Device and method for measuring volume expansion and shrinkage rate of controllable low-strength material in hardening process

By designing a volume expansion and contraction measurement device including containers, fixtures and laser rangefinders, the problem that the prior art is difficult to reflect the multi-dimensional volume changes of controllable low-strength materials is solved, and the high volume stability of the material is achieved Accuracy evaluation.

CN118937152APending Publication Date: 2024-11-12GUANGDONG XINTANG SONG NEW TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411306887.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing volume stability testing methods are difficult to accurately reflect the volume changes of controllable low-strength materials in the multi-dimensional direction, making it difficult to evaluate their volume stability in practical applications.

Method used

A volume expansion and contraction measurement device including a container, a fixture and a laser rangefinder is designed to form a sphere by filling a controllable low-strength material into an elastic bag and suspending it in water, using a test cylinder and a correction cylinder to measure the liquid. surface change, accurately calculate the volume change rate.

Benefits of technology

It can more accurately reflect the subtle volume changes of controllable low-strength materials during hardening, help evaluate the possible volume stability problems in practical applications, and improve the measurement accuracy and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937152A_ABST
    Figure CN118937152A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of expansion and shrinkage rate determination, and discloses a controllable low-strength material hardening process volume expansion and shrinkage rate determination device and a determination method. The measuring device comprises a container, and a fixing device used for fixing a ball is arranged in the container. The ball body is an elastic bag filled with a raw material of a controllable low-strength material; a test measuring cylinder and a correction measuring cylinder are fixedly arranged on the upper surface of the container, the test measuring cylinder is communicated with the container, and the correction measuring cylinder is not communicated with the container; the test measuring cylinder and the correction measuring cylinder are symmetrically arranged around the central point of the upper surface of the container. The provided measuring device can reflect the fine change condition of the volume of the controllable low-strength material in multiple dimensions in the hardening process, so that the volume expansion and shrinkage rate is measured and calculated, and the volume stability problem possibly occurring in the actual application process of the controllable low-strength material can be evaluated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of expansion and contraction rate measurement, and mainly to a device and method for measuring the volume expansion and contraction rate of a controllable low-strength material during a hardening process. Background Art

[0002] According to the definition of the American Concrete Institute, controlled low-strength material (CLSM) is a backfill material with high fluidity that can be self-compacted under the action of its own weight without or with little vibration. Its 28-day unconfined compressive strength shall not exceed 8.3MPa, but must be greater than 0.3MPa.

[0003] In general, controlled low-strength materials are mainly composed of water, cement and fine aggregate. However, due to its lower strength requirements, controlled low-strength materials are also the perfect carrier for many wastes and by-products. The American Concrete Institute also proposed that as long as the performance test is carried out before the experiment and the strength requirements are met, any available industrial waste can be used to replace aggregates to prepare controlled low-strength materials. At the same time, because of the self-compacting, self-leveling and low-cost working characteristics of controlled low-strength materials, they are widely used in geotechnical engineering such as structural backfill, pipeline lining, void filling, road base, bridge access, etc.

[0004] At present, controllable low-strength materials often have problems such as cracking or volume shrinkage during use, which will affect the performance of controllable low-strength materials and affect their use. The existing indoor test method for volume stability is difficult to accurately evaluate the volume stability of controllable low-strength materials, affecting the applicability judgment of controllable low-strength materials. For example, in the "Autoclaved Aerated Concrete Performance Test Method" (GB / T11969-2020), measuring heads are bonded at both ends of the 40mm×40mm×160mm specimen, and then the length change over time is measured to calculate the drying shrinkage value. During the test, the measuring head is easy to fall off, resulting in inaccurate measurement results and test failure. Moreover, the existing volume stability test method mainly measures the length change in the linear direction, which is difficult to reflect the volume change caused by the multi-dimensional direction of the controllable low-strength material. Therefore, the existing technology still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a device for measuring the volume expansion and contraction rate of a controllable low-strength material during the hardening process, aiming to solve the problem that the existing volume stability test method is difficult to reflect the volume changes caused by the multi-dimensional directions of the controllable low-strength material.

[0006] The technical solution of this application is as follows: In a first aspect, the present application provides a device for measuring the volume expansion and contraction rate of a controllable low-strength material during hardening, wherein the device comprises a container, wherein a fixing device for fixing a sphere is provided in the container; The sphere is an elastic bag for filling with raw materials of controllable low-strength material; A test cylinder and a correction cylinder are fixedly arranged on the upper surface of the container, the test cylinder is in communication with the interior of the container, and the correction cylinder is not in communication with the interior of the container; The test measuring cylinder and the correction measuring cylinder are centrally symmetrically arranged about the center point of the upper surface of the container.

