Method for transferring silicon layers
By implanting H2+, H+ and He+ ions into a single-crystal silicon donor substrate and annealing to form a damaged layer, the problem of time-consuming and uneven silicon layer transfer in the prior art is solved, realizing efficient and low-cost ultra-thin silicon layer transfer, which is suitable for the preparation of silicon structures on fully depleted insulators.
Patent Information
- Application Number
- CN202410992502.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-08
- Filing Date
- 2019-05-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies for transferring silicon layers from donor substrates to disposal substrates are time-consuming, expensive, and have poor thickness uniformity, especially when fabricating extremely thin silicon layers, where efficient layer transfer is difficult to achieve.
H2+, H+, or a combination of H2+ and H+ and He+ ions are implanted into a silicon dioxide layer on the front surface of a monocrystalline silicon donor substrate, followed by annealing at low temperature to form a damaged layer, and then splitting after bonding to transfer a silicon layer with a thickness between about 500 angstroms and about 2500 angstroms.
This technology enables efficient and low-cost transfer of ultrathin silicon layers from donor substrates to treatment substrates, ensuring thickness uniformity and applicability to the fabrication of silicon-on-insulator structures, thereby reducing production costs.
Smart Images

Figure CN118943075A_ABST
Abstract
Description
[0001] Information about divisional applications
[0002] This case is a divisional application. The parent case of the divisional application is an invention patent application with application date of May 23, 2019, application number 201980038984.3, and invention name “Method for transferring a silicon thin layer”.
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS
[0004] This application claims the benefit of priority to U.S. Provisional Application No. 62 / 682,228, filed on June 8, 2018, the disclosure of which is incorporated by reference as if set forth in its entirety. Technical Field
[0005] The present invention relates generally to the field of semiconductor wafer fabrication. More specifically, the present invention relates to a method of transferring a thin silicon layer from a donor substrate to a handle substrate in the fabrication of a silicon-on-insulator structure. Background Art
[0006] Semiconductor wafers are generally prepared from a single crystal ingot, such as a silicon ingot, which is trimmed and ground to have one or more planes or cuts for proper orientation of the wafer in subsequent processes. The ingot is then cut into individual wafers. Although reference will be made herein to semiconductor wafers constructed from silicon, other materials may be used to prepare semiconductor wafers, such as germanium, silicon carbide, silicon germanium, gallium arsenide, and other alloys of Group III and Group V elements, such as gallium nitride or indium phosphide, or alloys of Group II and Group VI elements, such as cadmium sulfide or zinc oxide.
[0007] Semiconductor wafers, such as silicon wafers, can be used to prepare composite layer structures. Composite layer structures, such as semiconductors on insulators, and more specifically, silicon on insulator (SOI) structures, generally include a handle wafer or layer, a device layer, and an insulating (i.e., dielectric) film (usually an oxide layer) between the handle layer and the device layer. The thickness of the device layer is generally between 0.01 microns and 20 microns, such as between 0.05 microns and 20 microns. A thick film device layer may have a device layer thickness between about 1.5 microns and about 20 microns. A thin film device layer may have a thickness between about 0.01 microns and about 0.20 microns. In general, composite layer structures such as silicon on insulator (SOI), silicon on sapphire (SOS), and silicon on quartz are produced by bringing two wafers into close contact, thereby inducing bonding by van der Waal forces, followed by heat treatment to strengthen the bonding. Annealing can convert terminal silanol groups into siloxane bonds between the two interfaces, thereby strengthening the bonding.
[0008] After the thermal anneal, the bonded structure is further processed to remove a large portion of the donor wafer to achieve the layer transfer. For example, a wafer thinning technique such as etching or grinding, commonly referred to as etch-back SOI (i.e., BESOI), may be used in which a silicon wafer is bonded to a handle wafer and then the silicon wafer is slowly etched away until only a thin layer of silicon remains on the handle wafer. See, for example, U.S. Pat. No. 5,189,500, the disclosure of which is incorporated herein by reference as if fully set forth. This method is time consuming and expensive, wastes one of the substrates, and generally does not have suitable thickness uniformity for layers less than a few microns.
[0009] Another common method of achieving layer transfer utilizes hydrogen implantation followed by thermally induced delamination. Particles (atoms or ionized atoms, such as hydrogen atoms or a combination of hydrogen and helium atoms) are implanted at a specific depth below the front surface of the donor wafer. The implanted particles form a cleavage plane in the donor wafer at the specific depth at which they are implanted. The surface of the donor wafer is cleaned to remove organic compounds or other contaminants, such as boron compounds, that were deposited on the wafer during the implantation process.
[0010] Next, the front surface of the donor wafer is bonded to the handle wafer by a hydrophilic bonding process to form a bonded wafer. Prior to bonding, the donor wafer and / or the handle wafer are activated by exposing the surfaces of the wafers to a plasma containing, for example, oxygen or nitrogen. Exposure to the plasma modifies the structure of the surfaces in a process commonly referred to as surface activation, which renders the surface of one or both of the donor wafer and the handle wafer hydrophilic. Additionally, the surface of the wafer may be chemically activated by a wet treatment such as SCI cleaning or hydrofluoric acid. The wet treatment and plasma activation may occur in either order, or the wafer may be subjected to only one treatment. Next, the wafers are pressed together and a bond is formed therebetween. Due to van der Waals forces, this bond is relatively weak and must be strengthened before further processing can occur.
[0011] In some processes, the hydrophilic bond between the donor wafer and the handle wafer (i.e., the bonding wafer) is strengthened by heating or annealing the bonded wafer pair. In some processes, the wafer bonding may occur at a low temperature, such as between about 300° C. and about 500° C. In some processes, the wafer bonding may occur at an elevated temperature, such as between about 800° C. and about 1100° C. The elevated temperature causes covalent bonds to form between the adjoining surfaces of the donor wafer and the handle wafer, thereby solidifying the bond between the donor wafer and the handle wafer. While the bonded wafer is being heated or annealed, the particles previously implanted in the donor wafer weaken the cleavage plane.
[0012] Next, a portion of the donor wafer is separated (i.e., cleaved) from the bonded wafer along a cleavage plane to form an SOI wafer. The cleavage may be performed by placing the bonded wafer in a fixture, wherein a mechanical force is applied perpendicular to the opposing side of the bonded wafer to pull a portion of the donor wafer away from the bonded wafer. According to some methods, a suction cup is used to apply the mechanical force. The partial separation of the donor wafer is induced by applying a mechanical wedge at the edge of the bonded wafer at the cleavage plane to induce crack propagation along the cleavage plane. Next, the mechanical force applied by the suction cup pulls a portion of the donor wafer away from the bonded wafer, thereby forming an SOI wafer.
