Perovskite solar cell and preparation method thereof

By optimizing the interface between the insulating layer and the hole transport layer in perovskite solar cells and introducing formamidine thiocyanate into the perovskite absorption layer, the problem of interface chemical reaction reducing battery performance is solved, and the short-circuit current is significantly improved , open circuit voltage and photoelectric conversion efficiency.

CN118946172APending Publication Date: 2024-11-12TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411024781.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The interface chemical reaction of existing perovskite solar cells reduces cell performance, especially the interface optimization between the charge transport layer and the perovskite absorption layer is insufficient.

Method used

First apply a layer of insulating layer with moderate thickness on the transparent conductive substrate of perovskite solar cells to optimize the interface between the insulating layer and the hole transport layer, and introduce formicamidine thiocyanate as an additive in the perovskite solution to improve the The grain size and stability of the perovskite absorption layer improve the interface characteristics between the hole transport layer and the perovskite absorption layer.

Benefits of technology

By optimizing interface characteristics, the short-circuit current, open-circuit voltage, filling factor and photoelectric conversion efficiency of perovskite solar cells are significantly improved, internal charge transmission resistance and non-radiation recombination are reduced, and battery performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946172A_ABST
    Figure CN118946172A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solar cells, and provides a perovskite solar cell. The perovskite solar cell includes: an electrode; the electron transport layer is arranged on one side of the electrode; the perovskite absorption layer is arranged on one side, far away from the electrode, of the electron transfer layer; the hole transport layer is arranged on one side, far away from the electron transport layer, of the perovskite absorption layer; the insulating layer is arranged on one side, far away from the perovskite absorption layer, of the hole transport layer; and the transparent conductive substrate is arranged on one side, far away from the hole transport layer, of the insulating layer. Therefore, the perovskite solar cell has higher short-circuit current, higher open-circuit voltage, higher fill factor and higher photoelectric conversion efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular, to perovskite solar cells and preparation methods thereof, and further to electrical equipment. Background Art

[0002] Organic-inorganic halide perovskite solar cells (PSCs) have become a cutting-edge technology in the field of solar cells due to their excellent optoelectronic performance and low-cost manufacturing potential. Among them, the interface optimization between the charge transport layer and the perovskite absorption layer is the key to improving the performance of PSCs. However, the interface chemical reaction of perovskite solar cells prepared by existing technologies will reduce the performance of the cell.

[0003] Therefore, it is urgent to reduce the interfacial chemical reactions of perovskite solar cells to improve the performance of perovskite solar cells. Summary of the invention

[0004] The present application aims to solve at least one of the technical problems existing in the prior art to a certain extent. To this end, the present application provides a perovskite solar cell.

[0005] In a first aspect of the present application, the present application proposes a perovskite solar cell. According to an embodiment of the present application, the perovskite solar cell comprises:

[0006] electrode;

[0007] An electron transport layer, wherein the electron transport layer is disposed on one side of the electrode;

[0008] A perovskite absorption layer, wherein the perovskite absorption layer is disposed on a side of the electron transport layer away from the electrode;

[0009] A hole transport layer, the hole transport layer being disposed on a side of the perovskite absorption layer away from the electron transport layer;

[0010] An insulating layer, the insulating layer being disposed on a side of the hole transport layer away from the perovskite absorption layer;

[0011] and a transparent conductive substrate, wherein the transparent conductive substrate is arranged on a side of the insulating layer away from the hole transport layer. Thus, the perovskite solar cell has a higher short-circuit current, a higher open-circuit voltage, a higher fill factor and a higher photoelectric conversion efficiency.

[0012] In some embodiments, the thickness of the insulating layer is 1.9 nm to 4.1 nm. Thus, the insulating layer with moderate thickness optimizes the interface between the insulating layer and the hole transport layer, reduces defects and non-radiative recombination, reduces internal charge transfer resistance, and improves the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0013] In some embodiments, the thickness of the insulating layer is 2nm to 4nm. Thus, the insulating layer with moderate thickness further optimizes the interface between the insulating layer and the hole transport layer, reduces defects and non-radiative recombination, reduces internal charge transfer resistance, and improves the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0014] In some embodiments, the insulating layer includes at least one of metal oxide, metal nitride, non-metal oxide, organic compound and high molecular polymer.

[0015] In some embodiments, the insulating layer includes at least one of aluminum oxide, silicon dioxide, aluminum nitride, titanium dioxide, zinc oxide, 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and choline chloride.

