Light-emitting device and preparation method thereof
By setting a functional layer in the quantum dot light emitting diode and using ferrocene derivatives to bridge the light emitting layer and the charge functional layer, the problem of the complex imbalance between the quantum dot light emitting layer and the electron transport layer is solved, and the luminous efficiency and lifetime are improved.
Patent Information
- Application Number
- CN202310542379.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing quantum dot light emitting diodes, the energy barrier between the quantum dot light emitting layer and the electron transport layer is smaller than that of the hole transport layer, resulting in the recombination imbalance between holes and electrons in the light emitting layer, increasing exciton quenching and reducing luminous efficiency.
Setting a functional layer between the luminescent layer and the charge functional layer, using ferrocene and/or its derivatives as electron transfer medium materials, bridging the luminescent layer and the charge functional layer, balancing the injection of electrons and holes, weakening the recombination imbalance, resulting in quenching of excitons.
The luminescence efficiency of the light emitting device is improved, the interface aging between the light emitting layer and the charge functional layer is slowed down, the probability of organic ligand falling off is reduced, the electron transmission is enhanced, and the life of the light emitting device is extended.
Smart Images

Figure CN118946180A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of display technology, and in particular to a light-emitting device and a preparation method thereof. Background Art
[0002] With the in-depth development of quantum dot preparation technology, the stability and luminous efficiency of quantum dots are constantly improving. Therefore, there have been many studies on the application of quantum dots in light emitting diodes. Specifically, the structure of quantum dots generally includes three parts, namely, a core, a shell, and an organic ligand bound to the core and the shell by chelation or other binding methods. Among them, the core and the shell provide the quantum dots with photoluminescence function. The organic ligand has the function of stabilizing the core and the shell on the one hand, and improving the ability of the core and the shell to dissolve or disperse in organic solvents on the other hand.
[0003] In existing light-emitting diodes that use quantum dot materials as light-emitting materials, since the energy barrier between the quantum dot light-emitting layer and the electron transport layer is smaller than the energy barrier from the hole transport layer to the quantum dot light-emitting layer, the recombination of holes and electrons in the quantum dot light-emitting layer during the transmission process is unbalanced, which increases the exciton quenching caused by non-radiative recombination and damages the organic ligands of the quantum dots, thereby reducing the luminescence efficiency of the device. Summary of the invention
[0004] The object of the present invention is to provide a light emitting device and a method for preparing the same, aiming to solve the technical problem of low light emitting efficiency of existing light emitting devices.
[0005] Another object of the present invention is to provide a method for preparing a light emitting device.
[0006] Another object of the present invention is to provide a display device.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0008] A light-emitting device comprises a first electrode, a light-emitting layer, a functional layer, a charge functional layer, and a second electrode which are sequentially stacked, wherein the material of the functional layer comprises ferrocene and / or a derivative of ferrocene as shown in the following formula I:
[0009]
[0010] In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
[0011] Accordingly, a method for preparing a light emitting device comprises the steps of:
[0012] providing a first electrode;
[0013] Disposing a light-emitting layer on the first electrode;
[0014] Disposing a functional layer on the light-emitting layer;
[0015] disposing a charge functional layer on the functional layer; and
[0016] Disposing a second electrode on the charge functional layer and encapsulating it; or
[0017] providing a second electrode;
[0018] providing a charge functional layer on the second electrode;
[0019] Disposing a functional layer on the charge functional layer;
[0020] disposing a light-emitting layer on the functional layer; and
[0021] Disposing a first electrode on the light-emitting layer and encapsulating it;
[0022] Wherein, the material of the functional layer includes ferrocene and / or a derivative of ferrocene as shown in the following formula I:
[0023]
[0024] In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
[0025] The light-emitting device provided by the present invention is provided with the functional layer between the light-emitting layer and the charge functional layer, wherein the ferrocene and / or the derivative of ferrocene in the functional layer can bridge the light-emitting layer and the charge functional layer as an electron transfer medium material, so as to realize stable electron transfer from the charge functional layer to the light-emitting layer through the functional layer, thereby balancing the electron injection and the hole injection, reducing the existing exciton quenching caused by the unbalanced recombination of holes and electrons in the light-emitting layer, and improving the luminous efficiency of the light-emitting device. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 A schematic diagram of the structure of a light emitting device provided by an embodiment of the present invention;
[0028] Figure 2 It is a schematic flow chart of a method for preparing a vertical light-emitting device provided in an embodiment of the present invention;
[0029] Figure 3 It is a schematic flow chart of a method for preparing an inverted light-emitting device provided in an embodiment of the present invention.
[0030] Reference numerals: 101 - first electrode, 102 - light-emitting layer, 103 - functional layer, 104 - charge functional layer, 105 - second electrode. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention. In addition, it should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0032] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0033] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as ug, mg, g, kg, etc.
[0034] like Figure 1 As shown, an embodiment of the present invention provides a light-emitting device, comprising a first electrode 101, a light-emitting layer 102, a functional layer 103, a charge functional layer 104, and a second electrode 105 which are sequentially stacked, wherein the material of the functional layer comprises ferrocene and / or a derivative of ferrocene as shown in the following formula I,
[0035]
[0036] In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
[0037] In this embodiment, the functional layer is provided between the light-emitting layer and the charge functional layer, wherein ferrocene and / or a derivative of ferrocene in the functional layer can serve as an electron transfer medium material to bridge the light-emitting layer and the charge functional layer, so as to achieve stable electron transfer from the charge functional layer to the light-emitting layer through the functional layer, thereby balancing electron injection and hole injection, reducing the existing exciton quenching caused by the unbalanced recombination of holes and electrons in the light-emitting layer, and improving the luminescence efficiency of the light-emitting device.
