Gas separation membrane

By introducing an additional layer of M-(O-)x group into the gas separation membrane, the problem of reducing breathability caused by the protective layer is solved, and a gas separation membrane with high breathability and selectivity is achieved, which enhances the mechanical properties of the membrane .

CN118946400APending Publication Date: 2024-11-12YESTAR ADVANCED MATERIALS (SUZHOU) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380030412.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the conventional gas separation membrane contains a protective layer, the breathability is poor, making it difficult to simultaneously protect the discriminating layer from mechanical damage and maintain good breathability.

Method used

An additional layer containing M-(O-)x group is adopted, M is a metal or metal-like atom, with a value of x of at least 4, the additional layer is located on the opposite side of the support and discriminating layer, and is formed during plasma treatment. , ensuring that the additional layer is substantially constant throughout the depth, containing 1.5 to 10 atomic % M groups to improve the breathability and separation selectivity of the membrane.

Benefits of technology

The breathability of the gas separation membrane is significantly improved, while maintaining the selectivity of the discriminating layer, avoiding the reduction of the breathability of the protective layer, and enhancing the mechanical strength and durability of the membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059710950000031
    Figure BDA0005059710950000031
  • Figure BDA0005059710950000111
    Figure BDA0005059710950000111
  • Figure BDA0005059710950000141
    Figure BDA0005059710950000141
Patent Text Reader

Abstract

A gas separation membrane comprising the following layers: (i) a support layer; (ii) a discriminating layer; (iii) an additional layer wherein the additional layer comprises a group of formula (1): M-(O-) x formula (1) wherein each M is independently a metal or metalloid atom; o is an oxygen atom; and the value of each x is independently at least 4; and (iv) optionally a protective layer; wherein (a) the support layer (i) and the additional layer (iii) are located on opposite sides of the discrimination layer (ii); and (b) the additional layer (iii) comprises 1.5 at% to 10 at% of M of a group of formula (1) wherein M is as defined above.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to gas separation membranes (GSM) and their preparation and use.

[0002] Gas separation membranes generally include a support (for providing mechanical strength) and a discriminating layer for distinguishing between the gases to be separated. Typically, a protective layer is included on the discriminating layer to protect the discriminating layer from mechanical damage during processes such as handling and use of the membrane. Damage to the discriminating layer may have adverse consequences, such as significantly reducing the selectivity of the GSM.

[0003] Typically, the protective layer comprises polysiloxane and is formed on the discriminating layer by a wet chemical coating process.

[0004] While protective layers comprising polysiloxanes are useful for protecting the discriminating layer from damage, they also significantly reduce the breathability of the GSM. There is a need for a GSM that includes both a protective layer and good breathability.

[0005] According to a first aspect of the present invention, there is provided a gas separation membrane comprising the following layers:

[0006] (i) a support layer;

[0007] (ii) discrimination layer;

[0008] (iii) an additional layer, wherein the additional layer comprises a group of formula (1):

[0009] M-(O-) x

[0010] Formula (1)

[0011] in:

[0012] Each M is independently a metal or metalloid atom;

[0013] O is an oxygen atom; and

[0014] each value of x is independently at least 4; and

[0015] (iv) an optional protective layer;

[0016] in:

[0017] (a) the support layer (i) and the additional layer (iii) are located on opposite sides of the discriminating layer (ii); and

[0018] (b) The additional layer (iii) comprises 1.5 to 10 atomic % of M of the group of formula (1), wherein M is as defined above.

[0019] In this specification, the term "comprising" should be interpreted as requiring the presence of the stated parts, steps or components, but does not exclude the presence of one or more additional parts, steps or components. The use of the indefinite article "a" or "an" to refer to an element does not exclude the possibility of more than one element, unless the context clearly requires one and only one element. Therefore, the indefinite article "a" or "an" usually means "at least one". The optional groove layer is usually abbreviated as "GL", the discrimination layer or separation layer (ii) is usually abbreviated as "DL", and the optional protective layer (iv) is usually abbreviated as "PL".

[0020] In this specification, the separation or discrimination layer (ii) means a layer having separation selectivity. The layer having separation selectivity means a layer in which carbon dioxide (CO 2) is supplied to the obtained membrane by setting the total pressure on the gas supply side to 0.5 MPa at 40° C. after forming a membrane having a thickness of 0.05 to 30 μm. 2 ) and methane (CH 4 ) of pure gas, the permeability coefficient of carbon dioxide (P CO2 ) and the permeability coefficient of methane (P CH4 ) ratio (P CO2 / P CH4 ) is greater than 10. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In the attached picture:

[0022] FIG. 1( a ) is a schematic vertical cross-sectional view showing a gas separation membrane ( 10 ) including a support layer (i) ( 1 ), a discriminating layer (ii) ( 2 ), and an additional layer (iii) ( 3 ).

[0023] Figure 1(b) is the same as Figure 1(a), except that GSM also includes a protection layer (iv) (4)

[0024] In both Figures 1(a) and 1(b), the discriminating layer (2) is characterized by high gas selectivity, thereby providing the main function of the GSM. The protective layer (4) in Figure 1(b) is intended to reduce mechanical damage that the discriminating layer (2) and the additional layer (3) may suffer during, for example, handling and use of the GSM. The protective layer (iv) (4) typically has high gas permeability and high durability, thereby protecting the DL from mechanical damage.

[0025] Preferably, the support layer (i) comprises a porous sheet material ("PSM"). The PSM provides mechanical strength to the GSM and reduces the possibility of damage to the GSM when used under high pressure and / or high temperature.

[0026] Preferred PSMs include, for example, woven and nonwoven fabrics and combinations thereof.

[0027] The PSM can be composed, for example, of any suitable polymer or natural fiber. Examples of such polymers include polysulfone, polyethersulfone, polyimide, polyetherimide, polyamide, polyamideimide, polyacrylonitrile, polycarbonate, polyester, polyacrylate, cellulose acetate, polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, poly(4-methyl-1-pentene), particularly polyacrylonitrile.

[0028] Many suitable PSMs are commercially available. Alternatively, the PSM can be prepared using techniques known in the art for preparing such materials. In one embodiment, the optional PSM can be prepared by curing the curable component in a manner similar to that used to prepare the membrane, for example while ensuring that the pores of the PSM are too large to discriminate between different gases.

[0029] Preferably, layer (iii) is in contact with layer (ii). Typically, layer (ii) is sandwiched between layer (i) and layer (iii) and is in direct contact with layer (i) and layer (iii).

[0030] When layer (iv) is present, layer (iii) is typically sandwiched between layer (ii) and layer (iv) and is in direct contact with layer (ii) and layer (iv).

[0031] Optionally, for example, for the purpose of improving the wettability and / or adhesion of the support layer, the PSM may be subjected to corona discharge treatment, glow discharge treatment, flame treatment, ultraviolet irradiation treatment, or the like.