[0007] The volume expansion and contraction rate measuring device provided in the present application can reflect the subtle changes in the volume of the controllable low-strength material during the hardening process, thereby calculating the volume expansion and contraction rate of the controllable low-strength material, which is helpful to evaluate the volume stability problems that may arise in the actual application of the controllable low-strength material.

[0008] Furthermore, the fixing device includes a net bag and a plurality of hooks, and the hooks fix the net bag so that the net bag does not contact the inner wall of the container. The net bag and the hooks fix the sphere so that it is suspended in the water without floating or sinking, which can better reflect the overall volume change of the controllable low-strength material.

[0009] Furthermore, the container comprises a barrel body and a barrel cover.

[0010] Further, some of the hooks are fixedly arranged at the bottom of the barrel, and some of the hooks are fixedly arranged at the inner surface of the barrel cover. The density of the sphere as a whole is compared with the density of water, and then the hooks at the bottom of the barrel or the inner surface of the barrel cover are selected as needed to ensure that the sphere is suspended in the water.

[0011] Furthermore, a drain valve is provided at the bottom of the barrel body, and an exhaust valve is provided at the center of the barrel cover.

[0012] Furthermore, a sealing ring is fixedly installed on the inner edge of the barrel cover, and the top end of the barrel body abuts against the sealing ring; The side wall of the barrel body is provided with a buckle for fixing the barrel cover.

[0013] Furthermore, the volume of the container is not less than 50L; The elastic bag is a balloon, and the size of the balloon is 36 inches.

[0014] Furthermore, a transparent cover is provided on the measuring cylinder openings of the test measuring cylinder and the correction measuring cylinder; The transparent cover is provided with a penetrating pinhole.

[0015] Furthermore, a first laser rangefinder and a second laser rangefinder are fixedly arranged on the upper surface of the container, the detection port of the first laser rangefinder is aligned with the liquid level of the liquid column in the test cylinder, and the detection port of the second laser rangefinder is aligned with the liquid level of the liquid column in the correction cylinder.

[0016] In a second aspect, the present application further provides a method for measuring the volume expansion and contraction rate of a controllable low-strength material during hardening as described in the first aspect, wherein the method comprises the following steps: Preparing raw materials of controllable low-strength materials and measuring the wet density of the raw materials of controllable low-strength materials; The raw material of the controllable low-strength material is poured into the elastic bag and the elastic bag is in an expanded state, and the bag is sealed to obtain a sphere, and the initial volume of the sphere is measured, and the density of the sphere is measured. The difference between the wet density of the raw material of the controllable low-strength material and the density of the sphere does not exceed 50 kg / m 3 ; Filling water into a container, placing the sphere into the container and fixing the sphere in the water by the fixing device; Fill the test cylinder with water until a liquid column appears in the test cylinder, read the initial liquid level value of the test cylinder, fill the correction cylinder with water, and read the initial liquid level value of the correction cylinder; At a preset age, reading the liquid level value of the test measuring cylinder, reading the liquid level value of the correction measuring cylinder, and obtaining the volume change of the sphere during the age according to the changes in the liquid level values ​​of the test measuring cylinder and the correction measuring cylinder during the age; The volume change of the sphere during the age is compared with the initial volume of the sphere to obtain the volume expansion and contraction rate of the controllable low-strength material during the age.

[0017] Beneficial effect: The volume expansion and contraction rate measuring device provided in the present application can reflect the subtle changes in the volume of the controllable low-strength material during the hardening process, thereby calculating the volume expansion and contraction rate of the controllable low-strength material, which is helpful to evaluate the volume stability problems that may occur in the actual application of the controllable low-strength material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a physical picture of the device for measuring the volume expansion and contraction rate during the hardening process of controllable low-strength materials in this application.

[0019] Figure 2 This is a schematic diagram of the structure of a device for measuring the volume expansion and contraction rate during the hardening process of a controllable low-strength material in this application.

[0020] Figure 3 This is a schematic diagram of the structure of a device for measuring the volume expansion and contraction rate during the hardening process of a controllable low-strength material in this application.

[0021] Figure 4 This is a schematic diagram of the steps of the measuring method of the device for measuring the volume expansion and contraction rate during the hardening process of controllable low-strength materials in this application.

[0022] Figure 5 This is a schematic diagram of the dimensions of a laser rangefinder.

[0023] Figure 6 The volume expansion and contraction rate data of the controllable low-strength material of Examples 1-3 of the present application within 120 hours of the hardening process.

[0024] Explanation of reference numerals: 1. Container; 11. Barrel body; 111. Drain valve; 112. Buckle; 12. Barrel cover; 121. Exhaust valve; 122. Sealing ring; 21. Test measuring cylinder; 22. Correction measuring cylinder; 23. First laser rangefinder; 24. Second laser rangefinder; 25. Transparent cover; 26. Laser rangefinder column; 3. Fixing device; 31. Net bag; 32. Hook; 4. Sphere. DETAILED DESCRIPTION

[0025] The present application provides a device and method for measuring the volume expansion and contraction rate of a controllable low-strength material during hardening. To make the purpose, technical solution and effect of the present application clearer and more specific, the present application is further described in detail below. It should be understood that the specific implementation methods described herein are only used to explain the present application and are not used to limit the present application.

