Composite membrane unit, preparation method thereof, battery cell and all-solid-state battery

By designing composite diaphragm units, using microwave pretreatment and thermal cladding technology, the problem of poor adhesion of solid-state battery electrode sheets is solved, the electrochemical performance and cycle stability of the battery are improved, and the battery capacity and safety are achieved. sex.

CN118943461AActive Publication Date: 2024-11-12ZHUHAI KECHUANG LITHIUM BATTERY TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411035078.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-22
Filing Date
2024-07-30
Publication Date
2024-11-12
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

In the prior art, poor compatibility and coordination of solid interfaces in all-solid-state battery cells lead to poor electrical performance and poor cycle stability.

Method used

Design a composite diaphragm unit, including a positive electrode diaphragm, an electrolyte diaphragm and an anode diaphragm arranged in sequence, to ensure good contact compatibility and stability between the diaphragms through microwave pretreatment and thermal cladding machine. Specific parameters include the thickness of the positive electrode diaphragm ~ 2 mm, the thickness of the electrolyte diaphragm ~ 50 μm, the thickness of the negative electrode diaphragm 25 μm ~ 1 mm, the mass fraction of the active material and the solid electrolyte are 95 ~ 97%, respectively, and added to the diaphragm Polytetrafluoroethylene and SP conductive agents.

Benefits of technology

It achieves good adhesion of solid-state battery electrode sheets, improves ion conduction performance, extends the cycle life of the battery, and improves the electrochemical performance and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943461A_ABST
    Figure CN118943461A_ABST
Patent Text Reader

Abstract

The invention provides a composite membrane unit, a preparation method thereof, a battery cell and an all-solid-state battery. The composite membrane unit comprises a positive electrode membrane, an electrolyte membrane and a negative electrode membrane which are sequentially stacked, the positive electrode membrane comprises a positive electrode active material, the electrolyte membrane comprises a solid electrolyte, and the negative electrode membrane comprises a negative electrode active material; the thickness of the positive electrode membrane is 50 microns to 2 mm, the thickness of the electrolyte membrane is 5 microns to 50 microns, and the thickness of the negative electrode membrane is 25 microns to 1 mm. According to the invention, an integral membrane unit which simultaneously comprises the positive electrode membrane, the electrolyte membrane and the negative electrode membrane with specific thicknesses is designed, so that the problem that the adhesion of materials cannot be well realized by secondary coating in the preparation process of the electrode plate of the solid-state battery is effectively solved; therefore, the problems that the gap of a solid-solid interface is too large, the ion conducting performance is difficult to improve, the battery capacity is low and the circularity is poor are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of solid-state batteries, and in particular to a composite diaphragm unit, a preparation method thereof, a battery cell and an all-solid-state battery. Background Art

[0002] As a new generation of battery technology, solid-state batteries have higher energy density, better safety performance and longer service life, and are the safest development direction of future battery technology.

[0003] However, in the preparation process of solid-state batteries, the prior art usually coats the solid electrolyte on the positive electrode sheet or the negative electrode sheet to form a battery cell. However, this wet coating method cannot achieve the adhesion of the material well, resulting in too large a gap at the solid-solid interface, making it difficult to improve the ion conductivity of the solid-solid interface and unable to effectively exert the battery capacity. Chinese patent CN 218274694U discloses a dry composite electrode sheet, which includes a diaphragm unit, and the active material in the diaphragm unit includes a positive electrode active material or a negative electrode active material. The diaphragm unit is arranged on the surface of the current collector to obtain a positive electrode sheet or a negative electrode sheet to solve the technical problem that it is difficult to compound multiple active materials in wet electrode technology. However, when the diaphragm unit provided by the patent is used in a solid-state battery, if a battery cell is to be obtained, the solid electrolyte membrane layer needs to be further compounded, and the corresponding problem of poor solid-solid interface fusion still exists.

