Preparation method of thermal conversion oxidation product of Bi-doped Cu prussian blue compound
CuBi2O4@Co3O4 material was prepared by thermal conversion and oxidation method of Bi-doped Cu Prussian blue compounds, which solved the problem of insufficient performance of the negative electrode material of the supercapacitor, achieved high specific capacitance and good rate performance, and was suitable for the negative electrode of the supercapacitor.
Patent Information
- Application Number
- CN202411157107.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
The performance of the negative electrode materials of existing supercapacitors is insufficient, especially the energy density of asymmetric supercapacitors is limited, and most metal organic framework materials have poor electrical conductivity, making it difficult to apply in negative electrode materials.
CuBi2O4@Co3O4 material was prepared by thermal conversion oxidation method using Bi-doped CuPrussian blue compounds, and CuBi-PBAs precursors were synthesized by hydrothermal method, and thermal conversion products were obtained by solid phase calcination, maintaining their morphological structure and forming calcium. Titanium-type composite oxides improve electrochemical performance.
The prepared CuBi2O4@Co3O4 material has excellent electrochemical properties, including high specific capacitance, good rate performance and cycle stability. It is suitable for supercapacitor negative electrode materials, effectively limiting the capacitance attenuation caused by volume expansion and contraction during charging and discharging. .
Smart Images

Figure CN118942925A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of supercapacitor electrode materials, and in particular relates to a preparation method and application of a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound. Background Art
[0002] Supercapacitors (SCs), also known as electrochemical capacitors, are unconventional energy devices based on the principle of electrochemical energy conversion. They are new energy storage devices between rechargeable batteries and traditional capacitors. They have attracted widespread attention for their fast charging and discharging speeds, long cycle life, and high output power. For example, supercapacitors are now used in hybrid platforms for heavy vehicles, trucks, and buses, as well as to store regenerative braking energy for electric vehicles and light rail. However, the electrochemical performance of supercapacitors depends mainly on excellent electrode materials. Significant progress has been made in finding positive electrode materials. In contrast, the energy density of asymmetric supercapacitors is mainly limited by the negative electrode materials.
[0003] Metal-organic frameworks (MOFs) are a new type of porous crystalline material composed of metal cations and organic ligands. Due to their high specific surface area and large internal pore size, they have attracted extensive attention in the field of supercapacitors. However, due to their poor conductivity, most MOFs are used as sacrificial precursors to prepare their derivatives to improve electrochemical performance. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound and its application in view of the deficiencies in the above-mentioned prior art. The CuBi-PBAs prepared by the method have a rough and porous surface, and after thermal conversion, they shrink unevenly and undergo ligand pyrolysis, and the product surface becomes smooth. The morphology of the synthesized CuBi2O4@Co3O4 material product remains intact, the arrangement is uniform, and the electrochemical performance is excellent, and it is widely used in the negative electrode of supercapacitors.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound, the method comprising:
[0006] S1. Dissolve polyethylene glycol in deionized water containing acetic acid, stir magnetically until completely dissolved, add Cu(NO3)2·3H2O and Bi(NO3)3·5H2O, stir magnetically to mix evenly, and obtain solution a;
[0007] Add K3[Co(CN)6] into deionized water and stir magnetically until completely dissolved to obtain solution b;
[0008] The solution b is added to the solution a, and the mixture is evenly mixed by magnetic stirring at room temperature, and C6H5Na3O7 is added for treatment to obtain a solution c;
[0009] S2, subjecting the solution c obtained in S1 to a hydrothermal reaction, filtering under reduced pressure after the reaction is completed, washing the separated precipitate, and vacuum drying to obtain a Prussian blue-like compound, i.e., a CuBi-PBAs precursor;
[0010] S3. Under air atmosphere, the CuBi-PBAs precursor obtained in S1 is annealed, and after naturally cooling to room temperature, a thermal conversion oxidation product of Bi-doped Cu-based Prussian blue compound is obtained, namely, CuBi2O4@Co3O4 material.
[0011] Preferably, the usage ratio of the polyethylene glycol and the deionized water containing acetic acid in S1 is (0.5-1) g:30 mL.
[0012] Preferably, the molar ratio of Cu(NO3)2·3H2O, Bi(NO3)3·5H2O, K3[Co(CN)6], and C6H5Na3O7 in S1 is (2~4)mmol:(2~4)mmol:2mmol:9mmol.
