Mixed aliphatic-aromatic polyesters

By controlling the catalyst combination and reaction conditions, a mixed aliphatic-aromatic polyester containing a specific ratio of saturated aliphatic dicarboxylic acids and aromatic dicarboxylic acids was prepared. This solved the problems of high glass transition temperature and residual cyclic oligomers in the prior art, achieving a low glass transition temperature and improved chain flexibility, and obtaining a biodegradable polyester with excellent thermal and mechanical properties.

CN118946614APending Publication Date: 2024-11-12NOVAMONT SPA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280087501.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-06
Filing Date
2022-12-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies struggle to produce aliphatic-aromatic polyesters with lower glass transition temperatures and improved chain flexibility and mechanical properties, and residual cyclic oligomers negatively impact the polyester's characteristics.

Method used

By selecting appropriate catalyst combinations and reaction conditions, and controlling the amount of residual mixed cyclic oligomers, a mixed aliphatic-aromatic polyester containing a specific ratio of saturated aliphatic dicarboxylic acids and aromatic dicarboxylic acids is prepared. Esterification and polycondensation steps are employed, and catalysts containing titanium and phosphorus compounds are used to control the oligomer content.

Benefits of technology

This study achieved a low glass transition temperature and improved chain flexibility in aliphatic-aromatic polyesters, while reducing the negative impact of residual cyclic oligomers on mechanical properties, resulting in a biodegradable polyester with excellent thermal properties and processability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004925376410000081
    Figure BDA0004925376410000081
  • Figure BDA0004925376410000101
    Figure BDA0004925376410000101
  • Figure BDA0004925376410000111
    Figure BDA0004925376410000111
Patent Text Reader

Abstract

Mixed aliphatic-aromatic polyester having suitable thermal properties and terminal acidity, characterized by having a dicarboxylic acid component comprising at least three saturated aliphatic C4-C24 dicarboxylic acids, C1-C24 alkyl esters thereof, salts thereof and mixtures thereof, azelaic acid and succinic acid being always present.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to mixed aliphatic-aromatic polyesters having suitable thermal properties and terminal acidity, characterized by having a dicarboxylic acid component comprising at least three saturated aliphatic C4-C24 dicarboxylic acids, their C1-C24 alkyl esters, their salts and mixtures thereof, with azelaic acid and succinic acid always present. Existing technology

[0002] It is known that the use of biodegradable polymers instead of non-biodegradable polymers has become a promising and essential way to avoid unbearable environmental damage.

[0003] Of course, biodegradable polymers must have excellent processability as well as excellent thermal and mechanical properties to be effectively used in a wide variety of applications, such as for the production of films and / or containers. It is also known that biodegradable aliphatic-aromatic polyesters produced from diacids and diols are particularly desirable for their flexible properties with a low glass transition temperature (Tg) and amorphous properties that provide improved chain flexibility compared to more crystalline products.

[0004] See, for example, the article entitled “Effect of Monomer Structure on Crystallisation and Glass Transition of Flexible Copolyesters” by Pan et al. (J. Polym. Environ. (2017) 25: 1051-1061).

[0005] Although the Tg behavior of various combinations of aliphatic-aromatic polyesters is known (see for example patent EP 3240818 B1), polyesters having a lower glass transition temperature and all the advantages indicated above are not easily available.

[0006] It is also known that the content of residual mixed cyclic oligomers in aliphatic-aromatic polyesters is undesirable since such contents adversely affect the properties of the polyester, in particular the mechanical properties and the transparency properties of the films obtained therefrom.

[0007] Patent application WO 2016 / 050963 describes a combined process for the production of polyesters, comprising an esterification or transesterification step and a subsequent polycondensation step, characterized in that the polycondensation step is carried out in the presence of a catalyst comprising a mixture of at least one compound containing titanium and at least one compound containing zirconium, wherein the Ti / (Ti+Zr) weight ratio is equal to or higher than 0.01 and lower than 0.70.

[0008] WO 2016 / 050963 teaches that polyesters with reduced residual cyclic oligomer formation can be obtained.

[0009] These residual cyclic oligomers are partially removed by distillation during the polycondensation step. However, some of these residual cyclic oligomers remain trapped in the polyester formed.

[0010] It has been found that by appropriately choosing the conditions of the process described in patent application WO 2016 / 050963, in particular by adding the phosphorus-containing compound in a suitable amount relative to the catalyst used, as well as specific temperature and pressure conditions, mixed aliphatic-aromatic polyesters can be obtained with a controlled amount of residual mixed cyclic oligomers which successfully bring about the desired reduction in the glass transition temperature of the mixed aliphatic-aromatic polyesters according to the invention.

[0011] In the present invention, "mixed aliphatic-aromatic polyester" means an aliphatic-aromatic polyester having at least three saturated aliphatic dicarboxylic acids.

[0012] In the present invention, "residual mixed cyclic oligomers" means those residual cyclic oligomers that remain in the polymer species after the polycondensation process and have a molecular mass (MM) below 1000. Summary of the Invention

[0013] One aspect of the present invention comprises a mixed aliphatic-aromatic polyester comprising:

[0014] (a) a dicarboxylic acid component, the dicarboxylic acid component comprising:

[0015] (a1) 40 to 80 % by mole of units derived from at least one aromatic dicarboxylic acid;

[0016] (a2) 20 to 60 % by mole of units derived from at least three saturated aliphatic C4-C24 dicarboxylic acids, their C1-C24 alkyl esters, their salts and mixtures thereof, azelaic acid and succinic acid being always present.

[0017] (b) Aliphatic diol component.

[0018] Another aspect of the present invention is a film obtained from the above-mentioned mixed aliphatic aromatic polyester, preferably a film obtained from a mixture of the above-mentioned mixed aliphatic aromatic polyester with other polymers and possibly other components. DETAILED DESCRIPTION

[0019] In a preferred aspect of the present invention, the mixed aliphatic-aromatic polyester is characterized in that it contains residual mixed cyclic oligomers in an amount of 1.0% to 4.0%, wherein the residual mixed cyclic oligomers are characterized in that the ratio between cyclic oligomers containing at least two types of aliphatic dicarboxylic acid units with an MM below 1000 and cyclic oligomers containing only one type of aliphatic dicarboxylic acid units with an MM below 1000 is from 0.30 to 1.40, more preferably from 0.40 to 1.20, even more preferably from 0.80 to 1.14, and is further characterized in that the main saturated aliphatic dicarboxylic acid in component a2 is from 40% by mole to 92% by mole compared to the sum of all other saturated aliphatic dicarboxylic acids.

[0020] The term "primarily saturated aliphatic dicarboxylic acid" in the present invention is intended to be used when the ratio of the acids is not equimolar, and thus the term designates a saturated aliphatic dicarboxylic acid present in a greater molar percentage than the percentage of each of the other saturated aliphatic dicarboxylic acids.

[0021] Advantageously, the residual mixed cyclic oligomer content is between 2% and 3.5%.

[0022] As regards the mixed aliphatic-aromatic polyesters produced by the process according to the invention, these comprise a diol component (component b) derived from at least one aliphatic diol selected from 1,2-ethanediol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, 2-methyl-1,3-propanediol, dianhydrosorbitol, dianhydromannitol, dianhydroiditol, diols having a molecular weight of 100 to 4000, such as polyethylene glycol, polypropylene glycol, and mixtures thereof.

[0023] Preferably, the diol component comprises at least 50% by mole of one or more diols selected from 1,2-ethylene glycol, 1,3-propylene glycol, and 1,4-butanediol.