[0004] Based on this, how to provide a composite membrane unit and its corresponding preparation method to make the compatibility and coordination of multiple solid-solid interfaces in the all-solid-state battery cell structure better, thereby effectively improving the electrical performance and stability of the final all-solid-state battery, is one of the important technical problems that need to be solved in this field. Summary of the invention

[0005] The main purpose of the present invention is to provide a composite diaphragm unit, a preparation method thereof, a battery cell and a solid-state battery, so as to solve the problem of poor solid-solid interface compatibility and coordination in all-solid-state battery cells in the prior art, which leads to poor electrical performance and poor cycle stability of the all-solid-state battery.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a composite membrane unit, which includes a positive electrode membrane, an electrolyte membrane and a negative electrode membrane stacked in sequence, wherein: the positive electrode membrane includes a positive electrode active material, the electrolyte membrane includes a solid electrolyte, and the negative electrode membrane includes a negative electrode active material; the thickness of the positive electrode membrane is 50μm~2mm, the thickness of the electrolyte membrane is 5μm~50μm, and the thickness of the negative electrode membrane is 25μm~1mm.

[0007] Furthermore, based on the weight of the positive electrode membrane as 100%, the mass fraction of the positive electrode active material is 95-97%, based on the weight of the electrolyte membrane as 100%, the mass fraction of the solid electrolyte is 95-97%, and based on the weight of the negative electrode membrane as 100%, the mass fraction of the negative electrode active material is 95-97%.

[0008] Furthermore, the positive electrode active material is selected from one or more of lithium iron phosphate, sodium iron pyrophosphate and sodium vanadium phosphate; and / or the solid electrolyte is selected from one or more of lithium squarate, lithium nickelate, lithium cobaltate and lithium ferrate; and / or the negative electrode active material is selected from one or more of graphite, hard carbon, silicon carbon and carbon-coated graphite.

[0009] Furthermore, the positive electrode membrane, the electrolyte membrane and the negative electrode membrane each independently further include polytetrafluoroethylene and / or SP conductive agent.

[0010] The second aspect of the present invention provides a method for preparing a composite membrane unit, comprising the following steps: membrane preparation: preparing a first positive electrode membrane including a positive electrode active material, a first electrolyte membrane including a solid electrolyte, and a first negative electrode membrane including a negative electrode active material; membrane pretreatment: performing microwave pretreatment on the first positive electrode membrane, the first electrolyte membrane, and the second negative electrode membrane, respectively, to obtain a second positive electrode membrane, a second electrolyte membrane, and a second negative electrode membrane, respectively; membrane lamination: using a hot laminating machine, laminating the second positive electrode membrane, the second electrolyte membrane, and the second negative electrode membrane in a sequentially stacked manner to obtain the composite membrane unit.

[0011] Furthermore, the microwave pretreatment conditions for the first positive electrode membrane, the first electrolyte membrane and the second negative electrode membrane are independently: power 50-100 W, time 5-10 min.

[0012] Furthermore, the temperature of the thermal laminating machine is set to 70° C. to 200° C., and the laminating pressure is set to 30T to 200T.

[0013] Furthermore, during the lamination process, the roller gap of the thermal laminating machine is set to 5 μm to 2 mm, and the feeding speed is 5 m / s to 70 m / s.

[0014] A third aspect of the present invention provides a battery cell, comprising a positive electrode current collector, a negative electrode current collector and a diaphragm unit, wherein the diaphragm unit is the above-mentioned diaphragm unit.

[0015] A fourth aspect of the present invention provides an all-solid-state battery comprising the above-mentioned battery cell.

[0016] By applying the technical solution of the present invention, an integral membrane unit including a positive electrode membrane, an electrolyte membrane and a negative electrode membrane of a specific thickness is designed, thereby effectively solving the problem that the secondary coating in the preparation process of solid-state battery electrode sheets cannot achieve good adhesion of the materials, which leads to excessive gaps at the solid-solid interface, difficulty in improving the ion conductivity performance, low battery capacity and poor cyclability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0018] Figure 1 It is a schematic diagram of the structure of the composite diaphragm unit in this application;

[0019] Figure 2 It is a working schematic diagram of the heat laminating machine in this application;

[0020] Figure 3 It is a schematic diagram of the structure of the battery cell in this application.