[0016] In some embodiments, the insulating layer is formed of aluminum oxide.

[0017] In some embodiments, the insulating layer is formed of aluminum oxide with a porosity of less than 5%. Thus, the insulating layer uses aluminum oxide with a porosity of less than 5%, has a dense structure, reduces holes and charge recombination defects, prevents the penetration of chemicals, moisture and oxygen, and effectively improves the performance of perovskite solar cells, including short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency.

[0018] In some embodiments, the insulating layer is formed of non-porous aluminum oxide. Thus, the insulating layer is made of non-porous aluminum oxide, which has a dense structure, reduces holes and charge recombination defects, prevents the penetration of chemicals, moisture and oxygen, and can effectively further improve the performance of perovskite solar cells, including short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency.

[0019] In some embodiments, the hole transport layer includes [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACZ), benzoic acid, 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene) (Spiro-OMe TAD), nickel oxide (NiO x ), polyethylene terephthalate and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine (PFN-BR), and x is 0.5 to 1.5.

[0020] In some embodiments, the hole transport layer comprises [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8.75-13.75):1. Thus, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine with a moderate mass ratio can reduce the adsorption of water molecules by the hole transport layer, thereby improving the hydrophobicity of the hole transport layer, thereby improving the coverage of perovskite on the hole transport layer, and further improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0021] In some embodiments, the hole transport layer comprises [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (10-12.5):1. Thus, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine with a moderate mass ratio can reduce the adsorption of water molecules by the hole transport layer, thereby improving the hydrophobicity of the hole transport layer, thereby increasing the coverage of perovskite on the hole transport layer, and further improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0022] In some embodiments, the material of the perovskite absorber layer includes formamidine thiocyanate.

[0023] In the second aspect of the present application, the present application proposes a method for preparing the perovskite solar cell described in the first aspect of the present application, the method comprising: forming an insulating layer on one side of a transparent conductive substrate; forming a hole transport layer on the side of the insulating layer away from the transparent conductive substrate; forming a perovskite absorption layer on the side of the hole transport layer away from the insulating layer; forming an electron transport layer on the side of the perovskite absorption layer away from the hole transport layer; and forming an electrode on the side of the electron transport layer away from the perovskite absorption layer. Thus, the method can prepare a perovskite solar cell with higher short-circuit current, higher open-circuit voltage, higher fill factor and higher photoelectric conversion efficiency.

[0024] In some embodiments, the forming of the insulating layer on one side of the transparent conductive substrate is achieved by: subjecting one side of the transparent conductive substrate to a first coating treatment with an aluminum oxide solution containing 0.1 to 0.3 mg / mL; subjecting the first coating treatment product to a first annealing treatment to obtain the insulating layer, wherein the first annealing treatment is performed at a temperature of 95 to 105° C. for 8 to 12 minutes.

[0025] In some embodiments, the forming of the hole transport layer on the side of the insulating layer away from the transparent conductive substrate is achieved by: subjecting the insulating layer to a second coating treatment on the side of the insulating layer away from the transparent conductive substrate containing 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid solution; subjecting the second coating treatment product to a second annealing treatment to obtain the hole transport layer, and the second annealing treatment is performed at a temperature of 95 to 105° C. for 8 to 12 minutes.

[0026] In some embodiments, the second coating treatment is performed on 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 0.3 to 0.5 mg / mL of 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine solution, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8.75 to 13.75):1.

[0027] In some embodiments, the second coating treatment is performed on 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 0.3 to 0.5 mg / mL of 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine solution, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (10 to 12.5):1.

[0028] In some embodiments, forming a perovskite absorption layer on a side of the hole transport layer away from the insulating layer is achieved by: subjecting a solution containing a perovskite transport material to a third coating treatment on a side of the hole transport layer away from the insulating layer; subjecting the third coating treatment product to a third annealing treatment to obtain the perovskite absorption layer, and the third annealing treatment is performed at a temperature of 120 to 140° C. for 18 to 22 minutes.

[0029] In some embodiments, a solution containing a perovskite transport material and formamidine thiocyanate is subjected to the third coating treatment on the side of the hole transport layer away from the insulating layer, the concentration of the perovskite transport material in the solution is 1.2 mol / mL, the concentration of the formamidine thiocyanate in the solution is 1-2 mg / mL, and the molar mass ratio of the perovskite transport material to the formamidine thiocyanate is 1.2:(1-2).