[0038] Furthermore, in this embodiment, the functional layer can effectively slow down the aging of the material of the interface layer between the light-emitting layer and the charge functional layer. At the same time, the probability of the organic ligand bound to the quantum dot light-emitting material on the surface of the light-emitting layer falling off is reduced, and the defects on the surface of the light-emitting layer are also reduced, thereby improving the luminous efficiency of the light-emitting device. In addition, because ferrocene and its derivatives are electron-rich materials, they can also enhance the transmission of electrons to a certain extent, thereby helping to improve the luminous efficiency of the light-emitting device.
[0039] Preferably, in formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, thiol, cyano, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted cycloalkyl having 4-20 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-20 ring atoms, substituted or unsubstituted aryl having 6-20 ring atoms, substituted or unsubstituted heteroaryl having 6-20 ring atoms, and n1 and n2 are independently selected from 0-2.
[0040] More preferably, the ferrocene derivative is one or more of 1,1'-bis(phenylphosphino)ferrocene, 1,1'-ferrocene diboronate, 1,1'-ferrocenedicarboxylic acid, ferrocenylcarboxylic acid, bromoferrocene, ferrocenylacetic acid, and o-ferrocenylformylbenzoic acid.
[0041] In this embodiment, the ferrocene derivatives used are all simple to prepare and easy to obtain materials, which is beneficial to reducing the preparation cost of the light-emitting device.
[0042] In some embodiments, the light-emitting layer is a quantum dot light-emitting layer, and the material of the quantum dot light-emitting layer includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound, and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, Z At least one of nSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the IV-VI group compound is selected from SnS, SnSe, SnTe, PbS, PbSe, At least one of PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, and the III-V group compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, At least one of AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2.
[0043] The core of the core-shell structured quantum dots includes any one of the above-mentioned single structure quantum dots, and the shell material of the core-shell structured quantum dots includes CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and at least one of the above-mentioned single structure quantum dots.
[0044] The charge functional layer includes a metal oxide, the material of which is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium.
[0045] The material of the first electrode and / or the second electrode includes one or more of metals, carbon materials and metal oxides, the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes doped or undoped metal oxides, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2.
[0046] It is understood that when the material of the quantum dot light-emitting layer includes the quantum dots, the material of the quantum dot light-emitting layer also includes a ligand connected to the surface of the quantum dots, and the ligand includes but is not limited to at least one of an amine ligand, a carboxylic acid ligand, a thiol ligand, a (oxy)phosphine ligand, a phospholipid, a soft phosphine or polyvinyl pyridine, wherein the amine ligand is selected from methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, nonylamine, decylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine, tributylamine, or trioctylamine. The invention relates to a method for preparing an alkyl amine, wherein the alkyl amine is selected from at least one of formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid or benzoic acid; the thiol ligand is selected from at least one of methyl mercaptan, ethyl mercaptan, propanethiol, butanethiol, pentanethiol, hexanethiol, octadecanethiol, dodecanethiol, hexadecanethiol, octadecanethiol or benzyl mercaptan; and the (oxygen) phosphine ligand is selected from at least one of methyl phosphine, ethyl phosphine, propyl phosphine, butyl phosphine, pentyl phosphine, octyl phosphine, dioctyl phosphine, tributyl phosphine or trioctyl phosphine.
[0047] In some embodiments, the thickness of the functional layer is 3-10 nm, the thickness of the light-emitting layer is 10-50 nm, and the thickness of the charge functional layer is 10-50 nm.
[0048] In the present embodiment, the charge functional layer is an electron transport layer. It is understandable that if the functional layer is too thick, the voltage drop between the light-emitting layer and the charge functional layer will increase, resulting in the inability to inject carriers or less injection, thereby reducing the luminous efficiency of the light-emitting device. If the functional layer is too thin, there will be a part of the interface between the light-emitting layer and the charge functional layer that is not effectively supported by the organic metal framework of ferrocene and / or ferrocene derivatives, which will lead to the existence of relatively serious aging phenomenon in this part of the interface. Preferably, the thickness of the functional layer is 3-10nm, the thickness of the light-emitting layer is 10-50nm, and the thickness of the charge functional layer is 10-50nm, wherein the thickness of the light-emitting layer and the thickness of the charge functional layer can be set to be the same or different.
[0049] In some embodiments, a hole functional layer is disposed between the light-emitting layer and the first electrode, and the hole functional layer includes a hole injection layer and / or a hole transport layer.
[0050] The material of the hole transport layer and / or the hole injection layer includes at least one of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tris(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.
[0051] Specifically, the thickness of the hole injection layer is 10-50 nm, and the thickness of the hole transport layer is 10-50 nm, wherein the thickness of the hole injection layer and the hole transport layer can be set to be the same or different, and no further limitation is made in this embodiment.
[0052] On the other hand, an embodiment of the present invention also provides a method for preparing a light emitting device, wherein the light emitting device is a positive type device, such as Figure 2 As shown, the following steps are included:
[0053] S10, providing a first electrode;
[0054] S20, providing a light-emitting layer on the first electrode;
[0055] S30, disposing a functional layer on the light-emitting layer;
[0056] S40, disposing a functional layer on the light-emitting layer;
[0057] S50, disposing a second electrode on the charge functional layer and encapsulating it;
[0058] Wherein, the material of the functional layer includes ferrocene and / or a derivative of ferrocene as shown in the following formula I:
[0059]
[0060] In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
[0061] An embodiment of the present invention provides a method for preparing a positive light-emitting device, wherein the material of the light-emitting layer includes a quantum dot light-emitting material, the material of the charge functional layer includes a metal oxide, the material of the functional layer includes ferrocene and / or a derivative of ferrocene, and ferrocene and / or a derivative of ferrocene can be used as an electron transfer medium material to bridge the light-emitting layer and the charge functional layer to achieve stable electron transfer from the charge functional layer to the light-emitting layer through the functional layer, thereby balancing electron injection and hole injection, reducing the existing exciton quenching caused by the unbalanced recombination of holes and electrons in the light-emitting layer, and improving the luminescence efficiency of the light-emitting device.