[0013] According to other methods, the bonded pair may instead be subjected to a period of high temperature to separate a portion of the donor wafer from the bonded wafer. Exposure to high temperature causes cracks to initiate and propagate along the cleavage plane, thereby separating a portion of the donor wafer. The cracks are formed due to the formation of voids by the implanted ions (which grow by Ostwald ripening). The voids are filled with hydrogen and helium. The voids become thin plates. The pressurized gas in the thin plates propagates microcavities and microcracks, which weaken the silicon on the implanted surface. If the annealing is stopped at the appropriate time, the weakened bonded wafer can be split by a mechanical process. However, if the heat treatment continues for a longer time and / or occurs at a higher temperature, the microcracks propagate to the extent that all cracks merge along the cleavage plane, thereby separating a portion of the donor wafer. This method allows for better uniformity of the transfer layer and allows the donor wafer to be recycled, but generally requires heating the implant and bonded pair to a temperature close to 500°C. Summary of the invention
[0014] The present invention is directed to a method of transferring a silicon layer from a single crystal silicon donor substrate to a handling substrate, the method comprising: (a) implanting H through a silicon dioxide layer in contact with a front surface of the single crystal silicon donor substrate and through the front surface of the single crystal silicon donor substrate; 2 + Ions, H + Ion or H 2 + Ions and H + The single crystal silicon donor substrate comprises two parallel main surfaces (one of which is the front surface and the other of which is the rear surface), a circumferential edge connecting the front surface and the rear surface, a central plane between the front surface and the rear surface, a central axis perpendicular to the front surface, and a bulk region between the front surface and the rear surface; (b) implanting He through the silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate and through the front surface of the single crystal silicon donor substrate +ions; (c) annealing the ion-implanted single crystal silicon donor substrate at a temperature and for a duration sufficient to form a damage layer in the single crystal silicon donor substrate; (d) bonding the silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate to a dielectric layer in contact with the handling substrate to thereby prepare a multi-layer substrate; (e) annealing the multi-layer substrate; and (f) splitting the annealed multi-layer substrate at the damaged layer in the single crystal silicon donor substrate to thereby transfer the silicon layer having a thickness between about 500 angstroms and about 2500 angstroms from the single crystal silicon donor substrate to the handling substrate.
[0015] Other objects and features will be in part elucidated and in part pointed out hereinafter. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figures 1A to 1F A process flow according to some embodiments of the present invention is depicted.
[0017] Figure 2 To depict H implanted at 16kev and 22kev, respectively + He + Figure 1 shows the SRIM-calculated depth distribution of ions. These data were obtained according to the method of Example 1.
[0018] Figure 3 To depict various H 2 + Plot of the dose-shifted silicon device layer thickness variation range (·) after cleavage.
[0019] Figure 4 To depict H implanted at 8kev and 11kev respectively + He + Figure 1. SRIM calculated depth distribution of ions. These data were obtained according to the method of Example 2. DETAILED DESCRIPTION
[0020] The fully depleted silicon-on-insulator (FD-SOI) structure relies on an ultra-thin silicon layer on a buried oxide layer (BOX). The buried oxide layer can have a conventional thickness (about 100 nanometers to about 200 nanometers) or it can also be ultra-thin, for example, between 10 nm and 25 nm. The ultra-thin silicon layer enables the silicon under the transistor gate (the body of the transistor) of a CMOS device to be completely depleted of charge. Therefore, the present invention is directed to a method of transferring an ultra-thin silicon layer from a donor substrate to a handle substrate.
[0021] According to the present invention, a method for preparing a semiconductor-on-insulator composite structure (SOI, e.g., a silicon-on-insulator composite structure) having a relatively thin silicon device layer is provided. In some embodiments, the SOI structure further comprises a relatively thin dielectric layer, e.g., a buried oxide layer. Thus, in some embodiments, the present invention is directed to a method of transferring a thin silicon layer having a thickness between about 500 angstroms and about 2500 angstroms from a donor substrate to a handle substrate. According to some embodiments of the present invention, hydrogen (H 2 + and / or H + ) ions and helium (He + ) ions are co-implanted into a donor substrate at low ion energy. The co-implanted donor substrate is annealed to form a damage layer in the donor substrate. The depth of the damage layer determines the thickness of the silicon layer transferred to the handling substrate.
[0022] To achieve thin layer transfer, the implantation energy of the gas ions is kept low, especially when the oxide layer on the donor wafer is also thin (e.g., hundreds of angstroms). Transferring a thin silicon device layer enables the fabrication of a fully depleted SOI structure (FD-SOI). Low-power, high-performance CMOS applications based on FD-SOI require limiting the thickness of the silicon device layer and the thickness of the buried oxide layer. Thin layers can be transferred by limiting the ion beam energy during ion implantation. In addition, according to some embodiments, the manufacturing cost is further reduced by reducing the implantation dose.
[0023] I. Semiconductor donor substrate and semiconductor processing substrate
[0024] Substrates used in the present invention include semiconductor donor substrates (eg, single crystal semiconductor donor wafers) and semiconductor handle substrates (eg, single crystal semiconductor handle wafers). The semiconductor device layers in the semiconductor-on-insulator composite structure are derived from the semiconductor donor substrate.
[0025] Figures 1A to 1F Describes a process flow according to some embodiments of the present invention. Figure 1A, depicting an exemplary non-limiting semiconductor donor substrate 100, such as a single crystal semiconductor donor wafer. In general, the single crystal semiconductor donor substrate 100 includes two substantially parallel major surfaces. One of the parallel surfaces is a front surface 102 of the single crystal semiconductor donor substrate 100, and the other parallel surface is a back surface 104 of the single crystal semiconductor donor substrate 100. The single crystal semiconductor donor substrate 100 includes a circumferential edge 106 joining the front surface 102 and the back surface 104. The single crystal semiconductor donor substrate 100 includes a central axis 108, which is perpendicular to the two substantially parallel major surfaces 102, 104 and is also perpendicular to a central plane 110 defined by a midpoint between the front surface 102 and the back surface 104. The single crystal semiconductor donor substrate 100 includes a bulk region between the two substantially parallel major surfaces 102, 104. Because semiconductor wafers (e.g., silicon wafers) typically have some total thickness variation (TTV), warp, and bow, the midpoints defining the center plane 110 between every point on the front surface 102 and every point on the back surface 104 may not fall exactly within a plane. However, in practice, the TTV, warp, and bow are typically quite small, so that close approximations of the midpoints can be considered to fall within an imaginary center plane 110 that is approximately equidistant from the front and back surfaces 102, 104.
[0026] Prior to any operation described herein, the front surface 102 and the back surface 104 of the single crystal semiconductor donor substrate 100 may be substantially the same. A surface is referred to as a "front surface" or a "back surface" only for convenience and generally to distinguish the surface on which the operations of the method of the present invention are performed. In the context of the present invention, the "front surface" of the single crystal semiconductor donor substrate 100 refers to the main surface of the substrate through which ions are implanted. The front surface becomes the inner surface of the bonding structure. Therefore, the "back surface" of the single crystal semiconductor donor substrate 100 refers to the main surface that becomes the outer surface of the bonding structure. Similarly, the "front surface" of the handling substrate refers to the main surface of the handling substrate that becomes the inner surface of the bonding structure, and the "back surface" of the handling substrate refers to the main surface that becomes the outer surface of the bonding structure. After completing the conventional bonding and splitting steps, the single crystal semiconductor donor substrate forms a semiconductor device layer of a semiconductor-on-insulator (e.g., silicon-on-insulator) composite structure.
[0027] The handling substrate and the single crystal semiconductor donor substrate may be single crystal semiconductor wafers. In preferred embodiments, the semiconductor wafer comprises a material selected from the group consisting of silicon, silicon carbide, silicon germanium, gallium arsenide, gallium nitride, indium phosphide, indium gallium arsenide, germanium, and combinations thereof. Additionally, the handling wafer may comprise sapphire, quartz, or glass. The single crystal semiconductor wafers of the present invention (e.g., single crystal silicon handling wafers and single crystal silicon donor wafers) typically have a nominal diameter of at least about 150 mm, at least about 200 mm, at least about 300 mm, or at least about 450 mm. The wafer thickness may vary between about 100 microns and about 5000 microns, such as between about 100 microns and about 1500 microns, such as between about 250 microns and about 1500 microns, such as between about 300 microns and about 1000 microns, suitably within the range of about 500 microns to about 1000 microns. In some specific embodiments, the wafer thickness may be about 725 microns. In some embodiments, the wafer thickness may be about 775 microns.
