Gas separation membrane

By using an additional layer and a discriminating layer containing specific metal oxygen groups in the gas separation membrane, combined with a support and a protective layer, the problem of lowering breathability in the prior art is solved, and efficient gas separation and purification effects are achieved.

CN118946398APending Publication Date: 2024-11-12YESTAR ADVANCED MATERIALS (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030342.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the conventional gas separation membrane contains a polysiloxane protective layer, the air permeability is reduced and it is difficult to have both a protective layer and good air permeability, which affects its gas separation performance.

Method used

A gas separation membrane structure including a support, a discriminating layer, an additional layer and a protective layer, wherein the additional layer and the discriminating layer contain specific metal or metal-like oxygen groups, respectively, are formed by plasma treatment to improve the breathability of the film and Selective.

Benefits of technology

It realizes the air permeability and selectivity of the gas separation membrane while maintaining the protective layer function, enhances the mechanical strength and durability of the membrane, and is suitable for gas separation and purification applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059451260000041
    Figure BDA0005059451260000041
  • Figure BDA0005059451260000141
    Figure BDA0005059451260000141
  • Figure BDA0005059451260000161
    Figure BDA0005059451260000161
Patent Text Reader

Abstract

A gas separation membrane comprising the following layers: (i) an optional support layer; (ii) a discriminating layer; (iii) an additional layer; and (iv) optionally a protective layer; wherein (a) the additional layer (iii) and the discrimination layer (ii) each independently comprise a group of formula (1): M-(O-) x formula (1) wherein each M is independently a metal or metalloid atom; o is an oxygen atom; and the value of each x is independently at least 4; (b) the additional layer (iii) comprises 1.5 to 10 at% of M of a group of formula (1) wherein M is as defined above; and (c) the discrimination layer (ii) comprises more than 10 atom% of M of a group of formula (1), where M is as defined above.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application relates to gas separation membranes (GSMs) and their preparation and use.

[0002] Gas separation membranes typically consist of a support (for mechanical strength) and a discriminating layer for distinguishing between the gases to be separated. A protective layer is often included above the discriminating layer to protect it from mechanical damage during processes such as handling and use of the membrane. Damage to the discriminating layer can have adverse consequences, such as significantly reducing the selectivity of the gas separation membrane.

[0003] Typically, the protective layer comprises polysiloxane and is formed on the discriminating layer by a wet chemical coating process.

[0004] Although protective layers comprising polysiloxanes are useful for protecting the discriminating layer from damage, they also significantly reduce the breathability of the GSM. There is a need for a GSM comprising a protective layer and having good breathability.

[0005] According to a first aspect of the present invention, there is provided a gas separation membrane comprising the following layers:

[0006] (i) an optional support layer;

[0007] (ii) discrimination layer;

[0008] (iii) additional layers; and

[0009] (iv) an optional protective layer;

[0010] in,

[0011] (a) The additional layer (iii) and the discriminating layer (ii) each independently comprise a group of formula (1):

[0012] M-(O-) x

[0013] Formula (1)

[0014] in:

[0015] Each M is independently a metal or metalloid atom;

[0016] O is an oxygen atom; and

[0017] Each value of x is independently at least 4;

[0018] (b) the additional layer (iii) comprises 1.5 to 10 atomic % of M groups of formula (1), wherein M is as defined above; and

[0019] (c) The discriminating layer (ii) comprises more than 10 atomic % of M groups of formula (1), wherein M is as defined above.

[0020] In this specification, the term "comprising" should be interpreted as requiring the presence of the stated parts, steps, or components, but does not exclude the presence of one or more additional parts, steps, or components. The use of the indefinite article "a" or "an" to refer to an element does not exclude the possibility of more than one element being present, unless the context clearly requires one and only one element. The optional groove layer (see below) is often referred to as "GL", the discrimination layer (ii) is often referred to as "DL", the additional layer (iii) is sometimes referred to as "FL", and the optional protective layer (iv) is often referred to as "PL".

[0021] In this specification, the separation or discrimination layer (ii) means a layer having separation selectivity. The layer having separation selectivity means a layer in which, when a membrane having a thickness of 0.05 to 30 μm is formed and pure gases of carbon dioxide (CO 2 ) and methane (CH 4 ) are supplied to the resulting membrane at 40° C. by setting the total pressure on the gas supply side to 0.5 MPa, the permeability coefficient (P CO2 ) and the permeability coefficient of methane (P CH4 ) ratio (P CO2 / P CH4 ) is above 10. This is in contrast to the additional layer (iii), which has no gas separation selectivity and has a selectivity much less than 10, even more preferably less than 5. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In the attached figure:

[0023] Figure 1 (a) is a schematic vertical cross-sectional view of a GSM (10) according to the present invention comprising an optional support layer (1), a discriminating layer (ii) (2) and an additional layer (iii) (3).

[0024] Figure 1(b) is the same as Figure 1(a), except that the GSM (10) further includes a protective layer (iv) (4).

[0025] In both Figures 1(a) and 1(b), the discriminating layer (ii) is characterized by high gas selectivity, thereby providing the primary function of the GSM. The protective layer (iv) in Figure 1(b) is intended to reduce mechanical damage to the discriminating layer (ii) and the additional layer (iii) during, for example, handling and use of the GSM. The protective layer (iv) typically has high gas permeability and durability, thereby protecting the DL from mechanical damage.

[0026] The optional support layer can be porous or non-porous.

[0027] A non-porous support layer (sometimes called a "release layer") can be used to provide a foundation for building a membrane. The non-porous support layer can also be used to provide mechanical strength to the GSM during storage and transportation, and is typically peeled off before using the GSM (otherwise the support layer would be non-porous, which would prevent gas from flowing through the GSM).

[0028] The non-porous support layer optionally comprises a non-porous sheet and a (porous) grooved layer. In one embodiment, removing the non-porous sheet from the GSM also removes the grooved layer. In another embodiment, removing the non-porous sheet from the GSM does not remove the grooved layer, but rather the grooved layer remains in contact with the discriminating layer even after the non-porous sheet has been removed from the GSM.

[0029] Examples of non-porous sheets that can be used as or for the support layer include polyethylene terephthalate sheets having a release coating (e.g., a silicone coating) on ​​one or both sides. Such sheets are commercially available from various suppliers, including Mitsui Chemicals Tohcello, Ltd., as PET-O1-BM (ultra-low peel strength), PET-O1-BU (ultra-low peel strength), PET-O2-BU (medium peel strength), PET-O3-BU (medium-high peel strength), PET-O3-B3 (high peel strength), and PET-D13-BU (having two sides, one with medium-high peel strength and the other with low peel strength).

