Positive pole piece and preparation method thereof, sodium ion battery, battery module and battery pack

By setting a sodium supplement layer between the positive electrode current collector and the film layer in a sodium-ion battery, and controlling its thickness ratio and optimizing its composition, the problem of unsatisfactory volumetric energy density improvement in sodium-ion batteries was solved, achieving higher energy density and safety.

CN118943289APending Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310533923.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing sodium-ion batteries suffer from irreversible sodium-ion loss during the first charge, resulting in unsatisfactory improvements in volumetric energy density.

Method used

A sodium replenishment layer is set between the positive electrode current collector and the positive electrode film layer, and the ratio of the thickness of the sodium replenishment layer to the thickness of the positive electrode film layer is controlled within the range of 0.01≤H1/H2≤0.2. The mass ratio of sodium replenishment agent, conductive agent and binder is optimized, and a dense sodium replenishment layer is formed by gravure coating process.

Benefits of technology

It improves the volumetric energy density and rate performance of sodium-ion batteries, enhances electrode conductivity consistency and adhesion, and reduces battery safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004225804540000151
    Figure BDA0004225804540000151
  • Figure BDA0004225804540000161
    Figure BDA0004225804540000161
  • Figure BDA0004225804540000171
    Figure BDA0004225804540000171
Patent Text Reader

Abstract

According to the positive electrode plate, the sodium supplementing layer is arranged between the positive electrode current collector and the positive electrode film layer, and the thickness of the sodium supplementing layer and the thickness of the positive electrode film layer are controlled to meet a certain relationship, so that the volume energy density of a sodium ion battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of sodium ion batteries, and in particular to a positive electrode plate and a preparation method thereof, a sodium ion battery, a battery module, a battery pack and an electrical device. Background Art

[0002] With the increasing cost of lithium ore, sodium-ion batteries have shown good application prospects in the fields of energy storage and power batteries due to their low cost. However, sodium-ion batteries will experience irreversible sodium ion loss during the first charging process, which reduces the energy density of sodium-ion batteries. Energy density is the most important parameter to measure the ability of a battery system to store electrical energy, and can be divided into mass energy density and volume energy density. The volume energy density of sodium-ion batteries is an important parameter in battery research and development, and its size is related to the effective use of the battery. If the volume energy density is high, the output capacity of the battery in a small volume can be improved. However, the current effect of improving the volume energy density of sodium-ion batteries is still not ideal.

[0003] Therefore, how to improve the volumetric energy density of sodium-ion batteries has become an important research topic. Summary of the invention

[0004] In view of the problems existing in the background technology, the present application provides a positive electrode plate, which can effectively improve the volume energy density of a sodium ion battery.

[0005] The positive electrode sheet provided in the first aspect of the present application includes a positive electrode current collector, a sodium supplement layer and a positive electrode film layer. The sodium supplement layer is arranged between the positive electrode current collector and the positive electrode film layer. The thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer satisfy: 0.01≤H1 / H2≤0.2.

[0006] The present application can improve the volume energy density of the sodium ion battery by providing a sodium supplement layer between the positive electrode current collector and the positive electrode film layer, and controlling the thickness of the sodium supplement layer and the thickness of the positive electrode film layer to satisfy the above relationship.

[0007] In some embodiments, according to the first aspect, a first example of the first aspect is provided, and H1 and H2 satisfy: 0.05≤H1 / H2≤0.1.

[0008] By optimizing the relationship between H1 and H2, it is beneficial to further improve the volume energy density of sodium-ion batteries.

[0009] In some embodiments, according to the first aspect, a second example of the first aspect is provided, 5 μm≤H1≤30 μm.

[0010] By optimizing the thickness of the sodium supplement layer, it is beneficial to further improve the volume energy density of sodium ion batteries.

[0011] In some embodiments, according to the first aspect, a third example of the first aspect is proposed, the sodium supplement layer includes a sodium supplement. The sodium supplement includes an inorganic compound of sodium. Preferably, the sodium supplement includes one or more of Fe, Ni, Mn, Co, and V.