[0026] like Figure 1-Figure 3 As shown, the present application is a device for measuring the volume expansion and contraction rate of a controllable low-strength material hardening process, which includes a container 1, in which a fixing device 3 for fixing a sphere 4 is arranged; The sphere 4 is an elastic bag for being filled with raw materials of controllable low-strength material; A test cylinder 21 and a correction cylinder 22 are fixedly arranged on the upper surface of the container 1. The test cylinder 21 is connected to the interior of the container 1, while the correction cylinder 22 is not connected to the interior of the container 1. The test measuring cylinder 21 and the correction measuring cylinder 22 are arranged symmetrically about the center point of the upper surface of the container 1 .

[0027] By setting the test cylinder 21 and the correction cylinder 22 symmetrically about the center point of the upper surface of the container 1 , the correction cylinder 22 can synchronously reflect the influence of environmental factors on the reading measurement, so as to correct the reading of the test cylinder 21 .

[0028] The volume expansion and contraction rate measuring device provided in the present application can reflect the subtle changes in the volume of the controllable low-strength material during the hardening process, thereby calculating the volume expansion and contraction rate of the controllable low-strength material, which is helpful to evaluate the volume stability problems that may arise in the actual application of the controllable low-strength material.

[0029] like Figure 4 As shown, the present application also provides a method for measuring the volume expansion and contraction rate of the controllable low-strength material hardening process as described above, which includes the following steps: (1) Prepare the raw material of the controllable low-strength material and measure the wet density of the raw material of the controllable low-strength material: r 0; (2) Pour the raw material of the controllable low-strength material into the elastic bag and make the elastic bag expand, seal it to obtain the sphere 4, and measure the mass of the sphere 4 M 1 and initial volume V 1. Measure the density of sphere 4 r 1, r 0 and r The difference between 1 and 50 kg / m 3 ; (3) Pour water into the container 1, place the sphere 4 into the container 1 and fix the sphere 4 in the water by the fixing device 3; (4) Fill the test cylinder 21 with water until a liquid column appears in the test cylinder 21, and read the initial liquid level value of the test cylinder 21. L 0, add water to the correction cylinder 22, and read the initial liquid level value of the correction cylinder 22 L '0; (5) At the preset age n days, read the liquid level value of the test cylinder 21 L n , read the liquid level value of the correction cylinder 22 L ' n According to the changes in the liquid level values ​​of the test cylinder 21 and the correction cylinder 22 during the age, the volume change of the sphere 4 during the age is obtained. V ; (6) The volume change of sphere 4 during the age period △ V With the initial volume of sphere 4 V 1, and the volume expansion and contraction rate e of the controllable low-strength material during the age is obtained. v .

[0030] In step (2), the comparison r 0 and r 1, r 0 and r The difference between 1 and 50 kg / m 3 ;like r 0 and r 1 The difference between the two exceeds 50kg / m 3 The steps of the assay method are restarted.

[0031] The density of sphere 4 is r 1 is represented by formula (I): ——Formula (I); Volume change of sphere 4 during the age period△ V It is expressed as formula (II): ——Formula (II); Controllable volume expansion and contraction rate of low-strength materials over time v It is expressed as formula (III): ——Formula (III); In the above formula, r 0——Wet density of raw materials of controllable low-strength materials (kg / m 3 ); M 1——The mass of the sphere 4 after the raw material of the controllable low-strength material is poured (kg); V 1——The volume of the sphere 4 after the raw material of the controllable low-strength material is poured (m 3 ); r 1——Density of the sphere 4 after the raw material of the controllable low-strength material is poured (kg / m 3 ); L 0——the initial liquid level value of the test cylinder 21 (ml); L n ——the liquid level value of the test cylinder 21 at the age of n days (ml); L '0——the initial liquid level value of the correction cylinder 22 (ml); L ' n ——the liquid level value of the correction measuring cylinder 22 at the age of n days (ml); Δ V ——Volume change of sphere 4 during the age period (ml); e v ——Volume expansion and contraction rate of controllable low-strength material at the age of n days (%).

[0032] Among them, step (2) measures r 1, compare r 1 and r 0, density calculation is accurate to 1kg / m 3 , r 1 and r The difference between 0 and 50kg / m 3 , the test is successful, and the subsequent determination method steps are continued; if r 1 and r The difference between 0 and 50 kg / m 3, then re-mix and restart the steps of the determination method. The wet density of the raw materials of the controllable low-strength material will affect its strength and volume change. r 1 and r 0, the larger the difference is, the larger the error of the measured volume expansion and contraction rate is.