[0021] The above drawings include the following reference numerals:

[0022] 10. Positive electrode membrane; 20. Electrolyte membrane; 30. Negative electrode membrane. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0024] As described in the background technology, the prior art has the problem that the solid-solid interface compatibility and coordination in the all-solid-state battery core are poor, which leads to poor electrical performance and poor cycle stability of the all-solid-state battery. In order to solve the above technical problems, the first aspect of the present invention provides a composite membrane unit, such as Figure 1 As shown, the composite membrane unit includes a positive electrode membrane 10, an electrolyte membrane 20 and a negative electrode membrane 30 which are stacked in sequence, wherein: the positive electrode membrane 10 includes a positive electrode active material, the electrolyte membrane 20 includes a solid electrolyte, and the negative electrode membrane 30 includes a negative electrode active material; the thickness of the positive electrode membrane 10 is 50μm to 2mm, the thickness of the electrolyte membrane 20 is 5μm to 50μm, and the thickness of the negative electrode membrane 30 is 25μm to 1mm.

[0025] The membrane unit provided by the present invention includes a positive electrode membrane 10, an electrolyte membrane 20 and a negative electrode membrane 30. There is good contact compatibility between the three membranes, thereby avoiding the problem of poor solid-solid interface coordination and easy detachment caused by secondary coating of active slurry in the prior art. The obtained membrane unit structure has good stability, exhibits excellent electrochemical performance and long cycle life, is easy to industrialize, and has high safety. In particular, the present invention also strictly controls the thickness. Within the above-mentioned thickness range, the three membranes in the obtained membrane unit structure can not only achieve good and stable compounding, but also ensure that the membrane unit exhibits excellent electrochemical performance.

[0026] Furthermore, for the above-mentioned membrane unit provided by the present invention, in order to further improve its electrochemical performance, it is preferred that the mass fraction of the positive electrode active material is 95-97% based on the weight of the positive electrode membrane 10 being 100%, the mass fraction of the solid electrolyte is 95-97% based on the weight of the electrolyte membrane 20 being 100%, and the mass fraction of the negative electrode active material is 95-97% based on the weight of the negative electrode membrane 30 being 100%.

[0027] In several preferred embodiments, the positive electrode active material is selected from one or more of lithium iron phosphate, sodium iron phosphate pyrophosphate and sodium vanadium phosphate; and / or, the solid electrolyte is selected from one or more of lithium quartz, lithium nickelate, lithium cobaltate and lithium ferrate; and / or, the negative electrode active material is selected from one or more of graphite, hard carbon, silicon carbon and carbon-coated graphite. In theory, whether it is the positive electrode active material, the solid electrolyte and the negative electrode active material, they can all be selected from the types commonly used in the art, but for the membrane unit system containing three membranes provided by the present invention, the inventor has selected the above-mentioned specific material types through a large number of experiments, and found that the membrane unit obtained thereby has better electrochemical performance and structural stability.

[0028] In order to further improve various properties of the obtained membrane unit, it is preferred that the positive electrode membrane 10, the electrolyte membrane 20 and the negative electrode membrane 30 each independently further include polytetrafluoroethylene and / or SP conductive agent.

[0029] In a preferred embodiment, the positive electrode membrane 10 includes 97% lithium iron phosphate, 1% PTFE and 2% SP, the electrolyte membrane 20 includes 97% lithium quartz, 1% PTFE and 2% SP, and the negative electrode membrane 30 includes 97% graphite, 1% PTFE and 2% SP. The inventors have selected the membrane unit of this specific component through a large number of experiments, and found that the membranes in the membrane unit have better compatibility and coordination, so the membrane unit as a whole also shows more superior structural stability and higher electrochemical performance.

[0030] The second aspect of the present invention provides a method for preparing a composite membrane unit, comprising the following steps: membrane preparation: preparing a first positive electrode membrane including a positive electrode active material, a first electrolyte membrane including a solid electrolyte, and a first negative electrode membrane including a negative electrode active material; membrane pretreatment: performing microwave pretreatment on the first positive electrode membrane, the first electrolyte membrane, and the second negative electrode membrane, respectively, to obtain a second positive electrode membrane, a second electrolyte membrane, and a second negative electrode membrane, respectively; membrane lamination: using a hot laminating machine, laminating the second positive electrode membrane, the second electrolyte membrane, and the second negative electrode membrane in a sequentially stacked manner to obtain the composite membrane unit.

