Method for manufacturing lithium metal negative electrode and battery pack comprising same

During the manufacturing process of the lithium battery pack, a perforated structure and a lithium-philic surface are formed on the metal substrate and a lithium metal layer is applied, the problem of poor bonding of the lithium electrode and the current collector is solved, and the cycle stability of the battery pack is improved. life.

CN118943302APending Publication Date: 2024-11-12GM GLOBAL TECHNOLOGY OPERATIONS LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311393476.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2023-10-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the manufacturing process of existing lithium battery packs, the bond between the lithium metal negative electrode and the current collector is poor, resulting in the lithium ions being easily disengaged from the electrode layer during the cycle, affecting the cycle stability and life of the battery pack.

Method used

A method is adopted to form a layer of photosensitive material on a metal substrate, form a perforated structure by mask etching and pyrolysis, then heat to form a lithium-philic surface in an oxygen-containing environment, and finally apply lithium metal to the carbon layer to achieve the lithium layer chemical combination.

Benefits of technology

The bonding force between the lithium metal negative electrode and the current collector is improved, the cycle stability and life of the battery pack are enhanced, and the separation between the lithium ions and the electrode layer is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943302A_ABST
    Figure CN118943302A_ABST
Patent Text Reader

Abstract

A lithium ion circulating battery includes a negative electrode current collector and a lithium metal layer deposited thereon. The negative electrode current collector has a layered structure including a metal substrate and a carbon layer formed in situ on the metal substrate. The negative electrode current collector includes a plurality of perforations extending therethrough. The lithium metal layer is chemically bonded to the carbon layer of the negative electrode current collector. The negative electrode current collector is manufactured by a method including a photolithography process, a pyrolysis process, and a surface functionalization process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to methods of making lithium metal negative electrodes for cycling lithium ion batteries, and more particularly to methods of making perforated metal current collectors having lithiophilic surfaces for lithium metal negative electrodes. Background Art

[0002] The information provided in this section is intended to generally introduce the background of the present disclosure. To the extent that work currently named as inventors is described in this section, and aspects of the specification that may not have been otherwise identified as prior art at the time of filing, are not admitted, either explicitly or implicitly, as prior art to the present disclosure.

[0003] The present disclosure relates to methods of making lithium metal negative electrodes for cycling lithium ion batteries, and more particularly to methods of making perforated metal current collectors having lithophilic surfaces for lithium metal negative electrodes.

[0004] Lithium batteries are widely used in various portable electronic devices and are promising candidates for meeting the requirements of electric vehicles (including hybrid electric vehicles) due to their high energy and power density. Secondary lithium batteries generally include a negative electrode, a positive electrode, and an electrolyte, which provides a medium for lithium ion conduction between the negative electrode and the positive electrode during the discharge and charge process of the battery. During the manufacturing process, the electrodes are usually deposited in the form of a thin layer on a conductive metal current collector. Summary of the invention

[0005] A method for manufacturing a lithium metal negative electrode for a battery pack for cycling lithium ions, comprising steps (a)-(h). In step (a), a photosensitive material layer is formed on the surface of a metal substrate. In step (b), a mask is positioned above the metal substrate and the photosensitive material layer, the mask including a plurality of holes extending therethrough, so that the photosensitive material layer includes a covered area and a plurality of uncovered areas corresponding to the plurality of holes in the mask. In step (c), the uncovered areas of the photosensitive material layer are exposed to radiation. In step (d), the uncovered areas of the photosensitive material layer are removed from the metal substrate, so that the metal substrate includes a decorative area corresponding to the covered area of ​​the photosensitive material layer and a plurality of exposed areas corresponding to the uncovered areas of the photosensitive material layer. In step (e), the plurality of exposed areas are removed from the metal substrate by etching, so that the photosensitive material layer and the metal substrate include a plurality of perforations extending therethrough. In step (f), the covered areas of the photosensitive material layer remaining on the surface of the metal substrate are pyrolyzed to remove functional groups therefrom and convert the covered areas of the photosensitive material layer into a carbon layer. In step (g), a lithiophilic surface is formed on the carbon layer by heating the metal substrate and the carbon layer in an oxygen-containing environment. In step (h), lithium is applied to the metal substrate over the carbon layer to form a lithium metal negative electrode, wherein the lithium is applied to the metal substrate such that a continuous layer of lithium is chemically bonded to the lithiophilic surface on the carbon layer.

[0006] The photosensitive material layer may include an organic polymer. In this case, the photosensitive material layer may include carbon greater than or equal to about 40% on an atomic basis.

[0007] Exposing the uncovered areas of the layer of photosensitive material to radiation in step (c) may include exposing the uncovered areas of the photosensitive material to visible light, ultraviolet (UV) light, electron beam radiation, X-ray radiation, or a combination thereof.

[0008] Exposing the uncovered areas of the photosensitive material layer to radiation in step (c) can make the uncovered areas soluble in a liquid developer. In this case, the uncovered areas of the photosensitive material layer can be removed from the surface of the metal substrate by washing the metal substrate with a liquid developer in step (d).

[0009] The metal substrate may be made of copper, and the plurality of bare areas may be removed from the metal substrate in step (e) by electrochemical etching.

[0010] Pyrolyzing the covered region of the photosensitive material layer in step (f) may include heating the covered region of the photosensitive material layer in a hydrogen-containing ambient at a temperature greater than or equal to about 800° C. and less than or equal to about 1000° C.

[0011] The carbon layer formed on the surface of the metal substrate in step (f) may contain greater than 95 wt % carbon.

[0012] The metal substrate may have a thickness greater than or equal to about 1 micrometer and less than or equal to about 4 millimeters. The carbon layer may have a thickness greater than or equal to about 10 nanometers and less than or equal to about 100 nanometers.

[0013] Forming the lithiophilic surface on the carbon layer in step (g) may include heating the metal substrate and the carbon layer in an oxygen-containing environment at a temperature greater than or equal to about 200° C. and less than or equal to about 600° C. The lithiophilic surface formed on the carbon layer may include a plurality of oxygen-containing reactive groups covalently bonded to the carbon layer.

[0014] The lithium may be applied to the metal substrate in step (h) by applying a solid lithium metal layer to the metal substrate over the carbon layer or by pouring molten lithium onto the metal substrate over the carbon layer.

[0015] The plurality of perforations may have at least one cross-sectional dimension greater than or equal to about 2 microns and less than or equal to about 1 millimeter.

[0016] Lithium may be applied to the metal substrate in step (h) such that the lithium extends into the plurality of through-holes.

[0017] The lithium metal negative electrode may have a thickness of greater than or equal to about 1 micron to less than or equal to about 30 microns.

