Pole piece, battery cell and electric equipment
By optimizing the embedding ratio of the welding part in the electrode sheet and using roller welding technology, the over-welding or dummy welding problems during welding of the composite liquid collector and aluminum foil are solved, and the welding quality of the electrode sheet and the mechanical properties of the battery core are improved.
Patent Information
- Application Number
- CN202410938921.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-12
AI Technical Summary
When the composite liquid collector is ultrasonic welding with aluminum foil, the polymer layer and the metal layer are poorly fused, which can easily lead to over-welding or dummy welding, affecting the welding quality and safety of the electrode sheet.
A pole sheet structure is designed, including a current collector, a first adapter layer and a second adapter layer. The thickness of the welded portion embedded support layer is optimized to ensure that the embedding ratio of the welded portion is 0.1≤(D1+D2)/H1≤0.8 Within the range, welding efficiency and quality are improved through roller welding technology.
It effectively reduces the phenomenon of dummy and over-welding, improves the welding strength and stability of the electrode sheet, and enhances the mechanical properties and current carrying capacity of the battery cell.
Smart Images

Figure CN118943376A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the field of battery technology, and in particular to a pole piece, a battery cell and an electrical device. Background Art
[0002] Composite current collector is a sandwich-type pole piece composed of metal, polymer and metal structure, which has attracted wide attention from battery developers. This current collector uses polymer as the pole piece skeleton, thereby reducing the thickness of the metal layer. Such a pole piece structure can reduce metal burrs when the battery cell is mechanically damaged, thus solving the safety risks caused by mechanical damage to the battery cell.
[0003] In the process of realizing the present application, the inventors found that: currently, the metal-polymer-metal structure of the composite current collector includes metal and non-metal materials. When the current collector and the aluminum foil are ultrasonically welded, the polymer layer cannot blend well with the metal, which can easily cause problems such as over-welding or cold welding. Summary of the invention
[0004] The embodiments of the present application aim to provide a pole piece, a battery cell and an electrical device, which can improve the current situation where over-welding or cold welding is easily produced during ultrasonic welding of a current collector and an aluminum foil.
[0005] In order to solve the above technical problems, this application adopts the following technical solutions:
[0006] In the first aspect, a pole piece is provided, comprising a current collector, a first transfer layer and a second transfer layer, wherein the pole piece is further provided with a welding portion. The current collector comprises a first metal layer, a support layer and a second metal layer arranged along a first direction. The first transfer layer is connected to the side of the first metal layer away from the support layer. The second transfer layer is connected to the side of the second metal layer away from the support layer. Wherein, the pole piece is further provided with a welding portion, the welding portion is located at the connection between the first transfer layer and the first metal layer, and the welding portion is located at the connection between the second transfer layer and the second metal layer, along the first direction, on one side of the first transfer layer, the thickness of the welding portion embedded in the support layer is D1, on one side of the second transfer layer, the thickness of the welding portion embedded in the support layer is D2, and the thickness of the support layer is H1; the ratio of D1 and D2 to the thickness of the support layer satisfies: 0.1≤(D1+D2) / H1≤0.8. D1 / H1≥0.05, D2 / H1≥0.05.
[0007] In the above scheme, the welding part is provided so that the first transfer layer and the second transfer layer are welded to the current collector, wherein the first transfer layer is welded to the first metal layer of the current collector, and the second transfer layer is welded to the second metal layer of the current collector, so as to facilitate fusion. The welding part obtained after the electrode piece is welded will be embedded toward the support layer, and the thickness of the welding part embedded in the support layer is further optimized so that the thickness of the welding part embedded in the support layer from both sides of the support layer and the thickness of the support layer itself meet: 0.1≤(D1+D2) / H1≤0.8, thereby reducing the phenomenon of cold welding caused by the welding part being embedded in the support layer too little when the ratio of the thickness of the welding part embedded in the support layer is less than 0.1, reducing the influence of weak welding on the electrode piece, or reducing the phenomenon of over-welding caused by the welding part being embedded in the support layer too much when the ratio of the thickness of the welding part embedded in the support layer is greater than 0.8, reducing the influence of over-welding on the mechanical properties of the support layer on the electrode piece. D1 / H1≥0.05, D2 / H1≥0.05, limiting the lower limits of D1 and D2 can reduce the phenomenon of cold soldering caused by the small welding part on one side.
[0008] In one or more embodiments, along the first direction, the ratio of D1 and D2 to the thickness of the support layer satisfies: 0.4≤(D1+D2) / H1≤0.6, thereby further reducing the number of cold welds or over welds at the welded portion.
