Rapid heat treatment method and apparatus

By employing a rapid heat treatment method, the problem of low manufacturing efficiency in the mass production of solid-state lithium metal battery separators was solved, achieving efficient and stable separator production and improving lithium-ion conductivity and separator stability.

CN118946533APending Publication Date: 2024-11-12QUANTUMSPACE BATTERY INC
View PDF 30 Cites 0 Cited by

Patent Information

Application Number
CN202380021075.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies make it difficult to efficiently manufacture stable solid electrolyte separators for solid-state lithium metal batteries, especially in mass production, where the sintering process cannot guarantee efficient manufacturing and stability of the separators.

Method used

The rapid thermal sintering (RTP) method is used to sinter lithium-filled garnet and other materials at high temperature and in a short time. The heating element is kept at an appropriate distance from the material, and silicon carbide, molybdenum or carbon heating elements are used for rapid sintering. The atmosphere is controlled to ensure the stability and quality of the separator.

Benefits of technology

This technology enables efficient mass production of solid electrolyte separators, improving separator stability and ion conductivity while reducing production time and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946533A_ABST
    Figure CN118946533A_ABST
Patent Text Reader

Abstract

Separators for solid state lithium metal batteries are fabricated using rapid thermal treatment methods and apparatuses. Comprising high-temperature sintering. The temperature and time of heating, and the distance between the heating element and the material to be sintered together result in satisfactory physical properties, such as porosity, of the separator in the batch process.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 309,985, filed on February 14, 2022, entitled “RAPID THERMAL PROCESSING METHOD AND APPARATUS,” and to U.S. Provisional Patent Application No. 63 / 314,296, filed on February 25, 2022, entitled “RAPID THERMAL PROCESSING METHOD AND APPARATUS.” Both applications are hereby incorporated by reference in their entirety for all purposes. This application is also related to the following applications: International PCT Patent Application No. PCT / US2022 / 019641, filed on March 9, 2022, entitled “RAPID CERAMIC PROCESSING TECHNIQUES AND EQUIPMENT,” and U.S. Patent Application No. 17 / 905,822, filed on September 8, 2022, entitled “RAPID CERAMIC PROCESSING TECHNIQUES AND EQUIPMENT.” Both of these applications are also incorporated herein by reference in their entirety for all purposes. Technical Field

[0003] The present application relates to rechargeable batteries, in particular solid-state lithium metal batteries, and more specifically to a rapid thermal processing method and apparatus for manufacturing solid electrolytes for lithium metal batteries in a batch process, such as but not limited to lithium lanthanum titanate, lithium aluminum titanium phosphate (LATP), lithium aluminum germanium phosphate (LAGP) or lithium filled garnet oxide. In some examples, these ceramics are deposited in layers on top of a metal layer. These two layers constitute a double-layer structure. Background Art

[0004] Solid-state lithium metal batteries include an anode, a cathode, and a solid electrolyte separator. The solid electrolyte separator is able to conduct lithium ions between the anode and the cathode. There is a great need for separators that have this property and can be manufactured efficiently.

[0005] Prior art, such as U.S. Pat. No. 10,563,918 B2 or U.S. Pat. No. 10,840,544 B2, describes certain methods of sintering lithium-filled garnets (crystalline lithium lanthanum zirconium oxide or "LLZO"), such as batch sintering of LLZO. Some methods of high-throughput continuous sintering of ceramics are disclosed in U.S. Pat. No. 10,766,165 B2; and International PCT Patent Application Publication No. WO2017 / 003980 A1. SUMMARY OF THE INVENTION

[0007] The following description describes various aspects of methods and apparatus for manufacturing separators in solid-state lithium metal batteries using rapid thermal processing (RTP). In some aspects, these methods involve sintering materials at high temperatures for a short time to mass-produce separators. According to an embodiment, the temperature ranges from about 900°C to about 2000°C. According to an embodiment, the time period ranges from about 5 seconds to about 30 minutes. According to an embodiment, the heating element is about 1 mm to about 2000 mm away from the material to be sintered. According to an embodiment, the heating element is as close as possible to the material being sintered, because the surfaces of the heating element and the material being sintered allow one or two heating elements to not contact the material being sintered. According to an embodiment, the sintered material includes LATP, LAGP or LLZO. In some aspects, the device includes one or more heating elements that are close enough to the material to be sintered. According to an embodiment, the heating element may include different forms of silicon carbide, molybdenum or carbon.

[0008] Some embodiments relate to sintered products prepared according to the methods disclosed herein. Other embodiments relate to rechargeable batteries prepared according to the methods disclosed herein. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Figure 1 is a schematic diagram of an apparatus in one embodiment.

[0010] Figure 2 is a schematic diagram of an apparatus in one embodiment.

[0011] Figure 3 is a schematic diagram of an apparatus in one embodiment.

[0012] Figures 4A-4C Shown are films produced in different examples.

[0013] Figure 5 is a schematic diagram of an apparatus in one embodiment.

[0014] Figures 6A-6C Shown is a view of a structure in one embodiment for facilitating processing of a dual layer structure for passage through a rapid thermal processing apparatus.

[0015] Fig. 7A and 7B Shown are various views of a dual layer assembly through a rapid thermal processing apparatus in one embodiment.

[0016] Figure 8 is a schematic diagram of an apparatus in one embodiment.

[0017] Fig. 9 Shown are two films produced in one example.

[0018] Fig.10Cycling data for a bilayer cell including a film made according to the Examples is shown.

[0019] Fig.11 Cycling data for multilayer cells including thin films made according to the Examples are shown.

[0020] Fig.12 A thin film made according to one embodiment is shown.

[0021] Fig.13 A thin film made according to one embodiment is shown.

[0022] Fig.14 A cross section of a green film is shown in one embodiment before heat treatment.

[0023] Fig.15 Shows Fig.14 The cross section of the raw film after the heat treatment process described in this application.

[0024] Fig.16 An example of a thin film made according to one embodiment is shown.

[0025] Fig.17 An example of a thin film made according to one embodiment is shown.

[0026] Fig.18 An example of a thin film made according to one embodiment is shown.

[0027] Fig.19 An embodiment of a support plate stack disclosed in the present application is shown.

[0028] Detailed Description

[0029] The following description enables a person of ordinary skill to make and use the disclosed subject matter and to incorporate the subject matter into many applications. Various modifications and various uses in different applications are apparent to a person of ordinary skill. The general principles described in this application are applicable to a wide range of embodiments. Therefore, the application is not limited to the embodiments provided, but is given the broadest scope consistent with the principles and novel features disclosed in this application.

[0030] In the following detailed description, many specific details are listed to provide a deeper understanding of the disclosed structures and techniques. However, it is apparent that one of ordinary skill in the art can implement these disclosed structures and techniques without being limited to these specific details. In other cases, in order not to dilute the present application, well-known structures and devices will be shown in block diagram form rather than in detailed form.

[0031] definition

[0032] In the present application, when a number is limited, such as about 15% weight % (% w / w), the term "about" refers to the limited value, and may also include values ​​within the range of ± 10% of the value. For example, about 15% w / w includes 15% w / w and 13.5% w / w, 14% w / w, 14.5% w / w, 15.5% w / w, 16% w / w or 16.5% w / w. For example, "about 75 ° C " includes 75 ° C and 67 ° C, 68 ° C, 69 ° C, 70 ° C, 71 ° C, 72 ° C, 73 ° C, 74 ° C, 75 ° C, 76 ° C, 77 ° C, 78 ° C, 79 ° C, 80 ° C, 81 ° C, 82 ° C or 83 ° C.

[0033] In the present application, "selected from the group consisting of..." refers to a single member from the group, a plurality of members from the group, or a combination of members from the group. For example, the members selected from the group consisting of A, B, and C may include only A, only B, or only C, or may include A and B, A and C, B and C, or A, B, and C.

[0034] Unless otherwise specified, the term "electrochemical cell" or "battery cell" in this application refers to a single cell including a positive electrode and a negative electrode, which are ionically connected between the two through an electrolyte. In some embodiments, the battery or module includes multiple positive electrodes and / or multiple negative electrodes enclosed in a container, such as a stack of electrochemical cells. A stack of electrochemical cells may be referred to as a multi-layer cell. A symmetric cell is a cell with two lithium metal anodes separated by a solid electrolyte.

[0035] The term "electrochemical stack" in this application refers to one or more units, each of which includes at least a negative electrode (such as Li, LiC6), a positive electrode (such as FeF3, NiF x (where x is 2 or 3), nickel cobalt aluminum oxide (NCA), lithium iron phosphate (LFP), LiNi x Mn y Co z O2, [NMC] or LiNi x Al y Co z O2[NCA], wherein x+y+z=1, 0≤x≤1, 0≤y≤1 and 0≤z≤1, may be combined with a solid electrolyte or a gel electrolyte), and a solid electrolyte (e.g., an oxide electrolyte described in the present application, such as a lithium-filled garnet (e.g., Li7La3Zr2O) between and in contact with the positive electrode and the negative electrode 12)). In some examples, between the solid electrolyte and the positive electrode, there is an additional layer containing a flexible electrolyte (e.g., a gel electrolyte, a gel polymer electrolyte). The electrochemical stack may include one of the above-mentioned units. An electrochemical stack may include several of the above-mentioned units arranged in an electrically connected manner (e.g., electrically connected in series or in parallel). In some embodiments, when the electrochemical stack includes several units, the units are layered or laminated together in a column. In some embodiments, when the electrochemical stack includes several units, the units are layered or laminated in an array. In some examples, when the electrochemical stack includes several units, the stacks are arranged so that two or more positive electrodes share a negative electrode current collector. Alternatively, in some examples, when the electrochemical stack includes multiple units, the stacks are arranged so that two or more negative electrodes share a positive electrode current collector. Unless otherwise stated, the electrochemical stack includes a positive electrode current collector, a solid electrolyte, and a negative electrode, and may also include a bonding layer between the positive electrode and the solid electrolyte.

[0036] The term "positive electrode" in this application refers to the electrode in a secondary battery that releases positive ions such as Li during battery discharge. + Conduct, flow or move toward the electrode. The term "negative electrode" in this application refers to the electrode in a secondary battery that conducts, flows or moves positive ions such as Li during battery discharge. + Flow or move away from the electrode. In a battery consisting of a lithium metal electrode and a conversion chemical, an intercalation chemical, or a combination of conversion / intercalation chemicals, including an electrode (i.e., a cathode active material), the electrode with the conversion chemical, the intercalation chemical, or the combination of conversion / intercalation chemicals is called the positive electrode. In some uses, the cathode is used instead of the positive electrode and the anode is used instead of the negative electrode. When a lithium secondary battery is charged, lithium ions flow from the positive electrode (such as NiF x , NMC, NCA) to the negative electrode (such as Li-metal). When the lithium secondary battery is discharged, the lithium ions move from the negative electrode to the positive electrode.

[0037] The term "positive terminal" in this application refers to an electrical connection to the positive electrode. The positive terminal may also be referred to as a positive current collector.

[0038] The term "negative terminal" in this application refers to an electrical connection to the negative electrode. The negative terminal may also be referred to as a negative electrode current collector.

[0039] The term "cathode active material" in this application refers to a material that can intercalate lithium ions or react with lithium ions in a reversible manner. For example, LiMPO4 (M = Fe, Ni, Co, Mn); Li x Ti y O z , where x is 0 to 8, y is 1 to 12, and z is 1 to 24; LiMn 2a Nia O4, where a is 0 to 2; nickel cobalt aluminum oxide; LiNi x Mn y Co z O2, x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1; LiNi x Co y Al z O2, wherein x+y+z=1, 0≤x≤1, 0≤y≤1, 0≤z≤1. In these chemical formulas, x, y and z are selected so that the chemical formula is charge neutral.

[0040] The term "solid cathode" in this application refers to a cathode that does not include a liquid electrolyte. The terms "cathode" and "anode" in this application refer to the electrodes of a battery. The cathode and anode are usually referred to as positive and negative electrodes, respectively, in the relevant field.

[0041] The term "solid-state cathode electrolyte" or the term "cathode electrolyte" in this application refers to an ionic conductor that is intimately mixed with or surrounded by a cathode (ie, positive electrode) active material.

[0042] The term "electrolyte" in this application refers to an electrolyte that allows ions (such as Li + ) in which electrons migrate but do not allow electrons to conduct through them. For example, the ratio of ionic conductivity to electronic conductivity is at least 10 6 times. The electrolyte is used to insulate the cathode and anode of a secondary battery while allowing ions (such as Li + ) is transported through the electrolyte.

[0043] The term "solid electrolyte separator" in this application is used interchangeably with the term "solid separator" and refers to a conductive ion (e.g., Li +) but does not conduct electrons. A solid electrolyte separator is a solid material suitable for electrically isolating the positive and negative electrodes of a lithium secondary battery, while also providing a channel for lithium ion conduction. Examples of inorganic solid electrolytes include oxide electrolytes and sulfide electrolytes, which will be further described below. Non-limiting examples of sulfide electrolytes can be found, for example, in U.S. Patent No. 9,172,114, authorized on October 27, 2015, and U.S. Patent Application No. 2017-0162901A1, published on June 8, 2017. Non-limiting examples of oxide electrolytes are U.S. Patent Application No. 2015-0200420A1, published on July 16, 2015 (authorized on October 31, 2017, Patent No. 9806372). In some embodiments, the inorganic solid electrolyte also includes a polymer, which is referred to as a composite electrolyte. Composite electrolytes are shown, for example, in U.S. Patent No. 9,666,870. For various purposes, the entire contents of the above-mentioned U.S. patents and published U.S. patent applications are hereby incorporated by reference into this application as a whole.

[0044] The term "annealing" as used herein refers to heating a material in a reducing atmosphere, such as in dry air or argon, Ar / H2 and N2, for example, from 100°C to 1400°C, or for example, 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, 1350°C or 1450°C. Examples of some annealing methods can be found in U.S. Pat. No. 9,966,630 B2, which is incorporated herein by reference in its entirety for all purposes.