[0062] Furthermore, in this embodiment, the functional layer can effectively slow down the aging of the material of the interface layer between the light-emitting layer and the charge functional layer. At the same time, the probability of the organic ligand bound to the quantum dot light-emitting material on the surface of the light-emitting layer falling off is reduced, and the defects on the surface of the light-emitting layer are also reduced, thereby improving the luminous efficiency of the light-emitting device. In addition, because ferrocene and / or ferrocene derivatives themselves belong to electron-rich materials, they can also enhance the transmission of electrons to a certain extent, thereby helping to improve the luminous efficiency of the light-emitting device.
[0063] For the preparation method of a positive light-emitting device, the first electrode provided in step S10 is an anode disposed on a substrate, wherein the material of the first electrode includes one or more of a metal, a carbon material and a metal oxide, the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes doped or undoped metal oxides, including ITO, FTO, ATO, A One or more of ZO, GZO, IZO, MZO and AMO, or a composite electrode comprising a metal sandwiched between doped or undoped transparent metal oxides, the composite electrode comprising one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2.
[0064] In some embodiments, preparing a light-emitting layer on the first electrode in step S20 includes: dispersing one or more quantum dots in an organic solvent to prepare a quantum dot solution, and then depositing the quantum dot solution on the surface of the first electrode to prepare the light-emitting layer.
[0065] Specifically, the light-emitting layer is a quantum dot light-emitting layer; the material of the quantum dot light-emitting layer includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSe At least one of Te, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the IV-VI group compound is selected from SnS, SnSe, SnTe, PbS, PbSe, Pb At least one of SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, wherein the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, A At least one of lPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2.
[0066] The core of the core-shell structured quantum dots includes any one of the above-mentioned single structure quantum dots, and the shell material of the core-shell structured quantum dots includes CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and at least one of the above-mentioned single structure quantum dots.
[0067] In some embodiments, preparing a functional layer on the light-emitting layer in step S30 includes: dispersing one or more of ferrocene and / or ferrocene derivatives in an organic solvent to obtain a mixed solution with a concentration of 5-10 mg / ml, and then depositing the mixed solution on the light-emitting layer to prepare the functional layer.
[0068] Specifically, the thickness of the functional layer is 3-10 nm. In the present embodiment, if the functional layer is too thick, the voltage drop between the light-emitting layer and the charge functional layer will increase, resulting in the inability to inject carriers or less injection, thereby reducing the luminous efficiency of the light-emitting device. If the functional layer is too thin, there will be a part of the interface between the light-emitting layer and the charge functional layer that is not effectively supported by the organic metal framework of ferrocene and / or ferrocene derivatives, resulting in relatively serious aging of the part of the interface.
[0069] In some embodiments, preparing a charge functional layer on the functional layer in step S40 includes: dispersing one or more metal oxides in an organic solvent to prepare a metal oxide solution, and then depositing the metal oxide solution on the functional layer to prepare the charge functional layer.
[0070] Among them, the charge functional layer is an electron transport layer, and the concentration of the metal oxide solution is 10-50 mg / ml. It should be noted that the concentration of the metal oxide solution cannot be too high. If the concentration is too high, the probability of collision between particles in the metal oxide solution will increase, resulting in agglomeration, and the thickness of the prepared film of the charge functional layer will be too large, resulting in corresponding obstruction of charge transport. If the concentration is too low, the thickness of the prepared film of the charge functional layer will be uneven, thereby affecting the performance of the prepared light-emitting device.
[0071] Specifically, the charge functional layer includes a metal oxide, the material of the metal oxide is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium.
[0072] In some embodiments, the second electrode is prepared on the charge functional layer by evaporation, and the second electrode is a cathode disposed on a substrate. The material of the second electrode includes one or more of a metal, a carbon material, and a metal oxide. The metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene, and carbon fiber; the metal oxide includes a doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, or includes a doped or undoped transparent metal oxide. A composite electrode with a metal sandwiched between the materials, the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2, wherein the thickness of the second electrode is 60-100nm. It should be noted that the thickness of the second electrode cannot be set too thin. If the thickness of the second electrode is too thin, it is easy to cause uneven evaporation, thereby affecting the luminous efficiency of the prepared light-emitting device.
[0073] In some embodiments, before the step of preparing a second electrode on the charge functional layer and encapsulating it, the method further comprises:
[0074] The light-emitting layer, the functional layer and the charge functional layer are subjected to a heating treatment at 80-120° C. for 5-30 minutes.
[0075] In this embodiment, after the charge functional layer is prepared on the functional layer, the stack formed by the light-emitting layer, the functional layer and the charge functional layer is further subjected to a heat treatment at 80-120° C. By heating the stack, the ferrocene and / or ferrocene derivatives of the functional layer can effectively bridge the light-emitting layer and the charge functional layer to form an organic metal framework structure. It should be noted that the heating temperature should not be too high. If the heating temperature is too high, the prepared film layer will be destroyed, resulting in the performance of the prepared light-emitting device being affected.