[0024] More preferably, the diol component comprises or consists of 1,2-ethanediol, 1,4-butanediol, or a mixture thereof.

[0025] Even more preferably, the diol component comprises or consists of 1,4-butanediol.

[0026] The dicarboxylic acid component of the polyester produced by the process according to the invention comprises, relative to the total dicarboxylic acid component, 40% to 80% by mole, preferably 40% to 75% by mole, more preferably 42% to 52% by mole, even more preferably 45% to 49% by mole of units derived from at least one aromatic dicarboxylic acid (component a1) and 20% to 60% by mole, preferably 25% to 60% by mole, more preferably 48% to 58% by mole, even more preferably 51% to 55% by mole of units derived from at least three saturated aliphatic dicarboxylic acids (component a2). The dicarboxylic acid component is further characterized in that the main saturated aliphatic dicarboxylic acid in component a2 accounts for less than 92% by mole relative to the sum of all other saturated aliphatic dicarboxylic acids and is greater than 40% by mole relative to the sum of all saturated aliphatic dicarboxylic acids.

[0027] The aromatic dicarboxylic acid is advantageously chosen from terephthalic acid, isophthalic acid, 2,5-furandicarboxylic acid, esters, salts and mixtures thereof.

[0028] In a preferred embodiment, the aromatic dicarboxylic acid comprises:

[0029] - 1 to 99%, preferably 5 to 95% and more preferably 10 to 80% by mole of terephthalic acid, its esters or salts;

[0030] - 99% to 1%, preferably 95% to 5%, and more preferably 90% to 20% by mole of 2,5-furandicarboxylic acid, an ester or a salt thereof.

[0031] In a particularly preferred form of the invention, the aromatic dicarboxylic acid is terephthalic acid, its esters and salts.

[0032] Regarding component a2, the mole % of saturated aliphatic carboxylic acids of renewable origin is preferably greater than 30%, more preferably greater than 40%, even more advantageously greater than 50% of the sum of the saturated dicarboxylic acids.

[0033] The succinic acid in component a2 is also characterized by being 5 to 67% by mole of the sum of all other saturated aliphatic dicarboxylic acids, preferably 10 to 50% by mole of the sum of all other saturated aliphatic dicarboxylic acids, even more preferably 20 to 35% by mole.

[0034] The azelaic acid in component a2 is preferably 3 to 92 mol %, preferably 10 to 50 mol %, even more preferably 15 to 35 mol %, relative to the sum of all other saturated aliphatic dicarboxylic acids.

[0035] The aliphatic dicarboxylic acids are advantageously selected from: saturated C4-C24, preferably C4-C13, more preferably C4-C11 aliphatic dicarboxylic acids; their C1-C24, preferably C1-C4 alkyl esters; their salts; and mixtures thereof.

[0036] In a preferred embodiment of the present invention, the aliphatic dicarboxylic acid is selected from the group consisting of succinic acid, glutaric acid, 2-methylglutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassyl acid, and C1-24 alkyl esters thereof.

[0037] In a preferred embodiment of the present invention, the main saturated aliphatic dicarboxylic acid is at least 40% by mole, preferably more than 60% by mole, more preferably more than 65% by mole, and even more preferably more than 85% by mole, relative to the sum of all saturated aliphatic dicarboxylic acids. The main saturated aliphatic dicarboxylic acid is preferably selected from the group consisting of succinic acid, adipic acid, azelaic acid, sebacic acid, brassyl acid; their C1-C24, preferably C1-C4 esters; their salts; and mixtures thereof, however, succinic acid and azelaic acid are always present.

[0038] In a preferred embodiment of the process according to the invention, the mixed aliphatic-aromatic polyester produced is advantageously selected from:

[0039] (A) Polyesters comprising repeating units derived from aromatic dicarboxylic acids of the phthalic acid type, preferably terephthalic acid, aromatic dicarboxylic acids and aliphatic diols (AAPE-A), characterized in that the aromatic unit content is from 42 to 60% by mole, preferably from 45 to 49.5% by mole, relative to the total moles of the dicarboxylic acid component.

[0040] AAPE-A polyester is preferably selected from the group consisting of: poly(1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene terephthalate), poly(1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene sebacate-co-1,4-butylene terephthalate). -butylene glycol esters), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene brassyl acid-co-1,4-butylene terephthalate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene sebacate-co- 1,4-butylene terephthalate), poly(1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene adipate-co-1,4-butylene brassyl acid-co-1,4-butylene terephthalate), poly(1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene brassyl acid-co-1,4-butylene terephthalate), poly(1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene brassyl acid -butylene glycol ester-co-1,4-butylene sebacate-co-1,4-butylene terephthalate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene sebacate-co-1,4-butylene brassyl acid-co-1,4-butylene terephthalate).

[0041] (B) A polyester comprising repeating units derived from an aromatic heterocyclic dicarboxylic acid compound, preferably 2,5-furandicarboxylic acid, an aromatic dicarboxylic acid and an aliphatic diol (AAPE-B), characterized in that the content of aromatic units is from 40 to 80% by mole, preferably from 40 to 75% by mole, relative to the total moles of the dicarboxylic acid component.

[0042] The AAPE-B polyester is preferably selected from the group consisting of poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene adipate-co-2,5-furandicarboxylate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene sebacate-co-2,5-furandicarboxylate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene brassyl acid-co-2,5-furandicarboxylate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene sebacate-co- -2,5-furandicarboxylate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene adipate-co-brazilyl acid-co-2,5-furandicarboxylate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-brazilyl acid-co-1,4-butylene sebacate-co-2,5-furandicarboxylate), poly(1,4-butylene azelaic acid-co-1,4-butylene succinate-co-1,4-butylene adipate-co-1,4-butylene sebacate-co-brazilyl acid-co-2,5-furandicarboxylate).

[0043] In a preferred aspect of the present invention, the polyester produced by the process according to the invention is characterized by a content of residual mixed cyclic oligomers of 1.0% to 4.0%, wherein the oligomers are characterized by a ratio between cyclic oligomers comprising at least two types of aliphatic dicarboxylic acid units with an MM below 1000 and cyclic oligomers comprising only one type of aliphatic dicarboxylic acid units with an MM below 1000 of 0.30 to 1.40, more preferably from 0.40 to 1.20, even more preferably from 0.81 to 1.14, and is further characterized in that the main saturated aliphatic dicarboxylic acid in component a2 is less than 92% by mole relative to the sum of all other saturated aliphatic dicarboxylic acids and greater than 40% by mole relative to the sum of all other saturated aliphatic dicarboxylic acids.

[0044] In a preferred aspect of the present invention, the cyclic oligomer comprising only one type of aliphatic dicarboxylic acid unit is (ADA-BDO)2, (AZA-BDO)2, (SEBA-BDO)2, (BRA-BDO)2, (SUC-BDO)2, (ADA-BDO)3, (AZA-BDO)3, (SEBA-BDO)3, (BRA-BDO)3, (SUC-BDO)3, (ADA-BDO)4, (AZA-BDO)4, (SUC-BDO)4.