[0031] With respect to the above-mentioned diaphragm unit, the present invention provides a preparation method thereof, wherein three diaphragms are prepared separately and pre-treated, and then thermally laminated to obtain a diaphragm unit. The method is simple and easy to operate, and can efficiently prepare the required diaphragm unit. In particular, the preparation method provided by the present invention also overcomes the problem that the three dry-process diaphragms cannot be effectively laminated, and effectively realizes the preparation of the overall diaphragm unit through appropriate microwave pre-treatment and thermal lamination.

[0032] In several typical embodiments, in order to improve the compatibility between the three membranes, thereby improving the structural consistency and stability of the resulting membrane unit, and ultimately improving its electrochemical performance, the conditions for microwave pretreatment of the first positive electrode membrane, the first electrolyte membrane, and the second negative electrode membrane are independently: power 50-100 W, time 5-10 min.

[0033] Also, after obtaining the first positive electrode membrane, the first electrolyte membrane and the second negative electrode membrane, in order to achieve lamination between the three, the inventors compared and screened the relevant parameters of the thermal laminating machine through a large number of experiments. In several typical implementations, the temperature of the thermal laminating machine is preferably set to 70°C ~ 200°C, and the laminating pressure is set to 30T ~ 200T. Under these conditions, a membrane unit with a more stable structure and better long-cycle stability is obtained.

[0034] Furthermore, during the lamination process, in order to improve the structural consistency of the membrane unit and reduce the possibility of peeling and detachment, the roll gap of the thermal laminator is preferably set to 5 μm to 2 mm and the feeding speed is 5 m / s to 70 m / s.

[0035] The third aspect of the present invention provides a battery cell, comprising a positive electrode current collector, a negative electrode current collector and a membrane unit, wherein the membrane unit is the above-mentioned membrane unit. The battery cell is a fully solid structure, has a complete and continuous structure, has an extremely low water content, and exhibits good electrical performance and safety stability.

[0036] The fourth aspect of the present invention provides an all-solid-state battery, which includes the above-mentioned battery cell. The obtained all-solid-state battery not only has excellent charge and discharge performance, but also exhibits excellent cycle stability due to its internal cell and even the stable pole piece structure.

[0037] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0038] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0039] Example 1

[0040] 1. Preparation of a composite diaphragm unit:

[0041] (1) Diaphragm preparation and pretreatment:

[0042] (1-1) Positive electrode membrane: A positive electrode active material of lithium iron phosphate is mixed with 97% of lithium iron phosphate, 1% of PTFE and 2% of SP by weight, and a first positive electrode membrane is prepared by stirring premixing, air flow fiberization, oven heating and roller pressing. The first positive electrode membrane is subjected to microwave pretreatment with a power of 100 W and a time of 5 min to obtain a second positive electrode membrane with a thickness of 2 mm;

[0043] (1-2) Electrolyte membrane: solid electrolyte lithium squarate is mixed with 97% of solid electrolyte, 1% of PTFE and 2% of SP by weight, and a first electrolyte membrane is prepared by stirring premixing, air flow fiberization, oven heating and roller pressing to form a membrane; the first electrolyte membrane is subjected to microwave pretreatment with a power of 50 W and a time of 10 min to obtain a second electrolyte membrane with a thickness of 12 μm;

[0044] (1-3) Negative electrode membrane: A mixture of negative electrode active materials including graphite of 97%, PTFE of 1% and SP of 2% was prepared by stirring premixing, air flow fiberization, oven heating and roller pressing to obtain a first negative electrode membrane; the first negative electrode membrane was subjected to microwave pretreatment at a power of 100 W for 5 min to obtain a second negative electrode membrane with a thickness of 1 mm.

[0045] (2) Overlap: Press Figure 1 The positional relationship of the schematic diagram is as follows. The second negative electrode membrane, the second electrolyte membrane, and the second positive electrode membrane are loaded onto the thermal laminating machine. The thermal laminating temperature is set to 120°C, the laminating pressure is set to 50T, the roll gap is set to 3mm, the loading speed is set to 30m / s, and the ... Figure 2The schematic diagram is laminated to obtain a diaphragm unit pole roll; the diaphragm unit pole roll is cut by a cutting machine to obtain a diaphragm unit.