[0018] The method may further include, after step (h), assembling the lithium metal negative electrode into a battery.

[0019] A method for manufacturing a lithium metal negative electrode for a battery pack for cycling lithium ions, comprising steps (a)-(h). In step (a), a photosensitive material layer is formed on the surface of a metal substrate. In step (b), a mask is positioned above the metal substrate and the photosensitive material layer, the mask including a plurality of holes extending therethrough, so that the photosensitive material layer includes a covered area and a plurality of uncovered areas corresponding to the plurality of holes in the mask. In step (c), the uncovered areas of the photosensitive material layer are exposed to radiation. In step (d), the uncovered areas of the photosensitive material layer are removed from the metal substrate, so that the metal substrate includes a decorative area corresponding to the covered area of ​​the photosensitive material layer and a plurality of exposed areas corresponding to the uncovered areas of the photosensitive material layer. In step (e), the plurality of exposed areas are removed from the metal substrate by etching, so that the metal substrate includes a plurality of perforations extending therethrough. In step (f), the covered areas of the photosensitive material layer remaining on the surface of the metal substrate are pyrolyzed to remove functional groups therefrom and convert the covered areas of the photosensitive material layer into a carbon layer. In step (g), a lithium-philic surface is formed on the carbon layer by heating the metal substrate and the carbon layer in an oxygen-containing environment, wherein the lithium-philic surface comprises a plurality of -hydroxyl and / or -carboxyl groups covalently bonded to the carbon layer. In step (h), lithium is applied to the metal substrate over the carbon layer to form a lithium metal negative electrode, wherein the lithium is applied to the metal substrate such that a continuous lithium layer is chemically bonded to the lithium-philic surface on the carbon layer via a plurality of hydrogen bonds.

[0020] A battery pack for circulating lithium ions includes a negative electrode current collector and a lithium metal layer deposited on the negative electrode current collector. The negative electrode current collector has a first major surface, an opposite second major surface, and a plurality of perforations extending therethrough. The plurality of perforations are defined by a wall surface extending from the first major surface of the negative electrode current collector to the second major surface. The negative electrode current collector has a layered structure, including a metal substrate and a carbon layer formed in situ on the metal substrate. The carbon layer defines the first major surface of the negative electrode current collector. The lithium metal layer is deposited on the first major surface of the negative electrode current collector. The lithium metal layer is chemically bonded to the carbon layer by a plurality of hydrogen bonds.

[0021] The plurality of perforations may have at least one cross-sectional dimension greater than or equal to about 2 microns and less than or equal to about 1 millimeter.

[0022] The negative electrode current collector may have a thickness greater than or equal to about 1 micrometer and less than or equal to about 4 millimeters.

[0023] The carbon layer may have a thickness greater than or equal to about 10 nanometers and less than or equal to about 100 nanometers.

[0024] The lithium metal layer may extend from the first major surface of the negative electrode current collector to the second major surface into a plurality of perforations in the negative electrode current collector.The lithium metal layer may have a thickness of greater than or equal to about 1 micron to less than or equal to about 30 microns.

[0025] The present invention provides the following solutions:

[0026] Scheme 1. A method for manufacturing a lithium metal negative electrode for a battery pack for cycling lithium ions, the method comprising:

[0027] (a) forming a photosensitive material layer on the surface of a metal substrate;

[0028] (b) positioning a mask over the metal substrate and the photosensitive material layer, the mask including a plurality of holes extending therethrough, such that the photosensitive material layer includes a covered area and a plurality of uncovered areas corresponding to the plurality of holes in the mask;

[0029] (c) exposing the uncovered areas of the layer of photosensitive material to radiation;

[0030] (d) removing the uncovered area of ​​the photosensitive material layer from the metal substrate, so that the metal substrate includes a decorative area corresponding to the covered area of ​​the photosensitive material layer and a plurality of exposed areas corresponding to the uncovered area of ​​the photosensitive material layer;

[0031] (e) removing the plurality of exposed areas from the metal substrate by etching, such that the photosensitive material layer and the metal substrate include a plurality of through-holes extending therethrough;

[0032] (f) pyrolyzing the covered region of the photosensitive material layer remaining on the surface of the metal substrate to remove functional groups therefrom and convert the covered region of the photosensitive material layer into a carbon layer;

[0033] (g) forming a lithium-philic surface on the carbon layer by heating the metal substrate and the carbon layer in an oxygen-containing environment; and

[0034] (h) applying lithium to the metal substrate over the carbon layer to form a lithium metal negative electrode, wherein the lithium is applied to the metal substrate such that a continuous layer of lithium is chemically bonded to a lithiophilic surface on the carbon layer.

[0035] Option 2. A method according to Option 1, wherein the photosensitive material layer comprises an organic polymer, and wherein the photosensitive material layer comprises greater than or equal to about 40% carbon on an atomic basis.

[0036] Option 3. The method according to Option 1, wherein exposing the uncovered area of ​​the photosensitive material layer to radiation in step (c) comprises:

[0037] The uncovered areas of the photosensitive material are exposed to visible light, ultraviolet (UV) light, electron beam radiation, X-ray radiation, or a combination thereof.

[0038] Option 4. A method according to Option 1, wherein in step (c), the uncovered area of ​​the photosensitive material layer is exposed to radiation to make the uncovered area soluble in a liquid developer, and wherein in step (d), the uncovered area of ​​the photosensitive material layer is removed from the surface of the metal substrate by washing the metal substrate with a liquid developer.

[0039] Option 5. A method according to Option 1, wherein the metal substrate is made of copper, and wherein in step (e) the multiple exposed areas are removed from the metal substrate by electrochemical etching.

[0040] Scheme 6. The method according to Scheme 1, wherein in step (f), pyrolyzing the covered area of ​​the photosensitive material layer comprises:

[0041] The covered area of ​​the photosensitive material layer is heated in a hydrogen-containing ambient at a temperature greater than or equal to about 800° C. and less than or equal to about 1000° C.

[0042] Option 7. A method according to Option 1, wherein the carbon layer formed on the surface of the metal substrate in step (f) contains greater than 95 weight % carbon.

[0043] Option 8. A method according to Option 1, wherein the metal substrate has a thickness greater than or equal to about 1 micron and less than or equal to about 4 millimeters, and wherein the carbon layer has a thickness greater than or equal to about 10 nanometers and less than or equal to about 100 nanometers.

[0044] Scheme 9. The method according to Scheme 1, wherein forming a lithium-philic surface on the carbon layer in step (g) comprises:

[0045] heating the metal substrate and the carbon layer at a temperature of greater than or equal to about 200° C. and less than or equal to about 600° C. in an oxygen-containing environment, and

[0046] The lithium-philic surface formed on the carbon layer comprises a plurality of oxygen-containing reactive groups covalently bonded to the carbon layer.