[0033] Among them, the raw material of the controllable low-strength material is slurry. The room temperature and water temperature during the test can be controlled at 20±2℃. The volume change value is calculated accurately to 0.1ml, and the volume expansion and contraction rate is calculated accurately to 0.01%. When ev﹥0, it means volume expansion; when ev﹤0, it means volume contraction.

[0034] In the present application, a controllable low-strength material is filled into a balloon to form a whole. As the volume shrinks or expands due to the hydration reaction of cementitious materials such as cement, the balloon will also shrink or expand, thereby causing the volume of water in the sealed container 1 to expand or shrink. The change in the volume of the balloon is represented by reading the numerical change of the liquid level in the test cylinder 21.

[0035] Specifically, the fluidity of controllable low-strength materials is generally high, and moisture is easily separated from powder or aggregate, which also includes foam lightweight soil mixed with air. The present application pours the controllable low-strength materials into elastic bags for testing, which can better simulate the usage conditions. Moreover, when the controllable low-strength materials are poured and used, in order to reduce the adverse effects of moisture evaporation, the surface is covered with a film and watered to maintain moisture. Therefore, the provided measuring device and measuring method reflect the volume change caused by the transition from fluid to solid under a moisturizing state.

[0036] In the present application, the poured sphere 4 is ensured to have a density close to that of the controllable low-strength material, the elastic bag is basically filled with the slurry, and before hardening, the elastic bag remains in close contact with the slurry, and the volume of the elastic bag will change with the volume of the slurry. Then, by filling the container 1 with water, the water completely wraps the sphere 4 filled with the controllable low-strength material. The change in the amount of water can directly reflect the volume change of the controllable low-strength material caused by the multi-dimensional direction during the hardening process. Even if the raw material is a controllable low-strength material (foam lightweight soil) including air foam, the expansion and contraction rate can be reflected in time.

[0037] Specifically, the elastic bag may also be other elastic materials that can be loaded with raw materials of controllable low-strength materials and can reflect volume changes in liquids, preferably a balloon.

[0038] In a specific embodiment of the present application, the test cylinder 21 and the correction cylinder 22 have the same specifications and shapes. The test cylinder 21 is connected to the inside of the container 1 to reflect the volume change in the container 1, and the correction cylinder 22 is not connected to the inside of the container 1. By using the correction cylinder 22 as a correction for the rise and fall of the liquid level caused by factors such as liquid evaporation and thermal expansion and contraction deformation during the test process, the rise and fall of the liquid level caused by the volume change of the test sample can be more accurately reflected to reduce the measurement error. Among them, both the test cylinder 21 and the correction cylinder 22 can use a cylinder with a test range of 100ml and an accuracy of 1ml.

[0039] In a specific embodiment of the present application, the fixing device 3 includes a net bag 31 and a plurality of hooks 32, and the hooks 32 fix the net bag 31 so that the net bag 31 does not contact the inner wall of the container 1. In the present application, the sphere 4 is placed in the net bag 31 and fixed by the hooks 32, so as to ensure that the hardening process is carried out stably, reduce the impact on the volume expansion and contraction rate, and fix the sphere 4 so that it is suspended in the water and does not float or sink, which can better reflect the overall volume change of the controllable low-strength material. Among them, the net bag 31 can be made of nylon.

[0040] Specifically, in step (3) of the method for measuring the volume expansion and contraction rate of a controllable low-strength material hardening process provided by the device, the steps of filling water into the container 1, placing the sphere 4 into the container 1, and fixing the sphere 4 in the water by the fixing device 3 include: (31) Pour water into the container 1, put the sphere 4 into the net bag 31, and hang the net bag 31 on the hook 32 to fix the sphere 4 in the water.

[0041] In a specific embodiment of the present application, the container 1 includes a barrel body 11 and a barrel cover 12 .

[0042] Specifically, in step (3) of the measuring method of the provided device for measuring the volume expansion and contraction rate during the hardening process of a controllable low-strength material, injecting water into the container 1 is specifically injecting water into the barrel body 11.

[0043] In a specific embodiment of the present application, part of the hook 32 is fixedly arranged at the bottom of the barrel body 11, and part of the hook 32 is fixedly arranged on the inner surface of the barrel cover 12. Figure 2 As shown, when the sphere 4 is heavier than water as a whole, a hook 32 is provided on the inner surface of the barrel cover 12 so that the sphere 4 is fixedly suspended in the water without contacting the barrel cover 12 or the bottom of the barrel body 11; Figure 3 As shown, when the sphere 4 is lighter than water as a whole, a hook 32 is provided at the bottom of the barrel 11 to ensure that the sphere 4 does not float up and contact the barrel cover 12. Among them, by providing multiple hooks 32, it can be ensured that the sphere 4 is subjected to a relatively uniform force, and it is easy to show multi-dimensional volume changes, and the performance of the controllable low-strength material can be more accurately grasped.