[0045] In the direction of one preference in the book, it includes very few types of aliphatic binary acids and low-carbon materials (ADA-BDO-AZA-BDO), (ADA-BDO-SEBA-BDO), (ADA-BDO-BRA-BDO) (ADA-BDO-SUC-BDO), (AZA-BDO-SEBA-BDO), (AZA-BDO-BRA-BDO), (AZA-BDO-SUC-BDO), (SEBA-BDO-BRA-BDO), (SEBA-BDO-SUC-BDO), (SUC-BDO-BRA-BDO), (ADA-BDO)2-(AZA-BDO) , (ADA-BDO)-(AZA-BDO)2 , (ADA-BDO)2-(SEBA-BDO) , (ADA-BDO)-(SEBA-BDO)2 , (ADA-BDO)2-(BRA-BDO) , (ADA-BDO)-(BRA-BDO)2 , (ADA-BDO)2-(SUC-BDO) , (ADA-BDO)-(SUC-BDO)2, (AZA-BDO)2-(SUC-BDO), (AZA-BDO)-(SUC-BDO)2, (SEB-BDO)2-(SUC-BDO), (SEB-BDO)-(SUC-BDO)2, (BRA-BDO)2-(SUC-BDO), (BRA-BDO)-(SUC-BDO)2 , (AZA-BDO)2-(SEBA-BDO) , (AZA-BDO)-(SEBA-BDO)2 , (AZA-BDO)2-(BRA-BDO) , (AZA-BDO)-(BRA-BDO)2 , (SEBA-BDO)2-(BRA-BDO) , (SEBA-BDO)-(BRA-BDO)2 , (ADA-BDO)-(PTA-BDO)-(AZ-BDO) , (ADA-BDO)-(PTA-BDO)-(SEBA-BDO) , (ADA-BDO)-(PTA-BDO)-(BRA-BDO) , (SEBA-BDO)-(PTA-BDO)-(AZ-BDO)(BRA-BDO)-(PTA-BDO)-(AZ-BDO), (BRA-BDO)-(PTA-BDO)-(SEBA-BDO) , (ADA-BDO)-(PTA-BDO)-(SUC-BDO) , (AZA-BDO)-(PTA-BDO)-(SUC-BDO), (SEB-BDO)-(PTA-BDO)-(SUC-BDO) , (BRA-BDO)-(PTA-BDO)-(SUC-BDO), (ADA-BDO)-(AZA-BDO)-(SEBA-BDO) , (ADA-BDO)-(AZA-BDO)-(BRA-BDO) , (ADA-BDO)-(BRA-BDO)-(SEBA-BDO) , (BRA-BDO)-(AZA-BDO)-(SEBA-BDO) , (ADA-BDO)-(AZA-BDO)-(SUC-BDO) , (SEBA-BDO)-(AZA-BDO)-(SUC-BDO) , (BRA-BDO)-(AZA-BDO)-(SUC-BDO) , (SEBA-BDO)-(BRA-BDO)-(SUC-BDO) , (SEBA-BDO)-(ADA-BDO)-(SUC-BDO), (ADA-BDO)2-(AZA-BDO)2, (ADA-BDO)2-(SEBA-BDO)2, (ADA-BDO)2-(BRA-BDO)2; wherein ADA is the ester of adipic acid and a diol component, AZA is the ester of azelaic acid and a diol component, SUC is the ester of succinic acid and a diol component, SEBA is the ester of sebacic acid and a diol component, BRA is the ester of brassylic acid and a diol component, PTA is the ester of terephthalic acid, and BDO is the diol component 1,4-butanediol.

[0046] As an example, the cyclic oligomer (SUC-BDO-AZA-BDO) comprises butylene succinate units and butylene azelate units.

[0047] In addition to the dicarboxylic acid component and the diol component, the mixed aliphatic-aromatic polyester according to the invention preferably comprises repeating units derived from at least one hydroxy acid or the corresponding lactone in an amount of 0 to 49%, preferably 0 to 30%, by mole, relative to the total moles of the dicarboxylic acid component.

[0048] Examples of suitable hydroxy acids are glycolic acid or glycolide, hydroxybutyric acid, hydroxycaproic acid, hydroxyvaleric acid, 7-hydroxyheptanoic acid, 8-hydroxycaproic acid, 9-hydroxynonanoic acid, lactic acid or lactide.

[0049] The hydroxy acids can be inserted into the chain as such or they can be pre-reacted with diacids or diols.

[0050] Mixed aliphatic-aromatic polyesters are produced in the following process, which comprises the following stages:

[0051] 1. subjecting a mixture comprising an aliphatic diol, at least one aromatic dicarboxylic acid and at least three saturated aliphatic dicarboxylic acids, their esters, salts or derivatives to esterification and / or transesterification to produce oligomers;

[0052] 2. Polycondensing the oligomer obtained from step 1 in the presence of a catalyst possibly containing zirconium or a mixture thereof and a phosphorus-containing compound belonging to the family of organic phosphates or phosphites, at a temperature ranging from 220° C. to 260° C. and a pressure ranging from 0.5 mbar to 350 mbar.

[0053] Advantageously, the compound comprising phosphorus is chosen from compounds of formula (1) or (2):

[0054]

[0055] Wherein R1, R2 and R3 can be selected from any one of the following: H, C1-C20 alkyl or cycloalkyl, C6-C20 aryl, alkylaryl, or polyalkylene oxide or polyalkylene oxide chain.

[0056] The catalyst comprises a mixture of at least one titanium-containing compound and a titanium to phosphorus ratio of 2 to 20, preferably 3 to 15.

[0057] In the process according to the invention for preparing mixed aliphatic-aromatic polyesters, the hydroxy acid is advantageously added during the esterification step.

[0058] Long molecules having two functional groups, including long molecules having non-terminal functional groups, may also be present in an amount of not more than 10% by mole relative to the total moles of the dicarboxylic acid component.

[0059] Examples are dimer acid, ricinoleic acid and acids incorporating epoxy functions, and also polyoxyethylenes having a molecular weight of 200 to 10,000.

[0060] In the process according to the invention for preparing mixed aliphatic-aromatic polyesters, these long molecules having two functional groups are advantageously added during the esterification step.

[0061] Diamines, amino acids and amino alcohols may also be present in percentages up to 30 mole percent of the total moles of the dicarboxylic acid component.

[0062] In the process according to the invention for preparing mixed aliphatic-aromatic polyesters, such diamines, amino acids and amino alcohols are advantageously added during the esterification step.

[0063] During the esterification step of the process for preparing mixed aliphatic-aromatic polyesters according to the present invention, one or more molecules characterized by having 3 or more reactive functional groups may be added in an amount of 0.02 to 3% by mole relative to the total moles of the dicarboxylic acid component (and any hydroxy acids) to obtain a branched product.

[0064] Examples of such molecules are glycerol, pentaerythritol, trimethylolpropane, citric acid, dipentaerythritol, monoanhydrosorbitol, monoanhydromannitol, triglycerides or polyglycerols.

[0065] The molecular weight Mn of the mixed aromatic-aliphatic polyesters according to the invention is preferably greater than 20,000, more preferably >30,000, even more preferably >50,000.

[0066] As for the polydispersity index of the molecular weight Mw / Mn, it is preferably from 1.5 to 10, more preferably from 1.6 to 5, and even more preferably from 1.8 to 2.5.

[0067] The molecular weights Mn and Mw can be measured by gel permeation chromatography (GPC).

[0068] The assay was performed using a chromatography system maintained at 40°C, using a set of two columns in series (particle sizes of 5 μm and 3 μm with mixed pore size), a refractive index detector, chloroform as eluent (flow rate 0.5 ml / min), and polystyrene as a reference standard.