[0045] In some examples, the film is heated in an apparatus described herein or in a method described herein. In some embodiments, the film is heated to 1000°C. In some embodiments, the film is heated to 1010°C. In some embodiments, the film is heated to 1020°C. In some embodiments, the film is heated to 1030°C. In some embodiments, the film is heated to 1040°C. In some embodiments, the film is heated to 1050°C. In some embodiments, the film is heated to 1060°C. In some embodiments, the film is heated to 1070°C. In some embodiments, the film is heated to 1080°C. In some embodiments, the film is heated to 1090°C. In some embodiments, the film is heated to 1100°C. In some embodiments, the film is heated to 1110°C. In some embodiments, the film is heated to 1120°C. In some embodiments, the film is heated to 1130°C. In some embodiments, the film is heated to 1140°C. In some embodiments, the film is heated to 1150°C. In some embodiments, the film is heated to 1160°C. In some embodiments, the film is heated to 1170°C. In some embodiments, the film is heated to 1180°C. In some embodiments, the film is heated to 1190°C. In some embodiments, the film is heated to 1200°C. In some embodiments, the film is heated to 1210°C. In some embodiments, the film is heated to 1220°C. In some embodiments, the film is heated to 1230°C. In some embodiments, the film is heated to 1240°C. In some embodiments, the film is heated to 1250°C.

[0046] The terms "separator" and "conductive Li + ion separator" are used interchangeably; unless otherwise expressly stated, the separator is a Li-conducting + Abbreviation for ion separator.

[0047] Unless otherwise expressly stated, the separator used in the present application is stable when in contact with lithium metal. When the lithium metal and the separator material are in close contact and heated to at least 200°C in a differential scanning calorimeter, if there is no significant exothermic reaction, it is proved that the contact with the lithium metal is stable. In one embodiment, stability refers to kinetic stability, and the ASR is increased by about 100 or more by establishing a solid electrolyte interface (SEI). In one embodiment, stability refers to kinetic stability, and the ASR is increased by about 1000 or more by establishing SEI. In different embodiments, stability can be kinetic stability, by establishing SEI to increase the ASR in the range of about 100 to about 1000. In one embodiment, stability can be defined according to the initial ASR when in contact with lithium and the change in ASR after long-term contact with lithium. In one embodiment, long-term contact can be exposure to lithium for about 30 days at a temperature of about 60°C.

[0048] The term "thickness" or "film thickness" in this application refers to the distance between the top and bottom surfaces or surfaces, or the intermediate measured distance. The top and bottom surfaces or surfaces in this application refer to the side with the largest geometric surface area.

[0049] When defining a solid electrolyte, "thin" in this application means that the thickness dimension is less than 200 μm, sometimes less than 100 μm, in some cases between 0.1 and 60 μm, and in other cases about 10 nm to about 100 μm; in other cases, the thickness is about 1 μm, 10 μm, or 50 μm.

[0050] The term "lithium-filled garnet" in this application refers to an oxide having crystal structure characteristics related to the garnet crystal structure. For various purposes, U.S. Patent Application 2015 / 0099190 (filed on October 7, 2014, published on April 9, 2015, Serial No. 14 / 509,029) is incorporated herein by reference in its entirety. This application describes a lithium-filled garnet solid electrolyte for solid-state lithium rechargeable batteries.

[0051] Unless otherwise stated to the contrary, the lithium-filled garnet described in this application includes compounds having the formula Li A La B M′ C M″ D Zr E O F 、Li A La B M′ C M″ D Ta E O F or Li A La B M′ C M″ D Nb E O F where 4 < A < 8.5, 1.5 < B < 4, 0 ≤ C ≤ 2, 0 ≤ D ≤ 2, 0 ≤ E ≤ 2.5, 10 < F < 13, and in each instance M′ and M″ are selected from Al, Mo, W, Ga, Nb, Sb, Ca, Ba, Sr, Ce, Hf, Rb, Ta; or the formula Li a La b Zr c Al d Me″ e O f where 5 < a < 7.7, 2 < b < 4, 0 ≤ c ≤ 2., 0 ≤ d ≤ 2, 0 ≤ e ≤ 2, 10 < f < 13, and Me″ is a metal selected from Nb, Ta, V, W, Mo, Ga, or Sb.

[0052] The lithium-filled garnet can also be in accordance with the composition Li A La B M′ C M″ D Zr E O F 、Li A La B M′ C M″ D Ta E O F or Li A La B M′ C M″ D Nb E O F , where 4 < a < 8.5, 1.5 < B < 4, 0 ≤ C ≤ 2, 0 ≤ D ≤ 2, 0 ≤ E < 3, 10 < F < 13, and in each instance M′ and M″ are selected from Ga, Al, Mo, W, Nb, Sb, Ca, Ba, Sr, Ce, Hf, Rb, Ta respectively, or Li a La b Zr c Al d Me″ e O f , where 5 < a < 8.5, 2 < b < 4, 0 < c ≤ 2.5, 0 ≤ d < 2, 0 ≤ e < 2, 10 < f < 13, and Me″ is a metal selected from Ga, Nb, Ta, V, W, Mo or Sb; and as described in U.S. Patent Application No. 2015 / 0099190. The lithium-filled garnets and garnets in this application generally include but are not limited to: Li 7.0 La3(Zr t1 + Nb t2 + Ta t3 )O 12 + 0.35Al 12 O3; where (t1 + t2 + t3 = 2) such that La:(Zr / Nb / Ta) is 3:2. In addition, the garnets used in this application include but are not limited to Li x La3Zr2O F+yAl2O3, where x ranges from 5.5 to 9; y ranges from 0.05 to 1. In these examples, the subscripts x, y, and F are chosen so that the garnet is charge neutral. In some embodiments, x is 7 and y is 1.0. In some embodiments, x is 5 and y is 1.0. In some embodiments, x is 6 and y is 1.0. In some embodiments, x is 8 and y is 1.0. In some embodiments, x is 9 and y is 1.0. In some embodiments, x is 7 and y is 0.35. In some embodiments, x is 5 and y is 0.35. In some embodiments, x is 6 and y is 0.35. In some embodiments, x is 8 and y is 0.35. In some embodiments, x is 9 and y is 0.35. In some embodiments, x is 7 and y is 0.7. In some embodiments, x is 5 and y is 0.7. In some embodiments, x is 6 and y is 0.7. In some embodiments, x is 8 and y is 0.7. In some embodiments, x is 9 and y is 0.7. In some embodiments, x is 7 and y is 0.75. In some embodiments, x is 5 and y is 0.75. In some embodiments, x is 6 and y is 0.75. In some embodiments, x is 8 and y is 0.75. In some embodiments, x is 9 and y is 0.75. In some embodiments, x is 7 and y is 0.8. In some embodiments, x is 5 and y is 0.8. In some embodiments, x is 6 and y is 0.8. In some embodiments, x is 8 and y is 0.8. In some embodiments, x is 9 and y is 0.8. In some embodiments, x is 7 and y is 0.5. In some embodiments, x is 5 and y is 0.5. In some embodiments, x is 6 and y is 0.5. In some embodiments, x is 8 and y is 0.5. In some embodiments, x is 9 and y is 0.5. In some embodiments, x is 7 and y is 0.4. In some embodiments, x is 5 and y is 0.4. In some embodiments, x is 6 and y is 0.4. In some embodiments, x is 8 and y is 0.4. In some embodiments, x is 9 and y is 0.4. In some embodiments, x is 7 and y is 0.3. In some embodiments, x is 5 and y is 0.3. In some embodiments, x is 6 and y is 0.3. In some embodiments, x is 8 and y is 0.3. In some embodiments, x is 9 and y is 0.3. In some embodiments, x is 7 and y is 0.22. In some embodiments, x is 5 and y is 0.22. In some embodiments, x is 6 and y is 0.22. In some embodiments, x is 8 and y is 0.22. In some embodiments, x is 9 and y is 0.22. In addition, garnet in this application includes but is not limited to Li x La3Zr2O 12 +yAl2O3. In one embodiment, the lithium-filled garnet composition described in the present application meets the requirements of Li7Li3Zr2O 12In another embodiment, the lithium-filled garnet composition described in the present application meets the requirements of Li7Li3Zr2O 12 In another embodiment, the lithium-filled garnet composition described in the present application conforms to Li7Li3Zr2O 12 0.22Al2O3. In another embodiment, the lithium-filled garnet composition described in the present application meets the requirements of Li7Li3Zr2O 12 0.35Al2O3. In certain other embodiments, the lithium-filled garnet composition described in the present application conforms to Li7Li3Zr2O 12 0.5Al2O3. In another embodiment, the lithium-filled garnet composition described in the present application meets the requirements of Li7Li3Zr2O 12 0.75Al2O3.

[0053] Garnet in this application does not include YAG garnet (i.e. yttrium aluminum garnet or Y3Al5O 12 ). The garnet in the present application does not include garnets based on silicates, such as European garnet, almandine, iron garnet, sea garnet or cinnamon stone, sand feldspar, uvai and anthelite, as well as solvate-almandine-iron garnet and uvai-iron garnet-anthodite. The garnet in the present application does not include non-silicates with the general formula X3Y2(SiO4)3, wherein X is Ca, Mg, Fe and or Mn; Y is Al, Fe and / or Cr.

[0054] The term "green film" or "green tape" in this application refers to an unsintered tape or film, which includes lithium-filled garnet, a precursor of lithium-filled garnet, or a combination thereof, and at least one of a binder, a plasticizer, carbon, a dispersant, a solvent, or a combination thereof. "Green film tape" in this application refers to a roll of dry or not dry green film casting tape, a continuous layer, or a cut portion thereof. Green body can be used interchangeably with green film or green tape. Green tape can also include a green body patch (i.e., a metal layer patch coating) deposited on a metal layer.

[0055] "Atmosphere control" in this application refers to a system that controls moisture content, oxygen content, gas flow rate, gas temperature, gas content, gas concentration, total pressure, vacuum, and combinations thereof in a closed or confined space. The system reacts to the sensed conditions and changes the atmosphere so that the atmosphere is more consistent with certain predetermined conditions; in this sense, the atmosphere control is dynamic. In this case, the atmosphere refers to the gas environment in direct contact with the green tape being heated, calcined, sintered, or cooled; or the gas environment in direct contact with the sintered tape being heated, sintered, annealed, or cooled. In some examples described in this application, the atmosphere control includes controlling the flow rate of an inlet gas composed of any one of oxygen, argon, nitrogen, helium, and / or hydrogen. In some examples described in this application, the atmosphere control includes controlling the amount of water, oxygen, and lithium in a gaseous state in direct contact with the green tape being heated, calcined, sintered, or cooled, or with the sintered tape being heated, sintered, annealed, or cooled. Atmosphere control using various gas curtains, gas densities, gas flow rates, gas flow directions, or gas pulses in, around, and near ovens, furnaces, and any inlets or outlets, and any openings through which materials such as green tape or sintered articles enter or exit the oven or furnace. Atmosphere control can refer to systems that use nitrogen, argon, forming gas, dry air, or humidified air in an enclosed or confined space. Atmosphere control can refer to systems that impose a partial vacuum on the system, such as when the pressure is less than atmospheric pressure.

[0056] The term "sintered bilayer" in this application refers to a two-layer structure comprising a sintered solid electrolyte and a metal foil. The term "green bilayer" in this application refers to a two-layer structure comprising a green film and a metal foil.

[0057] "Gas curtain" in this application refers to the gas flow rate at certain inlets or outlets of the oven (such as the green tape inlet and the sintered film outlet) where the gas flow rate is set. For example, at standard pressure and temperature, the gas flow rate is between 1-50 liters / minute. For example, at standard pressure and temperature, the gas flow rate may be greater than 50 liters / minute. The gas curtain has a pressure sensor at the outlet. The gas curtain passes through the inlet or outlet of the oven to control the flow of gas in the oven. The gas curtain can help maintain a certain atmosphere in the oven by preventing some or all of the gas from leaving or entering the oven.

[0058] The term "dry air" in this application refers to air with low humidity. The clean room can be supplied with dry air. The dry air is characterized by a dew point of less than -20°C, less than -30°C, less than -40°C, less than -50°C, less than -60°C or less than -70°C.

[0059] Figure 1An overview of an RTP apparatus and associated methods according to an embodiment is shown. Heating elements 110 and 120 heat a material 130 placed between the elements at a desired temperature and time to produce a sintered element 140, which is used as a separator between the anode and cathode elements in a solid-state battery. The heating elements 110 and 120 are positioned so that they are at an appropriate distance from the material 130. In one embodiment, the material 130 is located on the heating element 120. In one embodiment, the material 130 is located on a support plate 135, which is in turn located on the heating element 120. In an embodiment, one heating element 110 / 120 can be omitted.

[0060] The area specific resistance (ASR) in this application is measured by electrochemical cycling using an Arbin or Biologic instrument, unless otherwise specified to the contrary.

[0061] The ionic conductivity in this application is measured by electrical impedance spectroscopy.

[0062] The term "ambient conditions" in this application refers to room temperature and natural atmosphere, such as the earth's atmosphere comprising about 78% N2 and 21% O2; and / or moisture is also present. Ambient conditions include standard temperature and pressure, and relative humidity is not less than 1%.