[0009] In one or more embodiments, the thickness of the support layer along the first direction is H1, the thickness of the first metal layer along the first direction is H2, and the thickness of the second metal layer along the first direction is H3. 4μm≤H1≤18.4μm, 0.8μm≤H2≤3μm, 0.8μm≤H3≤3μm; and 6.5μm≤H1+H2+H3≤20μm. So that the support layer of the current collector has stable mechanical properties, and the first metal layer and the second metal layer are provided, so as to facilitate welding with the above-mentioned first transfer layer and the second transfer layer.
[0010] In one or more embodiments, along the first direction, the support layer, the first metal layer and the second metal layer satisfy: 13 μm ≤ H1 ≤ 16 μm, 1 μm ≤ H2 ≤ 3 μm, 1 μm ≤ H3 ≤ 3 μm. This structure enables the current collector to have good mechanical properties and current carrying capacity.
[0011] In one or more embodiments, along the first direction, the thickness of the first transfer layer is Z1, 8 μm≤Z1≤20 μm. The thickness of the second transfer layer is Z2, 8 μm≤Z2≤20 μm. This reduces the thickness of the pole piece and the occupied space.
[0012] In one or more embodiments, the width of the first transfer layer is Z3, 10 mm ≤ Z3 ≤ 20 mm; the width of the second transfer layer is Z4, 10 mm ≤ Z4 ≤ 20 mm, thereby reducing the width and occupied space of the pole piece.
[0013] In one or more embodiments, the welding part is provided with a plurality of welding feet, and the plurality of welding feet are arranged in a dot-shaped interval in the area of the welding part; the ratio of the area of the welding feet to the area of the welding part is B, 0.3≤B≤0.7. When the ratio B is less than 0.3, the area of the welding feet accounts for too small an area of the welding part, which is easy to cause a cold weld; when the ratio is greater than 0.7, the area of the welding feet accounts for too large an area of the welding part, which is easy to cause an over-weld.
[0014] In one or more embodiments, along the second direction, the width D3 of the weld foot portion satisfies: 10 μm ≤ D3 ≤ 50 μm; the second direction is perpendicular to the first direction and extends along the length of the current collector, thereby reducing the possibility of cold welding or over welding of the weld foot portion.
[0015] In one or more embodiments, the projection of the first transfer layer along the first direction at least partially overlaps with the current collector, the projection of the second transfer layer along the first direction at least partially overlaps with the current collector, and the welding portion is located in the overlapping area of the projections of the first transfer layer, the current collector, and the second transfer layer. Thus, the welding portion welds the first transfer layer and the second transfer layer to the two sides of the current collector relative to each other, so as to facilitate welding of the first transfer layer and the second transfer layer with other external metal materials.
[0016] In one or more embodiments, in the pole piece, along the first direction, the thickness of the overlapping portion of the welding portion, the first transfer layer, the current collector, and the second transfer layer is A1; the thickness of the overlapping portion of the first transfer layer, the current collector, and the second transfer layer is A2; the difference between A1 and A2 is: 10μm≤A1-A2≤30μm. Through the above structure, the portion of the pole piece with a thickness of A1 is thicker, thereby improving the structural strength of the pole piece and improving the structural stability of the pole piece.
[0017] In one or more embodiments, along the first direction, the current collector is provided with an empty foil area in the region where the projections of the first transfer layer and the second transfer layer overlap, and the empty foil area is used for welding the first transfer layer and / or the second transfer layer.
[0018] In one or more embodiments, along the second direction, the length of the empty foil area is K1, 1mm≤K1≤5mm; the second direction is perpendicular to the first direction and extends along the length of the current collector, thereby leaving space for welding.
[0019] In one or more embodiments, along the second direction, the length of the empty foil area is K1, 2.5 mm ≤ K1 ≤ 3.5 mm, so as to further reserve space for welding.
[0020] In one or more embodiments, the material of the support layer includes polypropylene, polyethylene, polyurethane, polyethylene terephthalate, etc., so that the support layer has good mechanical properties.
[0021] In a second aspect, a battery cell is provided, comprising an electrode assembly, wherein the electrode assembly comprises the above-mentioned electrode sheet.
[0022] In a third aspect, an electrical device is provided, comprising the above-mentioned battery cell.
[0023] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.
[0025] Figure 1 It is a schematic diagram provided by one or more embodiments of the present application;
[0026] Figure 2 is another schematic diagram provided by one or more embodiments of the present application;
[0027] Figure 3 is another schematic diagram provided by one or more embodiments of the present application;
[0028] Figure 4 It is a schematic diagram of one of the test methods provided in this application.
[0029] The figures are as follows:
[0030]
[0031] DETAILED DESCRIPTION
[0032] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0033] It should be noted that when an element is described as being "fixed on" or "disposed on" another element, it may be directly on the other element, or one or more intermediate elements may exist therebetween. When an element is described as being "connected to" or "welded to" another element, it may be directly connected / welded to the other element, or one or more intermediate elements may exist therebetween.