[0069] The thermal properties of the mixed aromatic-aliphatic polyesters according to the present invention have been determined by differential scanning calorimetry (DSC) using a Perkin Elmer Pyris Diamond calorimeter under the conditions given below:

[0070] - Isothermal at -80°C for 60 seconds

[0071] - Scan 1 from -80°C to 200°C at 20°C / min

[0072] -Isothermal at 200°C for 60 seconds

[0073] - Perform the second scan from 200°C to -80°C at 10°C / min

[0074] - Isothermal at -80°C for 60 seconds

[0075] - Perform the third scan from -80°C to 200°C at 20°C / min

[0076] At the glass transition temperature, there is a change in specific heat (ΔCp), which can be detected as a jump and a change in the slope of the DSC curve. TM Software (specifically designed for processing DSC graphs) draws two lines that ideally continue the baseline before and after the transition and the tangent line of the maximum slope point of the curve, and calculates the glass transition temperature (Tg) from the second scan. The glass transition temperature in the present invention is defined as the point where half of the heat capacity increase is reached (midpoint temperature).

[0077] In the process of patent WO2016 / 050963, by using a catalyst comprising a mixture of at least one titanium-containing compound and at least one zirconium-containing compound, wherein the Ti / (Ti+Zr) weight ratio in the polycondensation step is higher than 0.01 and lower than 0.70, preferably higher than 0.02 and lower than 0.60, a lower amount of residual cyclic oligomers can be obtained after extraction of the polycondensation distillate.

[0078] In particular, the content of these residual cyclic oligomers is measured gravimetrically after separation from the polycondensation distillate.

[0079] In contrast, in the present invention, the amount of residual mixed cyclic oligomers remaining in the formed polyester can be controlled by using a mixture of a phosphorus-containing compound having a titanium to phosphorus ratio of 2 to 20, preferably 3 to 15, and at least one titanium-containing compound, wherein the ratio of cyclic oligomers containing at least two types of dicarboxylic aliphatic units having an MM below 1000 to cyclic oligomers containing only one type of dicarboxylic aliphatic units having an MM below 1000 is from 0.30 to 1.40.

[0080] The extracted residual mixed cyclic oligomers were determined gravimetrically.

[0081] An accurately weighed sample of approximately 30 g of the polymer was extracted with 150 ml of acetonitrile at 40°C for 96 hours. The liquid phase was recovered by filtration and the particles on the filter were washed with 25 ml of acetonitrile. The two aliquots were combined in a 250 ml volumetric flask and the solvent was evaporated to constant weight on a rotary evaporator at 45°C. The composition of the residual mixed cyclic oligomers was analyzed by dissolving the oligomers in 1 ml of THF and diluting with acetonitrile to a concentration of approximately 1000 ppm. 100 μl of the acetonitrile / THF solution was diluted with 800 μl of methanol and 100 μl of 0.1% N aqueous ammonium acetate.

[0082] The analysis was performed by HPLC-MS using a Thermo Accela 1250 HPLC instrument connected to a Thermo LCQ Fleet mass spectrometer in ESI+ mode.

[0083] Materials were separated according to the characteristics described in Table 1 using a Phenomenex Luna Omega C18 PS 100 x 2.1 mm 1.6 μm column for elution.

[0084]

[0085] Table 1: Elution characteristics

[0086] Oligomers were identified based on the molecular mass (MM) of protonated and ammonia adducts. The percentage of residual mixed cyclic oligomers was determined by processing the chromatogram in basic peak mode and integrating the species identified as cyclic oligomers based on molecular mass. The ratio of the sum of the areas of the peaks assigned to oligomers containing at least two aliphatic acids with an MM less than 1000 to the sum of the areas of the peaks assigned to cyclic oligomers containing only one type of aliphatic dicarboxylic acid unit with an MM less than 1000 represents the fraction of mixed cyclic oligomers.

[0087] The terminal acid group content of the mixed aromatic-aliphatic polyester is preferably less than 100 meq / kg, preferably less than 60 meq / kg, and even more preferably less than 40 meq / kg.

[0088] The content of terminal acid groups can be measured as follows: 1.5 g to 3 g of polyester are placed in a 100 ml flask together with 60 ml of chloroform.

[0089] After the polyester was completely dissolved, 25 ml of 2-propanol was added, and 1 ml of deionized water was added immediately before analysis.

[0090] The resulting solution was titrated with a previously standardized solution of KOH in ethanol.

[0091] The endpoint of the titration is determined using an appropriate indicator such as a glass electrode for acid-base titrations in non-aqueous solvents.

[0092] The content of terminal acid groups was calculated from the consumption of KOH solution in ethanol according to the following equation:

[0093]

[0094] Where: Veq = ml of KOH solution in ethanol at the endpoint of the sample titration; Vb = ml of KOH solution in ethanol required to achieve pH = 9.5 during the blank titration; T = concentration of KOH solution in ethanol in mol / L; P = weight of the sample in grams.

[0095] When used in typical applications of plastics (e.g., bubble film formation, injection molding, foam products, etc.), the melt mass flow rate (MFR) of the mixed aliphatic-aromatic polyester according to the present invention is preferably 500 g / 10 min to 1 g / 10 min, more preferably 100 g / 10 min to 2 g / 10 min, and even more preferably 80 g / 10 min to 3 g / 10 min. An MFR of 25 g / 10 min to 3.5 g / 10 min (measured according to ISO 1133-1 at 190° C. / 2.16 kg) can be advantageously used.

[0096] Preferably, the mixed aliphatic-aromatic polyester according to the present invention has an intrinsic viscosity (measured with an Ubbelohde viscometer at 25° C. for a solution in CHCl 3 at a concentration of 0.2 g / dl) of greater than 0.4 dl / g, preferably from 0.4 dl / g to 2 dl / g, more preferably from 0.7 dl / g to 1.5 dl / g.

[0097] Preferably, the mixed aliphatic-aromatic polyesters according to the present invention are biodegradable.

[0098] In the meaning of the present invention, a biodegradable polymer is understood to mean a biodegradable polymer having a relative biodegradability relative to microcrystalline cellulose of 90% or more after 180 days according to ISO 14855-1 (2013).

[0099] In a preferred aspect of the present invention, the mixed aliphatic-aromatic polyester comprising 45 to 49% by mole of units derived from at least one aromatic dicarboxylic acid (component a1), based on the total dicarboxylic acid component, and 20 to 60% by mole of units derived from succinic acid, based on the total dicarboxylic acid component, is biodegradable in industrial composting according to standard EN 13432.

[0100] Preferably, the mixed aliphatic-aromatic polyesters according to the invention can be used in a mixture with one or more polymers of synthetic or natural origin, whether biodegradable or not, which can also be obtained by a reactive extrusion process.

[0101] In particular, the mixed aliphatic aromatic polyesters according to the present invention are particularly suitable for the production of films when mixed with other polymers and preferably with a suitable combination of other components. Advantageously, such films exhibit excellent mechanical properties.

[0102] In a particularly preferred aspect of the present invention, films made from a mixture of mixed aromatic aliphatic polyesters comprise:

[0103] i) 30 to 95% by weight, relative to the sum of components i. to v., of at least one mixed aliphatic aromatic polyester;

[0104] ii) 0.1% to 50% by weight, relative to the sum of components i. to v., of at least one polymer of natural origin;

[0105] iii) 0% to 40% of at least one polyhydroxyalkanoate, relative to the sum of components i. to v.;

[0106] iv) 0% to 15% of at least one inorganic filler, relative to the sum of components i. to v.;

[0107] v) 0% to 5% by weight, relative to the sum of components i. to v., of at least one crosslinker and / or chain extender comprising at least one difunctional and / or polyfunctional compound containing isocyanates, peroxides, carbodiimides, isocyanurates, oxazolines, epoxides, anhydrides, divinyl ethers and mixtures thereof.