[0047] Option 10. A method according to Option 1, wherein in step (h) lithium is applied to the metal substrate by applying a solid lithium metal layer to the metal substrate above the carbon layer or by pouring molten lithium onto the metal substrate above the carbon layer.

[0048] Option 11. A method according to Option 1, wherein the plurality of perforations have at least one cross-sectional dimension greater than or equal to about 2 microns and less than or equal to about 1 millimeter.

[0049] Embodiment 12. The method according to embodiment 1, wherein in step (h), lithium is applied to the metal substrate such that the lithium extends into the plurality of through-holes.

[0050] Option 13. A method according to Option 1, wherein the lithium metal negative electrode has a thickness of greater than or equal to about 1 micron and less than or equal to about 30 microns.

[0051] Scheme 14. The method according to Scheme 1, further comprising:

[0052] After step (h), the lithium metal negative electrode is assembled into a battery.

[0053] Scheme 15. A method for manufacturing a lithium metal negative electrode for a battery pack for cycling lithium ions, the method comprising:

[0054] (a) forming a photosensitive material layer on the surface of a metal substrate;

[0055] (b) positioning a mask over the metal substrate and the photosensitive material layer, the mask including a plurality of holes extending therethrough, such that the photosensitive material layer includes a covered area and a plurality of uncovered areas corresponding to the plurality of holes in the mask;

[0056] (c) exposing the uncovered areas of the layer of photosensitive material to radiation;

[0057] (d) removing the uncovered area of ​​the photosensitive material layer from the metal substrate, so that the metal substrate includes a decorative area corresponding to the covered area of ​​the photosensitive material layer and a plurality of exposed areas corresponding to the uncovered area of ​​the photosensitive material layer;

[0058] (e) removing the plurality of exposed areas from the metal substrate by etching, such that the metal substrate includes a plurality of through-holes extending therethrough;

[0059] (f) pyrolyzing the covered region of the photosensitive material layer remaining on the surface of the metal substrate to remove functional groups therefrom and convert the covered region of the photosensitive material layer into a carbon layer;

[0060] (g) forming a lithiophilic surface on the carbon layer by heating the metal substrate and the carbon layer in an oxygen-containing environment, the lithiophilic surface comprising a plurality of -hydroxyl and / or -carboxyl groups covalently bonded to the carbon layer; and

[0061] (h) applying lithium to the metal substrate over the carbon layer to form a lithium metal negative electrode, wherein the lithium is applied to the metal substrate such that a continuous layer of lithium is chemically bonded to a lithiophilic surface on the carbon layer through multiple hydrogen bonds.

[0062] Solution 16. A circulating lithium ion battery pack, the battery pack comprising:

[0063] A negative electrode current collector having a first major surface, an opposing second major surface, and a plurality of perforations extending therethrough, the plurality of perforations being defined by wall surfaces extending from the first major surface to the second major surface of the negative electrode current collector, wherein the negative electrode current collector has a layered structure comprising:

[0064] Metal substrates; and

[0065] a carbon layer formed in situ on the metal substrate, the carbon layer defining a first major surface of the negative electrode current collector; and

[0066] a lithium metal layer deposited on a first major surface of the negative electrode current collector,

[0067] The lithium metal layer is chemically bonded to the carbon layer via a plurality of hydrogen bonds.

[0068] Embodiment 17. A battery pack according to Embodiment 16, wherein the plurality of perforations have at least one cross-sectional dimension greater than or equal to about 2 microns and less than or equal to about 1 millimeter.

[0069] Option 18. A battery pack according to Option 16, wherein the negative electrode current collector has a thickness greater than or equal to about 1 micron and less than or equal to about 4 millimeters.

[0070] Embodiment 19. A battery pack according to Embodiment 16, wherein the carbon layer has a thickness greater than or equal to about 10 nanometers and less than or equal to about 100 nanometers.

[0071] Option 20. A battery pack according to Option 16, wherein the lithium metal layer extends from the first major surface of the negative electrode collector to the second major surface into a plurality of perforations in the negative electrode collector, and wherein the lithium metal layer has a thickness of greater than or equal to about 1 micron to less than or equal to about 30 microns.

[0072] Further areas of applicability of the present disclosure will become apparent from the detailed description, claims and drawings.The detailed description and specific examples are intended to be illustrative only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] The present disclosure will be more fully understood through the detailed description and accompanying drawings, in which:

[0074] Figure 1 is a schematic perspective view of a motor vehicle powered by a battery pack including a plurality of battery modules.

[0075] Figure 2 yes Figure 1 Schematic cross-sectional view of a portion of one of the battery modules of FIG. 1 , the battery module comprising a plurality of battery cells in a stacked arrangement.

[0076] Figure 3 is a schematic cross-sectional view of a cycling lithium-ion battery including a lithium metal negative electrode disposed on a perforated current collector.

[0077] Figure 4 yes Figure 3 Schematic front view of a perforated current collector.

[0078] Figure 5 yes Figure 3 Magnified cross-sectional view of a portion of a lithium metal negative electrode and a perforated current collector.

[0079] Figure 6A-6E Schematically depicting the manufacturing Figure 3 The steps in the method of producing a lithium metal negative electrode and a perforated current collector.

[0080] Among the drawings, reference numerals may be repeated to identify similar and / or identical elements. DETAILED DESCRIPTION

[0081] The presently disclosed methods can be used to make lithium metal negative electrodes for cycling lithium ion batteries and can help facilitate the production of relatively large scale batteries.

[0082] Figure 1 A motor vehicle 2 is depicted that is powered by an electric motor 4 that draws power from a battery pack 6 that includes one or more battery modules 8. The battery modules 8 may be electrically coupled together in a series and / or parallel arrangement to meet the capacity and power requirements required by the electric motor 4. The vehicle 2 may be a pure electric vehicle and may be powered solely by the electric motor 4, or the vehicle 2 may be a hybrid electric vehicle and may be powered by both the electric motor 4 and an internal combustion engine (not shown).

[0083] like Figure 2 As shown in , each battery module 8 includes one or more electrochemical cells or batteries 10 that circulate lithium ions. In practice, the batteries 10 in the battery module 8 are typically assembled as stacked layers, including a negative electrode layer 12, a negative electrode current collector 13, a positive electrode layer 14, a positive electrode current collector 15, and a separator layer 16. Each battery 10 is defined by a negative electrode layer 12 and a positive electrode layer 14 separated by a separator layer 16. The negative electrode layer 12 is disposed in a position electrically connected to the negative electrode current collector 13, and the positive electrode layer 14 is disposed in a position electrically connected to the positive electrode current collector 15. As shown in FIG. Figure 2As shown in , these layers can be stacked so that some of the negative electrode collectors 13 and the positive electrode collectors 15 are double-sided and include negative electrode layers 12 or positive electrode layers 14 on both sides thereof. In this arrangement, adjacent negative electrode layers 12 and positive electrode layers 14 share a single negative current collector 13 or positive current collector 15.

