Separator for electrochemical device and electrochemical device including the same

By forming a porous coating and an electrode adhesion layer on the surface of the porous polymer substrate of the lithium secondary battery separator, the problem of insufficient thermal shrinkage and adhesion of the lithium secondary battery at high temperature is solved, and the heat resistance of the separator is improved and adhesion properties enhance battery safety and performance.

CN118943657APending Publication Date: 2024-11-12LG ENERGY SOLUTION LTD

Patent Information

Application Number
CN202411142437.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-07-07
Filing Date
2021-05-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The partitions of lithium secondary batteries have thermal shrinkage problems under high temperature conditions, which leads to safety hazards. Due to material characteristics, the adhesion between the partition and the electrode is insufficient and easy to separate.

Method used

A porous coating including inorganic particles and binder polymer is formed on the surface of the porous polymer substrate, and an adhesive polymer with good adhesion is coated on the upper surface to form an electrode adhesion layer to enhance the partition plate heat resistance and adhesion properties.

Benefits of technology

High heat resistance and improved electrode adhesion under high temperature conditions are achieved, reducing internal short circuit risk and mechanical performance deterioration, and improving battery safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943657A_ABST
    Figure CN118943657A_ABST
Patent Text Reader

Abstract

The invention relates to a separator for an electrochemical device and an electrochemical device including the same. The present disclosure relates to a separator for an electrochemical device and a lithium secondary battery comprising the same, the separator comprising: a first porous coating layer provided on one surface of a porous polymer substrate, including first inorganic particles and a first binder polymer, and having an interstitial volume pore structure; a second porous coating layer disposed on the other surface of the porous polymer substrate, including second inorganic particles and a second binder polymer, and having a node-line hole structure; and an electrode adhesion layer disposed on an upper surface of the first porous coating layer, and including a third binder polymer. The separator for an electrochemical device according to the present disclosure has high heat resistance and improved adhesion to an electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a Chinese patent application with an application date of May 31, 2021, application number "202180021968.0", and invention name "Separator for an electrochemical device and an electrochemical device comprising the separator". Technical Field

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims the priority of Korean Patent Application No. 10-2020-0065375 filed in Korea on May 29, 2020, and Korean Patent Application No. 10-2020-0083387 filed in Korea on July 7, 2020, the disclosures of which are incorporated herein by reference.

[0004] The present disclosure relates to a separator for an electrochemical device and an electrochemical device including the same. More particularly, the present disclosure relates to a separator for an electrochemical device having high heat resistance and improved adhesion performance and an electrochemical device including the same. Background Art

[0005] In recent years, energy storage technology has received increasing attention. As the application field of energy storage technology has expanded to mobile phones, cameras, laptops and even electric vehicles, the demand for high energy density of electrochemical devices used as power sources for electronic devices has increased. Lithium secondary batteries are the best electrochemical devices to meet the demand, and many studies are being conducted on lithium secondary batteries.

[0006] A lithium secondary battery includes a positive electrode, a negative electrode, an electrolyte solution and a separator. Ensuring the safety of the lithium secondary battery is a challenge in the manufacture and use of the lithium secondary battery.

[0007] In particular, the separator generally uses a polyolefin-based porous polymer substrate, and the polyolefin-based porous polymer substrate exhibits severe thermal shrinkage behavior at high temperatures due to its material characteristics and process characteristics, resulting in safety issues such as internal short circuits.

[0008] In addition, generally, an electrode assembly is formed by stacking a separator and an electrode, and the electrode adhesion of the separator is insufficient due to the material characteristics of the separator, so there is a high possibility that the electrode and the separator are separated from each other.

[0009] To solve these problems, a method has been proposed in which a porous coating layer including inorganic particles and a binder polymer is formed on both surfaces of a porous polymer substrate, and a mixture of a binder polymer having good adhesion to an electrode is coated on the surface of the porous coating layer to form an adhesion layer.

[0010] However, according to this method, the binder polymer of the adhesion layer enters and blocks the pores of the porous coating layer, and a sufficient amount of the binder polymer does not remain on the surface of the porous coating layer to form an adhesion layer sufficient to ensure adhesion properties to the electrode.

[0011] Therefore, the demand for separators having high heat resistance and good adhesion to electrodes remains high. Summary of the invention

[0012] Technical issues

[0013] The present disclosure is directed to providing a separator for an electrochemical device having high heat resistance and improved adhesion performance, and an electrochemical device including the separator.

[0014] Technical Solution

[0015] In order to solve the above-mentioned problems, according to one aspect of the present disclosure, a separator for an electrochemical device according to the following embodiments is provided.

[0016] A first embodiment relates to a separator for an electrochemical device, comprising:

[0017] porous polymer substrate;

[0018] a first porous coating layer disposed on one surface of a porous polymer substrate and comprising first inorganic particles and a first binder polymer disposed on all or part of the surface of the first inorganic particles to connect and hold the first inorganic particles together, wherein interstitial volumes are formed between the first inorganic particles that are in substantial contact with each other and are empty spaces that form pores;

[0019] a second porous coating layer disposed on the other surface of the porous polymer substrate and comprising a plurality of nodes, the nodes comprising second inorganic particles and a second binder polymer coating at least a portion of the surface of the second inorganic particles; and a node connecting portion comprising at least one thread-like filament formed by the second binder polymer of the node, the filament extending from the node and connecting another node, wherein the node connecting portion has a three-dimensional network structure in which a plurality of filaments derived from the second binder polymer cross each other; and

[0020] An electrode adhesion layer is disposed on an upper surface of the first porous coating layer and includes a third binder polymer.

[0021] According to the second embodiment, in the first embodiment, the average particle size of the first inorganic particles may be smaller than the average particle size of the second inorganic particles.

[0022] According to the third embodiment, in the second embodiment, the average particle diameter of the first inorganic particles may be 0.01 to 0.99 times the average particle diameter of the second inorganic particles.

[0023] According to a fourth embodiment, in the second or third embodiment, an average particle diameter of the first inorganic particles may be 10 nm to 800 nm.

[0024] According to a fifth embodiment, in any one of the second to fourth embodiments, the average particle diameter of the second inorganic particles may be 200 nm to 1000 nm.

[0025] According to a sixth embodiment, in any one of the first to fifth embodiments, the average pore diameter of the first porous coating layer may be 40 nm to 150 nm.

[0026] According to a seventh embodiment, in any one of the first to sixth embodiments, the third binder polymer may have a weight average molecular weight of about 250,000 to about 500,000 measured by gel permeation chromatography.

[0027] According to an eighth embodiment, in any one of the first to seventh embodiments, the third binder polymer may have a radius of gyration of 150 nm to 500 nm.

[0028] According to a ninth embodiment, in any one of the first to eighth embodiments, the first binder polymer may include at least one of styrene-butadiene rubber, an acrylic polymer, carboxymethyl cellulose, or polyvinyl alcohol.

[0029] According to a tenth embodiment, in any one of the first to ninth embodiments, the second binder polymer may include at least one of poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene), or poly(vinylidene fluoride-co-trifluoroethylene).

[0030] According to an eleventh embodiment, in any one of the first to tenth embodiments, the third binder polymer may include at least one of poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene), or poly(vinylidene fluoride-co-trifluoroethylene).

[0031] According to the twelfth embodiment, in any one of the first to eleventh embodiments, the separator for an electrochemical device may have a heat shrinkage rate of 20% or less in each of the longitudinal direction (Machine Direction) and the transverse direction (Transverse Direction) when measured after the separator is placed at 150°C for 30 minutes.

[0032] According to a thirteenth embodiment, in any one of the first to twelfth embodiments, the separator for an electrochemical device may have an adhesion strength to an electrode of 70 gf / 25 mm or more.

[0033] In order to solve the above-mentioned problems, according to one aspect of the present disclosure, an electrochemical device of the following embodiments is provided.

[0034] The fourteenth embodiment is directed to an electrochemical device such as a secondary battery, including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is the separator for an electrochemical device according to any one of the first to thirteenth embodiments.

[0035] According to a fifteenth embodiment, in the fourteenth embodiment, the electrochemical device may be a lithium secondary battery.

[0036] Beneficial Effects

[0037] A separator for an electrochemical device according to one embodiment of the present disclosure includes a first porous coating layer having high heat resistance on one surface of a porous polymer substrate and a second porous coating layer having good adhesion on the other surface of the porous polymer substrate, thereby providing high heat resistance and improved adhesion to an electrode.

[0038] The average particle size of the first inorganic particles of the separator for an electrochemical device according to one embodiment of the present disclosure is smaller than the average particle size of the second inorganic particles, thereby providing high heat resistance and improved adhesion to an electrode.

[0039] The separator for an electrochemical device according to one embodiment of the present disclosure may have an electrode adhesion layer on the upper surface of a first porous coating layer having high heat resistance by adjusting the average pore size of the first porous coating layer, the weight average molecular weight of the third binder polymer of the electrode adhesion layer, and / or the radius of gyration of the third binder polymer. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The accompanying drawings illustrate preferred embodiments of the present disclosure, and together with the foregoing disclosure, are used to provide a further understanding of the technical spirit of the present disclosure. However, the present disclosure should not be interpreted as being limited to the accompanying drawings.

[0041] Figure 1 is a schematic diagram of a separator for an electrochemical device according to one embodiment of the present disclosure.

[0042] Figure 2 is a scanning electron microscope (SEM) image of a thin film of the first porous coating layer for a separator for an electrochemical device according to a preferred embodiment of the present disclosure.

[0043] Figure 3 is a SEM image of a thin film of the second porous coating layer for a separator for an electrochemical device according to a preferred embodiment of the present disclosure. DETAILED DESCRIPTION

[0044] Hereinafter, preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms or words used in the specification and the appended claims should not be interpreted as limited to the general and dictionary meanings, but are interpreted based on the meanings and concepts corresponding to the technical aspects of the present disclosure on the basis of the principle that the inventor is allowed to appropriately define the terms to obtain the best interpretation.

[0045] Therefore, the embodiments described herein and the elements shown in the drawings are only the most preferred embodiments of the present disclosure and are not intended to fully describe the technical aspects of the present disclosure. Therefore, it should be understood that various other equivalents and modifications may be made thereto when an application is filed.

[0046] The specific terms used in the following detailed description of the present disclosure are provided for convenience, but are not intended to limit the present disclosure. In the specification, "a surface", "another surface" or "upper surface" refers to the position and direction in the corresponding drawings, and is not limited thereto. These terms include the words listed above, their derivatives and words with similar meanings.

[0047] Throughout the specification, it will be understood that when a layer is referred to as being on "one surface," "the other surface" or "upper surface" of another layer, the layer may be placed in contact with the surface of the other layer and intervening layers may be present.