[0028] In a particularly preferred embodiment, the single crystal semiconductor wafer comprises a single crystal silicon wafer cut from a single crystal ingot grown according to a conventional Czochralski crystal growth method or a floating zone growth method. For example, such methods and standard silicon cutting, grinding, etching and polishing techniques are disclosed in F. Shimura, "Semiconductor Silicon Crystal Technology" (Academic Press, 1989) and "Silicon Chemical Etching" (J. Grabmaier ed.) (Springer-Verlag, NY, 1982), which are incorporated herein by reference. Preferably, the wafer is polished and cleaned by standard methods known to those skilled in the art. For example, see WC O'Mara et al., "Handbook of Semiconductor Silicon Technology" Noyes Publications. For example, the wafers may be cleaned with a standard SC1 solution (5 parts water: 1 part aqueous ammonium hydroxide (29 wt%): 1 part aqueous hydrogen peroxide (30 wt%)) / SC2 solution (6 parts water: 1 part aqueous hydrochloric acid (37 wt%): 1 part aqueous hydrogen peroxide (30 wt%)) as needed. In some embodiments, the single crystal silicon wafers of the present invention are single crystal silicon wafers cut from single crystal ingots grown according to conventional Czochralski ("Cz") crystal growth methods, typically having a nominal diameter of at least about 150 mm, at least about 200 mm, at least about 300 mm, or at least about 450 mm. Preferably, both the single crystal silicon handle wafer and the single crystal silicon donor wafer have a mirror-polished front surface finish free of surface defects (e.g., scratches, large particles, etc.). The wafer thickness may vary from about 250 microns to about 1500 microns, such as between about 300 microns and about 1000 microns, suitably in the range of about 500 microns to about 1000 microns. In some specific embodiments, the wafer thickness may be between about 725 microns and about 800 microns, such as between about 750 microns and about 800 microns. In some embodiments, the wafer thickness may be about 725 microns. In some embodiments, the wafer thickness may be about 775 microns.
[0029] In some embodiments, the single crystal semiconductor wafer (i.e., the single crystal semiconductor handle wafer and the single crystal semiconductor donor wafer) contains interstitial oxygen having a concentration generally achieved by the Czochralski growth method. In some embodiments, the single crystal semiconductor wafer contains oxygen at a concentration between about 4 PPMA and about 18 PPMA. In some embodiments, the semiconductor wafer contains oxygen at a concentration between about 10 PPMA and about 35 PPMA. In some embodiments, the single crystal silicon wafer contains oxygen at a concentration of no greater than about 10 PPMA. The interstitial oxygen may be measured according to SEMI MF 1188-1105.
[0030] The single crystal semiconductor donor substrate 100 and the handling substrate may have any resistivity obtainable by the Czochralski or floating zone method. Therefore, the resistivity of the single crystal semiconductor donor substrate 100 and the handling substrate is based on the requirements of the final use / application of the structure of the present invention. Therefore, the resistivity can vary from milliohms or less to megohms or more. In some embodiments, the single crystal semiconductor donor substrate 100 is undoped. In some embodiments, the handling substrate 200 is undoped. In some embodiments, the single crystal semiconductor donor substrate 100 includes a p-type or n-type dopant. In some embodiments, the handling substrate 200 includes a p-type or n-type dopant. Suitable dopants include boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type). The dopant concentration is selected based on the desired resistivity of the single crystal semiconductor donor substrate.
[0031] In some embodiments, the single crystal semiconductor donor substrate 100 has a relatively low minimum bulk resistivity, such as less than about 100 ohm-cm, less than about 50 ohm-cm, less than about 1 ohm-cm, less than about 0.1 ohm-cm, or even less than about 0.01 ohm-cm. In some embodiments, the single crystal semiconductor donor substrate 100 has a relatively low minimum bulk resistivity, such as less than about 100 ohm-cm or between about 1 ohm-cm and about 100 ohm-cm. The low resistivity wafer may include electrically active dopants such as boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type).
[0032] In some embodiments, the single crystal semiconductor donor substrate 100 has a relatively high minimum bulk resistivity. High resistivity wafers are generally cut from single crystal ingots grown by the Czochralski method or the floating zone method. High resistivity wafers may include electrically active dopants, such as boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type), generally at very low concentrations. Cz-grown silicon wafers may be subjected to thermal annealing at a temperature ranging from about 600° C. to about 1000° C. to annihilate thermal donors caused by oxygen incorporated during crystal growth. In some embodiments, the single crystal semiconductor handle wafer has a minimum bulk resistivity of at least 100 Ohm-cm or even at least about 500 Ohm-cm, such as between about 100 Ohm-cm and about 100,000 Ohm-cm, or between about 500 Ohm-cm and about 100,000 Ohm-cm, or between about 1000 Ohm-cm and about 100,000 Ohm-cm, or between about 500 Ohm-cm and about 10,000 Ohm-cm. In some preferred embodiments, the single crystal semiconductor handle wafer has a bulk resistivity between about 1000 Ohm-cm and about 6,000 Ohm-cm, or between about 1000 Ohm-cm and about 10,000 Ohm-cm, or between about 1000 Ohm-cm and about 6000 Ohm-cm, or between about 2000 Ohm-cm and about 10,000 Ohm-cm, or between about 3000 Ohm-cm and about 10,000 Ohm-cm, or between about 3000 Ohm-cm and about 5,000 Ohm-cm. In some preferred embodiments, the single crystal semiconductor handle wafer has a bulk resistivity between about 1000 Ohm-cm and about 6,000 Ohm-cm. Methods for preparing high-resistivity wafers are known in the art, and such high-resistivity wafers are available from commercial suppliers such as Sun Edison Semiconductor Ltd. (St. Peters, MO; formerly MEMC Electronic Materials).
[0033] Single crystalline semiconductor donor substrate 100 may include single crystalline silicon.Single crystalline semiconductor donor substrate 100 may have any of (100), (110), or (111) crystal orientations, and the choice of crystal orientation may depend on the end use of the structure.
[0034] The front surface 102, the back surface 104, or both surfaces of the single crystal semiconductor donor substrate 100 may be oxidized, as appropriate, according to methods known in the art. The oxidation may be accomplished by methods known in the art, such as thermal oxidation (where some portion of the deposited semiconductor material film will be consumed), CVD oxidation deposition, or by exposure to a standard cleaning solution, such as an SC1 / SC2 cleaning solution. The single crystal semiconductor donor substrate 100 may be thermally oxidized in a furnace such as an ASM A400 or ASM A400XT. In the oxidizing environment, the temperature may be in the range of from 750° C. to 1100° C., such as between about 800° C. to about 1200° C. The oxidizing environment atmosphere may be an inert gas such as Ar or N 2 ) and O 2 The oxygen content can vary from 1% to 10% or more. In some embodiments, the oxidizing ambient atmosphere can be as high as 100% ("dry oxidation"). In some embodiments, the ambient atmosphere can include an inert gas (e.g., Ar or N 2 ) and oxidizing gases (such as O 2 and water vapor) ("wet oxidation"). In an exemplary embodiment, the donor wafer may be loaded into a vertical furnace such as an ASM A400 or ASM A400XT. N 2 and O 2 The temperature is ramped to the oxidation temperature. At the desired temperature, water vapor is introduced into the gas stream. After the desired oxide thickness is obtained, the water vapor and O 2 The furnace temperature is lowered and the wafer is removed from the furnace. In an embodiment where the single crystal semiconductor donor substrate 100 is a single crystal silicon donor substrate, the oxide layer 120 comprises silicon dioxide. Figure 1B The oxide layer 120 on the front surface 102, the back surface 104, or both may be between about 100 angstroms and about 1000 angstroms, such as between about 100 angstroms and about 700 angstroms, or between about 100 angstroms and about 500 angstroms, or between about 100 angstroms and about 250 angstroms.