[0032] As PSM, for example, ultrafiltration membranes can be used, such as polysulfone ultrafiltration membranes, cellulose ultrafiltration membranes, polytetrafluoroethylene ultrafiltration membranes, polyvinylidene fluoride ultrafiltration membranes, and particularly polyacrylonitrile ultrafiltration membranes. Asymmetric ultrafiltration membranes can also be used, including ultrafiltration membranes comprising a porous polymer membrane (preferably having a thickness of 10 to 150 μm, more preferably 20 to 100 μm) and an optional woven or nonwoven fabric support.

[0033] The PSM is preferably as thin as possible as long as it provides the necessary structural strength to the GSM.

[0034] Preferably, the PSM comprises pores having an average pore size of 0.001 to 10 μm, preferably 0.01 to 1 μm (i.e., before the PSM has been converted to GSM). Preferably, the PSM comprises pores having an average pore size at the surface of 0.001 to 0.1 μm, preferably 0.005 to 0.05 μm. The average pore size can be determined by, for example, observing the surface of the PSM by scanning electron microscopy ("SEM"), or by cutting through the PSM and measuring the diameter of the pores within the porous PSM, again by SEM, and then calculating the average.

[0035] The porosity at the surface of the PSM can also be expressed as % porosity, i.e.

[0036]

[0037] The area required for the above calculations can be determined by examining the surface of the PSM by SEM prior to converting the PSM into a gas separation membrane.Thus, in preferred embodiments, the % porosity of the PSM is >1%, more preferably >3%, especially >10%, and more especially >20%.

[0038] Alternatively, the porosity of the PSM can be determined by measuring the N 2 The gas flow rate can be determined by any suitable technique, such as using a Pololux Flowmeter available from Polometer.com. TM 1000 devices. Typically, the Polorlux TM 1000 is set at maximum pressure (about 34 bar) and measures N 2 The gas flow rate (L / min) through the PSM under test. 2 (18.5 mm effective diameter) with an effective sample area of ​​N passing through the PSM at a pressure of approximately 34 bar. 2 The flow rate is preferably >1 L / min, more preferably >5 L / min, particularly >10 L / min, and more particularly >25 L / min. The higher of these flow rates is preferred because it reduces the likelihood that the gas flux of the resulting GSM will be reduced by the PSM. The above pore size and porosity refer to the pore size and porosity of the PSM before conversion to the GSM of the present invention.

[0039] The porosity of layer (i) (as a whole) can be expressed as CO 2 Gas permeability (unit: m 3 (STP) / m 2 .s.kPa). If the GSM is intended for gas separation, the CO 2 The gas permeability is preferably 5 to 150×10 -5 m 3 (STP) / m 2 .s.kPa, more preferably 5 to 100×10 -5 m 3 (STP) / m 2 .s.kPa, most preferably 7 to 70×10 -5 m 3 (STP) / m 2 .s.kPa.

[0040] Layer (i) (as a whole) has no gas separation selectivity compared to the discriminating layer (ii).

[0041] The average thickness of layer (i) (as a whole) is preferably from 20 to 500 μm, preferably from 50 to 400 μm, in particular from 100 to 300 μm.

[0042] Preferably, layer (i) further comprises a channel layer ("GL"). When layer (i) comprises a GL, the GL is preferably located between the PSM and the discriminating layer (ii) (in direct contact with the discriminating layer (ii)).

[0043] The additional layer (iii) may contain M from other sources, not just M derived from groups of formula (1). Thus the "total atomic % of M present in the additional layer (iii)" (as distinct from the atomic % of M of groups of formula (1) as described in claim 1) includes M from all sources, including but not limited to M from groups of formula (1). For example, the "total atomic % of M present in the additional layer (iii)" includes M from other sources, such as from one or more groups of formula (2):

[0044] M-(O-) z

[0045] Formula (2)

[0046] in:

[0047] M is a metal or metalloid atom;

[0048] O is an oxygen atom; and

[0049] The value of z is 1, 2, or 3.

[0050] Typically, the additional layer (iii) comprises groups of the formula (1) and groups of the formula (2).

[0051] Preferably, each M (in formula (1) and formula (2)) is independently silicon, titanium, zirconium or aluminum. Preferably, each M (in formula (1) and formula (2)) is silicon, titanium, zirconium and / or aluminum.

[0052] Preferably, the additional layer (iii) comprises greater than 10 atomic % and less than 50 atomic % of M of the group of formula (1), in particular 12 to 30 atomic % of M of the group of formula (2), more particularly 13 to 27 atomic % of M of the group of formula (2), wherein M is as defined above.

[0053] Preferably, the additional layer (iii) comprises 2 to 9 atomic % of M, more preferably 3 to 8 atomic % of M, of the radical of formula (1), wherein M is as defined above.

[0054] When the additional layer (iii) comprises more than 10 atomic % of M of the group of formula (1), the gas permeability of the GSM is significantly reduced or plummeted, and the additional layer also becomes discriminating. 2 and CH 4 There is no separation selectivity or discrimination between the gases. When the additional layer (iii) contains less than 1.5 atomic % of M of formula (1), the permeability of GSM is significantly reduced.

[0055] Preferably, the total atomic % of M present in the additional layer (iii) (i.e. M from all sources, e.g. from groups of formula (1) + groups of formula (2)) is from 13.5 to 35 atomic %, in particular from 15 to 33 atomic %, more in particular from 16 to 32 atomic %. Preferably, the composition of the additional layer (iii) is substantially constant over its depth. For example, over at least 80% of the depth of the additional layer (iii), the atomic % of M of groups of formula (1) present in the additional layer (iii) varies by less than 25% (more preferably less than 10%, in particular less than 5%) relative to the average atomic % of M in the additional layer (iii). For example, if the average atomic % of M in the additional layer (iii) is "X %", then over at least 80% of the depth of the additional layer (iii), the atomic % of M in the additional layer (iii) is preferably from 0.75X to 1.25X (more preferably from 0.9X to 1.1X, in particular from 0.95X to 1.05X).

[0056] The atomic % of M in the additional layer (iii) (and in DL (ii)) (e.g. derived from groups of formula (1) and from any groups of formula (2), etc.) can be determined using surface analysis equipment, such as by X-ray photoelectron spectroscopy (XPS) (e.g. using GC-IB / XPS gas cluster ion beam XPS). Such equipment can also be used to determine the atomic % of M at the top surface and at different depths in and below the surface in the additional layer (iii) and any other layers (e.g. DL or GL, when present). A suitable device for performing surface analysis to determine the atomic % of M in each layer is the VersaProbe II XPS apparatus ("ULVAC-PHI") from Physical Electronics, Inc. The ULVAC-PHI is preferably provided with a monochromatic Al K α (1486.6eV, 15W 25KV An X-ray source with a raster size of 300 μm × 300 μm) is used. For charge compensation, low energy electrons and Ar ions can be flooded when measuring the atomic % of M in each layer. An Ar gas cluster beam (5 kV, 20 nA, 2 mm × 2 mm) can be used for depth profile analysis. From this analysis, the atomic % of M and any other elements (such as carbon and oxygen) present in the additional layer (iii) can be measured. At the data point where the atomic % of M is the highest, the atomic % of M in the additional layer (iii) can be determined. This will include M from all sources, such as the groups of formula (1) or formula (2) defined above, and the amount of M in each of these groups can be quantified separately. For example, when M is silicon, Si-(O) 4 Groups and Si-(O-) z The atomic % of silicon in the group (where z is 1, 2 or 3) can be quantified by this method. In the spectrum of Si2p, the binding energy at 102.6 eV is defined as the group of formula (2), while the binding energy at 103.8 eV is defined as the group of formula (1), wherein formula (1) and formula (2) are as defined above. The area ratio of Si2p at 102.6 eV and 103.8 eV can be converted into an atomic ratio (atomic %) so that the sum of the areas of the separated peak components will correspond to the atomic % of Si.