[0048] Terms such as “first”, “second” and the like are used to distinguish one element from another element, and each element is not limited by the terms.

[0049] According to one aspect of the present disclosure, a separator for an electrochemical device includes:

[0050] porous polymer substrate;

[0051] a first porous coating layer disposed on one surface of a porous polymer substrate and comprising first inorganic particles and a first binder polymer disposed on all or part of the surface of the first inorganic particles to connect and hold the first inorganic particles together, interstitial volumes being formed between the first inorganic particles that are in substantial contact with each other and being empty spaces that form pores;

[0052] a second porous coating layer, the second porous coating layer being disposed on another surface of the porous polymer substrate and comprising: a plurality of nodes, the nodes comprising second inorganic particles and a second binder polymer coating at least a portion of the surface of the second inorganic particles; and a node connecting portion, the node connecting portion comprising at least one filament in the form of a thread formed by the second binder polymer of the node, the filament extending from the node and connecting another node, wherein the node connecting portion has a three-dimensional (3D) network structure in which a plurality of filaments derived from the second binder polymer cross each other; and

[0053] An electrode adhesion layer is disposed on an upper surface of the first porous coating layer and includes a third binder polymer.

[0054] Figure 1 is a schematic diagram of a separator for an electrochemical device according to one embodiment of the present disclosure.

[0055] Reference Figure 1 , a separator 1 for an electrochemical device according to one embodiment of the present disclosure includes a porous polymer substrate 10 .

[0056] In one embodiment of the present disclosure, the porous polymer substrate 10 is not limited to a specific type, and may include any material commonly used in the corresponding technical field for the separator of the electrochemical device without limitation. The porous polymer substrate may be a film including a polymer material, and non-limiting examples of polymer materials may include at least one of polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide or polyethylene naphthalene. In addition, the porous polymer substrate may include a non-woven fabric or a porous polymer film made of the above-mentioned polymer material or a stack of two or more thereof. Specifically, the porous polymer substrate may be any one of the following a) to e):

[0057] a) porous membranes formed by melting and extruding polymers,

[0058] b) a multilayer film formed by stacking the porous film of a) into two or more layers,

[0059] c) nonwoven webs made of filaments obtained by melting / spinning polymers,

[0060] d) a multilayer film formed by stacking the nonwoven web of c) into two or more layers,

[0061] e) A porous film having a multilayer structure comprising at least two of a) to d).

[0062] In one embodiment of the present disclosure, the thickness of the porous polymer substrate 10 may be 5 μm to 50 μm. The thickness range of the porous polymer substrate is not limited to the above range, but when the thickness is within the above range, the mechanical properties of the separator may be prevented from being degraded, damaged, and increased in resistance when the electrochemical device is used. Meanwhile, there is no limitation on the pore size and porosity in the porous polymer substrate, but the pore size may be 0.01 μm to 50 μm, and the porosity may be 10% to 95%.

[0063] Reference Figure 1 , a separator 1 for an electrochemical device according to one embodiment of the present disclosure includes a first porous coating layer 20 on one surface of a porous polymer substrate 10 , the first porous coating layer 20 including first inorganic particles and a first binder polymer.

[0064] The first porous coating layer 20 may be formed by coating a slurry including first inorganic particles and a first binder polymer on one surface of the porous polymer substrate 10 and drying it.

[0065] In the first porous coating layer 20, the first inorganic particles are held together by the first binder polymer that adheres the first inorganic particles to each other (i.e., the first binder polymer connects and holds the first inorganic particles together), and the first porous coating layer 20 and the porous polymer substrate 10 are held bonded to each other by the first binder polymer. The first inorganic particles of the first porous coating layer 20 are substantially in contact with each other in a closely packed structure, and interstitial volumes formed between the first inorganic particles in contact with each other become pores of the first porous coating layer 20.

[0066] The separator having the first porous coating layer 20 has good heat resistance due to the densely packed structure of inorganic particles, but may have poor adhesion to an electrode.

[0067] In one embodiment of the present disclosure, the first porous coating layer 20 may be an aqueous coating layer using an aqueous slurry. The aqueous slurry refers to a slurry using water as a solvent or a dispersion medium for a polymer.

[0068] In a specific embodiment of the present disclosure, the first binder polymer may include at least one of styrene-butadiene rubber, acrylic polymer, carboxymethyl cellulose, or polyvinyl alcohol, but is not limited thereto.

[0069] Specifically, the styrene-butadiene rubber may be dispersed in the dispersion medium in the form of particles. The acrylic polymer may include an acrylic homopolymer consisting only of acrylic monomers, or may include a copolymer of acrylic monomers and another monomer. For example, the acrylic polymer may include a monomer selected from at least one of methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, acrylic acid and methyl methacrylate. The acrylic polymer may include polyacrylic acid or polyacrylate. Polyacrylic acid may be dissolved in a solvent. For example, the first binder polymer may be a mixture of an acrylic copolymer and polyacrylic acid. Polyacrylic acid has high resistance and poor adhesion properties, but has good heat resistance, so when polyacrylic acid is used as the first binder polymer, the separator 1 for an electrochemical device having the first porous coating 20 may have better heat resistance. Since water is used as a solvent or a dispersion medium, these polymers are environmentally friendly, and when forming and drying the first porous coating 20 on one surface of a porous polymer substrate, a very large amount of heat is not required and no additional explosion-proof equipment is required, which makes it easier to form the first porous coating 20.

[0070] In one embodiment of the present disclosure, the thickness of the first porous coating layer 20 may be in the range of 1 μm to 5 μm, or 2 μm to 4 μm, or 2 μm to 3 μm. When the first porous coating layer 20 has the thickness in the above range, the thinning of the separator, the low resistance of the separator, and the high heat resistance can be ensured.

[0071] In one embodiment of the present disclosure, the average pore size of the first porous coating layer 20 may be 40 nm to 150 nm, or 45 nm to 120 nm, or 50 nm to 100 nm. When the average pore size of the first porous coating layer 20 satisfies the above range, the third binder polymer of the electrode adhesion layer can be prevented from penetrating into the pores of the first porous coating layer 20 when forming the electrode adhesion layer as described below, thereby ensuring adhesion to the electrode, and thus the electrode adhesion layer can be easily formed on the upper surface of the first porous coating layer 20. In addition, it is easy to prevent excessive increases in resistance and manufacturing costs of the separator.

[0072] Furthermore, in one embodiment of the present disclosure, the maximum pore size of the first porous coating layer 20 may be 200 nm to 400 nm, or 250 nm to 350 nm.

[0073] In one embodiment of the present disclosure, the average pore size or the maximum pore size of the first porous coating layer 20 may be adjusted according to the average particle size of the first inorganic particles.

[0074] In one embodiment of the present disclosure, the average pore size or the maximum pore size of the first porous coating 20 can be measured by capillary flow porometry. Capillary flow porometry measures the diameter of the smallest pore in the thickness direction. Therefore, in order to measure the average pore size or the maximum pore size of the first porous coating 20 by capillary flow porometry, it is necessary to separate the first porous coating 20 from the porous polymer substrate 10 and wrap the separated first porous coating 20 in a non-woven fabric to support the first porous coating 20. In this case, the average pore size of the non-woven fabric should be much larger than the average pore size of the first porous coating 20.

[0075] In one embodiment of the present disclosure, the porosity of the first porous coating layer 20 may be 45% to 70%, or 50% to 70%, or 55% to 70%. When the first porous coating layer 20 has the above porosity, the third binder polymer may be easily prevented from penetrating into the pores of the first porous coating layer 20.

[0076] The porosity of the first porous coating layer 20 can be measured by subtracting a volume converted by the weight and density of each component of the first porous coating layer 20 from a volume calculated using the thickness, width, and length of the first porous coating layer 20. The porosity of the first porous coating layer 20 can be measured by a 6-point BET method according to a nitrogen adsorption-flow method using a scanning electron microscope (SEM) image, a mercury porosimeter, or a porosimetry analyzer (Bell Japan Inc, Belsorp-IImini).

[0077] Reference Figure 1 The separator 1 for an electrochemical device includes a second porous coating layer 30 located on the other surface of the porous polymer substrate 10, the second porous coating layer 30 including second inorganic particles and a second binder polymer. The second porous coating layer 30 may be formed by coating a slurry including second inorganic particles and a second binder polymer on the other surface of the porous polymer substrate 10, performing phase separation, and drying.

[0078] The second porous coating 30 includes: a node, the node includes a second inorganic particle and a second binder polymer coating at least part of the surface of the second inorganic particle; and a thread-like filament formed by the second binder polymer of the node, wherein at least one filament extends from a node and the filament is arranged in a manner that connects any node to another node. A plurality of filaments derived from the second binder polymer cross each other to form a three-dimensional network structure of a non-woven fabric-like structure, the second inorganic particles are at least partially embedded in the filaments of the second binder polymer within the network structure, and the particles are distributed at a predetermined distance from each other through the filaments. In the present disclosure, the pores of the second porous coating 30 refer to the space formed between the filaments that cross each other. In terms of high porosity, the second inorganic particles can be spaced apart by a distance that is at least equal to or greater than the average diameter range of the second inorganic particles. The diameter of the filament can be smaller than the diameter of the node.

[0079] The second porous coating layer 30 has a unique pore structure of a node-filament composite material, which is different from a pore structure such as a finger-like structure formed by non-solvent diffusion of the second binder polymer or a benard cell formed by opening a portion of the second binder polymer. The separator having the second porous coating layer 30 has good adhesion to the electrode, but may have poor heat resistance.

[0080] In one embodiment of the present disclosure, the second porous coating layer 30 may be an organic coating layer using an organic slurry. The organic slurry refers to a slurry using an organic solvent as a dispersion medium, as opposed to an aqueous slurry using water as a solvent or dispersion medium for a polymer.

[0081] In a specific embodiment of the present disclosure, the second binder polymer may be a poly(vinylidene fluoride)-based copolymer. Specifically, the second binder polymer may include at least one of poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene), or poly(vinylidene fluoride-co-trifluoroethylene). For example, when the second binder polymer includes poly(vinylidene fluoride-co-hexafluoropropylene) or poly(vinylidene fluoride-co-tetrafluoroethylene), optimal results can be obtained. These polymers have good adhesion, so the separator for an electrochemical device having a second porous coating 30 is easy to have good adhesion with the electrode.

[0082] In one embodiment of the present disclosure, the thickness of the second porous coating layer 30 may be 0.5 μm to 5 μm, or 1 μm to 4 μm, or 3 μm to 4 μm. When the second porous coating layer 30 has a thickness in the above range, adhesion to the electrode is good, and as a result, the battery strength of the battery can be increased. In addition, it may be advantageous in terms of the cycle characteristics and resistance characteristics of the battery.