[0108] The polymer of natural origin (component ii) is selected from the group comprising starch, cellulose, chitin, chitosan, alginates, proteins such as gluten, zein, casein, collagen, gelatin, natural gums, rosin acid and its derivatives, lignin itself, or purified, hydrolyzed, alkalized, etc. lignin or its derivatives.

[0109] Starches and celluloses may be modified, and these include starch or cellulose esters having a degree of substitution of 0.2 to 2.5, hydroxypropylated starches, starches modified with fatty chains, and cellophane.

[0110] Component (ii) is preferably starch.

[0111] Starch can be used in both destructurized and gelatinized forms or as a filler.

[0112] Modified starch is understood to mean starch as described in patents EP 0 118 240 and EP 0 327 505, in particular starch treated in such a way that it does not exhibit a so-called "Maltese cross" in polarized light under an optical microscope and does not exhibit a so-called "ghost image" under phase contrast under an optical microscope.

[0113] The starch may be the continuous or dispersed phase, or it may be in a co-continuous form.

[0114] In the case of dispersed starch, the starch granule size is measured in a cross section relative to the direction of flow during extrusion (or in any case relative to the direction of film production).

[0115] The granule size of the starch was measured from the two-dimensional shapes generated by transverse cross-sections. The average starch granule size was calculated as the arithmetic mean of the granule sizes.

[0116] If the particle has a circular cross-section, the particle size corresponds to the diameter of the circle.

[0117] In the case of particles having an elliptical cross-section or otherwise resembling an ellipse, the particle size (d) is calculated using the following formula:

[0118]

[0119] where d1 is the minor axis of an ellipse to which the particle can be compared and d2 is its major axis.

[0120] The starch granules are characterised by an arithmetic mean diameter of less than 1 micron, and more preferably less than 0.5 μm, measured as described above.

[0121] Regarding component iii of the above membrane, it optionally comprises at least one polyhydroxyalkanoate, which preferably represents 0% to 40%, more preferably 2% to 37%, and even more preferably 10% to 25% of the sum of components i. to v.

[0122] The polyhydroxyalkanoate is most preferably selected from the group consisting of polyesters of lactic acid, poly-ε-caprolactone, polyhydroxybutyrate, polyhydroxybutyrate-valerate, polyhydroxybutyrate-propionate, polyhydroxybutyrate-hexanoate, polyhydroxybutyrate-decanoate, polyhydroxybutyrate-dodecanoate, polyhydroxybutyrate-hexadecanoate, polyhydroxybutyrate-octadecanoate, poly-3-hydroxybutyrate-4-hydroxybutyrate. Preferably, the polyhydroxyalkanoate comprises at least 80% by weight of one or more polyesters of lactic acid.

[0123] In a preferred embodiment, the lactic acid polyester is selected from the group consisting of poly-L-lactic acid, poly-D-lactic acid, poly-DL-lactic acid stereocomplexes, copolymers containing more than 50% by mole of said lactic acid polyesters, or mixtures thereof. Particularly preferred are lactic acid polyesters containing at least 95% by weight of repeating units derived from L-lactic acid or D-lactic acid or mixtures thereof, having a molecular weight Mw higher than 50,000 and a shear viscosity (according to ASTM standard D3835 at T = 190 ° C, shear rate = 1000 s) of 50 to 500 Pa.s, preferably 100 to 300 Pa.s. -1 , D = 1mm, L / D = 10).

[0124] In a particularly preferred embodiment, the lactic acid polyester comprises at least 95% by weight of units derived from L-lactic acid, <5% of repeating units derived from D-lactic acid, has a melting point in the range of 135°C to 180°C, a glass transition temperature (Tg) in the range of 55°C to 65°C and an MFR in the range of 1 g / 10 min to 50 g / 10 min (measured according to ISO 1133-1 at 190°C and 2.16 kg). Commercial examples of lactic acid polyesters having these properties include the biopolymer product Ingeo TM 4043D, 3250D and 6202D.

[0125] As for the inorganic filler (component iv) of the above-mentioned membrane, it is present in an amount of 0% to 15% by weight, preferably 0.1% to 8%, even more preferably 3% to 5% by weight, relative to the sum of components i. to v. The inorganic filler is preferably chosen from kaolin, barite, clay, talc, calcium and magnesium, calcium carbonate, iron and lead carbonates, aluminum hydroxide, diatomaceous earth, aluminum sulfate, barium sulfate, silica, mica, titanium dioxide and wollastonite.

[0126] In a preferred embodiment of the present invention, the inorganic filler comprises talc, mica, calcium carbonate, or a mixture thereof, present in the form of particles having an average arithmetic diameter measured relative to the major axis of the particles of less than 10 microns, more preferably an average arithmetic diameter of less than 2 microns (measured according to ASTM 13320).

[0127] As far as the crosslinker and / or chain extender (component v) of the above-mentioned membrane is concerned, it is present at 0 to 5% by weight, preferably 0 to 0.5% by weight, relative to the sum of components i. to v.

[0128] The crosslinking agent and / or chain extender is selected from difunctional and / or polyfunctional compounds with a group selected from the group consisting of isocyanates, peroxides, carbodiimides, isocyanurates, oxazoline, epoxide, anhydride or divinyl ether or a mixture thereof.

[0129] Particularly preferred are mixtures of difunctional and / or polyfunctional compounds carrying isocyanate groups and difunctional and / or polyfunctional compounds carrying epoxide groups, even more preferably containing at least 75% by weight of difunctional and / or polyfunctional compounds carrying isocyanate groups.

[0130] The compound having a difunctional group and a polyfunctional group containing an isocyanate group is preferably selected from p-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4-diphenylmethane diisocyanate, 1,3-phenylene-4-chlorodiisocyanate, 1,5-naphthalene diisocyanate, 4,4-diphenylene diisocyanate, 3,3'-dimethyl-4,4-diphenylmethane diisocyanate, 3-methyl-4,4'-diphenylmethane diisocyanate, diphenyl ester diisocyanate, 2,4-cyclohexane diisocyanate, 2,3-cyclohexane diisocyanate, The isocyanate group-containing compound is 4,4-diphenylmethane diisocyanate, 1,3-diisocyanate, 1,2-diisocyanate, and mixtures thereof. In a preferred embodiment, the isocyanate group-containing compound is 4,4-diphenylmethane diisocyanate.

[0131] As regards the difunctional and polyfunctional compounds bearing peroxide groups, these are preferably chosen from: benzoyl peroxide, lauroyl peroxide, isononanoyl peroxide, di-(tert-butylperoxyisopropyl)benzene, tert-butyl peroxide, dicumyl peroxide, α,α′-di-(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hex-3-yne, di(4-tert-butylcyclohexyl)peroxydicarbonate, dihexadecyl peroxydicarbonate, dimyristyl peroxydicarbonate, 3,6,9-triethyl-3,6,9-trimethyl-1,4,7-triperoxynonane, di(2-ethylhexyl)peroxydicarbonate and mixtures thereof.