[0030] In a third aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device includes: the perovskite solar cell described in the first aspect of the present application or the third aspect of the present application.

[0031] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0033] Figure 1 Schematic diagram of the structure of an inversion perovskite solar cell according to an embodiment of the present application.

[0034] Figure 2 The present invention is a flow chart of a method for preparing an inversion perovskite solar cell according to an embodiment of the present application.

[0035] Figure 3 Scanning electron microscope images of a perovskite solar cell without (a) adding formamidine thiocyanate (FASCN) and with (b) adding formamidine thiocyanate (FASCN) according to an embodiment of the present application.

[0036] Description of reference numerals:

[0037] Perovskite solar cells 100;

[0038] Electrode 01; electron transport layer 02; perovskite absorption layer 03; hole transport layer 04; insulating layer 05; transparent conductive substrate 06. DETAILED DESCRIPTION

[0039] The embodiments of the present application are described in detail below. Examples of the embodiments are shown in the drawings, but unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of actually identical structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0040] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field to which this application belongs; the terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application; unless otherwise specified, the numerical values ​​of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application).

[0041] The terms "including" and "having" in the specification and claims of the present application and any modifications thereof are open expressions, that is, including the contents specified in the present application but not excluding other contents.

[0042] In the description of the present application, it should be understood that the terms "width", "thickness", etc. indicate orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0043] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. "First feature" and "second feature" may include one or more of the features.

[0044] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0045] In the description of the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0046] In the description of the present application, “plurality” means two or more.

[0047] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.

[0048] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0049] Organic-inorganic halide perovskite solar cells (PSCs) have become a hot topic in the field of solar technology due to their excellent optoelectronic properties and manufacturing cost advantages. In PSCs, specific self-assembled monolayers (SAM-HTLs) act as hole transport layers, which significantly improve the power conversion efficiency of the cells by optimizing the interface properties. However, the existing technology for depositing self-assembled monolayers has the problem of uneven film formation due to insufficient wettability of the transparent conductive substrate.

[0050] To solve these problems, the present application improves the wettability of the transparent conductive substrate and promotes the uniform deposition of the self-assembled monolayer by first coating an insulating layer on the transparent conductive substrate of the perovskite solar cell, and introduces specific additives into the perovskite solution to improve the grain size and stability of the perovskite absorption layer, optimize the interface properties between the hole transport layer and the perovskite absorption layer, thereby improving the kinetic performance of the carriers, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0051] Based on this, in the first aspect of the present application, the present application proposes a perovskite solar cell 100. According to an embodiment of the present application, referring to Figure 1 , the perovskite solar cell 100 comprises:

[0052] Electrode 01;

[0053] An electron transport layer 02, wherein the electron transport layer 02 is disposed on one side of the electrode 01;

[0054] A perovskite absorption layer 03, wherein the perovskite absorption layer 03 is disposed on a side of the electron transport layer 02 away from the electrode 01;

[0055] A hole transport layer 04, wherein the hole transport layer 04 is disposed on a side of the perovskite absorption layer 03 away from the electron transport layer 02;

[0056] An insulating layer 05, wherein the insulating layer 05 is disposed on a side of the hole transport layer 04 away from the perovskite absorption layer 03;

[0057] and a transparent conductive substrate 06, wherein the transparent conductive substrate 06 is disposed on a side of the insulating layer 05 away from the hole transport layer 04. The present application improves the surface energy of the transparent conductive substrate, increases the affinity with the subsequently coated material, improves the wettability, and promotes a more uniform deposition of the hole transport layer on the insulating layer to form a continuous, defect-free film, which is essential for effective charge extraction and transport, and improves the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0058] In some embodiments, the thickness of the insulating layer is 1.9nm to 4.1nm, for example, it can be 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, 3.0nm, 3.1nm, 3.2nm, 3.3nm, 3.4nm, 3.5nm, 3.6nm, 3.7nm, 3.8nm, 3.9nm, 4nm, 4.1nm and the range between any two point values ​​thereof, such as 1.9nm to 4nm, 1.9nm to 3.9nm, 1.9nm to 3.8nm and 1.9nm to 3.7nm. Therefore, an insulating layer with moderate thickness can ensure the interface quality with the hole transport layer, reduce interface defects and help balance the extraction and transfer of charges, reduce non-radiative recombination at the interface and reduce the charge transfer resistance and recombination inside the battery, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.