[0083] In one embodiment of the present disclosure, the average pore size of the second porous coating 30 may be 50 nm to 2,000 nm, or 100 nm to 900 nm. In one embodiment of the present disclosure, the average pore size of the second porous coating 30 may be measured by capillary flow porometry. Capillary flow porometry measures the diameter of the smallest pore in the thickness direction. Therefore, in order to measure the average pore size of the second porous coating 30 by capillary flow porometry, it is necessary to separate the second porous coating 30 from the porous polymer substrate 10, and wrap the separated second porous coating 30 in a non-woven fabric to support the second porous coating 30, in which case the average pore size of the non-woven fabric should be much larger than the average pore size of the second porous coating 30.

[0084] In one embodiment of the present disclosure, the porosity of the second porous coating layer 30 may be 40% to 85%, or 50% to 75%. When the average pore size of the second porous coating layer 30 is within the above range, the dynamic characteristics of the pressing process that can withstand adhesion to the electrode can be easily ensured, the surface porosity does not increase too much, and it may be suitable for ensuring adhesion to the electrode. In addition, when the porosity of the second porous coating layer 30 is within the above range, it is generally higher than the porosity of the porous polymer substrate 10, thereby providing an ion permeability advantage.

[0085] The porosity of the second porous coating layer 30 can be measured by subtracting a volume converted by the weight and density of each component of the second porous coating layer 30 from a volume calculated using the thickness, width, and length of the second porous coating layer 30. The porosity of the second porous coating layer 30 can be measured by a 6-point BET method according to a nitrogen adsorption-flow method using a scanning electron microscope (SEM) image, a mercury porosimeter, or a porosimetry analyzer (Bell Japan Inc, Belsorp-IImini).

[0086] The first inorganic particle or the second inorganic particle may include, but is not limited to, any type of electrochemically stable inorganic particle. That is, the first inorganic particle and / or the second inorganic particle may include, but is not limited to, any type of inorganic particle that does not cause oxidation and / or reduction reactions within the operating voltage range of the applied electrochemical device (e.g., 0 to 5 V versus Li / Li+). Specifically, using inorganic particles capable of transporting ions as the first inorganic particle and / or the second inorganic particle can increase the ionic conductivity in the electrochemical device, thereby contributing to performance improvement. In addition, using inorganic particles with a high dielectric constant as the first inorganic particle and / or the second inorganic particle can help increase the degree of dissociation of electrolyte salts (such as lithium salts) in the liquid electrolyte, thereby increasing the ionic conductivity of the electrolyte solution.

[0087] For the above reasons, the first inorganic particle and / or the second inorganic particle may include high dielectric constant inorganic particles having a dielectric constant of 5 or greater, or 10 or greater. Non-limiting examples of inorganic particles having a dielectric constant of 5 or greater may include BaTiO3, BaSO4, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3 (PLZT, 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O3 - PbTiO3 (PMN - PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, Y2O3, SiO2, Al2O3, γ - AlOOH, Al(OH)3, SiC, or TiO2, or at least one of them.

[0088] The first inorganic particle and / or the second inorganic particle may include inorganic particles capable of transporting lithium ions or a mixture thereof. That is, inorganic particles containing lithium but not storing lithium and having the function of moving lithium ions can be used. Non-limiting examples of inorganic particles capable of transporting lithium ions may include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), (LiAlTiP) x O y -based glass such as 14Li2O - 9Al2O3 - 38TiO2 - 39P2O5 (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li xLa y TiO3, where 0 < x < 2 and 0 < y < 3), such as Li 3.25 Ge 0.25 P 0.75 S4 lithium thiophosphate germanate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), such as lithium nitride (Li x N y , where 0 < x < 4 and 0 < y < 2), such as SiS2-based glass (Li x Si y S z , where 0 < x < 3, 0 < y < 2, 0 < z < 4), or P2S5-based glass (Li x P y S z , where 0 < x < 3, 0 < y < 3, 0 < z < 7), or at least one of the above. When high dielectric constant inorganic particles and inorganic particles capable of transporting lithium ions are used in combination, their synergistic effect can be amplified.

[0089] In one embodiment of the present disclosure, the average particle size of the first inorganic particles may be smaller than the average particle size of the second inorganic particles. Since the average particle size of the first inorganic particles is smaller, the first inorganic particles can be denser per unit volume, thereby improving heat resistance. At the same time, the adhesion of the second porous coating to the electrode can be easily ensured.

[0090] In one embodiment of the present disclosure, the average particle size of the first inorganic particles may be 0.01 times to 0.99 times, or 0.03 times to 0.9 times, or 0.1 times to 0.5 times the average particle size of the second inorganic particles. If the average particle size of the first inorganic particles is within the above range, the first inorganic particles can be denser per unit volume, so better heat resistance can be provided, and the adhesion of the second porous coating to the electrode can be easily ensured.

[0091] In one embodiment of the present disclosure, the average particle size of the first inorganic particles may be 10 nm to 800 nm, or 15 nm to 600 nm, or 20 nm to 400 nm, or 20 nm to 200 nm. For example, the average particle size of the first inorganic particles may be smaller than the average particle size of the second inorganic particles, and the average particle size of the first inorganic particles may be 10 nm to 800 nm, or 15 nm to 600 nm, or 20 nm to 400 nm, or 20 nm to 200 nm.

[0092] In one embodiment of the present disclosure, the average particle size of the second inorganic particles may be 200nm to 1000nm, or 200nm to 400nm, or 400nm to 900nm, or 500nm to 800nm. For example, the average particle size of the first inorganic particles may be smaller than the average particle size of the second inorganic particles, and the average particle size of the second inorganic particles may be 200nm to 1000nm, or 400nm to 900nm, or 500nm to 800nm.

[0093] In one embodiment of the present disclosure, the average particle size of the first inorganic particles may be smaller than the average particle size of the second inorganic particles, the average particle size of the first inorganic particles may be 10nm to 800nm, 15nm to 600nm, or 20nm to 400nm, or 20nm to 200nm, and the average particle size of the second inorganic particles may be 200nm to 1000nm, or 200nm to 400nm, or 400nm to 900nm, or 500nm to 800nm. For example, when the average particle size of the first inorganic particles is 200nm, the average particle size of the second inorganic particles may be greater than 200nm, within the range of 200nm to 1000nm.

[0094] In one embodiment of the present disclosure, the average particle size of the first inorganic particles may be smaller than the average particle size of the second inorganic particles, the average particle size of the first inorganic particles may be 10nm to 100nm, or 15nm to 60nm, or 20nm to 40nm, and the average particle size of the second inorganic particles may be 200nm to 1000nm, or 200nm to 400nm, or 400nm to 900nm, or 500nm to 800nm.

[0095] When the average particle size of the first inorganic particles satisfies the above range, the first porous coating layer 20 can have better heat resistance. Specifically, when the average particle size of the first inorganic particles is 800 nm or less, since the size of the first inorganic particles is small, the first inorganic particles can be densely arranged in the first porous coating layer 20. When there is an internal or external change, the densely arranged first inorganic particles in the first porous coating layer 20 can be used to suppress the thermal shrinkage of the separator.

[0096] When the average particle size of the second inorganic particles satisfies the above range, the resistance does not increase and good adhesion can be ensured. Specifically, when the average particle size of the second inorganic particles is 200nm or more, the specific surface area of ​​the second inorganic particles can be prevented from excessively increasing, which makes it easy to prevent the amount of the second binder polymer used to form the second porous coating layer 30 from excessively increasing. Therefore, the resistance of the separator can be easily prevented from rising.

[0097] The average particle size of the first inorganic particles and the second inorganic particles used herein refers to the D50 particle size, and the "D50 particle size" refers to the particle size at 50% in the cumulative particle size distribution. The particle size can be measured using a laser diffraction method. Specifically, after the powder to be measured is dispersed in a dispersion medium and introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), the particle size distribution is calculated by measuring the difference in diffraction patterns according to the particle size when the particles pass through a laser beam. The D50 particle size can be measured by calculating the particle size at 50% in the cumulative particle size distribution in a measuring device.

[0098] Considering the thickness, average pore size and porosity of the first porous coating layer 20 of the present disclosure finally formed, the weight ratio between the first inorganic particles and the first binder polymer included in the slurry for forming the first porous coating layer 20 can be determined. In a specific embodiment of the present disclosure, the weight ratio between the first inorganic particles and the first binder polymer can be 90:10 to 99:1, or 95:5 to 98.5:1.5. When the weight ratio of the first inorganic particles to the first binder polymer is within the above range, it is easy to form a gap volume between the first inorganic particles that are substantially in contact with each other, thereby improving the thermal shrinkage of the separator and improving resistance to foreign impurities. In addition, the average pore size and porosity of the first porous coating layer 20 can be ensured, so that it is easy to form an electrode adhesion layer on the upper surface of the first porous coating layer 20, and it is easy to maintain adhesion between the first inorganic particles, so that it is easy to improve the mechanical properties of the first porous coating layer 20.

[0099] Considering the thickness, average pore size and porosity of the second porous coating layer 30 of the present disclosure finally formed, the weight ratio between the second inorganic particles and the second binder polymer included in the slurry for forming the second porous coating layer 30 can be determined. In a specific embodiment of the present disclosure, the weight ratio between the second inorganic particles and the second binder polymer can be 50:50 to 80:20, or 60:40 to 75:25. When the weight ratio of the second inorganic particles to the second binder polymer is within the above range, a node-line structure is easily formed, the node-line structure comprising: a plurality of nodes, the plurality of nodes comprising the second inorganic particles and the second binder polymer coating at least part of the surface of the second inorganic particles; and a node connecting portion, the node connecting portion comprising at least one filament in the shape of a thread formed by the second binder polymer of the node, the filament extending from the node and connecting another node, wherein the node connecting portion has a three-dimensional network structure, wherein a plurality of filaments derived from the second binder polymer cross each other, thereby improving the close contact between the separator surface and its adjacent electrode. In addition, the average pore size and porosity of the second porous coating layer 30 may be ensured, thereby easily improving final battery performance, and the adhesion between the second inorganic particles may be easily maintained, thereby easily improving the mechanical properties of the second porous coating layer 30 .

[0100] Reference Figure 1 , a separator 1 for an electrochemical device includes an electrode adhesion layer 40 including a third binder polymer on an upper surface of a first porous coating layer 20. The electrode adhesion layer 40 imparts adhesion to the first porous coating layer 20 having good heat resistance but low adhesion to an electrode, so that the surface of the porous polymer substrate having the first porous coating layer 20 is well adhered to the electrode. The electrode adhesion layer 40 may be formed by coating a coating liquid including a third binder polymer on an upper surface of the first porous coating layer 20, performing phase separation, and drying.

