Preparation method of polymer-two-dimensional nanosheet composite material aqueous zinc ion battery negative electrode protection layer

Through the protective layer of polymer-two-dimensional nanosheet composite material, the negative electrode self-corrosion and dendrite problems in aqueous zinc ion batteries are solved, and the long-term stable cycle and efficient electrochemical performance of zinc ion batteries are achieved, which significantly improves the stability of the battery. and reversibility.

CN118943274APending Publication Date: 2024-11-12TIANJIN UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410983184.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The presence of side reactions such as self-corrosion of the negative electrode, hydrogen evolution and dendrite growth in the aqueous zinc ion battery seriously restricts its large-scale application. The existing protective layer materials have insufficient mechanical properties and barrier effects, and it is impossible to effectively avoid dendrite puncture and electrolyte consumption.

Method used

Polymer-two-dimensional nanosheet composite material is used as the negative electrode protective layer. By combining GO, iCOF, MOF, MXene and other two-dimensional materials with polyether polyamide block copolymer PEBAX, cast film liquid is formed and dripped through pipette. Cast on the surface of zinc foil to form a tight and uniform protective layer to avoid dendrites and side reactions.

Benefits of technology

The desolvation of zinc ions is achieved, which extends the cycle life of the battery and significantly improves the stability. It can maintain a stable cycle of more than 3500 hours under high load conditions, which significantly improves the reversibility and Coulomb efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943274A_ABST
    Figure CN118943274A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of new energy, and relates to a preparation method of a polymer-two-dimensional nanosheet composite material aqueous zinc ion battery negative electrode protection layer. The method mainly comprises the following steps: uniformly blending different types of two-dimensional nano materials, such as graphene oxide (GO), an ionic covalent organic framework nanosheet (iCOF), a metal organic framework material (MOF), transition metal carbonitride (MXene), vermiculite and the like, with a polyether polyamide block copolymer (PEBAX) to prepare a composite material membrane casting solution; and dripping and casting on the surface of the zinc electrode, and drying to obtain the composite material protective layer. The iCOF (Li) nanosheet used in the invention is prepared from 1, 3, 5-triformyl phloroglucinol (Tp) and 2, 5-diaminobenzene sulfonic acid (PA-SO3H) through a phase transfer polymerization method, and the iCOF (Li) nanosheet is prepared after ion exchange with lithium acetate (LiAC). The other two-dimensional materials and PEBAX can be directly purchased. The uniform and compact composite material protection layer is prepared on the surface of the metal zinc through a drop casting method, operation is easy, and the large-scale application potential is achieved. The protective layer has excellent mechanical properties, can block corrosion of electrolyte to the zinc negative electrode, and inhibits hydrogen evolution reaction; the obtained zinc negative electrode can be used for preparing an aqueous zinc ion battery, rich functional groups in the composite material can accelerate the desolvation process of zinc ions, promote uniform deposition of zinc and avoid dendritic crystal growth, and long-term stable circulation and good capacity retention ratio of the zinc ion battery are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of new energy technology, and specifically relates to a preparation method and application of a negative electrode protective layer of an aqueous zinc ion battery of a polymer-two-dimensional nanosheet composite material. Background Art

[0002] In recent years, with the continuous development of science and technology and the economy, the demand for energy has continued to increase, and environmental problems have become increasingly serious. How to balance energy and environmental issues has become a top priority in contemporary research. Common clean energy sources such as wind energy, tidal energy, and solar energy are often limited by time and weather conditions, and stable energy storage equipment is needed to expand their application areas. Traditional lithium-ion batteries have the disadvantages of high price and strong pollution. The development of new green and environmentally friendly energy storage devices is of great significance. Among various metal batteries, aqueous zinc-ion batteries have high natural abundance, low cost, and large theoretical capacity (820mAh g -1 or 5854 mAh cm -3 ), redox potential lower than the standard reduction potential (-0.76V), environmental friendliness, good stability and other advantages have become a research hotspot. Aqueous zinc-ion batteries use metallic zinc as the negative electrode and aqueous electrolyte solutions such as zinc sulfate (ZnSO4) and zinc trifluoromethanesulfonate (Zn(OTf)2) as the electrolyte. The operation does not require a vacuum environment and is simple and convenient. However, in aqueous zinc-ion batteries, there are self-corrosion of the negative electrode, hydrogen evolution, dendrite growth and a series of side reactions, which seriously limit their large-scale application.