[0084] Figure 3 An electrochemical cell or battery 20 of circulating lithium ions is depicted. The battery 20 can generate an electric current during discharge, which can be used to power a load device (e.g., the motor 4), and can be recharged by connecting to a power source. Figure 1 and Figure 2 1 , in various aspects, the battery pack 20 may be used to power the electric motor 4 of the motor vehicle 2. Additionally or alternatively, the battery pack 20 may be used in other transportation applications (e.g., motorcycles, boats, tractors, buses, motorbikes, mobile homes, campers, tanks, and aircraft), and may be used to power fixed and / or portable electronic devices, components, and devices used in a variety of other industries and applications, including, by way of non-limiting example, industrial, residential and commercial construction, consumer products, industrial equipment and machinery, agricultural or farm equipment, and heavy machinery.

[0085] The battery 20 includes a lithium metal negative electrode 22 disposed on a negative electrode current collector 24, a positive electrode 26 disposed on a positive electrode current collector 28, a separator 30, and an electrolyte 32. In practice, the negative electrode current collector 24 and the positive electrode current collector 28 are electrically coupled to a power source or load 34 (e.g., a motor 12) via an external circuit 36. The negative electrode 22 and the positive electrode 26 are configured so that when the battery 20 is at least partially charged, an electrochemical potential difference is established between the negative electrode 22 and the positive electrode 26. During the discharge process of the battery 20, the electrochemical potential established between the negative electrode 22 and the positive electrode 26 drives a spontaneous redox reaction within the battery 20 and releases lithium ions and electrons at the negative electrode 22. The released lithium ions move from the negative electrode 22 to the positive electrode 26 through the separator 30 and the ion-conductive electrolyte 32, and the electrons move from the negative electrode 22 to the positive electrode 26 via the external circuit 36, which generates an electric current. After the negative electrode 22 has been partially or completely depleted of lithium, the battery 20 may be charged by connecting the negative electrode 22 and the positive electrode 26 to a power source 34, which drives a non-spontaneous redox reaction within the battery 20 and releases lithium ions and electrons from the positive electrode 26. Repeated discharge and charge of the battery 20 may be referred to herein as "cycling," where a full discharge event followed by a full charge event is considered a complete cycle.

[0086] Negative electrode current collector 24 is electrically conductive and provides an electrical connection between lithium metal negative electrode 22 and external circuit 36. Referring now to Figure 3 , Figure 4 and Figure 5 , the negative electrode current collector 24 is macroporous and has a first major surface 38, an opposing second major surface 40, and a plurality of perforations 42 extending therethrough. The plurality of perforations 42 are defined by wall surfaces 44 extending from the first major surface 38 to the second major surface 40 of the negative electrode current collector 24. The plurality of perforations 42 can help ensure good bonding between the lithium metal negative electrode 22 and the negative electrode current collector 24, and can help prevent delamination of the lithium metal negative electrode 22 from the negative electrode current collector 24 during cycling of the battery 20.

[0087] like Figure 4 As shown in , the plurality of perforations 42 may be substantially evenly spaced apart from one another within the negative electrode current collector 24 and may present substantially the same cross-sectional shape. Figure 4 In the embodiment, each of the plurality of perforations 42 has a circular cross-sectional shape. In other embodiments, the cross-sectional shape of the plurality of perforations 42 may be an ellipse or a polygon, such as a triangle, a square, a rectangle, a hexagon, a quadrilateral, an octagon or a combination thereof. Each of the plurality of perforations 42 may have at least one cross-sectional dimension greater than or equal to about 2 microns and less than or equal to about 1 mm. For example, each of the plurality of perforations 42 may have a circular cross-sectional shape and a diameter greater than or equal to about 2 microns and less than or equal to about 1 mm. The plurality of perforations 42 may provide a porosity or void volume fraction greater than or equal to about 0.5 to less than or equal to about 0.99 for the negative electrode current collector 24. The negative electrode current collector 24 may have a length 46 extending from its first end to the opposite second end and a width 48 extending from its first side to the opposite second side. The length 46 and width 48 of the negative electrode current collector 24 may be the same or different. The length 46 and width 48 of the negative electrode current collector 24 may each be greater than or equal to about 6 centimeters, about 10 centimeters, or about 15 centimeters and less than or equal to about 60 centimeters, about 50 centimeters, or about 30 centimeters.

[0088] like Figure 5 As shown in , the negative electrode current collector 24 has a layered structure and includes a metal substrate 50 and an overlying carbon layer 52. The first major surface 38 of the negative electrode current collector 24 is defined by the carbon layer 52, and the second major surface 40 of the negative electrode current collector 24 is defined by the metal substrate 50. A plurality of perforations 42 extend completely through the metal substrate 50 and the carbon layer 52, such that the wall surface 44 is defined by both the metal substrate 50 and the carbon layer 52. The carbon layer 52 can help ensure good bonding between the lithium metal negative electrode 22 and the negative electrode current collector 24.

[0089] The metal substrate 50 is made of an electrochemically inert metal. For example, the metal substrate 50 can be made of copper or a copper-based material. The carbon layer 52 contains carbon and can be essentially composed of carbon or composed of carbon. For example, the carbon layer 52 may contain greater than 95% by weight, greater than 97% by weight, or greater than 99% by weight of carbon. The negative electrode current collector 24 may have a thickness greater than or equal to about 1 micron, about 5 microns, or about 10 microns and less than or equal to about 4 millimeters, about 60 microns, or about 30 microns defined between its first major surface 38 and the second major surface 40. The carbon layer 52 may have a thickness greater than or equal to about 10 nanometers and less than or equal to about 100 nanometers.