[0034] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "upper", "lower", "top", "bottom", "inside" and "outside" are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present application and simplifying the description. They do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0035] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0036] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0037] Reference to "embodiment" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. In addition, the technical features involved in the different embodiments of the present application described below may be combined with each other as long as they do not conflict with each other.
[0038] In the first place, see Figure 1 and Figure 2The present application provides a pole piece 1000, which includes a current collector 100, a first transfer layer 200, and a second transfer layer 300. In addition, the pole piece 1000 is provided with a welding portion 400. The current collector 100 includes a first metal layer 110, a support layer 120, and a second metal layer 130 arranged along a first direction X. The first transfer layer 200 is connected to a side of the first metal layer 110 that is away from the support layer 120. The second transfer layer 300 is connected to a side of the second metal layer 130 that is away from the support layer 120. The welding part 400 is located at the connection between the first transfer layer 200 and the first metal layer 110, and the welding part 400 is located at the connection between the second transfer layer 300 and the second metal layer 130. Along the first direction X, on one side of the first transfer layer 200, the welding part 400 is embedded in the support layer 120 with a thickness of D1, and on one side of the second transfer layer 300, the welding part 400 is embedded in the support layer 120 with a thickness of D2, and the thickness of the support layer 120 is H1; the ratio of D1 and D2 to the thickness of the support layer 120 satisfies: 0.1≤(D1+D2) / H1≤0.8. The welding part 400 is provided so that the first transfer layer 200 and the second transfer layer 300 are welded to the current collector 100, wherein the first transfer layer 200 is welded to the first metal layer 110 of the current collector 100, and the second transfer layer 300 is welded to the second metal layer 130 of the current collector 100, so as to facilitate fusion. Among them, the welding part 400 obtained after welding the pole piece 1000 will pass through the first metal layer 110 and the second metal layer 130 from both sides and be embedded toward the support layer 120, and further optimize the thickness of the welding part 400 embedded in the support layer 120 so that the thickness of the welding part 400 embedded in the support layer 120 and the thickness of the support layer 120 itself satisfy: 0.1≤(D1+D2) / H1≤0.8, thereby reducing the cold welding phenomenon caused by the thickness of the welding part 400 embedded in the support layer 120 when the ratio of the welding part 400 embedded in the support layer 120 is less than 0.1, reducing the influence of weak welding on the pole piece 1000, or reducing the over-welding phenomenon caused by the thickness of the welding part 400 embedded in the support layer 120 when the ratio of the welding part 400 embedded in the support layer 120 is greater than 0.8, reducing the influence of the over-welding phenomenon on the mechanical properties of the support layer 120 on the pole piece 1000. That is, when (D1+D2) / H1 is greater than 0.8, it is easy to cause over-welding of the welding part 400, thereby destroying the mechanical properties of the supporting layer 120, increasing the resistance of the current collector 100, and reducing the current carrying capacity of the current collector 100; and when (D1+D2) / H1 is less than 0.1, the welding part 400 after welding will not be connected to the supporting layer 120, which is easy to cause cold welding, resulting in insufficient bonding strength between the first transfer layer 200 and the second transfer layer 300 and the current collector 100, thereby reducing the current carrying capacity and mechanical properties of the current collector 100.
[0039] It should be further explained that the current collector 100 is a composite structure composed of a variety of structures. The first metal layer 110 and the second metal layer 130 are made of the same material. On the one hand, the current carrying capacity of the pole piece 1000 is stable, and the resistance of the current collector 100 is not uneven due to different metal materials, which affects the passage of current; on the other hand, the same metal materials have the same physical properties during the welding process, which makes the welding stable and efficient. In the present application, roller welding is used between the first transfer layer 200 and the first metal layer 110, and roller welding is used between the second transfer layer 300 and the second metal layer 130. The advantage of this welding method is that the welding efficiency is high. Roller welding is solid phase welding. The metal is heated to a certain temperature, and then pressure is applied with a roller to plastically deform the joint surface to produce a metal bond. The internal resistance after welding is low, so that the conductive performance of the pole piece 1000 is good. Optionally, the materials of the first metal layer 110 and the second metal layer 130 include aluminum, copper, etc. It is worth mentioning that the materials of the first transfer layer 200 and the second transfer layer 300 include aluminum and copper. In order to facilitate the welding between the first transfer layer 200 and the first metal layer 110, and to facilitate the welding between the second transfer layer 300 and the second metal layer 130, the materials of the first metal layer 110, the second metal layer 130, the first transfer layer 200 and the second transfer layer 300 are the same, so that during the roller welding process, the first transfer layer 200 and the first metal layer 110, as well as the second transfer layer 300 and the second metal layer 130 can be fused together, thereby improving the welding efficiency while ensuring the current carrying capacity.