[0057] In one embodiment, the additional layer (iii) comprises a substantially constant amount of 1.5 to 10 atomic % of M of the group of formula (1) over the entire depth of the additional layer (iii). For example, the atomic % of M of the group of formula (1) present in the additional layer (iii) varies by less than 25% relative to the average atomic % of M over the entire depth of the additional layer (iii). By constructing Si-(O-) 4 The substantially constant atomic % of Si (1.5 to 10% higher than DL) can be considered that the additional layer (iii) is formed in a CO 2 and CH 4 or in gases such as CO 2 and O 2 , O 2 and N 2 or H 2 and CH 4 There is little separation selectivity or no discrimination between gases such as CO. In the present application, no gas selectivity means that a person skilled in the art would not propose to use the additional layer (iii) as a CO 2 and CH 4 or such as CO 2 and O 2 , O 2 and N 2 or H 2 and CH 4Sources or implementations of meaningful gas separations between gases such as .

[0058] The atomic % of M of the group of formula (1) (wherein M is as defined above) is the atomic % of M present in the relevant layer as a group of formula (1). Similarly, the atomic % of M of the group of formula (2) (wherein M is as defined above) is the atomic % of M present in the relevant layer as a group of formula (2).

[0059] In one embodiment, the additional layer (iii) is obtainable or obtained by a process comprising plasma treatment. Suitable plasma treatment processes include plasma deposition, in particular plasma treatment of a compound comprising M, thereby forming an additional layer (iii) comprising a group of formula (1) and optionally a group of formula (2), each as defined above. A preferred plasma treatment process is carried out using a precursor at atmospheric pressure in the absence of oxygen and / or air.

[0060] The groups of formula (1) and, if present, the groups of formula (2), each as defined and preferred above, are present in layer (iii), but they may optionally also be present in layer (ii) when the discriminating layer (ii) has also been treated with plasma (as described in detail below).

[0061] In one embodiment, the additional layer (iii) is applied to the discriminating layer (ii) by a plasma treatment process using precursor compounds providing groups of formula (1). As carrier gas a noble gas such as argon or helium can be used.

[0062] The plasma treatment process for applying layer (iii) to layer (ii) is preferably carried out at a temperature of 0.30-9.00 J / cm 2 (and using low pressure or even in (remote) atmospheric pressure plasma treatment).

[0063] The plasma treatment process for applying layer (iii) to layer (ii) preferably uses 5 to 500 cm 3 (STP) / min, more preferably 50 to 200 cm 3 (STP) / min, particularly preferably 80 to 120 cm 3 The low-pressure plasma treatment is preferably carried out at a gas pressure of 0.6 to 100 Pa, more preferably 1 to 60 Pa, particularly preferably 2 to 40 Pa.

[0064] When silicon-containing precursor compounds are used during the plasma treatment, this results in the additional layer (iii) being deposited on layer (ii) as a silicon dioxide-like top surface comprising groups of formula (1) and optionally groups of formula (2), all as defined above.

[0065] The average thickness of the additional layer (iii) is generally from 1 to 1500 nm, more preferably from 5 to 1000 nm, even more preferably from 10 to 500 nm.

[0066] According to a second aspect of the present invention, there is provided a method for forming the gas separation membrane of the first aspect of the present invention, comprising the following steps:

[0067] (a) applying the discriminating layer (ii) to the support layer (i) by a wet coating process, a physical vapor deposition process, a chemical vapor deposition process, an induced deposition process, an atomic layer deposition process or a plasma treatment process; and

[0068] (b) applying an additional layer (iii) to the discriminating layer (ii) (DL) by a plasma treatment process; and

[0069] Optionally (c) a protective layer (iv) is applied to the additional layer (iii).

[0070] In a preferred embodiment, the discriminating layer (ii) is applied to the support layer (i) by a plasma treatment process (e.g. using a plasma treatment apparatus). A preferred plasma treatment process for applying the discriminating layer (ii) to the support layer (i) comprises the use of an atmospheric pressure glow discharge plasma, such as described in US10427111, page 40, line 4 to page 41, line 36, which is incorporated herein by reference. For example, the support layer (i) may be exposed to an atmospheric pressure glow discharge plasma to form the discriminating layer (ii) thereon.

[0071] The plasma treatment process that can be used for step (b) and optionally for step (a) is preferably carried out using a plasma treatment device comprising a treatment space and a first electrode and a second electrode in the treatment space so as to generate an atmospheric pressure glow discharge plasma between the first electrode and the second electrode. The electrodes can be provided with a dielectric barrier in various arrangements. In one arrangement, the dielectric barrier of at least one electrode is formed by a polymer film or an inorganic dielectric. Polymers such as polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE) or polyethylene (PE) or ceramics such as silicon dioxide or alumina, or combinations of these, can be used, and microporous dielectric materials attached to the electrodes can also be used.

[0072] In a preferred embodiment, the additional layer (iii) is applied to the discriminating layer (ii) using an atmospheric pressure glow discharge plasma (as a plasma treatment process).

[0073] As mentioned above, preferably, the atomic % of M of the group of formula (1) in the additional layer (iii) is substantially constant from the top surface to the entire depth of the additional layer (iii). In order to achieve a substantially constant atomic % of M of the group of formula (1) in the additional layer (iii), the manufacturing process of the additional layer (iii) is preferably different from the process for manufacturing the DL using precursors in the presence of rare and inert gases and in the absence of oxygen (when the DL is manufactured using plasma treatment).

[0074] In step (b), the plasma treatment process preferably comprises applying a plasma at 0.03 to 30 W / cm 2 An atmospheric pressure glow discharge plasma is generated at an effective power density of preferably less than 120 seconds. Preferably, the processing space is free of oxygen (eg, the processing space comprises an oxygen-free inert gas).

[0075] In step (a), the plasma treatment process (when used) preferably comprises a plasma treatment process at 0.1 to 30 W / cm 2 Atmospheric pressure glow discharge plasma is generated at an effective power density of preferably less than 60 seconds. Preferably, in this case, in step (a), the processing space comprises an oxygen-rich atmosphere.

[0076] Therefore, it is preferred that both steps (a) and (b) comprise a plasma treatment process, wherein step (b) is performed in an atmosphere free of oxygen and step (a) is performed in an atmosphere containing oxygen.

[0077] The plasma treatment process may be carried out using a precursor compound, particularly an organosilicon compound. The preferred plasma treatment process in step (b) uses a precursor compound. The precursor compound may be contained in the treatment space and preferably at a concentration of 0.1 to 10 J / cm 2 of energy (in step (b)).