[0035] In some embodiments, the oxide layer 120 is relatively thin, for example, between about 5 angstroms and about 25 angstroms, for example, between about 10 angstroms and about 15 angstroms. The thin oxide layer on both sides of the semiconductor wafer can be obtained by exposure to a standard cleaning solution, such as an SC1 / SC2 cleaning solution. In some embodiments, the SC1 solution comprises 5 parts deionized water, 1 part aqueous NH 4 OH (ammonium hydroxide, 29% by weight NH 3 ) and 1 part aqueous H 2 O 2(hydrogen peroxide, 30%). In some embodiments, the wafer may be oxidatively treated by exposure to an aqueous solution comprising an oxidizing agent, such as an SC2 solution. In some embodiments, the SC2 solution comprises 5 parts deionized water, 1 part aqueous HCl (hydrochloric acid, 39% by weight), and 1 part aqueous H 2 O 2 (hydrogen peroxide, 30%).
[0036] II. Ion implantation
[0037] Ion implantation can be performed in commercially available instruments such as Applied Materials' Quantum II, QuantumLEAP, or Quantum X. According to some embodiments, the implanted ions include H + and / or H 2 + Ions and He + Combination of ions. + Before H ion implantation + and / or H 2 + Ions can be implanted in He + After the H ion implantation + and / or H 2 + ions, or He + Ions are implanted simultaneously with H + and / or H 2 + Ions are implanted at a density and for a duration sufficient to form a damaged layer in the semiconductor donor substrate. Figure 1C ion implantation occurs through the oxide layer 120 and the front surface 102 of the single crystal semiconductor donor substrate 100, so that the single crystal semiconductor donor substrate 100 includes H at a peak depth D1. + and / or H 2 + Ions and He at peak depth D2 + ions. Peak depths D1 and D2 are for illustration only and are not to be considered drawn to scale. The lengths of peak depths D1 and D2 are measured from the front surface 102 of the single crystal silicon donor substrate 100 along the central axis 108. The implantation depth determines the thickness of the single crystal semiconductor device layer in the final SOI structure.
[0038] In some embodiments, the method includes injecting hydrogen ions (e.g., H 2 + Ions, H + Ion or H 2 + and H +The hydrogen ions are implanted at an average depth D1 measured from the front surface toward the center plane. As measured from the front surface of the single crystal silicon donor substrate along the central axis, the average depth D1 of the implanted hydrogen ions may range from about 100 angstroms to about 4000 angstroms, from about 100 angstroms to about 3000 angstroms, or between about 500 angstroms and about 3000 angstroms, or between about 500 angstroms and about 2500 angstroms. In some embodiments, at an implantation energy between about 10 KeV and about 40 KeV (e.g., between about 20 KeV and about 40 KeV or between about 25 KeV and about 35 KeV, such as about 16 KeV or about 32 KeV), the hydrogen ions are implanted at an average depth D1 measured from the front surface toward the center plane. As measured from the front surface of the single crystal silicon donor substrate along the central axis, the average depth D1 of the implanted hydrogen ions may range from about 100 angstroms to about 4000 angstroms, from about 100 angstroms to about 3000 angstroms, or between about 500 angstroms and about 2500 angstroms. 2 + The ion implantation dose can be from 4.3×10 15 ions / cm 2 to 1.1×10 16 ions / cm 2 In the range of about 6.8×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 In some embodiments, at an implantation energy between about 20 KeV and about 40 KeV or between about 25 KeV and about 35 KeV (e.g., about 16 KeV or about 32 KeV), H 2 + The ion implantation dose can be from about 4.3 × 10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 In the range of about 6×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 In some embodiments, at an implantation energy between about 10 KeV and about 30 KeV (e.g., between about 15 KeV and about 20 KeV, e.g., about 16 KeV), H 2 + The ion implantation dose can be from about 5.9 × 10 15 ions / cm 2 To about 6.7×10 15 ions / cm 2 In some embodiments, at an implantation energy between about 5 KeV and about 20 KeV (e.g., between about 10 KeV and about 20 KeV, e.g., about 16 KeV), H + The ion implantation dose can be from about 5 × 10 15 ions / cm 2 To about 2×10 16 ions / cm2 In some embodiments, at an implantation energy between about 5 KeV and about 20 KeV (e.g., between about 10 KeV and about 20 KeV, e.g., about 16 KeV), H + The ion implantation dose can be from about 1.1 × 10 16 ions / cm 2 To about 2×10 16 ions / cm 2 In some embodiments, at an implantation energy between about 5 KeV and about 20 KeV (e.g., between about 10 KeV and about 20 KeV, e.g., 16 KeV), H + The ion implantation dose can be from about 6.1×10 15 ions / cm 2 To about 6.8×10 15 ions / cm 2 In some embodiments, H can be added within the above dosage range and energy. 2 + and H + The combination of ions is implanted to an average depth D1 measured from the front surface toward the center plane.
[0039] In some embodiments, the method includes directing helium ions (e.g., He + ions) are implanted to an average depth D2 measured from the front surface 102 along the central axis 108. As measured from the front surface of the single crystal silicon donor substrate along the central axis, the average depth D2 of the implanted helium ions may range from about 100 angstroms to about 4000 angstroms, from about 100 angstroms to about 3000 angstroms, or between about 500 angstroms to about 3000 angstroms, or between about 500 angstroms to about 2500 angstroms. In some embodiments, at an implantation energy between about 5 KeV and about 30 KeV (e.g., between about 10 KeV and about 25 KeV, or between about 15 KeV and about 25 KeV, such as about 22 KeV), the total helium ion implantation dose may range from about 6×10 15 ions / cm 2 To about 2×10 16 ions / cm 2 , from about 6×10 15 ions / cm 2 To about 1.3×10 16 ions / cm 2 , from about 6.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 , from about 6.6×10 15 ions / cm 2To about 8×10 15 ions / cm 2 In some embodiments, at an implantation energy between about 5 KeV and about 30 KeV (e.g., between about 10 KeV and about 25 KeV or between about 15 KeV and about 25 KeV, e.g., about 22 KeV), the total helium ion implantation dose may range from about 6×10 15 ions / cm 2 To about 2×10 16 ions / cm 2 , from about 6×10 15 ions / cm 2 To about 1.3×10 16 ions / cm 2 , from about 6.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 , from about 6.6×10 15 ions / cm 2 To about 8×10 15 ions / cm 2 In some embodiments, at an implantation energy between about 5 KeV and about 20 KeV (e.g., between about 5 KeV and about 15 KeV, such as 11 KeV), the total helium ion implantation dose may range from about 6×10 15 ions / cm 2 To about 2×10 16 ions / cm 2 , from about 6×10 15 ions / cm 2 To about 1.3×10 16 ions / cm 2 , from about 6.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 , from about 6.6×10 15 ions / cm 2 To about 8×10 15 ions / cm 2 or from about 6.6×10 15 ions / cm 2 To about 7×10 15 ions / cm 2 .