[0132] The difunctional and polyfunctional compounds with carbodiimide groups preferably used in the composition according to the invention are selected from the group consisting of: poly(cyclooctylenecarbodiimide), poly(1,4-dimethylenecyclohexylenecarbodiimide), poly(cyclohexylenecarbodiimide), poly(ethylenecarbodiimide), poly(butylenecarbodiimide), poly(isobutylenecarbodiimide), poly(nonylenecarbodiimide), poly(dodecylenecarbodiimide), poly(neopentylenecarbodiimide), poly(1,4-dimethylenephenylenecarbodiimide), poly(2,2',6,6'-tetraisopropyldiphenylenecarbodiimide) Poly(2,4,6-triisopropyl-1,3-phenylenecarbodiimide) Poly(2,6-diisopropyl-1,3-phenylenecarbodiimide) Poly(tolylcarbodiimide), poly(4,4'-diphenylmethanecarbodiimide), poly(3,3'-dimethyl-4,4'-biphenylenecarbodiimide), poly(p-phenylenecarbodiimide), poly(m-phenylenecarbodiimide), poly(3,3'-dimethyl-4,4'-diphenylmethanecarbodiimide), poly(naphthylenecarbodiimide), poly(isophoronecarbodiimide), poly(cumenecarbodiimide), p-phenylenebis(ethylcarbodiimide), 1,6-hexamethylenebis(ethylcarbodiimide), 1,8-octamethylenebis(ethylcarbodiimide), 1,10-decamethylenebis(ethylcarbodiimide), 1,12-decamethylenebis(ethylcarbodiimide), and mixtures thereof.

[0133] Examples of difunctional and polyfunctional compounds carrying epoxy groups that can be advantageously used in the composition according to the invention are all polyepoxides from epoxidized oils and / or from styrene-glycidyl ether-methyl methacrylate or glycidyl ether-methyl methacrylate, comprised in the molecular weight range of 1000 to 10000 and having an epoxide number per molecule of 1 to 30 and preferably 5 to 25, the epoxides being selected from the group comprising diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polyglycerol polyglycidyl ether, 2-butylene oxide, polyglycerol polyglycidyl ether, isoprene diepoxide and cycloaliphatic diepoxides, 1,4-cyclohexanedimethanol diglycidyl ether, glycidyl 2-methylphenyl ether, glycerol propoxylated triglycidyl ether, glycerol propoxylated triglycidyl ether, tetraglycidyl ether of meta-xylenediamine and diglycidyl ether of bisphenol A, and mixtures thereof.

[0134] Together with compounds such as those described above with isocyanate groups, peroxide groups, carbodiimide groups, isocyanurate groups, The difunctional and polyfunctional compounds of oxazoline, epoxide, anhydride and divinyl ether groups may also use a catalyst to increase the reactivity of the reactive groups. In the case of polyepoxides, fatty acid salts may be preferably used, and calcium stearate and zinc stearate may be even more preferably used.

[0135] In a particularly preferred embodiment of the present invention, the crosslinking agent and / or chain extender comprises a compound with isocyanate groups, preferably 4,4-diphenylmethane-diisocyanate; and / or a compound with carbodiimide groups; and / or a compound with epoxy groups, preferably of the styrene-glycidyl ether methyl methacrylate type.

[0136] In addition to film production, the mixed aliphatic-aromatic polyesters according to the invention are extremely suitable for use alone or in mixtures with other polymers in many practical applications to produce products such as, for example, fibers, nonwovens, foils, prints, thermoformed articles, blown articles, expanded articles and laminated articles, including those produced by extrusion coating techniques.

[0137] Examples of products according to the invention comprising mixed aliphatic-aromatic polyesters are:

[0138] - Films, including uniaxially oriented and biaxially oriented films, and multilayer films with other polymeric materials;

[0139] - as mulch films for use in agricultural fields;

[0140] - stretch films, including those for food, for bales in agriculture, and for wrapping waste;

[0141] -Bags and liners for collecting organic materials such as food scraps and grass clippings;

[0142] - Both single-layer and multi-layer thermoformed food packaging, such as containers for milk, yogurt, meat, beverages, etc.;

[0143] - coatings obtained using extrusion coating technology;

[0144] - multilayer laminates with layers of cardboard, plastic, aluminum, metal films;

[0145] - For the production of expanded or expandable beads in special sintered forms;

[0146] - expanded and semi-expanded products, including expanded masses formed from pre-expanded granules;

[0147] - Expanded foam, thermoformed expanded sheet, and containers made therefrom for food packaging;

[0148] -Containers generally used for fruits and vegetables;

[0149] - Compositions containing as fillers gelatinized starch, destructurized starch and / or complex starch, native starch, flour, other fillers of natural, plant or inorganic origin.

[0150] - Fibers, microfibers, composite fibers with a core consisting of a rigid polymer such as PLA, PET, PTT, etc. and a sheath of the material according to the invention, dablens, fibers with various cross-sections from round to multilobal, flocked fabrics, woven and nonwoven fabrics or spunbonded or thermally bonded fabrics for use in the health, hygiene, agriculture and clothing sectors.

[0151] They can also be used in applications as a replacement for plasticized PVC.

[0152] The process according to the invention for preparing mixed aliphatic-aromatic polyesters comprises an esterification or transesterification stage and a polycondensation stage, and is characterized in that the polycondensation stage is carried out in the presence of a catalyst comprising at least one titanium-containing compound and possibly at least one zirconium-containing compound. When the zirconium-containing compound is present, the Ti / (Ti+Zr) weight ratio is equal to or higher than 0.01 and equal to or lower than 0.7, preferably higher than 0.02 and equal to or lower than 0.60.

[0153] Furthermore, the catalyst is used in a mixture with a phosphorus compound belonging to the family of organic phosphates or phosphites.

[0154] Advantageously, the compound comprising phosphorus is chosen from compounds of formula (1) or (2):

[0155]

[0156] Wherein R1, R2 and R3 can be selected from any one of the following: H, C1-C20 alkyl or cycloalkyl, C6-C20 aryl, alkylaryl, or polyalkylene oxide or polyalkylene oxide chain.

[0157] In a particularly preferred aspect, the phosphorus-containing compound is trioctyl phosphate.

[0158] In a preferred aspect of the process, the catalyst comprises a mixture of at least one titanium-containing compound and the weight ratio of titanium to phosphorus is from 2 to 20, preferably from 3 to 15.

[0159] The esterification / transesterification stage is preferably fed with a molar ratio of aliphatic diol to dicarboxylic acid, esters and salts thereof of preferably 1 to 2.5, preferably 1.05 to 1.9.

[0160] The dicarboxylic acids, their esters or salts, the aliphatic diols and any other comonomers constituting the polyester may be fed separately to this stage, thereby being mixed in the reactor, or alternatively premixed, preferably at T < 70° C., before being sent to the reactor.

[0161] It is also possible to premix some of the components and subsequently change their composition, for example during the esterification / transesterification reaction.

[0162] In the case of polyesters in which the dicarboxylic acid component comprises repeating units derived from several dicarboxylic acids, whether aliphatic or aromatic, it is also possible to premix some of these with the aliphatic diol (preferably at T < 70°C) and thereby add the remaining portion of the dicarboxylic acid, diol and any other comonomers to the esterification / transesterification reactor.

[0163] The esterification / transesterification stage of the process is advantageously carried out at a temperature of 200 to 250° C. and a pressure of 0.7 to 1.5 bar, preferably in the presence of an esterification / transesterification catalyst.