[0090] The lithium metal negative electrode 22 is electrochemically active and is disposed on the first major surface 38 of the negative electrode current collector 24. The lithium metal negative electrode 22 contains lithium (Li) and may be substantially composed of lithium or composed of lithium. For example, the lithium metal negative electrode 22 may contain greater than 97% by weight of lithium, or optionally greater than 99% by weight of lithium. The lithium metal negative electrode 22 may be substantially free of elements or compounds that undergo a reversible redox reaction with lithium during operation of the battery 20. For example, the lithium metal negative electrode 22 may be substantially free of an intercalation host material that is configured to reversibly insert or embed lithium ions or an alloy material that can be electrochemically alloyed with lithium and form a compound phase. In addition, the lithium metal negative electrode 22 may be substantially free of a conversion material or alloy material that can be electrochemically alloyed with lithium and form a compound phase. Some examples of materials that may be intentionally excluded from the lithium metal negative electrode 22 include carbon-based materials (e.g., graphite, activated carbon, carbon black, and graphene), silicon and silicon-based materials, tin oxide, aluminum, indium, zinc, cadmium, lead, germanium, tin, antimony, titanium oxide, lithium titanium oxide, lithium titanate, lithium oxide, metal oxides (e.g., iron oxide, cobalt oxide, manganese oxide, copper oxide, nickel oxide, chromium oxide, ruthenium oxide, and / or molybdenum oxide), metal phosphides, metal sulfides, and metal nitrides (e.g., phosphides, sulfides, and / or nitrides of iron, manganese, nickel, copper, and / or cobalt). The lithium metal negative electrode 22 may be substantially free of a polymer binder. Some examples of polymer binders that may be intentionally excluded from the lithium metal negative electrode 22 include polyvinylidene fluoride (PVdF), ethylene propylene diene rubber (EPDM), styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), and polyacrylic acid.

[0091] like Figure 3 and Figure 5As shown in , the lithium metal negative electrode 22 is disposed on the first major surface 38 of the negative electrode current collector 24 and can extend at least partially into the plurality of perforations 42. For example, the lithium metal negative electrode 22 can extend into the plurality of perforations 42 and extend completely through the negative electrode current collector 24 from its first major surface 38 to the second major surface 40. Depending on the state of charge of the battery 20, the lithium metal negative electrode 22 can have a thickness greater than 0 microns and less than or equal to 100 microns. The lithium metal negative electrode 22 is chemically bonded to the carbon layer 52 on the first major surface 38 of the negative electrode current collector 24 via a plurality of hydrogen bonds.

[0092] The positive electrode 26 is configured to store and release lithium ions during the discharge and charge process of the battery pack 20, and includes an electrochemically active (electroactive) material that can undergo a reversible redox reaction with lithium, such as a material that can fully perform lithium insertion and deinsertion, alloying and dealloying, or plating and stripping. In one form, the electroactive material of the positive electrode 26 may include an intercalation host material that can reversibly insert or insert lithium ions. In this case, the electroactive material of the positive electrode 26 may include a lithium transition metal oxide. For example, the electroactive material of the positive electrode 26 may include a layered oxide represented by the formula LiMeO2, an olivine-type oxide represented by the formula LiMePO4, a spinel-type oxide represented by the formula LiMe2O4, a tavorite represented by one or both of the following formulas LiMeSO4F or LiMePO4F, where Me is a transition metal (e.g., Co, Ni, Mn, Fe, Al, V, or a combination thereof), or a combination thereof. In some embodiments, the electroactive material of the positive electrode 26 may include a lithium transition metal oxide selected from lithium cobalt oxide (LCO), lithium manganese oxide (LMO), lithium nickel manganese cobalt oxide (NMC), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese aluminum oxide (NCMA) and lithium manganese iron phosphate (LMFP). In another form, the electroactive material of the positive electrode 26 may include a conversion material, which includes a component that can undergo a reversible electrochemical reaction with lithium, wherein the component undergoes a phase change or a change in crystal structure accompanied by a change in oxidation state. In this case, the electroactive material of the positive electrode 26 may include sulfur, selenium, tellurium, iodine, a halide (e.g., fluoride or chloride), a sulfide, a selenide, a telluride, an iodide, a phosphide, a nitride, an oxide, an oxysulfide, an oxyfluoride, a sulfur fluoride, a sulfur oxyfluoride, or lithium and / or a metal compound thereof. Examples of suitable metals included in the conversion material of the electroactive material of the positive electrode 26 include iron, manganese, nickel, copper and cobalt.

[0093] The electroactive material of the positive electrode 26 can be mixed with a conductive agent and a binder. The conductive agent is formulated to provide good electron penetration to the positive electrode 26 and can include a carbon-based material. For example, the conductive agent may include particles of high surface area carbon black, acetylene black or graphite, carbon fibers (e.g., carbon nanofibers), carbon nanohorns, carbon nanotubes (e.g., single-walled or multi-walled carbon nanotubes), onion-like carbon, graphene (e.g., graphene nanosheets), graphene oxide, or a combination thereof. The binder is configured to have good adhesion and bonding to the positive electrode 26, and can include an organic polymer. Examples of organic polymers include polyvinylidene fluoride (PVDF), ethylene propylene diene monomer (EPDM), styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), and / or polyacrylic acid (PAA).

[0094] The positive electrode current collector 28 is conductive and provides an electrical connection between the positive electrode 24 and the external circuit 38. The positive electrode current collector 28 is made of an electrochemically inert conductive material such as a metal. For example, the positive electrode current collector 28 can be made of copper, copper-based materials, aluminum, aluminum-based materials, nickel, nickel-based materials, iron-based materials (such as stainless steel), titanium-based materials, tin-based materials, or combinations thereof. In various aspects, the positive electrode current collector 28 can be made of aluminum or an aluminum-based material.

[0095] The separator 30 physically and electrically isolates the positive electrode 26 and the negative electrode 22 from each other while allowing lithium ions to pass therethrough. The separator 30 has an open microporous structure and may include organic and / or inorganic materials. For example, the separator 30 may include a polymer or a combination of polymers. For example, the separator 30 may include one or more polyolefins, such as polyethylene (PE), polypropylene (PP), polyamide (PA), poly(tetrafluoroethylene) (PTFE), polyvinylidene fluoride (PVdF) and / or poly(vinyl chloride) (PVC). In one form, the separator 30 may include a polymer laminate, such as a laminate of PE and PP. In various aspects, the separator 30 may include a ceramic coating (not shown) disposed on one or both sides thereof. In this case, the ceramic coating may include particles of aluminum oxide (Al2O3) and / or silicon dioxide (SiO2).