[0046] 2. Preparation of battery cells: Load the membrane unit to the laminating machine, and also load the positive electrode current collector and the negative electrode current collector to the laminating machine; Figure 3 The schematic diagram (i.e., the first layer of positive current collector, the first diaphragm unit, the first layer of negative current collector, the second diaphragm unit, the second layer of positive current collector, the third diaphragm unit, and the second layer of negative current collector are stacked in sequence, and in each diaphragm unit, the positive diaphragm is in direct contact with the positive current collector, and the negative diaphragm is in direct contact with the negative current collector) is stacked in an orderly manner by a robot and then hot-pressed at a temperature of 120°C for 30 seconds to obtain a battery cell.

[0047] Among them, the positive electrode current collector is 12μm carbon-coated aluminum foil, and the negative electrode current collector is 6μm carbon-coated copper foil.

[0048] 3. Preparation of solid-state batteries: The obtained solid-state battery cells are baked, assembled, formed, and divided into capacities to prepare solid-state batteries with a designed capacity of 10Ah.

[0049] Example 2

[0050] 1. Preparation of a composite diaphragm unit:

[0051] The only difference between this embodiment and embodiment 1 is that the content of lithium iron phosphate, an active material, in the positive electrode is changed to 90%, the content of lithium succinate in the solid electrolyte is changed to 98%, and the content of graphite, an active material, in the negative electrode is changed to 90%.

[0052] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0053] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0054] Example 3

[0055] 1. Preparation of a composite diaphragm unit:

[0056] The only difference between this embodiment and embodiment 1 is that the content of lithium iron phosphate, an active material, in the positive electrode is changed to 98%, the content of lithium succinate in the solid electrolyte is changed to 90%, and the content of graphite, an active material, in the negative electrode is changed to 98%.

[0057] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0058] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0059] Example 4

[0060] 1. Preparation of a composite diaphragm unit:

[0061] The difference between this embodiment and embodiment 1 is that the microwave pretreatment conditions for the first positive electrode membrane, the first electrolyte membrane and the first negative electrode membrane are changed to a power of 20 W and a time of 20 min.

[0062] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0063] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0064] Example 5

[0065] 1. Preparation of a composite diaphragm unit:

[0066] The difference between this embodiment and embodiment 1 is that the microwave pretreatment conditions for the first positive electrode membrane, the first electrolyte membrane and the first negative electrode membrane are changed to a power of 120 W and a time of 2 minutes.

[0067] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0068] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0069] Example 6

[0070] 1. Preparation of a composite diaphragm unit:

[0071] The only difference between this embodiment and embodiment 1 is that in the step (2) of laminating, the thermal laminating temperature is set to 60° C. and the laminating pressure is set to 250T.

[0072] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0073] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0074] Example 7

[0075] 1. Preparation of a composite diaphragm unit:

[0076] The only difference between this embodiment and embodiment 1 is that in the step (2) of laminating, the thermal laminating temperature is set to 220° C. and the laminating pressure is set to 25T.

[0077] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0078] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0079] Example 8

[0080] 1. Preparation of a composite diaphragm unit:

[0081] The only difference between this embodiment and embodiment 1 is that in the step (2) of laminating, the feeding speed of the thermal laminating is set to 4 m / s.

[0082] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0083] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0084] Example 9

[0085] 1. Preparation of a composite diaphragm unit:

[0086] The only difference between this embodiment and embodiment 1 is that in the step (2) of laminating, the feeding speed of the thermal laminating is set to 75 m / s.

[0087] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0088] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0089] Example 10

[0090] 1. Preparation of a composite diaphragm unit:

[0091] The only difference between this embodiment and embodiment 1 is that PTFE and SP are not added during the preparation of the positive electrode membrane, the solid electrolyte membrane and the negative electrode membrane.