[0101] In one embodiment of the present disclosure, the third binder polymer may have a weight average molecular weight measured by gel permeation chromatography (GPC) of 250,000 to 500,000, or 270,000 to 450,000, or 250,000 to 400,000.

[0102] The weight average molecular weight was measured by gel permeation chromatography (GPC: gel permeation chromatography, PLGPC220, Agilent Technologies) under the following conditions:

[0103] -Chromatographic column: PL Olexis (Polymer Laboratories)

[0104] -Solvent: TCB (Trichlorobenzene)

[0105] -Flow rate: 1.0ml / min

[0106] -Sample concentration: 1.0mg / ml

[0107] -Injection volume: 200μl

[0108] - Column temperature: 160℃

[0109] -Detector: Agilent High Temperature RI detector

[0110] - Standard: Polystyrene (fit to a cubic polynomial)

[0111] In one embodiment of the present disclosure, the radius of gyration of the third binder polymer of the separator 1 for an electrochemical device may be 150 nm to 500 nm, or 150 nm to 450 nm, or 150 nm to 400 nm.

[0112] In this case, the radius of gyration or radius of gyration of the third binder polymer refers to the average distance from the center of mass of the third binder polymer chain to the break of each polymer chain.

[0113] The radius of gyration of the third binder polymer can be different according to the interaction between the binder polymer and the solvent, and can be different according to the weight average molecular weight of the binder polymer.For example, due to the high molecular weight of the polymer, the main chain length of the polymer is longer, so the radius of gyration of the polymer may increase.In addition, as the degree of solubility of the polymer in the selected solvent is higher, the main chain of the polymer may be untied and the radius of gyration of the polymer may increase.On the contrary, due to the lower solubility of the polymer in the selected solvent, the entanglement tendency of the polymer main chain in the solvent may increase, so even for the polymer of the same molecular weight, its radius of gyration may also be reduced.

[0114] In one embodiment of the present disclosure, the radius of gyration can be measured by a dynamic light scattering (DLS) method. The dynamic light scattering method includes emitting a laser to a polymer, detecting the scattering (Doppler shift) of light with different phases according to the Brownian motion speed of dispersed particles in the polymer, and calculating the radius of gyration distribution of the polymer. For example, the radius of gyration can be measured using an Otsuka DLS-8000.

[0115] When the third binder polymer has a weight average molecular weight and / or a radius of gyration within the above range, the third binder polymer can be more easily prevented from penetrating into the pores of the first porous coating layer 20, and the coating uniformity caused by the excessively high viscosity of the coating liquid including the third binder polymer can be prevented from being reduced. In addition, due to the high elastic modulus of the third binder polymer, when the electrode and the separator are attached by lamination, the problem of insufficient adhesion to the electrode due to the unmodified third binder polymer can be easily prevented.

[0116] In one embodiment of the present disclosure, the third binder polymer may be a poly(vinylidene fluoride)-based copolymer. Specifically, the third binder polymer may include at least one of poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene), or poly(vinylidene fluoride-co-trifluoroethylene). For example, when the third binder polymer includes poly(vinylidene fluoride-co-hexafluoropropylene) or poly(vinylidene fluoride-co-tetrafluoroethylene), optimal results may be obtained. Since these polymers have good adhesion, the separator for an electrochemical device having an electrode adhesion layer 40 can easily ensure excellent adhesion to an electrode.

[0117] In one embodiment of the present disclosure, the thickness of the electrode adhesion layer 40 may be in the range of 0.5 μm to 1.5 μm, or 0.6 μm to 1.2 μm, or 0.6 μm to 1.0 μm. When the electrode adhesion layer 40 has a thickness in the above range, the adhesion to the electrode may be good, and as a result, the battery strength of the battery may be increased. In addition, it may be advantageous in terms of the cycle characteristics and resistance characteristics of the battery.

[0118] In a specific embodiment of the present disclosure, the thickness of the separator 1 may be in the range of 7 μm to 18 μm.

[0119] A separator for an electrochemical device according to an embodiment of the present disclosure has different pore structures in a first porous coating layer disposed on one surface of a porous polymer substrate and a second porous coating layer disposed on the other surface of the porous polymer substrate.

[0120] When a porous coating layer having high heat resistance is formed on both surfaces of a porous polymer substrate as before, and an electrode adhesion layer is formed using an adhesive polymer having good adhesion properties on each surface of the porous coating layer to ensure adhesion to the electrode, the adhesive polymer having good adhesion enters and blocks the pores of the porous coating layer, and a sufficient amount of the adhesive polymer does not remain on the upper surface of the porous coating layer, thereby failing to form an electrode adhesion layer.

[0121] The separator 1 for an electrochemical device according to an embodiment of the present disclosure includes a first porous coating layer 20 on one surface of a porous polymer substrate 10 and a second porous coating layer 30 on another surface of the porous polymer substrate 10, thereby having high heat resistance and improved adhesion to an electrode. Specifically, the separator 1 for an electrochemical device according to an embodiment of the present disclosure may have heat resistance through the first porous coating layer 20, and have adhesion to an electrode through the second porous coating layer 30. The first porous coating layer 20 has high heat resistance but poor adhesion to an electrode, but the separator 1 according to an embodiment of the present disclosure has an electrode adhesion layer 40 including a third binder polymer on an upper surface of the first porous coating layer 20, thereby providing improved adhesion to an electrode.

[0122] The separator for an electrochemical device according to an embodiment of the present disclosure may include an electrode adhesion layer 40 located on the upper surface of the first porous coating layer 20 to prevent the third binder polymer from penetrating into the pores of the first porous coating layer 20 by adjusting the average pore size of the first porous coating layer 20, the weight average molecular weight of the third binder polymer, or the radius of gyration of the third binder polymer.

[0123] For example, the electrode adhesion layer 40 may be formed on the upper surface of the first porous coating layer 20 to prevent the third binder polymer from penetrating into the pores of the first porous coating layer 20 by adjusting the average pore size of the first porous coating layer 20 and the weight average molecular weight of the third binder polymer.

[0124] In addition, the electrode adhesion layer 40 may be formed on the upper surface of the first porous coating layer 20 to prevent the third binder polymer from penetrating into the pores of the first porous coating layer 20 by adjusting the average pore size of the first porous coating layer 20 and the radius of gyration of the third binder polymer.

[0125] In addition, the electrode adhesion layer 40 may be formed on the upper surface of the first porous coating layer 20 to prevent the third binder polymer from penetrating into the pores of the first porous coating layer 20 by simultaneously adjusting the average pore size of the first porous coating layer 20, the weight average molecular weight of the third binder polymer, and the radius of gyration of the third binder polymer.

[0126] In one embodiment of the present disclosure, when the separator for an electrochemical device is placed at 150°C for 30 minutes and measured, the heat shrinkage in each of the longitudinal direction (Machine Direction) and the transverse direction (Transverse Direction) may be 20% or less, or 0% to 20%, or 0% to 10%, or 0% to 5%, or 0% to 3%.

[0127] In one embodiment of the present disclosure, the separator for an electrochemical device may have an adhesion strength to an electrode of 70 gf / 25 mm or more, or 90 gf / 25 mm or more, or 100 gf / 25 mm or more.

[0128] For example, the separator for an electrochemical device may have an adhesion strength with electrodes of 70 gf / 25 mm or more, or 90 gf / 25 mm or more, or 100 gf / 25 mm or more on both surfaces of the separator.

[0129] In one embodiment of the present disclosure, after inserting the separator between 100 μm PET films and allowing the separator to be adhered by a roll laminator, the adhesion to the electrode can be measured by the force required to separate the two separators when force is applied to the adhered separator from two directions at a measuring speed of 300 mm / min.

[0130] For example, two separators are stacked opposite to each other and interposed between 100 μm PET films, and the separators are passed through a roll laminator at 100° C. while being subjected to a pressure of 2 kgf / cm 2 The two separators were adhered by heating at a speed of 0.3 m / min for 30 seconds under a pressure of 0.5 m / min, and the ends of the two adhered separators were installed in a UTM device (LLOYD Instrument LF Plus). Force was applied in two directions at a measuring speed of 300 mm / min. The adhesion of the separator to the electrode can be measured based on the force required to separate the adhered separators.

[0131] The separator for an electrochemical device according to an embodiment of the present disclosure may be manufactured by the following method, but is not limited thereto.

[0132] A method of manufacturing a separator for an electrochemical device according to an embodiment of the present disclosure includes:

[0133] Step (S1): preparing a porous polymer substrate;

[0134] Step (S2): coating a first slurry including first inorganic particles, a first binder polymer and a first solvent on one surface of the porous polymer substrate and drying to form a first porous coating layer;

[0135] Step (S3): coating a second slurry including second inorganic particles, a second binder polymer, and a second solvent on the other surface of the porous polymer substrate;

[0136] Step (S4): coating a coating liquid including a third binder polymer and a third solvent on the upper surface of the first porous coating layer;

[0137] Step (S5): performing phase separation on the result of step (S3) and the result of step (S4) using the first non-solvent and the second non-solvent, respectively; and

[0138] Step (S6): The result of step (S5) is dried to form a second porous coating layer and an electrode adhesion layer.

[0139] Hereinafter, main steps of the manufacturing method will be described.

[0140] First, a porous polymer substrate is prepared. The porous polymer substrate can be used as described above, and can be manufactured by forming pores by a method commonly used in the corresponding technical field, such as a wet method using a solvent, a diluent or a pore-forming agent or a dry method using a stretching process to ensure that the above material has good air permeability and porosity.

[0141] Subsequently, a first slurry including first inorganic particles, a first binder polymer, and a first solvent is coated on one surface of the porous polymer substrate and dried to form a first porous coating layer ( S2 ).

[0142] In a specific embodiment of the present disclosure, for detailed information on the types of the first inorganic particles and the first binder polymer, the average particle size of the first inorganic particles, and the weight ratio between the first inorganic particles and the first binder polymer, refer to the above description.

[0143] The first solvent may be used as a solvent that dissolves the first binder polymer, or a dispersion medium that does not dissolve the first binder polymer and disperses the first binder polymer, depending on the type of the first binder polymer.

[0144] In a specific embodiment of the present disclosure, the first binder polymer may include at least one of styrene-butadiene rubber, acrylic polymer, polyvinyl alcohol or carboxymethyl cellulose. Specifically, styrene-butadiene rubber may be dispersed in the first solvent in the form of particles. Acrylic polymer may include polyacrylic acid and polyacrylate. Polyacrylic acid may be dissolved in the first solvent.