[0003] In aqueous zinc-ion batteries, the flaky or spike-like metal zinc produced by the uneven deposition of zinc ions on the negative electrode surface is called dendrites. The formation of zinc dendrites will seriously affect the battery performance. The generated dendrites will penetrate the isolation layer and eventually cause the battery to short-circuit. After the dendrites are separated from the electrode, they will form "dead zinc", which will reduce the coulombic efficiency (CE) and reversibility of the battery. In addition, corrosion and hydrogen evolution reaction (HER) occurring on the negative electrode surface will consume the electrolyte, generate a large amount of hydrogen and cause the battery to swell. There are many ways to improve the performance of aqueous zinc-ion batteries, mainly including: diaphragm modification, adding additives to the electrolyte, artificially constructing a negative electrode protective layer, etc.

[0004] In existing research, artificially constructing a protective layer on the negative electrode surface can effectively avoid direct contact between the metal negative electrode and the electrolyte. Commonly used protective layer materials can be divided into two-dimensional inorganic materials and organic polymer materials. Two-dimensional materials have excellent mechanical properties, but poor ductility, weak bonding with zinc foil, and cannot be evenly coated; polymer materials have good barrier effects, but poor mechanical properties and insufficient resistance to dendrite puncture. Therefore, it is necessary to select appropriate components, develop a polymer-two-dimensional nanosheet composite material that combines the advantages of both, and use a simple method to make a negative electrode protective layer to improve the performance of aqueous zinc-ion batteries. Summary of the invention

[0005] The primary purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a negative electrode protective layer of an aqueous zinc ion battery using a polymer-two-dimensional nanosheet composite material. The method has simple conditions and is easy to operate. The zinc negative electrode coated with the composite material is assembled into an aqueous zinc ion battery. The obtained zinc negative electrode has excellent reversibility and can maintain a long-term stable cycle of the battery.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a negative electrode protective layer of an aqueous zinc ion battery of a polymer-two-dimensional nanosheet composite material comprises the following steps:

[0008] S1: Place GO powder (MOF, MXene, vermiculite) in water and stir at a low speed on a magnetic stirring table until it is evenly dispersed to obtain a two-dimensional material aqueous solution; obtain covalent organic framework nanosheets through 1,3,5-triformylphloroglucinol (Tp) and 2,5-diaminobenzenesulfonic acid (Pa-SO3H), filter and wash, and exchange ions with lithium acetate, and take the supernatant as the COFs aqueous solution.

[0009] S2: placing the solid particles of polyether polyamide block copolymer (PEBAX) in a mixed solution of anhydrous ethanol and deionized water, wherein the volume fraction ratio of the two is 1:3 to 3:1, heating to 50°C-100°C, and reacting for 2-12 hours to completely dissolve the solid particles.

[0010] S3: PEBAX solution and aqueous solution of two-dimensional materials (GO, COFs, MOF, vermiculite, MXene, etc.) are added into a beaker at a volume ratio of 1:1 to 1:5, magnetically stirred overnight at room temperature, then ultrasonicated for 0.5-2 hours to fully mix, and allowed to stand to form a casting solution.

[0011] S4: drop-casting the casting solution prepared in step S3 onto the surface of the metal zinc foil by a pipette gun, and setting it aside at room temperature until it is completely dried for later use.

[0012] The specific method for synthesizing the ionic covalent organic framework (iCOF) nanosheets described in step S1 is as follows:

[0013] iCOF(H)(TpPa-SO3H) nanosheets were synthesized by phase transfer polymerization. 2,5-Diaminobenzenesulfonic acid (Pa-SO3H) was dissolved in deionized water by ultrasonic treatment to form an aqueous solution. Then, 1,3,5-triformylphloroglucinol (Tp) was dissolved in n-octanoic acid and ultrasonically treated to form an organic solution. Finally, the Tp organic solution was slowly added to the top of the Pa-SO3H aqueous solution. The synthesis system was carried out at room temperature and undisturbed conditions for several days to promote the growth of iCOF(H) nanosheets. The bottom solution of the synthesized iCOF(H) nanosheets was dialyzed in deionized water to remove the residual amine precursor.