[0012] By optimizing the types of sodium supplements, it is beneficial to improve the rate performance of sodium ion batteries while increasing the volume energy density of sodium ion batteries.

[0013] In some embodiments, according to the first aspect, a fourth example of the first aspect is proposed, wherein the sodium supplement comprises Na2NiO2, Na5FeO4, Na4Ni 0.5 Mn 1.5 One or more of O4, Na6CoO4, Na5V2(PO4)3.

[0014] By optimizing the types of sodium supplements, it is beneficial to further improve the rate performance of sodium ion batteries while increasing the volume energy density of sodium ion batteries.

[0015] In some embodiments, according to the first aspect, a fifth example of the first aspect is provided, wherein the sodium supplement layer further includes a conductive agent and a binder.

[0016] Adding a conductive agent to the sodium supplement layer is beneficial to reducing the electron transfer impedance between interfaces, increasing the conductivity of the positive electrode current collector and the positive electrode film layer, and reducing the film resistance. Adding a binder to the sodium supplement layer is beneficial to increasing the bonding force between the sodium supplement layer and the positive electrode film layer and the positive electrode current collector, improving the brittleness of the electrode sheet, and reducing the occurrence of problems such as cold pressing demoulding and winding corner demoulding.

[0017] In some embodiments, according to the first aspect, a sixth example of the first aspect is proposed, wherein the mass ratio of the sodium supplementer, the conductive agent, and the binder is (40-91):(5-40):(4-30).

[0018] By optimizing the mass ratio of the sodium supplement, the conductive agent and the binder, it is beneficial to achieve a compromise in improving energy density, improving conductivity and improving adhesion.

[0019] A second aspect of the present application provides a method for preparing a positive electrode sheet, comprising the following steps:

[0020] mixing a sodium supplement agent and a solvent to obtain a sodium supplement slurry;

[0021] coating the sodium supplement slurry on the surface of the positive electrode current collector, and obtaining a sodium supplement layer after drying; and

[0022] forming a positive electrode film layer on the sodium supplement layer;

[0023] The thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer satisfy: 0.01≤H1 / H2≤0.2.

[0024] The positive electrode sheet obtained by the preparation method of the present application can improve the volume energy density of the sodium ion battery.

[0025] In some embodiments, according to the second aspect, a first example of the second aspect is provided, wherein the coating method of the sodium supplement slurry comprises gravure coating.

[0026] The use of gravure coating of the sodium supplement slurry is beneficial to obtaining a dense sodium supplement layer, reducing the thickness of the sodium supplement layer, and improving the volume energy density of the battery.

[0027] In some embodiments, according to the second aspect, a second example of the second aspect is provided, wherein the preparation of the sodium supplement slurry includes mixing a sodium supplement agent, a solvent, a conductive agent, and a binder.

[0028] Adding a conductive agent to the sodium supplement slurry is beneficial to reducing the electron transfer impedance between interfaces and increasing the conductivity of the positive electrode current collector and the positive electrode film layer. Adding a binder to the sodium supplement slurry is beneficial to increasing the bonding force between the sodium supplement layer and the positive electrode film layer and the positive electrode current collector, improving the brittleness of the pole piece and reducing the occurrence of problems such as powder loss and light transmission at the corners of the inner circle of winding.

[0029] A third aspect of the present application provides a sodium ion battery, comprising the positive electrode sheet of the first aspect of the present application or the positive electrode sheet obtained by the preparation method of the second aspect of the present application.

[0030] A fourth aspect of the present application provides a battery module, comprising the sodium ion battery of the third aspect of the present application.

[0031] A fifth aspect of the present application provides a battery pack, comprising the sodium ion battery of the third aspect of the present application or the battery module of the fourth aspect of the present application.

[0032] A sixth aspect of the present application provides an electrical device, comprising at least one of the sodium ion battery of the third aspect of the present application, the battery module of the fourth aspect of the present application, and the battery pack of the fifth aspect of the present application.