[0040] Preferably, H 2 + Ions, H + Ion or H 2+ Ions and H + The peak density of the combined ions (D1) and He + The peak densities (D2) of the ions are within about 1000 angstroms of each other, within about 600 angstroms of each other, within about 500 angstroms of each other, within about 450 angstroms of each other, within about 400 angstroms of each other, within about 300 angstroms of each other, or within about 200 angstroms of each other.
[0041] In some embodiments, it may be desirable for the single crystal semiconductor donor wafer (e.g., single crystal silicon donor wafer) to undergo cleaning after implantation. In some preferred embodiments, the cleaning may include a Piranha clean (a mixture of sulfuric acid and hydrogen peroxide) followed by a DI water rinse and a SC1 (a mixture of water: aqueous ammonium hydroxide: aqueous hydrogen peroxide in a 5:1:1 ratio) and a SC2 (a mixture of water: aqueous hydrochloric acid: aqueous hydrogen peroxide in a 6:1:1 ratio) clean.
[0042] III. annealing
[0043] In some embodiments of the present invention, the ion-implanted single crystal semiconductor donor substrate 100 is annealed at a temperature sufficient to form a thermally activated damage layer or cleavage plane 130 in the single crystal semiconductor donor substrate. This annealing occurs prior to bonding. By utilizing low implantation energies, the damage layer 130 occurs at a depth capable of transferring a thin silicon layer to the handle substrate, for example, a thickness between about 500 angstroms and about 2500 angstroms.
[0044] An example of a suitable tool may be a simple box furnace such as the Blue M model. In some preferred embodiments, the ion implanted single crystal semiconductor donor substrate is annealed at a temperature of from about 200° C. to about 350° C., from about 225° C. to about 350° C., such as between about 250° C. to about 300° C. The thermal annealing may occur for a duration of up to about 10 minutes to about 10 hours, such as about 10 minutes to about 2 hours or between about 10 minutes to about 60 minutes. Thermal annealing within these temperature ranges is sufficient to form the thermally activated cleavage plane 130. After the thermal annealing for activating the cleavage plane 130, the surface of the single crystal semiconductor donor substrate is preferably cleaned. In some preferred embodiments, the cleaning may include a peroxysulfuric acid clean (a mixture of sulfuric acid and hydrogen peroxide) followed by a DI water rinse and a SC1 (a mixture of water: aqueous ammonium hydroxide: aqueous hydrogen peroxide in a ratio of 5:1:1) and a SC2 (a mixture of water: aqueous hydrochloric acid: aqueous hydrogen peroxide in a ratio of 6:1:1) clean.
[0045] IV. Plasma Activation
[0046] In some embodiments, the ion-implanted and annealed single crystal semiconductor donor substrate is subjected to oxygen plasma and / or nitrogen plasma surface activation. In some embodiments, the oxygen plasma surface activation tool is a commercially available tool, such as a tool purchased from EV Group, such as 810LT Low Temperature Plasma Activation System. An ion implanted and optionally cleaned single crystal semiconductor donor wafer is loaded into the chamber. The chamber is evacuated and a source of oxygen and / or nitrogen in a carrier gas (e.g., argon) is used to backfill the chamber to a pressure less than atmospheric pressure to thereby generate a plasma. Oxygen and / or water are suitable source gases for plasma oxidation processes. Ammonia and / or nitrogen and / or nitric oxide (NO) and / or nitrous oxide (N 2 The Oxynitride plasma activation may include oxygen and nitrogen sources in the ambient atmosphere. The single crystal semiconductor donor wafer is exposed to this plasma for a desired time, which may range from about 1 second to about 120 seconds. The oxygen or nitrogen plasma surface oxidation is performed to make the front surface of the single crystal semiconductor donor substrate hydrophilic and suitable for bonding to the handle substrate. After the plasma activation, the activated surface is rinsed with deionized water. Then, the water is dried off before bonding.
[0047] V. Preparation of bonding structure
[0048] refer to Figure 1E , then, the oxide layer 120 on the front surface 102 of the single crystal semiconductor donor substrate 100 having the cleavage plane or damage layer 130 is bonded to the main surface of the semiconductor handling substrate 200 (by bringing these surfaces into close contact). In some embodiments, the semiconductor handling substrate 200 includes a dielectric layer. The dielectric layer may include an insulating material selected from silicon dioxide, silicon nitride, silicon oxynitride, hafnium oxide, titanium oxide, zirconium oxide, lanthanum oxide, barium oxide, and any combination thereof. In some embodiments, the dielectric layer includes one or more insulating materials selected from the group consisting of silicon dioxide, silicon nitride, silicon oxynitride, and any combination thereof. In some embodiments, the dielectric layer has a thickness of at least about 1 nanometer thick or at least about 10 nanometers thick, such as between about 10 nanometers and about 10,000 nanometers, between about 10 nanometers and about 5,000 nanometers, between 50 nanometers and about 500 nanometers, or between about 100 nanometers and about 400 nanometers, such as about 50 nanometers, about 75 nanometers, about 85 nanometers, about 100 nanometers, about 150 nanometers, about 175 nanometers, or about 200 nanometers. The dielectric layer can be between about 100 angstroms and about 1000 angstroms, such as between about 100 angstroms and about 700 angstroms, or between about 100 angstroms and about 500 angstroms, or between about 100 angstroms and about 250 angstroms. In some embodiments, the dielectric layer is much thinner, such as between about 5 angstroms and about 25 angstroms, such as between about 10 angstroms and about 15 angstroms.
[0049] In some embodiments, the dielectric layer may include one or more insulating layers, such as two insulating layers, three insulating layers, or more insulating layers. Each dielectric layer may include a material selected from the group consisting of silicon dioxide, silicon nitride, and silicon oxynitride. Each insulating layer may have a thickness of at least about 1 nanometer thick or at least about 10 nanometers thick, such as between about 10 nanometers and about 10,000 nanometers, between about 10 nanometers and about 5,000 nanometers, between 50 nanometers and about 500 nanometers, or between about 100 nanometers and about 400 nanometers, such as about 50 nanometers, about 75 nanometers, about 85 nanometers, about 100 nanometers, about 150 nanometers, about 175 nanometers, or about 200 nanometers.
[0050] Since in some embodiments, the mechanical bond is relatively weak, the bonded structure may be further annealed to solidify the bond between the single crystal semiconductor donor substrate 100 and the handling substrate 200. In some embodiments of the present invention, the bonded structure is annealed at a temperature sufficient to form a thermally activated cleavage plane in the single crystal semiconductor donor substrate. An example of a suitable tool may be a simple box furnace such as the Blue M model. In some preferred embodiments, the bonded structure is annealed at a temperature from about 200° C. to about 400° C. (e.g., from about 300° C. to about 400° C.). Thermal annealing may occur for a duration of from 10 minutes to about 10 hours (e.g., from about 10 minutes to about 60 minutes).