[0078] In a preferred embodiment, the treatment space used in step (b) comprises an atmosphere free of air or oxygen and a 0.1 to 10 J / cm 2 power density.

[0079] In a preferred embodiment, the plasma treatment process used in steps (a) and / or (b) comprises stabilizing an atmospheric pressure glow discharge plasma according to any of the methods described in, for example, US6774569 or EP1383359.

[0080] In a preferred embodiment, the plasma treatment process used in step (b) comprises exposing the discriminating layer (ii) to an atmospheric pressure glow discharge plasma, wherein the plasma is stabilized by an inductive and capacitive (LC) matching network as described in, for example, EP1917842.

[0081] In another embodiment, the additional layer (iii) may be applied to layer (ii) (DL) using a plasma treatment in a low pressure plasma environment as described in US10427111.

[0082] In another embodiment, the plasma treatment apparatus for performing the plasma treatment step may include a conveying device for conveying layer (i) (support layer) or the combination of layer (i) + (ii) through the electrode. In addition, the conveying device may include a tensioning mechanism for maintaining layer (i) or layer (i) + (ii) in close contact with the electrode.

[0083] In one embodiment, the additional layer (iii) can be obtained from one or more precursor compounds that can be contained in the processing space. Precursor compounds that can be used to provide the group of formula (1) (as defined above) and the optional group of formula (2) (as defined above) include TEOS (tetraethyl orthosilicate), HMDSO (hexamethyldisiloxane), TMOS (tetramethyl orthosilicate), TMCTS (1,3,5,7-tetramethylcyclotetrasiloxane), D4 OMCTS (octamethylcyclotetrasiloxane), D5 (decamethylcyclopentasiloxane), D6 (dodecylcyclohexasiloxane), bis (triethoxysilyl) ethane (BTESE), TPOT (tetrapropyl orthotitanate), TEOT (titanium ethoxide), TTIP (titanium tetraisopropoxide) or ZTB (zirconium tetra-tert-butoxide).

[0084] A substantially uniform additional layer (iii) can be prepared using an atmospheric pressure glow discharge apparatus as described in EP 1917842, using an inductive and capacitive (LC) matching network. In this embodiment, the additional layer (iii) has an average thickness of 1 to 1000 nm, even more preferably 10 to 500 nm.

[0085] Therefore, in a preferred embodiment of the method of the second aspect of the invention, step (a) comprises applying the discriminating layer (ii) to the support layer (i) by a plasma treatment process, and step (b) comprises applying the additional layer (iii) to the discriminating layer (ii) by a plasma treatment process.

[0086] As described above, layer (i) preferably comprises a PSM and an optional groove layer ("GL"). The GL (when present) is preferably attached to (e.g. coated on) the PSM. In addition, the GSM optionally includes a PL. When the GSM does not contain a PL, it can still be used for gas separation, or it can be sold as a commercial product so that customers can apply their own customized PL according to their needs. The optional GL and PL are permeable to gases and generally have a low ability to distinguish between gases. When present, the GL and PL preferably comprise a polymer resin, particularly a polysiloxane. Preferred polysiloxanes present in or as the GL and / or PL are poly(dimethyl)siloxanes, for example comprising -Si-(CH 3 ) 2 -O- repeating units.

[0087] The average thickness of GL (when present) is preferably from 50 to 2400 nm, more preferably from 150 to 800 nm, especially from 200 to 650 nm.

[0088] The average thickness of the PL (when present) is preferably from 10 to 10000 nm, more preferably from 50 to 5000 nm, especially from 100 to 3000 nm.

[0089] Preferred GL and PL each independently comprise groups capable of bonding to metals, for example by covalent bonds, ionic bonds and / or by hydrogen bonds, preferably by covalent bonds. The properties of these groups depend to some extent on the chemical composition of the GL / PL and the properties of the metal, but typically these groups are selected from epoxy groups, oxetane groups, carboxylic acid groups, amino groups, hydroxyl groups, vinyl groups, hydrogen groups and thiol groups. More preferably, GL and PL each independently comprise polymers having carboxylic acid groups, epoxy groups or oxetane groups, vinyl groups, hydrogen groups, or a combination of two or more of these groups. These polymers can be formed on a support by a method comprising the following process: curing a radiation-curable or heat-curable composition, in particular a curable (e.g. radiation-curable) composition comprising a polymerizable dialkylsiloxane. The latter option can be used to provide preferred GL and PL comprising dialkylsiloxane groups.

[0090] The polymerizable dialkylsiloxane that may be present in the optional GL and PL is preferably a monomer comprising dialkylsiloxane groups, or a polymerizable oligomer or polymer comprising dialkylsiloxane groups. For example, as described in more detail below, the GL and / or PL may be prepared from a radiation-curable composition comprising a partially crosslinked radiation-curable polymer comprising dialkylsiloxane groups. Typical dialkylsiloxane groups have the formula -{O-Si(CH 3 ) 2}n-, wherein n is at least 1, for example 1 to 100. Poly(dialkylsiloxane) compounds having terminal vinyl groups are also available, and these compounds can be incorporated into GL by a curing process.

[0091] In one embodiment, GL does not contain Si-C 6 H 5 The group.

[0092] In one embodiment, PL does not contain Si-C 6 H 5 The group.

[0093] The irradiation of the radiation-curable composition to form the optional GL or PL (sometimes referred to as "curing" in this specification) can be carried out using any source that provides the necessary radiation wavelength and intensity to polymerize the radiation-curable composition and thereby form a GL on the PSM or a PL on the additional layer (iii). For example, electron beams, ultraviolet radiation (UV), visible light and / or infrared radiation can be used to irradiate (cure) the radiation-curable composition, and the appropriate radiation is selected to match the components of the composition.

[0094] The optional GL and PL are preferably each independently obtained by curing a curable composition comprising:

[0095] (1) 0.5 to 25 wt. % of radiation-curable components, at least one of which contains dialkylsiloxane groups;

[0096] (2) 0 to 5 wt % of a photoinitiator; and

[0097] (3) 70 to 99.5% by weight of an inert solvent.

[0098] Preferably, the curable composition used to prepare the GL / PL has a titanium:silicon molar ratio of at least 0.0005, more preferably from 0.001 to 0.1, especially from 0.003 to 0.03.

[0099] The radiation-curable component of component (1) generally comprises at least one radiation-curable group. Radiation-curable groups include ethylenically unsaturated groups (e.g. (meth)acrylic groups (e.g. CH 2 =CR 1 C(O)-groups), especially (meth)acrylate groups (e.g. CH 2 =CR 1 C(O)O- groups), (meth)acrylamide groups (e.g. CH 2 =CR 1 C(O)NR 1 - group), where each R 1are independently H or CH 3 ), especially oxetane or epoxy groups (such as glycidyl and epoxycyclohexyl).