[0030] The porous support layer also provides mechanical strength to the GSM and, due to its porosity, does not need to be removed before using the GSM. The porous support layer typically remains a permanent component of the GSM and provides mechanical strength even when the GSM is used to separate or purify gases, thereby reducing the likelihood of damage to the GSM when used under high pressure and / or high temperature. Penetration of other layers of the GSM (e.g., the groove layer or the discriminating layer) into the porous support layer can provide a very strong bond between the support layer and the rest of the GSM.

[0031] Optionally, the support layer comprises a non-porous layer and a porous layer, preferably the porous layer is in contact with the discriminating layer (ii).

[0032] Preferred porous support layers include, for example, woven or nonwoven fabrics and combinations thereof.

[0033] The support layer can be made of, for example, any suitable polymer or natural fiber. Examples of such polymers include polysulfone, polyethersulfone, polyimide, polyetherimide, polyamide, polyamideimide, polyacrylonitrile, polycarbonate, polyester, polyacrylate, cellulose acetate, polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, poly(4-methyl-1-pentene), in particular polyacrylonitrile or polyethylene terephthalate (PET).

[0034] Many materials suitable for making the support layer are commercially available. Alternatively, the support layer can be prepared using techniques known in the art for preparing such materials. In one embodiment, the porous support layer can be prepared by curing the curable component in a manner similar to that used to prepare the membrane, for example, while ensuring that the pores of the porous support layer are too large to discriminate between different gases.

[0035] Preferably, layer (iii) is in contact with layer (ii). Typically, layer (ii) is sandwiched between layer (i) and layer (iii) and is in direct contact with layer (i) and layer (iii).

[0036] When layer (iv) is present, layer (iii) is typically sandwiched between layer (ii) and layer (iv) and is in direct contact with layer (ii) and layer (iv).

[0037] Optionally, for example, for the purpose of improving the wettability and / or adhesion of the support layer, the support layer has been subjected to corona discharge treatment, glow discharge treatment, flame treatment, ultraviolet irradiation treatment, or the like.

[0038] As the porous support layer, for example, an ultrafiltration membrane can be used, such as a polysulfone ultrafiltration membrane, a cellulose ultrafiltration membrane, a polytetrafluoroethylene ultrafiltration membrane, a polyvinylidene fluoride ultrafiltration membrane, and in particular a polyacrylonitrile ultrafiltration membrane. Asymmetric ultrafiltration membranes can also be used, including ultrafiltration membranes comprising a porous polymer membrane (preferably with a thickness of 10 to 150 μm, more preferably 20 to 100 μm) and an optional woven or non-woven fabric support.

[0039] The support layer is preferably as thin as possible as long as it provides the necessary structural strength to the GSM.

[0040] Preferably, the support layer comprises pores having an average pore size of 0.001 to 10 μm, preferably 0.01 to 1 μm (i.e., before the support layer has been converted into a gas separation membrane). Preferably, the support layer comprises pores having an average pore size at the surface of 0.001 to 0.1 μm, preferably 0.005 to 0.05 μm. The average pore size can be determined, for example, by observing the surface of the support layer by scanning electron microscopy ("SEM"), or by cutting through the support layer and measuring the diameter of the pores within the porous support layer, again by SEM, and then calculating the average value.

[0041] The porosity at the surface of the support layer can also be expressed as % porosity, i.e.

[0042]

[0043] The area required for the above calculations can be determined by examining the surface of the support layer by SEM before converting it into a gas separation membrane. Thus, in preferred embodiments, the % porosity of the support layer is >1%, more preferably >3%, especially >10%, and even more especially >20%.

[0044] Alternatively, the porosity of the support layer can be characterized by measuring the N2 gas flow rate through the support layer. The gas flow rate can be determined by any suitable technique, such as using a Pololux ® instrument available from Polometer.com. TM 1000 devices. Typically, the Polorlux TM The 1000 is set at the maximum pressure (about 34 bar) and the flow rate (L / min) of N2 gas through the tested support layer is measured. 2 The effective sample area of ​​18.5 mm (effective diameter) is preferably 1 L / min, more preferably 5 L / min, particularly 10 L / min, and even more particularly 25 L / min at a pressure of about 34 bar. The higher of these flow rates is preferred because it reduces the likelihood that the gas flux of the resulting GSM will be reduced by the support layer. The above pore size and porosity refer to the pore size and porosity of the support layer before conversion into the GSM of the present invention.

[0045] The porosity of layer (i) (as a whole) can be expressed as the CO2 gas permeability (in m 3 (STP) / m 2 .s.kPa). If the GSM is intended for gas separation, the CO2 gas permeability of layer (i) is preferably in the range of 5 to 150×10 -5 m 3 (STP) / m 2 .s.kPa, more preferably 5 to 100×10 -5 m 3 (STP) / m 2 .s.kPa, most preferably 7 to 70×10 -5 m 3 (STP) / m 2 .s.kPa.

[0046] Layer (i) (when present as a whole) has no gas separation selectivity compared to the discriminating layer (ii).

[0047] The average thickness of layer (i) (as a whole) is preferably from 20 to 500 μm, preferably from 50 to 400 μm, in particular from 100 to 300 μm.

[0048] Typically, the support layer (i) and the additional layer (iii) are on either side of the discriminating layer (ii).

[0049] Preferably, layer (i) further comprises a channel layer ("GL"), preferably a channel layer comprising a silicone or polysiloxane polymer. When layer (i) comprises a silicone or polysiloxane polymer channel layer, the channel layer is preferably located between the support layer and the discriminating layer (ii).

[0050] The discriminating layer (ii) and the additional layer (iii) may contain M from other sources, not just M derived from groups of formula (1). Thus, the "total atomic % of M" present in the discriminating layer (ii) and the additional layer (iii) (as distinct from the atomic % of M of groups of formula (1) as stated in claim 1) includes M from all sources, including but not limited to M from groups of formula (1). For example, the "total atomic % of M" present in the discriminating layer (ii) and the additional layer (iii) includes M from other sources, such as from one or more groups of formula (2):

[0051] M-(O-) z

[0052] Formula (2)

[0053] in:

[0054] M is a metal or metalloid atom;

[0055] O is an oxygen atom; and

[0056] The value of z is 1, 2, or 3.

[0057] Typically, DL(ii) and the additional layer (iii) each independently comprise a group of formula (1) and a group of formula (2). However, preferably, DL(ii) comprises a greater amount of groups of formula (1) than groups of formula (2). When DL(ii) or the additional layer (iii) contains groups of formula (2), preferably, M in the group of formula (1) is the same metal or metalloid atom as M in the group of formula (2) of that layer. M in the groups of formula (1) and formula (2) in DL(ii) may be the same as or different from M in the groups of formula (1) and formula (2) in the additional layer (iii).

[0058] Preferably, each M is independently silicon, titanium, zirconium or aluminum.

[0059] Preferably, DL comprises more than 10 atomic % and less than 50 atomic % of M of the group of formula (1), in particular 12 to 30 atomic % of M of the group of formula (1), more in particular 13 to 27 atomic % of M of the group of formula (1), wherein M is as defined above.