[0059] In some embodiments, the thickness of the insulating layer is 2 nm to 4 nm.

[0060] In some embodiments, the insulating layer includes at least one of metal oxide, metal nitride, non-metal oxide, organic compound and high molecular polymer.

[0061] In some embodiments, the insulating layer includes at least one of aluminum oxide, silicon dioxide, aluminum nitride, titanium dioxide, zinc oxide, 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and choline chloride.

[0062] In some embodiments, the insulating layer is formed of aluminum oxide.

[0063] In some embodiments, the insulating layer is formed of aluminum oxide with a porosity of less than 5%. The structure of the insulating layer formed of aluminum oxide with a porosity of less than 5% is denser, reducing holes and defects, and reducing defects that may serve as charge carrier recombination centers; in addition, the insulating layer formed of aluminum oxide with a porosity of less than 5% can prevent chemical species, moisture and oxygen from penetrating, reducing the possibility of chemical activity and chemical corrosion, as well as environmental factors such as moisture and oxygen penetrating into the battery, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0064] In some embodiments, the insulating layer is formed of non-porous aluminum oxide. The structure of the insulating layer formed of non-porous aluminum oxide is more compact, with fewer holes and defects, and fewer defects that may serve as charge carrier recombination centers; in addition, the insulating layer formed of non-porous aluminum oxide can prevent chemical species, moisture, and oxygen from penetrating, reducing the possibility of chemical activity and chemical corrosion, as well as environmental factors such as moisture and oxygen penetrating into the battery, thereby further improving the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the perovskite solar cell.

[0065] In some embodiments, the hole transport layer includes but is not limited to [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACZ), benzoic acid, 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene), poly Ethylene terephthalate, poly(3-hexylthiophene) (P3HT), poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonate) (PEDOT:PSS), spirobis(terthiophene)benzodithiophene (Spiro-TTB), tetrafluoro-7,7,8,8-tetracyanoquinolinium (F4-TCNQ), hexafluoro-7,7,8,8-tetracyanoquinodimethane (F6TCNNQ), 2,2'-(1,4-phenylene)bis-4-(2-ethylhexyloxy)phenyl-1-phenyloctanone (TAPC), nickel oxide (NiO x), polyethylene terephthalate, copper thiocyanate (CuSCN), copper aluminum oxide (CuAlO2), vanadium pentoxide (V2O5), cadmium sulfide (CdS), cadmium selenide (CdSe), poly (9,9-di-n-decylfluorene) bromide and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, at least one of which x is 0.5 to 1.5.

[0066] In some embodiments, the hole transport layer comprises [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and the mass ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8.75 to 13.75):1.

[0067] In some embodiments, the hole transport layer comprises [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and the mass ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (10 to 12.5):1.

[0068] In some embodiments, the electron transport layer material includes but is not limited to at least one of titanium dioxide (TiO2), tin dioxide (SnO2), zinc oxide (ZnO), zirconium dioxide (ZrO2), gallium zinc oxide (GZO), indium zinc oxide (IZO), transparent conductive iron oxide (FTO), transparent conductive indium oxide (ITO), barium stannate (BaSnO3), fullerene C60 (C60), fullerene C70 (C70) and [6,6]-phenyl-C61-butyric acid methyl ester (PCBM).

[0069] In some embodiments, the perovskite absorber layer comprises ABX3, wherein A comprises but is not limited to methylamine cation (FA + ), methylammonium cation (MA + ), cesium cation (Cs + ), rubidium cation (Rb + ), potassium cation (K + ) at least one of; B includes but is not limited to lead cations (Pb 2+ ), tin cation (Sn 2+ ), copper cation (Cu 2+ ), zinc cation (Zn 2+ ), gallium cation (Ga 2+ ), calcium cation (Ca 2+) at least one of; X includes but is not limited to fluoride anion (F - ), chloride anion (Cl - ), bromide anion (Br - ), iodide anion (I - )

[0070] In some embodiments, the ABX3 is formamidinium lead iodide perovskite (FAPbI3).

[0071] In some embodiments, the electrode includes at least one of copper (Cu), silver (Ag), and gold (Au).

[0072] In some embodiments, the perovskite absorber layer further comprises an additive, wherein the additive comprises formamidine thiocyanate.