[0044] Specifically, step (3) of the method for measuring the volume expansion and contraction rate of a controllable low-strength material hardening process provided by the device specifically comprises the following steps: (30) Compare the density of sphere 4 r 1 and the density of water r 水 ; (31) Pour water into container 1. r 1< r 水 When the net bag 31 is hung on the hook 32 fixedly arranged at the bottom of the barrel body 11, the fixed ball 4 is suspended in the water; r 1> r 水 When the net bag 31 is hung on the hook 32 fixedly arranged on the inner surface of the bucket cover 12, the fixed sphere 4 is suspended in the water.

[0045] in, r 水 ——Density of water (kg / m 3 ).

[0046] When the density of sphere 4 r 1 and the density of water r 水 At the same time, the ball 4 can be fixed by the hook 32 at the bottom of the barrel body 11 or the inner surface of the barrel cover 12, tighten the net bag 31 and suspend the ball 4 in the water. During the test phase, the water body is not disturbed and the net bag 31 is prevented from contacting the inner wall of the container 1.

[0047] In a specific embodiment of the present application, a drain valve 111 is provided at the bottom of the barrel body 11. The drain valve 111 is provided to facilitate drainage for the next test.

[0048] In a specific embodiment of the present application, an exhaust valve 121 is provided at the center of the barrel cover 12. If there is air in the container 1, the test accuracy will also be affected. When measuring, the exhaust valve 121 can be opened, and water can be added to the test cylinder 21 until the water is full and overflows from the exhaust valve 121, and then the exhaust valve 121 can be closed to complete the exhaust.

[0049] Specifically, in step (4) of the measuring method of the device for measuring the volume expansion and contraction rate of the controllable low-strength material hardening process, the step of filling the test cylinder 21 with water until a liquid column appears comprises: (41) Fill the barrel 11 with water, cover the barrel cover 12, open the exhaust valve 121, and pour water into the test cylinder 21 until the water overflows from the exhaust valve 121. Close the exhaust valve 121 and continue to pour water into the test cylinder 21 until a liquid column appears in the test cylinder 21.

[0050] The liquid level of the liquid column is above 1 / 3 of the test cylinder 21. This prevents the controllable low-strength material to be tested from shrinking to a large extent, causing the liquid level to fall into the container 1 and cannot be read.

[0051] In a specific embodiment of the present application, a sealing ring 122 is fixedly installed on the inner edge of the barrel cover 12, and the top of the barrel body 11 abuts against the sealing ring 122; the side wall of the barrel body 11 is provided with a buckle 112 for fixing the barrel cover 12. By providing the sealing ring 122 and the buckle 112, the barrel cover 12 can be fixed and well sealed at the same time. If the sealing is not done properly, the reading of the test cylinder 21 will have a large error, affecting the measurement accuracy of the expansion and contraction rate.

[0052] Specifically, in step (41) of the method for measuring the volume expansion and contraction rate of the controllable low-strength material hardening process, after closing the barrel cover 12, the step of fastening the buckle 112 is also included.

[0053] In a specific embodiment of the present application, the volume of the container 1 is not less than 50L; the elastic bag is a balloon, and the size of the balloon is 36 inches. When the balloon is filled with the controllable low-strength material as the sphere 4, the volume is not less than 10L, but smaller than the volume of the container 1. By using a container 1 and a balloon of sufficient size, the error factors therein are avoided from having a greater impact on the expansion and contraction rate data, and the actual situation of the volume change of the controllable low-strength material is more easily reflected.

[0054] In a specific embodiment of the present application, a transparent cover 25 is provided on the measuring cylinder mouth of the test measuring cylinder 21 and the correction measuring cylinder 22; a penetrating pinhole is provided on the transparent cover 25. The transparent cover 25 is used to reduce the evaporation of water in the measuring cylinder into the air and reduce the error caused by the evaporation. The penetrating pinhole (not shown in the drawings) provided on the transparent cover 25 can ensure that the pressure difference between the inside and outside of the measuring cylinder is consistent, avoiding the influence on the change of the liquid level in the measuring cylinder.

[0055] Specifically, in step (4) of the measuring method of the device for measuring the volume expansion and contraction rate of the controllable low-strength material hardening process, after water is filled to the test cylinder 21 until a liquid column appears, the following steps are also included: The transparent cover 25 is placed on the measuring cylinder opening of the test measuring cylinder 21 . After water is filled into the correction measuring cylinder 22 , the following steps are also included: the transparent cover 25 is placed on the measuring cylinder opening of the correction measuring cylinder 22 .