[0076] In some embodiments, the step S20 of providing a light-emitting layer on the first electrode includes:
[0077] A hole functional layer is arranged on the first electrode, and then a light emitting layer is arranged on the hole functional layer, wherein the hole functional layer includes a hole transport layer and / or the hole injection layer.
[0078] Among them, the material of the hole transport layer and / or the hole injection layer includes at least one of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tri(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.
[0079] Specifically, in this embodiment, the first electrode on the substrate is first subjected to ultraviolet treatment for 10-30 minutes, preferably for 15 minutes, and then a solution containing the hole injection layer material is spin-coated on the first electrode, and the solvent is removed by heating and annealing is performed to prepare the hole injection layer. The material of the hole injection layer is PEDOT:PSS with a doping ratio of 1:6, and the content of PEDOT:PSS as a solute in the prepared PEDOT:PSS solution is 1.5wt%, and the thickness of the obtained hole injection layer is 10-50nm.
[0080] Furthermore, in this embodiment, a solution containing the hole transport layer material is spin-coated on the prepared hole injection layer, and the hole transport layer is prepared by heating to remove the solvent and annealing. Preferably, the hole transport layer has a thickness of 10-50 nm.
[0081] Furthermore, an embodiment of the present invention also provides a method for preparing a light emitting device, wherein the light emitting device is an inverted device, such as Figure 3 As shown, the following steps are included:
[0082] E10, providing a second electrode;
[0083] E20, providing a charge functional layer on the second electrode;
[0084] E30, providing a functional layer on the charge functional layer;
[0085] E40, providing a light-emitting layer on the functional layer;
[0086] E50. Dispose a first electrode on the light-emitting layer and perform encapsulation.
[0087] Wherein, the material of the functional layer includes ferrocene and / or a derivative of ferrocene as shown in the following formula I:
[0088]
[0089] In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
[0090] An embodiment of the present invention provides a method for preparing an inverted light-emitting device, wherein the material of the light-emitting layer includes a quantum dot light-emitting material, the material of the charge functional layer includes a metal oxide, the material of the functional layer includes ferrocene and / or a derivative of ferrocene, and ferrocene and / or a derivative of ferrocene can be used as an electron transfer medium material to bridge the light-emitting layer and the charge functional layer to achieve stable electron transfer from the charge functional layer to the light-emitting layer through the functional layer, thereby balancing electron injection and hole injection, reducing the existing exciton quenching caused by the imbalance of recombination of holes and electrons in the light-emitting layer, and improving the luminescence efficiency of the light-emitting device.
[0091] Furthermore, in this embodiment, the functional layer can effectively slow down the aging of the material of the interface layer between the light-emitting layer and the charge functional layer. At the same time, the probability of the organic ligand bound to the quantum dot light-emitting material on the surface of the light-emitting layer falling off is reduced, and the defects on the surface of the light-emitting layer are also reduced, thereby improving the luminous efficiency of the light-emitting device. In addition, because ferrocene and / or ferrocene derivatives themselves belong to electron-rich materials, they can also enhance the transmission of electrons to a certain extent, thereby helping to improve the luminous efficiency of the light-emitting device.
[0092] For the preparation method of an inverted light-emitting device, the second electrode provided in step E10 is a cathode disposed on a substrate, wherein the material of the second electrode includes one or more of a metal, a carbon material, and a metal oxide, the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene, and carbon fibers; the metal oxide includes a doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, the composite The combined electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2, wherein the thickness of the second electrode is 60-100nm, and the substrate is one of ITO, fluorine-doped tin oxide (FTO), aluminum-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), indium-doped zinc oxide (IZO), magnesium-doped zinc oxide (MZO), and aluminum-doped magnesium oxide (AMO). It should be noted that the thickness of the second electrode cannot be set too thin. If the thickness of the second electrode is too thin, it is easy to cause uneven evaporation, thereby affecting the luminous efficiency of the prepared light-emitting device.
[0093] In some embodiments, preparing a charge functional layer on the second electrode in step E20 includes: dispersing one or more metal oxides in an organic solvent to prepare a metal oxide solution, and then depositing the metal oxide solution on the second electrode to prepare the charge functional layer.
[0094] Among them, the charge functional layer is an electron transport layer, and the concentration of the metal oxide solution is 10-50 mg / ml. It should be noted that the concentration of the metal oxide solution cannot be too high. If the concentration is too high, the probability of collision between particles in the metal oxide solution will increase, resulting in agglomeration. In addition, the thickness of the prepared film of the charge functional layer is too large, which can easily lead to obstruction of charge transport. If the concentration is too low, the thickness of the prepared film of the charge functional layer will be uneven, thereby affecting the performance of the prepared light-emitting device.
[0095] Specifically, the charge functional layer includes a metal oxide, the material of the metal oxide is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium.
[0096] In some embodiments, preparing a functional layer on the charge functional layer in step E30 includes: dispersing one or more of ferrocene and / or ferrocene derivatives in an organic solvent to obtain a mixed solution with a concentration of 5-10 mg / ml, and then depositing the mixed solution on the charge functional layer to prepare the functional layer.
[0097] Specifically, the thickness of the functional layer is 3-10 nm. In the present embodiment, if the functional layer is too thick, the voltage drop between the light-emitting layer and the charge functional layer will increase, resulting in the inability to inject carriers or less injection, thereby reducing the luminous efficiency of the light-emitting device. If the functional layer is too thin, there will be a part of the interface between the light-emitting layer and the charge functional layer that is not effectively supported by the organic metal framework of ferrocene and / or ferrocene derivatives, resulting in relatively serious aging of the part of the interface.