[0063] "Binder" in this application refers to a polymer with the ability to increase the adhesion and / or cohesion of a material, such as a solid in a raw tape. Suitable binders include, but are not limited to, PVDF, PVDF-HFP, SBR, and ethylene-olefin copolymers. "Binder" refers to a material that can help bond another material. For example, polyvinyl butyral in this application is a binder because it can be used to bond garnet materials. Other binders include polycarbonate. Other binders include polyacrylates and polymethacrylates. These binders are merely examples and are not the entire range of binders considered herein. Useful adhesives in the present application include, but are not limited to, polypropylene (PP), polyethylene, atactic polypropylene (aPP), isotactic polypropylene (iPP), ethylene-propylene rubber (EPR), ethylene-pentene copolymer (EPC), polyisobutylene (PIB), butadiene rubber (SBR), polyolefins, polyethylene-co-octene (PE-co-PO), polyethylene-co-methylene cyclopentane (PE-co-PMCP), polymethyl methacrylate (and other acrylic acids), acrylic acid, polyethylene-acetal resin, polyvinyl butyral resin, PVB, polyvinyl acetal resin, stereo block polypropylene, polypropylene polymethylpentene copolymer, polyethylene oxide (PEO), PEO block copolymer, silicone, etc. In some examples, including any of the above, the binder is a polymer selected from polyacrylonitrile (PAN), polypropylene, polyethylene, polyoxide (PEO), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyoxide poly(allyl glycidyl ester) PEO-AGE, polyoxide 2-methoxyethoxyethyl glycidyl ester (PEO-MEEGE), polyoxyethylene 2-methoxyethoxyethyl glycidyl ester poly(allyl glycidyl ether) (PEO-MEEGE-AGE), polysiloxane, polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), ethylene propylene (EPR), nitrile rubber (NPR), styrene butadiene rubber (SBR), polybutadiene polymer, polybutadiene rubber (PB), polyisobutadiene rubber (PIB), polyolefin, α-polyolefin, ethylene α-polyolefin, polyisobutadiene rubber (PI), polychloroprene rubber (CR), acrylonitrile butadiene rubber (NBR) and polyacrylate (PEA).

[0064] The term "cast film" in this application refers to the process of delivering or transferring a liquid or slurry to a mold or substrate so that the liquid or slurry is shaped or formed into a film. Casting can be accomplished by doctor knife, Meyer rod, comma coater, gravure coater, micro gravure, reverse comma coater, slot die, slide and / or belt casting, and other methods.

[0065] Figure 2An overview of an RTP device and related methods according to an embodiment is shown. Figure 1 As shown, the heating elements 110 and 120 heat the material 130 placed between the elements to form a sintered element 140. The controller 250 controls the heating elements 110 and 120 to heat the material 130 to a desired temperature. In some embodiments, the controller controls the furnace temperature to increase the furnace temperature to a desired temperature range at a rate of 300° C. per minute.

[0066] The controller 250 also controls a conveyor, which includes rollers 270, 275 and a conveyor belt 280, to convey the material 130 on the conveyor belt 280 between the heating elements 110 and 120. The controller 250 further controls the conveyor to keep the material 130 between the heating elements 110 and 120 for a desired time. In one embodiment, the conveyor belt 280 is located on the heating element 120. In one embodiment, the material 130 is located on the conveyor belt 280. In one embodiment, the material 130 is located on the support plate 135, which is in turn located on the conveyor belt 280. In an embodiment, one heating element 110 / 120 can be omitted.

[0067] According to an embodiment, the heating elements 110 and 120 may be carbon plates or carbon paper. In some instances, the carbon plates or carbon paper contain conductive carbon. According to an embodiment, the heating elements 110 and 120 may be molybdenum plates or molybdenum paper. In some instances, the molybdenum plates or molybdenum paper may contain conductive molybdenum. Applying an electric current heats the conductive carbon plate or conductive carbon paper element at an appropriate rate to promote sintering within the temperature range described in the present application.

[0068] In an embodiment, the heating element is 1 mm to 2000 mm away from the material being sintered. In an embodiment, the heating element is 1 mm to 200 mm away from the material being sintered. In an embodiment, the heating element is as close as 1 mm to 10 mm away from the material being sintered. According to an embodiment, the distance between the heating element and the material being sintered can be measured in a variety of ways based on the position of the material relative to the heating element as the material passes along the conveyor.

[0069] In an embodiment, the sintering temperature ranges from 900°C to 1200°C. In an embodiment, the sintering temperature ranges from 950°C to 1150°C. In an embodiment, the sintering temperature ranges from 1000°C to 1100°C. In an embodiment, the sintering temperature ranges from 1000°C to 1300°C. In an embodiment, the sintering temperature ranges from 1050°C to 1250°C. In an embodiment, the sintering temperature ranges from 1100°C to 1200°C.

[0070] In one embodiment, the time period of heating is from 5 seconds to 30 minutes. In one embodiment, the time period ranges from 5 seconds to 25 minutes. In one embodiment, the time period ranges from 5 seconds to 20 minutes. In one embodiment, the time period ranges from 5 seconds to 15 minutes. In one embodiment, the time period ranges from 5 seconds to 10 minutes. In one embodiment, the time period ranges from 5 seconds to 5 minutes. In one embodiment, the time period ranges from 5 seconds to 4 minutes. In one embodiment, the time period ranges from 5 seconds to 3 minutes. In one embodiment, the time period ranges from 5 seconds to 4 minutes. In one embodiment, the time period ranges from 5 seconds to 1 minute.

[0071] In some examples, the heating elements 110 and 120 have the same area as the material 130. In some examples, the heating elements 110 and 120 are longer than the material 130 and as wide as the material 130. In some examples, the heating elements 110 and 120 are the same length as the material 130 and wider than the material 130. In some examples, the heating elements 110 and 120 are shorter than the material 130. In embodiments with a single heating element, the heating element can have any of the above-described planar relationships with the material 130.

[0072] In some embodiments, the material 130 has a length of about 50 mm to about 300 mm and a width of about 50 mm to about 300 mm. In some embodiments, the material 130 has a length of about 50 mm to about 150 mm and a width of about 50 mm to about 150 mm. In some embodiments, the length of the material 130 is between about 60 mm and about 120 mm and the width is between about 60 mm and about 120 mm. In a specific embodiment, the material 130 is 64 mm×79 mm after sintering. In a specific example, the material 130 is about 64 mm×about 80 mm after sintering. In a specific example, the material 130 is about 64 mm×about 85 mm after sintering. In a specific example, the material 130 is about 65 mm×about 80 mm after sintering. In a specific example, the material 130 is about 65 mm×about 85 mm after sintering. In a specific example, the material 130 is about 75 mm×about 90 mm after sintering. In a specific example, the material 130 is about 110 mm x about 110 mm after sintering. In a specific example, the material 130 is about 115 mm x about 115 mm after sintering. In a specific example, the material is about 110 mm x about 115 mm after sintering.

[0073] In some examples, when the green film on the metal foil undergoes a sintering process to become a sintered material, the material becomes dense and its size is reduced. As described in this application, the x and y directions are along the width and length of the green film, and the z direction is along the height of the green film.

[0074] In some cases, the material shrinks primarily in the z-direction. In some cases, the height of the double-layer green film is reduced by at least 30%, 40%, 50%, or 60%. In some cases, the height of the double-layer green film is reduced by about 40%, 45%, or 50%.

[0075] The thickness of the green bilayer can be measured using a drop gauge or FIB sections imaged using a SEM.

[0076] The thickness of the sintered bilayer can be measured by FIB cutting, SEM imaging, ion milling cross-sectioning or double-sided inverse laser interferometry.

[0077] In an embodiment, the sintering process is performed under a reducing or inert gas atmosphere. The inert atmosphere includes argon (Ar) or nitrogen (N2). The reducing atmosphere may include Ar mixed with hydrogen (H2) or N2 mixed with H2.

[0078] In one embodiment, an oxidant is mixed in the gas or atmosphere in contact with the green tape during sintering. These oxidants include H2O, O2 or clean dry air. In some examples, the sintering furnace does not include an oxidant mixed in the gas or atmosphere in contact with the sintered film.

[0079] The oxygen or O2 level in the gas during the process described herein is less than about 100 ppm, 50 ppm or 10 ppm. The water or H2O level in the gas during the process described herein is less than about 100 ppm, 50 ppm or 10 ppm.

[0080] In some embodiments, the sintering process includes using argon gas.

[0081] In some embodiments, the sintering process includes using nitrogen (N2) gas.

[0082] In some embodiments, the sintering process includes using hydrogen gas. In some embodiments, the concentration of the H2 gas is about 5% v / v.

[0083] In some embodiments, the sintering process includes using water (H2O) gas.

[0084] In an embodiment, the atmosphere in the device is uniform or substantially uniform. The atmosphere of the inert gas or gas mixture is uniform throughout the device, or at least uniform above and / or below the material to be sintered. In an embodiment, the temperature in the device is uniform or substantially uniform. The temperature of the inert gas or gas mixture is uniform throughout the device, or at least uniform above and / or below the material to be sintered.

[0085] In some examples, the process includes using atmosphere control with a narrow oven opening around the material being sintered.

[0086] In some examples, using atmosphere control includes using excess flow at the oven inlet and outlet. In some embodiments, using atmosphere control includes using a N2 or Ar filled glove box around various components (such as drums). In some embodiments, using atmosphere control includes using overpressure in the oven.

[0087] In some embodiments, atmosphere pressure control of the atmosphere inside the tool is used. In some cases, a partial vacuum may be used, where the pressure is about 0.01 Torr, 0.1 Torr, or 0.5 Torr. In some cases, the gas flow may be reintroduced into the vacuum system.

[0088] In some embodiments, using atmosphere control includes controlling the amount of H2O in the heating device. In some embodiments, using atmosphere control includes controlling the amount of oxygen in the heating device. In some embodiments, using atmosphere control includes controlling the amount of O2 in the heating device to less than 100 ppm. In some embodiments, using atmosphere control includes controlling the amount of O2 in the heating device to a level below 10 ppm. In some embodiments, using atmosphere control includes controlling the amount of O2 in the heating device to a level below 1 ppm. In some embodiments, using atmosphere control includes controlling the amount of H2 in the heating device. In some embodiments, using atmosphere control includes controlling the amount of N2 in the heating device.

[0089] In some embodiments, using atmosphere control includes controlling the amount of H2O in the heating device. In some embodiments, using atmosphere control includes controlling the amount of H2O in the heating device to less than 100 ppm. In some embodiments, using atmosphere control includes controlling the amount of H2O in the heating device to less than 10 ppm.

[0090] In some embodiments, using atmosphere control includes using forming gas in a heating device. In some examples, the forming gas is a mixture of hydrogen (H2) and Ar. In some examples, using atmosphere control includes using forming gas in a heating device. In some cases, the forming gas is a mixture of hydrogen (H2) and nitrogen (N2). In some embodiments, using atmosphere control includes using forming gas in a heating device. In some cases, the forming gas is a mixture of H2, Ar and N2. In these examples, the volume of H2 accounts for only a few percent of the forming gas. For example, in some cases, H2 is present in the forming gas at a volume of 1%, 2%, 3%, 4%, 6%, 7%, 8%, 9% or 10%. In some other instances, H2 is present in the forming gas at a volume of about 1%, about 2%, about 3%, about 4%, about 6%, about 7%, about 8%, about 9% or about 10%. In certain other examples, H2 is present in the synthesis gas at about 1-2%, about 2-3%, about 3-4%, about 4-5%, about 6-7%, about 7-8%, about 8-9%, or about 9-10%. In other examples, H2 is present in the synthesis gas at 1-2%, 2-3%, 3-4%, 4-5%, 6-7%, 7-8%, 8-9%, or 9-10%. In other examples, H2 is present in the synthesis gas at 1-5%, 2-5%, 3-5%, 5-9%, 5-7%, 4-6%, 3-7%, or 2-8%.

[0091] In other examples, using atmosphere control includes using Ar gas, N2 gas or a combination thereof in the heating device. In some examples, the gas is Ar, and in other examples, the gas is N2. In other examples, the gas is a mixture of Ar and N2.

[0092] In some examples, in certain parts of the production line, such as parts of the production line where sintering is not performed, the use of atmosphere control includes the use of oxidizing gases. For example, H2O can be used alone or in combination with the gases in the previous sections. For example, O2 can be used alone or in combination with the gases in the previous sections. For example, CDA (clean dry air) can be used alone or in combination with the gases in the previous sections.

[0093] In some examples, using atmosphere control includes using an enclosure to provide a closed environment with atmosphere control around or near the heating device, such as a closed environment filled with nitrogen, with some areas exposed to a reducing environment. The reducing environment can be achieved by providing a partial pressure of H2 or CO.

[0094] In some embodiments, the green tape is subjected to rapid sintering. The time at a temperature above room temperature for any given portion of the film can vary from 30 minutes to 10 hours. The time at a temperature above room temperature for any given portion of the film can be 30 minutes to 5 hours. The time spent at a temperature above room temperature for any given portion of the film can be 1 hour to 5 hours. The time spent at a temperature above room temperature for any given portion of the film can be 2 hours to 4 hours.

[0095] In some embodiments, the green tape is subjected to rapid sintering. The time at the sintering temperature for any given portion of the film may be between 15 seconds and 20 minutes. In other examples, the time at the sintering temperature for any given portion of the film may be between 1 minute and 10 minutes. In other examples, the time at the sintering temperature for any given portion of the film may be between 1 minute and 5 minutes. In other examples, the time at the sintering temperature for any given portion of the film may be between 1 minute and 2 minutes.

[0096] To avoid surface contamination of the sintered or pre-sintered parts as they pass through the continuous production line (CML), the film can be cooled to below 40°C. In some embodiments, the film is maintained in an atmosphere with a low water content. For example, the water content is less than 10 ppm. In some embodiments, the film is maintained in an atmosphere consisting primarily of argon. In some embodiments, the film is maintained in an atmosphere consisting primarily of nitrogen. In some embodiments, the film is maintained in clean dry air (CDA).

[0097] In some examples, an air box (tunnel structure) is used in conjunction with an exhaust port.

[0098] In some examples, an air box with a feedback loop is used in the heating device, forming the intake duct and O2 sensor.

[0099] In some embodiments, the material to be sintered is subjected to a binder burnout (BBO) prior to sintering. During the BBO process, organic matter in the material evaporates or burns off from the material to be sintered. During the BBO process, the atmosphere in contact with the material to be sintered may be oxidizing. In some cases, the BBO atmosphere is not oxidizing and organic matter evaporates from the material to be sintered. The BBO step occurs before the sintering step.