[0013] Preferably, the hydrothermal reaction temperature in S2 is 40° C. to 80° C., and the hydrothermal reaction time is 4 h to 6 h.
[0014] Preferably, the pore size of the filter material used for filtering in S2 is 0.22 μm to 0.45 μm;
[0015] The washing method is: first washing with ionized water for 3 to 5 times, and then washing with anhydrous ethanol for 3 to 5 times;
[0016] The vacuum drying temperature is 60° C. to 80° C., and the vacuum drying time is 8 h to 12 h.
[0017] Preferably, the annealing method in S3 is: heating from room temperature to 500° C. to 750° C. at a heating rate of 3° C. / min to 8° C. / min, and annealing at a constant temperature for 1 h to 3 h.
[0018] The present invention also provides the use of the thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound prepared by the above preparation method, and the thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound is used in the negative electrode of a supercapacitor.
[0019] Preferably, when the thermally converted oxidation product of the Bi-doped Cu-based Prussian blue compound is used in the negative electrode of a supercapacitor, the -1The specific capacitance at the current density is 897.6F·g -1 ~951F·g -1 , and the current density is 10A·g -1 The specific capacitance under the condition of 1A·g -1 The current density is 72.4% to 87.3% of the initial specific capacitance.
[0020] Prussian blue (PB) and its analogs (PBAs) are a type of MOF. Their special molecular architecture between metal and organic ligands and their nanoporous structure bring special chemical and physical properties. As a coordination polymer, Prussian blue-like compounds are used as precursors or transition products to synthesize other target products, which is one of their major uses. By heat-treating Prussian blue-like compounds in air, this type of metal organic framework is converted into metal oxides with special structures through thermal conversion. The thermal conversion products prepared with Prussian blue-like compounds as precursors have the same morphology and structure as the precursors, with fast and reversible electrolyte diffusion rate and efficient ion transmission path. At the same time, it also ensures that the material does not change significantly in the long-term charge and discharge process, and has the advantage of stability.
[0021] Cu-based oxides have high redox activity and open pore structures, which are conducive to the transport of ions. The metal oxides obtained by using PBAs as precursors have open pore structures, which shorten the path for ion migration in the electrode / electrolyte and provide a large number of active sites for redox reactions. Bi doping can construct a heterojunction structure to enhance the conductivity of the material, increase the speed and depth of ion shuttle in the electrolyte, and improve not only the rate performance of the material, but also the specific capacity of the material. CuBi2O4@Co3O4 material is a perovskite-type composite oxide structure with a wide working window at negative potentials, and can be used as a negative electrode material for supercapacitors.
[0022] The present invention synthesizes CuBi-PBAs material uniformly doped with Bi as a precursor by hydrothermal method, and then thermally transforms it by solid phase calcination method to obtain CuBi2O4 and Co3O4 assemblies with perovskite structure, and precisely controls the morphology of CuBi-PBAs and its thermal transformation products at the molecular level to synthesize Bi-doped Cu-based Prussian blue analogs with good monodispersity. The present invention designs a hydrothermal method to synthesize CuBi-PBAs material under acidic conditions using polyethylene glycol aqueous solution as solvent. Polyethylene glycol can be adsorbed on the surface of the material to become a barrier to prevent particle aggregation, and acidic conditions can effectively inhibit Bi 3+Hydrolysis, C6H5Na3O7 as a chelating agent, has a strong chelating ability in the acidic range, through the strong binding effect between the chelating agent molecules and metal ions, it can form a compound with higher stability and larger molecular weight. The synthesized CuBi-PBAs material is annealed in air to obtain the assembled CuBi2O4@Co3O4 material. Due to the variable morphology and structure of Prussian blue-like compounds, the conversion product has the same morphology and structure as the precursor. At the same time, because the C and N elements in the cyanide bond are oxidized in an oxygen-containing atmosphere and converted into CO2, NO x At the same time, combined with the intrinsic pore structure of the metal organic framework material, the target product has more special properties than traditional metal oxide bulk materials. The product has a perovskite-type composite oxide structure and has good stability.