[0092] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0093] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0094] Comparative Example 1

[0095] Preparation of a liquid battery:

[0096] (1) Preparation of positive electrode sheet: The positive electrode main materials of lithium iron phosphate, PVDF and SP are mixed in a ratio of 95:2.5:2.5 to obtain a positive electrode slurry with a solid content of 30%; the obtained slurry is coated on a 12 μm carbon-coated aluminum foil, which is a positive electrode current collector, by a coating machine, and the positive electrode sheet is obtained after baking and rolling;

[0097] (2) Preparation of negative electrode sheet: The negative electrode main materials graphite, CMC and SP are mixed in a ratio of 95:2.5:2.5 to obtain a negative electrode slurry with a solid content of 30%; the obtained slurry is coated on a 6 μm carbon-coated copper foil, which is a negative electrode current collector, by a coating machine, and the negative electrode sheet is obtained after baking and rolling;

[0098] (3) Preparation of liquid batteries: The obtained positive electrode sheets and negative electrode sheets are cut by a cutting machine to obtain cut electrode sheets; the cut positive and negative electrode sheets and separators are stacked and hot pressed to obtain bare cells; the bare cells are passed through an automated cell assembly production line to obtain cells; the cells are baked, injected, formed, sealed, and divided to obtain liquid batteries. The electrolyte is LiPF6 electrolyte.

[0099] Comparative Example 2

[0100] Preparation of solid-state batteries based on wet process:

[0101] (1) Preparing a positive electrode sheet with an electrolyte coating: first prepare a positive electrode sheet according to the method in Comparative Example 1, then stir solid electrolyte lithium squarate, PVDF, and SP in a ratio of 94:3:3 to obtain an electrolyte slurry with a solid content of 30%; then apply the slurry on the prepared positive electrode sheet through a coating machine, cover it, bake, and roll to obtain a positive electrode sheet with an electrolyte coating;

[0102] (2) Preparation of negative electrode sheet: Prepared in the same manner as in Comparative Example 1;

[0103] (3) Preparation of solid-state batteries: The positive and negative electrode sheets with electrolyte coatings are cut through a cutting machine to obtain cut electrode sheets; the cut electrode sheets are stacked and hot pressed to obtain bare cells; the bare cells are passed through an automated cell assembly production line to obtain solid-state cells; the solid-state cells are passed through an automated formation and capacity separation production line to obtain solid-state batteries.

[0104] Comparative Example 3

[0105] 1. Preparation of a composite diaphragm unit:

[0106] The only difference between this embodiment and embodiment 1 is that the process parameters are changed so that the thickness of the obtained second positive electrode membrane is 40 μm, the thickness of the second solid electrolyte membrane is 4 μm, and the thickness of the second negative electrode membrane is 20 μm.

[0107] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0108] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0109] Comparative Example 4

[0110] 1. Preparation of a composite diaphragm unit:

[0111] The only difference between this embodiment and embodiment 1 is that the process parameters are changed so that the thickness of the obtained second positive electrode membrane is 2.5 mm, the thickness of the second solid electrolyte membrane is 60 μm, and the thickness of the second negative electrode membrane is 1.5 mm.

[0112] 2. Preparation of battery cells: The three membrane units obtained above are prepared into battery cells in the manner of Example 1.

[0113] 3. Preparation of solid-state battery: proceed according to the method in Example 1.

[0114] Test Method

[0115] Pole moisture: Use moisture meter to test the pole.

[0116] Electrode resistivity: The electrode is tested using a four-probe tester.

[0117] The interface after the battery is fully charged: the color of the negative electrode and the number of black spots on it represent defects.

[0118] The first discharge capacity of the battery: using charge and discharge test equipment, adopt 0.01C for formation and separate capacity for testing.

[0119] Battery capacity retention rate: The battery was operated at room temperature of 25 degrees Celsius in a charging and discharging device, and its capacity retention rate was tested after 20 and 100 cycles at a charge and discharge rate of 0.1C.

[0120] Battery puncture safety: When the battery is fully charged, a puncture test is performed using a puncture device.

[0121] The resistivity of the positive and negative electrode sheets obtained in Example 1 and Comparative Example 1 was tested respectively, and the moisture content of the four electrodes was tested after being baked for 6 hours. The results are shown in Table 1.

[0122] The above tests were performed on the batteries obtained in each embodiment and comparative example, and the results are shown in Table 2.