[0096] The electrolyte 32 is ionically conductive and provides a medium for lithium ion conduction between the positive electrode 26 and the negative electrode 22. In assembly, the battery pack 20 is saturated with the electrolyte 32, and the positive electrode 26, the separator 30 and the negative electrode 22 are in direct physical contact with the electrolyte 32. The electrolyte 32 can be in the form of a non-aqueous liquid electrolyte, a gel electrolyte or a solid electrolyte. When the electrolyte 32 is in liquid form, the electrolyte 32 can include a non-aqueous liquid electrolyte solution that includes a lithium salt dissolved or ionized in a non-aqueous aprotic organic solvent or a mixture of non-aqueous aprotic organic solvents. Examples of lithium salts include LiClO4, LiAlCl4, LiI, LiBr, LiSCN, LiBF4, LiB(C6H5)4, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, Li2CO3, LiPF6, and combinations thereof. Examples of non-aqueous aprotic organic solvents include cyclic carbonates (i.e., ethylene carbonate, propylene carbonate), acyclic carbonates (i.e., dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate), aliphatic carboxylates (i.e., methyl formate, methyl acetate, methyl propionate), γ-lactones (i.e., γ-butyrolactone, γ-valerolactone), acyclic ethers (i.e., 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane) and / or cyclic ethers (i.e., tetrahydrofuran, 2-methyltetrahydrofuran). Electrolyte 32 may optionally include one or more additives, such as one or more of lithium difluoro(oxalato)borate (LiDFOB), lithium bis(oxalato)borate (LiBOB), fluoroethylene carbonate (FEC), and vinylene carbonate (VC).

[0097] Reference now Figure 6A-6E , the negative electrode current collector 32 is manufactured by a method including a photolithography process, a pyrolysis process, and a surface functionalization process. Thereafter, an overlying lithium metal negative electrode 22 is formed on the negative electrode current collector 32. The method of manufacturing the negative electrode current collector 32 and the lithium metal negative electrode 22 may include one or more of the following steps. Fig. 6A As shown in , in a first step, a metal substrate 150 having a major surface 154 is provided, and a photosensitive material layer 156 is deposited on the major surface 154 of the metal substrate 150. The metal substrate 150 may have substantially the same composition as the metal substrate 50. In addition, the length and width of the metal substrate 150 may have substantially the same length and width as the negative electrode current collector 24.

[0098] The photosensitive material layer 156 includes a photosensitive material, which may include an organic polymer. The organic polymer may include carbon (C) greater than or equal to about 40%, optionally about 45%, or optionally about 50% based on atoms. In various aspects, the photosensitive material may include a mixture of quinone azide (e.g., naphthoquinone diazo (DNQ)) and phenol formaldehyde resin (also known as novolac resin). The photosensitive material layer 156 may be deposited on the main surface 154 of the metal substrate 150 by applying a thin film (not shown) of a precursor solution to the main surface 154 of the metal substrate 150. The precursor solution may include a mixture of a photosensitive material and a solvent. The photosensitive material may constitute greater than or equal to 1% by weight and less than or equal to 15% by weight of the precursor solution. Thereafter, the solvent may be removed from the precursor solution, for example, by drying, to form the photosensitive material layer 156. The photosensitive material layer 156 may extend substantially continuously above the main surface 154 of the metal substrate 150, and may have a thickness greater than or equal to about 15 nanometers and less than or equal to about 150 nanometers.

[0099] In a second step, a mask 158 is disposed over the metal substrate 150 and the photosensitive material layer 156. The mask 158 includes a plurality of holes 160 extending therethrough. As such, when the mask 158 is positioned over the photosensitive material layer 156, the photosensitive material layer 156 has covered areas 162 covered by the mask 158 and a plurality of uncovered areas 164 corresponding to the plurality of holes 160 in the mask 158.

[0100] In a third step, radiation 166 is directed to the photosensitive material layer 156 such that uncovered areas 164 of the photosensitive material layer 156 are exposed to the radiation 166, while covered areas 162 are not exposed to the radiation 166 due to the placement of the mask 158. The uncovered areas 164 of the photosensitive material layer 156 may be exposed to the radiation 166, for example, by exposing the uncovered areas 164 of the photosensitive material layer 156 to visible light, ultraviolet (UV) light, electron beam radiation, X-ray radiation, or a combination thereof. In various aspects, the radiation 166 may include UV light.

[0101] like Figure 6BAs shown in , in the fourth step, the mask 158 is removed from the photosensitive material layer 156, and the uncovered areas 164 of the photosensitive material layer 156 exposed to the radiation 166 are removed from the metal substrate 150. After the uncovered areas 164 of the photosensitive material layer 156 are removed, the metal substrate 150 has a decorative area 168 corresponding to the covered areas 162 of the photosensitive material layer 156 and a plurality of exposed areas 170 corresponding to the uncovered areas 164 of the photosensitive material layer 156. The photosensitive material of the photosensitive material layer 156 can be a positive photoresist. In this case, exposing the uncovered areas 164 of the photosensitive material layer 156 to the radiation 166 can decompose, degrade and / or make the uncovered areas 164 of the photosensitive material layer 156 soluble in a liquid developer, while the covered areas 162 of the photosensitive material layer 156 can remain insoluble in the liquid developer. In this case, the uncovered areas 164 of the photosensitive material layer 156 may be removed from the metal substrate 150 by washing the metal substrate 150 with a liquid developer. The liquid developer may include a polar solvent, such as water.

[0102] like Figure 6C As shown in , in the fifth step, multiple bare areas 170 are removed from the metal substrate 150 by etching, so that the metal substrate 150 and the photosensitive material layer 156 have multiple through-holes 142 extending therethrough. Multiple bare areas 170 can be removed from the metal substrate 150 using electrochemical etching techniques. In this case, the metal substrate 150 including the covered area 162 of the photosensitive material layer 156 is immersed in an electrolyte solution and electrically coupled to the positive electrode of a current source. At the same time, a metal object made of the same metal as the metal substrate 150 is immersed in the electrolyte solution. When the current source is turned on, the metal object will act as a cathode and the metal substrate 150 will act as an anode, and the metal located in the multiple bare areas 170 of the metal substrate 150 will be dissolved, thereby generating multiple through-holes 142. Alternatively, multiple bare areas 170 can be removed from the metal substrate 150 by applying an etchant solution to the metal substrate 150. Examples of etchant solutions include aqueous solutions of ammonium hydroxide, nitric acid, ferric chloride (FeCl3), and combinations thereof.

[0103] In the sixth step, the covered area 162 of the photosensitive material layer 156 remaining on the major surface 154 of the metal substrate 150 is pyrolyzed by heating the photosensitive material layer 156 and the metal substrate 150 in a controlled environment 172. In various aspects, the controlled environment 172 can be a hydrogen-containing environment. For example, the controlled environment 172 can include a mixture of an inert carrier gas (e.g., argon) and hydrogen. The hydrogen gas can constitute greater than or equal to about 1 volume % to less than or equal to about 10 volume % of the gas in the controlled environment 172. During the pyrolysis step, the photosensitive material layer 156 and the metal substrate 150 can be heated in the controlled environment 172 at a temperature greater than or equal to about 800° C. (degrees Celsius) and less than or equal to about 1000° C. for greater than or equal to about 1 hour, or optionally about 6 hours and less than or equal to about 24 hours, or optionally about 18 hours. In various aspects, the photosensitive material layer 156 and the metal substrate 150 can be heated in the controlled environment 172 at a temperature of about 900° C. for about 12 hours. During the pyrolysis step, functional groups are removed from the photosensitive material layer 156 and the covered area 162 of the photosensitive material layer 156 is converted into a carbon layer 152 ( Fig.6D ). In other words, the carbon layer 152 is formed in-situ on the major surface 154 of the metal substrate 150. The carbon layer 152 may have substantially the same composition and thickness as the carbon layer 52. In addition, the plurality of through-holes 142 extending through the metal substrate 150 and the carbon layer 152 may have substantially the same physical properties as the plurality of through-holes 42.