[0145] In a specific embodiment of the present disclosure, the first solvent may include at least one of water, methanol, ethanol or isopropanol. When the first solvent is water, it is environmentally friendly, does not require excessive heat when forming and drying the first porous coating on one surface of the porous polymer substrate, and does not require additional explosion-proof equipment, which makes it easier to form the first porous coating. When the first solvent is water, the first binder polymer may be a binder polymer dissolved or dispersed in water. When the first solvent is water, the substrate may be hydrophilized, or a small amount of surfactant may be added to the first slurry to ensure wettability between the porous polymer substrate and the first slurry.

[0146] The first slurry can be prepared by dissolving or dispersing the first binder polymer in the first solvent and adding and dispersing the first inorganic particles. The first inorganic particles can be added in a pulverized form with a predetermined average particle size, or the first inorganic particles can be added to a solution in which the first binder polymer is dissolved, and then the first inorganic particles can be pulverized and dispersed using a ball milling method while being controlled to have a predetermined average particle size.

[0147] In a specific embodiment of the present disclosure, the first slurry can be coated on one surface of the porous polymer substrate by a predetermined coating method, and non-limiting examples of the coating method may include dip coating, die coating, roll coating, comma coating, blade coating, Mayer rod coating, reverse roll coating and direct roll coating.

[0148] According to a specific embodiment of the present disclosure, the first slurry after coating can be dried by a drying method commonly used in manufacturing a separator. For example, the first slurry coated can be dried by air for 3 to 45 seconds or 5 to 40 seconds. When drying is performed within the above time range, the residual solvent can be removed without reducing the yield.

[0149] In order to ensure heat resistance and adhesion, when a porous coating layer having high heat resistance is formed on both surfaces of a porous polymer substrate, it is impossible to connect the porous polymer substrate having the porous coating layers formed on both surfaces of the porous polymer substrate to another porous polymer substrate, and continuous production cannot be achieved.

[0150] However, when the first porous coating layer is formed only on one surface of the porous polymer substrate, it is easy to connect the porous polymer substrate having the first porous coating layer to another porous polymer substrate having the first porous coating layer on one surface. Therefore, it is easy to continuously form a coating layer on the other surface of the porous polymer substrate having the first porous coating layer on one surface.

[0151] In the first porous coating layer formed as described above, the first inorganic particles are held together by the first binder polymer that adheres the first inorganic particles to each other, and the first inorganic particles and the porous polymer substrate are held in a bonded state by the first binder polymer, and an interstitial volume is formed between the first inorganic particles that are in substantial contact with each other and is an empty space that forms pores of the first porous coating layer.

[0152] Subsequently, a second slurry including second inorganic particles, a second binder polymer, and a second solvent is coated on the other surface of the porous polymer substrate ( S3 ).

[0153] After the first slurry is coated on only one surface of the porous polymer substrate and dried to form a first porous coating layer, a step of coating a second slurry (S3) is performed.

[0154] In a specific embodiment of the present disclosure, for detailed information on the types of the second inorganic particles and the second binder polymer, the average particle diameter of the second inorganic particles, and the weight ratio between the second inorganic particles and the second binder polymer, refer to the above description.

[0155] The second solvent refers to a solvent for the second binder polymer. In a specific embodiment of the present disclosure, the second solvent may include at least one of acetone, tetrahydrofuran, methylene chloride, chloroform, trimethyl phosphate, triethyl phosphate, methyl ethyl ketone (MEK), toluene, hexane, cyclohexane, dimethyl formamide (DMF), dimethyl acetamide (DMAc), or N-methyl-2-pyrrolidone (NMP).

[0156] The second slurry can be prepared by dissolving the second binder polymer in the second solvent and adding and dispersing the second inorganic particles. The second inorganic particles can be added in a pulverized form with a predetermined average particle size, or the second inorganic particles can be added to a solution in which the second binder polymer is dissolved, and then the second inorganic particles can be pulverized and dispersed using a ball milling method while being controlled to have a predetermined average particle size.

[0157] In a specific embodiment of the present disclosure, the second slurry can be coated on the other surface of the porous polymer substrate by a predetermined coating method, and non-limiting examples of the coating method may include dip coating, die coating, roll coating, comma coating, blade coating, Mayer rod coating, reverse roll coating and direct roll coating.

[0158] Subsequently, a coating liquid including a third binder polymer and a third solvent is coated on the upper surface of the first porous coating layer (S4).

[0159] When the coating step (S4) is performed after the second slurry coated on the other surface of the porous polymer substrate is coated and dried to form a second porous coating layer, the coating liquid easily penetrates into the pores of the underlying first porous coating layer, making it difficult to ensure the intended adhesion performance.

[0160] In contrast, the coating step (S4) is performed when the second solvent of the second slurry coated on the other surface of the porous polymer substrate is not dried. Therefore, when the second solvent of the second slurry is not dried, the coating liquid is coated on the upper surface of the first porous coating layer.

[0161] In the process of coating the second slurry on the other surface of the porous polymer substrate, the second solvent of the second slurry penetrates into the pores of the porous polymer substrate. In addition, the second solvent of the second slurry penetrates into the pores of the first porous coating formed on one surface of the porous polymer substrate opposite to the other surface of the porous polymer substrate coated with the second slurry. After the second solvent of the second slurry penetrates into the pores of the first porous coating, an electrode adhesion layer can be formed on the upper surface of the first porous coating to minimize the penetration of the third binder polymer into the pores of the first porous coating when the coating solution including the third binder polymer is coated on the upper surface of the first porous coating, thereby ensuring sufficient adhesion to the electrode.

[0162] In one embodiment of the present disclosure, the solid content of the second slurry may be 15% to 50%, or 20% to 45%. When the solid content of the second slurry satisfies the above range, the probability that the second binder polymer dissolved by the second solvent in the second slurry blocks the pores of the first porous coating layer is very low, so the pores of the first porous coating layer can be easily prevented from being blocked.

[0163] For detailed information on the kind of the third binder polymer and the weight average molecular weight and radius of gyration of the third binder polymer, refer to the above description.

[0164] The third solvent refers to a solvent for the third binder polymer.

[0165] In a specific embodiment of the present disclosure, the third solvent may be at least one of acetone, tetrahydrofuran, methylene chloride, chloroform, trimethyl phosphate, triethyl phosphate, methyl ethylketone (MEK), toluene, hexane, cyclohexane, dimethyl formamide (DMF), dimethyl acetamide (DMAc), or N-methyl-2-pyrrolidone (NMP).

[0166] In a specific embodiment of the present disclosure, the coating liquid can be coated on the upper surface of the first porous coating layer by a predetermined coating method, and non-limiting examples of the coating method may include dip coating, die coating, roll coating, comma coating, blade coating, Mayer rod coating, reverse roll coating, and direct roll coating.

[0167] Subsequently, phase separation (S5) is performed in the resultant of step (S3) and the resultant of step (S4) using the first non-solvent and the second non-solvent, respectively. The phase separation step is a step of phase separation of the coated second slurry and the coating liquid to form a second porous coating layer and an electrode adhesion layer. After the second slurry is coated on the other surface of the porous polymer substrate and the coating liquid is coated on the upper surface of the first porous coating layer, a phase separation process can be performed to form a pore structure in the second porous coating layer and the electrode adhesion layer.

[0168] The first non-solvent refers to a non-solvent for the second binder polymer. In a specific embodiment of the present disclosure, the first non-solvent is not limited to a specific type and may include any non-solvent that does not dissolve the second binder polymer and is partially compatible with the second solvent, specifically, the first non-solvent may include at least one of water, methanol, ethanol, isopropanol, propylalcohol, butylalcohol, butandiol, ethylene glycol, or propylene glycol.

[0169] The first non-solvent may be used to perform phase separation in the second slurry. The phase separation step may use the following methods: a gas-phase induced phase separation method, which includes performing phase separation by condensing the first non-solvent introduced by steam on the surface coated with the second slurry; a non-solvent induced phase separation method, which includes performing phase separation by directly immersing the membrane coated with the second slurry in a tank containing the first non-solvent; a method of spraying the first non-solvent in the form of a gas or droplets on the surface coated with the second slurry; and a method of directly phase separating the coated second slurry. In this case, the direct phase separation method may include performing phase separation by adding the first non-solvent to the second slurry, coating the second slurry on another surface of the porous polymer substrate, and drying. In particular, the non-solvent induced phase separation method may include additionally passing the first non-solvent through a pressing roller after phase separation to minimize the amount of the first non-solvent, thereby reducing the burden in the drying step.

[0170] The gas phase induced phase separation will be described below.

[0171] The gas-phase induced phase separation may include exposing the separator coated with the second slurry on the other surface of the porous polymer substrate to a first non-solvent atmosphere in a gas or droplet state to induce phase separation. In this case, the first non-solvent may be introduced in a gaseous state. When the first non-solvent is introduced in a gaseous state, a small amount of the first non-solvent may be used for phase separation and promote the drying of the second slurry.

[0172] In this case, the temperature at which the first non-solvent in a gaseous or droplet state is added may be in the range of 15° C. to 70° C. When the addition temperature of the gaseous first non-solvent satisfies the above range, the first non-solvent is easily kept in a gaseous state, the drying speed of the second slurry can be ensured, thereby improving the yield, and it is easy to prevent the second solvent and the first non-solvent from being dried too quickly due to insufficient phase separation.

[0173] In addition, phase separation can be performed under the condition that the vapor pressure of the first non-solvent is 40% to 80% or 60% to 75% of the saturated vapor pressure during phase separation. When the vapor pressure of the first non-solvent satisfies the above range, the problem of insufficient phase separation due to too little amount of the first non-solvent or uneven coating due to excessive phase separation can be easily prevented.

[0174] The non-solvent induced phase separation will be described below.

[0175] The second slurry coated on the other surface of the porous polymer substrate can be immersed in a coagulant solution including a first non-solvent for a predetermined time. Therefore, in the coagulant solution, the first non-solvent replaces the second solvent in the second slurry, induces phase separation, and solidification of the second binder polymer occurs. In this process, the second porous coating layer including the second binder polymer and the second inorganic particles becomes porous. Subsequently, the first non-solvent can be replaced by washing with a pure first non-solvent to replace the second solvent remaining in the second porous coating layer, and then the first non-solvent is removed in a drying furnace to form a second porous coating layer on the other surface of the porous polymer substrate.

[0176] The coagulant solution may include a single first non-solvent or a mixed solvent of the first non-solvent and the second solvent as described above. When a mixed solvent of the first non-solvent and the second solvent is used, the amount of the first non-solvent may be 60 wt % or more based on 100 wt % of the coagulant solution in terms of forming a good pore structure and improving productivity.