[0100] Figure 3 An overview of an RTP apparatus and related methods according to an embodiment is shown. Figure 3The apparatus in the embodiment uses a heating lamp 300 to sinter the material 130. In an embodiment, the lamp 300 is a halogen lamp. The heat from the heating lamp 300 passes through a container 310 that supports the material 130. In an embodiment, the container acts as a susceptor. In an embodiment, the material is placed on a support plate 315. In an embodiment, the support plate can be omitted. In an embodiment, the support plate 315 can act as a susceptor.

[0101] Non-limiting examples of support plates can be found in WO2016168723A1 and WO2016168691A1, both published on October 20, 2016; and U.S. Patent No. 10563918, granted on February 18, 2020. The above patent applications and patents are incorporated by reference in their entirety into this application for all purposes.

[0102] As described in the present application, the method of sintering the material can be by a heating method, tool or device based on a carbon plate. As described in the present application, the method of sintering the material can be by a heating method, tool or device based on a lamp.

[0103] In an embodiment, the cover 320 fits over the opening 330. The solid arrow 340 shows faster heat transfer. The dashed arrow 350 indicates slower heat transfer. Depending on the embodiment, more than 50% of incident light in the wavelength range of 300-700nm, the wavelength range of 800-2500nm, the wavelength range of 2.5-1000μm, or the wavelength range of 100-400nm can pass through the cover. In an embodiment, the gas is caused to flow through the inner surface of the cover 320 by controlling the device. In an embodiment, the cover 320 can be omitted, especially if the stack including the material 130 and the support plate 315 is relatively thick relative to the height of the opening 330. In an embodiment, the material 130 is sintered to form a Figure 1 and 2 The sintered element 140 is shown. As previously mentioned, the sintered element 140 can be used as a separator in a solid-state battery. In an embodiment, the separator is a solid electrolyte. In an embodiment, the separator includes lithium-filled garnet.

[0104] Figure 5 The apparatus for rapid thermal processing in the embodiment is shown. Figure 5 In FIG. 1 , a controller 250 controls a conveyor 290 that includes a plurality of rollers 295 and a plurality of heating elements 110, each of which is located in a separate zone 150 of the device according to the different embodiments shown. Figure 5In the embodiment, the material 130 is placed on the support plate 135. In various embodiments, the material 130 may include the lithium-filled garnet discussed above. In various embodiments, the support plate 135 may include a foil of the type discussed above, such that the material 130 and the support plate 135 together form a double-layer structure, which is formed by Figure 5 An apparatus is provided to produce a sintered material 140 as shown.

[0105] According to an embodiment, there may be Figure 5 More than three zones 150 are shown. Depending on the embodiment, there may be from 1 to 50 such zones. One or more central zones in the apparatus may sinter the material 130, the zones before that may heat the material before sintering, and the zones after that may cool the material after sintering. Depending on the embodiment, the atmosphere in each zone may be wet or dry.

[0106] According to embodiments, the conveyor 290 can be a long continuous conveying mechanism in which the rollers 295 run along a straight path. According to embodiments, the rollers 295 can be arranged in a square, rectangular, other polygonal configurations, and an elliptical or circular path. In the latter embodiment, the conveyor describes a continuous path in which materials can be placed and removed from the conveyor at adjacent points rather than at separate starting and ending points.

[0107] According to an embodiment, the controller 250 may control the zones 150 individually to define a desired temperature profile for heating and cooling the material 130 and sintering the material 140. In one embodiment, one or more central zones 150 may sinter the material 130 at a temperature range of 900°C to 2000°C. In an embodiment, the temperature range may be 1000°C to 1900°C. In an embodiment, the temperature range may be 1100°C to 1800°C. In an embodiment, the temperature range may be 1200°C to 1700°C. In an embodiment, the temperature range may be 1000°C to 1700°C. In an embodiment, the temperature range may be 1100°C to 1600°C. In an embodiment, the temperature range may be 1200°C to 1500°C. In an embodiment, the temperature range may be 1000°C to 1400°C. In an embodiment, the temperature range may be 1100°C to 1300°C. In an embodiment, the temperature range may be 1000°C to 1200°C.

[0108] Depending on the embodiment, the temperature profile just discussed may heat the material 130 at any desired rate before the material 130 reaches the zone 150 where sintering is performed. In different embodiments, the rate may vary between 10°C / min and 250°C / min. In different embodiments, the rate may vary between 20°C / min and 200°C / min. In different embodiments, the rate may vary between 25°C / min and 150°C / min. In different embodiments, the rate may vary between 30°C / min and 100°C / min. In different embodiments, the rate may vary between 10°C / min and 50°C / min. In different embodiments, the rate may vary between 15°C / min and 45°C / min. In different embodiments, the rate may vary between 20°C / min and 40°C / min. In different embodiments, the rate may vary between 10°C / min and 40°C / min. In different embodiments, the rate may vary between 15°C / min and 35°C / min. In different embodiments, the rate may vary between 20°C / min and 30°C / min.

[0109] Although some figures of the present application show a double-layer structure being conveyed through a furnace, in embodiments there are additional structures surrounding the double-layer structure. Some of these additional structures may be referred to as accessories. In embodiments, there is one accessory located below the double-layer structure and another accessory located above the double-layer structure. In various embodiments, these accessories are planar or plate-like, with a length and width greater than the length and width of the double-layer structure sandwiched between them.

[0110] According to an embodiment, the material of the accessory used to convey the bi-layer structure through the series of furnace zones can be selected from the group consisting of alumina (Al2O3), zirconium toughened alumina (ZTA), mullite (3Al2O32SiO2 or 2Al2O3SiO2), aluminum nitride (AlN) or silicon carbide (SiC). In one embodiment, the part of the accessory above the bi-layer structure can be made of one of the above materials, while the part of the accessory located between the conveyor and the bi-layer structure is made of another material. For example, if the accessory is made of alumina, one piece may be made of printed alumina and the other piece may be made of dense alumina.

[0111] In some embodiments, a frame is provided between the upper fitting and the double-layer structure so that the membrane is not in contact with the upper fitting. According to an embodiment, the material of the frame provided between the fitting and the foil may be selected from the group consisting of porous alumina, alumina-zirconia mixture, lithium aluminate, lithium tantalate, alumina, silica, silicates such as cordierite, Ni, iron alloys, nickel alloys, cobalt alloys, iron-nickel-cobalt alloys or combinations thereof. In one embodiment, the frame material may be textured on one or both sides. The texture may reduce the contact area between the frame and the foil, allowing for a larger BBO path. In one embodiment, the texture comprises vertical grooves on the frame. In one embodiment, the texture comprises horizontal grooves on the frame. In another embodiment, the texture comprises horizontal and vertical grooves on the frame. In an embodiment, the grooves may be arranged repetitively (i.e., arranged equidistant from each other). In one embodiment, the material is textured on one side, the texture facing the material.

[0112] Fig. 6A and 6B The top and bottom views of the frame structure according to different embodiments are shown respectively. Fig. 6A In the embodiment, the frame structure 600 includes a frame 610 having an opening 620. An accessory 630 extends below the frame 610. The frame 610 is inserted between the upper accessory and the double-layer structure so that the central part of the material in the double-layer structure does not contact the accessory part. When the double-layer structure is assembled in the accessory for sintering, the accessory 630 contacts the double-layer structure to prevent the frame 610 from contacting the double-layer structure. Figure 6B A top view of the frame structure 600 is shown, wherein the attachment 630 is indicated by dashed lines on the bottom side of the frame 610 . Figure 6C Frame 610 is shown on material 130 .

[0113] like Fig. 7A and 7B As shown, according to various embodiments, structure 700 is placed into a furnace. Fig. 7A For the decomposition diagram, Figure 7B 1 and 13 are assembled diagrams. In these diagrams, the double-layer structure including the material 130 and the foil 135 is placed on the lower accessory plate 720. The frame structure 600 is placed on the double-layer structure. The upper accessory plate 710 is placed on the frame structure 600. In the description of various embodiments of the present application, the upper and lower accessory plates 710 and 720 may be collectively referred to as accessories.

[0114] Figure 8 Shows the Figure 5 The corresponding structure of part of Fig. 7A and 7B The structure 700 is shown passing through a furnace to produce a sintered material 140 .

[0115] During sintering, the bilayer can be oriented in two ways relative to the ground: green film on top, metal foil on bottom, or metal foil on top, green film on bottom. The examples described in this application place the metal foil on the bottom to minimize interaction with the support plate or bracket, and the green film on the top to facilitate the binder to leave the film during binder burnout heating.

[0116] According to an embodiment, the accessory has a size range between 50*50mm and 200*200mm. The size of the accessory can be up to 300*300mm. The accessory does not have to be square. In one embodiment, the width of the accessory is about 50mm. In one embodiment, the width of the accessory is about 60mm. In one embodiment, the width of the accessory is about 70mm. In one embodiment, the width of the accessory is about 80mm. In one embodiment, the width of the accessory is about 90mm. In one embodiment, the width of the accessory is about 100mm. In one embodiment, the width of the accessory may be about 110mm. In one embodiment, the width of the accessory may be about 120mm. In one embodiment, the width of the accessory may be about 130mm. In one embodiment, the width of the accessory may be about 140mm. In one embodiment, the width of the accessory may be about 150mm. In one embodiment, the width of the accessory may be about 160mm. In one embodiment, the width of the accessory may be about 170mm. In one embodiment, the width of the accessory may be about 180mm. In one embodiment, the width of the accessory may be about 190mm. In one embodiment, the width of the fitting is about 200 mm. The width of the fitting may also be in increments of less than 10 mm, depending on the embodiment.

[0117] In an embodiment, the length of the accessory is about 50 mm. In an embodiment, the length of the accessory is about 60 mm. In an embodiment, the length of the accessory is about 70 mm. In an embodiment, the length of the accessory is about 80 mm. In an embodiment, the length of the accessory is about 90 mm. In an embodiment, the length of the accessory is about 100 mm. In an embodiment, the length of the accessory is about 110 mm. In an embodiment, the length of the accessory is about 120 mm. In an embodiment, the length of the accessory is about 130 mm. In an embodiment, the length of the accessory is about 140 mm. In an embodiment, the length of the accessory is about 150 mm. In an embodiment, the length of the accessory is about 160 mm. In an embodiment, the length of the accessory is about 170 mm. In an embodiment, the length of the accessory is about 180 mm. In an embodiment, the length of the accessory is about 190 mm. In an embodiment, the length of the accessory is about 200 mm. The length of the accessory may be increased or decreased within 10 mm, depending on the embodiment.

[0118] According to an embodiment, the foil has a size range between about 40*40mm and about 190*190mm. The fitting does not have to be square. In one embodiment, the width of the fitting is about 40mm. In one embodiment, the width of the fitting is about 50mm. In one embodiment, the width of the fitting is about 60mm. In one embodiment, the width of the fitting is about 70mm. In one embodiment, the width of the fitting is about 80mm. In one embodiment, the width of the fitting is about 90mm. In one embodiment, the width of the fitting is about 100mm. In one embodiment, the width of the fitting is about 110mm. In one embodiment, the width of the fitting is about 120mm. In one embodiment, the width of the fitting is about 130mm. In one embodiment, the width of the fitting is about 140mm. In one embodiment, the width of the fitting is about 150mm. In one embodiment, the width of the fitting is about 160mm. In one embodiment, the width of the fitting is about 170mm. In one embodiment, the width of the fitting is about 180mm. In one embodiment, the width of the fitting is about 190mm. The width of the fitting may be increased or decreased by 10 mm, depending on the embodiment.

[0119] In an embodiment, the length of the foil is greater than about 50 mm. In one embodiment, the length of the foil is about 60 mm. In one embodiment, the length of the foil is about 70 mm. In one embodiment, the length of the foil is about 80 mm. In one embodiment, the length of the foil is about 90 mm. In one embodiment, the length of the foil is about 100 mm. In one embodiment, the length of the foil is about 110 mm. In one embodiment, the length of the foil is about 120 mm. In one embodiment, the length of the foil is about 130 mm. In one embodiment, the length of the foil is about 140 mm. In one embodiment, the length of the foil is about 150 mm. In one embodiment, the length of the foil is about 160 mm. In one embodiment, the length of the foil is about 170 mm. In one embodiment, the length of the foil is about 180 mm. In one embodiment, the length of the foil is about 190 mm. In general, depending on the embodiment, the length of the foil can be between 40 mm and 190 mm. In general, the foil is a single piece of metal foil, rather than a ribbon that is significantly longer than it is wide.

[0120] Another way to compare the size of the foil to the size of the accessory is to compare the distance on each side between the perimeter of the foil and the perimeter of the accessory. In one embodiment, the distance on each side between the foil and the accessory is about 5mm. In one embodiment, the distance on each side between the foil and the accessory is about 6mm. In one embodiment, the distance on each side between the foil and the accessory is about 7mm. In one embodiment, the distance on each side between the foil and the accessory is about 8mm. In one embodiment, the distance on each side between the foil and the accessory is about 9mm. In one embodiment, the distance on each side between the foil and the accessory may be about 10mm. In one embodiment, the distance on each side between the foil and the accessory is about 11mm. In one embodiment, the distance on each side between the foil and the accessory is about 12mm. In one embodiment, the distance on each side between the foil and the accessory is about 13mm. In one embodiment, the distance on each side between the foil and the accessory is about 14mm. In one embodiment, the distance on each side between the foil and the accessory is about 15mm. In one embodiment, the distance on each side between the foil and the accessory may be about 16mm. In one embodiment, the distance on each side between the foil and the accessory is about 17mm. In one embodiment, the distance between the foil and the accessory is about 18 mm on each side. In one embodiment, the distance between the foil and the accessory may be about 19 mm on each side. In one embodiment, the distance between the foil and the accessory may be about 20 mm on each side.