[0014] Ion exchange process. The treated iCOF(H) nanosheets were added to lithium acetate (LiAC) to form a solution and stirred vigorously. Then, the solution was further dialyzed to completely remove the residual LiAC. The resulting suspension was recorded as iCOF(Li) and its concentration was characterized by freeze-drying.

[0015] Preferably, the PEBAX model in step S1 is PEBAX 1657, the mass fraction of the solution is 1 to 15 wt %, and the concentration of the two-dimensional material aqueous solution is 1 to 5 mg / mL.

[0016] Preferably, the stirring time of the two-dimensional material aqueous solution in step S1 is 8 to 12 hours.

[0017] Preferably, the casting solution in step S3 is stirred for 10 to 24 hours.

[0018] Preferably, in the specific method for synthesizing the ionic covalent organic framework (iCOF) nanosheets in step S1, the concentrations of the Pa-SO3H aqueous solution and the Tp organic solution are 0.001 to 0.01 M. The synthesis system needs to be carried out at room temperature for 1 to 5 days.

[0019] Preferably, in the specific method for synthesizing the ionic covalent organic framework (iCOF) nanosheets in step S1, the dialysis treatment time is 1 to 5 days. During the ion exchange process, the concentration of the iCOF (H) nanosheet solution is 0.5 to 2M.

[0020] The second object of the present invention is to prepare a zinc negative electrode coated with a composite material aqueous zinc ion battery negative electrode protective layer using the above method.

[0021] The present invention also provides an aqueous zinc ion battery, characterized in that a zinc negative electrode coated with the composite material aqueous zinc ion battery negative electrode protective layer is used.

[0022] The advantages and beneficial effects of the present invention are:

[0023] 1. The present invention is a method for preparing a negative electrode protective layer of a water-based zinc ion battery made of a polymer-two-dimensional nanosheet composite material, which is simple and convenient to operate and has low cost. The polymer used is PEBAX, and the two-dimensional materials include but are not limited to GO, iCOF, MOF, vermiculite, MXene, etc., which have a wide range of applications.

[0024] 2. The present invention discloses a method for preparing a negative electrode protective layer of an aqueous zinc ion battery of a polymer-two-dimensional nanosheet composite material. The prepared protective layer is tightly bonded to the zinc foil, is dense and uniform, and can promote the desolvation reaction of zinc ions and accelerate their uniform deposition, thereby obtaining a zinc anode without dendrites and other side reactions.

[0025] 3. The present invention is a method for preparing a negative electrode protective layer of a water-based zinc ion battery using a polymer-two-dimensional nanosheet composite material. The modified electrode is made into a symmetrical battery at 25°C and 1 mA / cm 2 、1mAh / cm 2 Under these conditions, the battery can cycle stably for more than 3,500 hours, which is much longer than a symmetric battery made using unmodified zinc foil as the negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the preparation method of the present invention;

[0027] Figure 2 This is a scanning electron microscope image of the surface morphology of the zinc electrode after being coated with a polymer-two-dimensional nanosheet composite material protective layer as described in Example 1 of the present invention;

[0028] Figure 3 The cycle performance analysis of the zinc-zinc (Zn-Zn) symmetric battery assembled in Example 1 of the present invention and the comparative example;

[0029] Figure 4 This is the cycle performance analysis of the Zn-Zn assembled in Example 1 of the present invention under high current conditions of a symmetrical battery;

[0030] Figure 5 The Zn-Zn symmetrical battery assembled in Example 2 of the present invention is 1 mA / cm 2 (1mAh / cm 2 ) after cycling for 60 hours under the conditions of scanning electron microscope (SEM) of the zinc negative electrode surface;

[0031] Figure 6 The cycle performance analysis of the Zn-Zn symmetric battery assembled in Example 2 of the present invention and the comparative example;