[0060] Preferably, the additional layer (iii) comprises 2 to 9 atomic % of M, more preferably 3 to 8 atomic % of M, of the group of formula (1), wherein M is as defined above.

[0061] When the additional layer (iii) contains more than 10 atomic % of M of the formula (1), the gas permeability of the GSM is significantly reduced or plummets, and the additional layer also becomes discriminating. Thus, the additional layer (iii) no longer has separation selectivity or discriminates between gases such as CO2 and CH4 compared to the discriminating layer (ii). When the additional layer (iii) contains less than 1.5 atomic % of M of the formula (1), the permeability of the GSM is significantly reduced.

[0062] Preferably, the additional layer (iii) comprises 9 to 30.5 atomic % of M groups of formula (2), more preferably 20 to 30 atomic % of M groups of formula (2), wherein M is as defined above.

[0063] Preferably, the total atomic % of M present in the additional layer (iii) (i.e. M from all sources, e.g. from groups of formula (1) + groups of formula (2)) is 13.5 to 35 atomic %, in particular 15 to 33 atomic %, more in particular 16 to 32 atomic %.

[0064] Preferably, the composition of the additional layer (iii) is substantially constant over its depth. For example, over at least 80% of the depth of the additional layer (iii), the atomic % of M of the group of formula (1) present in the additional layer (iii) varies by less than 25% (more preferably less than 10%, especially less than 5%) relative to the average atomic % of M in the additional layer (iii). For example, if the average atomic % of M in the additional layer (iii) is "X %", then over at least 80% of the depth of the additional layer (iii), the atomic % of M in the additional layer (iii) is preferably from 0.75X to 1.25X (more preferably from 0.9X to 1.1X, especially from 0.95X to 1.05X).

[0065] The atomic % of M (e.g., derived from groups of formula (1) and from any groups of formula (2), etc.) in the additional layer (iii) (and in the DL (ii)) can be determined using surface analysis equipment, such as by X-ray photoelectron spectroscopy (XPS) (e.g., using GC-IB / XPS gas cluster ion beam XPS). Such equipment can also be used to determine the atomic % of M at the top surface and at various depths in and below the surface in the additional layer (iii) and any other layers (e.g., DL or GL, when present). A suitable instrument for performing the analysis to determine the atomic % of M in each layer is the VersaProbe II XPS apparatus ("ULVAC-PHI") from Physical Electronics, Inc. The ULVAC-PHI is preferably provided with a monochromated Al K α (1486.6eV, 15W25KV An X-ray source with a raster size of 300 μm × 300 μm) is used. For charge compensation, low energy electrons and Ar ions can be flooded when measuring the atomic % of M in each layer. An Ar gas cluster beam (5 kV, 20 nA, 2 mm × 2 mm) can be used for depth profile analysis. Based on this analysis, the atomic % of M and any other elements (such as carbon and oxygen) present in the additional layer (iii) can be measured. At the data point where the atomic % of M is the highest, the atomic % of M in the additional layer (iii) can be determined. This will include M from all sources, such as the groups of formula (1) or formula (2) defined above, and the amount of M in each of these groups can be quantified separately. For example, when M is silicon, the Si-(O)4 group and the Si-(O-) z The atomic % of silicon in a group (where z is 1, 2, or 3) can be quantified by this method. In the spectrum of Si2p, the binding energy at 102.6 eV is defined as the group of formula (2), while the binding energy at 103.8 eV is defined as the group of formula (1), wherein formula (1) and formula (2) are as defined above. The area ratio of Si2p at 102.6 eV and 103.8 eV can be converted to an atomic ratio (atomic %) so that the sum of the areas of the separated peak components will correspond to the atomic % of Si.

[0066] In one embodiment, the additional layer (iii) comprises a substantially constant value of 1.5 to 10 atomic % of M of the group of formula (1) throughout the depth of the additional layer (iii). For example, the atomic % of M of the group of formula (1) present in the additional layer (iii) varies by less than 25% relative to the average atomic % of M throughout the depth of the additional layer (iii). By constructing a substantially constant atomic % of Si of Si-(O-)4 in the composition of the additional layer (iii) (1.5 to 10% higher than the DL), it can be believed that the additional layer (iii) has little separation selectivity or does not discriminate between gases such as CO2 and CH4 or between gases such as CO2 and O2, O2 and N2 or H2 and CH4. Having no gas selectivity in this application means that a person skilled in the art would not propose that the additional layer (iii) be used as a source or embodiment for meaningful gas separations between CO2 and CH4 or between gases such as CO2 and O2, O2 and N2 or H2 and CH4.

[0067] In another embodiment, the discriminating layer (ii) comprises a substantially constant value of greater than 10 atomic % of groups M of formula (1) throughout the depth of the discriminating layer (ii). For example, the atomic % of groups M of formula (1) present in the discriminating layer (ii) varies by less than 25% relative to the average atomic % of M throughout the depth of the discriminating layer (ii).

[0068] The atomic % of M of the group of formula (1) (wherein M is as defined above) is the atomic % of M present in the relevant layer as a group of formula (1). Similarly, the atomic % of M of the group of formula (2) (wherein M is as defined above) is the atomic % of M present in the relevant layer as a group of formula (2).

[0069] In one embodiment, the additional layer (iii) can be obtained or obtained by a process comprising plasma treatment. Suitable plasma treatment processes include plasma deposition, in particular plasma deposition of a compound comprising M, thereby forming an additional layer (iii) comprising a group of formula (1) and optionally a group of formula (2) (each as defined above). Preferred plasma treatment processes for depositing M in the form of a group of formula (1) on layer (ii) and optionally depositing a group of formula (2) (each as defined above) on layer (ii) are carried out using precursors at atmospheric pressure in the absence of oxygen and / or air.

[0070] In another embodiment, the discriminating layer (ii) can be obtained or obtained by a process comprising plasma deposition of M in the form of a group of formula (1) onto layer (i) and optionally plasma deposition of a group of formula (2) (each as defined above) onto layer (i). Suitable plasma treatment processes include plasma deposition, in particular plasma deposition of a compound comprising M, thereby forming a discriminating layer (ii) comprising a group of formula (1) and optionally a group of formula (2) (each as defined above).

[0071] In one embodiment, the additional layer (iii) is applied to the discriminating layer (ii) by a plasma treatment process using precursor compounds providing groups of formula (1) (as defined above). As carrier gas a noble gas such as argon or helium may be used.

[0072] The plasma treatment process for applying layer (iii) to layer (ii) is preferably carried out at a temperature between 0.30 and 9.00 J / cm 2 (and using low pressure or even in (remote) atmospheric pressure plasma treatment).