[0100] The amount of radiation curable component (i.e. component (1)) present in the curable composition for preparing the optional GL and / or the optional PL is preferably 1 to 20 wt %, more preferably 2 to 15 wt %. In a preferred embodiment, component (1) of the curable composition for preparing the GL and / or the PL comprises a partially crosslinked radiation curable polymer comprising dialkylsiloxane groups.

[0101] The function of the inert solvent (3) is to provide the composition with a viscosity suitable for the particular method of applying the curable composition to the support. For high-speed application methods, low-viscosity inert solvents are generally selected. Examples of suitable inert solvents are mentioned above in relation to the preparation of the polymer sheet.

[0102] The amount of inert solvent (3) (ie component (3)) present in the curable composition for preparing the optional GL and / or PL is preferably 70 to 99.5% by weight, more preferably 80 to 99% by weight, especially 90 to 98% by weight.

[0103] Inert solvents are not radiation curable.

[0104] The composition may contain other components, such as surfactants, surface tension modifiers, viscosity building agents, biocides, and / or other components capable of copolymerizing with other ingredients.

[0105] The function of the discriminating layer (ii) is to discriminate between gases, separating the feed gas mixture into a permeate gas that passes through the GSM and a retentate that cannot pass through the GSM. The permeate gas and the retentate generally contain the same gas as the feed gas mixture, but one is enriched in at least one gas present in the feed gas, while the same gas in the other is depleted. The average thickness of the discriminating layer is preferably 1 nm to 2 μm, more preferably 3 nm to 1 μm, and especially 5 nm to 200 nm.

[0106] DL (layer (ii)) can be capable of discriminating between gases to be separated (e.g. from CH 4 Separation of CO 2 ). Preferably, the selectivity of the discriminating layer (ii) for one gas to be separated over another gas to be separated is at least 10. In contrast, the selectivity of the additional layer (iii) for one gas to be separated over another gas to be separated is much lower than 10, for example, less than 8, or even much lower than 5.

[0107] The discriminating layer (ii) can be prepared (in a wet coating process) from a composition comprising a polymer, an inert solvent and optionally an initiator. The inert solvent can be any solvent capable of dissolving the polymer used to form the discriminating layer (ii). The suitability of the solvent is determined by the nature of the polymer and the desired concentration. Suitable solvents include water; 5-10 Alkanes, such as cyclohexane, heptane and / or octane; alkylbenzenes, such as toluene, xylene and / or C 10-16 Alkylbenzene; C 1-6 Alkanols, for example methanol, ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, cyclopentanol and / or cyclohexanol; linear amides, for example dimethylformamide or dimethylacetamide; ketones and ketoalcohols, for example acetone, methyl ether ketone, methyl isobutyl ketone, cyclohexanone and / or diacetone alcohol; ethers, for example tetrahydrofuran and / or dioxane; diols, preferably diols having 2 to 12 carbon atoms, for example 1,5-pentanediol, ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol and / or thiodiglycol; oligo- or polyalkylene glycols, for example diethylene glycol, triethylene glycol, polyethylene glycol and / or polypropylene glycol; triols, for example glycerol and / or 1,2,6-hexanetriol; mono-C 1-4 Alkyl ethers, preferably mono-C 1-4 Alkyl ethers, for example 2-methoxyethanol, 2-(2-methoxyethoxy)ethanol, 2-(2-ethoxyethoxy)ethanol, 2-[2-(2-methoxyethoxy)ethoxy]ethanol, 2-[2-(2-ethoxyethoxy)ethoxy]ethanol and / or ethylene glycol monoallyl ether; cyclic amides, for example 2-pyrrolidone, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, caprolactam and / or 1,3-dimethylimidazolidinone; cyclic esters, for example caprolactone; sulfoxides, for example dimethyl sulfoxide and / or sulfolane; and mixtures comprising two or more of the aforementioned solvents, in particular mixtures comprising methyl ethyl ketone and tetrahydrofuran.

[0108] The discriminating layer (ii) preferably comprises, as polymer, polyimide, cellulose acetate, polyethylene oxide or polyetherimide, in particular a polyimide comprising trifluoromethyl groups. Particularly preferred discriminating layer (ii) comprises a polyimide containing groups of formula (3):

[0109]

[0110] wherein Ar is an aromatic group and R is a carboxylic acid group, a sulfonic acid group, a hydroxyl group, a thiol group, an epoxy group or an oxetane group.

[0111] Polyimides containing trifluoromethyl groups can be prepared by conventional methods, such as those described in US Pat. Reissue No. 30,351 (based on US Pat. No. 3,899,309), US Pat. No. 4,717,394, and US Pat. No. 5,085,676.

[0112] In one embodiment of the method of the second aspect of the invention, as described in the above step (a) and as described in WO2022 / 207359 applied by the present applicant (included herein by reference), the discriminating layer (ii) is prepared by plasma surface treatment of the support layer (i) comprising polysiloxane GL, as a result of which the discriminating layer (ii) comprises a gradient of the atomic % of M of the group of formula (1), and the surface atomic % of M of the group of formula (1) of the discriminating layer is greater than 10.

[0113] The GSM of the present invention may be packaged and supplied commercially to companies that assemble gas separation modules, for example for their own use or for onward sale.

[0114] According to a third aspect of the present invention, there is provided a gas separation module comprising one or more gas separation membranes according to the first aspect of the present invention.

[0115] The gas separation module of the present invention preferably further comprises a feed carrier and a permeate carrier, optionally wound onto the perforated tube.

[0116] Preferred gas separation modules include spiral type modules, hollow fiber type modules, pleated type modules, tubular type modules and plate and frame type modules.

[0117] According to a fourth aspect of the present invention, there is provided use of the gas separation membrane of the first aspect of the present invention or the gas separation module of the third aspect of the present invention for separating gases and / or for purifying feed gases.

[0118] The gas separation membranes and modules of the present invention are particularly suitable for separating a feed gas containing a target gas into a gas stream rich in the target gas and a gas stream poor in the target gas. For example, a feed gas containing polar and non-polar gases can be separated into a gas stream rich in polar gases and a gas stream poor in polar gases. In many cases, the feed gas rich in polar gases is more concentrated than the non-polar gases (e.g., alkanes, H 2 and N 2 ), the membrane is resistant to polar gases (such as CO 2 , H 2 S. NH 3 、SO x and nitrogen oxides, especially NO x ) has a high permeability. Therefore, the polar gas is preferably CO 2 , H 2 S. NH3 、SO x , nitrogen oxides or a combination of two or more thereof. The non-polar gas is preferably N 2 , H 2 , alkanes or a combination of two or more thereof.

[0119] Preferably, the polar and non-polar gases are gaseous when at 25°C.

[0120] The target gas may be, for example, a gas that has value to the user of the module or element and that the user wishes to collect. Alternatively, the target gas may be an undesirable gas, such as a pollutant or "greenhouse gas," that the user wishes to separate from the gas stream to meet product specifications or to protect the environment.