[0177] According to a specific embodiment of the present disclosure, the second porous coating layer can be dried by a drying method commonly used in manufacturing separators. For example, the second porous coating layer can be dried by air for 3 to 45 seconds or 5 to 40 seconds. When drying is performed within the above time range, the residual solvent can be removed without reducing the yield.

[0178] The second porous coating formed as described above includes: a node, the node includes a second inorganic particle and a second binder polymer, the second binder polymer coats at least part of the surface of the second inorganic particle; and a thread-like filament formed by the second binder polymer of the node, wherein at least one filament extends from a node and the filament is arranged in a manner that any node is connected to another node. Multiple filaments derived from the second binder polymer cross each other to form a three-dimensional network structure of a non-woven fabric-like structure, the second inorganic particle is at least partially embedded in the filaments of the second binder polymer in the network structure, and the particles are distributed at a predetermined distance from each other through the filaments. In addition, pores are formed between the intersecting filaments.

[0179] The second non-solvent refers to a non-solvent for the third binder polymer. In a specific embodiment of the present disclosure, the second non-solvent is not limited to a specific type and may include any non-solvent that does not dissolve the third binder polymer and is partially compatible with the third solvent, specifically, the second non-solvent may include at least one of water, methanol, ethanol, isopropanol, propylalcohol, butylalcohol, butandiol, ethylene glycol, or propylene glycol.

[0180] Phase separation can be performed in the coating liquid using a second non-solvent. The phase separation step can use the following methods: a gas-phase induced phase separation method, which includes performing phase separation by condensing a second non-solvent introduced by steam on a surface coated with the coating liquid; a non-solvent induced phase separation method, which includes performing phase separation by directly immersing a membrane coated with the coating liquid in a tank containing a second non-solvent; a method of spraying a second non-solvent in the form of a gas or droplets on a surface coated with the coating liquid; and a method of directly phase-separating the coated coating liquid. In this case, the direct phase separation method may include performing phase separation by adding a predetermined second non-solvent to the coating liquid, coating the coating liquid on the upper surface of the first porous coating layer, and drying. In particular, the non-solvent induced phase separation method may include additionally passing the second non-solvent through a pressing roller after phase separation to minimize the amount of the second non-solvent, thereby reducing the burden in the drying step.

[0181] The gas phase induced phase separation will be described below.

[0182] The gas-phase induced phase separation may include exposing the separator coated with the coating liquid on the upper surface of the first porous coating layer to a second non-solvent atmosphere in a gas or droplet state to induce phase separation. In this case, the second non-solvent may be introduced in a gaseous state. When the second non-solvent is introduced in a gaseous state, a small amount of the second non-solvent may be used for phase separation and promote the drying of the coating liquid.

[0183] In this case, the temperature at which the second non-solvent in a gas or droplet state is added may be in the range of 15° C. to 70° C. When the addition temperature of the gaseous second non-solvent satisfies the above range, the second non-solvent is easily kept in a gaseous state, the drying speed of the coating liquid can be ensured, thereby improving the yield, and it is easy to prevent insufficient phase separation caused by the third solvent and the second non-solvent being dried too quickly.

[0184] In addition, the phase separation can be performed under the condition that the vapor pressure of the second non-solvent is 40% to 80% or 60% to 75% of the saturated vapor pressure during the phase separation. When the vapor pressure of the second non-solvent satisfies the above range, the problem of insufficient phase separation due to too small an amount of the second non-solvent or uneven coating due to excessive phase separation can be easily prevented.

[0185] The non-solvent induced phase separation will be described below.

[0186] The second slurry coated on the other surface of the porous polymer substrate can be immersed in a coagulant solution including a second non-solvent for a predetermined time. Therefore, in the coagulant solution, the second non-solvent can replace the third solvent in the coating solution, induce phase separation, and solidification of the third binder polymer occurs. In this process, the electrode adhesion layer including the third binder polymer becomes porous. Subsequently, the second non-solvent can be replaced by washing with a pure second non-solvent to replace the third solvent remaining in the electrode adhesion layer, and then the second non-solvent is removed in a drying furnace to form an electrode adhesion layer on the upper surface of the first porous coating.

[0187] The coagulant solution may include a second non-solvent alone or a mixed solvent of the second non-solvent and the third solvent as described above. When a mixed solvent of the second non-solvent and the third solvent is used, the amount of the second non-solvent may be 60 wt % or more based on 100 wt % of the coagulant solution in terms of forming a good pore structure and improving productivity.

[0188] According to a specific embodiment of the present disclosure, the electrode adhesion layer can be dried by a drying method commonly used in manufacturing separators. For example, the electrode adhesion layer can be dried by air for 3 to 45 seconds or 5 to 40 seconds. When the drying time is within the above range, the residual solvent can be removed without reducing the yield.

[0189] The first nonsolvent and the second nonsolvent may be of the same kind, or may be of different kinds.

[0190] In one embodiment of the present disclosure, when the first non-solvent and the second non-solvent are the same non-solvent, under the atmosphere of the second non-solvent (or the first non-solvent), the other surface of the porous polymer substrate coated with the second slurry and the upper surface of the first porous coating layer coated with the coating liquid can be phase-separated simultaneously.

[0191] In addition, in another embodiment of the present disclosure, when the first non-solvent and the second non-solvent are the same non-solvent, phase separation can occur simultaneously by immersing a separator including a porous polymer substrate coated with a second slurry on another surface and a first porous coating layer coated with a coating liquid on an upper surface in a coagulant solution including the second non-solvent (first non-solvent).

[0192] In order to simultaneously ensure heat resistance and adhesion, when a porous coating layer having high heat resistance is formed on both surfaces of a porous polymer substrate, it is impossible to connect the porous polymer substrate having the porous coating layers on both surfaces to another porous polymer substrate, and continuous production cannot be achieved.

[0193] However, the method for manufacturing a separator for an electrochemical device according to an embodiment of the present disclosure forms the first porous coating layer only on one surface of a porous polymer substrate, and therefore it is easy to connect the porous polymer substrate having the first porous coating layer to another porous polymer substrate having the first porous coating layer on one surface, thereby continuously forming a separator.

[0194] Meanwhile, although the specification describes the method for manufacturing a separator for an electrochemical device according to an embodiment of the present disclosure in the order of forming a first porous coating layer, forming a second porous coating layer, and forming an electrode adhesion layer, the separator for an electrochemical device of the present disclosure is not necessarily manufactured in this order.

[0195] A method for manufacturing a separator for an electrochemical device according to another embodiment of the present disclosure can manufacture a separator for an electrochemical device by adjusting the average pore size of the first porous coating layer, the weight average molecular weight of the third binder polymer included in the electrode adhesion layer, and / or the radius of gyration of the third binder polymer.

[0196] The method for manufacturing a separator for an electrochemical device according to another embodiment of the present disclosure can form an electrode adhesion layer on the upper surface of the first porous coating layer with a sufficient adhesion level to the electrode because the third binder polymer is not introduced into the pores of the first porous coating layer having an average pore size of 40 nm to 150 nm. Therefore, after applying and drying the second slurry, the electrode adhesion layer can be formed by applying the coating liquid on the upper surface of the first porous coating layer and drying it.

[0197] Alternatively, the electrode adhesion layer may be formed by applying a coating liquid on the upper surface of the first porous coating layer and drying the coating liquid immediately after the first porous coating layer is formed and before the second slurry is applied.

[0198] In one embodiment of the present disclosure, the average pore size of the first porous coating layer may be adjusted by adjusting the average particle size of the first inorganic particles.

[0199] The method for manufacturing a separator for an electrochemical device according to another embodiment of the present disclosure can form an electrode adhesion layer on the upper surface of the first porous coating layer with a sufficient adhesion level to the electrode because the third binder polymer having a weight average molecular weight of 250,000 to 500,000 measured by gel permeation chromatography is not introduced into the pores of the first porous coating layer. Therefore, after applying and drying the second slurry, the electrode adhesion layer can be formed by applying the coating liquid on the upper surface of the first porous coating layer and drying it.

[0200] Alternatively, the electrode adhesion layer may be formed by applying a coating liquid on the upper surface of the first porous coating layer and drying the coating liquid immediately after the first porous coating layer is formed and before the second slurry is applied.

[0201] The method for manufacturing a separator for an electrochemical device according to another embodiment of the present disclosure can form an electrode adhesion layer on the upper surface of the first porous coating layer with a sufficient adhesion level to the electrode because the third binder polymer having a radius of gyration of 150 nm to 500 nm is not introduced into the pores of the first porous coating layer. Therefore, after applying and drying the second slurry, the electrode adhesion layer can be formed by applying the coating liquid on the upper surface of the first porous coating layer and drying.

[0202] Alternatively, the electrode adhesion layer may be formed by applying the coating liquid on the upper surface of the first porous coating layer and drying the coating liquid immediately after the first porous coating layer is formed and before the second slurry is applied.

[0203] When manufacturing an electrochemical device, the separator for an electrochemical device according to the present disclosure may be placed between a positive electrode and a negative electrode.

[0204] The electrochemical device of the present disclosure may include any type of device using an electrochemical reaction, and specific examples may include primary and secondary batteries, fuel cells, solar cells, or capacitors (e.g., supercapacitors). In secondary batteries, in particular, the electrochemical device may be a lithium secondary battery including a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0205] The electrode used with the separator for an electrochemical device of the present disclosure is not limited to a specific type and may be manufactured by bonding an electrode active material to an electrode current collector by a general method known in the technical field related to the present disclosure.

[0206] Among the electrode active materials, non-limiting examples of positive electrode active materials may include: layered compounds or compounds having one or more transition metals, such as lithium cobalt composite oxide (LiCoO2), lithium nickel oxide (LiNiO2); lithium manganese oxide, such as Li 1+x Mn 2-x O4 (x = 0 ~ 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides, such as LiV3O5, LiV3O4, V2O5, Cu2V2O7; LiNi 1-x M x Ni-site lithium nickel oxide represented by O2 (M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, x = 0.01-0.3); 2-x M x Lithium manganese composite oxides represented by Li2Mn3MO5 (M=Fe, Co, Ni, Cu or Zn); LiMn2O4 in which Li is partially substituted with alkaline earth metal ions; disulfides and Fe2(MoO4)3, but are not limited thereto.

[0207] Non-limiting examples of the negative electrode active material may include any negative electrode active material commonly used in negative electrodes of electrochemical devices, and specifically may include lithium adsorption materials such as lithium metal or lithium alloys, carbon, petroleum coke, activated carbon, graphite, or other carbons.

[0208] Non-limiting examples of the positive electrode current collector may include foil made of aluminum, nickel, or a combination thereof, and non-limiting examples of the negative electrode current collector may include foil made of copper, gold, nickel, or a copper alloy, or a combination thereof.