[0073] The plasma treatment process for applying layer (iii) to layer (ii) preferably uses a plasma treatment of 5 to 500 cm 3 (STP) / min, more preferably 50 to 200 cm 3 (STP) / min, particularly preferably 80 to 120 cm 3 The low-pressure plasma treatment is preferably carried out at a gas pressure of 0.6 to 100 Pa, more preferably 1 to 60 Pa, particularly preferably 2 to 40 Pa.

[0074] When silicon-containing precursor compounds are used during the plasma treatment, this results in the additional layer (iii) being deposited on layer (ii) as a silicon dioxide-like top surface comprising groups of formula (1) and optionally groups of formula (2), all as defined above.

[0075] The average thickness of the additional layer (iii) is generally from 1 to 1,500 nm, more preferably from 5 to 1,000 nm, even more preferably from 10 to 500 nm.

[0076] According to a second aspect of the present invention, there is provided a method for forming the gas separation membrane of the first aspect of the present invention, comprising the steps of:

[0077] (a) applying a discriminating layer (ii) to the support layer (i) by a plasma treatment process; and

[0078] (b) applying an additional layer (iii) to the discriminating layer (ii) (DL) by a plasma treatment process; and

[0079] Optionally (c) applying a protective layer (iv) to the additional layer (iii).

[0080] When the support layer (i) is a non-porous sheet or comprises a non-porous sheet, the method of the second aspect of the present invention optionally further comprises the step of removing the non-porous sheet from the gas separation membrane.

[0081] In a preferred embodiment, the discriminating layer (ii) is applied to the support layer (i) by a plasma treatment process (e.g., using a plasma treatment apparatus). Preferred plasma treatment processes for applying the discriminating layer (ii) to the support layer (i) include using an atmospheric pressure glow discharge plasma, such as described in US Pat. No. 10,427,111, page 40, line 4 to page 41, line 36, which is incorporated herein by reference. For example, the support layer (i) may be exposed to an atmospheric pressure glow discharge plasma to form the discriminating layer (ii) thereon.

[0082] The plasma treatment process that can be used for step (a) and step (b) is preferably carried out using a plasma treatment device comprising a treatment space and a first electrode and a second electrode in the treatment space so as to generate an atmospheric pressure glow discharge plasma between the first electrode and the second electrode. The electrodes can be provided with a dielectric barrier in various arrangements. In one arrangement, the dielectric barrier of at least one electrode is formed by a polymer film or an inorganic dielectric. Polymers such as polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE) or polyethylene (PE) or ceramics such as silicon dioxide or aluminum oxide, or combinations of these, can be used, and microporous dielectric materials attached to the electrodes can also be used.

[0083] In a preferred embodiment, the additional layer (iii) is applied to the discriminating layer (ii) using atmospheric pressure glow discharge plasma (as a plasma treatment process).

[0084] As mentioned above, preferably, the atomic % of M of the group of formula (1) in the additional layer (iii) is substantially constant over the entire depth of the additional layer (iii). In order to achieve a substantially constant atomic % of M of the group of formula (1) in the additional layer (iii), the manufacturing process of the additional layer (iii) is preferably different from the process for manufacturing the DL using precursors in the presence of rare and inert gases and in the absence of oxygen.

[0085] In step (b), the plasma treatment process preferably comprises applying a plasma at a temperature of 0.03 to 30 W / cm2 in the treatment space containing the layer (i). 2 An atmospheric pressure glow discharge plasma is generated at an effective power density of preferably less than 120 seconds. Preferably, the processing space is free of oxygen (eg, the processing space comprises an oxygen-free inert gas).

[0086] In step (a), the plasma treatment process preferably comprises a plasma treatment process at a temperature of 0.1 to 30 W / cm 2 The atmospheric pressure glow discharge plasma is generated at an effective power density of preferably less than 60 seconds. Preferably, in this case, in step (a), the processing space comprises an oxygen-rich atmosphere.

[0087] Therefore, it is preferred that both steps (a) and (b) comprise a plasma treatment process, wherein step (b) is performed in an atmosphere free of oxygen and step (a) is performed in an atmosphere containing oxygen.

[0088] The plasma treatment process can generally be carried out using a precursor compound, particularly an organosilicon compound. The preferred plasma treatment process in step (b) uses a precursor compound. The precursor compound can be contained in the treatment space and preferably at a rate of 0.1 to 10 J / cm 2 of energy (in step (b)).

[0089] In a preferred embodiment, the treatment space used in step (b) comprises an air-free or oxygen-free atmosphere and a 0.1 to 10 J / cm 2 power density.

[0090] In a preferred embodiment, the plasma treatment process used in steps (a) and / or (b) comprises stabilizing an atmospheric pressure glow discharge plasma according to any of the methods described in, for example, US6774569 or EP1383359.

[0091] In a preferred embodiment, the plasma treatment process used in step (b) comprises exposing the discriminating layer (ii) to an atmospheric pressure glow discharge plasma, wherein the plasma is stabilized by an inductive and capacitive (LC) matching network as described in, for example, EP1917842.

[0092] In another embodiment, the additional layer (iii) may be applied to layer (ii) (DL) using a plasma treatment in a low pressure plasma environment as described in US10427111.

[0093] In another embodiment, the plasma treatment apparatus for performing the plasma treatment step may include a transport device for transporting layer (i) (support layer) or the combination of layers (i) + (ii) through the electrode. In addition, the transport device may include a tensioning mechanism for maintaining layer (i) or layers (i) + (ii) in close contact with the electrode.

[0094] In one embodiment, the additional layer (iii) can be obtained from one or more precursor compounds that can be contained in the processing space.

[0095] Precursor compounds that can be used to provide the group of formula (1) (as defined above) and optionally the group of formula (2) (as defined above) include TEOS (tetraethyl orthosilicate), HMDSO (hexamethyldisiloxane), TMOS (tetramethyl orthosilicate), TMCTS (1,3,5,7-tetramethylcyclotetrasiloxane), D4 OMCTS (octamethylcyclotetrasiloxane), D5 (decamethylcyclopentasiloxane), D6 (dodecamethylcyclohexasiloxane), silane (SiH4), bis(triethoxysilyl)ethane (BTESE), TPOT (tetrapropyl orthotitanate), TEOT (titanium ethoxide), TTIP (titanium tetraisopropoxide) or ZTB (zirconium tetra-tert-butoxide).

[0096] The substantially uniform additional layer (iii) can be prepared by using an atmospheric pressure glow discharge apparatus as described in EP 1917842, with an inductive and capacitive (LC) matching network. In this embodiment, the additional layer (iii) has an average thickness of 1 to 1000 nm, even more preferably 10 to 500 nm.

[0097] Therefore, in a preferred embodiment of the method of the second aspect of the invention, step (a) comprises applying the discriminating layer (ii) to the support layer (i) by a plasma treatment process, and step (b) comprises applying the additional layer (iii) to the discriminating layer (ii) by a plasma treatment process.