[0033] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. DETAILED DESCRIPTION

[0034] The exemplary embodiments of the present disclosure will be described in more detail below. However, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application. The terms "including" and "having" and any variations thereof in the specification and claims of this application are intended to cover non-exclusive inclusions.

[0036] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.

[0037] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and the "multiple" in "one or more" means more than two (including two).

[0038] In the description of the embodiments of the present application, the term "and / or" is merely a term used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent three situations: A exists, A and B exist at the same time, and B exists.

[0039] The above-mentioned summary of the invention of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0040] With the increasing cost of lithium ore, sodium-ion batteries have shown good application prospects in the fields of energy storage and power batteries due to their low cost. However, sodium-ion batteries will experience irreversible sodium ion loss during the first charging process, which reduces the energy density of sodium-ion batteries. Energy density is the most important parameter to measure the ability of a battery system to store electrical energy, and can be divided into mass energy density and volume energy density. The volume energy density of sodium-ion batteries is an important parameter in battery research and development, and its size is related to the effective use of the battery. High volume energy density is beneficial to improving the output capacity of the battery in a small volume. However, the current effect of improving the volume energy density of sodium-ion batteries is still not ideal. Therefore, how to improve the volume energy density of sodium-ion batteries has become an important research topic.

[0041] In order to solve the above problems, the present application designs a positive electrode plate, by setting a sodium supplement layer between the positive current collector and the positive electrode film layer, so that the sodium supplement layer participates in the discharge during the first charge and discharge process of the sodium ion battery, and releases a large amount of sodium ions to supplement the sodium ions lost when the negative electrode first forms the SEI film; at the same time, the ratio of the thickness H1 of the sodium supplement layer to the thickness H2 of the positive electrode film layer is controlled to meet 0.01≤H1 / H2≤0.2, thereby effectively improving the volume energy density of the sodium ion battery. H1 / H2 is too large or too small, which is not conducive to the improvement of volume energy density. When H1 / H2 is too large, the amount of sodium supplement is certain, but the proportion of inert components such as conductive agents and binders will be too large, resulting in a decrease in volume energy density; when H1 / H2 is too small, the supplemented sodium ions cannot make up for the sodium ions lost when the negative electrode first forms the SEI film, and the sodium supplement effect is poor, and the volume energy density cannot be effectively improved.

[0042] The technical solution described in the embodiments of the present application is applicable to positive electrode sheets, and is also applicable to methods for preparing positive electrode sheets, sodium ion batteries using positive electrode sheets, battery modules using sodium ion batteries, battery packs using sodium ion batteries or battery modules, and electrical devices using at least one of sodium ion batteries, battery modules and battery packs.

[0043] In the first aspect, according to some embodiments of the present application, the present application provides a positive electrode sheet. It includes a positive electrode current collector, a sodium supplement layer and a positive electrode film layer. The sodium supplement layer is arranged between the positive electrode current collector and the positive electrode film layer. The thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer satisfy: 0.01≤H1 / H2≤0.2.

[0044] The present application can improve the volume energy density of the sodium ion battery by providing a sodium supplement layer between the positive electrode current collector and the positive electrode film layer, and controlling the thickness of the sodium supplement layer and the thickness of the positive electrode film layer to satisfy the above relationship.

[0045] In addition, due to processing technology and other reasons, there may be scratches, pits and other defects on the surface of the positive electrode collector. Taking aluminum foil as the positive electrode collector as an example, the production of aluminum foil is made of aluminum ingots as raw materials and rolled through a cold rolling process, but during the processing, scratches and pits will inevitably appear on the surface of the aluminum foil. Defects such as, will affect the conductivity consistency of the electrode during use, and then lead to uneven battery charge and discharge reactions, which may cause safety problems such as short circuit and thermal runaway in the battery. The sodium supplement layer of the present application can cover the defects on the surface of the positive electrode collector in a filling manner, improve the conductivity consistency of the electrode, and thus improve the safety of the battery.

[0046] In some specific embodiments, H1 / H2 may be 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, or 0.2.