[0032] Figure 7 The cycle performance analysis of the zinc-vanadium pentoxide (Zn-V2O5) full battery assembled in Example 3 of the present invention and the comparative example;

[0033] Figure 8 This is a scanning electron microscope image of the surface morphology of the untreated zinc electrode in the comparative example of the present invention;

[0034] Fig. 9 The Zn-Zn symmetrical battery assembled with the untreated zinc plate in the comparative example of the present invention has a current of 1 mA / cm 2 (1mAh / cm 2 ) after cycling for 60 hours under the conditions of scanning electron microscope (SEM) of the zinc negative electrode surface. DETAILED DESCRIPTION

[0035] The technical solution of the present invention will be further described in detail below in conjunction with specific embodiments. The described embodiments are only part of the embodiments of the present invention, which are only used to explain the present invention and are not intended to limit the scope of protection of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] In the examples of the present invention, if the specific conditions are not specified, the preparation is carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are conventional products that can be purchased commercially.

[0037] like Figure 1 As shown, the present invention is a method for preparing a negative electrode protective layer of an aqueous zinc ion battery of a polymer-two-dimensional nanosheet composite material. The selected polymer is PEBAX 1657, and applicable two-dimensional materials include but are not limited to GO, iCOF, MOF, vermiculite, MXene, etc.

[0038] Example 1

[0039] A method for preparing a negative electrode protective layer of an aqueous zinc ion battery of a polymer-two-dimensional nanosheet composite material, the steps are as follows:

[0040] First, GO powder was placed in water and stirred at low speed on a magnetic stirring table for 12 hours to obtain a GO aqueous solution; PEBAX solid particles were placed in a mixed solution of ethanol: water with a volume fraction ratio of 3:1 and heated to 70°C to completely dissolve it. Secondly, PEBAX solution and GO aqueous solution were added to a beaker in a ratio of 1:1, magnetically stirred overnight at room temperature, and then ultrasonicated for 1 hour to fully mix them, and then allowed to stand to form a casting solution.

[0041] The casting solution prepared above was drop-casted on the surface of the metal zinc foil by a pipette gun, left at room temperature for 8 hours, and then used after being completely dried.

[0042] The casting solution described in Example 1 has a PEBAX solution mass fraction of 5 wt %, a GO aqueous solution concentration of 2 mg / mL, and a zinc foil thickness of 50 μm, which is cut into circular electrodes with a diameter of 12 mm using a slicer.

[0043] The zinc plate coated with the polymer-two-dimensional nanosheet composite material protective layer prepared above was used as the positive and negative electrodes of the aqueous zinc ion battery, and the electrolyte used was 3M Zn(OTf)2, and the amount used was 150μL. Under normal temperature and natural conditions, a Zn-Zn symmetrical battery was assembled. The battery shell model used was CR2032.

[0044] The assembly order of the aqueous zinc ion battery is negative electrode shell, spring, gasket, zinc electrode plate coated with a polymer-two-dimensional nanosheet composite material protective layer, glass fiber separator (GF), zinc electrode plate coated with a polymer-two-dimensional nanosheet composite material protective layer, and positive electrode shell.

[0045] The surface morphology of the zinc electrode coated with the polymer-two-dimensional nanosheet composite material protective layer described in Example 1 is as follows Figure 2 As shown, it can be seen that the protective coating surface is uniform and dense, and the flat protective layer is closely combined with the zinc plate without obvious defects.

[0046] like Figure 3 As shown, the Zn-Zn symmetrical cell described in Example 1 was placed in an electrochemical workstation and operated at 25°C, 1 mA / cm 2 (1mAh / cm 2 ) conditions for long-term cycling, the Zn-Zn symmetric battery protected by the polymer-two-dimensional nanosheet composite material can stably maintain a cycle of more than 3600 hours, which is about 24 times (150 hours) of the cycle life of the untreated Zn-Zn symmetric battery under the same conditions. This proves that the present invention can effectively avoid a series of negative effects in aqueous zinc ion batteries, effectively extend the cycle life of the battery and enhance its stability.