[0040] In some preferred embodiments, along the first direction X, the thickness of the welding part 400 embedded in the support layer 120 is D1, and the thickness of the welding part 400 embedded in the support layer 120 is D2, 0.1≤(D1+D2) / H1≤0.8. The phenomenon of cold welding or over-welding of the welding part 400 is further reduced. D1 / H1≥0.05, D2 / H1≥0.05. Through the above structure, in one or more embodiments of the present application, an embodiment with better current carrying capacity and better mechanical properties can be obtained, as shown in the analysis of the embodiments and comparative examples below. Thereby reducing the phenomenon of cold welding or over-welding of the welding part 400, thereby reducing the cold welding of the welding part 400, resulting in insufficient connection strength between the current collector 100, the first transfer layer 200 and the second transfer layer 300, affecting the current carrying capacity of the current collector 100, or reducing the over-welding of the welding part 400, resulting in structural damage to the support layer 120 in the current collector 100, affecting the mechanical properties of the current collector 100. D1 / H1≥0.05, D2 / H1≥0.05, limiting the lower limits of D1 and D2 can reduce the phenomenon of cold soldering caused by the small welding part on one side.
[0041] For the above current collector 100, see Figure 1 and Figure 2The thickness of the support layer 120 along the first direction X is H1, the thickness of the first metal layer 110 along the first direction X is H2, and the thickness of the second metal layer 130 along the first direction X is H3; 4μm≤H1≤18.4μm, 0.8μm≤H2≤3μm, 0.8μm≤H3≤3μm; and 6.5μm≤H1+H2+H3≤20μm. In order to ensure the mechanical properties of the current collector 100, the thickness of the support layer 120 is between 4μm and 18.4μm. If the thickness is too small, it will easily lead to insufficient support performance of the current collector 100 and poor force-bearing capacity of the current collector 100; if the thickness is too large, it will affect the volume of the current collector 100, resulting in an increase in the thickness of the pole piece 100, or, when the overall thickness of the current collector 100 is constant, the thickness of the support layer 120 occupies too much of the thickness of the current collector 100, resulting in a reduction in the thickness of the first metal layer 110 and the second metal layer 130, which may easily lead to a decrease in the current-carrying capacity of the current collector 100 and an increase in resistance.
[0042] Preferably, see Figure 1 and Figure 2 Along the first direction X, the support layer 120, the first metal layer 110 and the second metal layer 130 satisfy: 13μm≤H1≤16μm, 1μm≤H2≤3μm, 1μm≤H3≤3μm. This further improves the mechanical properties of the support layer 120 and also makes the first metal layer 110 and the second metal layer 130 have better electrical conductivity.
[0043] In one or more embodiments of this application, please refer to Figure 1 and Figure 2 . For the above-mentioned first transfer layer 200 and the second transfer layer 300, along the first direction X, the thickness of the first transfer layer 200 is Z1, 8μm≤Z1≤20μm; the thickness of the second transfer layer 300 is Z2, 8μm≤Z2≤20μm. The width of the first transfer layer 200 is Z3, 10mm≤Z3≤20mm; the width of the second transfer layer 300 is Z4, 10mm≤Z4≤20mm. It is worth mentioning that the thickness of the first transfer layer 200 and the width of the second transfer layer 300 arranged on both sides of the current collector 100 can be equal or unequal, and the thickness of the first transfer layer 200 and the thickness of the second transfer layer 300 arranged on both sides of the current collector 100 can be equal or unequal. When a plurality of pole pieces 1000 need to be stacked, the thickness of the first transfer layer 200 and / or the second transfer layer 300 of two adjacent pole pieces 1000 can be reduced to reduce the overall thickness and further improve space utilization.
[0044] In one or more embodiments of this application, please refer to Figure 1 and Figure 2. The welding portion 400 is provided with a plurality of welding feet 410, and the plurality of welding feet 410 are arranged at intervals in a dotted manner in the area of the welding portion 400. The ratio of the area of the welding foot 410 to the area of the welding portion 400 is B, and 0.3≤B≤0.7. When the ratio B is less than 0.3, the area of the welding foot 410 accounts for too small an area of the welding portion 400, which is easy to cause a cold solder joint; when the ratio is greater than 0.7, the area of the welding foot 410 accounts for too large an area of the welding portion 400, which is easy to cause an over-soldering. The welding foot 410 is located at the junction of the first metal layer 110, the first transfer layer 200 and at least a portion of the support layer 120, and at the junction of the second metal layer 130, the second transfer layer 300 and at least a portion of the support layer 120. Among them, the weld foot 410 can be cylindrical along the first direction X, and the diameter of the weld foot 410 is between 1mm and 5mm. Preferably, the diameter of the weld foot 410 is 2mm, so as to improve the connection ability of the weld foot 410, improve the connection stability between the first transfer layer 200 and the first metal layer 110, and improve the connection stability between the second transfer layer 300 and the second metal layer 130. It can be understood that the weld foot 410 arranged at intervals in a dotted manner causes the first transfer layer 200 and / or the second transfer layer 300 to deform by embedding without overall compression, thereby improving the roll welding efficiency and reducing the waste of materials. And when the ratio B is less than or equal to 0.7, the roll welding efficiency can be further improved and the roll welding cost can be reduced. Specifically, when the ratio B is greater than 0.7, on the one hand, it will cause the welding part 400 to be over-welded, and on the other hand, the number of weld foot 410 needs to be increased. In the roll welding process, the number of welding points for roll welding the weld foot 410 needs to be increased, thereby reducing the roll welding efficiency.
