Metal-doped silicon-carbon composite material and preparation method thereof

By depositing rare earth metals and metal lithium in porous carbon and combining amorphous carbon cladding, the conductivity and interface impedance problems of new silicon carbon materials are solved, and the power performance and cycling performance of silicon carbon composite materials are significantly improved, achieving More efficient battery performance.

CN118943343APending Publication Date: 2024-11-12GUIZHOU HUIYANG TECH INNOVATION RES CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411301508.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing new silicon carbon materials have poor electronic conductivity and interface impedance, resulting in poor power performance, limited improvement range of non-metallic dopants and increased material defects.

Method used

Using metal-doped silicon-carbon composite materials, by depositing rare earth metal and metal lithium in porous carbon, combining amorphous carbon cladding, electron conductivity and specific capacity are improved, and passivation treatment is carried out through acetylene/oxygen mixed gas to form Stable silica and amorphous carbon coating improve interfacial impedance.

Benefits of technology

It significantly improves the power performance, first-time efficiency and cycling performance of silicon-carbon composite materials, reduces material defects and expansion, and improves the storage performance and cycling stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943343A_ABST
    Figure CN118943343A_ABST
Patent Text Reader

Abstract

The invention discloses a metal-doped silicon-carbon composite material and a preparation method thereof, the composite material has a core-shell structure, the core is a metal lithium and rare earth metal-doped silicon-carbon material, and the shell is amorphous carbon. The preparation method comprises the following steps: mixing rare earth metal steam with heteroatoms under the vacuum degree of less than or equal to 0.1 Torr, introducing the mixture into large-aperture porous carbon, introducing lithium steam, carrying out nanometer silicon deposition through silane gas cracking, and finally carrying out amorphous carbon coating. According to the invention, the power performance, the first efficiency and the cycle performance of silicon carbon can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery materials, and specifically relates to a metal-doped silicon-carbon composite material, and also relates to a preparation method of the metal-doped silicon-carbon composite material. Background Art

[0002] The new silicon-carbon material is composed of a core of porous carbon and nano-silicon deposited in the pores, and amorphous carbon coated on its surface. The porous carbon has a poor electronic conductivity due to its own porous structure, and the contact between nano-silicon and the porous carbon core and between porous carbon and amorphous carbon is poor, resulting in a large interface impedance, which reduces power performance. At present, the measures to improve the power performance of new silicon-carbon materials mainly include doping with metal or non-metal compounds to improve the electronic conductivity of the material and improve the interface impedance between materials, thereby improving the electronic conductivity of the material; or coating the surface with compounds with high ion conductivity to improve the ion conductivity of the material. For example, patent application number CN202310340377.0 discloses a preparation method of a low-expansion silicon-carbon negative electrode material and its silicon-carbon negative electrode material and application. The preparation method is: the carbon source and the non-metallic activator are mixed evenly and sintered to obtain modified porous carbon; then the silane cracking method is used to add polysilane solution to the modified porous carbon by liquid spraying, carbonizing, and obtaining a silicon-carbon composite material. Although the electronic conductivity of the material can be reduced by non-metallic dopants, the improvement of the interface impedance between the materials is not large, and the doping of non-metallic materials causes the defects of the material to increase, thereby reducing the initial efficiency. Summary of the invention

[0003] The purpose of the present invention is to overcome the above-mentioned disadvantages and provide a metal-doped silicon-carbon composite material that can improve the power performance, initial efficiency and cycle performance of silicon-carbon.

[0004] Another object of the present invention is to provide a method for preparing the metal-doped silicon-carbon composite material.

[0005] The present invention discloses a metal-doped silicon-carbon composite material, the composite material presents a core-shell structure, the core is metal lithium and its rare earth metal doped silicon-carbon material, the shell is amorphous carbon, and the mass ratio of the shell is 5-10% calculated based on the mass ratio of the composite material being 100%.

[0006] A method for preparing a metal-doped silicon-carbon composite material of the present invention comprises the following steps: Step S1: adding a rare earth metal compound to a vacuum furnace, evacuating to a vacuum degree of ≤0.1 Torr, heating to 1500-2000° C., heating the rare earth metal compound to generate rare earth metal compound vapor, and mixing it with a heteroatom gas (volume ratio, rare earth metal compound: heteroatom gas = 10:1-5), and passing it into a large-pore porous carbon at a flow rate of 100-500 SCCM for 60-600 minutes to obtain a metal-doped porous carbon; Step S2: According to the mass ratio of metal-doped porous carbon: metallic lithium: silane gas = 100: 5-15: 100-200, the metal-doped porous carbon is transferred to a vacuum furnace, and metallic lithium is spread on the bottom, and then heated to 1400-1600°C to generate lithium vapor deposited in the metal-doped porous carbon, cooled to 450-650°C, silane gas is introduced at a flow rate of 100-500SCCM for 30-300min, cooled to 200-300°C, acetylene / oxygen mixed gas (volume ratio, acetylene: oxygen = 10: 1-5) is introduced, and amorphous carbon is coated at a flow rate of 50-200SCCM for 30-300min to obtain a metal-doped silicon-carbon composite material.