[0023] Compared with the prior art, the present invention has the following advantages:
[0024] The invention provides a preparation method of a Bi-doped Cu-type Prussian blue compound and its thermal conversion product. Cu(NO3)2·3H2O, Bi(NO3)3·5H2O, and K3[Co(CN)6] are used as raw materials, a CuBi-PBAs precursor is synthesized by a hydrothermal method, and then a thermal conversion product CuBi2O4@Co3O4 material is obtained by a solid phase calcination method. The synthesized CuBi-PBAs precursor has a thick rhombus sheet structure, which can promote the physical adsorption of electrolyte ions on the electrode surface and the redox ability of the material. The Prussian blue-like compound can become a high-performance electrode material through the porous structural characteristics and high charge transfer ability. The thermal conversion product forms a dense and smooth prismatic CuBi2O4@Co3O4 material on the basis of maintaining the structure of the CuBi-PBAs precursor. As a multi-metal composite oxide, it not only has a high specific capacitance, but also can form a synergistic effect between different metal phases, which can effectively limit the capacitance attenuation caused by the volume expansion and contraction of the material during the charging and discharging process. CuBi2O4@Co3O4 material is a perovskite composite metal oxide with a special crystal structure, non-stoichiometric oxygen, and metals existing in a mixed valence state. It has good stability, high redox activity, high specific capacitance, and good electrochemical properties such as rate performance and cycle stability. It can be widely used in supercapacitor negative electrode materials.
[0025] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the CuBi-PBAs precursor prepared in Example 1 of the present invention.
[0027] Figure 2This is the SEM image of the thermal conversion product CuBi2O4@Co3O4 material prepared in Example 1 of the present invention.
[0028] Figure 3 XRD patterns of the CuBi-PBAs precursor and the thermal conversion product CuBi2O4@Co3O4 material prepared in Example 1 of the present invention and the corresponding standard cards.
[0029] Figure 4 The cyclic voltammograms of the thermal conversion product CuBi2O4@Co3O4 material prepared in Example 1 of the present invention at different scan rates.
[0030] Figure 5 This is a constant current charge and discharge diagram of the thermal conversion product CuBi2O4@Co3O4 material prepared in Example 1 of the present invention at different current densities.
[0031] Figure 6 This is a cycle performance diagram of the thermal conversion product CuBi2O4@Co3O4 material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] Example 1
[0033] The method for preparing the thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound of this embodiment is as follows:
[0034] S1. Dissolve 0.5 g of polyethylene glycol in 30 mL of deionized water containing 5 mL of glacial acetic acid, stir at 500 r / min for 15 min until completely dissolved, add 3 mmol of Cu(NO3)2·3H2O and 3 mmol of Bi(NO3)3·5H2O, stir at 600 r / min for 25 min until completely dissolved, to obtain solution a; the average molecular weight of the polyethylene glycol is 6000;
[0035] 2 mmol K3[Co(CN)6] was added into 30 mL deionized water and stirred at 500 r / min for 15 min until completely dissolved to obtain solution b.
[0036] The solution b was added dropwise to the solution a, and the mixture was stirred at 500 r / min for 25 min at room temperature until the mixture was uniformly mixed. 9 mmol C6H5Na3O7 was added, and the mixture was stirred at 600 r / min for 25 min at room temperature until the mixture was uniformly mixed, to obtain a solution c.
[0037] S2, the solution c obtained in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and a hydrothermal reaction was carried out at a temperature of 60°C for 5 hours. After the reaction was completed, the solution was filtered under reduced pressure through a water-based microporous filter membrane with a pore size of 0.22 μm, and the filtration speed was controlled to leave the filtrate in droplets. The separated precipitate was washed, first with deionized water for 5 times, then with anhydrous ethanol for 5 times, and then vacuum dried at a temperature of 60°C for 12 hours to obtain a light blue Prussian blue-like compound, i.e., a CuBi-PBAs precursor;
[0038] SEM image of CuBi-PBAs precursor, such as Figure 1 As shown, the CuBi-PBAs precursor is composed of thick rhombic flake structures with a rough surface and a porous structure;
[0039] S3. Spread 1 g of the CuBi-PBAs precursor obtained in S1 with a thickness of 2 mm into a 99% alumina square crucible, place the crucible in a muffle furnace, and perform annealing treatment in an air atmosphere. The annealing method is: heating from room temperature to 750°C at a heating rate of 5°C / min, and annealing at a constant temperature for 2 hours; after naturally cooling to room temperature, a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound is obtained, namely, the CuBi2O4@Co3O4 material.
[0040] The SEM image of the thermal conversion product CuBi2O4@Co3O4 material prepared in this example is as follows Figure 2 As shown, the thermal conversion product CuBi2O4@Co3O4 material has a prismatic structure, which is similar to the precursor structure. Due to the uneven shrinkage of the material and the pyrolysis of the ligand during the heat treatment process, the surface is smooth and presents a dense and porous structure.