[0047] like Figure 4 As shown, the Zn-Zn symmetrical cell described in Example 1 was placed in an electrochemical workstation and operated at 25°C, 10 mA / cm 2 (10mAh / cm 2 ) Under long-term cycling conditions with high current, the Zn-Zn symmetric battery protected by the polymer-two-dimensional nanosheet composite material can stably maintain cycling for more than 1000 hours. Under high current conditions that the untreated Zn-Zn symmetric battery cannot withstand, the present invention can still maintain long-term reversible cycling of the aqueous zinc ion battery.

[0048] Example 2

[0049] iCOF(H)(TpPa-SO3H) nanosheets were synthesized by phase transfer polymerization. 0.3mmol Pa-SO3H was dissolved in 30mL deionized water by ultrasonic treatment to form an aqueous solution. Then, 0.1mmol Tp was dissolved in 20mL n-octanoic acid and ultrasonically treated for 30min to form an organic solution. Finally, the Tp organic solution was added dropwise to the top of the Pa-SO3H aqueous solution. The reaction was carried out at room temperature for 5 days to promote the growth of iCOF(H) nanosheets. The bottom solution of the synthesized iCOF(H) nanosheets was dialyzed in deionized water to remove the residual amine precursor.

[0050] Ion exchange process. The treated iCOF(H) nanosheets were added to 1M lithium acetate (LiAC) solution and stirred vigorously for 3 days. Then, the solution was further dialyzed to completely remove the residual LiAC. The resulting suspension was recorded as iCOF(Li) and its concentration was characterized by freeze drying. The concentration of the iCOF(Li) solution was about 1 mg / mL.

[0051] The PEBAX solution and the iCOF solution were added into a beaker in a volume ratio of 1:1, magnetically stirred at room temperature overnight, then ultrasonicated for 1 hour to fully mix, and allowed to stand to form a casting solution.

[0052] The casting solution prepared above was drop-casted on the surface of the metal zinc foil by a pipette gun, left at room temperature for 8 hours, and then used after being completely dried.

[0053] The casting solution described in Example 2 has a PEBAX solution mass fraction of 5 wt %, and the zinc foil used has a thickness of 50 μm, which is cut into circular electrodes with a diameter of 12 mm using a slicer.

[0054] The zinc plate coated with the polymer-two-dimensional nanosheet composite material protective layer prepared above was used as the positive and negative electrodes of the aqueous zinc ion battery, and the electrolyte used was 3M Zn(OTf)2, and the amount used was 150μL. Under normal temperature and natural conditions, a Zn-Zn symmetrical battery was assembled. The battery shell model used was CR2032.

[0055] The assembly order of the aqueous zinc ion battery is negative electrode shell, spring, gasket, zinc electrode plate coated with a polymer-two-dimensional nanosheet composite material protective layer, glass fiber separator (GF), zinc electrode plate coated with a polymer-two-dimensional nanosheet composite material protective layer, and positive electrode shell.

[0056] like Figure 5 As shown, the Zn-Zn symmetric cell described in Example 2 was placed in an electrochemical workstation and operated at 25°C, 1 mA / cm 2 (1mAh / cm 2) conditions for 60 hours, and observed the deposition morphology on the surface of the zinc plate. Obviously, under the action of the protective layer, the plate still had a relatively smooth surface after 60 hours of cycling, and no obvious dendrite formation and corrosion were observed.

[0057] like Figure 6 As shown, the Zn-Zn symmetric cell described in Example 2 was placed in an electrochemical workstation and operated at 25°C, 1 mA / cm 2 (1mAh / cm 2 ) conditions for long-term cycling, the Zn-Zn symmetric battery protected by the polymer-two-dimensional nanosheet composite material can stably maintain the cycle for more than 2500 hours, proving that the present invention has certain scalability for different types of two-dimensional materials, and the two schemes mentioned in the above examples can effectively improve the performance of aqueous zinc-ion batteries.