[0047] In some specific embodiments, the positive electrode current collector may be a conventional metal foil or a composite current collector (a metal material may be disposed on a polymer substrate to form a composite current collector). As an example, the positive electrode current collector may be an aluminum foil.

[0048] In some specific embodiments, the positive electrode film layer includes a positive electrode active material. The specific type of the positive electrode active material is not limited, and active materials known in the art that can be used for the positive electrode of a sodium ion battery can be used, and those skilled in the art can select according to actual needs.

[0049] For example, the positive electrode active material may include at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.

[0050] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide may be, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.

[0051] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n-A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence state.

[0052] Polyanionic compounds can also be those with sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.

[0053] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedral unit (ZO y ) m+ and an optional halogen anion. Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, which may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.

[0054] Polyanionic compounds include NaFePO4, Na3V2(PO4)3, NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).

[0055] As an optional technical solution of the present application, the Prussian blue compound can be a compound having sodium ions, transition metal ions and cyanide ions (CN - The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds may be, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.

[0056] The positive electrode film layer may also optionally include a binder, a conductive agent and other optional additives.

[0057] As an example, the conductive agent may be one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, Super P (SP), graphene and carbon nanofibers.

[0058] As an example, the binder can be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0059] In some embodiments, H1 and H2 satisfy: 0.05≤H1 / H2≤0.1.

[0060] By optimizing the relationship between H1 and H2, it is beneficial to further improve the volume energy density of sodium-ion batteries.

[0061] In some embodiments, 5 μm≤H1≤30 μm.

[0062] The thickness of the sodium supplement layer is related to the volume energy density of the battery. When releasing the same amount of sodium ions, the smaller the thickness of the sodium supplement layer, the greater the volume energy density of the battery. By optimizing the thickness of the sodium supplement layer, it is helpful to further improve the volume energy density of sodium ion batteries.

[0063] In some specific embodiments, the thickness H1 of the sodium supplement layer may be 5 μm, 10 μm, 15 μm, 20 μm, 25 μm or 30 μm.

[0064] In some embodiments, the sodium supplement layer includes a sodium supplement. The sodium supplement may include an inorganic compound of sodium. Preferably, the sodium supplement may include one or more of Fe, Ni, Mn, Co, and V.

[0065] The sodium supplement containing the above elements has a higher discharge voltage platform, which can make the sodium ions deintercalated from the negative electrode diffuse preferentially into the sodium supplement layer inside the positive electrode plate, so that the sodium ions are gradiently distributed in the depth direction of the plate. During large current discharge, the "gradient distribution" of sodium ions can make the sodium ions quickly embed into the positive electrode material, which is beneficial to improve the rate performance of sodium ion batteries, while improving the volume energy density of sodium ion batteries.

[0066] In some embodiments, the sodium supplement may include Na2NiO2, Na5FeO4, Na4Ni 0.5 Mn 1.5One or more of O4, Na6CoO4, Na5V2(PO4)3.

[0067] By optimizing the types of sodium supplements, it is beneficial to further improve the rate performance of sodium ion batteries while increasing the volume energy density of sodium ion batteries.

[0068] In some embodiments, the sodium supplement layer further includes a conductive agent and a binder.

[0069] Adding a conductive agent to the sodium supplement layer is beneficial to reducing the electron transfer impedance between interfaces, increasing the conductivity of the positive electrode current collector and the positive electrode film layer, and reducing the film resistance. Adding a binder to the sodium supplement layer is beneficial to increasing the bonding force between the sodium supplement layer and the positive electrode film layer and the positive electrode current collector, improving the brittleness of the electrode sheet, and reducing the occurrence of problems such as powder loss and light transmission at the corners of the inner circle of winding.

[0070] In some embodiments, the conductive agent may include one or more of conductive carbon black, carbon nanotubes, superconducting carbon, acetylene black, Ketjen black, graphene, and carbon nanofibers.

[0071] In some specific embodiments, the binder may include one or more of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR).