[0104] like Fig.6D As shown in , in the seventh step, the metal substrate 150 and the carbon layer 152 are heated in an oxygen-containing environment 174 to form a lithium-philic surface on the metal substrate 150 and the carbon layer 152. The oxygen-containing environment 174 may contain greater than or equal to about 10 volume %, or optionally about 20 volume % of oxygen. In various aspects, the oxygen-containing environment 174 may include air. During the formation of the lithium-philic surface, the metal substrate 150 and the carbon layer 152 may be heated in the oxygen-containing environment 174 at a temperature greater than or equal to about 200° C. and less than or equal to about 600° C. for greater than or equal to about 0.5 hour and less than or equal to about 2 hours. In various aspects, the metal substrate 150 and the carbon layer 152 may be heated in the oxygen-containing environment 174 at a temperature of about 450° C. The lithium-philic surface formed on the metal substrate 150 and the carbon layer 152 may include a plurality of lithium-philic portions 176 ( Fig. 6E ). The lithium-philic portion 176 may include an oxygen-containing reactive group covalently bonded to the surface of the carbon layer 152. Examples of the oxygen-containing reactive group include -hydroxyl (-OH) and / or -carboxyl (-COOH).

[0105] In an eighth step (not shown), lithium is applied to the metal substrate 150 over the carbon layer 152 to form the lithium metal negative electrode 22. After the lithium is applied to the metal substrate 150 over the carbon layer 152, the metal substrate 150 and the carbon layer 152 together define the negative electrode current collector 32. The lithium is applied to the metal substrate 150 so that a continuous lithium layer is disposed over the metal substrate 150 and the carbon layer 152, the continuous lithium layer being chemically bonded to the carbon layer 152 (and optionally the metal substrate 150) through a plurality of hydrogen bonds. When the lithium is applied to the metal substrate 150 from above the carbon layer 152, the lithium may be in a solid phase, a liquid phase, and / or a gas phase. For example, the lithium may be applied to the metal substrate 150 from above the carbon layer 152 by applying a solid lithium metal layer to the metal substrate 150, by pouring molten lithium onto the metal substrate 150 from above the carbon layer 152, or by chemical vapor deposition.

[0106] In the ninth step, the lithium metal negative electrode 22 and the negative electrode current collector 32 may be combined with the positive electrode 26, the positive electrode current collector 28, the separator 30 and the electrolyte 32 and assembled into the form of the battery 20. In this case, the chemical bond between the lithium formed in the lithium metal negative electrode 22 and the carbon layer 152 of the negative electrode current collector 32 may help prevent the lithium metal negative electrode 22 from being delaminated from the negative electrode current collector 32 during the cycle of the battery 20.

[0107] The above description is essentially only exemplary and is absolutely not intended to limit the present disclosure, its application or use. The broad teachings of the present disclosure can be implemented in various forms. Therefore, although the present disclosure includes specific examples, the true scope of the present disclosure should not be limited thereto, because after studying the drawings, the specification and the appended claims, other modifications will become apparent. It should be understood that one or more steps in the method may be implemented in different orders (or simultaneously) without changing the principles of the present disclosure. In addition, although each embodiment is described above as having certain features, any one or more features described in any embodiment of the present disclosure can be implemented in any other embodiment and / or combined with the features of any other embodiment, even if the combination is not explicitly described. In other words, the embodiments are not mutually exclusive, and the mutual replacement of one or more embodiments is still within the scope of the present disclosure.

[0108] The terms used herein are only for the purpose of describing specific exemplary embodiments, and are not intended to be limiting. Unless the context clearly indicates otherwise, as used herein, the singular forms "a", "an" and "the" may be intended to also include plural forms. The terms "comprise", "include", "cover" and "have" are compatible, and therefore specify the presence of the features, elements, compositions, steps, integers, operations and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or their groups. Although the open term "comprising" should be understood as a non-limiting term for describing and claiming the various embodiments described herein, in some aspects, the term may be understood as alternatively being a more restrictive and limited term, such as "consisting of..." or "consisting essentially of..." Thus, for any given embodiment of a narration composition, material, assembly, element, feature, integer, operation and / or method step, the present disclosure also specifically includes an embodiment consisting of or essentially consisting of such narrated compositions, materials, assemblies, elements, features, integers, operations and / or method steps. In the case of “consisting of,” alternative embodiments exclude any additional compositions, materials, components, elements, features, integers, operations, and / or method steps, while in the case of “consisting essentially of,” any additional compositions, materials, components, elements, features, integers, operations, and / or method steps that materially affect the basic and novel characteristics are excluded from such embodiments, but any compositions, materials, components, elements, features, integers, operations, and / or method steps that do not materially affect the basic and novel characteristics may be included in the embodiments.

[0109] Any method steps, processes, and operations described herein are not to be construed as necessarily requiring their performance in the particular order discussed or illustrated, unless expressly identified as an order of performance. It is also to be understood that additional or alternative steps may be employed unless otherwise stated.

[0110] When a component, element, or layer is referred to as being "on," "engaged," "connected," or "coupled" to another element or layer, it may be directly on, engaged, connected, or coupled to another component, element, or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on," "directly engaged," "directly connected," or "directly coupled" to another element or layer, there may be no intervening elements or layers. Other words used to describe the relationship between elements should be interpreted in a similar manner (e.g., "between" versus "directly between," "adjacent" versus "directly adjacent," etc.). As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.

[0111] Although the terms first, second, third, etc. can be used to describe various steps, elements, components, regions, layers and / or sections in this article, unless otherwise specified, these steps, elements, components, regions, layers and / or sections should not be limited by these terms. These terms can only be used to distinguish a step, element, component, region, layer or section from another step, element, component, region, layer or section. Unless the context clearly indicates, terms such as "first", "second" and other numerical terms do not imply order or sequence when used in this article. Therefore, the first step, element, component, region, layer or section discussed below can be referred to as the second step, element, component, region, layer or section without departing from the teaching of exemplary embodiments.