[0058] Example 3

[0059] The preparation method of a polymer-two-dimensional nanosheet composite water-based zinc ion battery negative electrode protective layer is the same as in Experimental Example 1. The zinc plate coated with the polymer-two-dimensional nanosheet composite protective layer is used as the negative electrode of the water-based zinc ion battery, and the electrolyte used is 3M Zn(OTf)2, and the amount used is 150μL. The positive electrode made of hydrophilic carbon cloth and vanadium pentoxide (V2O5) is assembled into a Zn-V2O5 full battery under normal temperature and natural conditions. The battery shell model used is CR2032.

[0060] The assembly order of the full battery is negative electrode shell, spring, gasket, zinc electrode plate coated with polymer-two-dimensional nanosheet composite material protective layer, glass fiber separator (GF), V2O5 positive electrode, and positive electrode shell.

[0061] The assembled PG@Zn-V2O5 full battery was tested for cycle performance at 25°C and 2A / g. Figure 7 The initial discharge capacity of the Zn-V2O5 full battery is about 200mAh / g. After more than 2000 cycles, the capacity retention rate is about 80%, and the coulombic efficiency remains above 99.5%.

[0062] Example 4

[0063] The preparation method of a polymer-two-dimensional nanosheet composite water-based zinc ion battery negative electrode protective layer is the same as in Experimental Example 2. The zinc plate coated with the polymer-two-dimensional nanosheet composite protective layer is used as the negative electrode of the water-based zinc ion battery, and the electrolyte used is 3M Zn(OTf)2, and the amount used is 150μL. The positive electrode made of hydrophilic carbon cloth and vanadium pentoxide (V2O5) is assembled into a Zn-V2O5 full battery under normal temperature and natural conditions. The battery shell model used is CR2032.

[0064] The assembly order of the full battery is negative electrode shell, spring, gasket, zinc electrode plate coated with polymer-two-dimensional nanosheet composite material protective layer, glass fiber separator (GF), V2O5 positive electrode, and positive electrode shell.

[0065] Comparative Example

[0066] The untreated zinc plate was directly used as the positive and negative electrodes of the aqueous zinc ion battery. The electrolyte used was 3M Zn(OTf)2, and the amount used was 150μL. Under normal temperature and natural conditions, a Zn-Zn symmetrical battery was assembled. The battery shell model used was CR2032.

[0067] The zinc foil has a thickness of 50 μm and a diameter of 12 mm.

[0068] The surface morphology of the original zinc electrode is as follows Figure 8 As shown, scratches and flaws can be seen on the surface of the uncoated zinc plate. The uneven surface is more likely to lead to the formation of dendrites and the occurrence of side reactions.

[0069] The Zn-Zn symmetrical cell described in the comparative example was placed in an electrochemical workstation and operated at 25°C and 1 mA / cm 2 (1mAh / cm 2 ) for 60 hours, and observe the deposition morphology on the surface of the zinc plate. Fig. 9 As shown, large dendrites and sunken holes are formed on its surface, and it short-circuit and become inactive within 150 hours.

[0070] In summary, the present invention provides a method for preparing a negative electrode protective layer of an aqueous zinc ion battery of a polymer-two-dimensional nanosheet composite material, which can obtain a stable negative electrode protective layer through extremely simple operation steps under room temperature and normal pressure, has low process difficulty and low cost, and thus has industrial application prospects for large-scale production and preparation. At the same time, the selectable two-dimensional materials include but are not limited to GO, iCOF, MOF, vermiculite, MXene, etc., and have a wide range of applications. After the aqueous zinc ion battery is actually made, the protective layer shows excellent performance in both the Zn-Zn symmetric battery and the Zn-V2O5 full battery, can effectively prolong the stability of the battery, and paves the way for the practical application of aqueous zinc ion batteries.

[0071] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. A method for preparing a negative electrode protective layer of a water-based zinc ion battery of a polymer-two-dimensional nanosheet composite material, characterized in that: The following steps are involved: A polyether polyamide block copolymer solution is mixed with different types of two-dimensional nanosheet solutions to prepare a casting solution, and a polymer-two-dimensional nanosheet composite material protective layer is formed on the zinc surface by a drop casting method.