[0098] In some embodiments, preparing a light-emitting layer on the functional layer in step E40 includes: dispersing one or more quantum dots in an organic solvent to prepare a quantum dot solution, and then depositing the quantum dot solution on the surface of the functional layer to obtain the light-emitting layer.
[0099] In some embodiments, the first electrode is prepared on the light-emitting layer by evaporation, and the first electrode is an anode. The material of the first electrode includes one or more of a metal, a carbon material, and a metal oxide, and the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb, and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene, and carbon fiber; the metal oxide includes a doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO, and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2, and TiO2 / Al / TiO2.
[0100] It should be noted that, in this embodiment, before the step of providing the first electrode on the light-emitting layer and performing packaging in step E50, the following steps are also included:
[0101] The light-emitting layer, the functional layer and the charge functional layer are subjected to a heating treatment at 80-120° C. for 5-30 minutes.
[0102] In this embodiment, after the light-emitting layer is prepared on the functional layer, the light-emitting layer, the functional layer and the charge functional layer are further subjected to heat treatment at 80-120° C. By heating the stack composed of the light-emitting layer, the functional layer and the charge functional layer, the ferrocene and / or ferrocene derivatives of the functional layer can effectively bridge the light-emitting layer and the charge functional layer to form an organic metal framework structure. It should be noted that the heating temperature should not be too high. If the heating temperature is too high, the prepared film layer will be destroyed, resulting in the performance of the prepared light-emitting device being affected.
[0103] In some embodiments, the step of providing a first electrode on the light-emitting layer and performing packaging in step E50 further includes:
[0104] A hole functional layer is arranged on the light emitting layer, and then the first electrode is arranged on the hole functional layer and encapsulated, wherein the hole functional layer includes a hole transport layer and / or the hole injection layer.
[0105] Specifically, the material of the hole transport layer and / or the hole injection layer includes at least one of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tris(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.
[0106] Specifically, in this embodiment, a solution containing the hole injection layer material is spin-coated on the light-emitting layer, and the solvent is removed by heating and annealing is performed to obtain the hole injection layer. The heating temperature is 100-200°C, the heating time is 10-30 minutes, the material of the hole injection layer is PEDOT:PSS with a doping ratio of 1:6, and the content of PEDOT:PSS as a solute in the prepared PEDOT:PSS solution is 1.5wt%, and the thickness of the obtained hole injection layer is 10-50nm.
[0107] Furthermore, in this embodiment, a solution containing the hole transport layer material is spin-coated on the prepared hole injection layer, and the hole transport layer is prepared by heating to remove the solvent and annealing. Preferably, the hole transport layer has a thickness of 10-50 nm.
[0108] The following is a further explanation of a method for preparing a photoelectric device of the present invention through specific examples:
[0109] Example 1
[0110] This embodiment is a positive type photoelectric device, and the preparation steps are as follows:
[0111] The ITO glass sheet was placed in a glass dish filled with ethanol solution, and ultrasonicated with acetone, deionized water, and ethanol for 20 minutes in sequence, and then dried with a nitrogen gun; then, the cleaned ITO glass sheet was placed in oxygen plasma for further cleaning for 10 minutes; the surface of the ITO substrate was treated with ultraviolet-ozone irradiation for 15 minutes to obtain an anode;
[0112] Spin coating a PEDOT:PSS dispersion with a concentration of 1.5 wt% on the above ITO substrate at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole injection layer with a thickness of 30 nm;
[0113] Spin coating a dispersion of TFB with a concentration of 20 mg / mL on the surface of the hole injection layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole transport layer with a thickness of 15 nm;
[0114] Spin coating a 20 mg / mL CdSe n-octane solution on the surface of the hole transport layer away from the hole injection layer at a rotation speed of 2000 r / min for 30 s to form a light-emitting layer with a thickness of 30 nm;
[0115] Spin coating a dispersion of ferrocenecarboxylic acid with a concentration of 5 mg / mL on the surface of the light-emitting layer away from the hole transport layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a functional layer with a thickness of 3 nm;
[0116] A ZnO dispersion with a concentration of 30 mg / mL was spin-coated on the surface of the functional layer away from the light-emitting layer at a rotation speed of 3000 r / min for 30 s, and annealed at 80° C. for 30 min to form a charge functional layer with a thickness of 50 nm, i.e., an electron transport layer, and then heated at 80° C. for 10 min;
[0117] At a vacuum degree of 1x10 -6 Under the condition of mbar, Ag was sequentially evaporated on the charge functional layer at a rate of 1 angstrom / second for 100 seconds to form a 100 nm metal layer;
[0118] Encapsulation is performed to obtain a quantum dot light emitting diode.
[0119] Example 2
[0120] This embodiment is a positive type photoelectric device, and the preparation steps are as follows:
[0121] The ITO glass sheet was placed in a glass dish filled with ethanol solution, and ultrasonicated with acetone, deionized water, and ethanol for 20 minutes in sequence, and then dried with a nitrogen gun; then, the cleaned ITO glass sheet was placed in oxygen plasma for further cleaning for 10 minutes; the surface of the ITO substrate was treated with ultraviolet-ozone irradiation for 15 minutes to obtain an anode;
[0122] Spin coating a PEDOT:PSS dispersion with a concentration of 1.5 wt% on the above ITO substrate at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole injection layer with a thickness of 30 nm;
[0123] Spin coating a dispersion of TFB with a concentration of 20 mg / mL on the surface of the hole injection layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole transport layer with a thickness of 15 nm;
[0124] Spin coating a 20 mg / mL CdSe n-octane solution on the surface of the hole transport layer away from the hole injection layer at a rotation speed of 2000 r / min for 30 s to form a light-emitting layer with a thickness of 30 nm;
[0125] Spin coating a dispersion of ferrocenecarboxylic acid with a concentration of 5 mg / mL on the surface of the light-emitting layer away from the hole transport layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a functional layer with a thickness of 5 nm;
[0126] A ZnO dispersion with a concentration of 30 mg / mL was spin-coated on the surface of the functional layer away from the light-emitting layer at a rotation speed of 3000 r / min for 30 s, and annealed at 80° C. for 30 min to form a charge functional layer with a thickness of 50 nm, i.e., an electron transport layer, and then heated at 80° C. for 10 min;
[0127] At a vacuum degree of 1x10 -6 Under the condition of mbar, Ag was sequentially evaporated on the charge functional layer at a rate of 1 angstrom / second for 100 seconds to form a 100 nm metal layer;
[0128] Encapsulation is performed to obtain a quantum dot light emitting diode.