[0051] In some embodiments, annealing may occur at relatively high pressures, such as between about 0.5 MPa and about 200 MPa, such as between about 0.5 MPa and about 100 MPa, such as between about 0.5 MPa and about 50 MPa, or between about 0.5 MPa and about 10 MPa, or between about 0.5 MPa and about 5 MPa. In conventional bonding methods, the temperature may be limited by "auto-cleavage". This occurs when the pressure of the thin plate at the implantation surface exceeds the external isostatic pressure. Therefore, conventional annealing may be limited to a bonding temperature between about 350° C. and about 400° C. due to auto-cleavage. After implantation and bonding, the wafers are weakly held together. But the gap between the wafers is sufficient to prevent gas penetration or escape. The weak bond can be strengthened by heat treatment, but the cavity formed during implantation is filled with gas. When heated, the gas in the cavity is pressurized. It is estimated that, depending on the dosage, the pressure can reach 0.2 to 1 GPa (Cherkashin et al., J. Appl. Phys. 118, 245301 (2015)). When the pressure exceeds a critical value, the layers delaminate. This refers to auto-splitting or thermal splitting. It prevents higher annealing temperatures or longer annealing times. According to some embodiments of the present invention, bonding occurs at high pressure (e.g., between about 0.5 MPa and about 200 MPa, such as between about 0.5 MPa and about 100 MPa, between about 0.5 MPa and about 50 MPa, or between about 0.5 MPa and about 10 MPa, or between about 0.5 MPa and about 5 MPa), thereby achieving bonding at high temperature. In some embodiments, the bonded structure is annealed at a temperature from about 300°C to about 700°C, from about 400°C to about 600°C (e.g., between about 400°C to about 450°C or even between about 450°C to about 600°C or between about 350°C to about 450°C). Increasing the thermal budget will have a positive impact on the bond strength. The thermal annealing may occur for a duration of up to about 0.5 hours to about 10 hours (e.g., between about 0.5 hours to about 3 hours), preferably, a duration of about 2 hours. Thermal annealing within these temperature ranges is sufficient to form a thermally activated cleavage plane. In conventional bond annealing, the edges of both the handle wafer and the donor wafer are significantly separated by roll off. In this region, there is no layer transfer. It is called a terrace. It is expected that boost bonding will reduce this terrace, thereby extending the SOI layer further outward toward the edge. This mechanism is based on the compression and "zippering" of trapped air pockets outward. After thermal annealing for activating the cleavage planes, the bonded structure can be cleaved.
[0052] After thermal annealing, the bond between the single crystalline semiconductor donor substrate 100 and the handling substrate 200 is strong enough to induce layer transfer via cleaving the bonded structure at the cleavage plane. Cleaving may occur according to techniques known in the art. In some embodiments, the bonded structure may be placed in a conventional cleaving station with one side attached to a fixed chuck and the other side attached to an articulated arm via an additional chuck. A crack is induced near the chuck attachment and the movable arm pivots about the hinge to cleave the wafer apart. Cleaving removes a portion of the semiconductor donor wafer, thereby leaving a single crystalline semiconductor device layer 300, preferably a silicon device layer, on the semiconductor-on-insulator composite structure. See also Figure 1F The method of the present invention is capable of transferring a thin layer of silicon from a donor substrate to a handle substrate. Thus, in some embodiments, the silicon layer has a thickness between about 500 angstroms and about 2500 angstroms.
[0053] After cleaving, the cleaved structure may be subjected to a high temperature anneal to further strengthen the bond between the transfer device layer 300 and the handling substrate. An example of a suitable tool may be a vertical furnace such as ASM A400. In some preferred embodiments, the bonded structure is annealed at a temperature from about 1000° C. to about 1200° C., preferably at about 1000° C. The thermal annealing may occur for a duration of up to about 0.5 hours to about 8 hours, preferably, for a duration of about 2 hours to 4 hours. Thermal annealing within these temperature ranges is sufficient to strengthen the bond between the transfer device layer and the single crystal semiconductor handling substrate.
[0054] After cleaving and high temperature annealing, the bonded structure may be subjected to a cleaning process designed to remove the thin thermal oxide and clean particles from the surface. In some embodiments, the bonded structure may be cleaned by using H in a horizontal flow single wafer epitaxial reactor. 2 The single crystal semiconductor device layer is subjected to a gas phase HCl etching process as a carrier gas to achieve a desired thickness and smoothness.
[0055] In some embodiments, an epitaxial layer may be deposited on the transferred single crystal semiconductor device layer 300. The deposited epitaxial layer may include electrical properties that are substantially the same as the underlying single crystal semiconductor device layer 300. Alternatively, the epitaxial layer may include electrical properties that are different from the underlying single crystal semiconductor device layer 300. The epitaxial layer may include a material selected from the group consisting of silicon, silicon carbide, silicon germanium, gallium arsenide, gallium nitride, indium phosphide, indium gallium arsenide, germanium, and combinations thereof. Depending on the desired properties of the final integrated circuit device, the epitaxial layer may include a dopant selected from boron (p-type), gallium (p-type), aluminum (p-type), indium (p-type), phosphorus (n-type), antimony (n-type), and arsenic (n-type). The resistivity of the epitaxial layer may be in the range from 1 to 50 Ohm-cm, typically from 5 to 25 Ohm-cm. In some embodiments, the epitaxial layer may have a thickness between about 10 nanometers and about 20 microns, between about 20 nanometers and about 3 microns, such as between about 20 nanometers and about 2 microns, such as between about 20 nanometers and about 1.5 microns or between about 1.5 microns and about 3 microns.
[0056] The finished SOI wafer may then undergo final metrology inspection and finally be cleaned using a typical SC1-SC2 process.
[0057] The present invention can be further illustrated by the following non-limiting examples.
[0058] Example 1.
[0059] The single crystal silicon donor substrate was subjected to ion implantation. First, the wafer was subjected to 7×10 15 cm -2 Dose of He + Ion implantation. The implantation energy is 22 KeV. Afterwards, the wafer is subjected to H 2 + Ion implantation or H + Ion implantation. 2 + The ion implantation energy is 32 KeV. + The ion implantation energy was 16 KeV and the dose was varied according to Table 1.
[0060] The Stopping and Range of Ions in Matter (SRIM) calculations show that H + He + The peak difference of the depth profile is about 450 angstroms. See Figure 1. The ion implanted donor substrate was bonded to a handle substrate, annealed, and cleaved. Table 1 further provides the cleavage results.
[0061] Table 1: Various H 2 + and H + The result of mechanical splitting of the dose
[0062] <![CDATA[H 2 + Dosage]]> <![CDATA[H + Dosage]]> Split results <![CDATA[3.1x 10 15 cm -2 ]]> No division <![CDATA[6.8x 10 15 cm -2 ]]> No division <![CDATA[3.7x 10 15 cm -2 ]]> No division <![CDATA[4x 10 15 cm -2 ]]> No division <![CDATA[4.3x 10 15 cm -2 ]]> Split <![CDATA[4.6x 10 15 cm -2 ]]> Split <![CDATA[4.9x 10 15 cm -2 ]]> Split <![CDATA[5.2x 10 15 cm -2 ]]> Split <![CDATA[5.5x 10 15 cm -2 ]]> Split <![CDATA[5.8x 10 15 cm -2 ]]> Split <![CDATA[1.22x 10 16 cm -2 ]]> Split <![CDATA[7.6x 10 15 cm -2 ]]> Split <![CDATA[7.9x 10 15 cm -2 ]]> Split <![CDATA[8.2x 10 15 cm -2 ]]> Split <![CDATA[8.5x 10 15 cm -2 ]]> Split <![CDATA[8.8x 10 15 cm -2 ]]> Split <![CDATA[9.1x 10 15 cm -2 ]]> Split <![CDATA[9.4x 10 15 cm -2 ]]> Split <![CDATA[9.7x 10 15 cm -2 ]]> Split <![CDATA[2x 10 16 cm -2 ]]> Split <![CDATA[1.03x 10 16 cm -2 ]]> Split
[0063] According to the results shown in Table 1, if He + The ion implantation dose is fixed at 7×10 at 22 KeV. 15 cm -2 , then less than 4.3×10 15 cm -2 H 2 + The ion implantation dose is less than 6.8×10 15 cm -2 H + No fragmentation was observed at the ion implantation dose.