[0098] The function of the discriminating layer (ii) is to discriminate between gases, separating the feed gas mixture into a permeate gas that passes through the GSM and a retentate that cannot pass through the GSM. In order to discriminate between gases, the DL contains more than 10 atomic % of M of the formula (1), wherein M is as defined above.

[0099] The permeate gas and retentate typically contain the same gases as the feed gas mixture, but one is enriched in at least one gas present in the feed gas, while the other is depleted of the same gas.

[0100] The average thickness of the discriminating layer (ii) is preferably from 1 nm to 2 μm, more preferably from 3 nm to 1 μm, in particular from 5 to 200 nm.

[0101] The support layer (i) preferably comprises a porous support (e.g., made of any of the porous support materials described above) and a grooved layer ("GL"). The GL is preferably attached to (e.g., coated on) the porous support. When the support layer (i) comprises a non-porous support (e.g., for providing mechanical strength during storage or transportation), the non-porous support is typically removed (e.g., peeled off) before use of the GSM.

[0102] The GSM optionally comprises a protective layer (iv) made of a material similar to that used to make the GL.

[0103] When the GSM does not contain a PL and / or support layer (i), it can still be used for gas separation, or it can be sold as a commercial product so that consumers can apply their own customized PL according to their needs. The optional GL and PL are permeable to gases and generally have a low ability to distinguish between gases. When present, the GL and PL preferably comprise a polymer resin, particularly a polysiloxane. Preferred polysiloxanes present in or as the GL and / or PL are poly(dimethyl)siloxanes, for example polymers comprising repeating -Si-(CH3)2-O- units.

[0104] The average thickness of the GL (when present) is preferably from 50 to 2,400 nm, more preferably from 150 to 800 nm, especially from 200 to 650 nm.

[0105] The average thickness of the PL (when present) is preferably from 10 to 10,000 nm, more preferably from 50 to 5,000 nm, especially from 100 to 3,000 nm.

[0106] Preferably, the GL and PL each independently contain groups capable of bonding to the metal, for example, by covalent bonds, ionic bonds, and / or by hydrogen bonds, preferably by covalent bonds. The properties of these groups depend to some extent on the chemical composition of the GL / PL and the properties of the metal, but typically these groups are selected from epoxy groups, oxetane groups, carboxylic acid groups, amino groups, hydroxyl groups, vinyl groups, hydrogen groups, and thiol groups. More preferably, the GL and PL each independently contain a polymer having carboxylic acid groups, epoxy groups, or oxetane groups, vinyl groups, hydrogen groups, or a combination of two or more of these groups. These polymers can be formed on a support by a method comprising curing a radiation-curable or heat-curable composition, particularly a curable (e.g., radiation-curable) composition containing a polymerizable dialkylsiloxane. The latter option can be used to provide preferred GL and PL containing dialkylsiloxane groups.

[0107] The polymerizable dialkylsiloxane that may be present in the optional GL and PL is preferably a monomer containing dialkylsiloxane groups, or a polymerizable oligomer or polymer containing dialkylsiloxane groups. For example, as described in more detail below, the GL and / or PL can be prepared from a radiation-curable composition comprising a partially crosslinked radiation-curable polymer containing dialkylsiloxane groups. Typical dialkylsiloxane groups have the formula -{O-Si(CH3)2}n-, where n is at least 1, e.g., 1 to 100. Poly(dialkylsiloxane) compounds having terminal vinyl groups are also available, and these compounds can be incorporated into the GL during the curing process.

[0108] In one embodiment, GL does not contain a group of formula Si-C6H5.

[0109] In one embodiment, PL does not contain a group of formula Si—C 6 H 5 .

[0110] Irradiation of the radiation-curable composition to form the optional GL or PL (sometimes referred to as "curing" in this specification) can be performed using any source that provides the necessary radiation wavelength and intensity to polymerize the radiation-curable composition and thereby form a GL on the support layer or a PL on the additional layer (iii). For example, electron beams, ultraviolet radiation (UV), visible light, and / or infrared radiation can be used to irradiate (cure) the radiation-curable composition, and the appropriate radiation is selected to match the components of the composition.

[0111] The optional GL and the optional PL are preferably each independently obtained by curing a curable composition comprising:

[0112] (1) 0.5 to 25 wt. % of radiation-curable components, at least one of which contains dialkylsiloxane groups;

[0113] (2) 0 to 5 weight percent photoinitiator; and

[0114] (3) 70 to 99.5% by weight of an inert solvent.

[0115] Preferably, the curable composition used to prepare the GL / PL has a titanium:silicon molar ratio of at least 0.0005, more preferably from 0.001 to 0.1, especially from 0.003 to 0.03.

[0116] The radiation curable component of component (1) generally comprises at least one radiation curable group. Radiation curable groups include ethylenically unsaturated groups (eg (meth) acrylic groups (eg CH2=CR 1 C(O)-groups), especially (meth)acrylate groups (e.g. CH2=CR 1C(O)O-groups), (meth)acrylamide groups (e.g. CH2=CR 1 C(O)NR 1 - group), wherein each R 1 independently H or CH3), particularly oxetane or epoxy groups (eg glycidyl and epoxycyclohexyl).

[0117] In addition to providing a smooth surface for the discriminating layer, the GL also provides some additional mechanical strength to the GSM, even in cases where the GSM has been prepared by peeling off the non-porous sheet after storage and transport. The amount of radiation-curable component (i.e. component (1)) present in the curable composition for preparing the optional GL and / or optional PL is preferably 1 to 20 wt%, more preferably 2 to 15 wt%. In a preferred embodiment, component (1) of the curable composition for preparing the GL and / or PL comprises a partially crosslinked radiation-curable polymer comprising dialkylsiloxane groups.

[0118] The function of the inert solvent (3) is to provide the composition with a viscosity suitable for the particular method of applying the curable composition to the support. For high-speed application methods, low-viscosity inert solvents are generally selected. Examples of suitable inert solvents are mentioned above in connection with the preparation of the polymer sheet.

[0119] The amount of inert solvent (3) (i.e. component (3)) present in the curable composition for preparing the optional GL and / or PL is preferably 70 to 99.5% by weight, more preferably 80 to 99% by weight, especially 90 to 98% by weight.

[0120] Inert solvents are not radiation curable.

[0121] The composition may contain other components such as surfactants, surface tension modifiers, viscosity building agents, biocides and / or other components capable of copolymerizing with other ingredients.

[0122] The gas separation membranes of the present invention can be packaged and supplied commercially to companies that assemble gas separation modules, for example for their own use or for onward sale.

[0123] According to a third aspect of the present invention, there is provided a gas separation module comprising one or more gas separation membranes according to the first aspect of the present invention.

[0124] The gas separation module of the present invention preferably further comprises a feed carrier and a permeate carrier, optionally wound onto the perforated tube.