[0129] Example 3
[0130] This embodiment is a positive type photoelectric device, and the preparation steps are as follows:
[0131] The ITO glass sheet was placed in a glass dish filled with ethanol solution, and ultrasonicated with acetone, deionized water, and ethanol for 20 minutes in sequence, and then dried with a nitrogen gun; then, the cleaned ITO glass sheet was placed in oxygen plasma for further cleaning for 10 minutes; the surface of the ITO substrate was treated with ultraviolet-ozone irradiation for 15 minutes to obtain an anode;
[0132] Spin coating a PEDOT:PSS dispersion with a concentration of 1.5 wt% on the above ITO substrate at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole injection layer with a thickness of 30 nm;
[0133] Spin coating a dispersion of TFB with a concentration of 20 mg / mL on the surface of the hole injection layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole transport layer with a thickness of 15 nm;
[0134] Spin coating a 20 mg / mL CdSe n-octane solution on the surface of the hole transport layer away from the hole injection layer at a rotation speed of 2000 r / min for 30 s to form a light-emitting layer with a thickness of 30 nm;
[0135] Spin coating a dispersion of ferrocenecarboxylic acid with a concentration of 5 mg / mL on the surface of the light-emitting layer away from the hole transport layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a functional layer with a thickness of 8 nm;
[0136] A ZnO dispersion with a concentration of 30 mg / mL was spin-coated on the surface of the functional layer away from the light-emitting layer at a rotation speed of 3000 r / min for 30 s, and annealed at 80° C. for 30 min to form a charge functional layer with a thickness of 50 nm, i.e., an electron transport layer, and then heated at 80° C. for 10 min;
[0137] At a vacuum degree of 1x10 -6 Under the condition of 100 mbar, Ag was sequentially evaporated on the charge functional layer at a rate of 1 angstrom / second for 100 s to form a 100 nm metal layer;
[0138] Encapsulation is performed to obtain a quantum dot light emitting diode.
[0139] Example 4
[0140] This embodiment is a positive type photoelectric device, and the preparation steps are as follows:
[0141] The ITO glass sheet was placed in a glass dish filled with ethanol solution, and ultrasonicated with acetone, deionized water, and ethanol for 20 minutes in sequence, and then dried with a nitrogen gun; then, the cleaned ITO glass sheet was placed in oxygen plasma for further cleaning for 10 minutes; the surface of the ITO substrate was treated with ultraviolet-ozone irradiation for 15 minutes to obtain an anode;
[0142] Spin coating a PEDOT:PSS dispersion with a concentration of 1.5 wt% on the above ITO substrate at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole injection layer with a thickness of 30 nm;
[0143] Spin coating a dispersion of TFB with a concentration of 20 mg / mL on the surface of the hole injection layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole transport layer with a thickness of 15 nm;
[0144] Spin coating a 20 mg / mL CdSe n-octane solution on the surface of the hole transport layer away from the hole injection layer at a rotation speed of 2000 r / min for 30 s to form a light-emitting layer with a thickness of 30 nm;
[0145] Spin coating a dispersion of ferrocenecarboxylic acid with a concentration of 5 mg / mL on the surface of the light-emitting layer away from the hole transport layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a functional layer with a thickness of 10 nm;
[0146] A ZnO dispersion with a concentration of 30 mg / mL was spin-coated on the surface of the functional layer away from the light-emitting layer at a rotation speed of 3000 r / min for 30 s, and annealed at 80° C. for 30 min to form a charge functional layer with a thickness of 50 nm, i.e., an electron transport layer, and then heated at 80° C. for 10 min;
[0147] At a vacuum degree of 1x10 -6 Under the condition of 100 mbar, Ag was sequentially evaporated on the charge functional layer at a rate of 1 angstrom / second for 100 s to form a 100 nm metal layer;
[0148] Encapsulation is performed to obtain a quantum dot light emitting diode.
[0149] Comparative Example 1
[0150] This comparative example is a positive photoelectric device, and the specific steps are as follows:
[0151] The ITO glass sheet was placed in a glass dish filled with ethanol solution, and ultrasonicated with acetone, deionized water, and ethanol for 20 minutes in sequence, and then dried with a nitrogen gun; then, the cleaned ITO glass sheet was placed in oxygen plasma for further cleaning for 10 minutes; the surface of the ITO substrate was treated with ultraviolet-ozone irradiation for 15 minutes to obtain an anode;
[0152] Spin coating a PEDOT:PSS dispersion with a concentration of 1.5 wt% on the above ITO substrate at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole injection layer with a thickness of 30 nm;
[0153] Spin coating a dispersion of TFB with a concentration of 20 mg / mL on the surface of the hole injection layer at a rotation speed of 3000 r / min for 30 s, and annealing at 80° C. for 30 min to form a hole transport layer with a thickness of 15 nm;
[0154] Spin coating a 20 mg / mL CdSe n-octane solution on the surface of the hole transport layer away from the hole injection layer at a rotation speed of 2000 r / min for 30 s to form a light-emitting layer with a thickness of 30 nm;
[0155] A ZnO dispersion with a concentration of 30 mg / mL was spin-coated on the surface of the light-emitting layer away from the hole transport layer at a rotation speed of 3000 r / min for 30 s, and annealed at 80° C. for 30 min to form a charge functional layer with a thickness of 50 nm, i.e., an electron transport layer, and then heated at 80° C. for 10 min;
[0156] At a vacuum degree of 1x10 -6 Under the condition of 100 mbar, Ag was sequentially evaporated on the charge functional layer at a rate of 1 angstrom / second for 100 s to form a 100 nm metal layer;
[0157] Encapsulation is performed to obtain a quantum dot light emitting diode.