[0064] After splitting, the measurement is based on H 2 + The thickness variation of the transferred silicon device layer varies with the ion implantation dose. Figure 3 , which depicts various H 2 + The thickness variation range of the silicon device layer after splitting due to the dose transfer (·). Figure 2 and 3 The data shown in the figure can determine that: when H 2 + The ion implantation dose is at least 6×10 15 cm -2 And He + The ion implantation dose is fixed at 7×10 at 22Kev energy. 15 cm -2 When H is , the minimum thickness variation of the transferred silicon device layer is obtained. Obviously, H which minimizes the thickness variation of the transferred silicon device layer 2 + The ion implantation dose is significantly greater than the H required to achieve fragmentation by mechanical fragmentation. 2 + Ion implantation dose.
[0065] Example 2.
[0066] The single crystal silicon donor substrate was subjected to ion implantation. Each wafer was subjected to He + Ions and H 2 + or H + Ion implantation of one of the + , H 2 + and H + The implantation dose of each of He is variable. + The ion implantation dose is 6.6×10 15 cm -2 to 7×10 15 cm-2 He + The implantation energy of the ion dose is 11 KeV. 2 + The ion implantation energy is 16 KeV and H + The ion implantation energy is 8 KeV. SRIM calculations show that H + He + The peak difference of the depth profile is about 200 angstroms. Figure 4 .
[0067] The ion implanted donor substrate was bonded to a handle substrate, annealed, and cleaved. Table 2 further provides the cleavage results.
[0068] Table 2: Various H 2 + and H + The result of mechanical splitting of the dose
[0069]
[0070]
[0071] At very low He + energy (i.e., 11 KeV), the total implantation was as low as 5.9 × 10 15 cm -2 H + Successful mechanical splitting can be obtained.
[0072] Having described the invention in detail, it will be apparent that modifications and variations may be made without departing from the scope of the invention as defined in the appended claims.
[0073] When introducing elements of the present invention or its preferred embodiment(s), the articles "a", "an" and "the" are intended to mean that there are one or more of the elements. The terms "comprising", "including" and "having" are intended to be inclusive and mean that there may be additional elements other than the listed elements.
[0074] In view of the above it will be seen that the several objects of the invention are achieved and other advantageous results attained.
[0075] As various changes could be made in the above products and methods without departing from the scope of the invention, it is intended that all matter contained in the above description and shown in the accompanying drawings shall be interpreted as illustrative and not in a limiting sense.
Claims
1. A method of transferring a silicon layer from a single crystal silicon donor substrate to a handle substrate, the method comprising: (a) implanting H2 through a silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate and through the front surface of the single crystal silicon donor substrate + Ions, H + Ions or H2 + Ions and H + ions, the single crystal silicon donor substrate comprising two parallel main surfaces, a circumferential edge connecting the front surface and the rear surface, a central plane between the front surface and the rear surface, a central axis perpendicular to the front surface, and a bulk region between the front surface and the rear surface, one of the two parallel main surfaces is the front surface and one of the two parallel main surfaces is the rear surface, wherein the H2 + The ions are implanted at an implantation energy between about 10 KeV and about 30 KeV, and the H + The ions are implanted at an implantation energy between about 5 KeV and about 20 KeV, wherein the H2 + Ions, H + Ions or H2 + Ions and H + The combined peak density (D1) of the ions is between about 100 angstroms and about 3000 angstroms; (b) implanting He through the silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate and through the front surface of the single crystal silicon donor substrate + ions, wherein the He + The ions are implanted at an implantation energy between about 5 KeV and about 30 KeV, wherein the He ... + The peak density (D2) of the ions is between about 100 angstroms and about 3000 angstroms, and further wherein H2 + Ions, H + Ions or H2 + Ions and H + The peak density (D1) and He + The peak densities (D2) of ions are within about 450 angstroms of each other; (c) annealing the ion-implanted single crystal silicon donor substrate at a temperature between about 200° C. and about 350° C. and for a duration sufficient to form a damage layer in the single crystal silicon donor substrate; (d) bonding the silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate to a dielectric layer in contact with the handle substrate to thereby prepare a multi-layer substrate; (e) annealing the multilayer substrate at a temperature between about 200° C. and about 400° C. and for a duration sufficient to thermally activate the damaged layer; and (f) cleaving the annealed multilayer substrate at the damaged layer in the single crystal silicon donor substrate to thereby transfer the silicon layer having a thickness between about 500 angstroms and about 2500 angstroms from the single crystal silicon donor substrate to the handle substrate.
2. The method of claim 1, wherein step (a) occurs before step (b).
3. The method of claim 1, wherein step (b) occurs before step (a).
4. The method of claim 1, wherein steps (a) and (b) occur simultaneously.
5. The method of claim 1, wherein step (a) comprises: (i) implanting the nanostructured carbon nanotubes at an implant energy between about 10 KeV and about 30 KeV, at a rate of about 4.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 The dose between implanted H2 + ions; (ii) at an implantation energy between about 5 KeV and about 20 KeV, based on about 5×10 15 ions / cm 2 To about 2×10 16 ions / cm 2 The dose implanted between + ions; or (iii) at an implantation energy between about 10 KeV and about 30 KeV, based on about 4.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 The dose between implanted H2 + ions, and at an implantation energy between about 5 KeV and about 20 KeV, the 15 ions / cm 2 To about 2×10 16 ions / cm 2 The dose implanted between + ion.
6. The method of claim 1, wherein step (a) comprises: (i) implanting the nanostructured carbon nanotubes at an implant energy between about 10 KeV and about 30 KeV, at a rate of about 4.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 The dose between implanted H2 +ions; (ii) at an implantation energy between about 5 KeV and about 20 KeV, based on about 1.1×10 16 ions / cm 2 To about 2×10 16 ions / cm 2 The dose implanted between + ions; or (iii) at an implantation energy between about 10 KeV and about 30 KeV, based on about 4.3×10 15 ions / cm 2 To about 1.1×10 16 ions / cm 2 The dose between implanted H2 + ions, and at an implantation energy between about 5 KeV and about 20 KeV, the 16 ions / cm 2 To about 2×10 16 ions / cm 2 The dose implanted between + ion.
7. The method of claim 1, wherein step (a) comprises: (i) implanting the nanostructured carbon nanotubes at an implant energy between about 10 KeV and about 30 KeV, at a temperature of about 5.9×10 15 ions / cm 2 To about 6.7×10 15 ions / cm 2 The dose between implanted H2 + ions; (ii) at an implantation energy between about 5 KeV and about 20 KeV, based on about 6.1×10 15 ions / cm 2 To about 6.8×10 15 ions / cm 2 The dose implanted between + ions; or (iii) at an implantation energy between about 10 KeV and about 30 KeV, based on about 5.9×10 15 ions / cm 2 To about 6.7×10 15 ions / cm 2 The dose between implanted H2 + ions, and at an implantation energy between about 5 KeV and about 20 KeV, the 15 ions / cm 2 To about 6.8×10 15 ions / cm 2 The dose implanted between + ion.