[0123] Table 1

[0124]

[0125] Table 2

[0126]

[0127]

[0128] From the above description, it can be seen that the integral diaphragm unit provided by the above-mentioned embodiments of the present invention effectively solves the problem that the secondary coating in the preparation process of the solid-state battery electrode sheet cannot achieve good adhesion of the material, which in turn leads to excessive gaps at the solid-solid interface, difficulty in improving the ion conductivity performance, low battery capacity and poor cyclability.

[0129] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0130] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A composite diaphragm unit, characterized in that: The composite membrane unit comprises a positive electrode membrane (10), an electrolyte membrane (20) and a negative electrode membrane (30) which are stacked in sequence, wherein: The positive electrode membrane (10) includes a positive electrode active material, the electrolyte membrane (20) includes a solid electrolyte, and the negative electrode membrane (30) includes a negative electrode active material; The thickness of the positive electrode membrane (10) is 50 μm to 2 mm, the thickness of the electrolyte membrane (20) is 5 μm to 50 μm, and the thickness of the negative electrode membrane (30) is 25 μm to 1 mm.

2. The composite diaphragm unit according to claim 1, characterized in that: Taking the weight of the positive electrode membrane (10) as 100%, the mass fraction of the positive electrode active material is 95-97%, taking the weight of the electrolyte membrane (20) as 100%, the mass fraction of the solid electrolyte is 95-97%, and taking the weight of the negative electrode membrane (30) as 100%, the mass fraction of the negative electrode active material is 95-97%.

3. The composite diaphragm unit according to claim 2, characterized in that: The positive electrode active material is selected from one or more of lithium iron phosphate, sodium iron pyrophosphate and sodium vanadium phosphate; and / or, the solid electrolyte is selected from one or more of lithium squarate, lithium nickelate, lithium cobaltate and lithium ferrate; and / or, the negative electrode active material is selected from one or more of graphite, hard carbon, silicon carbon and carbon-coated graphite.

4. The composite membrane unit according to any one of claims 1 to 3, characterized in that: The positive electrode membrane (10), the electrolyte membrane (20) and the negative electrode membrane (30) each independently further include polytetrafluoroethylene and / or SP conductive agent.

5. A method for preparing a composite diaphragm unit, characterized in that: The steps include: Membrane preparation: preparing a first positive electrode membrane including a positive electrode active material, a first electrolyte membrane including a solid electrolyte, and a first negative electrode membrane including a negative electrode active material; Membrane pretreatment: performing microwave pretreatment on the first positive electrode membrane, the first electrolyte membrane and the second negative electrode membrane respectively to obtain a second positive electrode membrane, a second electrolyte membrane and a second negative electrode membrane respectively; Membrane lamination: using a thermal laminating machine, laminating the second positive electrode membrane, the second electrolyte membrane and the second negative electrode membrane in a sequentially stacked manner to obtain the composite membrane unit.

6. The method for preparing the composite diaphragm unit according to claim 5, characterized in that: The microwave pretreatment conditions for the first positive electrode membrane, the first electrolyte membrane and the second negative electrode membrane are independently: power 50-100 W, time 5-10 min.

7. The method for preparing a composite membrane unit according to claim 5 or 6, characterized in that: The temperature of the thermal laminating machine is set to 70° C. to 200° C., and the laminating pressure is set to 30T to 200T.

8. The method for preparing a composite membrane unit according to any one of claims 5 to 7, characterized in that: During the laminating process, the roller gap of the heat laminating machine is set to 5 μm to 2 mm, and the feeding speed is 5 m / s to 70 m / s.

9. A battery cell, comprising a positive electrode current collector, a negative electrode current collector and a membrane unit, characterized in that: The diaphragm unit is the diaphragm unit according to any one of claims 1 to 4.

10. An all-solid-state battery, characterized in that: The all-solid-state battery includes the battery cell according to claim 9.

Citation Information

Patent Citations

  • Solid-state battery and preparation method therefor

    CN107240718A

  • Lithium ion battery electrode plate / solid electrolyte composite membrane, preparation method and application of lithium ion battery electrode plate / solid electrolyte composite membrane in lithium ion battery

    CN114203948A

  • Battery cell preparation method and system, battery cell and battery

    CN114284568A

  • All-solid-state battery cell structure, preparation method thereof and all-solid-state battery cell group

    CN114430072A

  • Solid-state battery and preparation method thereof

    CN116470235A