[0158] Furthermore, in order to verify the advancement of the light-emitting device prepared in the embodiment of the present invention, the performance of the light-emitting devices prepared in each embodiment and comparative example was tested, wherein the life test method is as follows: the test environment is 25°C and 60RH%, the light-emitting device is driven at a constant current of 2mA, the brightness change of the light-emitting device is tested using a silicon photonic system, and the time required for the maximum brightness of the light-emitting device to decay from 100% to 95% after the light-emitting device is powered on is recorded.
[0159] The external quantum efficiency (EQE) detection method is: using FPD optical characteristic equipment, controlling the QE PRO spectrometer, Keithley2400, and Keithley6485 efficiency test system through Lab View, measuring parameters such as voltage, current, brightness, and luminous spectrum, and calculating the external quantum efficiency EQE. Among them, the voltage when the brightness of the light-emitting device reaches 1nite is the start-up voltage. The test results are shown in the following table:
[0160] sample EQE(%) Lifespan (h) Example 1 11.5 8114.6 Example 2 11.93 8571.3 Example 3 13.24 10350.7 Example 4 12.65 9655.8 Comparative Example 1 10.06 6858.9
[0161] It can be seen from the data in the table that the external quantum efficiency of the light-emitting devices of Examples 1 to 4 is significantly higher than that of the light-emitting device of Comparative Example 1. It can be understood that in Examples 1 to 4, the functional layer is arranged between the light-emitting layer and the charge functional layer. The functional layer can balance the recombination of holes and electrons in the light-emitting layer, and weaken the exciton quenching caused by the imbalance of recombination of holes and electrons in the light-emitting layer, so that the luminescence efficiency of the prepared light-emitting device is improved. At the same time, the aging of the material of the interface layer between the light-emitting layer and the charge functional layer can be effectively slowed down by setting the functional layer, and the probability of the organic ligand bound to the quantum dot light-emitting material on the surface of the light-emitting layer falling off is reduced, and the defects on the surface of the light-emitting layer are also reduced. To a certain extent, the luminescence efficiency of the prepared light-emitting device is also improved.
[0162] At the same time, it can be seen from the data in the table that the lifespan of the light-emitting devices of Examples 1 to 4 is also significantly higher than that of Comparative Example 1. It can be understood that in Examples 1 to 4, the functional layer set up can effectively slow down the aging of the material of the interface layer between the light-emitting layer and the charge functional layer, thereby improving the lifespan of the prepared light-emitting device. However, when the thickness of the functional layer is too large, the voltage drop between the light-emitting layer and the charge functional layer is increased, which will have a negative impact on the lifespan of the prepared light-emitting device.
[0163] Therefore, in the present invention, the functional layer is arranged between the light-emitting layer and the charge functional layer, and the ferrocene and / or ferrocene derivatives in the functional layer can serve as electron transfer medium materials to bridge the light-emitting layer and the charge functional layer. On the one hand, stable electron transfer from the charge functional layer to the light-emitting layer through the functional layer is achieved, and the electron injection and hole injection at the light-emitting layer are balanced, thereby improving the luminous efficiency of the prepared light-emitting device. On the other hand, the aging of the material of the interface layer between the light-emitting layer and the charge functional layer is effectively slowed down by the arrangement of the functional layer. At the same time, the probability of the organic ligand bound to the quantum dot light-emitting material on the surface of the light-emitting layer falling off is also reduced, and the defects on the surface of the light-emitting layer are also reduced, thereby to a certain extent, the luminous efficiency of the prepared light-emitting device can also be improved.
[0164] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A light-emitting device, comprising a first electrode, a light-emitting layer, a functional layer, a charge functional layer, and a second electrode stacked in sequence, characterized in that: The material of the functional layer includes ferrocene and / or a derivative of ferrocene as shown in the following formula I: In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
2. The light emitting device according to claim 1, characterized in that: In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C10 chain alkyl, substituted or unsubstituted C1-C10 alkoxy, substituted or unsubstituted cycloalkyl having 4-20 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-20 ring atoms, substituted or unsubstituted aryl having 6-20 ring atoms, substituted or unsubstituted heteroaryl having 6-20 ring atoms, and n1 and n2 are independently selected from 0 to 2.
3. The light emitting device according to claim 2, characterized in that: The ferrocene derivative is one or more of 1,1'-bis(phenylphosphino)ferrocene, 1,1'-ferrocene diboronate, 1,1'-ferrocene dicarboxylic acid, ferrocenecarboxylic acid, bromoferrocene, ferrocenyl acetic acid, and o-ferrocenylformylbenzoic acid.