8. The method of claim 1, wherein step (b) comprises: implanting the substrate at an implant energy between about 5 KeV and about 30 KeV according to about 6×10 15 ions / cm 2 To about 8×10 15 ions / cm 2 The dose implanted He + ion.
9. The method of claim 1, wherein step (b) comprises: implanting the substrate at an implant energy between about 10 KeV and about 30 KeV according to about 6×10 15 ions / cm 2 To about 8×10 15 ions / cm 2 The dose implanted He + ion.
10. The method of claim 1, wherein step (b) comprises: implanting the substrate at an implant energy between about 5 KeV and about 20 KeV at a rate of about 6.6×10 15 ions / cm 2 To about 7×10 15 ions / cm 2 The dose implanted He + ion.
11. The method according to claim 1, wherein H2 measured from the front surface of the single crystal silicon donor substrate along the central axis + Ions, H + Ions or H2 + Ions and H + The combined peak density (D1) of the ions is between about 500 angstroms and about 2500 angstroms.
12. The method of claim 1, wherein the He measured from the front surface of the single crystal silicon donor substrate along the central axis is + The peak density (D2) of ions is between about 500 angstroms and about 3000 angstroms.
13. The method according to claim 1, wherein H2 + Ions, H + Ions or H2 + Ions and H + The peak density (D1) and He + The peak densities (D2) of ions are within about 400 angstroms of each other.
14. The method according to claim 1, wherein H2 + Ions, H + Ions or H2 + Ions and H + The peak density (D1) and He+ The peak densities (D2) of ions are within about 200 angstroms of each other.
15. The method of claim 1, wherein step (c) comprises annealing the ion implanted single crystal silicon donor substrate at a temperature between about 250°C and about 300°C for a duration between 10 minutes and 60 minutes.
16. The method of claim 1, wherein step (e) comprises annealing the multilayer substrate at a temperature between about 300°C and about 400°C for a duration between 10 minutes and 60 minutes.
17. The method of claim 1, wherein the silicon layer having the thickness between about 500 angstroms and about 2500 angstroms transferred from the single crystal silicon donor substrate to the handle substrate has a thickness variation of less than about 10 angstroms.
18. The method of claim 1, wherein step (e) comprises annealing the multilayer substrate at a pressure between about 0.5 MPa and about 200 MPa.
19. A method of transferring a silicon layer from a single crystal silicon donor substrate to a handle substrate, the method comprising: (a) implanting H through a silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate and through the front surface of the single crystal silicon donor substrate + ions, the single crystal silicon donor substrate comprising two parallel main surfaces, a circumferential edge connecting the front surface and the rear surface, a central plane between the front surface and the rear surface, a central axis perpendicular to the front surface, and a bulk region between the front surface and the rear surface, one of the two parallel main surfaces is the front surface and one of the two parallel main surfaces is the rear surface, wherein the H + The ions are implanted at an implantation energy between about 5 KeV and about 20 KeV, wherein the H + The peak density (D1) of ions is between about 100 angstroms and about 3000 angstroms; (b) implanting He through the silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate and through the front surface of the single crystal silicon donor substrate + ions, wherein the He + The ions are implanted at an implantation energy between about 5 KeV and about 30 KeV, wherein the He ... + The peak density (D2) of ions is between about 100 angstroms and about 3000 angstroms, and further wherein H + The peak density (D1) of He +The peak densities (D2) of ions are within about 450 angstroms of each other; (c) annealing the ion-implanted single crystal silicon donor substrate at a temperature between about 200° C. and about 350° C. and for a duration sufficient to form a damage layer in the single crystal silicon donor substrate; (d) bonding the silicon dioxide layer in contact with the front surface of the single crystal silicon donor substrate to a dielectric layer in contact with the handle substrate to thereby prepare a multi-layer substrate; (e) annealing the multilayer substrate at a temperature between about 200° C. and about 400° C. and for a duration sufficient to thermally activate the damaged layer; and The annealed multilayer substrate is cleaved at the damaged layer in the single crystal silicon donor substrate to thereby transfer the silicon layer having a thickness between about 500 angstroms and about 2500 angstroms from the single crystal silicon donor substrate to the handle substrate.
20. The method of claim 19, wherein step (a) occurs before step (b).
21. The method of claim 19, wherein step (b) occurs before step (a).
22. The method of claim 19, wherein steps (a) and (b) occur simultaneously.
23. The method of claim 19, wherein step (a) comprises: implanting the nanostructured carbon nanotubes at an implant energy between about 5 KeV and about 20 KeV, at a rate of about 5×10 15 ions / cm 2 To about 2×10 16 ions / cm 2 The dose implanted between + ion.
24. The method of claim 19, wherein step (a) comprises: implanting the nanostructured carbon nanotubes at an implant energy between about 5 KeV and about 20 KeV at a rate of about 1.1×10 16 ions / cm 2 To about 2×10 16 ions / cm 2 The dose implanted between + ion.
25. The method of claim 19, wherein step (a) comprises: implanting the substrate at an implant energy between about 5 KeV and about 20 KeV at about 6.1×10 15 ions / cm 2 To about 6.8×10 15 ions / cm 2 The dose implanted between + ion.
26. The method of claim 19, wherein step (b) comprises: implanting the substrate at an implant energy between about 5 KeV and about 30 KeV according to about 6×10 15 ions / cm 2 To about 8×10 15 ions / cm 2 The dose implanted He + ion.
27. The method of claim 19, wherein step (b) comprises: implanting the substrate at an implant energy between about 10 KeV and about 30 KeV according to about 6×10 15 ions / cm 2 To about 8×10 15 ions / cm 2 The dose implanted He + ion.
28. The method of claim 19, wherein step (b) comprises: implanting the substrate at an implant energy between about 5 KeV and about 20 KeV at a rate of about 6.6×10 15 ions / cm 2 To about 7×10 15 ions / cm 2 The dose implanted He + ion.
29. The method of claim 19, wherein H measured from the front surface of the single crystal silicon donor substrate along the central axis is + The peak density (D1) of ions is between about 500 angstroms and about 2500 angstroms.
30. The method of claim 19, wherein the He measured from the front surface of the single crystal silicon donor substrate along the central axis is + The peak density (D2) of ions is between about 500 angstroms and about 3000 angstroms.
31. The method of claim 19, wherein H + The peak density (D1) of He + The peak densities (D2) of ions are within about 400 angstroms of each other.
32. The method of claim 19, wherein H + The peak density (D1) of He + The peak densities (D2) of ions are within about 200 angstroms of each other.
33. The method of claim 19, wherein step (c) comprises annealing the ion implanted single crystal silicon donor substrate at a temperature between about 250°C and about 300°C for a duration between 10 minutes and 60 minutes.
34. The method of claim 19, wherein step (e) comprises annealing the multilayer substrate at a temperature between about 300°C and about 400°C for a duration between 10 minutes and 60 minutes.
35. The method of claim 19, wherein the silicon layer having the thickness between about 500 angstroms and about 2500 angstroms transferred from the single crystal silicon donor substrate to the handle substrate has a thickness variation of less than about 10 angstroms.
36. The method of claim 19, wherein step (e) comprises annealing the multilayer substrate at a pressure between about 0.5 MPa and about 200 MPa.