[0073] In some embodiments, the thickness of the hole transport layer is 10 to 20 nm, for example, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm and ranges between any two of them, such as 10 to 19 nm, 10 to 18 nm and 10 to 17 nm. Thus, a hole transport layer with a moderate thickness is conducive to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.

[0074] In some embodiments, the thickness of the electron transport layer is 30-40 nm, for example, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, 35 nm, 36 nm, 37 nm, 38 nm, 39 nm, 40 nm and range values ​​between any two of them, such as 30-39 nm, 30-38 nm and 30-37 nm. Thus, an electron transport layer with moderate thickness is conducive to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.

[0075] In some embodiments, the thickness of the perovskite absorption layer is 500-800nm, for example, it can be 500nm, 550nm, 600nm, 650nm, 700nm, 750nm, 760nm, 770nm, 780nm, 790nm, 800nm ​​and the range between any two of them, such as 500-790nm, 500-780nm and 500-770nm. Thus, the perovskite absorption layer with moderate thickness is conducive to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.

[0076] In some embodiments, the thickness of the electrode is 100-200 nm, for example, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm and range values ​​between any two of them, such as 100-190 nm, 100-180 nm and 100-170 nm. Thus, an electrode with moderate thickness is conducive to improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.

[0077] In the second aspect of the present application, the present application proposes a method for preparing the battery described in the first aspect of the present application, referring to Figure 2 , the method comprising:

[0078] S100: forming an insulating layer on one side of the transparent conductive substrate;

[0079] S200: forming a hole transport layer on a side of the insulating layer away from the transparent conductive substrate;

[0080] S300: forming a perovskite absorption layer on a side of the hole transport layer away from the insulating layer;

[0081] S400: forming an electron transport layer on a side of the perovskite absorption layer away from the hole transport layer;

[0082] S500: forming an electrode on a side of the electron transport layer away from the perovskite absorption layer. Thus, the method can prepare a perovskite solar cell with higher short-circuit current, higher open-circuit voltage, higher fill factor and higher photoelectric conversion efficiency.

[0083] In some embodiments, forming an insulating layer on one side of the transparent conductive substrate is achieved by: subjecting one side of the transparent conductive substrate to a first coating treatment with an aluminum oxide solution containing 0.1 to 0.3 mg / mL; subjecting the first coating treatment product to a first annealing treatment to obtain the insulating layer, wherein the first annealing treatment is performed at a temperature of 95 to 105° C. for 8 to 12 minutes.

[0084] In some embodiments, the forming of the hole transport layer on the side of the insulating layer away from the transparent conductive substrate is achieved by: subjecting the insulating layer to a second coating treatment on the side of the insulating layer away from the transparent conductive substrate containing 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid solution; subjecting the second coating treatment product to a second annealing treatment to obtain the hole transport layer, and the second annealing treatment is performed at a temperature of 95 to 105° C. for 8 to 12 minutes.

[0085] In some embodiments, the second coating treatment is performed on 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 0.3 to 0.5 mg / mL of 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine solution, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8.75 to 13.75):1.

[0086] In some embodiments, the second coating treatment is performed on 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 0.3 to 0.5 mg / mL of 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine solution, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (10 to 12.5):1.

[0087] In some embodiments, forming a perovskite absorption layer on a side of the hole transport layer away from the insulating layer is achieved by: subjecting a solution containing a perovskite transport material to a third coating treatment on a side of the hole transport layer away from the insulating layer; subjecting the third coating treatment product to a third annealing treatment to obtain the perovskite absorption layer, and the third annealing treatment is performed at a temperature of 120 to 140° C. for 18 to 22 minutes.

[0088] In some embodiments, a solution containing a perovskite transport material and formamidine thiocyanate is subjected to the third coating treatment on the side of the hole transport layer away from the insulating layer, the concentration of the perovskite transport material in the solution is 1.2 mol / mL, the concentration of the formamidine thiocyanate in the solution is 1-2 mg / mL, and the molar mass ratio of the perovskite transport material to the formamidine thiocyanate is 1.2:(1-2). According to an embodiment of the present application, adding formamidine thiocyanate (FASCN) to a solution containing a perovskite material is beneficial to improving the grain size and stability of the perovskite particles. In addition, formamidine thiocyanate (FASCN) also regulates the interface properties of the self-assembled monolayer and the perovskite absorption layer, greatly improving the carrier dynamics.