[0041] Figure 3This is the XRD pattern of the CuBi-PBAs precursor and the thermal conversion product CuBi2O4@Co3O4 material prepared in this embodiment and the corresponding standard card. As shown in the figure, by comparing with the standard spectrum, it is obtained that the CuBi-PBAs precursor corresponds perfectly to the orthorhombic Cmcm crystal structure, and the sample is pure. It can be seen that the thermal conversion product CuBi2O4@Co3O4 material has diffraction peaks at 2θ=20.04°, 27.98°, 33.30°, 46.68°, 52.90° and 55.64°, corresponding to the (200), (211), (130), (141), (123), and (332) crystal planes of CuBi2O4, respectively, proving that the composite material does contain CuBi2O4 material. Diffraction peaks appear at 2θ=36.84, 38.74, 55.64, 65.28, and 74.38, corresponding to the (311), (222), (422), (440), and (620) crystal planes of Co3O4, respectively, proving that the composite material does contain Co3O4 components and the material is a CuBi2O4@Co3O4 multi-metal material oxide assembly.
[0042] Figure 4 This is the cyclic voltammogram of the thermal conversion product CuBi2O4@Co3O4 material prepared in the embodiment of the present invention at different scan rates. As shown in the figure, an obvious redox peak can be seen through the CV curve, which can prove that the material is a typical pseudocapacitive material; in addition, as the scan rate increases, the peak current of the redox peak increases significantly, indicating that the redox rate on the electrode is accelerated; at the same time, the overall shape of the curve does not change much, and the corresponding redox peak is well maintained, which means that the polarization phenomenon of the electrode is not obvious.
[0043] This embodiment also provides an application of a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound prepared by the above preparation method, wherein the thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound is applied in a negative electrode of a supercapacitor.
[0044] The CuBi2O4@Co3O4, acetylene black and PVDF prepared in this embodiment were mixed in a mass ratio of 8:1:1, where PVDF refers to a solution obtained by dissolving PVDF in anhydrous ethanol. The three were mixed and ground into a uniform slurry, which was applied on a 1×10 cm nickel foam and compacted under a pressure of 15 MPa. The vacuum drying was continued for 10 h to obtain the CuBi2O4@Co3O4 negative electrode material. The prepared negative electrode material was assembled into a standard three-electrode system for electrochemical performance testing, where the platinum electrode was the counter electrode, the calomel electrode was the reference electrode, and the electrolyte was 6MKOH. The measured results are as follows: Figure 5-6 shown.
[0045] Figure 5The constant current charge and discharge diagram of the thermal conversion product CuBi2O4@Co3O4 material prepared in this example at different current densities is shown in the figure. -1 The specific capacitances at different current densities are 951, 912.4, 885, 856, and 830 F·g -1 , indicating that the material has a high specific capacitance and the current density is 10A·g -1 The specific capacitance can still maintain 1A·g -1 The initial specific capacitance at the current density is 87.3%, which also shows that the material has good rate performance.
[0046] Figure 6 The cycle performance diagram of the CuBi2O4@Co3O4 composite material prepared in this example is shown in the figure. -1 At a current density of , the specific capacitance can still maintain 54.11% of the initial value after 3000 cycles, indicating that the material has good cycle stability.
[0047] Example 2
[0048] The method for preparing the thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound of this embodiment is as follows:
[0049] S1. Dissolve 1 g of polyethylene glycol in 30 mL of deionized water containing 5 mL of glacial acetic acid, stir at 500 r / min for 15 min until completely dissolved, add 4 mmol of Cu(NO3)2·3H2O and 2 mmol of Bi(NO3)3·5H2O, stir at 600 r / min for 25 min until completely dissolved, to obtain solution a; the average molecular weight of the polyethylene glycol is 6000;
[0050] 2 mmol K3[Co(CN)6] was added into 30 mL deionized water and stirred at 500 r / min for 15 min until completely dissolved to obtain solution b.
[0051] The solution b was added dropwise to the solution a, and the mixture was stirred at 500 r / min for 25 min at room temperature until the mixture was uniformly mixed. 9 mmol C6H5Na3O7 was added, and the mixture was stirred at 600 r / min for 25 min at room temperature until the mixture was uniformly mixed, to obtain a solution c.