[0045] Further, along the second direction Y, the width D3 of the weld foot 410 satisfies: 10μm≤D3≤50μm; the second direction Y is a direction perpendicular to the first direction X and extending along the length of the current collector 100. It should be noted that the width of the weld foot 410 in the second direction Y includes the distance between two adjacent weld feet 410, thereby preventing the distance between the two weld feet 410 from being too close and causing over-welding. Through the above structure, when the width of the weld foot 410 is less than 10μm, it is easy to cause over-welding of the weld foot 410, affecting the mechanical properties of the current collector 100 and reducing the ability to withstand local stress; when the width of the weld foot 410 is greater than 50μm, it is easy to cause a cold weld of the weld foot 410, affecting the connection stability between the current collector 100 and the first transfer layer 200 and / or the second transfer layer 300.
[0046] In one or more embodiments of this application, please refer to Figure 1 and Figure 2The projection of the first transfer layer 200 along the first direction X at least partially overlaps with the current collector 100, and the projection of the second transfer layer 300 along the first direction X at least partially overlaps with the current collector 100, and the welding portion 400 is located in the overlapping area of the projections of the first transfer layer 200, the current collector 100, and the second transfer layer 300. Thus, the welding portion 400 welds the first transfer layer 200 and the second transfer layer 300 to the two sides of the current collector 100 relatively, so as to facilitate the welding of the first transfer layer 200 and the second transfer layer 300 with other external metal materials. It can be understood that the projection of the first transfer layer 200 along the first direction X at least partially overlaps with the current collector 100, which means that the first transfer layer 200 in the first direction X is at least partially connected to the current collector 100, and in the second direction Y, the current collector 100 leaves other areas not connected to the first transfer layer 200 for other external parts to be connected to the current collector 100, and the area of the first transfer layer 200 not connected to the current collector 100 in the second direction Y can be used to connect other metal materials; accordingly, the projection of the second transfer layer 300 along the first direction X at least partially overlaps with the current collector 100, which means that the second transfer layer 300 in the first direction X is at least partially connected to the current collector 100, and in the second direction Y, the current collector 100 leaves other areas not connected to the second transfer layer 300 for other external parts to be connected to the current collector 100, and the area of the second transfer layer 300 not connected to the current collector 100 in the second direction Y can be used to connect other metal materials. Optionally, the regions where the first switching layer 200 and the second switching layer 300 are not connected to the current collector 100 can facilitate the connection between the plurality of pole pieces 1000 .
[0047] In one or more embodiments of the present application, please refer to 3. In the pole piece 1000, along the first direction X, the thickness of the overlapping portion of the welding portion 400, the first transfer layer 200, the current collector 100, and the second transfer layer 300 is A1; the thickness of the overlapping portion of the first transfer layer 200, the current collector 100 and the second transfer layer 300 is A2; the difference between A1 and A2 is: 10μm≤A1-A2≤30μm. Through the above structure, the portion of the pole piece 1000 with a thickness of A1 is thicker, thereby improving the structural strength of the pole piece 1000 and improving the structural stability of the pole piece. In combination with the above structure, the pole piece 1000 is further described. Before the pole piece 1000 is roller welded, the thickness of the pole piece 1000 is the sum of the thickness of the above-mentioned current collector 100, the thickness of the first transfer layer 200 and the thickness of the second transfer layer 300. After the pole piece 1000 is rolled, the pole piece 1000 is compressed by rolling, and the welding foot portion 410 is embedded in the current collector 100, the first transfer layer 200 and the second transfer layer 300, so that the first transfer layer 200 and the second transfer layer 300 are deformed around the welding foot portion 410, that is, the difference between the thickness of the welding portion 400 and the thickness of the portion of the pole piece 1000 outside the welding portion 400 is 10μm to 30μm, which is the deformation of the pole piece 1000 before and after welding. Through the above structure, when the deformation is less than 10μm, it means that the embedded thickness of the welding foot portion 410 is insufficient, which is easy to cause a cold weld; when the deformation is greater than 30μm, it means that the embedded thickness of the welding foot portion 410 is excessive, which is easy to cause an over-weld.