[0007] The above-mentioned method for preparing a metal-doped silicon-carbon composite material, wherein the rare earth metal compound described in step S1 is one of cerium chloride, scandium chloride, lanthanum chloride or yttrium chloride; the heteroatom compound is one of trimethylborane, thiourea, N-methylthiourea, thiol, thiophenol, pyridine, acrylonitrile or dicyandiamide gasification.

[0008] In the above-mentioned method for preparing a metal-doped silicon-carbon composite material, the silane gas in step S1 is one of the gases generated by heating trisilane, butadisilane, trichlorosilane, methyltrichlorosilane or dimethyldichlorosilane to 200-300°C.

[0009] Compared with the prior art, the present invention has obvious beneficial effects. It can be seen from the above technical scheme that the present invention prepares metal-doped porous carbon by depositing rare earth compounds and heteroatom gases in porous carbon by gasification, and improves the power performance of the material based on the high electronic conductivity of metal rare earth compounds and non-metallic heteroatoms. By sublimation, metallic lithium is sublimated into gas and deposited on metal-doped porous carbon to improve the electronic conductivity of the material, and nano-silicon is continuously deposited to improve the specific capacity of the composite material by relying on the high specific capacity of the nano-silicon itself. By passing acetylene / oxygen mixed gas, the metal-doped silicon-carbon precursor is passivated, and silicon dioxide and its amorphous carbon coating layer are generated on its surface. The coating layer is inert to the electrolyte, thereby improving the initial efficiency and its storage performance, and the coating layer restrains the expansion of nano-silicon during charging and discharging, thereby improving the cycle performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is the SEM image of the silicon-carbon composite material prepared in Example 1. DETAILED DESCRIPTION

[0011] Embodiment 1: A method for preparing a metal-doped silicon-carbon composite material comprises the following steps: Step S1: adding cerium chloride to a vacuum furnace, evacuating to a vacuum degree of ≤0.1 Torr, heating to 1800°C, heating the cerium chloride to steam, and mixing it with trimethylborane gas (volume ratio, cerium chloride gas: trimethylborane gas = 10:3), and passing it into large-pore porous carbon (pore size 10 nm) at a flow rate of 300 SCCM for 150 minutes to obtain metal-doped porous carbon; Step S2: 100 g of metal-doped porous carbon is transferred to a vacuum furnace, and 10 g of metallic lithium is spread on the bottom, and then heated to 1500°C to generate lithium vapor and deposited in the metal-doped porous carbon; then the temperature is lowered to 550°C and trisilane gas is introduced at a flow rate of 300 SCCM for 150 min, and finally the temperature is lowered to 250°C, and acetylene / oxygen mixed gas (volume ratio, acetylene: oxygen = 10:3) is introduced, and amorphous carbon is coated at a flow rate of 100 SCCM for 150 min to obtain a silicon-carbon composite material.

[0012] Embodiment 2: A method for preparing a metal-doped silicon-carbon composite material comprises the following steps: Step S1: adding scandium chloride into a vacuum furnace, evacuating to a vacuum degree of ≤0.1 Torr, heating to 2000°C, heating the scandium chloride to generate scandium chloride vapor, and mixing it with thiourea gas (volume ratio, scandium chloride gas:thiourea gas=10:1), and passing it into large-pore porous carbon (pore size 10 nm) at a flow rate of 100 SCCM for 600 minutes to obtain metal-doped porous carbon; Step S2: 100 g of metal-doped porous carbon is transferred to a vacuum furnace, and 5 g of metallic lithium is spread on the bottom, and then heated to 1400°C to generate lithium vapor and deposited in the metal-doped porous carbon; then the temperature is lowered to 450°C and trichlorosilane gas is introduced at a flow rate of 100 SCCM for 300 min, and finally the temperature is lowered to 200°C, acetylene / oxygen mixed gas (volume ratio, acetylene: oxygen = 10:1) is introduced, and amorphous carbon is coated at a flow rate of 50 SCCM for 300 min to obtain a silicon-carbon composite material.