[0121] The modules and GSM of the present invention are particularly suitable for removing polar gases (CO 2 , H 2 S) to purify natural gas (a mixture containing mainly methane); for purifying synthesis gas; and for removing CO from hydrogen and flue gas 2 Flue gases commonly come from fireplaces, ovens, furnaces, boilers, internal combustion engines, and power plants. The composition of flue gases depends on what is being burned, but generally they contain mostly nitrogen from the air (often more than two-thirds), carbon dioxide (CO 2 ) from the combustion, and nitrogen from the atmosphere. 2 ). Flue gases also contain low percentages of pollutants such as particulate matter, carbon monoxide, nitrogen oxides, and sulfur oxides. Recently, in response to environmental issues (global warming), CO 2 The separation and capture of

[0122] The module and GSM of the present invention are particularly suitable for the separation of: 2 and N 2 The feed gas is separated into a CO richer feed gas than the 2 The gas flow and the CO content of the feed gas 2 less airflow; will contain CO 2 and CH 4 The feed gas is separated into a CO richer feed gas than the 2 The gas flow and the CO content of the feed gas 2 less airflow; will contain CO 2 and H 2 The feed gas is separated into a CO richer feed gas than the 2 The gas flow and the CO content of the feed gas 2 Less airflow; will contain H 2 S and CH 4 The feed gas is separated into a feed gas richer in H 2 S gas flow and the H content of the feed gas2 S less airflow; and will contain H 2 S and H 2 The feed gas is separated into a feed gas richer in H 2 S gas flow and the H content of the feed gas 2 S less airflow;

[0123] The modules and GSMs of the present invention are particularly suitable for separating a "dirty" feed gas comprising polar gases, non-polar gases and hydrocarbons containing at least two (e.g., 2 to 7) carbon atoms into a permeate gas and a retentate gas, one of the two gases being rich in polar gases and the other being poor in polar gases.

[0124] The invention will now be illustrated by the following non-limiting examples in which all parts and percentages are by weight unless otherwise stated. Example

[0125] In these examples, the performance of the GSM was measured using a multilayer structure having the overall structure shown in Table 1, comprising a gas separation membrane under test having a support layer (i) of 05TH100S facing downward, a 05TH100S sheet, and a 42369 sheet.

[0126] The 05TH100S sheet and the 42369 sheet are described in more detail below.

[0127] Table 1 – Multilayer structure including GSM

[0128] Gas separation membrane tested 05TH100S sheet 42369 Sheet

[0129] In the examples, the feed gas used had the composition shown in Table 2 below.

[0130] Table 2

[0131]

[0132] The performance properties of the inventive GSM and comparative GSM were measured using the multilayer structures shown in Table 1 by the following techniques:

[0133] (A) Permeability

[0134] Feed gas having the composition described in Table 2 above was passed through the multilayer structure shown in Table 1 under test at 40°C and a gas feed pressure of 6000 kPa. CO was measured using a gas permeation cell having a measuring diameter of 2.0 cm. 2 、nC 4 H 10 and CH 4 Flux through the multilayer structures shown in Table 1.

[0135] After continuous use of the multilayer structure shown in Table 1 (including the tested GSM) for 5 minutes, CO was measured using the following equation: 2 、nC 4 H 10 and CH 4 The permeability (Q i ):

[0136] Q i =(θ Perm ·X Perm,i ) / (A·(P Feed ·X Feed,i -P Perm ·X Perm,i ))

[0137] in:

[0138] Q i = the permeability of the gas of interest (i.e., i is CO 2 or nC 4 H 10 or CH 4 )(m 3 (STP) / m 2 kPa s);

[0139] θ< Perm = permeation flow rate (m 3 (STP) / s);

[0140] X Perm,i = volume fraction of the relevant gas in the permeating gas;

[0141] A = membrane area (m 2 );

[0142] P Feed = feed gas pressure (kPa);

[0143] X Feed,i = volume fraction of the relevant gas in the feed gas;

[0144] P Perm = permeate gas pressure (kPa); and

[0145] STP is standard temperature and pressure, which is defined herein as 25.0°C and 1 atmosphere (101.325 kPa).

[0146] (Q i ) can be achieved through 1 GPU = 1×10 -6 cm 3 (STP) / (s·cm 2 cmHg).

[0147] CO will be higher than 150 GPU 2 The penetration rate is rated as good and will be less than or equal to 150 GPU of CO 2 The permeability of was evaluated as a comparative result, which was not good compared with the examples of the present invention.

[0148] (B) Selectivity

[0149] The selectivity (CO 2 / C 4 H 10 and CO 2 / CH 4 ; αCO 2 / C 4 H 10 and αCO 2 / CH 4 ) Based on the following equation, QCO is calculated from the above 2 and Qn-C 4 H 10 calculate:

[0150] αCO 2 / nC 4 H 10 =QCO 2 / Qn-C 4 H 10 ;

[0151] αCO 2 / CH 4 =QCO 2 / QCH 4

[0152] Among them, QCO 2 , QCH 4 and Qn-C 4 H 10 Determined by the method described in step (A) above.

[0153] αCO above 100 2 / nC 4 H 10 Values ​​are considered acceptable, while αCO values ​​below 100 2 / nC 4 H 10 The value is considered unacceptable.

[0154] αCO above 15 2 / CH 4 Values ​​are considered acceptable, while αCO values ​​less than 15 2 / CH4 The value is considered unacceptable.

[0155] (C) Groove layer thickness

[0156] The thickness of the channel layer is determined by cutting through the support layer (i) and measuring the thickness of the channel layer from the sheet outwards using a SEM.

[0157] (D) Atomic % of M in the group of formula (1)

[0158] The atomic % of M of the group of formula (1) in DL and FL was determined using the conventional method described above using a GC-IB / XPS gas cluster ion beam XPS apparatus ("ULVAC-PHI") from Physical Electronics, Inc. using X-ray photoelectron spectroscopy. The ULVAC-PHI was equipped with a monochromator Al K α (1486.6eV, 15W 25KV An X-ray source with a raster size of 300 μm × 300 μm was used. For charge compensation, low energy electrons and Ar ions can be flooded when measuring the atomic % of M in each layer. An Ar gas cluster beam (5 kV, 20 nA, 2 mm × 2 mm) can be used for depth profiling.

[0159] Preparation of gas separation membranes

[0160] The following materials were used to prepare the GSM and multilayer structures:

[0161] PAN is a porous sheet with an average thickness of 170-180 μm, which comprises a PET nonwoven support (thickness of 140-150 μm) with a porous polyacrylonitrile layer. PAN was obtained from Microdyn-Nadir GmbH, Germany, under the trade name UA100T.

[0162] HI is a nonwoven porous sheet (ie, support layer (i)) called Hi-star 05TH-100 from Hirose paper MFG Co. Ltd., having an average thickness of 150 μm.

[0163] X-22-162C is a dual-end reactive silicone with carboxylic acid reactive groups and a viscosity of 220 mm 2 / s and the equivalent weight of the reactive group was 2,300 g / mol, which was obtained from Shin-Etsu Chemical Co., Ltd. (MWT 4,600) (1 is an integer).

[0164]

[0165] DBU is 1,8-diazabicyclo[5.4.0]undec-7-ene from Sigma Aldrich.