[0056] In a specific embodiment of the present application, a first laser rangefinder 23 and a second laser rangefinder 24 are fixedly arranged on the upper surface of the container 1, the detection port of the first laser rangefinder 23 is aligned with the liquid level of the liquid column in the test cylinder 21, and the detection port of the second laser rangefinder 24 is aligned with the liquid level of the liquid column in the correction cylinder 22.

[0057] Specifically, Figure 2 As shown, the first laser rangefinder 23 and the second laser rangefinder 24 are fixedly connected to the upper surface (barrel cover 12) of the container 1 through the laser rangefinder column 26, ensuring that the detection port can be aligned with the liquid column in the measuring cylinder for distance measurement. The transparent cover 25 made of transparent material does not affect the penetration of the laser signal, which facilitates distance measurement. Figure 5 As shown, both the first laser rangefinder 23 and the second laser rangefinder 24 can use a laser rangefinder of model BL-200NZ-485, with a test range of 120mm-280mm, an accuracy of 0.2mm, and can automatically record data in real time.

[0058] Specifically, in the measuring method of the provided device for measuring the volume expansion and contraction rate during the hardening process of controllable low-strength materials, the liquid level reading of the test cylinder 21 is read by the first laser rangefinder 23, and the liquid level reading of the correction cylinder 22 is read by the second laser rangefinder 24.

[0059] Furthermore, before reading, a float or a piece of paper is placed on the liquid surface of the test cylinder 21 and the liquid surface of the correction cylinder 22. By placing a float or a piece of paper on the liquid surface, it is convenient to reflect the laser signal for distance measurement.

[0060] More specifically, the method for measuring the volume expansion and contraction rate of a controllable low-strength material hardening process provided by the present application comprises the following steps: (A) In a room with a room temperature of 20±2℃, prepare the raw materials of controllable low-strength materials that meet the requirements, with a volume of not less than 15L, and test the wet density of the raw materials of controllable low-strength materials r 0; (B) Pour the raw material of the controllable low-strength material into a balloon with a size of 36 inches, so that the balloon is in an expanded state with a volume of not less than 10L (not greater than the volume of the container 1). After the filling is completed, seal the balloon to obtain the sphere 4, and measure the mass of the sphere 4 M 1 and initial volume V 1. Measure the density of sphere 4 r 1, r 0 and r The difference between 1 and 50 kg / m 3 ; (C) Compare the density of sphere 4 r 1 and the density of water r 水 ; (D) Pour water into the barrel 11 and put the ball 4 into the nylon net bag 31. r 1< r 水 When the net bag 31 is hung on the hook 32 fixedly arranged at the bottom of the barrel body 11, the fixed ball 4 is suspended in the water; r 1> r水 When the net bag 31 is hung on the hook 32 fixedly arranged on the inner surface of the barrel cover 12, the fixed ball 4 is suspended in the water; (E) Fill the barrel 11 with water, cover the barrel cover 12, fasten the buckle 112, open the exhaust valve 121, and fill water from the test cylinder 21 until the water overflows from the exhaust valve 121, close the exhaust valve 121, and continue to fill water into the test cylinder 21 until a liquid column appears in the test cylinder 21, and the liquid level of the liquid column is above 1 / 3 of the test cylinder 21. Put a buoy or a piece of paper on the liquid surface of the test cylinder 21, cover the mouth of the cylinder with a transparent cover 25 with a penetrating pinhole, and turn on the first laser rangefinder 23 to read the initial liquid level value of the test cylinder 21. L 0, add water to the correction cylinder 22, place a float or paper on the liquid surface of the correction cylinder 22, cover the mouth of the cylinder with a transparent cover 25 with a penetrating pinhole, turn on the second laser rangefinder 24 to read the initial liquid level value of the correction cylinder 22 L '0; (F) At the preset age of 1, 2, ... n days, the liquid level value of the test cylinder 21 is read by the first laser rangefinder 23 L 1. L 2...... L n , the liquid level value of the correction cylinder 22 is read by the second laser rangefinder 24 L '1, L '2...... L ' n According to the changes in the liquid level values ​​of the test cylinder 21 and the correction cylinder 22 during the age, the volume change of the sphere 4 during the age of 1, 2...n days is obtained. V ; (G) After the test is finished, the readings of the first laser rangefinder 23, the second laser rangefinder 24, the test cylinder 21 and the correction cylinder 22 are recorded, the first laser rangefinder 23 and the second laser rangefinder 24 are turned off, the drain valve 111 is opened, and the sphere 4 is taken out.

[0061] (H) Arrange the test data, perform data correction, and calculate the expansion and contraction rate e within the age period v .

[0062] The density of sphere 4 is r 1 is expressed as formula (I), the volume change during the age period △ V Expressed as formula (II), the expansion and contraction rate within the age period e v It is expressed as formula (III): ——Formula (I); ——Formula (II); ——Formula (III).