[0164] The esterification / transesterification catalyst, which may also advantageously serve as a component of the catalyst in the polycondensation stage, may in turn be fed directly to the esterification / transesterification reactor, or may also be first dissolved in an aliquot of one or more of the dicarboxylic acid, its ester or salt, and / or the aliphatic diol to facilitate dispersion of the reaction mixture and make it more homogeneous.

[0165] The esterification / transesterification catalyst is selected from: organometallic tin compounds, such as stannic acid derivatives; titanium compounds, such as titanates such as tetrabutyl orthotitanate or tetra(isopropyl)orthotitanate; zirconium compounds, such as zirconates such as tetrabutyl orthozirconate or tetra(isopropyl)orthozirconate; antimony compounds; aluminum, such as Al-triisopropyl; and zinc compounds; and mixtures thereof.

[0166] As regards the organometallic esterification / transesterification catalysts of the type mentioned above, they are present during the esterification / transesterification stage of the above-mentioned process at a concentration of preferably 12 to 120 ppm of metal relative to the amount of polyester that could theoretically be obtained by converting all the dicarboxylic acids fed to the reactor.

[0167] The catalyst used in the esterification / transesterification step is a titanate, more preferably diisopropyl, triethanolamino titanate, preferably used at a concentration of 12 to 120 ppm of metal relative to the amount of polyester theoretically obtainable by converting all the dicarboxylic acid fed to the reactor.

[0168] Preferably, the reaction time of the esterification / transesterification step in the method according to the present invention is 4 to 8 hours.

[0169] At the end of the esterification / transesterification step, an oligomeric product is obtained having an Mn < 5000, an intrinsic viscosity of 0.05 to 0.15 dl / g and an acidity < 150 meq / kg.

[0170] At the end of the esterification / transesterification stage, the catalyst can be fed to the polycondensation stage along with the oligomer product.

[0171] The polycondensation step is carried out in the presence of a catalyst comprising titanium, possibly zirconium or a mixture thereof, and a phosphorus-containing compound belonging to the family of organic phosphates or phosphites, wherein the total amount of titanium in the catalyst is between 80 and 500 ppm relative to the amount of polyester theoretically obtainable by converting all the dicarboxylic acids fed to the reactor. The titanium to phosphorus ratio is between 2 and 20, preferably between 3 and 15. If present, the total amount of zirconium must be such as to maintain the Ti / (Ti+Zr) ratio within the range of 0.01 to 0.70.

[0172] In a preferred embodiment of the process according to the invention for preparing mixed aliphatic-aromatic polyesters, the polycondensation catalyst comprising titanium is a titanate advantageously selected from compounds having the general formula Ti(OR)4, wherein R is a ligand group comprising one or more atoms of carbon, oxygen, phosphorus and / or hydrogen.

[0173] Different ligand groups R can be present on the same titanium atom, but preferably they are identical to facilitate titanate preparation.

[0174] Furthermore, two or more ligands R may originate from a single compound and, in addition to being titanium-bound, may also be chemically bonded together (so-called polydentate ligands such as triethanolamine, citric acid, glycolic acid, malic acid, succinic acid, ethylenediamine).

[0175] R is advantageously selected from the group consisting of H, triethanolamine, citric acid, glycolic acid, malic acid, succinic acid, 3-oxobutyric acid, ethylenediamine, and linear or branched C1-C12 alkyl residues such as, for example, ethyl, propyl, n-butyl, pentyl, isopropyl, isobutyl, isopentyl, hexyl, ethylhexyl. In a preferred embodiment, R is selected from C1-C12 alkyl residues, preferably C1-C8, more preferably n-butyl.

[0176] The preparation of titanates is well known in the literature. Typically, these are prepared by reacting titanium tetrachloride with a precursor alcohol of the formula ROH in the presence of a base such as ammonia, or by transesterification of other titanates.

[0177] Commercial examples of titanates that can be used in a preferred embodiment of the process to prepare mixed aromatic-aliphatic polyesters according to the invention include (tetraisopropyl titanate), (tetra-n-butyl titanate) and (Diisopropyl triethanolamido titanate).

[0178] If a polycondensation catalyst comprising zirconium is used in combination with a polycondensation catalyst comprising titanium, it is advantageously a zirconate selected from compounds having the general formula Zr(OR)4, wherein R is a ligand group comprising one or more atoms of carbon, oxygen, phosphorus and / or hydrogen.

[0179] As in the case of titanates, several different, but preferably identical, ligand groups R can be present on the same zirconate atom.

[0180] In addition, the two or more ligands R can be derived from a single compound or, in addition to being zirconium-bonded, can also be chemically bonded together (so-called multidentate ligands such as triethanolamine, citric acid, glycolic acid, malic acid, succinic acid, ethylenediamine). R is advantageously selected from the group consisting of H, triethanolamine, citric acid, glycolic acid, malic acid, succinic acid, 3-oxobutanoic acid, ethylenediamine, and linear or branched C1-C12 alkyl residues such as ethyl, propyl, n-butyl, pentyl, isopropyl, isobutyl, isopentyl, hexyl, or ethylhexyl. In a preferred embodiment, R is selected from C1-C12, preferably C1-C8 alkyl residues, more preferably n-butyl.

[0181] The preparation of zirconates is known in the literature and is analogous to the preparation described above for titanates.

[0182] Commercial examples of zirconates that can be used in the process for preparing mixed aromatic-aliphatic polyesters according to the present invention include (tetra-n-butyl zirconate), Tyzor NPZ (tetra-n-propyl zirconate), IG-NBZ (tetra-n-butyl zirconate), Tytan TNBZ (tetra-n-butyl zirconate), Tytan TNPZ (tetra-n-propyl zirconate).

[0183] The polycondensation catalyst and the phosphorus-containing compound are fed to the polycondensation stage by feeding each component separately to the reactor.

[0184] It is also possible to premix some of the components and subsequently adjust the composition of the catalyst, for example when it is placed in contact with the oligomer product.

[0185] When a catalyst comprising a titanium compound and / or a zirconium compound is used in the esterification / transesterification step of the process according to the invention for preparing mixed aromatic-aliphatic polyesters, in a preferred embodiment of the process according to the invention, the catalyst is not separated from the oligomer product and is fed together with it to the polycondensation stage and advantageously used as polycondensation catalyst or as a component thereof, and by adding appropriate amounts of titanium compound and zirconium compound to the polycondensation stage, the molar ratio between titanium and zirconium can be adjusted.

[0186] It is possible that the catalyst used in the polycondensation stage may be the same as the catalyst used in the esterification / transesterification stage.

[0187] The polycondensation stage is advantageously carried out by feeding the oligomer product to a polycondensation reactor and allowing it to react in the presence of a catalyst at a temperature of 220 to 260° C. and a pressure of 0.5 to 350 mbar.

[0188] Preferably, the reaction time of the polycondensation stage is 4 to 8 hours.

[0189] Depending on the specific molecular weight characteristics and desired viscosity of the polyester, the following steps can be followed by the use of peroxides, divinyl ethers, Oxazolines, polyepoxides, di- and polyisocyanates, carbodiimides or dianhydrides, the process according to the invention may provide one or more stages including chain extension with other polymers, reactive processing or reactive extrusion.

[0190] The invention will now be illustrated by some embodiments, which are intended to be illustrative and not to limit the scope of protection of this patent application.

[0191] Example

[0192] Example 1 (Comparative) - Poly(1,4-butylene adipate-co-1,4-butylene sebacate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTAdSebSuc 50 / 28 / 22] was prepared with 50 mol% adipic acid, 28 mol% sebacic acid, and 22 mol% succinic acid relative to the sum of all aliphatic carboxylic acids.