[0166] UV-9300 is SilForce from Momentive Performance Materials Holdings TM UV-9300, whose epoxy equivalent weight is 950 g / mol ethylene oxide (MWT 9000, measured by viscosity) (m and n are integers).

[0167]

[0168] I0591 is 4-isopropyl-4'-methyldiphenyliodonium tetrakis(pentafluorophenyl)borate (C 40 H 18 BF 20 I).

[0169]

[0170] Ti(OiPr) 4 is titanium(IV) isopropoxide (MWT 284) from Dorf Ketal Chemicals.

[0171] n-Heptane was n-heptane from Brenntag Nederland BV.

[0172] MEK is 2-butanone from Brenntag Nederland BV.

[0173] CA is cellulose acetate CA-398-3 from Eastman Chemicals.

[0174] FOR is formamide from Thermo Scientific Acros.

[0175] AC is acetone from Sigma-Aldrich 179124.

[0176] PI is 6FDA-TeMPDx / DABAy, x / y=20 / 80; it was obtained from FUJIFILM Corporation and has the following structure:

[0177]

[0178] HMDSO is hexamethyldisiloxane supplied by Merck and used as precursor for the additional layer (iii) of the present invention.

[0179] MIBK is methyl isobutyl ketone from Brenntag Nederland BV.

[0180] DIOX is 1,3-dioxolane from Brenntag Nederland BV.

[0181] APTMS is 3-methoxysilylpropan-1-amine from Sigma-Aldrich.

[0182] 05TH100S sheet is a sheet from Hirose paper manufacturing (wet-laid polyester nonwoven / average thickness 100 μm / average weight 100 g / m 2 / Average density 0.93g / cm 3 ).

[0183] 42369 sheet is a macroporous sheet from Guilford (woven fabric made of polyethylene terephthalate and epoxy resin / average thickness 0.3 mm / 60 wpi (number of wales per 2.54 cm) / 59 cpi (number of courses per 2.54 cm)).

[0184] Preparation of gas separation membranes

[0185] Stage a) Preparation of partially cured polymer ("PCP polymer")

[0186] The components UV-9300, X-22-162C and DBU were dissolved in n-heptane in the amounts shown in Table 3 and maintained at 91° C. for 168 hours. The Si content (meq / g polymer) of the resulting polymer (PCP polymer) was 12.2, and the viscosity of the resulting PCP polymer solution at 25.0° C. was 125 mPas.

[0187] Table 3 – Ingredients used to prepare PCP polymers

[0188] Element Amount (weight %) UV-9300 (weight %) 46.395 X-22-162C (weight %) 13.596 DBU (wt%) 0.009 n-Heptane (weight %) 40.000

[0189] Stage b) Preparation of radiation-curable composition C

[0190] The PCP polymer solution from step a) was cooled to 20°C and diluted with n-heptane to obtain the PCP polymer concentrations shown in Table 4 below. The solution was then filtered through a filter paper with a pore size of 2.7 μm. A photoinitiator (I0591) and a metal complex (Ti(OiPr)) were then added in the amounts (wt%) shown in Table 4. 4 ), and a curable composition C is obtained. Ti(OiPr) present in the curable composition C 4The amount corresponds to 55.4 μmol Ti(OiPr) 4 / g PCP polymer. In addition, the molar ratio of metal to silicon in curable composition C was 0.0065.

[0191] Table 4 - Ingredients of Curable Composition C

[0192] Element Amount (weight %) PCP polymer 10.000 I0591 0.105 <![CDATA[Ti(OiPr) 4 ]]> 0.226 DBU 0.001 MEK 2.008 n-Heptane 87.660

[0193] Curable Composition C was used to prepare the groove layers in the GSMs of Examples 1 and 3 to 8 and Comparative Examples C1, C3 and C4 and the protective layers of Examples 7 to 9 and Comparative Examples C1-C4, as described in more detail below.

[0194] Step i. Preparation of PAN-GL support layer (i)

[0195] The porous support layer PAN-GL was prepared by applying the curable composition C to PAN and curing the composition as follows:

[0196] The curable composition C (prepared as described in stage b) above) was applied to the PAN (porous sheet) by meniscus dip coating at a speed of 10 m / min, and then the coated porous sheet was irradiated with an intensity of 16.8 kW / m (70%) using a Light Hammer LH10 from Fusion UV Systems equipped with a D bulb. The resulting support layer (i) (PAN-GL) comprises a porous sheet and polysiloxane (grooved layer with a dry thickness of 600 nm, and is used as GL in Examples 1 and 3 to 8 and Comparative Examples C1, C3 and C4). The GL comprises a metal complex (derived from Ti(OiPr) 4 The average GL thickness is determined by cutting through the support layer (i), measuring the thickness from the surface of the porous sheet outward by SEM at multiple locations, and calculating the average value.

[0197] Therefore, the porous support in Examples 1 and 3 to 8 and Comparative Examples C1, C3 and C4 is PAN-GL as shown in Table 6 below. Examples 2 and 9 and Comparative Example C2 use HI as the support layer and do not include GL.

[0198] Step ii.a) Formation of a discriminating layer (DL1) by plasma treatment (Examples 3 to 7 and Comparative Examples C3 and C4)

[0199] In Examples 3 to 7 and Comparative Examples C3 and C4, the discriminating layer DL1 was applied to the support shown in the second column of Table 6 using the atmospheric plasma apparatus described and used in FIG. 5 of EP1917842, and the carrier gas condition was set to an oxygen flow rate of 0.5 dm 3 (STP) / min, argon flow rate is 20dm 3(STP) / min, and then, as oxygen atom penetration treatment, 1.75J / cm 2 This resulted in DL1 with an average thickness of 60 nm.

[0200] The atomic % of M of the formula (1) of DL1 was determined by the above-mentioned method, and it was found that the atomic % of M was greater than 10.

[0201] Step ii.b) Preparation of discrimination layers DL2 and DL3 from compositions DLC2 and DLC3, respectively

[0202] Compositions DLC2 and DLC3 were prepared by mixing the ingredients shown in Table 5 below:

[0203] Table 5 - Compositions of DLC2 and DLC3

[0204] Ingredients (weight %) DLC2 DLC3 PI 1.00 0 CA 0 24.0 FOR 0 19.0 MAL 0 9.5 AC 0 47.5 APTMS 0.01 0 MIBK 3.00 0 DIOX 4.99 0 MEK 91.00 0

[0205] Compositions DLC2 and DLC3 were applied to the porous supports shown in the second column of Table 6 below, respectively, and the compositions were then cured to form discriminating layers DL2 and DL3.

[0206] For Example 2, Example 9 and Comparative Example C2, the composition DLC3 was coated on the HI support (excluding the groove layer) and dried by evaporating acetone for 18 seconds in a dry environment. Example 2, Example 9 and Comparative Example C2 were then immersed in cold water (about 2°C), washed with water at room temperature to remove any residual solvent and solvent exchanged (first with isopropanol and then with hexane). The hexane was then evaporated by dry air at 25°C to obtain a dry HI-D3 intermediate. The average total thickness of the composite membranes of Example 2, Example 9 and Comparative Example C2 was 2 μm.