[0063] The container 1 may be a stainless steel drum (barrel body 11 + barrel cover 12 ) with an outer diameter of 425 mm and a height of 400 mm, and a volume of not less than 50 L. The drain valve 111 may be disposed at a position 20 mm from the bottom of the barrel body 11 .

[0064] The present application fills a balloon with no less than 10L of controllable low-strength material slurry, and reflects the volume change caused by the controllable low-strength material in water after a certain age on the rise and fall of the liquid level in the test measuring cylinder 21, so as to indicate the volume change of the controllable low-strength material during hardening, thereby obtaining the expansion and contraction rate of the controllable low-strength material during the age.

[0065] The invention is further described below by means of specific examples.

[0066] Example 1 The controllable low-strength material of Example 1 is pure cement lightweight soil. The expansion and contraction rate of the pure cement lightweight soil is measured by the provided controllable low-strength material hardening process volume expansion and contraction rate measuring device. The measuring method includes the following steps: (A) In a room with a room temperature of 20±2℃, prepare the raw materials of pure cement lightweight soil that meet the requirements, with a volume of not less than 15L, and test the wet density of the raw materials of pure cement lightweight soil r 0; (B) Pour the raw materials of pure cement lightweight soil into a balloon with a size of 36 inches, so that the balloon is in an expanded state with a volume of not less than 10L (not greater than the volume of container 1). After the filling is completed, seal the balloon to obtain sphere 4 and measure the mass of sphere 4 M 1 and initial volume V 1. Measure the density of sphere 4 r 1, r 0 and r The difference between 1 and 50 kg / m 3 ; (C) Compare the density of sphere 4 r 1 and the density of water r 水 ; (D) Pour water into the barrel 11, put the ball 4 into the nylon net bag 31, hang the net bag 31 on the hook 32 fixed at the bottom of the barrel 11, and suspend the ball 4 in the water; (E) Fill the barrel 11 with water, cover the barrel cover 12, fasten the buckle 112, open the exhaust valve 121, and fill water from the test cylinder 21 until the water overflows from the exhaust valve 121, close the exhaust valve 121, and continue to fill water into the test cylinder 21 until a liquid column appears in the test cylinder 21, and the liquid level of the liquid column is above 1 / 3 of the test cylinder 21. Put a small piece of paper on the liquid level of the test cylinder 21, cover the mouth of the cylinder with a transparent cover 25 with a penetrating pinhole, and turn on the first laser rangefinder 23 to read the initial liquid level value of the test cylinder 21. L 0, add water to the correction cylinder 22, put a small piece of paper on the liquid level of the correction cylinder 22, cover the mouth of the cylinder with a transparent cover 25 with a penetrating pinhole, turn on the second laser rangefinder 24 to read the initial liquid level value of the correction cylinder 22 L '0; (F) At the preset age n hours, the liquid level value of the test cylinder 21 is read by the first laser rangefinder 23 L n , the liquid level value of the correction cylinder 22 is read by the second laser rangefinder 24 L ' n According to the changes in the liquid level values ​​of the test cylinder 21 and the correction cylinder 22 during the age, the volume change of the sphere 4 during the age of n hours is obtained. V ; (G) After the test is finished, the readings of the first laser rangefinder 23, the second laser rangefinder 24, the test cylinder 21 and the correction cylinder 22 are recorded, the first laser rangefinder 23 and the second laser rangefinder 24 are turned off, the drain valve 111 is opened, and the sphere 4 is taken out.

[0067] (H) Arrange the test data, perform data correction, and calculate the expansion and contraction rate of pure cement lightweight soil during the age period e v .

[0068] The density of sphere 4 is r 1 is expressed as formula (I), the volume change during the age period △ V Expressed as formula (II), the expansion and contraction rate within the age period e v It is expressed as formula (III): ——Formula (I); ——Formula (II); ——Formula (III).

[0069] The container 1 of Example 1 is a stainless steel drum (drum body 11 + drum cover 12 ) with an outer diameter of 425 mm and a height of 400 mm, and a volume of not less than 50 L. The drain valve 111 is arranged at a position 20 mm from the bottom of the drum body 11 .

[0070] The wet density of the raw material of pure cement lightweight soil in Example 1 is 730 kg / m 3 .

[0071] Example 2 The determination steps of Example 2 are basically the same as those of Example 1, except that the controllable low-strength material determined in Example 2 is desulfurized ash lightweight soil, and the wet density of the raw material of desulfurized ash lightweight soil in Example 2 is 814 kg / m 3 .

[0072] Example 3 The measurement steps of Example 3 are basically the same as those of Example 1, except that the controllable low-strength material measured in Example 3 is fly ash lightweight soil, and the wet density of the fly ash lightweight soil raw material in Example 3 is 735 kg / m 3 .