[0125] Preferred gas separation modules include spiral modules, hollow fiber modules, pleated modules, tubular modules, and plate-and-frame modules.

[0126] According to a fourth aspect of the present invention, there is provided use of the gas separation membrane of the first aspect of the present invention or the gas separation module of the third aspect of the present invention for separating gases and / or for purifying feed gases.

[0127] The gas separation membranes and modules of the present invention are particularly suitable for separating a feed gas containing a target gas into a target gas-rich gas stream and a target gas-depleted gas stream. For example, a feed gas containing polar and non-polar gases can be separated into a polar gas-rich gas stream and a polar gas-depleted gas stream. In many cases, the membrane is more sensitive to polar gases (e.g., CO2, H2S, NH3, SO2) than to non-polar gases (e.g., alkanes, H2, and N2). x and nitrogen oxides, especially NO x ) has a high permeability. Therefore, the polar gas is preferably CO2, H2S, NH3, SO x , nitrogen oxides or a combination of two or more thereof. The non-polar gas is preferably N2, H2, an alkane or a combination of two or more thereof.

[0128] Preferably, the polar and non-polar gases are gaseous when at 25°C.

[0129] The target gas may be, for example, a gas that is valuable to the user of the module or element and that the user wishes to collect. Alternatively, the target gas may be an undesirable gas, such as a pollutant or "greenhouse gas," that the user wishes to separate from the gas stream to meet product specifications or to protect the environment.

[0130] The modules and GSMs of the present invention are particularly suitable for purifying natural gas (a mixture mainly containing methane) by removing polar gases (CO2, H2S); for purifying synthesis gas; and for removing CO2 from hydrogen and flue gases. Flue gases typically come from fireplaces, ovens, furnaces, boilers, internal combustion engines and power plants. The composition of flue gases depends on what is being burned, but generally they contain mainly nitrogen from the air (usually more than two-thirds) and carbon dioxide (CO2) from combustion. Flue gases also contain a low percentage of pollutants such as particulate matter, carbon monoxide, nitrogen oxides and sulfur oxides. Recently, the separation and capture of CO2 has received attention in response to environmental problems (global warming).

[0131] The module and GSM of the present invention are particularly suitable for the following separations: separating a feed gas containing CO2 and N2 into a gas stream richer in CO2 than the feed gas and a gas stream less in CO2 than the feed gas; separating a feed gas containing CO2 and CH4 into a gas stream richer in CO2 than the feed gas and a gas stream less in CO2 than the feed gas; separating a feed gas containing CO2 and H2 into a gas stream richer in CO2 than the feed gas and a gas stream less in CO2 than the feed gas; separating a feed gas containing H2S and CH4 into a gas stream richer in H2S than the feed gas and a gas stream less in H2S than the feed gas; and separating a feed gas containing H2S and H2 into a gas stream richer in H2S than the feed gas and a gas stream less in H2S than the feed gas.

[0132] The modules and GSMs of the present invention are particularly suitable for separating a "dirty" feed gas comprising polar gases, non-polar gases and hydrocarbons containing at least two (e.g., 2 to 7) carbon atoms into a permeate gas and a retentate gas, one of the two gases being rich in polar gases and the other being poor in polar gases.

[0133] The invention will now be illustrated by the following non-limiting examples in which all parts and percentages are by weight unless otherwise indicated. Example

[0134] In these examples, the performance of the gas separation membrane was measured using a multilayer structure having the overall structure shown in Table 1, wherein the multilayer structure includes the gas separation membrane under test (which has a support layer (i) (when present) or a layer (ii) of 05TH100S facing downward), a 05TH100S sheet, and a 42369 sheet.

[0135] The 05TH100S sheet and the 42369 sheet are described in more detail below.

[0136] Table 1 – Multilayer structure including GSM

[0137] Tested gas separation membrane 05TH100S sheet 42369 sheet

[0138] In the examples, the feed gas used had the composition shown in Table 2 below.

[0139] Table 2

[0140]

[0141] The performance properties of the gas separation membranes of the present invention and comparative GSMs were measured using the multilayer structures shown in Table 1 by the following techniques:

[0142] (A) Permeability

[0143] The feed gas having the composition described in Table 2 above was passed through the multilayer structure shown in Table 1 under test at 40°C and a gas feed pressure of 6000 kPa. The CO2, n-C4H 10 and the flux of CH4 through the multilayer structure shown in Table 1.

[0144] After continuous use of the multilayer structure shown in Table 1 (including the tested GSM) for 5 minutes, the CO2, n-C4H 10 and CH4 permeability (Q i ):

[0145] Q i =(θ Perm ·X Perm,i ) / (A·(P Feed ·X Feed,i -P Perm ·X Perm,i ))

[0146] in:

[0147] Q i = the permeability of the relevant gas (i.e., i is CO2 or n-C4H 10 or CH4)(m 3 (STP) / m 2 kPa·s);

[0148] θ< Perm = permeation flow rate (m 3 (STP) / s);

[0149] X Perm,i = volume fraction of the relevant gas in the permeating gas;

[0150] A = membrane area (m 2 );

[0151] P Feed = feed gas pressure (kPa);

[0152] X Feed,i = volume fraction of the relevant gas in the feed gas;

[0153] P Perm = permeate gas pressure (kPa); and

[0154] STP is standard temperature and pressure, which is defined herein as 25.0°C and 1 atmosphere (101.325 kPa).

[0155] (Q i ) can be achieved through 1 GPU = 1×10 -6 cm3 (STP) / (s·cm 2 cmHg) to determine.

[0156] The permeability of CO 2 higher than 150 GPU was evaluated as good, and the permeability of CO 2 less than or equal to 150 GPU was evaluated as a comparative result, which was poor compared with the examples of the present invention.

[0157] (B) Selectivity

[0158] The selectivity (CO2 / C4H 10 and CO2 / CH4; αCO2 / C4H 10 and αCO2 / CH4) are calculated from the QCO2 and Qn-C4H 10 calculate:

[0159] αCO2 / n-C4H 10 =QCO2 / Qn-C4H 10 ;

[0160] αCO2 / CH4=QCO2 / QCH4

[0161] Among them, QCO2, QCH4 and Qn-C4H 10 Determine by the method described in step (A) above.

[0162] αCO2 / n-C4H above 100 10 Values ​​are considered acceptable, while αCO2 / n-C4H below 100 10 The value is considered unacceptable.

[0163] An αCO2 / CH4 value of 26 or more was considered good, while an αCO2 / CH4 value of less than 15 was considered unacceptable. An αCO2 / CH4 value of 26 to 15 was evaluated as acceptable.

[0164] (C) Groove layer thickness

[0165] The thickness of the channel layer is determined by cutting through the support layer (i) and measuring the thickness of the channel layer from the sheet outward using a SEM.