[0207] For Examples 1 and 8 and Comparative Example C1, composition DLC2 was coated on the PAN-GL support prepared in step (i) by meniscus dip coating at a coating speed of 10 m / min to prepare a discriminating layer DL2 with a dry thickness of 100 nm (measured by SEM).

[0208] Step iii) Forming the additional layer (iii) of the invention of Examples 1 to 9

[0209] Samples of intermediate composite films comprising the supports and DLs shown in Examples 1 to 9 of the second and third columns were exposed to atmospheric pressure glow discharge (APG) plasma using the precursor HMDSO, respectively, independently. The apparatus used for exposure is described in EP1917842. The precursor mass flow rate supplied by the controlled evaporation unit was 1.0 g / hr HMDSO. The precursor vapor was diluted in an argon process carrier gas. The flow rate of the process gas was 20 dm 3(STP) / min. The applied plasma energy density was changed, wherein Example 5 was 0.2W / cm 2 , Examples 1 to 3 and Examples 6 to 9 are 0.4 W / cm 2 , Example 4 is 0.8W / cm 2 , thereby obtaining different additional layers (iii) with different average thicknesses / amounts of M of formula (1). The average thickness of the obtained additional layer (iii) depends on the exposure time: 5 seconds for Example 5, 13 seconds for Examples 1 to 3 and Examples 6 to 9, and 15 seconds for Example 4, and the average thickness of each gas separation membrane is confirmed by cutting through the GSM and measuring the average thickness of each layer using a scanning electron microscope. The atomic % of M of the group of formula (1) in the additional layer (iii) and (in Examples 7 to 9 and Comparative Examples C1 to C4) PL was determined, including two measurements at a depth of 10 nm and 20 nm, and the average value was determined, which is then included in Table 6.

[0210] Step iv). Forming the protective layer of Examples 7 to 9 and Comparative Examples C1 to C4

[0211] In Comparative Examples C1 to C4, the curable composition C having the formulation described above was applied to the composite of layers (i) and (ii) by meniscus dip coating at a coating speed of 10 m / min to obtain the PL shown in column 5 of Table 6. The coated intermediate film was then cured by irradiation with a Light Hammer LH10 from Fusion UV Systems equipped with a D bulb at an intensity of 24 kW / m. The average thickness of each protective layer in the comparative examples shown in column 5 of Table 6 measured by SEM was as follows: 2400 nm for C1 to C3 and 100 nm for C4.

[0212] Examples 7 to 9 (on top of the additional layer (iii) of the invention) contained a PL also prepared in a similar manner as described above for the PL in Comparative Examples C1 to C4 from a curable composition C. These protective layers also had an average thickness of 2400 nm as measured by SEM.

[0213] In addition, the permeability (in GPU) and selectivity (in CO) of all GSMs were determined using the methods described above. 2 / CH 4 ), and the results are shown in Table 6:

[0214] Table 6 – Summary of membrane structure and membrane properties

[0215]

[0216] By comparing the results in Table 6 for the GSM of the invention with the comparative GSM containing the same DL, it can be seen that the permeability of the GSM is high when the additional layer (iii) is present. Furthermore, as shown in Examples 7 to 9, the permeability remains high even when layer (iii) is coated with a PL.

Claims

1. A gas separation membrane comprising the following layers: (i) a support layer; (ii) discrimination layer; (iii) an additional layer, wherein The additional layer comprises a group of formula (1): M-(O-) x Formula (1) in, Each M is independently a metal or metalloid atom; O is an oxygen atom; and each value of x is independently at least 4; and (iv) an optional protective layer; in, (a) the support layer (i) and the additional layer (iii) are located on opposite sides of the discriminating layer (ii); and (b) The additional layer (iii) comprises 1.5 to 10 atomic % of M of the group of formula (1), wherein M is as defined above.

2. The gas separation membrane according to claim 1, wherein The additional layer (iii) has no gas separation selectivity and comprises 2 to 9 atom % of M of the group of formula (1).

3. The gas separation membrane according to claim 1 or 2, wherein: The discriminating layer (ii) comprises more than 10 atomic % and less than 50 atomic % of M groups of formula (1).

4. A gas separation membrane according to any one of the preceding claims, wherein The average thickness of the additional layer (iii) is from 1 nm to 1,500 nm.

5. A gas separation membrane according to any one of the preceding claims, wherein The average thickness of the additional layer (iii) is 5 nm to 1,000 nm.

6. A gas separation membrane according to any one of the preceding claims, wherein The average value of the atomic % of M of the group of formula (1) of the additional layer (iii) is substantially constant over its entire depth.

7. A gas separation membrane as claimed in any one of the preceding claims, comprising a polysiloxane protective layer (iv).

8. The gas separation membrane according to claim 7, wherein: The average thickness of the protective layer (iv) is 10 nm to 10,000 nm.

9. A method for forming a gas separation membrane as claimed in any one of the preceding claims, comprising the steps of: (a) applying the discriminating layer (ii) to the support layer (i) by a wet coating process, a physical vapor deposition process, a chemical vapor deposition process, an induced deposition process, an atomic layer deposition process or a plasma enhanced chemical deposition process; as well as (b) applying said additional layer (iii) to said discriminating layer (ii) (DL) by a plasma treatment process; and Optionally (c) applying a protective layer (iv) to the additional layer (iii).

10. The method of claim 9, wherein: Step (b) is carried out by a plasma treatment process in the presence of one or more of the following precursor compounds: tetraethyl orthosilicate, hexamethyldisiloxane, tetramethyl orthosilicate, 1,3,5,7-tetramethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, bis(triethoxysilyl)ethane, tetrapropyl orthotitanate, titanium ethoxide, titanium tetraisopropoxide or zirconium tetra-tert-butoxide.

11. The method according to claim 9 or 10, wherein: Step (b) is carried out in an atmosphere free of oxygen.

12. The method according to any one of claims 9 to 11, wherein: Step (a) comprises applying said discriminating layer (ii) to said support layer (i) by a plasma treatment process, and step (b) comprises applying said additional layer (iii) to said discriminating layer (ii) by a plasma treatment process.

13. The method of claim 12, wherein: Step (a) provides a discriminating layer (ii) having more than 10 atomic % and less than 50 atomic % of M groups of formula (1), and step (b) provides an additional layer (iii) having from 1.5 atomic % to 10 atomic % of M groups of formula (1). 14 . A gas separation module comprising the gas separation membrane according to claim 1 .

15. Use of the gas separation membrane according to any one of claims 1 to 8 or the gas separation module according to claim 14 for separating gases and / or for purifying feed gases.

Citation Information

Patent Citations

  • Gas separation membrane, method of producing gas separation membrane, gas separation membrane module, and gas separator

    US10427111B2

  • Aromatic polyimide, polyester and polyamide separation membranes

    US3899309A

  • Polyimide gas separation membranes

    US4717394A

  • Novel multicomponent fluid separation membranes

    US5085676A

  • Apparatus for producing and sustaining a glow discharge plasma under atmospheric conditions