[0013] Embodiment 3: A method for preparing a metal-doped silicon-carbon composite material comprises the following steps: Step S1: adding lanthanum chloride to a vacuum furnace, evacuating to a vacuum degree of ≤0.1 Torr, heating to 2000°C, heating lanthanum chloride to generate lanthanum chloride vapor, and mixing with mercaptan gas (volume ratio, lanthanum chloride: mercaptan = 10:5), and passing it into large-pore porous carbon (pore size 10 nm) at a flow rate of 500 SCCM for 60 minutes to obtain metal-doped porous carbon; Step S2: 100 g of metal-doped porous carbon is transferred to a vacuum furnace, and 15 g of metallic lithium is spread on the bottom, and then heated to 1600° C. to generate lithium vapor and deposit it in the metal-doped porous carbon; then the temperature is lowered to 650° C. and butadiene silane gas is introduced at a flow rate of 500 SCCM for 30 min, and finally the temperature is lowered to 300° C. and acetylene / oxygen mixed gas (volume ratio, acetylene: oxygen = 10:5) is introduced at a flow rate of 200 SCCM for 30 min for amorphous carbon coating to obtain a silicon-carbon composite material. Comparative Example 1: A method for preparing a silicon-carbon composite material comprises: different from Example 1, cerium chloride gas is not introduced in step S1, and the rest is the same as Example 1.

[0014] Comparative Example 2: The difference from Example 1 is that no metallic lithium is added in step S2, and the rest is the same as Example 1.

[0015] Test Example 1: Morphology Test The silicon-carbon composite material in Example 1 was subjected to SEM testing, and the test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the material presents a spherical structure, and the particle size of the material is evenly distributed, with the particle size ranging from 5-10 μm.

[0016] Test Example 2: Physical and chemical tests and button cell tests Refer to GB / T38823-2020 "Silicon Carbon" to test the specific surface area and tap density of the silicon-carbon composite material, use a four-probe tester to test the powder resistivity of the silicon-carbon composite material, and use XRD to test its grain size La, and test the residual alkali content of the material; The silicon-carbon composite materials in Examples 1-3 and Comparative Examples 1-2 were used as negative electrode materials for lithium-ion batteries to prepare button batteries, and the preparation method was as follows: Add binder, conductive agent and solvent to the composite material, stir to make slurry, coat on copper foil, dry and roll to get negative electrode sheet; the binder used is polyvinylidene fluoride (PVDF), the conductive agent is conductive carbon black (SP), the solvent is N-methylpyrrolidone (NMP), the amount ratio of composite material, SP, PVDF and NMP is 90g:4g:6g:250mL; the electrolyte is lithium hexafluorophosphate (LiPF6), the mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with a volume ratio of 1:1 is used as solvent, and the electrolyte concentration is 1mol / L; the metal lithium sheet is the counter electrode, and the diaphragm is a polypropylene (PP) film. The button cell is assembled in an argon-filled glove box.

[0017] The electrochemical performance of button cells comprising the silicon-carbon composite materials of Examples 1-3 and Comparative Examples 1-2 was tested using a Wuhan Blue Power CT2001A battery tester with a charge and discharge voltage range of 0.005 V to 2.0 V and a charge and discharge rate of 0.1 C. The charging DCR (50% SOC) of the material was also tested.

[0018] The test results are shown in Table 1.

[0019] Table 1 project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 First discharge specific capacity (mAh / g) 1998.8 1924.5 2024.6 1811.8 1889.2 First efficiency (%) 94.8% 95.2% 94.3% 91.4% 92.1% <![CDATA[Specific surface area (m 2 / g)]]> 3.42 3.13 3.89 3.01 2.87 <![CDATA[Tap density (g / cm 3 ).]]> 1.04 1.01 1.07 0.95 0.90 Residual alkali (ppm) 165 134 193 212 72 Powder resistivity (Ω·cm) 0.78 0.86 0.69 1.78 2.21 DCR (Ω) 24.5 25.9 23.1 29.3 26.4 It can be seen from the data in Table 1 that the specific capacity, first efficiency, powder conductivity, full charge expansion and DCR of the silicon-carbon composite material prepared by the present invention are significantly better than those of the comparative example. The reason is that the electronic conductivity of the material is improved by doping rare earth metal materials and heteroatoms in the porous carbon, and metallic lithium is deposited in its core by vapor deposition, which reduces the defects of the material and improves the first efficiency and electronic conductivity.