[0052] S2, the solution c obtained in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and a hydrothermal reaction was carried out at a temperature of 80°C for 4 hours. After the reaction was completed, the solution was filtered under reduced pressure through a water-based microporous filter membrane with a pore size of 0.22 μm, and the filtration speed was controlled to leave the filtrate in droplets. The separated precipitate was washed, first with deionized water for 5 times, then with anhydrous ethanol for 5 times, and then vacuum dried at a temperature of 80°C for 8 hours to obtain a light blue Prussian blue-like compound, i.e., a CuBi-PBAs precursor;
[0053] S3. Spread 1 g of the CuBi-PBAs precursor obtained in S1 with a thickness of 2 mm into a 99% alumina square crucible, place the crucible in a muffle furnace, and perform annealing treatment in an air atmosphere. The annealing method is: heating from room temperature to 750°C at a heating rate of 8°C / min, and annealing at a constant temperature for 1 hour; after naturally cooling to room temperature, a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound is obtained, namely, the CuBi2O4@Co3O4 material.
[0054] This embodiment also provides an application of a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound prepared by the above preparation method, wherein the thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound is applied in a negative electrode of a supercapacitor.
[0055] The method for preparing the negative electrode of the supercapacitor is the same as that in Example 1.
[0056] The CV test of CuBi2O4@PPy prepared in this example at different scan rates can prove that the material is a typical pseudocapacitive material, and the polarization phenomenon of the electrode is not obvious. The constant current charge and discharge test at different current densities can calculate that the constant current charge and discharge at 1, 2, 5, 8, and 10 A·g -1 The specific capacitances at different current densities are 855.8, 758, 675, 624, and 620 F·g -1 , indicating that the material has a high specific capacitance. And the current density is 10A·g -1 The specific capacitance can still maintain 1A·g -1 The initial specific capacitance at current density is 72.4%, which also shows that the material has good rate performance.
[0057] Example 3
[0058] The method for preparing the thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound of this embodiment is as follows:
[0059] S1. Dissolve 1 g of polyethylene glycol in 30 mL of deionized water containing 5 mL of glacial acetic acid, stir at 500 r / min for 15 min until completely dissolved, add 2 mmol of Cu(NO3)2·3H2O and 4 mmol of Bi(NO3)3·5H2O, stir at 600 r / min for 25 min until completely dissolved, to obtain solution a; the average molecular weight of the polyethylene glycol is 6000;
[0060] 2 mmol K3[Co(CN)6] was added into 30 mL deionized water and stirred at 500 r / min for 15 min until completely dissolved to obtain solution b.
[0061] The solution b was added dropwise to the solution a, and the mixture was stirred at 500 r / min for 25 min at room temperature until the mixture was uniformly mixed. 9 mmol C6H5Na3O7 was added, and the mixture was stirred at 600 r / min for 25 min at room temperature until the mixture was uniformly mixed, to obtain a solution c.
[0062] S2, the solution c obtained in S1 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and a hydrothermal reaction was carried out at a temperature of 40°C for 6 hours. After the reaction was completed, the solution was filtered under reduced pressure through a water-based microporous filter membrane with a pore size of 0.45 μm, and the filtration speed was controlled to leave the filtrate in droplets. The separated precipitate was washed, first with deionized water for 3 times, then with anhydrous ethanol for 3 times, and then vacuum dried at a temperature of 60°C for 12 hours to obtain a light blue Prussian blue-like compound, i.e., a CuBi-PBAs precursor;
[0063] S3. Spread 1 g of the CuBi-PBAs precursor obtained in S1 with a thickness of 2 mm into a 99% alumina square crucible, place the crucible in a muffle furnace, and perform annealing treatment in an air atmosphere. The annealing method is: heating from room temperature to 500°C at a heating rate of 3°C / min, and annealing at a constant temperature for 3 hours; after naturally cooling to room temperature, a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound is obtained, namely, the CuBi2O4@Co3O4 material.
[0064] This embodiment also provides an application of a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound prepared by the above preparation method, wherein the thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound is applied in a negative electrode of a supercapacitor.
[0065] The method for preparing the negative electrode of the supercapacitor is the same as that in Example 1.
[0066] The CV test of CuBi2O4@PPy prepared in this example at different scan rates proves that the material is a typical pseudocapacitive material, and the polarization phenomenon of the electrode is not obvious. The constant current charge and discharge test at different current densities can calculate that the constant current charge and discharge at 1, 2, 5, 8, and 10 A·g -1 The specific capacitances at different current densities are 897.6, 873.6, 819, 756.8, and 750 F·g -1 , indicating that the material has a high specific capacitance. And the current density is 10A·g -1 The specific capacitance can still maintain 1A·g -1 The initial specific capacitance at the current density is 83.6%, which also shows that the material has good rate performance.