[0209] In one embodiment of the present disclosure, the conductive material used in the negative electrode and the positive electrode can be added in an amount of 1 wt % to 30 wt % based on the total weight of the active material layer, respectively. When the material has conductivity without causing chemical changes to the corresponding battery, the conductive material is not limited to any specific type, and the conductive material may include the following conductive materials: for example, graphite, such as natural graphite or artificial graphite; carbon black, such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers, such as carbon fibers or metal fibers; fluorocarbons; metal powders, such as aluminum powder and nickel powder; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; polyphenylene derivatives.

[0210] In one embodiment of the present disclosure, the binder for the negative electrode and the positive electrode contributes to the bonding of the active material and the conductive material and the bonding of the active material and the current collector, and can generally be added in an amount of 1% to 30% by weight based on the total weight of the active material layer. Examples of binders may include polyvinylidene fluoride (PVdF), polyacrylic acid (PAA), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber and various copolymers.

[0211] In one embodiment of the present disclosure, the electrochemical device includes an electrolyte solution, and the electrolyte solution may include an organic solvent and a lithium salt. In addition, the electrolyte solution may include an organic solid electrolyte or an inorganic solid electrolyte.

[0212] For example, the organic solvent may include aprotic organic solvents such as N-methyl-2-pyrrolidone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran (franc), 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0213] Lithium salts are materials that are easily soluble in organic solvents, and may include, for example, LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate and imide.

[0214] In addition, in order to improve the charge / discharge characteristics and flame retardancy, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-ethylene glycol dimethyl ether (glyme), hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N, N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol and aluminum chloride can be added to the electrolyte solution. In some cases, halogen-containing solvents such as carbon tetrachloride and trifluoroethylene can be added to impart non-flammability, and carbon dioxide gas can be added to improve high temperature storage characteristics.

[0215] For example, the organic solid electrolyte may include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, agitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymers containing ion dissociative groups.

[0216] For example, the inorganic solid electrolyte may include Li nitrides, halides and sulfates, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, Li3PO4-Li2S-SiS2.

[0217] Depending on the manufacturing process and the desired performance of the final product, the injection of the electrolyte solution can be performed in any suitable step of the battery manufacturing process. That is, the injection of the electrolyte solution can be applied before the battery assembly or in the last step of the battery assembly.

[0218] According to a specific embodiment of the present disclosure, a process of applying a separator for an electrochemical device to a battery may include a commonly used winding process of a separator and an electrode and a lamination, stacking, and folding process.

[0219] According to one specific embodiment of the present disclosure, a separator for an electrochemical device can be interposed between a positive electrode and a negative electrode of the electrochemical device, and when an electrode assembly is constructed by assembling a plurality of batteries or electrodes, the separator can be interposed between adjacent batteries or electrodes. The electrode assembly can have a variety of structures, for example, a simple stacking type, a jelly roll type, a stacking-folding type, and a lamination-stacked type.

[0220] Hereinafter, the present disclosure will be described in detail by way of example to help understand the present disclosure. However, the embodiments of the present disclosure may be modified in many other forms, and the scope of the present disclosure should not be construed as being limited to the following embodiments. The embodiments of the present disclosure are provided to fully explain the present disclosure to those of ordinary skill in the art of the present disclosure.

[0221] Example 1

[0222] The first slurry was prepared by mixing water as a first solvent, boehmite particles (Nabaltec, Actilox200SM, D50=200 nm) as first inorganic particles, and acrylic copolymer (Toyo ink, CSB-130) and carboxymethyl cellulose (GL CHEM, SG-L02) as first binder polymers in a weight ratio of 97:2:1. The solid content of the first slurry was 40%.

[0223] A polyolefin porous film (Senior, SW310H, thickness 9 μm, air permeation time: 93 sec / 100 cc) was prepared as a substrate, and the first slurry was coated on one surface of the polyolefin porous film to prepare a preliminary separator. The thickness of the first porous coating layer obtained by coating and drying the first slurry was 2.5 μm.

[0224] Subsequently, a second slurry was prepared by mixing NMP as a second solvent, alumina particles (Sumitomo, AES11, D50=600 nm) as second inorganic particles, and PVdF-HFP (Solvay, Solef 21510) and PVdF-TFE (Daikin, VT475) as a second binder polymer so that the weight ratio of the second inorganic particles, PVdF-HFP and PVdF-TFE was 65:30:5. The solid content of the second slurry was 25%.

[0225] Subsequently, PVdF-HFP (Solvay, Solef 21510, weight average molecular weight 290,000) as a third binder polymer was dissolved in NMP as a third solvent to prepare a coating liquid having a solid content of 2%. The radius of gyration of the third binder polymer in the coating liquid was 165 nm.

[0226] The second slurry was coated on one surface of the polyolefin porous polymer substrate of the prepared preliminary separator, and then the coating liquid was coated on the surface of the first porous coating layer, and then immersed in a coagulant solution in which the weight ratio of water and NMP was maintained at 6:4 to cause non-solvent induced phase separation. Subsequently, the separator was completed by washing with water several times and drying.

[0227] The total thickness of the manufactured separator was 15.3 μm, and the measured air permeation time was 185 sec / 100 cc. In this case, cross-sectional SEM analysis showed that the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.2 μm, and the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.6 μm.

[0228] Example 2

[0229] A preliminary separator was prepared in the same manner as in Example 1, except that the first inorganic particles were changed to the same alumina particles (Sumitomo, AES11, D50=600 nm) as in the second slurry, and the weight ratio of the composition of the first slurry was adjusted to 97.5:1.5:1.

[0230] In this case, the thickness of the first porous coating layer coated with the first slurry was 2.5 μm.

[0231] The total thickness of the manufactured separator was 15.3 μm, and the measured air permeation time was 174 sec / 100 cc. In this case, cross-sectional SEM analysis showed that the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.2 μm, and the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.6 μm.

[0232] Example 3

[0233] A preliminary separator was prepared in the same manner as in Example 1, except that the first inorganic particles were changed to fumed alumina (Evonik, Alu65, D50=20 nm), and the weight ratio of the composition of the first slurry was adjusted to 95:3:2.

[0234] In this case, the thickness of the first porous coating layer obtained by coating and drying the first slurry was 2.5 μm.

[0235] The total thickness of the manufactured separator was 15.2 μm, and the measured air permeation time was 193 sec / 100 cc. In this case, cross-sectional SEM analysis showed that the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.2 μm, and the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.5 μm.

[0236] Example 4

[0237] A preliminary separator was prepared in the same manner as in Example 1, except that the first inorganic particles were changed to a mixture of fumed alumina (Evonik, Alu65, D50=20 nm) and alumina particles (Sumitomo, AES11, D50=600 nm) in a weight ratio of 15:85.

[0238] In this case, the thickness of the first porous coating layer coated with the first slurry was 2.5 μm.

[0239] The total thickness of the manufactured separator was 15.1 μm, and the measured air permeation time was 183 sec / 100 cc. In this case, cross-sectional SEM analysis showed that the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.1 μm, and the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.5 μm.

[0240] Example 5

[0241] A preliminary separator was prepared in the same manner as in Example 3, except that the second inorganic particles were changed to boehmite particles (Nabaltec, Actilox 200SM, D50=200 nm).

[0242] In this case, the thickness of the first porous coating layer coated with the first slurry was 2.5 μm.

[0243] The total thickness of the manufactured separator was 15.0 μm, and the measured air permeation time was 203 sec / 100 cc. In this case, cross-sectional SEM analysis showed that the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.0 μm, and the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.5 μm.

[0244] Example 6

[0245] A preliminary separator was prepared in the same manner as in Example 3, except that the second inorganic particles were changed to a mixture of boehmite particles (Nabaltec, Actilox200SM, D50 = 200 nm) and fumed alumina (Evonik, Alu65, D50 = 20 nm) in a weight ratio of 1:1 (total D50 of the second inorganic particles = 110 nm). In this case, the thickness of the first porous coating layer coated with the first slurry was 2.5 μm.

[0246] The total thickness of the manufactured separator was 15.1 μm, and the measured air permeation time was 211 sec / 100 cc. In this case, cross-sectional SEM analysis showed that the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.1 μm, and the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.5 μm.

[0247] Example 7

[0248] The first slurry was prepared by mixing water as a first solvent, boehmite particles (Nabaltec, Actilox200SM, D50=200nm) and alumina particles (Evonik, Alu65, D50=20nm) as first inorganic particles in a weight ratio of 50:50, and acrylic copolymer (Toyo ink, CSB-130) and carboxymethyl cellulose (GL CHEM, SG-L02) as first binder polymers so that the weight ratio of the first inorganic particles, the acrylic copolymer and the carboxymethyl cellulose was 97:2:1. The solid content of the first slurry was 40%.

[0249] A polyolefin porous film (Senior, SW310H, thickness 9 μm, air permeation time: 93 sec / 100 cc) was prepared as a substrate, and the first slurry was coated on one surface of the polyolefin porous film to prepare a preliminary separator. The thickness of the first porous coating layer obtained by coating and drying the first slurry was 2.5 μm.

[0250] Subsequently, a second slurry was prepared by mixing N-methyl-2-pyrrolidone (NMP) as a second solvent, alumina particles (Sumitomo, AES11, D50=600 nm) as second inorganic particles, PVdF-HFP (Solvay, Solef 21510) and PVdF-TFE (Daikin, VT475) as a second binder polymer so that the weight ratio of the second inorganic particles, PVdF-HFP and PVdF-TFE was 65:30:5. The solid content of the second slurry was 25%.

[0251] The second slurry was coated on one surface of the polyolefin porous polymer substrate of the prepared preliminary separator, and then immersed in a coagulant solution in which the weight ratio of water and NMP was maintained at 6:4 to cause non-solvent induced phase separation. Subsequently, a second porous coating layer was formed by washing with water several times and drying. In this case, the cross-sectional SEM analysis result of the thickness of the second porous coating layer formed by coating and drying the second slurry was 3.2 μm.

[0252] Subsequently, PVdF-HFP (Solvay, Solef21510, weight average molecular weight 290,000) as the third binder polymer was dissolved in NMP as the third solvent to prepare a coating solution with a solid content of 2%. The radius of gyration of the third binder polymer in the coating solution was 165 nm. The coating solution was coated on the surface of the first porous coating layer and then immersed in a coagulant solution in which the weight ratio of water to NMP was maintained at 6:4 to cause non-solvent induced phase separation. Subsequently, the separator was manufactured by washing with water several times and drying.