4. The light emitting device according to claim 3, characterized in that: The light-emitting layer is a quantum dot light-emitting layer, and the material of the quantum dot light-emitting layer includes at least one of a single structure quantum dot and a core-shell structure quantum dot. The material of the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, Z At least one of CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, wherein the Group IV-VI compound is selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, At least one of SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPA s, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; and / or The core of the core-shell structured quantum dots comprises any one of the above-mentioned single structured quantum dots, and the shell material of the core-shell structured quantum dots comprises at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and the above-mentioned single structured quantum dots; and / or The charge functional layer comprises a metal oxide, wherein the material of the metal oxide is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium; and / or, The material of the first electrode and / or the second electrode includes one or more of metals, carbon materials and metal oxides, the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes doped or undoped metal oxides, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2.
5. The light emitting device according to claim 1, characterized in that: The thickness of the functional layer is 3-10 nm; and / or The thickness of the light-emitting layer is 10-50 nm; and / or The charge functional layer is an electron transport layer, and the thickness of the layer is 10-50 nm.
6. The light emitting device according to any one of claims 1 to 5, characterized in that: A hole functional layer is disposed between the light-emitting layer and the first electrode, and the hole functional layer includes a hole injection layer and / or a hole transport layer; and / or The material of the hole transport layer and / or the hole injection layer includes at least one of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tris(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.
7. A method for preparing a light emitting device, characterized in that: include: providing a first electrode; Disposing a light-emitting layer on the first electrode; Disposing a functional layer on the light-emitting layer; Disposing a charge functional layer on the functional layer; as well as Disposing a second electrode on the charge functional layer and encapsulating it; or providing a second electrode; providing a charge functional layer on the second electrode; Disposing a functional layer on the charge functional layer; disposing a light-emitting layer on the functional layer; and Disposing a first electrode on the light-emitting layer and encapsulating it; Wherein, the material of the functional layer includes ferrocene and / or a derivative of ferrocene as shown in the following formula I: In formula (I), R1 and R2 are each independently selected from one or more combinations of hydrogen, halogen, hydroxyl, carboxyl, nitro, sulfonic acid, aldehyde, mercapto, cyano, substituted or unsubstituted C1-C20 chain alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted cycloalkyl having 4-60 ring atoms, substituted or unsubstituted heterocycloalkyl having 4-60 ring atoms, substituted or unsubstituted aryl having 6-60 ring atoms, substituted or unsubstituted heteroaryl having 6-60 ring atoms, and n1 and n2 are independently selected from 0-5.
8. The method for preparing a light emitting device according to claim 7, characterized in that: Before the step of arranging a second electrode on the charge functional layer and encapsulating the layer, the method further comprises: The light emitting layer, the functional layer and the charge functional layer are subjected to a heating treatment at 80 to 120° C. for 5 to 30 minutes.
9. The method for preparing a light emitting device according to claim 7, characterized in that: The material of the first electrode and / or the second electrode includes one or more of metal, carbon material and metal oxide, the metal includes one or more of Al, Ag, Cu, Mo, Au, Ba, Ca, Yb and Mg; the carbon material includes one or more of graphite, carbon nanotubes, graphene and carbon fiber; the metal oxide includes doped or undoped metal oxide, including one or more of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO, or includes a composite electrode in which a metal is sandwiched between doped or undoped transparent metal oxides, and the composite electrode includes one or more of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2; and / or The light-emitting layer is a quantum dot light-emitting layer; the material of the quantum dot light-emitting layer includes at least one of a single structure quantum dot and a core-shell structure quantum dot, and the material of the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound, wherein the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, Z At least one of CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, wherein the Group IV-VI compound is selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, At least one of SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPA s, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs or InAlPSb, and the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; and / or The core of the core-shell structured quantum dots comprises any one of the above-mentioned single structured quantum dots, and the shell material of the core-shell structured quantum dots comprises at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS, ZnS and the above-mentioned single structured quantum dots; and / or The charge functional layer includes a metal oxide, the material of which is selected from one or more of doped or undoped zinc oxide, barium oxide, aluminum oxide, nickel oxide, titanium oxide, tin oxide, tantalum oxide, zirconium oxide, nickel oxide, lithium titanium oxide, zinc aluminum oxide, zinc manganese oxide, zinc tin oxide, lithium zinc oxide, indium tin oxide, cadmium sulfide, zinc sulfide, molybdenum sulfide, tungsten sulfide, copper sulfide, zinc tin, indium phosphide, gallium phosphide, copper indium sulfide, copper gallium sulfide, and barium titanate, and the doped elements include one or more of aluminum, magnesium, lithium, manganese, yttrium, lanthanum, copper, nickel, zirconium, cerium, and gadolinium.
10. The method for preparing a light emitting device according to claim 7, characterized in that: The step of providing a light-emitting layer on the first electrode comprises: A hole functional layer is arranged on the first electrode, and then a light emitting layer is arranged on the hole functional layer, wherein the hole functional layer includes a hole transport layer and / or the hole injection layer; and / or The step of providing a first electrode on the light-emitting layer and encapsulating the first electrode comprises: Arranging a hole functional layer on the light-emitting layer, and then arranging the first electrode on the hole functional layer and encapsulating it, wherein the hole functional layer includes a hole transport layer and / or the hole injection layer; and / or The material of the hole transport layer and / or the hole injection layer includes at least one of TFB, CuPc, PVK, Poly-TPD, DNTPD, TCATA, TCCA, CBP, TPD, NPB, NPD, PEDOT:PSS, TAPC, MCC, F4-TCNQ, HATCN, 4,4',4'-tris(N-3-methylphenyl-Nphenylamino)triphenylamine, polyaniline, transition metal oxides, transition metal sulfides, transition metal tinides, doped graphene, undoped graphene and C60.