer comprises the following arranged in sequence from the inside to the outside: Nitriding layer; a transition layer, wherein the material of the transition layer comprises at least one of Cr and CrN; and Diamond-like carbon layer.
2. The lock structure according to claim 1, It is characterized in that The thickness of the nitriding layer is 0.2 to 0.3 mm; and / or, The material of the lock body includes at least one of 35CrMnSi and 42CrMo.
3. The lock structure according to claim 1, It is characterized in that The transition layer includes a Cr layer and a CrN layer arranged in sequence from the inside to the outside, wherein: The thickness of the Cr layer is 0.1 to 0.2 μm; and / or, The thickness of the CrN layer is 0.5 to 1 μm; and / or, The thickness of the diamond-like carbon layer is 1-2 μm.
4. A method for preparing a lock structure according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Perform ion nitriding treatment on the surface of the lock body to obtain a nitrided layer; The material of the transition layer is plated on the surface of the nitriding layer to obtain the transition layer; A diamond-like carbon material is plated on the surface of the transition layer to form a diamond-like carbon layer, thereby obtaining a lock structure.
5. The method for preparing the lock structure according to claim 4, It is characterized in that The ion nitriding treatment is performed on the surface of the lock body to obtain a nitrided layer: The temperature of ion nitridation is 400-500° C.; and / or, The voltage of ion nitridation is -200 to -700 V; and / or, The pressure of ion nitridation is 250-300 Pa; and / or, The time for ion nitriding is 5 to 8 hours.
6. The method for preparing the lock structure according to claim 4, It is characterized in that The material of the transition layer plated on the surface of the nitriding layer, the transition layer comprises: Plating a Cr layer material on the surface of the nitrided layer to obtain a Cr layer; CrN is deposited on the surface of the Cr layer to form a CrN layer, thereby obtaining a transition layer.
7. The method for preparing the lock structure according to claim 6, It is characterized in that The substrate bias voltage of the Cr-plated layer is 20-40V; and / or, The target current for coating the Cr layer is 80 to 120A; and / or, The coating time of the Cr layer is 5 to 15 minutes; and / or, The pressure in the furnace for plating the Cr layer is 1-2 Pa; and / or, The temperature of the Cr coating is 450-470°C; and / or, The time for forming the CrN layer is 30 to 50 minutes.
8. The method for preparing the lock structure according to claim 4, It is characterized in that The diamond-like material is plated on the surface of the transition layer to form a diamond-like layer, thereby obtaining a lock structure; The plating temperature is 100-200°C; and / or, The plating time is 30 to 50 minutes; and / or, The plated substrate bias voltage is -200 to -300 V; and / or, The bias pulse frequency of the coating is 30 to 80 kHz; and / or, The pressure inside the plating furnace is 0.1~0.5Pa.
9. A lock box mechanism, It is characterized in that It comprises a lock head structure as described in any one of claims 1 to 3, or a lock head structure made by the preparation method of the lock head structure as described in any one of claims 4 to 8.
10. A container transportation system, It is characterized in that Comprising the lock box mechanism as claimed in claim 9.
Citation Information
Patent Citations
Diamond-like film and preparation method thereof
CN102658684A
Metal and diamond-like material composite coating and preparation method and application thereof as well as coating tool
CN107858684A
Method for plating diamond-like coating on surface of automobile transmission component and automobile transmission component
CN113802087A
Coating method applied to aluminum alloy processing cutter made of tool steel
CN114045458A
Thickened anti-theft lock seat, lockset device and container
CN215056308U