[0112] For ease of description, spatial or temporal relative terms may be used herein, such as "before", "after", "inside", "outside", "below", "beneath", "lower", "above", "upper", etc. to describe the relationship of one element or feature to other (one or more) elements or (one or more) features as shown in the drawings. Spatially or temporally relative terms may be intended to encompass different orientations of a device or system in use or operation in addition to the orientation shown in the drawings.

[0113] Throughout this disclosure, numerical values ​​represent approximate measurements or range limits to cover slight deviations from given values ​​and embodiments having approximately the values ​​mentioned and embodiments having exactly the values ​​mentioned. Except in the working examples provided at the end of the detailed description, all numerical values ​​of (e.g., amounts or conditions) parameters in this specification (including the appended claims) should be understood to be modified by the term "about" in all cases, regardless of whether "about" actually appears before the numerical value. "About" means that the numerical value allows a certain slight imprecision (close to the exact value of the value to a certain extent; approximately or reasonably approximate the value; almost). If the imprecision provided by "about" is not otherwise understood in this ordinary sense in the art, then "about" as used herein refers to at least the deviation that can be caused by the common methods of measuring and using such parameters. For example, "about" may include less than or equal to 5%, optionally less than or equal to 4%, optionally less than or equal to 3%, optionally less than or equal to 2%, optionally less than or equal to 1%, optionally less than or equal to 0.5%, and in some aspects optionally less than or equal to 0.1% deviation. Furthermore, the disclosure of a range includes disclosure of all values ​​within the entire range and further subdivided ranges, including disclosure of endpoints and subranges given for that range.

[0114] As used herein, the terms "composition" and "material" are used interchangeably and refer generally to a substance that contains at least a preferred chemical constituent, element, or compound, but which may also contain additional elements, compounds, or substances, including trace impurities, unless otherwise specified. A composition or material "based on X" refers generally to a composition or material in which "X" is the single largest component of the composition or material in terms of weight percent (%). This can include compositions or materials having greater than 50 wt % X, as well as compositions or materials having less than 50 wt % X, as long as X is the single largest component of the composition or material based on its overall weight. When a composition or material is referred to as being "substantially free" of a substance, the composition or material may contain less than 5 wt %, optionally less than 3 wt %, optionally less than 1 wt %, or optionally less than 0.1 wt % of that substance.

[0115] As used herein, the term "metal" may refer to a pure elemental metal or an alloy of an elemental metal with one or more other metals or nonmetallic elements, referred to as "alloying elements." The alloying elements may be selected to impart certain desirable properties to the alloy that are not exhibited by its base metal element.

Claims

1. A method for manufacturing a lithium metal negative electrode for a battery pack for cycling lithium ions, the method include: (a) forming a photosensitive material layer on the surface of a metal substrate; (b) positioning a mask over the metal substrate and the photosensitive material layer, the mask including a plurality of holes extending therethrough, such that the photosensitive material layer includes a covered area and a plurality of uncovered areas corresponding to the plurality of holes in the mask; (c) exposing the uncovered areas of the layer of photosensitive material to radiation; (d) removing the uncovered area of ​​the photosensitive material layer from the metal substrate, so that the metal substrate includes a decorative area corresponding to the covered area of ​​the photosensitive material layer and a plurality of exposed areas corresponding to the uncovered area of ​​the photosensitive material layer; (e) removing the plurality of exposed areas from the metal substrate by etching, such that the photosensitive material layer and the metal substrate include a plurality of through-holes extending therethrough; (f) pyrolyzing the covered area of ​​the photosensitive material layer remaining on the surface of the metal substrate to remove functional groups therefrom and convert the covered area of ​​the photosensitive material layer into a carbon layer containing greater than 95 weight percent carbon; (g) forming a lithiophilic surface on the carbon layer by heating the metal substrate and the carbon layer in an oxygen-containing environment, the lithiophilic surface comprising a plurality of oxygen-containing reactive groups covalently bonded to the carbon layer; and (h) applying lithium to the metal substrate over the carbon layer to form a lithium metal negative electrode, wherein the lithium is applied to the metal substrate such that a continuous layer of lithium is chemically bonded to a lithiophilic surface on the carbon layer through multiple hydrogen bonds.

2. The method of claim 1, wherein the photosensitive material layer comprises an organic polymer, and wherein the photosensitive material layer comprises greater than or equal to about 40% carbon on an atomic basis.

3. The method according to claim 1, wherein in step (c) the uncovered areas of the photosensitive material layer are exposed to radiation. include: The uncovered areas of the photosensitive material are exposed to visible light, ultraviolet (UV) light, electron beam radiation, X-ray radiation, or a combination thereof.

4. The method of claim 1 , wherein in step (c) the uncovered areas of the photosensitive material layer are exposed to radiation to render the uncovered areas soluble in a liquid developer, and wherein in step (d) the uncovered areas of the photosensitive material layer are removed from the surface of the metal substrate by washing the metal substrate with a liquid developer.

5. The method of claim 1, wherein the metal substrate is made of copper, and wherein the plurality of bare areas are removed from the metal substrate in step (e) by electrochemical etching.

6. The method according to claim 1, wherein in step (f) the covered area of ​​the photosensitive material layer is pyrolyzed include: The covered area of ​​the photosensitive material layer is heated in a hydrogen-containing ambient at a temperature greater than or equal to about 800° C. and less than or equal to about 1000° C.

7. The method of claim 1 , wherein the metal substrate has a thickness greater than or equal to about 1 micron and less than or equal to about 4 millimeters, and wherein the carbon layer has a thickness greater than or equal to about 10 nanometers and less than or equal to about 100 nanometers, and wherein the plurality of perforations have at least one cross-sectional dimension greater than or equal to about 2 microns and less than or equal to about 1 millimeter.

8. The method according to claim 1, wherein in step (g) a lithium-philic surface is formed on the carbon layer. include: heating the metal substrate and the carbon layer at a temperature of greater than or equal to about 200° C. and less than or equal to about 600° C. in an oxygen-containing environment, and The lithium-philic surface formed on the carbon layer comprises a plurality of -hydroxyl groups and / or -carboxyl groups covalently bonded to the carbon layer.

9. The method of claim 1 , wherein in step (h) lithium is applied to the metal substrate by applying a solid lithium metal layer to the metal substrate over the carbon layer or by pouring molten lithium onto the metal substrate over the carbon layer, and wherein in step (h) lithium is applied to the metal substrate such that lithium extends into the plurality of perforations.

10. The method of claim 1, wherein the lithium metal negative electrode has a thickness of greater than or equal to about 1 micron to less than or equal to about 30 microns.