[0121] In an embodiment, the outer dimensions of the frame may be the same as the dimensions of the foil. The width of each side of the frame may be different based on the degree of separation required for proper separation from the upper portion of the accessory. In one embodiment, the width of each side of the frame is about 1 mm. In one embodiment, the width of each side of the frame is about 1.5 mm. In one embodiment, the width of each side of the frame is about 2 mm. In one embodiment, the width of each side of the frame is about 2.5 mm. In one embodiment, the width of each side of the frame is about 3 mm. In one embodiment, the width of each side of the frame is about 3.5 mm. In one embodiment, the width of each side of the frame is about 4 mm. In one embodiment, the width of each side of the frame is about 4.5 mm. In one embodiment, the width of each side of the frame is about 5 mm. In one embodiment, the width of each side of the frame is about 5.5 mm. In one embodiment, the width of each side of the frame is about 6 mm.

[0122] In some examples, including any of the above, the solid electrolyte is rectangular in shape, with two surfaces, namely the top and bottom surfaces, which have the largest geometric surface area. As used in this application, assuming that the surface is flat, the surface area considered is the length multiplied by the width. At about 90° angles to the upper and lower surfaces are four edge surfaces, each of which has a geometric surface area less than the geometric surface area of ​​the upper and lower surfaces. In these examples, two of the four edge surfaces have a smaller geometric surface area than the other two surfaces.

[0123] In some examples, including any of the above, the solid electrolyte is square in shape, with two surfaces, top and bottom surfaces, having the largest geometric surface areas. At about 90° angles to the upper and lower surfaces are four edge surfaces, each of which has a geometric surface area less than the geometric surface area of ​​the upper and lower surfaces. In these examples, the four edge surfaces have approximately equal surface areas.

[0124] In some examples, including any of the above, the thickness of the green double layer is 1 μm to 100 μm. In some embodiments, the thickness of the green double layer is 20 μm to 100 μm. In some embodiments, the thickness of the green double layer is 40 μm to 100 μm. In some embodiments, the thickness of the green double layer is 20 μm to 80 μm. In some embodiments, the thickness of the green double layer is 40 μm to 80 μm. In some embodiments, the thickness of the green double layer is 20 μm to 60 μm. In some embodiments, the thickness of the green double layer is 10 μm to 50 μm. In some embodiments, the thickness of the green double layer is 10 μm-40 μm. In some embodiments, the thickness of the green double layer is 10 μm-30 μm. In some embodiments, the thickness of the green double layer is about 10 μm. In some embodiments, the thickness of the green double layer is about 11 μm. In some embodiments, the thickness of the green double layer is about 12 μm. In some embodiments, the thickness of the green double layer is about 13 μm. In some embodiments, the thickness of the green double layer is about 14 μm. In some embodiments, the thickness of the green bilayer is about 15 μm. In some embodiments, the thickness of the green bilayer is about 16 μm. In some embodiments, the thickness of the green bilayer is about 17 μm. In some embodiments, the thickness of the green bilayer is about 18 μm. In some embodiments, the thickness of the green bilayer is about 19 μm. In some embodiments, the thickness of the green bilayer is about 20 μm. In some embodiments, the thickness of the green bilayer is about 21 μm. In some embodiments, the thickness of the green bilayer is about 22 μm. In some embodiments, the thickness of the green bilayer is about 23 μm. In some embodiments, the thickness of the green bilayer is about 24 μm. In some embodiments, the thickness of the green bilayer is about 25 μm. In some embodiments, the thickness of the green bilayer is about 26 μm. In some embodiments, the thickness of the green bilayer is about 27 μm. In some embodiments, the thickness of the green bilayer is about 28 μm. In some embodiments, the thickness of the green bilayer is about 29 μm. In some embodiments, the thickness of the green bilayer is about 30 μm. In some embodiments, the thickness of the green bilayer is about 31 μm. In some embodiments, the thickness of the green bilayer is about 32 μm. In some embodiments, the thickness of the green bilayer is about 33 μm. In some embodiments, the thickness of the green bilayer is about 34 μm. In some embodiments, the thickness of the green bilayer is about 35 μm. In some embodiments, the thickness of the green bilayer is about 36 μm. In some embodiments, the thickness of the green bilayer is about 37 μm. In some embodiments, the thickness of the green bilayer is about 38 μm. In some embodiments, the thickness of the green bilayer is about 39 μm. In some embodiments, the thickness of the green bilayer is about 40 μm.

[0125] In some examples, including any of the above, the thickness of the bilayer after sintering is 1 μm-100 μm. In some embodiments, the thickness of the bilayer after sintering is 20 μm to 100 μm. In some embodiments, the thickness of the bilayer after sintering is 40 μm to 100 μm. In some embodiments, the thickness of the bilayer after sintering is 20 μm to 80 μm. In some embodiments, the thickness of the bilayer after sintering is 40 μm to 80 μm. In some embodiments, the thickness of the bilayer after sintering is 20 μm to 60 μm. In some embodiments, the thickness of the bilayer after sintering is 10 μm to 50 μm. In some embodiments, the thickness of the bilayer after sintering is 10 μm to 40 μm. In some embodiments, the thickness of the bilayer after sintering is 10 μm to 30 μm. In some embodiments, the thickness of the bilayer after sintering is about 10 μm. In some embodiments, the thickness of the bilayer after sintering is about 11 μm. In some embodiments, the thickness of the bilayer after sintering is about 12 μm. In some embodiments, the thickness of the bilayer after sintering is about 13 μm. In some embodiments, the thickness of the bilayer after sintering is about 14 μm. In some embodiments, the thickness of the bilayer after sintering is about 15 μm. In some embodiments, the thickness of the bilayer after sintering is about 16 μm. In some embodiments, the thickness of the bilayer after sintering is about 17 μm. In some embodiments, the thickness of the bilayer after sintering is about 18 μm. In some embodiments, the thickness of the bilayer after sintering is about 19 μm. In some embodiments, the thickness of the bilayer after sintering is about 20 μm. In some embodiments, the thickness of the bilayer after sintering is about 21 μm. In some embodiments, the thickness of the bilayer after sintering is about 22 μm. In some embodiments, the thickness of the bilayer after sintering is about 23 μm. In some embodiments, the thickness of the bilayer after sintering is about 24 μm. In some embodiments, the thickness of the bilayer after sintering is about 25 μm. In some embodiments, the thickness of the bilayer after sintering is about 26 μm. In some embodiments, the thickness of the bilayer after sintering is about 27 μm. In some embodiments, the thickness of the bilayer after sintering is about 28 μm. In some embodiments, the thickness of the bilayer after sintering is about 29 μm. In some embodiments, the thickness of the bilayer after sintering is about 30 μm. In some embodiments, the thickness of the bi-layer after sintering is about 31 μm. In some embodiments, the thickness of the bi-layer after sintering is about 32 μm. In some embodiments, the thickness of the bi-layer after sintering is about 33 μm. In some embodiments, the thickness of the bi-layer after sintering is about 34 μm. In some embodiments, the thickness of the bi-layer after sintering is about 35 μm. In some embodiments, the thickness of the bi-layer after sintering is about 36 μm. In some embodiments, the thickness of the bi-layer after sintering is about 37 μm. In some embodiments, the thickness of the bi-layer after sintering is about 38 μm. In some embodiments, the thickness of the bi-layer after sintering is about 39 μm. In some embodiments, the thickness of the bi-layer after sintering is about 40 μm. In some cases, the maximum thickness of the bi-layer after sintering is about 40 μm.

[0126] In some embodiments, when the solid electrolyte is sintered, the height of the film (along the z-axis) decreases, while the width and length of the film (along the x-axis and y-axis, respectively) remain substantially constant. Depending on the embodiment, the film shrinks by about 30% to about 40% due to sintering. Thus, for example, for a film having a film thickness of about 100 μm, the thickness of the film after sintering is between about 60 μm and about 70 μm.

[0127] In some examples, the solid electrolyte has a size of about 64 mm by 79 mm. In some examples, the solid electrolyte has a size of about (64 ± x) mm by about (79.5 ± y) mm, wherein x and y are between 1 and 10 mm.

[0128] The method and apparatus disclosed in the present application can be used to sinter lithium-filled garnets on metal foil. In some embodiments, the metal foil is a dense metal layer. In some examples, the metal foil is a dense metal layer, which also includes a ceramic. In some of these examples, the ceramic is a lithium-filled garnet.

[0129] In some examples, lithium-filled garnet (LLZO) is sintered onto a metal foil. In some embodiments, the metal foil is pure nickel. In these examples, the metal foil is a combination of nickel / iron. In some of these examples, the Ni content in the metal foil is 85-95% and the Fe content is 5-20%. In some of these examples, the Ni content in the metal foil is 90-95% and the Fe content is 5-10%. In some embodiments, the metal foil is Ni / Fe 93% / 7%. In these examples, the metal foil is Ni / Fe 95% / 5%. In these examples, the metal foil is Ni / Fe 97% / 3%.

[0130] In some examples, LLZO is sintered on a metal foil. In some embodiments, the metal foil is pure copper. In some embodiments, the metal foil is Cu / Fe 93% / 7%. In these examples, the metal foil is a combination of copper / iron.

[0131] In some examples, including any of the above, the sintered article comprises a double layer. In an example, the double layer comprises a metal foil and a ceramic film. In some embodiments, the sintered article comprises three layers. In some embodiments, the metal is Ni. In some cases, the thickness of Ni is about 1 μm. In some embodiments, the thickness of Ni is about 2 μm. In some cases, the thickness of Ni is about 3 μm. In some embodiments, the thickness of Ni is about 4 μm. In some embodiments, the thickness of Ni is about 5 μm. In some embodiments, the thickness of Ni is about 6 μm. In some embodiments, the thickness of Ni is about 7 μm. In some embodiments, the thickness of Ni is about 8 μm. In some embodiments, the thickness of Ni is about 9 μm. In some embodiments, the thickness of Ni is about 10 μm. In some embodiments, the thickness of Ni is about 11 μm. In some embodiments, the thickness of Ni is about 12 μm. In some embodiments, the thickness of Ni is about 13 μm. In some embodiments, the thickness of Ni is about 14 μm. In some embodiments, the thickness of Ni is about 15 μm. In some embodiments, the thickness of Ni is about 16 μm. In some embodiments, the thickness of Ni is about 17 μm. In some embodiments, the thickness of Ni is about 18 μm. In some embodiments, the thickness of Ni is about 19 μm. In some embodiments, the thickness of Ni is about 20 μm.

[0132] In some examples, the slurry is deposited on a foil to form a green tape with a foil backing. In some embodiments, the foil is a Mylar foil. The green tape with a foil backing can be wound into a roll to form an unsintered film roll with a foil backing. The unsintered film roll with a foil backing can be loaded onto the device described in the present application. In some examples, the method of using the device includes: (a) loading a roll of unsintered film with a foil backing on a front roller, (b) unwinding the unsintered film, (c) sintering the unsintered film to make a sintered film with a foil backing, and (d) in a controlled atmosphere, winding the sintered film with a foil backing onto a rear roller. In some cases, the foil backing can include nickel metal or nickel foil.

[0133] In some examples, the green film sintered using the apparatus is a double layer or a triple layer.

[0134] In some examples, various layer structures can be envisioned and sintered according to the sintering methods described in the present application: A) a single lithium-filled garnet material; B) a single lithium-filled garnet material, which may include active materials, binders, solvents and / or carbon; C) a double layer, which includes a layer of lithium-filled garnet and a layer of metal powder, foil or sheet; D) a double layer, which includes a layer of lithium-filled garnet and a layer including metal powder, foil or sheet; E) a double layer, which includes a layer of lithium-filled garnet material and a layer of metal powder, foil or sheet, and the lithium-filled garnet material optionally includes active material, binder, solvent, and / or carbon; F) three layers comprising two layers of lithium-filled garnet and a layer of metal powder, foil or sheet between and in contact with the garnet layers; G) three layers comprising two layers of lithium-filled garnet and a layer comprising metal powder, foil or sheet between and in contact with the garnet layers; H) three layers comprising two layers of lithium-filled garnet material and a layer of metal powder, foil or sheet between and in contact with the garnet layers, wherein each garnet layer optionally comprises active material, binder, solvent and / or carbon.

[0135] In some cases, a double layer can be sintered using the apparatus described herein. In some cases, a triple layer can be sintered using the CML described herein.

[0136] The three layers may include a lithium-filled garnet layer, a metal layer, and a second lithium-filled garnet layer on the other side of the metal layer. The three layers may be passed through the device with one lithium-filled garnet layer facing up and another lithium-filled garnet layer facing down.

[0137] The bilayer may include a layer of lithium-filled garnet and a layer of metal foil. The bilayer membrane may be passed through the device of the present application with the lithium-filled garnet facing up (ie, the metal layer at the bottom) or with the lithium-filled garnet facing down (ie, the metal layer at the top).

[0138] In an embodiment, the foil discussed above, upon which the material 130 (in an embodiment, lithium-filled garnet) is placed, is selected from the group consisting of nickel, iron, molybdenum, titanium, tungsten, and copper, alloys, and combinations thereof.

[0139] In some examples, the metal foil or metal layer is nickel, steel, stainless steel, copper, iron, aluminum, titanium, tungsten, molybdenum, Kovar, Invar, ceramic, Haynes 216, or a combination thereof.

[0140] In some examples, the metal layer includes Ni, Fe, Cu, Al, Sn, Mo, steel, alloys, or combinations thereof. For example, the metal layer may include Ni and Fe. For example, the metal layer may include about 70% Ni and about 30% Fe. For example, the metal layer may include Ni and Fe. For example, the metal layer may include about 80% Ni and about 20% Fe. For example, the metal layer may include Ni and Fe. For example, the metal layer may include about 90% Ni and about 10% Fe. For example, the metal layer may include about 91% Ni and about 9% Fe. For example, the metal layer may include about 92% Ni and about 8% Fe. For example, the metal layer may include about 93% Ni and about 7% Fe. For example, the metal layer may include about 94% Ni and about 6% Fe. For example, the metal layer may include about 95% Ni and about 5% Fe. For example, the metal layer may include about 6% Ni and about 4% Fe. For example, the metal layer may include about 97% Ni and about 3% Fe. For example, the metal layer may include about 98% Ni and about 2% Fe. For example, the metal layer may include about 99% Ni and about 1% Fe. In some embodiments, the metal layer is a metal sheet. In some embodiments, the metal layer is an aluminum sheet. In some embodiments, the metal layer is a nickel sheet. In some embodiments, the metal layer may be ductile.