[0089] In a third aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device includes: the perovskite solar cell described in the first aspect of the present application.

[0090] The scheme of the present application will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the literature in this area or the product specification are carried out. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0091] Embodiment 1:

[0092] The inverted perovskite solar cell prepared in this embodiment has a structure as shown in FIG. Figure 1 As shown in the figure, from bottom to top, there are transparent conductive substrate, insulating layer, hole transport layer, perovskite absorption layer, electron transport layer and copper electrode. The transparent conductive substrate is 10×10 cm 2 FTO; the hole transport layer is Me-4PACZ; the structure of the perovskite absorption layer is the most basic FAPbI3; the electron transport layer is C60 / SnO2; and the electrode is a copper electrode.

[0093] (1) Provide a transparent conductive substrate with a thickness of 2.18 mm.

[0094] (2) The insulating layer preparation method is as follows: First, the transparent conductive substrate is subjected to UV ozone surface treatment to improve the wettability of the transparent conductive substrate. Then, the prepared 0.2 mg / mL aluminum oxide is used to prepare an aluminum oxide insulating layer using a coating machine, and then annealed at 100°C for 10 minutes. The thickness of the aluminum oxide insulating layer is 3 nm.

[0095] (3) The preparation method of the hole transport layer is as follows: 0.5 mg / mL of the prepared Me-4PACZ and 0.4 mg / mL of 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine are mixed in a volume ratio of 9:1 (the corresponding mass ratio of Me-4PACZ to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 11.25:1) and stirred overnight. Then, the hole transport layer is prepared on the aluminum oxide insulating layer by slit coating, and then annealed at 100°C for 10 minutes. The thickness of the hole transport layer is 15 nm.

[0096] (4) The preparation method of the perovskite absorption layer is as follows: a 1.2 mol / mL perovskite solution based on formamidine lead iodide (FAPbI3) is dissolved in a solvent of dimethylformamide (DMF): N-methylpyrrolidone (NMP) in a ratio of 6:1, and 1.5 mg / mL of the additive material formamidine thiocyanate (FASCN) is added and stirred overnight. Subsequently, a perovskite film is prepared on the Me-4PACZ layer using slit coating and annealed at 130°C for 20 min. The thickness of the perovskite absorption layer is 550 nm.

[0097] (5) The preparation method of the electron transport layer is as follows: a C60 layer is prepared by thermal evaporation method, with a total thickness of 30 nm; a SnO2 layer is prepared by atomic layer deposition, with a thickness of 10 nm; wherein the C60 layer and the SnO2 layer constitute the electron transport layer of the perovskite solar cell.

[0098] (6) The preparation method of the copper electrode is as follows: on the surface of the hole transport layer, a copper electrode is deposited using a thermal evaporation evaporator, and the vacuum degree of the thermal evaporation chamber is 10 -5 Pa, the metal evaporation rate is 5nm / min, and the thickness of the copper electrode is 110nm.

[0099] Embodiment 2:

[0100] The experimental process of this embodiment is basically the same as that of embodiment 1, except that the thickness of the aluminum oxide insulating layer is 2 nm.

[0101] Embodiment 3:

[0102] The experimental process of this embodiment is basically the same as that of embodiment 1, except that the thickness of the aluminum oxide insulating layer is 4 nm.

[0103] Embodiment 4:

[0104] The experimental process of this embodiment is basically the same as that of embodiment 1, except that the thickness of the aluminum oxide insulating layer is 1.9 nm.

[0105] Embodiment 5:

[0106] The experimental process of this embodiment is basically the same as that of embodiment 1, except that the thickness of the aluminum oxide insulating layer is 4.1 nm.

[0107] Embodiment 6:

[0108] The experimental process of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, the volume ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 10:1 (the corresponding mass ratio of Me-4PACZ to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 12.5:1).

[0109] Embodiment 7:

[0110] The experimental process of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, the volume ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 8:1 (the corresponding mass ratio of Me-4PACZ to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 10:1).

[0111] Embodiment 8:

[0112] The experimental process of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, the volume ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 11:1 (the corresponding mass ratio of Me-4PACZ to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 13.75:1).

[0113] Embodiment 9:

[0114] The experimental process of this embodiment is basically the same as that of Embodiment 1, except that, in this embodiment, the volume ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 7:1 (the corresponding mass ratio of Me-4PACZ to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is 8.75:1).