[0048] In one or more embodiments of this application, please refer to Figure 1 and Figure 2 Along the first direction X, the current collector 100 is provided with an empty foil area 500 in the area where the projections of the first transfer layer 200 and the second transfer layer 300 overlap, and the empty foil area 500 is used for welding the first transfer layer 200 and / or the second transfer layer 300. By providing the empty foil area 500, roll welding and external connection of other metal materials, such as aluminum foil, copper foil, etc. are facilitated. Specifically, the empty foil area 500 is an area that is not coated with other materials, thereby reducing the influence of the coated materials on the roll welding.
[0049] Optionally, along the second direction Y, see Figure 1 and Figure 2 The length of the empty foil area 500 is K1, 1 mm ≤ K1 ≤ 5 mm. The second direction Y is perpendicular to the first direction X and extends along the length of the current collector 100. Thus, more space is reserved for external connection of other metal materials.
[0050] Preferably, along the second direction Y, see Figure 1 and Figure 2The length of the empty foil area 500 is K1, 2.5 mm ≤ K1 ≤ 3.5 mm. Thus, when more space is reserved for other metal materials to be connected externally, some space can be saved, thereby reducing the volume and occupied area of the pole piece 1000.
[0051] Optionally, the material of the support layer 120 includes polypropylene, polyethylene, polyurethane, polyethylene terephthalate, etc. Thus, the support layer 120 has good insulation performance, mechanical support performance, heat resistance, wear resistance, etc.
[0052] In combination with one or more embodiments given above, the present application specifically provides the following embodiments and comparative examples for testing. The testing methods include two methods: 1) By clamping the above-mentioned pole piece 1000 in a high-speed rail tensile machine, the pole piece 1000 is provided with two sides of the welding part 400 connected to the high-speed rail tensile machine respectively, and the speed of the high-speed rail tensile machine is set to 50mm / min, so as to test the tensile force that the welding part 400 can withstand after welding to obtain the "welding tensile force". The greater the welding tensile force, the stronger the mechanical properties of the embodiment or comparative example; 2) as Figure 4 As shown, the pole piece 1000 is connected to the same conductive element (at Figure 4 The bottom structure), one side of the welding portion 400 in the second direction Y is connected to the conductive element, and then the welding portion 400 is symmetrically cut into two identical areas in a "C" shape along the second direction Y, and the two identical areas are respectively connected to the positive and negative electrodes of the same circuit to form a conductive path. By providing the same voltage between the positive and negative electrodes of the conductive path of each embodiment and comparative example, the "welding resistance" is measured, wherein the smaller the welding resistance, the stronger the current carrying capacity of the embodiment. It can be understood that the welding resistance is only the resistance value of the embodiment or comparative example in this test, which is used to indicate the current carrying capacity of the embodiment or comparative example, and is not the actual resistance value of the embodiment or comparative example. It should be noted that the thickness of the first metal layer 110 and the second metal layer 130 of the current collector 100 in the following embodiments and comparative examples is 2μm, and the thickness of the polymer layer is 15μm.
[0053] Embodiment 1: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.1; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0054] Embodiment 2: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.3; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0055] Embodiment 3: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.4; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0056] Embodiment 4: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.5; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0057] Embodiment 5: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0058] Embodiment 6: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.8; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0059] Embodiment 7: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.3.
[0060] Embodiment 8: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.4.
[0061] Embodiment 9: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.6.
[0062] Embodiment 10: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.7.
[0063] Embodiment 11: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.2.
[0064] Embodiment 11: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.8.
[0065] Comparative Example 1: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.05; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0066] Comparative Example 2: The ratio of the thickness of the welding portion 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.9; the ratio of the area of the welding foot portion 410 to the area of the welding portion 400 is 0.5.
[0067] Through the above comparative examples and embodiments, the welding tension and welding resistance of the electrode piece 1000 after roller welding are measured to obtain Table 1.
[0068] Table 1:
[0069]
[0070] Through the above test, it is found that in comparative example 1, when the ratio of the thickness of the welding part 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is less than 0.1, the welding tension is low and the welding resistance is high; while in comparative example 2, when the ratio of the thickness of the welding part 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is greater than 0.8, the welding tension is low and the welding resistance is high. By comparing Example 11 and Example 12 with any one of Examples 7 to 10, it can be learned that the ratio of the thickness of the welding part 400 embedded in the supporting layer 120 to the thickness of the supporting layer 120 is 0.6. When the ratio of the welding foot 410 to the welding part 400 in Example 11 is less than 0.3, the mechanical properties are insufficient compared with any one of Examples 7 to 10, and the welding resistance is large; when the ratio of the welding foot 410 to the welding part 400 in Example 12 is greater than 0.7, the mechanical properties are insufficient relative to any one of Examples 7 to 10, and the welding resistance is high. Among the above multiple embodiments given in this application, embodiment 4 and embodiment 10 are more preferred embodiments, but it does not mean that the embodiments and preferred embodiments provided in this application are only the above 12 embodiments. That is, when the ratio of the thickness of the welding part 400 embedded in the support layer 120 to the thickness of the support layer 120 is 0.5; the ratio of the area of the weld leg 410 to the area of the welding part 400 is 0.5, or the ratio of the thickness of the welding part 400 embedded in the support layer 120 to the thickness of the support layer 120 is 0.6; the ratio of the area of the weld leg 410 to the area of the welding part 400 is 0.7, a more preferred embodiment can be obtained. Thereby, the pole piece 1000 obtains better mechanical properties and current carrying capacity after roller welding.