[0141] For example, the metal layer may comprise up to 20% iron. Fig.16 An example of a thin film made according to one embodiment is shown, where the Ni / Fe alloy foil has greater than 20% iron.

[0142] In some examples, the metal layer is about 1 μm thick. In some cases, the metal layer is about 2 μm thick. In some cases, the metal layer is about 3 μm thick. In some cases, the metal layer is about 4 μm thick. In some cases, the metal layer is about 5 μm thick. In some cases, the metal layer is about 6 μm thick. In some cases, the metal layer is about 7 μm thick. In some cases, the metal layer is about 8 μm thick. In some embodiments, the metal layer is about 9 μm thick. In some cases, the metal layer is about 10 μm thick. In some embodiments, the metal layer is about 11 μm thick. In some cases, the metal layer is about 12 μm thick. In some cases, the metal layer is about 13 μm thick. In some embodiments, the metal layer is about 14 μm thick. In some cases, the metal layer is about 15 μm thick. In some cases, the metal layer is about 16 μm thick. In some embodiments, the metal layer is about 17 μm thick. In some cases, the metal layer is about 18 μm thick. In some embodiments, the metal layer is about 19 μm thick. In some cases, the metal layer is about 20 μm thick. In some embodiments, the metal layer is made by electrodeposition. In some embodiments, the metal layer is made by roll annealing. In some embodiments, the metal layer is a bilayer of two metals. In some embodiments, the metal bilayer can be made by electrodeposition, sputtering or evaporating the top metal layer onto a metal foil.

[0143] In some examples, the thickness of the lithium-filled garnet-metal sintered film described in the present application is about 1 μm to about 100 μm. In some cases, these films are sintered with lithium-filled garnet and metal. The metal can be selected from the group consisting of Ni, Mg, Li, Fe, Al, Cu, Mo, Ti, steel, alloys thereof, and combinations thereof. The lithium-filled garnet and the metal are mixed into a powder and then sintered together to form a film. In some embodiments, the film includes a uniform mixture of lithium-filled garnet and metal. The relative amounts of lithium-filled garnet and metal can vary, from about 1% lithium-filled garnet to about 99% lithium-filled garnet by volume, with the remainder being metal.

[0144] In some embodiments, including any of the above, the lithium filled garnet is sintered onto the ceramic metal film.

[0145] According to embodiments, the materials described herein can be sintered within a process window in which materials such as lithium-filled garnet can be sintered without substantial defects (domain) and with suitable porosity. According to embodiments, the variables that can be used to define a suitable process window are related to the parameters of the furnace in which the sintering will be completed and the material formulation to be sintered. These variables include:

[0146] Furnace parameters:

[0147] Sintering temperature

[0148] Sintering heating rate (ramp rate)

[0149] Sintering residence time (in a specific zone, and / or total time in the furnace)

[0150] BBO temperature

[0151] BBO heating rate (ramp rate)

[0152] BBO residence time (in a specific zone, and / or total time in the furnace)

[0153] Cooling rate

[0154] formula:

[0155] Embryo density

[0156] Powder batch

[0157] Ceramic particle size

[0158] According to an embodiment, the parameters of the furnace have a parameter set that may be part of a defined process window within which sintering can be successfully performed, i.e., with few or no defects formed and with a suitable porosity (in some embodiments, less than 1%). In some embodiments, various combinations of sintering residence time and heating rate can define the process window. In different embodiments, the sintering residence time can vary from 1 to 10 minutes, and the heating rate can vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time can be 1 minute, and the heating rate can vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time can be 2 minutes, and the heating rate can vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time can be 3 minutes, and the heating rate can vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time can be 4 minutes, and the heating rate can vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time can be 5 minutes, and the heating rate can vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 6 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 7 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 8 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 9 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 10 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 1 minute, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 2 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 3 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 4 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 5 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 6 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 7 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 8 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 9 minutes, and the heating rate may vary from 6°C to 24°C / minute. In different embodiments, the sintering residence time may be 10 minutes, and the heating rate may vary from 6°C to 24°C / minute.

[0159] For each of the sintering residence times just mentioned, the heating rate may be at least 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 50°C, 75°C, 100°C, 125°C, 150°C, 175°C, or 200°C / minute, depending on the specific embodiment. In some embodiments, a heating rate of at least 25°C / minute, 50°C / minute, 75°C / minute, 100°C / minute, 125°C / minute, or 150°C / minute may be used, depending on the tool. As will be appreciated by those of ordinary skill, varying the heating rate may affect many other factors in the process, such as sintering residence time, gas flow, accessories, etc.

[0160] Fig.17 A film made according to the example is shown, where the temperature was ramped at 10°C / min up to 1160°C and the dwell time at 1160°C was 5 minutes. As shown, larger pores were formed in the film and defects were formed. This may be due to the lower ramp rate under these conditions.

[0161] In the process described in this application, different tools may require different gas residence times. The gas residence time can be as short as 1 minute or as long as 20 minutes. In some cases, the gas residence time is from 2 minutes to 15 minutes, 4 minutes to 13 minutes, or 4 minutes to 10 minutes.

[0162] As will be appreciated by one of ordinary skill, residence time may be resolved in seconds rather than minutes and heating rates may be resolved in fractions of degrees in order to better control particle size.

[0163] According to an embodiment, the greater the conveyor speed, the lower the residence time. For a multi-zone furnace, the longer each zone is, the faster the conveyor must move for a given residence time, depending on the embodiment.

[0164] According to an embodiment, sintering may be performed in one or more specific zones of the furnace. According to an embodiment, sintering may take place in parts of specific zones of the furnace.

[0165] In different embodiments, the speed at which the double-layer structure moves through each area of ​​the furnace can range from 20mm / min to 150mm / min, depending on the length of the area, the residence time, and the heating rate. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 25mm / min to 145mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 30mm / min to 140mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 35mm / min to 135mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 40mm / min to 130mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 45mm / min to 125mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 50mm / min to 120mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 60mm / min to 110mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 65mm / min to 105mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 70mm / min to 100mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 75mm / min to 95mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 70mm / min to 90mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 75mm / min to 95mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 80mm / min to 90mm / min.

[0166] In different embodiments, the speed at which the double-layer structure moves through each area of ​​the furnace can range from 20mm / min to 100mm / min, depending on the length of the area, the residence time, and the heating rate. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 25mm / min to 95mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 30mm / min to 90mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 35mm / min to 85mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 40mm / min to 80mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 45mm / min to 75mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 50mm / min to 70mm / min. In different embodiments, the double-layer structure can move through each area of ​​the furnace at a speed of 55mm / min to 65mm / min.

[0167] In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 50 mm / min to 100 mm / min. In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 55 mm / min to 95 mm / min. In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 60 mm / min to 90 mm / min. In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 65 mm / min to 85 mm / min. In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 70 mm / min to 80 mm / min.

[0168] In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 50 mm / min to 80 mm / min. In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 55 mm / min to 75 mm / min. In various embodiments, the double layer structure can move through various areas of the furnace at a speed of 60 mm / min to 70 mm / min.

[0169] In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 20mm / min to 80mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 25mm / min to 75mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 30mm / min to 70mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 35mm / min to 65mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 40mm / min to 60mm / min. In different embodiments, the double layer structure can move through various areas of the furnace at a speed of 45mm / min to 55mm / min.

[0170] In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 20mm / min to 30mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 25mm / min to 35mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 30mm / min to 40mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 35mm / min to 45mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 40mm / min to 50mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 50mm / min to 60mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 55mm / min to 65mm / min. In different embodiments, the double-layer structure can move through various areas of the furnace at a speed of 75mm / min to 85mm / min.

[0171] The apparatus, system and method described in the present application can be used to manufacture various materials. These materials include but are not limited to lithium-filled garnet films. These materials include but are not limited to a double layer of lithium-filled garnet film on a metal layer or a triple layer consisting of two lithium-filled garnet films and a metal layer between them. The apparatus, system and process described in the present application can be used to manufacture lithium-filled garnet thin films or composite materials, including but not limited to any of the following sintered thin films or film-containing materials: PCT / US2016 / 043428, filed on July 21, 2016, published as WO2017015511A1, entitled "PROCESS AND MATERIALSFOR CASTING AND SINTERING GREEN GARNET THIN FILMS"; PCT / US2019 / 056584, filed on October 16, 2019, published as WO2020081718A1, entitled "SINTERING LARGE AREA CERAMIC FILMS"; PCT / US2016 / 15209, filed on January 27, 2016, published as WO2017131676A1, entitled "ANNEALEDGARNET ELECTROLYTE “SEPARATORS”; PCT / US2017 / 039069, filed on January 23, 2017, published as WO2018236394A1, entitled “LITHIUM-STUFFED GARNET ELECTROLYTES WITH SECONDARYPHASE INCLUSIONS”; PCT / US2019 / 54117, filed on October 1, 2019, published as WO2020072524A1, entitled “METHOD OF MAKING AND USING AND ELECTROCHEMICAL CELL COMPRISING AN INTERLAYER”; and U.S. Patents 10,403,931, 10,290,895, 9,966,630 B2, 1,0347,937 B2, and 10,103,405. The entire contents of each of the above documents are incorporated into this application by reference for all purposes.

[0172] In some embodiments, including any of the above, the ceramic-metal film can be an oxide-metal film. In some embodiments, the film has a ceramic layer and a metal layer. In other examples, the film is a uniform mixture of ceramic and metal. In some examples, the ceramic-metal film includes ceramic and metal. In some embodiments, the volume percentage of ceramic is about 10% and the volume percentage of metal is about 90%. In some embodiments, the volume percentage of ceramic is about 20% and the volume percentage of metal is about 80%. In some embodiments, the volume percentage of ceramic is about 30% and the volume percentage of metal is about 70%. In some embodiments, the volume percentage of ceramic is about 40% and the volume percentage of metal is about 60%. In some embodiments, the volume percentage of ceramic is about 50% and the volume percentage of metal is about 50%. In some embodiments, the volume percentage of ceramic is about 60% and the volume percentage of metal is about 40%. In some embodiments, the volume percentage of ceramic is about 70% and the volume percentage of metal is about 30%. In some embodiments, the volume percentage of ceramic is about 80% and the volume percentage of metal is about 20%. In some embodiments, the volume percentage of ceramic is about 90% and the volume percentage of metal is about 10%. In some embodiments, the volume percentage of ceramic is about 5% and the volume percentage of metal is about 95%. In some embodiments, the volume percentage of the ceramic is about 15% and the volume percentage of the metal is about 85%. In some embodiments, the volume percentage of the ceramic is about 25% and the volume percentage of the metal is about 75%. In some embodiments, the volume percentage of the ceramic is about 35% and the volume percentage of the metal is about 65%. In some embodiments, the volume percentage of the ceramic is about 45% and the volume percentage of the metal is about 55%. In some embodiments, the volume percentage of the ceramic is about 55% and the volume percentage of the metal is about 45%. In some embodiments, the volume percentage of the ceramic is about 65% and the volume percentage of the metal is about 35%. In some embodiments, the volume percentage of the ceramic is about 75% and the volume percentage of the metal is about 25%. In some embodiments, the volume percentage of the ceramic is about 85% and the volume percentage of the metal is about 15%. In some embodiments, the volume percentage of the ceramic is about 95% and the volume percentage of the metal is about 5%.

[0173] In some examples, including any of the above, the ceramic-metal film includes an oxide and a metal. In some embodiments, the volume percentage of the oxide is about 10% and the volume percentage of the metal is about 90%. In some embodiments, the volume percentage of the oxide is about 20% and the volume percentage of the metal is about 80%. In some embodiments, the volume percentage of the oxide is about 30% and the volume percentage of the metal is about 70%. In some embodiments, the volume percentage of the oxide is about 40% and the volume percentage of the metal is about 60%. In some embodiments, the volume percentage of the oxide is about 50% and the volume percentage of the metal is about 50%. In some embodiments, the volume percentage of the oxide is about 60% and the volume percentage of the metal is about 40%. In some embodiments, the volume percentage of the oxide is about 70% and the volume percentage of the metal is about 30%. In some embodiments, the volume percentage of the oxide is about 80% and the volume percentage of the metal is about 20%. In some embodiments, the volume percentage of the oxide is about 90% and the volume percentage of the metal is about 10%. In some embodiments, the volume percentage of the oxide is about 5% and the volume percentage of the metal is about 95%. In some embodiments, the volume percentage of the oxide is about 15% and the volume percentage of the metal is about 85%. In some embodiments, the volume percentage of the oxide is about 25% and the volume percentage of the metal is about 75%. In some embodiments, the volume percentage of the oxide is about 35% and the volume percentage of the metal is about 65%. In some embodiments, the volume percentage of the oxide is about 45% and the volume percentage of the metal is about 55%. In some embodiments, the volume percentage of the oxide is about 55% and the volume percentage of the metal is about 45%. In some embodiments, the volume percentage of the oxide is about 65% and the volume percentage of the metal is about 32%. In some embodiments, the volume percentage of the oxide is about 75% and the volume percentage of the metal is about 25%. In some embodiments, the volume percentage of the oxide is about 85% and the volume percentage of the metal is about 15%. In some embodiments, the volume percentage of the oxide is about 95% and the volume percentage of the metal is about 5%.