[0166] (D) Atom % of M in the group of formula (1)

[0167] The atomic % of M in the group of formula (1) in DL and FL was determined using the conventional method described above using a GC-IB / XPS gas cluster ion beam XPS apparatus ("ULVAC-PHI") from Physical Electronics, Inc. using X-ray photoelectron spectroscopy. The ULVAC-PHI was equipped with a monochromator Al K α (1486.6eV, 15W 25KV An X-ray source (raster size 300 μm × 300 μm) was used. Low-energy electrons and Ar ions were flooded for charge compensation when measuring the atomic % of M in each layer. An Ar gas cluster beam (5 kV, 20 nA, 2 mm × 2 mm) was used for depth profiling.

[0168] Preparation of gas separation membranes

[0169] The following materials were used to prepare the GSM and multilayer structures:

[0170] PAN is a porous sheet with an average thickness of 170-180 μm, comprising a PET nonwoven support (thickness 140-150 μm) with a porous polyacrylonitrile layer. PAN was obtained from Microdyn-Nadir GmbH, Germany, under the trade name UA100T.

[0171] PET-O1-T is a non-porous polyethylene terephthalate sheet (manufactured by Mitsui Chemicals Tohcello., Ltd.) having a silicone resin-based thin film release agent on one side.

[0172] X-22-162C is a dual-ended reactive silicone with carboxylic acid reactive groups and a viscosity of 220 mm 2 / s and the equivalent weight of the reactive group was 2,300 g / mol, which was obtained from Shin-Etsu Chemical Co., Ltd. (MWT 4,600) (1 is an integer).

[0173]

[0174] DBU is 1,8-diazabicyclo[5.4.0]undec-7-ene from Sigma Aldrich.

[0175] UV-9300 is SilForce from Momentive Performance Materials Holdings TM UV-9300, which has an epoxy equivalent weight of 950 g / mol ethylene oxide (MWT 9000, determined by viscosity) (m and n are integers).

[0176]

[0177] I0591 is 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate (C 40 H 18 BF 20 I).

[0178]

[0179] Ti(OiPr)4 is titanium(IV) isopropoxide (MWT 284) from Dorf Ketal Chemicals.

[0180] n-Heptane was n-heptane from Brenntag Nederland BV.

[0181] MEK is 2-butanone from Brenntag Nederland BV.

[0182] HMDSO is hexamethyldisiloxane supplied by Merck and used as precursor for the additional layer (iii).

[0183] 05TH100S sheet is a sheet from Hirose paper manufacturing (wet-laid polyester nonwoven / average thickness 100 μm / average weight 100 g / m 2 / Average density 0.93g / cm 3 ).

[0184] 42369 sheet is a porous sheet from Guilford (woven fabric made of polyethylene terephthalate and epoxy resin / average thickness 0.3 mm / 60 wpi (number of wales per 2.54 cm) / 59 cpi (number of courses per 2.54 cm)).

[0185] Preparation of gas separation membranes

[0186] Stage a) Preparation of partially cured polymer ("PCP polymer")

[0187] The components UV-9300, X-22-162C, and DBU were dissolved in n-heptane in the amounts shown in Table 3 and maintained at 91° C. for 168 hours. The Si content (meq / g polymer) of the resulting polymer (PCP polymer) was 12.2, and the viscosity of the resulting PCP polymer solution at 25.0° C. was 125 mPas.

[0188] Table 3 – Ingredients used to prepare PCP polymers

[0189] Element Amount (weight %) UV-9300 (weight %) 46.395 X-22-162C (weight %) 13.596 DBU (wt%) 0.009 n-Heptane (weight %) 40.000

[0190] Stage b) Preparation of curable composition C

[0191] The PCP polymer solution from step a) was cooled to 20°C and diluted with n-heptane to obtain the PCP polymer concentration shown in Table 4 below. The solution was then filtered through filter paper with a pore size of 2.7 μm. A photoinitiator (I0591) and a metal complex (Ti(OiPr)4) were then added in the amounts (wt %) shown in Table 4 to obtain a curable composition C. The amount of Ti(OiPr)4 present in curable composition C corresponded to 55.4 μmol of Ti(OiPr)4 / gram of PCP polymer. Furthermore, the metal to silicon molar ratio in curable composition C was 0.0065.

[0192] Table 4 - Ingredients of Curable Composition C

[0193] Element Amount (weight %) PCP polymers 10.000 I0591 0.105 <![CDATA[Ti(OiPr)4]]> 0.226 DBU 0.001 MEK 2.008 n-heptane 87.660

[0194] Curable Composition C was used to prepare the groove layers ("GL") in Examples 1 to 4 and Comparative Examples CEx. 1 to CEx. 4. Additionally, Curable Composition C was used to prepare the protective layers in Example 4 and Comparative Example CEx. 4 (as described in more detail below).

[0195] Step i. Preparation of support layers SL1 and SL2

[0196] The curable composition C (prepared as described in stage b) above) was applied to PAN (porous sheet) by meniscus dip coating at a speed of 10 m / min and then irradiated using a Light Hammer LH10 from Fusion UV Systems equipped with a D bulb at an intensity of 16.8 kW / m (70%) to obtain a support layer SL1 comprising PAN and a groove layer with a dry thickness of 600 nm.

[0197] SL2

[0198] The support layer SL2 was prepared in the same manner as SL1, except that PET-O1-T (non-porous sheet) SL2 was used instead of PAN. SL2 included a groove layer with a dry thickness of 600 nm.

[0199] Step ii. Applying the discrimination layer (ii) to the support layers SL1 and SL2 to obtain SL1-DL1 and SL2-DL1

[0200] The discriminating layer is applied to each of the support layers SL1 and SL2 as follows:

[0201] The support layers (SL1 and SL2) were placed in an atmospheric plasma apparatus as described in Figure 5 of EP1917842. The discriminating layers were produced on the support layers (SL1 and SL2) using the following conditions: the oxygen flow rate was set to 0.5 dm 3 (STP) / min and the argon flow rate was set to 20 dm 3 (STP) / min. Plasma treatment at 1.75J / cm 2 The plasma treatment was carried out for 2 seconds with an input power of 100 nm. The plasma treatment provided a composite of the porous support SL1 and the discriminating layer DL1 (SL1-DL1) and a composite of the porous support SL2 and the discriminating layer DL1 (SL2-DL1). In each case, the discriminating layer DL1 had a thickness of 60 nm.

[0202] The atomic % of M of the group of formula (1) in the discriminating layer DL1 of SL1-DL1 and SL2-DL1 was determined by X-ray photoelectron spectroscopy using the method described in the above section (D), and it was found that in each case, the atomic % of M of the group of formula (1) was greater than 10 atomic %.