[0071] In combination with the above, the present application further provides a method for welding a pole piece 1000 on another aspect, which is applied to the pole piece 1000, wherein the pole piece 1000 includes: a current collector 100, a first transfer layer 200, a second transfer layer 300 and a pole ear, and the method includes: arranging the first transfer layer 200 and the second transfer layer 300 on both sides of the current collector 100; welding one end of the first transfer layer 200 and / or one end of the second transfer layer 300 to the current collector 100 by roller welding; welding the other end of the first transfer layer 200 and / or the other end of the second transfer layer 300 to the pole ear by ultrasonic welding or spot welding.
[0072] In a second aspect, the present application further provides a battery cell, the battery cell comprising an electrode assembly, and the electrode assembly comprises the above-mentioned electrode sheet 1000 .
[0073] In a third aspect, the present application also provides an electrical device, which includes a battery cell.
[0074] In an embodiment of the present application, a pole piece 1000 is provided, and the pole piece 1000 includes a current collector 100, a first transfer layer 200, and a second transfer layer 300. In addition, the pole piece 1000 is provided with a welding portion 400. The current collector 100 includes a first metal layer 110, a support layer 120, and a second metal layer 130 arranged along a first direction X. The first transfer layer 200 is connected to a side of the first metal layer 110 that is away from the support layer 120. The second transfer layer 300 is connected to a side of the second metal layer 130 that is away from the support layer 120. The welding part 400 is located at the connection between the first transfer layer 200 and the first metal layer 110, and the welding part 400 is located at the connection between the second transfer layer 300 and the second metal layer 130. Along the first direction X, on one side of the first transfer layer 200, the welding part 400 is embedded in the support layer 120 with a thickness of D1, and on one side of the second transfer layer 300, the welding part 400 is embedded in the support layer 120 with a thickness of D2, and the thickness of the support layer 120 is H1; the ratio of D1 and D2 to the thickness of the support layer 120 satisfies: 0.1≤(D1+D2) / H1≤0.8. The welding part 400 is provided so that the first transfer layer 200 and the second transfer layer 300 can be welded to the current collector 100, wherein the first transfer layer 200 is welded to the first metal layer 110 of the current collector 100, and the second transfer layer 300 is welded to the second metal layer 130 of the current collector 100, so as to facilitate fusion. Among them, the welding part 400 obtained after welding the pole piece 1000 will be embedded toward the supporting layer 120, and the thickness of the welding part 400 embedded in the supporting layer 120 is further optimized so that the thickness of the welding part 400 embedded in the supporting layer 120 from both sides of the supporting layer 120 and the thickness of the supporting layer 120 itself satisfy: 0.1≤(D1+D2) / H1≤0.8, thereby reducing the cold welding phenomenon caused by the welding part 400 being embedded too little in the supporting layer 120 when the ratio of the thickness of the welding part 400 embedded in the supporting layer 120 is less than 0.1, reducing the influence of weak welding on the pole piece 1000, or reducing the over-welding phenomenon caused by the welding part 400 being embedded too much in the supporting layer 120 when the ratio of the thickness of the welding part 400 embedded in the supporting layer 120 is greater than 0.8, reducing the influence of the over-welding phenomenon on the mechanical properties of the supporting layer 120 on the pole piece 1000.
[0075] Based on the same inventive concept, the present application also provides a battery cell, which includes an electrode assembly, and the electrode assembly includes a pole piece 1000. The pole piece 1000 has the same structure and effect as the pole piece 1000 mentioned above, and will not be described in detail here.
[0076] Based on the same inventive concept, the present application also provides an electrical device, which includes a battery cell. The battery cell has the same structure and effect as the battery cell described above, and will not be described in detail here.
[0077] It should be noted that the preferred embodiments of the present application are given in the specification and drawings of the present application. However, the present application can be implemented in many different forms and is not limited to the embodiments described in the specification. These embodiments are not used as additional limitations on the content of the present application. The purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive. In addition, the above-mentioned technical features continue to be combined with each other to form various embodiments not listed above, which are all regarded as the scope of the description of the present application; further, for ordinary technicians in this field, they can be improved or transformed according to the above description, and all these improvements and transformations should belong to the scope of protection of the claims attached to the present application.