[0073] The volume expansion and contraction rates of the controllable low-strength materials of Examples 1-3 within 120 hours are as follows: Figure 6 It can be found that the device for measuring the volume expansion and contraction rate during the hardening process of a controllable low-strength material and the corresponding measuring method provided in the present application can reflect the volume changes in multiple dimensions during the hardening process of a controllable low-strength material and can also effectively measure the expansion and contraction rate.

[0074] It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made according to the above description, and all these improvements and changes should fall within the scope of protection of the present application.

Claims

1. A device for measuring the volume expansion and contraction rate of a controllable low-strength material during hardening, characterized in that: It comprises a container (1), wherein a fixing device (3) for fixing a sphere (4) is arranged inside the container (1); The sphere (4) is an elastic bag for being filled with raw materials of controllable low-strength material; A test measuring cylinder (21) and a correction measuring cylinder (22) are fixedly arranged on the upper surface of the container (1); the test measuring cylinder (21) is in communication with the interior of the container (1), and the correction measuring cylinder (22) is not in communication with the interior of the container (1); The test measuring cylinder (21) and the correction measuring cylinder (22) are arranged symmetrically about the center point of the upper surface of the container (1).

2. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 1, characterized in that: The fixing device (3) comprises a net bag (31) and a plurality of hooks (32), wherein the hooks (32) fix the net bag (31) so that the net bag (31) does not contact the inner wall of the container (1).

3. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 2, characterized in that: The container (1) comprises a barrel body (11) and a barrel cover (12).

4. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 3, characterized in that: Part of the hook (32) is fixedly arranged at the bottom of the barrel body (11), and part of the hook (32) is fixedly arranged on the inner surface of the barrel cover (12).

5. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 3, characterized in that: A drainage valve (111) is provided at the bottom of the barrel body (11), and an exhaust valve (121) is provided at the center of the barrel cover (12).

6. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 5, characterized in that: A sealing ring (122) is fixedly mounted on the inner edge of the barrel cover (12), and the top end of the barrel body (11) abuts against the sealing ring (122); The side wall of the barrel body (11) is provided with a buckle (112) for fixing the barrel cover (12).

7. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 1, characterized in that: The volume of the container (1) is not less than 50L; The elastic bag is a balloon, and the size of the balloon is 36 inches.

8. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 1, characterized in that: The measuring cylinder openings of the test measuring cylinder (21) and the correction measuring cylinder (22) are provided with transparent covers (25); The transparent cover (25) is provided with a penetrating pinhole.

9. The device for measuring volume expansion and contraction rate during hardening process of controllable low-strength material according to claim 8, characterized in that: A first laser rangefinder (23) and a second laser rangefinder (24) are fixedly arranged on the upper surface of the container (1); a detection port of the first laser rangefinder (23) is aligned with the liquid surface of the liquid column in the test measuring cylinder (21), and a detection port of the second laser rangefinder (24) is aligned with the liquid surface of the liquid column in the correction measuring cylinder (22).

10. A method for measuring the volume expansion and contraction rate of a controllable low-strength material during hardening process according to any one of claims 1 to 9, characterized in that: The following steps are involved: Preparing raw materials of controllable low-strength material, and measuring the wet density of the raw materials of controllable low-strength material; The raw material of the controllable low-strength material is poured into the elastic bag and the elastic bag is expanded, and the bag is sealed to obtain a sphere (4), and the initial volume of the sphere (4) is measured, and the density of the sphere (4) is measured. The difference between the wet density of the raw material of the controllable low-strength material and the density of the sphere (4) does not exceed 50 kg / m 3 ; Filling the container (1) with water, placing the sphere (4) into the container (1), and fixing the sphere (4) by the fixing device (3) so as to suspend it in the water; Filling the test cylinder (21) with water until a liquid column appears in the test cylinder (21), reading the initial liquid level value of the test cylinder (21), and filling the correction cylinder (22) with water, reading the initial liquid level value of the correction cylinder (22); At a preset age, reading the liquid level value of the test cylinder (21), reading the liquid level value of the correction cylinder (22), and obtaining the volume change of the sphere (4) during the age according to the change of the liquid level values ​​of the test cylinder (21) and the correction cylinder (22) during the age; The volume change of the sphere (4) during the age is compared with the initial volume of the sphere (4), so as to obtain the volume expansion and contraction rate of the controllable low-strength material during the age.

Citation Information

Patent Citations

  • Device and method for determining self-shrinkage of cement-based material

    CN104155433A

  • Device and method for measuring free swell ratio of slurry

    CN104406650A

  • Expansion and shrinkage testing device in process from plasticity to condensation of self-leveling mortar

    CN220381129U

Cited By

  • Detection device for expansion rate of joint mixture

    CN120352584A

  • Foam light soil with low mixing amount of desulfurized fly ash and preparation method of foam light soil

    CN121270178A