[0072] In some embodiments, the mass ratio of the sodium supplementer, the conductive agent, and the binder may be (40-91):(5-40):(4-30).

[0073] By optimizing the mass ratio of the sodium supplement, the conductive agent and the binder, it is beneficial to achieve a compromise in improving energy density, improving conductivity and improving adhesion.

[0074] In some specific embodiments, the mass ratio of the sodium supplementer, the conductive agent and the binder may be 60:20:20, 91:5:4, 40:40:20, 60:10:30, 50:40:10, 70:15:15 or 80:5:15, etc.

[0075] A second aspect of the present application provides a method for preparing a positive electrode sheet, comprising the following steps:

[0076] mixing a sodium supplement agent and a solvent to obtain a sodium supplement slurry;

[0077] coating the sodium supplement slurry on the surface of the positive electrode current collector, and obtaining a sodium supplement layer after drying; and

[0078] forming a positive electrode film layer on the sodium supplement layer;

[0079] The thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer satisfy: 0.01≤H1 / H2≤0.2.

[0080] The positive electrode sheet obtained by the preparation method of the present application can improve the volume energy density of the sodium ion battery.

[0081] In some embodiments, the coating method of the sodium supplement slurry may include gravure coating.

[0082] The use of gravure coating of the sodium supplement slurry is beneficial to obtaining a dense sodium supplement layer, reducing the thickness of the sodium supplement layer, and improving the volume energy density of the battery.

[0083] In some embodiments, the preparation of the sodium supplement slurry includes mixing a sodium supplement agent, a solvent, a conductive agent, and a binder.

[0084] Adding a conductive agent to the sodium supplement slurry is beneficial to reducing the electron transfer impedance between interfaces and increasing the conductivity of the positive electrode current collector and the positive electrode film layer. Adding a binder to the sodium supplement slurry is beneficial to increasing the bonding force between the sodium supplement layer and the positive electrode film layer and the positive electrode current collector, improving the brittleness of the pole piece and reducing the occurrence of problems such as powder loss and light transmission at the corners of the inner circle of winding.

[0085] In some embodiments, the sodium supplement may include an inorganic compound of sodium. Preferably, the sodium supplement may include one or more of Fe, Ni, Mn, Co, and V.

[0086] When the sodium supplement contains the above elements, it is beneficial to improve the rate performance of the sodium ion battery while increasing the volume energy density of the sodium ion battery.

[0087] In some embodiments, the sodium supplement may include Na2NiO2, Na5FeO4, Na 1+x Ni 0.5 Mn 1.5 One or more of O4, Na6CoO4, Na5V2(PO4)3.

[0088] By optimizing the types of sodium supplements, it is beneficial to further improve the rate performance of sodium ion batteries while increasing the volume energy density of sodium ion batteries.

[0089] In some embodiments, the solvent may include one or more of N-methylpyrrolidone (NMP), tetrahydrofuran, dimethylformamide, water and anhydrous ethanol. However, the present application is not limited to these solvents, and those skilled in the art may select according to actual needs.

[0090] A third aspect of the present application provides a sodium ion battery, comprising the positive electrode sheet of the first aspect of the present application or the positive electrode sheet obtained by the preparation method of the second aspect of the present application.

[0091] A fourth aspect of the present application provides a battery module, comprising the sodium ion battery of the third aspect of the present application.

[0092] A fifth aspect of the present application provides a battery pack, comprising the sodium ion battery of the third aspect of the present application or the battery module of the fourth aspect of the present application.

[0093] A sixth aspect of the present application provides an electrical device, comprising at least one of the sodium ion battery of the third aspect of the present application, the battery module of the fourth aspect of the present application, and the battery pack of the fifth aspect of the present application.

[0094] The following examples describe the disclosure of the present application in more detail, and these examples are merely illustrative, as it will be apparent to those skilled in the art that various modifications and variations are made within the scope of the disclosure of the present application. Unless otherwise stated, all reagents used in the examples are commercially available or synthesized according to conventional methods, and the instruments used in the examples are commercially available.