Claims
1. A pole piece, It is characterized in that The pole piece comprises: A current collector, the current collector comprising a first metal layer, a support layer, and a second metal layer arranged along a first direction; A first transfer layer connected to a side of the first metal layer facing away from the support layer; a second transfer layer connected to a side of the second metal layer facing away from the support layer; The pole piece is further provided with a welding portion, the welding portion is located at the connection between the first transfer layer and the first metal layer, and the welding portion is located at the connection between the second transfer layer and the second metal layer. Along the first direction, on one side of the first transfer layer, the welding portion is embedded in the support layer with a thickness of D1, and on one side of the second transfer layer, the welding portion is embedded in the support layer with a thickness of D2, and the thickness of the support layer is H1; The ratio of D1 and D2 to the thickness of the support layer satisfies: 0.1≤(D1+D2) / H1≤0.8, D1 / H1≥0.05, D2 / H1≥0.
05.
2. The pole piece according to claim 1, It is characterized in that Along the first direction, the ratio of D1 and D2 to the thickness of the support layer satisfies: 0.4≤(D1+D2) / H1≤0.
6.
3. The pole piece according to claim 1, It is characterized in that The thickness of the support layer along the first direction is H1, the thickness of the first metal layer along the first direction is H2, and the thickness of the second metal layer along the first direction is H3; 4μm≤H1≤18.4μm, 0.8μm≤H2≤3μm, 0.8μm≤H3≤3μm; And 6.5μm≤H1+H2+H3≤20μm.
4. The pole piece according to claim 3, It is characterized in that Along the first direction, the support layer, the first metal layer and the second metal layer satisfy: 13 μm≤H1≤16 μm, 1 μm≤H2≤3 μm, 1 μm≤H3≤3 μm.
5. The pole piece according to claim 1, It is characterized in that Along the first direction, the thickness of the first transfer layer is Z1, 8 μm≤Z1≤20 μm; The thickness of the second transfer layer is Z2, 8 μm≤Z2≤20 μm.
6. The pole piece according to claim 5, It is characterized in that The width of the first transfer layer is Z3, 10mm≤Z3≤20mm; The width of the second transfer layer is Z4, 10mm≤Z4≤20mm.
7. The pole piece according to claim 1, It is characterized in that The welding portion is provided with a plurality of welding feet, and the plurality of welding feet are arranged at intervals in a dotted manner in the region of the welding portion; The ratio of the area of the weld foot portion to the area of the weld portion is B, and 0.3≤B≤0.
7.
8. The pole piece according to claim 7, It is characterized in that Along the second direction, the width D3 of the solder foot portion satisfies: 10 μm≤D3≤50 μm; The second direction is perpendicular to the first direction and extends along the length of the current collector.
9. The pole piece according to any one of claims 1 to 8, It is characterized in that The projection of the first transfer layer along the first direction at least partially overlaps with the current collector, the projection of the second transfer layer along the first direction at least partially overlaps with the current collector, and the welding portion is located in the overlapping area of the projections of the first transfer layer, the current collector and the second transfer layer.
10. The pole piece according to claim 9, It is characterized in that Along the first direction, the thickness of the overlapping portion of the welding portion, the first transfer layer, the current collector, and the second transfer layer is A1; the thickness of the overlapping portion of the first transfer layer, the current collector, and the second transfer layer is A2; The difference between A1 and A2 is: 10μm≤A1-A2≤30μm.
11. The pole piece according to claim 10, It is characterized in that Along the first direction, the current collector is provided with an empty foil area in the region where the projections of the first switching layer and the second switching layer overlap, and the empty foil area is used for welding the first switching layer and / or the second switching layer.
12. The pole piece according to claim 11, It is characterized in that Along the second direction, the length of the empty foil area is K1, 1mm≤K1≤5mm; The second direction is perpendicular to the first direction and extends along the length of the current collector.
13. The pole piece according to claim 12, It is characterized in that Along the second direction, the length of the empty foil area is K1, 2.5 mm≤K1≤3.5 mm.
14. The pole piece according to any one of claims 1 to 8, It is characterized in that The material of the support layer includes polypropylene, polyethylene, polyurethane, polyethylene terephthalate, etc.
15. A battery cell, It is characterized in that It comprises an electrode assembly, wherein the electrode assembly comprises a pole piece as claimed in any one of claims 1 to 14.
16. An electrical device, It is characterized in that Comprising the battery cell as claimed in claim 15.
Citation Information
Patent Citations
Battery tab welding structure and preparation method thereof and battery
CN111435727A
Pole piece and secondary battery
CN117832392A
Composite current collector, preparation method, and lithium ion battery
US20230378477A1
Plate and battery
WO2023088434A1
Cited By
Electrode sheet, battery cell, and electric device
WO2026012356A1