[0115] Embodiment 10:

[0116] The experimental process of this embodiment is basically the same as that of embodiment 1, except that the additive material formamidine thiocyanate (FASCN) is not used when preparing the perovskite absorption layer in this embodiment.

[0117] Embodiment 11:

[0118] The experimental process of this embodiment is basically the same as that of embodiment 1, except that when preparing the hole transport layer in this embodiment, NiO is first deposited before adding 0.5 mg / mL Me-4PACZ and 0.4 mg / mL 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine. x layer.

[0119] Comparative Example 1:

[0120] The experimental process of this comparative example is basically the same as that of Example 1. The difference from Example 1 is that the functional layers of the perovskite battery provided in this comparative example are basically the same as the functional layers of the perovskite battery in Example 1. The main difference is that no aluminum oxide insulating layer is prepared in this comparative example.

[0121] Test Example 1:

[0122] The performance of the perovskite solar cells prepared in Examples 1 to 11 and Comparative Example 1 was compared, and the parameters thereof are shown in Table 1. It can be seen that the photoelectric conversion efficiency of the perovskite solar cell with the aluminum oxide insulating layer is significantly improved.

[0123] Table 1: Performance test table

[0124] Perovskite solar panels <![CDATA[I SC (A)]]> <![CDATA[V OC (V)]]> FF(%) PCE(%) Example 1 0.0881 10.46 81.47 20.85 Example 2 0.0877 10.43 80.96 20.61 Example 3 0.0873 10.39 80.58 20.42 Example 4 0.0871 10.36 80.27 20.21 Example 5 0.0869 10.32 80.06 20.06 Example 6 0.0879 10.42 80.72 20.55 Example 7 0.0877 10.38 80.38 20.47 Example 8 0.0873 10.40 81.14 20.41 Example 9 0.0876 10.37 80.84 20.39 Example 10 0.0876 9.85 80.29 19.24 Embodiment 11 0.0831 10.41 80.91 19.44 Comparative Example 1 0.0857 9.98 77.29 18.36

[0125] Compared with Comparative Example 1, Examples 1 to 11 show that the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell with an aluminum oxide insulating layer are higher than those of the perovskite solar cell without an aluminum oxide insulating layer, especially the open-circuit voltage and fill factor. This indicates that the use of an aluminum oxide insulating layer in the perovskite solar cell increases the coverage of Me-4PACZ, increases carrier transport, and reduces non-radiative recombination.

[0126] By comparing Examples 1 to 3 with Examples 4 to 5, it can be seen that when the thickness of the aluminum oxide insulating layer is 2 nm to 4 nm, the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell are relatively high.

[0127] By comparing Examples 1 to 6, 7 and Examples 8 to 9, it can be seen that when the volume ratio of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8 to 10):1 (the corresponding mass ratio of Me-4PACZ to 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (10 to 12.5):1), the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency are higher.

[0128] Compared with Example 10, the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell prepared by adding thiocyanate formamidine (FASCN) are improved, and the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell prepared without adding thiocyanate formamidine (FASCN) are reduced, which indicates that the addition of thiocyanate formamidine (FASCN) further increases the grain size of the perovskite film and optimizes the carrier dynamics. Thus, the performance of the perovskite solar cell is further optimized, and its photoelectric conversion efficiency is increased from 17% to 20%.

[0129] Compared with Example 1 and Example 11, it can be obtained that NiO is removed x The performance of perovskite solar cells prepared by layer is better than that without removing NiO x The perovskite solar cell prepared by the layer has good performance, which shows that the addition of NiO x This will lead to increased non-radiative recombination and reduce the performance of perovskite solar cells.

[0130] Test Example 2:

[0131] In order to test the change of perovskite grain size after using the additive material formamidine thiocyanate (FASCN), SEM tests were performed on Example 1 and Example 6. Figure 3 As shown. Figure 3 It can be seen that the perovskite grain size after adding the additive material formamidine thiocyanate (FASCN) in Example 1 (right picture) is larger than that in Example 6 (left picture) without adding the additive material formamidine thiocyanate (FASCN), which shows that FASCN is beneficial to the growth of FAPbI3 grains and can improve carrier dynamics, thereby improving the open circuit voltage and photoelectric conversion efficiency of perovskite solar cells.