[0095] Example 1

[0096] (1) Preparation of positive electrode sheet

[0097] The sodium supplement agent Na6CoO4, the conductive agent (conductive carbon black) and the binder PVDF are fully and evenly mixed with the solvent N-methylpyrrolidone in a ratio of 60:20:20 to obtain a sodium supplement slurry; the sodium supplement slurry is coated on an aluminum foil by extrusion coating, and then dried in an oven and cold pressed to obtain a sodium supplement layer; thereafter, a sodium positive electrode slurry (the weight ratio is positive electrode active material (NaFePO4): acetylene black: PVDF = 95:3:2, used to form a positive electrode film layer) is coated on the sodium supplement layer, and the positive electrode sheet is obtained by drying, cold pressing, die cutting and slitting. In the obtained positive electrode sheet, the thickness H1 of the sodium supplement layer is 10 μm, the thickness H2 of the positive electrode film layer is 100 μm, and the ratio of the thickness H1 of the sodium supplement layer to the thickness H2 of the positive electrode film layer is 0.1.

[0098] (2) Preparation of negative electrode sheet

[0099] The negative electrode active material graphite, the conductive agent acetylene black, the binder styrene butadiene rubber, and the thickener sodium carboxymethyl cellulose are mixed in a weight ratio of graphite: acetylene black: styrene butadiene rubber: sodium carboxymethyl cellulose = 95:2:2:1, and an appropriate amount of deionized water is added and stirred to form a uniform negative electrode slurry; after coating the slurry on the negative electrode current collector copper foil, it is dried and cold pressed to obtain a negative electrode sheet.

[0100] (3) Preparation of electrolyte

[0101] The electrolytes were prepared according to the following method:

[0102] In an argon-filled glove box with a water content of <1 ppm, diethylene glycol dimethyl ether and tetrahydrofuran were mixed in a mass ratio of 1:3, sodium hexafluorophosphate (NaPF6) with a concentration of 1.0 mol / L was added, and after stirring evenly, an electrolyte was obtained.

[0103] (4) Preparation of sodium ion batteries

[0104] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, so that the isolation film is placed between the positive and negative electrode sheets to play an isolating role, and then they are wound to obtain a bare battery cell; the bare battery cell is placed in an outer package, and the prepared electrolyte is injected into the dried battery, and then after vacuum packaging, standing, formation, shaping and other processes, a sodium ion battery is obtained.

[0105] Example 2-Example 4

[0106] A sodium ion battery was prepared according to the method of Example 1, except that the thickness H1 of the sodium supplement layer, the thickness H2 of the positive electrode film layer and their ratio were different from those in Example 1, as shown in Table 1 below.

[0107] Table 1

[0108] serial number <![CDATA[H1 / μm]]> <![CDATA[H2 / μm]]> <![CDATA[H1 / H2]]> Example 1 10 100 0.1 Example 2 2 200 0.01 Example 3 7.5 150 0.05 Example 4 30 150 0.2

[0109] Example 5-Example 7

[0110] A sodium ion battery was prepared according to the method of Example 4, except that the thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer were different, as shown in Table 2 below.

[0111] Table 2

[0112]

[0113]

[0114] Example 8-Example 11

[0115] A sodium ion battery was prepared according to the method of Example 1, except that the sodium supplement was different from that of Example 1, as shown in Table 3 below.

[0116] Table 3

[0117] serial number Sodium supplements Example 1 <![CDATA[Na6CoO4]]> Example 8 <![CDATA[Na2NiO2]]> Example 9 <![CDATA[Na5FeO4]]> Example 10 <![CDATA[Na4Ni 0.5 Mn 1.5 O4]]> Embodiment 11 <![CDATA[Na5V2(PO4)3]]> Example 12 <![CDATA[Na3N]]>

[0118] Example 13

[0119] A sodium ion battery was prepared according to the method of Example 1, except that no conductive agent was added to the sodium supplement slurry.