2. A method for preparing a negative electrode protective layer for a composite material aqueous zinc ion battery according to claim 1, characterized in that: The following steps are involved: S1 Place GO powder (MOF, MXene, vermiculite) in water and stir at low speed on a magnetic stirring table until it is evenly dispersed to obtain a two-dimensional material aqueous solution; 1,3,5-triformylphloroglucinol (Tp) and 2,5-diaminobenzenesulfonic acid (Pa- SO3H) to obtain covalent organic framework nanosheets, which were filtered, washed, and ion-exchanged with lithium acetate (LiAC), and the supernatant was taken as the iCOF aqueous solution. S2: placing the solid particles of polyether polyamide block copolymer (PEBAX) in a mixed solution of anhydrous ethanol and deionized water, wherein the volume ratio of the two is 1:3 to 3:1, heating to 50°C-100°C, and reacting for 2-12 hours to completely dissolve the solid particles. S3: PEBAX solution and aqueous solution of two-dimensional materials (GO, iCOF, MOF, vermiculite, MXene, etc.) are added into a beaker at a volume ratio of 1:1 to 1:5, magnetically stirred overnight at room temperature, then ultrasonicated for 0.5-2 hours to fully mix, and allowed to stand to form a casting solution. S4: drop-casting the casting solution prepared in step S3 onto the surface of the metal zinc foil by a pipette gun, and setting it aside at room temperature until it is completely dried for later use.

3. The specific method for synthesizing the ionic covalent organic framework (iCOF) nanosheet according to claim 2 is as follows: iCOF(H)(TpPa-SO3H) nanosheets were synthesized by phase transfer polymerization. 2,5-Diaminobenzenesulfonic acid (Pa-SO3H) was dissolved in deionized water by ultrasonic treatment to form an aqueous solution. Then, 1,3,5-triformylphloroglucinol (Tp) was dissolved in n-octanoic acid and ultrasonically treated to form an organic solution. Finally, the Tp organic solution was added dropwise to the top of the Pa-SO3H aqueous solution. After several days of reaction, a two-phase mixture was obtained, in which the synthesized iCOF(H) nanosheets were enriched in the bottom aqueous solution, which was dialyzed to remove unreacted monomers. Ion exchange process. The treated iCOF(H) nanosheets were added to lithium acetate (LiAC) to form a solution and stirred vigorously. Then, the solution was further dialyzed to completely remove the residual LiAC. The resulting suspension was recorded as iCOF(Li) and its concentration was characterized by freeze-drying.

4. The method for preparing the negative electrode protective layer of a composite material aqueous zinc ion battery according to claim 2, characterized in that: The PEBAX model in S1 is PEBAX 1657, the solution mass fraction is 1-15wt%, and the concentration of the two-dimensional material aqueous solution is 1-5mg / mL.

5. The method for preparing the negative electrode protective layer of composite material aqueous zinc ion battery according to claim 2, characterized in that: The stirring time of the two-dimensional material aqueous solution in S1 is 8 to 12 hours.

6. The method for preparing the negative electrode protective layer of a composite material aqueous zinc ion battery according to claim 2, characterized in that: The casting solution in S3 is stirred for 10 to 24 hours.

7. The specific method for synthesizing ionic covalent organic framework (iCOF) nanosheets according to claim 3, characterized in that: The concentrations of the Pa-SO3H aqueous solution and the Tp organic solution are 0.001 to 0.01 M. The synthesis system needs to be carried out at room temperature for 1 to 5 days.

8. The specific method for synthesizing the ionic covalent organic framework (iCOF) nanosheet according to claim 3, characterized in that The dialysis treatment time is 1 to 5 days, and the concentration of the iCOF(H) nanosheet solution during the ion exchange process is 0.5 to 2M.

9. A zinc negative electrode coated with a composite material aqueous zinc ion battery negative electrode protective layer prepared by the method according to claim 1.

10. An aqueous zinc ion battery, characterized in that: A zinc negative electrode comprising the negative electrode protective layer of an aqueous zinc ion battery coated with a composite material as claimed in claim 9.

Citation Information

Cited By

  • Zinc pole piece coated with sulfonyl COF membrane, preparation method of zinc pole piece and aqueous zinc battery

    CN120473485A