[0174] In some examples, including any of the above, the ceramic-metal film includes ceramic and metal. In some embodiments, the weight percentage of the ceramic is about 10% and the weight percentage of the metal is about 90%. In some embodiments, the weight percentage of the ceramic is about 20% and the weight percentage of the metal is about 80%. In some embodiments, the weight percentage of the ceramic is about 30% and the weight percentage of the metal is about 70%. In some embodiments, the weight percentage of the ceramic is about 40% and the weight percentage of the metal is about 60%. In some embodiments, the weight percentage of the ceramic is about 50% and the weight percentage of the metal is about 50%. In some embodiments, the weight percentage of the ceramic is about 60% and the weight percentage of the metal is about 40%. In some embodiments, the weight percentage of the ceramic is about 70% and the weight percentage of the metal is about 30%. In some embodiments, the weight percentage of the ceramic is about 80% and the weight percentage of the metal is about 20%. In some embodiments, the weight percentage of the ceramic is about 90% and the weight percentage of the metal is about 10%. In some embodiments, the weight percentage of the ceramic is about 5% and the weight percentage of the metal is about 95%. In some embodiments, the weight percentage of the ceramic is about 15% and the weight percentage of the metal is about 85%. In some embodiments, the weight percentage of the ceramic is about 25% and the weight percentage of the metal is about 75%. In some embodiments, the weight percentage of the ceramic is about 35% and the weight percentage of the metal is about 65%. In some embodiments, the weight percentage of the ceramic is about 45% and the weight percentage of the metal is about 55%. In some embodiments, the weight percentage of the ceramic is about 55% and the weight percentage of the metal is about 45%. In some embodiments, the weight percentage of the ceramic is about 65% and the weight percentage of the metal is about 35%. In some embodiments, the weight percentage of the ceramic is about 75% and the weight percentage of the metal is about 25%. In some embodiments, the weight percentage of the ceramic is about 85% and the weight percentage of the metal is about 15%. In some embodiments, the weight percentage of the ceramic is about 95% and the weight percentage of the metal is about 5%.

[0175] In some embodiments, including any of the above, the ceramic in the ceramic-metal film is selected from alumina, silica, titania, lithium-filled garnet, lithium aluminate, aluminum hydroxide, aluminosilicate, lithium zirconate, lanthanum aluminate, lanthanum zirconate, lanthanum oxide, lithium oxide, zirconium oxide, Li2ZrO3, xLi2O-(1-x)SiO2 (where x = 0.01-0.99), aLi2O-bB2O3-cSiO2 (where a + b + c = 1), LiL a O2, LiAlO2, Li2O, Li3PO4 or a combination thereof.

[0176] In an example, the three layers include a metal foil and a green ceramic film on both sides of the metal foil. The thickness of the metal foil in the double or triple layer can be between 0.5 μm and 50 μm. The thickness of the metal foil in the double or triple layer can be between 3 μm and 30 μm. In some cases, the thickness of the metal foil in the double or triple layer can be between 5-20 μm. In another example, the thickness of the metal foil in the double or triple layer can be between 5 μm and 15 μm.

[0177] Fig.19 An embodiment is shown in which a bilayer (B) is sandwiched between a centerless cover (A) and a bottom support plate (C). In some embodiments, the centerless cover (A) is a top support plate. In some embodiments, the centerless cover (A) is a foam material. In some embodiments, including any of the above, the bilayer (B) includes a layer comprising a metal and another layer comprising a raw film or a sintered film. In some embodiments, the sintered film of the bilayer (B) is a lithium-filled garnet sintered film. In some embodiments, including any of the above, the layer comprising a metal in the bilayer (B) also includes lithium-filled garnet. In some embodiments, including any of the above, the layer comprising a metal comprises nickel (Ni). In some embodiments, including any of the above, the layer comprising a metal comprises copper (Cu). In some embodiments, including any of the above, the layer comprising a metal comprises iron (Fe). In some embodiments, including any of the above, the foam material is a metal foam. In some embodiments, including any of the above, the foam material is a porous nickel foam. Example

[0178] Unless otherwise stated, reagents, chemicals, and materials were purchased commercially.

[0179] Purchase bagged battery containers from Showa Denko.

[0180] The electrochemical potentiostat used was an Arbin potentiostat.

[0181] Electrical impedance spectroscopy (EIS) was performed using a Biologic VMP3, VSP, VSP-300, SP-150, or SP-200.

[0182] Scanning electron microscopy (SEM) was performed on a FEIQuanta SEM, Apreo SEM, Helios 600i, or Helios660FIB-SEM. (FIB stands for focused ion beam.)

[0183] The transmission electron microscopy (TEM) method was as follows.

[0184] Sample preparation: Samples for TEM measurements were prepared using a Ga ion source focused ion beam SEM (nanoDUET NB5000, from Hitachi High-Tech Corporation). In order to protect the material surface from the Ga ion beam, multiple protective layers were deposited before sampling; first the metal layer was deposited using a plasma coater, and then the carbon protective layer and tungsten layer were deposited using high vacuum evaporation and focused ion beam, respectively. Thin section sampling was performed using a focused ion beam. The prepared samples were measured under a transmission electron microscope.

[0185] X-ray powder diffraction (XRD) was performed using a Bruker D8 Advance A25 at room temperature (21-23°C) using Cu K-α radiation. Light source: Cu-Ka, wavelength: The X-ray was 40 kV, 25 mA. The detector was Bruker LYNXEYE XE, and the position sensitive detector (PSD) opening was 2.843. The divergence slit was 0.6 mm, and the anti-scatter slit was fixed at 5.0 mm.

[0186] Milling was performed using a Retsch PM 400 planetary ball mill. Mixing was performed using a Fisher Scientific vortex mixer, a Flaktek high-speed mixer, or a Primix thin-film homogenizer.

[0187] Casting was done on a TQC scale table. Calendering was done on an Innovative Machinery Company (IMC) calender.

[0188] Fig. 9 Two films made according to the examples are shown. The film on the left has dimensions of approximately 60 mm*75 mm. The film on the right has dimensions of approximately 75 mm*90 mm.

[0189] Example 1 - RTP Process

[0190] The green tape cast on the metal foil is unrolled and then cut to size for sintering. This is done here using a laser cutter, but in different processes it can also be cut using a blade blanking tool. The discrete green sheets are then stacked between support assemblies and placed on a bottom graphite heating plate that is part of the sintering unit and a top graphite heating plate close above. In this case, the support assembly is a dense Al2O3 plate, on which the green sheet with the coating side facing up is placed, followed by a ceramic or metal frame assembly, followed by another dense Al2O3 plate.

[0191] The stack was heated to 800°C at a heating rate of 50°C / min (range: 50°C / min-100°C / min) and held for 5 minutes. The gas (mainly argon) flow rate was 2.0 LPM (liters / minute). After removing the organic matter, the stack was sintered by heating to 1100°C at a heating rate of 100°C / min (range: 100°C / min-300°C / min) and held for 30 seconds. The graphite plate was then cooled to room temperature at a rate of 100°C / min (range: 100°C / min-300°C / min). After reaching room temperature, the sintered stack was removed from the furnace and unloaded.

[0192] Example 2 - Two-step process (RTP tool plus light tool)

[0193] As mentioned above, the green tape cast on the metal foil is unrolled and cut to the appropriate size for sintering. This is done here using a laser cutter, but in different processes it can also be cut using a blade blanking tool. The discrete green sheets are then stacked between support assemblies and placed on a bottom graphite heating plate that is part of the sintering device and a top graphite heating plate close above. In this case, the support assembly is a dense Al2O3 plate, on which the green sheet with the coated side facing up is placed, followed by a ceramic or metal frame assembly, followed by another dense Al2O3 plate.

[0194] In order to remove organic matter from the green layer, the graphite plate was heated to 800°C at a heating rate of 50°C / min (range: 50°C / min-100°C / min) and maintained for 5 minutes. The graphite plate was then cooled to room temperature at a rate of 100°C / min (range: 100°C / min-300°C / min). After reaching room temperature, the sintered laminate was removed from the graphite plate, moved to a lamp heating system, and placed on a graphite susceptor for sintering.

[0195] In the lamp heating system, the gas (mainly argon) flow rate is 0.25 LPM (liters / minute). During the sintering process, the graphite susceptor containing the stack to be sintered is heated to 1120°C at a heating rate of 300°C / min (range: 1080°C-1120°C) and maintained at this temperature for 30 seconds (range: 30 seconds-2 minutes). After reaching room temperature, the sintered stack is taken out of the heating system and unloaded.

[0196] Example 3 - Vacuum Furnace Tools

[0197] As mentioned above, the green tape cast on the metal foil is unrolled and cut to size for sintering. Here this is done using a laser cutter, but in different processes it can also be cut using a blade blanking tool. The discrete green sheets are then stacked between support components and placed on a support accessory used with the sintering device. In this case, the support component is a dense Al2O3 plate, on which the green sheet with the coating side facing up is placed, followed by a ceramic or metal frame assembly, followed by a metal sheet with the LiAlO2 coating, and then another dense Al2O3 plate.

[0198] The prepared sintered stack, including support accessories, support components and discrete green sheets, is placed in a vacuum furnace. In order to remove organic matter from the green layer, the furnace is heated to 780°C (range: 760°C to 840°C) at a heating rate of 30°C / min (range: 10°C / min to 30°C / min) at normal pressure and maintained for 15 minutes. The gas (mainly nitrogen) flow rate is 5.0LPM (liters / minute) (range: 5LPM-13LPM). After removing the organic matter, the furnace is heated to about 1200°C at a heating rate of 50°C / min for sintering and maintained for 1 minute. The furnace is then cooled to room temperature. After reaching room temperature, the sintered stack is removed from the furnace and unloaded. The cross-section of the resulting film is as shown Fig.18 shown.

[0199] Example 4 - Vacuum Furnace Process under Partial Vacuum Conditions

[0200] As mentioned above, the green tape cast on the metal foil is unrolled and cut to size suitable for sintering. Here it is done using a laser cutter, but in different processes it can also be cut using a blade blanking tool. The discrete green sheets are then stacked between support components and placed on a support assembly used with the sintering device. In this case, the support assembly refers to a dense Al2O3 plate, on which the green sheet with the coating side facing up is placed, followed by a ceramic or metal frame assembly, followed by a metal sheet with the LiAlO2 coating, and then another dense Al2O3 plate.

[0201] The prepared sintered stack, including support accessories, support components and discrete green sheets, is placed in a vacuum furnace. In order to remove organic matter from the green sheets, the furnace is heated to about 800°C at atmospheric pressure and maintained for 15 minutes. The gas flow rate is 5.0 LPM (liters per minute), mainly nitrogen. After the organic matter is removed, the furnace is cooled to room temperature. After reaching room temperature, the furnace is heated to about 15m 3 / hr rate to create a partial vacuum in the furnace with a dry vacuum pump, while flowing 5.0 LPM of nitrogen to create a pressure of 14 Torr. This state is maintained throughout the process, and the furnace is heated to about 1150°C at a heating rate of 50°C / min for sintering, and maintained for 1 minute. The furnace is then cooled to room temperature. After reaching room temperature, the pumping is stopped, the furnace is ventilated to atmospheric pressure with nitrogen, and the sintered laminate is removed from the furnace and unloaded.

[0202] Example 5

[0203] The prepared sintered stack, including support accessories, support assemblies and discrete green sheets, is loaded onto the conveyor of the RHK (roller hearth kiln). The thermal parameters of the RHK are specified to perform two processes. In order to remove organic matter from the green layer, the sintered stack is heated to 800°C at an effective heating rate of 24°C / min and held for 15 minutes. After removing the organic matter, the sintered stack is then heated to 1150°C at an effective heating rate of 24°C / min and held for 7 minutes. The sintered stack is then cooled to room temperature. After leaving the RHK, the sintered stack is removed from the conveyor and unloaded. The sintered film is then cut into sizes suitable for the battery cell structure using a laser cutter. The resulting film is made into battery cells for electrical testing, such as Fig.10 and 11 shown.

[0204] The battery was assembled with two double layers of NMC active materials. The thickness of the double layer was 35 μm, the width was 60 mm, and the length was 75 mm. The cathode was impregnated with a liquid cathode electrolyte containing a lithium salt and a solvent for dissolving the lithium salt. The battery was cycled at 25°C and 1 atm pressure with a charge rate of 1.35C and a discharge rate of 1C. Fig.10 As shown, after 300 cycles of 100% depth of discharge, the battery retained more than 90% of its initial capacity.

[0205] Example 6

[0206] The battery was assembled with six double-layer NMC active materials. The double-layer film had a thickness of 35 μm, a width of 60 mm, and a length of 75 mm. The cathode was impregnated with a liquid cathode electrolyte containing a lithium salt and a solvent for dissolving the lithium salt. The battery was cycled at 25°C and 1.5 atm pressure with a charge rate of 1C and a discharge rate of 1C. Fig.11 As shown, after 300 cycles of 100% discharge depth, the battery retained more than 95% of its initial capacity.

[0207] Example 7

[0208] As mentioned above, the green tape cast on the metal foil is unrolled and cut to size for sintering. This is done using a blade blanking tool, but in a different process it can also be cut using a laser cutter. The discrete green sheets are then stacked between support components and placed on a support assembly used with the sintering device. In this case, the support assembly is a dense Al2O3 plate with the green sheet with the coating facing up, followed by a ceramic or metal frame assembly, and then another dense Al2O3 plate with the LiAlO2 coating.

[0209] Example 8

[0210] The prepared sintered stack, including support accessories, support assemblies, and discrete green sheets, was placed in a three-inch tube furnace. To remove organic matter from the green layer, the furnace was heated to 800°C at a ramp rate of 10°C / min and held for 15 minutes. The gas flow rate was 0.25 LPM (liters per minute), mainly nitrogen. After removing the organic matter, the furnace was then heated to 1150°C for sintering at a ramp rate of 10°C / min and held for 5 minutes. The furnace was then cooled to room temperature at a rate of 10°C / min until the natural cooling rate of the furnace was reached. After reaching room temperature, the sintered stack was removed from the furnace and unloaded. Thin film imaging was performed using an optical microscope under coaxial illumination conditions to observe defects.