[0120] Embodiment 14

[0121] A sodium ion battery was prepared according to the method of Example 1, except that the mass ratio of the sodium supplement, the conductive agent and the binder was 60:20:0.5.

[0122] Example 15-Example 17

[0123] A sodium ion battery was prepared according to the method of Example 1, except that the mass ratios of the sodium supplement agent, the conductive agent and the binder in the sodium supplement slurry were different, as shown in Table 4 below.

[0124] Table 4

[0125]

[0126] Embodiment 18

[0127] A sodium ion battery was prepared according to the method of Example 1, except that the sodium supplement slurry was coated on the surface of the substrate by gravure coating.

[0128] Comparative Example 1-Comparative Example 2

[0129] A sodium ion battery was prepared according to the method of Example 1, except that the thickness H1 of the sodium supplement layer, the thickness H2 of the positive electrode film layer and their ratio were different from those in Example 1, as shown in Table 5 below.

[0130] Table 5

[0131]

[0132]

[0133] Characterization Test

[0134] 1. Test of the thickness of the sodium supplement layer H1 and the thickness of the positive electrode film layer H2

[0135] Ion polishing cross-section morphology analyzer was used for characterization test.

[0136] (1) Sample preparation: a. Use ceramic scissors to cut the electrode into 6mm*6mm size, stick it on the sample stage coated with paraffin, and make the sample slightly protrude (<1mm) from the edge of the sample stage. b. Set the polishing voltage and polishing time (90min at 7.5KV). The sample needs to be exposed to the laboratory environment (temperature 24±1℃, humidity 25%±10%) for about 1min. After cutting, immediately transfer the sample to the electron microscope sample chamber for vacuuming.

[0137] (2) Parameter settings: Mode: In-lens, Voltage: 10KV, Aperture: 30um, Working distance: 4.5mm.

[0138] (3) Test process: Take 2-3 photos at 500 times magnification (the field of view includes the upper and lower active materials and the current collector) to test the thickness of the sodium supplement layer H1 and the thickness of the positive electrode film layer H2.

[0139] Battery performance test

[0140] 1. Volume energy density test of sodium ion battery

[0141] At 25°C, the sodium ion battery is first charged to the rated upper limit voltage at a constant current of 0.33C, and then charged to a current of 0.05C at a constant voltage. Then, the battery is discharged to the rated lower limit voltage at a constant current of 0.33C. The discharge energy is recorded as the discharge amount of the sodium ion battery. The discharge energy is divided by the volume of the battery cell (the volume of the battery cell is tested using the drainage method: a sealed, uncharged battery cell is placed in a pool filled with water, and the volume of the water discharged is the volume of the battery cell) to obtain the corresponding volume energy density. The results are shown in Table 6 below.

[0142] 2. Rate performance test of sodium ion battery

[0143] At 25°C, the sodium ion battery is first charged to the rated upper limit voltage at a constant current of 0.33C, and then charged to a current of 0.05C at a constant voltage, and then the battery is discharged to the rated lower limit voltage at a constant current of 2C. The discharge capacity at this time is recorded as the 2C discharge capacity of the sodium ion battery, and the 0.33C discharge capacity is also defined, and the 2C discharge capacity / 0.33C discharge capacity is recorded as the rate performance index. The results are shown in Table 7 below.

[0144] 3. Test the film resistance of the positive electrode after cold pressing

[0145] The cold pressed positive electrode is cut into several 1540.25mm 2 The small disc was then measured with a film resistor meter and the average value was taken. The results are shown in Table 8 below.

[0146] 4. Brittleness test of positive electrode sheet of sodium ion battery

[0147] 1) Take 4cm×25cm (vertical) 100cm 2 For samples of area, sampling is carried out along the TD direction, and the number of samples is ≥ 4;

[0148] 2) 100cm 2 Sample area 100cm 2 Pre-folded (pre-folded in half by 25cm in the longitudinal direction);

[0149] 3) Place the pre-folded sample on the flat surface of the laboratory table and roll it once with a 2kg cylindrical roller;

[0150] 4) Fold the sample along the longitudinal crease. Observe the crease against light. If it is not transparent and not broken, it is an OK product; if it is transparent and broken, it is an NG product.