[0253] The total thickness of the manufactured separator was 15.3 μm, and the measured air permeation time was 185 sec / 100 cc. The thickness of the electrode adhesion layer formed by coating and drying the coating liquid was 0.6 μm as a result of cross-sectional SEM analysis.

[0254] Comparative Example 1

[0255] The first slurry prepared in Example 1 was coated on both surfaces of a polyolefin substrate and dried to prepare a preliminary separator, and the coating liquid prepared in Example 1 was coated on both surfaces of the preliminary separator, followed by non-solvent induced phase separation to manufacture a separator.

[0256] The total thickness of the first porous coating layer formed in the manufactured preliminary separator was 4.9 μm.

[0257] The total thickness of the manufactured separator was 14.6 μm, and the measured air permeation time was 213 sec / 100 cc. In this case, the thickness of the electrode adhesion layer formed by coating and drying the coating liquid was found to be 0.4 μm and 0.3 μm, respectively, by cross-sectional SEM analysis.

[0258] Comparative Example 2

[0259] The second slurry prepared in Example 1 was coated on both surfaces of a polyolefin substrate and then subjected to non-solvent induced phase separation to manufacture a separator.

[0260] The total thickness of the manufactured separator was 15.0 μm, and the measured air permeation time was 171 sec / 100 cc. In this case, the thickness of the porous coating layer analyzed by cross-sectional SEM was 3.1 μm and 2.9 μm, respectively.

[0261] Test Example 1: Measurement of the average pore size and porosity of the first porous coating layer

[0262] The average pore diameter and porosity of the first porous coating layers of the separators manufactured in Examples 2, 3 and 7 were measured, respectively, and the results are shown in Table 1 below.

[0263] The average pore size of the first porous coating layer was measured by capillary flow porosimetry using PMI iPore-1500AEX.

[0264] The porosity of the first porous coating layer is measured by subtracting a volume converted from the weight and density of each component of the first porous coating layer from a volume calculated using the thickness, width, and height of the first porous coating layer.

[0265]

Table 1

[0266] Example 2 Example 3 Example 7 Average particle size of the first inorganic particles (D50) (nm) 600 20 110 Average particle size of the first porous coating layer (nm) 146 21 89 Porosity of the first porous coating layer (%) 58 52 56

[0267] Test Example 2: Observation of the partition surface

[0268] The SEM image of the thin film of the first porous coating layer of the separator manufactured in Example 4 shows Figure 2 The SEM image of the thin film of the first porous coating layer shows the surface of the first porous coating layer before the electrode adhesion layer is formed.

[0269] The SEM image of the thin film of the second porous coating layer of the separator manufactured in Example 4 shows Figure 3 middle.

[0270] It can be seen that the first porous coating has an interstitial volume structure in densely packed inorganic particles, and the second porous coating has a node-line structure, which includes: nodes containing inorganic particles and adhesive polymers coating part of the surface of the inorganic particles, and linear filaments formed by the adhesive polymers of the nodes.

[0271] Test Example 3: Determination of separator performance

[0272] The weight average molecular weight of the third binder polymer and the radius of gyration of the third binder polymer of the separator produced in each of Examples 1 to 7 and Comparative Example 1 were measured, and the results are shown in Table 2 below.

[0273] In addition, the heat shrinkage rate and the adhesion to the electrode of the separator of each of Examples 1 to 7 and Comparative Examples 1 to 2 were measured by the following methods, and the results are shown in Table 2 below.

[0274] (1) Measurement of Weight Average Molecular Weight of Third Binder Polymer

[0275] The weight average molecular weight of the third binder polymer was measured by gel permeation chromatography (GPC: gel permeation chromatography, PL GPC220, Agilent Technologies) under the following conditions.

[0276] -Chromatographic column: PL Olexis (Polymer Laboratories)

[0277] -Solvent: TCB (Trichlorobenzene)

[0278] -Flow rate: 1.0ml / min

[0279] -Sample concentration: 1.0mg / ml

[0280] -Injection volume: 200μl

[0281] - Column temperature: 160℃

[0282] -Detector: Agilent High Temperature RI detector

[0283] - Standard: Polystyrene (fit to a cubic polynomial)

[0284] (2) Measurement of the Radius of Gyration of the Third Binder Polymer

[0285] The radius of gyration of the third binder polymer was measured by a dynamic light scattering method using Otsuka DLS-8000 at room temperature, and the third binder polymer used in each of Examples 1 to 7 and Comparative Example 1 was fully dissolved in the solvent used in each of Examples 1 to 7 and Comparative Example 1 by stirring at room temperature for 1 hour under a solid content of 2%, and the same solvent as the solvent was added to dilute to a concentration of 1 / 100.

[0286] (3) Measurement of thermal shrinkage of separator

[0287] The heat shrinkage of the separator was calculated by cutting the separator produced in each of Examples 1 to 7 and Comparative Examples 1 to 2 into a square of 10 cm in MD x 10 cm in TD, placing it in a constant temperature oven maintained at 150° C. for 30 minutes, and measuring the length changes in the longitudinal and transverse directions:

[0288] Thermal shrinkage at 150°C (%) = {(dimension before shrinkage - dimension after shrinkage) / dimension before shrinkage} X 100

[0289] (4) Measurement of adhesion strength between separator and electrode

[0290] Two separators manufactured in each of Examples 1 to 7 and Comparative Examples 1 to 2 were stacked in such a manner that the second porous coating layers faced each other or the electrode adhesion layers faced each other, and interposed between 100 μm PET films, and were adhered by a roll laminator at 100° C. In this case, the roll laminator was heated at a speed of 0.3 m / min for 30 seconds, and the pressure at this time was 2 kgf / cm 2 .

[0291] After mounting the ends of the two adhered separators on a UTM device (LLOYD Instrument LF Plus), the force required to separate the adhered separators was measured by applying force in two directions at a measuring speed of 300 mm / min.

[0292] When the separator manufactured in Comparative Example 1 was measured, the electrode adhesion layers faced each other, and when Comparative Example 2 was measured, the second porous coating layers faced each other.

[0293]

Table 2

[0294]

[0295]

[0296] As can be seen from Table 2, in the case of Examples 1 to 7, it can be seen that the heat shrinkage and the adhesion to the electrode are very good. In addition, it can be seen that Examples 1-5 and 7 using the second inorganic particles having a particle size of 200 nm or more exhibited better adhesion to the electrode than Example 6 using the second inorganic particles having an average particle size of less than 200 nm.

[0297] In contrast, in the case of Comparative Example 1, since the electrode adhesion layer on the upper surface of the first porous coating layer formed on both surfaces of the polyolefin polymer substrate penetrates into the pores of the first porous coating layer and the pores of the polyolefin polymer substrate, it is difficult to ensure adhesion performance, and there is a difference in adhesion performance between the two surfaces of the separator.

[0298] In addition, in the case of Comparative Example 2, the porous coating layer does not have a void volume structure, which makes it difficult to ensure the heat shrinkage rate.

Claims

1. A separator for an electrochemical device, comprising: a porous polymer substrate having a first surface and a second surface opposite the first surface; a first porous coating layer, the first porous coating layer being disposed on the first surface of the porous polymer substrate and comprising first inorganic particles and a first binder polymer disposed on all or part of the surface of the first inorganic particles to connect and hold the first inorganic particles together, the first inorganic particles being substantially in contact with each other in a close-packed structure, and interstitial volumes formed between the first inorganic particles in contact with each other becoming pores of the first porous coating layer; a second porous coating layer, the second porous coating layer being disposed on the second surface of the porous polymer substrate and comprising a plurality of nodes, the nodes comprising second inorganic particles and a second binder polymer coating at least a portion of the surface of the second inorganic particles; and a node connecting portion, the node connecting portion comprising at least one linear filament formed by the second binder polymer of the node, the filament extending from the node and connecting another node, wherein the node connecting portion has a three-dimensional network structure in which a plurality of filaments derived from the second binder polymer cross each other; and an electrode adhesion layer disposed on a surface of the first porous coating layer opposite to the porous polymer substrate and comprising a third binder polymer, wherein the first porous coating layer and the second porous coating layer have different pore structures, wherein the average particle size of the first inorganic particles is smaller than the average particle size of the second inorganic particles, The average pore size of the first porous coating layer is 40 nm to 150 nm. 2 . The separator for an electrochemical device according to claim 1 , wherein an average particle size of the first inorganic particles is 0.01 to 0.99 times an average particle size of the second inorganic particles. 3 . The separator for an electrochemical device according to claim 1 , wherein an average particle diameter of the first inorganic particles is 10 nm to 800 nm. 4 . The separator for an electrochemical device according to claim 1 , wherein an average particle diameter of the second inorganic particles is 200 nm to 1000 nm. 5 . The separator for an electrochemical device according to claim 1 , wherein an average pore diameter of the first porous coating layer is 45 nm to 120 nm. 6 . The separator for an electrochemical device according to claim 1 , wherein the porosity of the first porous coating layer is 45% to 70%. 7 . The separator for an electrochemical device according to claim 1 , wherein the third binder polymer has a weight average molecular weight of 250,000 to 500,000 as measured by gel permeation chromatography. 8 . The separator for an electrochemical device according to claim 1 , wherein the third binder polymer has a radius of gyration of 150 nm to 500 nm. 9 . The separator for an electrochemical device according to claim 1 , wherein the first binder polymer comprises at least one of styrene-butadiene rubber, acrylic polymer, carboxymethyl cellulose, or polyvinyl alcohol.

10. The separator for an electrochemical device according to claim 1, wherein the second binder polymer comprises at least one of poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene) or poly(vinylidene fluoride-co-trifluoroethylene).

11. The separator for an electrochemical device according to claim 1, wherein the third binder polymer comprises at least one of poly(vinylidene fluoride-co-hexafluoropropylene), poly(vinylidene fluoride-co-trichloroethylene), poly(vinylidene fluoride-co-tetrafluoroethylene) or poly(vinylidene fluoride-co-trifluoroethylene).

12. The separator for an electrochemical device according to claim 1, wherein the separator for an electrochemical device has a heat shrinkage rate of 20% or less in each of a longitudinal direction and a lateral direction when measured after the separator is left at 150°C for 30 minutes. 13 . The separator for an electrochemical device according to claim 1 , wherein the separator for an electrochemical device has an adhesion strength to an electrode of 70 gf / 25 mm or more. 14 . An electrochemical device comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is the separator for an electrochemical device according to claim 1 .

15. The electrochemical device according to claim 14, wherein the electrochemical device is a lithium secondary battery.

Citation Information

Patent Citations

  • Icebreaker

    KR1020200065375A

  • Bg(l)

    KR1020200083387A

Cited By

  • Preparation method and application of composite PVDF-HFP and polylysine nanofiber diaphragm

    CN121566051A