[0020] Test Example 3: Soft-pack battery test The silicon-carbon composite materials of Examples 1-3 and Comparative Examples 1-2 were mixed with 95% artificial graphite as negative electrode materials to prepare negative electrode sheets. 1 / 3 Co 1 / 3 Mn 1 / 3 O2) as the positive electrode; lithium hexafluorophosphate (LiPF6) as the electrolyte, a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (DEC) with a volume ratio of 1:1 as the solvent, and an electrolyte concentration of 1.3 mol / L; Celgard 2400 membrane as the separator, and a 5Ah soft pack battery was prepared. The liquid absorption and retention capacity, rate performance, and cycle performance of the negative electrode were tested respectively.

[0021] a. Liquid absorption capacity test Use a 1mL burette and draw 1mL of electrolyte, add a drop on the surface of the electrode, and count until the electrolyte is completely absorbed, and record the time t. The test results are shown in Table 2.

[0022] b. Cycle performance The soft pack batteries containing the silicon-carbon composite materials of Examples 1-3 and Comparative Examples 1-2 were subjected to cycle performance tests; the test conditions were: test voltage range 2.5-4.2V, 1C / 1C, temperature 25±3°C, 500 weeks. The test results are shown in Table 2.

[0023] C. HPPC rate test The charging DCR at different SOCs (5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%) was tested at a 3C rate. The test results are shown in Table 3.

[0024] Table 2 Lithium-ion battery Liquid absorption capacity (S) Cycle performance Example 1 98 94.5% Example 2 107 94.1% Example 3 86 95.2% Comparative Example 1 123 91.7% Comparative Example 2 136 89.3% It can be seen from Table 2 that the liquid absorption capacity and cycle performance of the soft-pack lithium-ion battery prepared using the silicon-carbon composite material of the present invention are better than those of the comparative example. The reason is that the silicon-carbon composite material of the present invention has a high specific surface area and a low powder resistivity, which improves the liquid retention performance of the battery. At the same time, the example material has low expansion, thereby improving the cycle performance.

[0025] Table 3 Table 3 shows the charging HPPC test of batteries prepared from the example materials and the comparative examples. It can be seen from the table that the DCR of the example materials is lower than that of the comparative examples. The reason is that the doping of rare earth metal compounds and heteroatoms in the example materials reduces the electronic conductivity, and the deposition of metallic lithium improves the electronic and ionic conductivity of the materials, thereby reducing the DCR.

[0026] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A metal-doped silicon-carbon composite material, the composite material presents a core-shell structure, the core is metal lithium and its rare earth metal doped silicon-carbon material, the shell is amorphous carbon, and the mass ratio of the shell is 5-10% calculated based on the mass ratio of the composite material being 100%.

2. A method for preparing a metal-doped silicon-carbon composite material, comprising the following steps: Step S1: adding a rare earth metal compound to a vacuum furnace, evacuating to a vacuum degree of ≤0.1 Torr, heating to 1500-2000° C., heating the rare earth metal compound to generate rare earth metal compound vapor, and mixing it with a heteroatom gas with a volume ratio of rare earth metal compound: heteroatom gas = 10:1-5, and passing it into a large-pore porous carbon at a flow rate of 100-500 SCCM for 60-600 minutes to obtain a metal-doped porous carbon; Step S2: According to the mass ratio of metal-doped porous carbon: metallic lithium: silane gas = 100: 5-15: 100-200, the metal-doped porous carbon is transferred to a vacuum furnace, and metallic lithium is spread on the bottom, and then heated to 1400-1600°C to generate lithium vapor deposited in the metal-doped porous carbon, cooled to 450-650°C, silane gas is introduced at a flow rate of 100-500SCCM for 30-300min, cooled to 200-300°C, and acetylene / oxygen mixed gas with a volume ratio of acetylene: oxygen = 10: 1-5 is introduced at a flow rate of 50-200SCCM for 30-300min for amorphous carbon coating to obtain a metal-doped silicon-carbon composite material.

3. A method for preparing a metal-doped silicon-carbon composite material as described in claim 2, wherein the rare earth metal compound described in step S1 is one of cerium chloride, scandium chloride, lanthanum chloride or yttrium chloride; the heteroatom compound is one of trimethylborane, thiourea, N-methylthiourea, thiol, thiophenol, pyridine, acrylonitrile or dicyandiamide gasification.

4. A method for preparing a metal-doped silicon-carbon composite material as described in claim 2, wherein the silane gas in step S1 is one of the gases generated by heating trisilane, butadisilane, trichlorosilane, methyltrichlorosilane or dimethyldichlorosilane to 200-300°C.

Citation Information

Cited By

  • Silicon-carbon composite material as well as preparation method and application thereof

    CN120727796A

  • Silicon-carbon composite material, method for preparing the same, and use thereof

    CN120727796B