[0151] 5) After the folding, continue to roll with a cylinder, and then observe the crease until the crease is transparent and broken, and record the number of rolling times n, (n-1) as the brittleness index. The results are shown in Table 8 below.

[0152] Table 6

[0153]

[0154]

[0155] Table 7

[0156]

[0157] Table 8

[0158]

[0159] It can be seen from the embodiments and comparative examples that the present application can improve the volume energy density of the sodium ion battery by providing a sodium supplement layer between the positive electrode current collector and the positive electrode film layer, and controlling the ratio of the thickness H1 of the sodium supplement layer to the thickness H2 of the positive electrode film layer within the range of 0.01-0.2.

[0160] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector, a sodium supplement layer and a positive electrode film layer, wherein the sodium supplement layer is arranged between the positive electrode current collector and the positive electrode film layer, and the thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer satisfy: 0.01≤H1 / H2≤0.

2.

2. The positive electrode sheet according to claim 1, characterized in that: H1 and H2 satisfy: 0.05≤H1 / H2≤0.

1.

3. The positive electrode sheet according to claim 1 or 2, characterized in that: 5μm≤H1≤30μm.

4. The positive electrode sheet according to claim 1 or 2, characterized in that: The sodium supplement layer includes a sodium supplement agent, and the sodium supplement agent includes an inorganic compound of sodium; preferably, the sodium supplement agent contains one or more of Fe element, Ni element, Mn element, Co element, and V element.

5. The positive electrode sheet according to claim 4, characterized in that: The sodium supplement includes Na2NiO2, Na5FeO4, Na4Ni 0.5 Mn 1.5 One or more of O4, Na6CoO4, Na5V2(PO4)3.

6. The positive electrode sheet according to claim 1 or 2, characterized in that: The sodium supplement layer also includes a conductive agent and a binder.

7. The positive electrode sheet according to claim 6, characterized in that: The mass ratio of the sodium supplement, the conductive agent and the binder is (40-91):(5-40):(4-30).

8. A method for preparing a positive electrode sheet, characterized in that: The following steps are involved: mixing a sodium supplement agent and a solvent to obtain a sodium supplement slurry; coating the sodium supplement slurry on the surface of the positive electrode current collector, and obtaining a sodium supplement layer after drying; and forming a positive electrode film layer on the sodium supplement layer; The thickness H1 of the sodium supplement layer and the thickness H2 of the positive electrode film layer satisfy: 0.01≤H1 / H2≤0.

2.

9. The preparation method according to claim 8, characterized in that: The coating method of the sodium supplement slurry includes gravure coating.

10. The preparation method according to claim 8 or 9, characterized in that: The preparation of the sodium supplement slurry comprises mixing the sodium supplement agent, the solvent, the conductive agent and the binder.

11. A sodium ion battery, characterized in that: A positive electrode sheet comprising the positive electrode sheet according to any one of claims 1 to 7 or a positive electrode sheet obtained by the preparation method according to any one of claims 8 to 10.

12. A battery module, characterized in that: Including the sodium ion battery according to claim 11.

13. A battery pack, characterized in that: Includes the sodium ion battery according to claim 11 or the battery module according to claim 12.

14. An electrical device, characterized in that: Includes at least one of the sodium ion battery of claim 11, the battery module of claim 12, and the battery pack of claim 13.

Citation Information

Patent Citations

  • Lithium ion battery positive electrode sheet, preparation method of lithium ion battery positive electrode sheet, and lithium ion battery

    CN106384808A

  • Multilayer positive plate with lithium / sodium supplementing function, battery and preparation method

    CN111834622A

  • Sodium-ion battery positive plate, preparation method thereof and sodium-ion battery

    CN112768699A

  • Positive plate, preparation method and battery

    CN114335428A

  • Positive pole piece and sodium ion battery

    CN115084433A