[0203] Example 1 - Application of an additional layer (iii) to obtain a gas separation membrane GSM1 according to the invention

[0204] A sample of SL1-DL1 (composed of the support layer (i) obtained in step (ii) above and the discriminating layer) was exposed to an atmospheric pressure glow discharge (APG) plasma using the precursor HMDSO. The apparatus used for exposure was as described in EP1917842. The precursor mass flow rate supplied by a controlled evaporation unit was 1.0 g / hr HMDSO. The precursor vapor was diluted in an (oxygen-free) argon process carrier gas. The flow rate of the process gas was 20 dm 3 (STP) / min. In all cases, the applied plasma energy density was 0.15 W / cm 2 , and the treatment time was 13 seconds. This obtained the gas separation membrane GSM1 of the present invention.

[0205] The thickness of the additional layer (iii) in GSM1 (ie SL1-DL1-FL1) was determined by cutting through the GSM1 and measuring the thickness of the additional layer (iii) using a scanning electron microscope. The thickness of the additional layer FL1 was found to be 100 nm.

[0206] The atomic % of M of the group of formula (1) in the additional layer FL1 in GSM1 was determined by X-ray photoelectron spectroscopy at depths of 10 nm and 20 nm using the method described in section (D) above and was found to be 2 atomic %.

[0207] Example 2 - Application of an additional layer (iii) to obtain a gas separation membrane GSM2 according to the invention

[0208] GSM2 was prepared in exactly the same manner as GSM1 described above, except that non-porous SL2-DL1 was used instead of SL1-DL1.

[0209] The thickness of the additional layer of GSM2 and the atomic % of M of the group of formula (1) in the additional layer of GSM2 were the same as those in GSM1 (100 nm thickness and 2 atomic %).

[0210] Example 3 - Removal of non-porous sheet from GSM2 to obtain gas separation membrane GSM3

[0211] The nonporous PET-O1-T sheet was peeled off from GSM2 to obtain GSM3. The thickness of the additional layer of GSM3 and the atomic % of M of the group of formula (1) in the additional layer of GSM3 were the same as those in GSM1 (100 nm thickness and 2 atomic %).

[0212] Example 4 - Preparation of Gas Separation Membrane GSM4 with Protective Layer

[0213] GSM4 was prepared by dip-coating GSM1 into curable composition C at a speed of 10 m / min. The coating was then cured by irradiation with a Light Hammer LH10 from Fusion UV Systems equipped with a D bulb at an intensity of 24 kW / m. The average thickness of the resulting protective layer in GSM4 was 2,400 nm, as measured by SEM.

[0214] Comparative Examples CEx.1 to CEx.4–CGSM1 to CGSM4

[0215] Comparative gas separation membranes CGSM1 to CGSM4 were prepared in the same manner as GSM1 to GSM4 of the present invention, except that the polymer layer was applied to the discriminating layer by meniscus dip coating of a curable polymer C at a speed of 10 m / min, instead of forming layer (iii) by plasma treatment. The coated discriminating layer was then cured by irradiation with a Light Hammer LH10 from Fusion UV Systems equipped with a D bulb at an intensity of 24 kW / m, to obtain comparative gas separation membranes CGSM1 to CGSM4, each of which had a polymer layer having an average thickness of 100 nm (measured by SEM) instead of layer (iii) of the present invention. In CGSM1, CGSM2, CGSM3, and CGSM4, the polymer layer used instead of layer (iii) had less than 1 atomic % of M of the group of formula (1), wherein M is as defined above.

[0216] The permeability and selectivity of the GSM described above and the comparative GSM were measured by the techniques described above, and the results are shown in Table 5 below:

[0217] Table 5 – Summary of GSMs, comparative GSMs and their properties

[0218]

[0219] Note: GSM2 and comparative CGSM2 included a non-porous sheet PET-O1-T to provide mechanical strength during storage and transportation. This non-porous sheet was removed (peeled off) to obtain GSM3 and CGSM3, respectively.

[0220] As can be seen from Table 5 above, GSM1, GSM3 and GSM4 of the present invention have significantly better permeability than comparative gas separation membranes CGSM1, CGSM3 and CGSM4, even when a protective layer is present (see Example 3). GSM2 and comparative CGSM2 were not tested due to the non-porous sheet.

Claims

1. A gas separation membrane comprising the following layers: (i) an optional support layer; (ii) discrimination layer; (iii) additional layers; and (iv) an optional protective layer; in, (a) The additional layer (iii) and the discriminating layer (ii) each independently comprise a group of formula (1): M-(O-) x Formula (1) in, Each M is independently a metal or metalloid atom; O is an oxygen atom; and Each value of x is independently at least 4; (b) the additional layer (iii) comprises 1.5 to 10 atomic % of M of the group of formula (1), wherein M is as defined above; and (c) The discriminating layer (ii) comprises more than 10 atomic % of M groups of formula (1), wherein M is as defined above.

2. The gas separation membrane according to claim 1, wherein The additional layer (iii) has no gas separation selectivity and comprises 2 to 9 atom % of M of the group of formula (1).

3. The gas separation membrane according to claim 1 or 2, wherein: The discriminating layer (ii) comprises more than 10 atomic % and less than 50 atomic % of M groups of formula (1).

4. A gas separation membrane according to any one of the preceding claims, wherein The thickness of the additional layer (iii) is 1 nm to 1,500 nm.

5. A gas separation membrane according to any one of the preceding claims, wherein The thickness of the additional layer (iii) is 5 nm to 1,000 nm.

6. A gas separation membrane according to any one of the preceding claims, wherein The average value of the atomic % of M groups of formula (1) contained in the additional layer (iii) is substantially constant over the entire depth of the additional layer (iii).

7. A gas separation membrane as claimed in any preceding claim, comprising a protective layer of polysiloxane on top of the additional layer (iii).

8. A method for forming a gas separation membrane as claimed in any one of the preceding claims, comprising the steps of: (a) applying the discriminating layer (ii) to the support layer (i) by a plasma treatment process; and (b) applying an additional layer (iii) to said discriminating layer (ii) (DL) by a plasma treatment process; and Optionally (c) applying a protective layer (iv) to the additional layer (iii).

9. The method of claim 8, wherein: Step (b) is carried out by a plasma treatment process in the presence of one or more of the following precursor compounds: tetraethyl orthosilicate, hexamethyldisiloxane, tetramethyl orthosilicate, 1,3,5,7-tetramethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, bis(triethoxysilyl)ethane, tetrapropyl orthotitanate, titanium ethoxide, titanium tetraisopropoxide or zirconium tetra-tert-butoxide.

10. The method according to claim 8 or 9, wherein: Step (b) is carried out in an atmosphere free of oxygen.

11. The method according to any one of claims 8 to 10, wherein: The support layer (i) is or comprises a non-porous sheet, and the method further comprises the step of removing the non-porous sheet from the gas separation membrane. 12 . A gas separation module comprising the gas separation membrane according to claim 1 .

13. Use of the gas separation membrane according to any one of claims 1 to 7 or the gas separation module according to claim 12 for separating gases and / or purifying feed gases.