[0211] Fig.13 is a micrograph of the film showing defects in the film, wherein the defects are large particles. Fig.13 The white spots in the image are the defects. In this example, the film was sintered at too high a temperature and the film was left on for too long, leading to the formation of defects.

[0212] Example 9

[0213] The temperature was raised to 1100° C. at a rate of 50° C. / min and maintained at the highest temperature (i.e., 1100° C.) for 1 minute to form a thin film. Fig.12 is a micrograph of the resulting film, showing the pores in the film. In this example, the film was sintered at too low a temperature and the residence time was too short. As one of ordinary skill in the art will appreciate, there is a direct correlation between the length of the residence time and the maximum sintering temperature. That is, an increase in one variable will directly affect the other.

[0214] Example 10

[0215] Fig.14 A cross section of a green film before heat treatment in one embodiment is shown. The green film has a thickness of about 50 μm.

[0216] Fig.15It shows the heat treatment process described in this application. Fig.14 Cross section of the green film. The thickness of the sintered film is about 25 μm.

[0217] Predictive Example - Fabrication of Sintered Solid-State Electrolytes

[0218] In the following prophetic example, a slurry is made by mixing lithium filled garnet, solvent, binder and plasticizer.

[0219] Predictive Example 1 (Slurry 1): LLZO powder is dispersed in ethanol containing 2% polyacrylic acid using an ultrasonic horn. Larger particles will precipitate. The supernatant is discarded and the recovered powder is dried in air. The collected powder, polyvinyl butyral, benzyl butyl phthalate, acetone and ethanol are added to a vial in a weight ratio of 37:3:3:29:29 and ball milled with ZrO2 beads of 2.0 mm diameter for 10-24 hours. The slurry is poured onto a polyester substrate with a doctor's knife; the film thickness is controlled by adjusting the blade height. The dried raw film is manually peeled off the polyester film substrate and cut into the desired size.

[0220] Predictive Example 2 (Slurry 2): LLZO powder containing 3 wt% polyacrylic acid was dispersed in ethanol. The second solution was polyvinyl butyral, benzyl butyl phthalate and acetone, mixed in a mass ratio of 1:1:10. The second solution was mixed with the first solution in equal amounts by volume. The resulting slurry was milled with ZrO2 beads for 8-16 hours. The slurry was cast onto a polyester substrate using a doctor blade, and the thickness was controlled by the doctor blade height. After drying in air, the film was manually peeled off the substrate and cut into the required size.

[0221] Prediction Example 3 (Slurry 3): Methylcellulose, polyethylene glycol and glycerol were dissolved in water to prepare a polymer aqueous solution. The weight ratio of each component was water:methylcellulose:polyethylene glycol:glycerol=100:1:4:4. LLZO powder was added to the polymer solution in equal weights. The slurry was mixed with ZrO2 beads for 5-60 minutes, and the slurry was poured onto a polyester film with a doctor blade; the thickness was controlled by the doctor blade gap. After drying in air, the tape was peeled off the polyester film substrate and cut into the required size.

[0222] Predictive Example 4 (Slurry 4): LLZO is ball milled in a mixture of equal parts of ethanol, xylene and toluene. 2-5 wt% of herring oil relative to the weight of LLZO is added dropwise over 30 minutes. 6-10 wt% of polyvinyl butyral relative to the weight of LLZO, 2-4 wt% of polyethylene glycol relative to the weight of LLZO and 3-7 wt% of benzyl butyl phthalate relative to the weight of LLZO are added and mixed. Cast into tapes on a polyester film substrate using a doctor blade. After drying at 45°C for 1-6 hours, remove the tape from the polyester film and cut to the required size.

[0223] Prediction Example 5 (Slurry 5): The slurry was prepared by ball milling 100 g LLZO powder, 2-4 g triolein, 100-200 g n-propyl propionate, and 15-25 g Elvacite E-2046. The slurry was poured onto the substrate with a doctor blade, dried, and then removed from the substrate.

[0224] Predictive Example 6 (Slurry 6): 20 g of LLZO powder, 25-40 g of a solvent mixture (ethanol: butanol: propylene glycol in a volume percentage of 70-80: 15-25: 0-5), 1-3 g of dibutyl phthalate, 1-4 g of PVB and 0.1-1 g of a dispersant were mixed in a mill to make a slurry. The dispersant may be a dispersant such as BYK's Anti-terra-202. After mixing, the slurry was filtered, deoxygenated and cast onto a substrate by slot die coating. The green tape was dried, removed from the substrate and cut into appropriate sizes.

[0225] Predictive Example 7 (Slurry 7): A slurry was prepared by mixing water (30 parts by mass), LLZO powder (12-18 parts by mass) and a binder solution (WB4101, WB40B-44, WB40B-53 from Polymer Innovations, 8 parts by mass) in a mill for at least one hour. After mixing, the slurry was filtered, deoxygenated, and cast onto a substrate via slot die coating. The green tape was dried, removed from the substrate, and cut into appropriate sizes.

[0226] Prediction Example 8 (Slurry 8): Grind LLZO powder in a mixed solvent of toluene, isopropanol and fish oil. Mix the mixture for 1-5 hours to make a slurry. Prepare an adhesive solution with toluene, isopropanol, polyvinyl butyral and butylphenyl phthalate. Add the adhesive solution to the slurry and mix. Deoxygenate, filter and cast the mixture onto a polymer carrier. Dry the green tape and press into 10-40 cm long sheets. Remove the pressed sheet from the carrier and then cut into the required size.

[0227] Prediction Example 9 (Slurry 9): 80 grams of calcined LLZO powder was mixed with 50 milliliters of a 33% by weight polyvinyl alcohol butyral toluene solution and 4 grams of a plasticizer dibutyl phthalate to prepare a calcined LLZO slurry. A 3% by weight polyacrylic acid binder was added to the solution. The slurry was cast into a tape on a polyester film substrate with a silicon coating. The cast mixed slurry was dried at room temperature for 2-6 hours to form a raw film. The raw film was pressed into a 10-40 cm long sheet. The pressed sheet was removed from the carrier and cut into a suitable size.

[0228] As described above, in different processes, the slurry can be poured onto a metal foil such as a nickel foil. In different processes, as described above, the slurry can be poured onto an alloy foil, such as a combination of nickel, copper and iron. In different processes, as described above, the slurry can be poured onto nickel and iron alloy foils. During the process of pouring the slurry onto the metal foil and drying it into a tape (green double layer), the green tape layer can be removed from the metal substrate or not. The slurry on the foil is then placed in the apparatus described in the present application for sintering.

[0229] After drying, the dried slurry is placed in Figure 3 In some embodiments, the binder is burned out in the device. In some embodiments, the binder is burned out outside the device. In some embodiments, the film is sintered in the device as shown. Figure 3 In some embodiments, the film is sintered on a susceptor in a device such as Figure 3 In some embodiments, the susceptor is directly sintered on the susceptor in the device shown. Figures 6A-6C and Figure 7A-7B The accessories and frame structure shown are Figure 5 , Figure 8 The film is sintered in the apparatus shown in the figure. Figure 4A -C.

[0230] The embodiments and examples described above are merely illustrative and non-limiting. A person of ordinary skill will recognize or confirm based on routine experiments that there are many equivalents for specific compounds, materials and steps. All of these equivalents are within the scope of protection and are included in the appended claims.

Claims

1. A device for sintering materials, the device comprising: a furnace for heating said material; as well as A controller, the controller is used to control the temperature of the furnace and the time of heating the material; wherein the controller controls the temperature of the furnace so that the material is sintered at a temperature between about 1050° C. and about 1250° C.; The controller controls the heating time of the material to be between about 30 seconds and 3 minutes, thereby sintering the material.

2. The device according to claim 1, wherein the furnace comprises a plurality of zones, each zone comprises one or more heating elements, the controller controls the temperature of each zone so as to gradually heat and cool the material, and the sintering is performed in a central zone of the plurality of zones.

3. The apparatus of claim 2, further comprising a conveyor on which the material is loaded, wherein the controller controls the conveyor to convey the material into, through, and out of each of the plurality of zones in the furnace.

4. The apparatus of claim 3, wherein the controller controls the conveyor to move through the furnace at a speed of approximately 20 mm to 80 mm per minute.

5. The device according to any of the above claims, further comprising a metal foil, the material being placed on the metal foil to be sintered into a double-layer structure, the thickness of the metal foil not exceeding 20 μm.

6. The device of claim 5, wherein the metal foil is selected from the group consisting of tungsten, nickel, copper, iron, titanium, molybdenum, alloys thereof, and combinations thereof.

7. Apparatus according to claim 5 or 6, further comprising a fitting on which the double-layer structure is placed and moved through the furnace.

8. The device according to claim 7, wherein the accessory comprises a first plate made of a material selected from the group consisting of alumina (Al2O3), zirconium-toughened alumina (ZTA), mullite (3Al2O32SiO2 or 2Al2O3SiO2), aluminum nitride (AlN) or silicon carbide (SiC).

9. The device according to claim 8, wherein the accessory includes a second plate made of a material selected from the following materials: alumina (Al2O3), zirconium-toughened alumina (ZTA), mullite (3Al2O32SiO2 or 2Al2O3SiO2), aluminum nitride (AlN) or silicon carbide (SiC), and the second plate is placed on the double-layer structure.

10. The device according to claim 9 further comprises a frame sandwiched between the double-layer structure and the second plate, the frame being made of a material selected from porous alumina, zirconia, lithium aluminate, lithium tantalate, alumina, silica, cordierite, Ni, Kovar or Invar.

11. The device according to claim 10, wherein the frame material is provided with horizontal and / or vertical groove textures on one or both sides.

12. The device according to any one of the above claims, wherein the controller controls the temperature of the furnace so that the furnace is heated to a preset temperature at a rate not exceeding 50°C / min.

13. The device according to claim 8, wherein the controller controls the temperature of the furnace so that the furnace is heated to a preset temperature at a rate of about 5-35°C / min.

14. The apparatus of any preceding claim, wherein the controller controls the speed at which the material passes through the furnace so that the material stays inside the furnace for a time between approximately 1 and 10 minutes.

15. A device as claimed in any preceding claim, wherein the material comprises a solid electrolyte.

16. Apparatus as claimed in any preceding claim, wherein the material comprises lithium-stuffed garnet.

17. A device as claimed in any preceding claim, wherein the material has a thickness of about 100 μm before sintering.

18. The device according to any of the preceding claims, wherein the thickness of the material after sintering is between about 10 and 50 μm.

19. A method for sintering a material, comprising: heating the material in a furnace; Controlling the temperature of the furnace so that the material is sintered at a temperature between about 1050° C. and about 1250° C.; The furnace is controlled to heat the material for a time period between about 30 seconds and 3 minutes, thereby sintering the material.

20. The method according to claim 19, wherein the furnace comprises a plurality of zones, each zone comprises one or more heating elements, and controlling the temperature of the furnace comprises controlling the temperature of each of the zones so as to gradually heat and cool the material, and the sintering is performed in a central zone of the plurality of zones.

21. The method of claim 20, further comprising conveying the material through the furnace, the controller controlling a conveyor to convey the material into, through, and out of each of a plurality of zones in the furnace.

22. The method of claim 21, wherein conveying the material comprises moving the material through the furnace at a speed of about 20 mm to about 80 mm per minute.

23. The method according to any one of claims 19 to 22, further comprising placing the material on a metal foil to sinter into a double-layer structure, wherein the thickness of the metal foil does not exceed 20 μm.

24. The method of claim 23, wherein the metal foil is selected from the group consisting of tungsten, nickel, copper, iron, titanium, molybdenum, and combinations thereof.

25. The method of claim 23 or 24, further comprising moving the double layer structure on the accessory through the furnace.

26. The method of claim 25, wherein the accessory comprises a first plate made of a material selected from the group consisting of alumina (Al2O3), zirconium toughened alumina (ZTA), mullite (3Al2O32SiO2 or 2Al2O3SiO2), aluminum nitride (AlN) or silicon carbide (SiC).

27. The method of claim 26, wherein the accessory comprises a second plate made of a material selected from the group consisting of alumina (Al2O3), zirconium toughened alumina (ZTA), mullite (3Al2O32SiO2 or 2Al2O3SiO2), aluminum nitride (AlN) or silicon carbide (SiC), the second plate being placed on top of the double-layer structure.

28. The method of claim 27, further comprising a frame sandwiched between the double-layer structure and the second plate, the frame being made of a material selected from porous alumina, zirconia, lithium aluminate, lithium tantalate, alumina, silica, cordierite, Ni, Kovar or Invar.

29. The method of claim 28, wherein the frame material is provided with a horizontal and / or vertical groove texture on one or both sides.

30. The method according to any one of claims 19 to 29, wherein controlling the temperature of the furnace comprises allowing the furnace to heat up to a preset temperature at a rate not exceeding 50°C / min.

31. The method according to claim 30, wherein controlling the temperature of the furnace comprises raising the temperature of the furnace to a preset temperature at a rate of about 5-35°C / min.

32. The method according to any one of claims 19 to 31, further comprising controlling the speed at which the material passes through the furnace so that the time the material stays inside the furnace is between about 1 and 10 minutes.

33. The method of any one of claims 19-32, wherein the material comprises a solid electrolyte.

34. The method of any one of claims 19-33, wherein the material comprises lithium-stuffed garnet.

35. The method according to any one of claims 19 to 34, wherein the material has a thickness of about 100 μm before sintering.

36. The method according to any one of claims 19 to 35, wherein the thickness of the material after sintering is approximately between 10 and 50 μm.

Citation Information

Patent Citations

  • Garnet materials for Li secondary batteries and methods of making and using garnet materials

    US10103405B2

  • Garnet materials for Li secondary batteries and methods of making and using garnet materials

    US10290895B2

  • Lithium-stuffed garnet electrolytes with secondary phase inclusions

    US10347937B2

  • Garnet materials for Li secondary batteries and methods of making and using garnet materials

    US10403931B2

  • Lithium stuffed garnet setter plates for solid electrolyte fabrication

    US10563918B2