[0132] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0133] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A perovskite solar cell, characterized in that: include: electrode; An electron transport layer, wherein the electron transport layer is disposed on one side of the electrode; A perovskite absorption layer, wherein the perovskite absorption layer is disposed on a side of the electron transport layer away from the electrode; A hole transport layer, the hole transport layer being disposed on a side of the perovskite absorption layer away from the electron transport layer; An insulating layer, the insulating layer being disposed on a side of the hole transport layer away from the perovskite absorption layer; and A transparent conductive substrate is disposed on a side of the insulating layer away from the hole transport layer.

2. The battery according to claim 1, characterized in that The thickness of the insulating layer is 1.9 nm to 4.1 nm.

3. The battery according to claim 1, characterized in that The thickness of the insulating layer is 2nm-4nm.

4. The battery according to any one of claims 1 to 3, characterized in that: The insulating layer includes at least one of metal oxide, metal nitride, non-metal oxide, organic compound and high molecular polymer.

5. The battery according to claim 4, characterized in that The insulating layer includes at least one of aluminum oxide, silicon dioxide, aluminum nitride, titanium dioxide, zinc oxide, 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine and choline chloride.

6. The battery according to claim 5, characterized in that The insulating layer is formed of aluminum oxide.

7. The battery according to claim 6, characterized in that The insulating layer is formed of aluminum oxide having a porosity of less than 5%.

8. The battery according to claim 7, characterized in that The insulating layer is formed of non-porous aluminum oxide.

9. The battery according to claim 1, characterized in that The hole transport layer includes [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid, benzoic acid, 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene), NiO x , polyethylene terephthalate and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and x is 0.5 to 1.

5.

10. The battery according to claim 9, characterized in that The hole transport layer comprises [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine, and the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8.75-13.75):

1.

11. The battery according to claim 1, characterized in that The material of the perovskite absorption layer includes formamidine thiocyanate.

12. A method for preparing a perovskite solar cell according to any one of claims 1 to 11, characterized in that: include: forming an insulating layer on one side of the transparent conductive substrate; forming a hole transport layer on a side of the insulating layer away from the transparent conductive substrate; forming a perovskite absorption layer on a side of the hole transport layer away from the insulating layer; forming an electron transport layer on a side of the perovskite absorption layer away from the hole transport layer; An electrode is formed on a side of the electron transport layer away from the perovskite absorption layer.

13. The method according to claim 12, characterized in that The insulating layer is formed on one side of the transparent conductive substrate by: Performing a first coating treatment on one side of the transparent conductive substrate by subjecting a solution containing 0.1 to 0.3 mg / mL of aluminum oxide; The first coating product is subjected to a first annealing treatment to obtain the insulating layer. The first annealing treatment is performed at a temperature of 95 to 105° C. for 8 to 12 minutes.

14. The method according to claim 12, characterized in that The forming of the hole transport layer on the side of the insulating layer away from the transparent conductive substrate is achieved in the following manner: Performing a second coating treatment on a side of the insulating layer away from the transparent conductive substrate by a solution containing 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid; The second coating product is subjected to a second annealing treatment to obtain the hole transport layer. The second annealing treatment is performed at a temperature of 95 to 105° C. for 8 to 12 minutes.

15. The method according to claim 14, characterized in that The method comprises subjecting 0.4 to 0.6 mg / mL of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid and 0.3 to 0.5 mg / mL of 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine solution to the second coating treatment, wherein the mass ratio of the [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid to the 1-(2-pyridyl)-N-(2-bromoethyl)-2-naphthylamine is (8.75 to 13.75):

1.

16. The method according to claim 12, characterized in that The forming of the perovskite absorption layer on the side of the hole transport layer away from the insulating layer is achieved by the following method: Performing a third coating treatment on a side of the hole transport layer away from the insulating layer with a solution containing a perovskite transport material; The third coating product is subjected to a third annealing treatment to obtain the perovskite absorption layer. The third annealing treatment is performed at a temperature of 120 to 140° C. for 18 to 22 minutes.

17. According to the method of claim 16, the third coating treatment is performed on the side of the hole transport layer away from the insulating layer with a solution containing a perovskite transport material and formamidine thiocyanate, the concentration of the perovskite transport material in the solution is 1.2 mol / mL, the concentration of the formamidine thiocyanate in the solution is 1-2 mg / mL, and the molar mass ratio of the perovskite transport material to the formamidine thiocyanate is 1.2:(1-2).

18. An electrical equipment, characterized in that: include: The perovskite solar cell according to any one of claims 1 to 11.