[0067] In summary, the present invention designs a method of synthesizing a CuBi-PBAs precursor by a hydrothermal method, and then obtaining its thermal conversion product, CuBi2O4@Co3O4 material, by a solid phase calcination method. The CuBi-PBAs precursor prepared by this method has a rough surface and a porous structure, which is conducive to the rapid diffusion of electrons during the charge and discharge process, has a fast and reversible electrolyte diffusion rate, an efficient ion transmission path and a stable structure, can promote the physical adsorption of electrolyte ions on the electrode surface, and improve the redox activity of the material. Its thermal conversion product, on the basis of maintaining the structure of the CuBi-PBAs precursor, forms a dense and smooth prismatic CuBi2O4@Co3O4 material, whose special crystal structure effectively improves the electron transport capacity of the electrode material, is not easy to collapse during the charge and discharge cycle, is more stable, not only has a higher specific capacitance, but also can form a synergistic effect between different metal phases, effectively limiting the capacitance attenuation caused by the volume expansion and contraction of the material during the charge and discharge process. The CuBi2O4@Co3O4 material becomes a high-performance electrode material with high specific capacitance, good rate performance and cycle stability, and can be widely used in supercapacitor negative electrode materials.
[0068] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound, characterized in that: The method is: S1. Dissolve polyethylene glycol in deionized water containing acetic acid, stir magnetically until completely dissolved, add Cu(NO3)2·3H2O and Bi(NO3)3·5H2O, stir magnetically to mix evenly, and obtain solution a; Add K3[Co(CN)6] into deionized water and stir magnetically until completely dissolved to obtain solution b; The solution b is added to the solution a, and the mixture is evenly mixed by magnetic stirring at room temperature, and C6H5Na3O7 is added for treatment to obtain a solution c; S2, subjecting the solution c obtained in S1 to a hydrothermal reaction, filtering under reduced pressure after the reaction is completed, washing the separated precipitate, and vacuum drying to obtain a Prussian blue-like compound, i.e., a CuBi-PBAs precursor; S3. Under air atmosphere, the CuBi-PBAs precursor obtained in S1 is annealed, and after naturally cooling to room temperature, a thermal conversion oxidation product of Bi-doped Cu-based Prussian blue compound is obtained, namely, CuBi2O4@Co3O4 material.
2. The method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound according to claim 1, characterized in that: The usage ratio of the polyethylene glycol and the deionized water containing acetic acid in S1 is (0.5-1) g:30 mL.
3. The method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound according to claim 1, characterized in that: The molar ratio of Cu(NO3)2·3H2O, Bi(NO3)3·5H2O, K3[Co(CN)6], and C6H5Na3O7 in S1 is (2~4)mmol:(2~4)mmol:2mmol:9mmol.
4. The method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound according to claim 1, characterized in that: The hydrothermal reaction temperature in S2 is 40° C. to 80° C., and the hydrothermal reaction time is 4 h to 6 h.
5. The method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound according to claim 1, characterized in that: The pore size of the filter material used for filtration in S2 is 0.22 μm to 0.45 μm; The washing method is: first washing with ionized water for 3 to 5 times, and then washing with anhydrous ethanol for 3 to 5 times; The vacuum drying temperature is 60° C. to 80° C., and the vacuum drying time is 8 h to 12 h.
6. The method for preparing a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound according to claim 1, characterized in that: The annealing method in S3 is: heating from room temperature to 500° C. to 750° C. at a heating rate of 3° C. / min to 8° C. / min, and annealing at a constant temperature for 1 h to 3 h.
7. An application of a thermal conversion oxidation product of a Bi-doped Cu-based Prussian blue compound prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound is used in the negative electrode of a supercapacitor.
8. The use according to claim 7, characterized in that: When the thermal conversion oxidation product of the Bi-doped Cu-based Prussian blue compound is used in the negative electrode of a supercapacitor, the -1 The specific capacitance at the current density is 897.6F·g -1 ~951F·g -1 , and the current density is 10A·g -1 The specific capacitance under the condition of 1A·g -1 The current density is 72.4% to 87.3% of the initial specific capacitance.