[0193] Esterification stage

[0194] A steel reactor with a geometric capacity of 60 liters, equipped with a mechanical stirring system, a nitrogen inlet, a distillation column, a high-boiling distillate removal system and a connection to a high vacuum system, was charged with the following at a molar ratio (MGR) of diol to dicarboxylic acid of 1.50: 8004 g of terephthalic acid, 3969 g of adipic acid, 3075 g of sebacic acid, 1411 g of succinic acid, 113850 g of 1,4-butanediol, 4.72 g of glycerol and 5.50 g of an 80% by weight solution of diisopropyltriethanolamidotitanate in ethanol (Tyzor TE, corresponding to 21 ppm of metal relative to the amount of PBTAdSebSuc theoretically obtainable by converting all the adipic acid, all the sebacic acid, all the succinic acid and all the terephthalic acid fed to the reactor).

[0195] The temperature of the mass was gradually increased to 230°C over a period of 120 minutes.

[0196] polycondensation stage

[0197] When at least 95% of the theoretical water had been distilled, 24.20 g of tetra-n-butyl titanate (corresponding to 154 ppm of metals relative to the amount of PBTADSebSuc theoretically obtainable by converting all the adipic, sebacic, succinic and terephthalic acids fed to the reactor) and 5.39 g of trioctyl phosphate (corresponding to 17.5 ppm of phosphorus relative to the amount of PBTADSebSuc theoretically obtainable by converting all the adipic, sebacic, succinic and terephthalic acids fed to the reactor, and thus corresponding to a Ti / P ratio of 10 by weight) were added. The reactor temperature was then raised to 242° C. and the pressure was gradually reduced to below 1.2 mbar over 60 minutes. The reaction was allowed to proceed for approximately 4.30 hours (the time required to obtain a PBTAdSebSuc MFR of 4.3 g / 10 min (at 190°C and 2.16 kg)) before the material was discharged as a string into a water bath and pelletized.

[0198] Example 2 - Poly(1,4-butylene adipate-co-1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTAdAzSuc 50 / 28 / 22] was prepared with 50 mol% adipic acid, 28 mol% azelaic acid, and 22 mol% succinic acid relative to the sum of all aliphatic carboxylic acids.

[0199] The operating conditions of Example 1 were repeated, except that 8082 g of terephthalic acid, 4008 g of adipic acid, 2890 g of azelaic acid, 1425 g of succinic acid, 13985 g of 1,4-butanediol, 4.77 g of glycerol, and 5.50 g of an 80% by weight solution of diisopropyltriethanolamidotitanate in ethanol (Tyzor TE, corresponding to 21 ppm of metal relative to the amount of PBTAdAzSuc theoretically obtainable by converting all the adipic acid, all the sebacic acid, all the succinic acid, and all the terephthalic acid fed to the reactor) were charged. A PBTAdAzSuc of 4.5 g / 10 min (at 190° C. and 2.16 kg) was obtained.

[0200] Example 3 - Poly(1,4-butylene adipate-co-1,4-butylene sebacate-co-1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTAdSebAzSuc 50 / 14 / 14 / 22] was prepared with 50 mol% adipic acid, 14 mol% sebacic acid, 14 mol% azelaic acid, and 22 mol% succinic acid relative to the sum of all aliphatic carboxylic acids.

[0201] The operating conditions of Example 1 were repeated, except that 8043 g of terephthalic acid, 3989 g of adipic acid, 1545 g of sebacic acid, 1438 g of azelaic acid, 1418 g of succinic acid, 13917 g of 1,4-butanediol, 4.74 g of glycerol, and 5.50 g of an 80% by weight solution of diisopropyltriethanolamido titanate in ethanol (Tyzor TE, corresponding to 21 ppm of metal relative to the amount of PBT A / Seb / A / Suc theoretically obtainable by converting all the adipic acid, all the sebacic acid, all the azelaic acid, all the succinic acid, and all the terephthalic acid fed to the reactor) were charged. This resulted in a PBT A / Seb / A / Suc with an MFR of 4.6 g / 10 min (at 190° C. and 2.16 kg).

[0202] Example 4 (Comparative) - Poly(1,4-butylene sebacate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTSebSuc 50 / 50] was prepared with 50 mole % sebacic acid and 50 mole % succinic acid relative to the sum of all aliphatic carboxylic acids.

[0203] The operating conditions of Example 1 were repeated, except that in the esterification stage, 7916 g of terephthalic acid, 5432 g of sebacic acid, 3173 g of succinic acid, 13698 g of 1,4-butanediol, 4.67 g of glycerol, and 5.50 g of an 80% by weight solution of diisopropyltriethanolamidotitanate in ethanol (Tyzor TE, corresponding to 21 ppm of metal relative to the amount of PBTSebSuc theoretically obtainable by converting all of the sebacic acid, all of the succinic acid, and all of the terephthalic acid fed to the reactor) were charged. No trioctyl phosphate was added during the polycondensation step. A PBTSebSuc having an MFR of 5.5 g / 10 min (at 190° C. and 2.16 kg) was obtained.

[0204] Example 5 (Comparative) - Poly(1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTAzSuc 50 / 50] was prepared with 50 mol% azelaic acid and 50 mol% succinic acid relative to the sum of all aliphatic carboxylic acids.

[0205] The operating conditions of Example 1 were repeated, except that in the esterification stage, 8054 g of terephthalic acid, 5143 g of azelaic acid, 3228 g of succinic acid, 13936 g of 1,4-butanediol, 4.75 g of glycerol, and 5.50 g of an 80% by weight solution of diisopropyltriethanolamidotitanate in ethanol (Tyzor TE, corresponding to 21 ppm of metal relative to the amount of PBTazSuc theoretically obtainable by converting all of the azelaic acid, all of the succinic acid, and all of the terephthalic acid fed to the reactor) were added. No trioctyl phosphate was added during the polycondensation step. A PBTazSuc with an MFR of 6.0 g / 10 min (at 190° C. and 2.16 kg) was obtained.

[0206] Example 6 Poly(1,4-butylene adipate-co-1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTAdAzSuc 50 / 18.5 / 31.5] was prepared with 50 mol% adipic acid, 18.5 mol% azelaic acid, and 31.5 mol% succinic acid relative to the sum of all aliphatic carboxylic acids.

[0207] Esterification stage

[0208] A steel reactor of 60 liters geometric capacity, equipped with a mechanical stirring system, a nitrogen inlet, a distillation column, a high-boiling distillate removal system and a connection to a high vacuum system, was charged with the following at a diol to dicarboxylic acid molar ratio (MGR) of 1.50: 8180 g of terephthalic acid, 4133 g of adipic acid, 2065 g of azelaic acid, 1933 g of succinic acid, 14153 g of 1,4-butanediol, 4.82 g of glycerol and 5.50 g of an 80% by weight solution of diisopropyltriethanolamidotitanate in ethanol (Tyzor TE, corresponding to 21 ppm of metal relative to the amount of PBTAdAzSuc theoretically obtainable by converting all the adipic acid, all the azelaic acid, all the succinic acid and all the terephthalic acid fed to the reactor).

[0209] The temperature of the mass was gradually raised to 230°C over a period of 120 minutes.

[0210] polycondensation stage

[0211] When at least 95% of the theoretical water had been distilled, 16.5 g of tetra-n-butyl titanate (corresponding to 105 ppm of metal relative to the theoretical amount of PBTADAzSuc that could be obtained by converting all the adipic, azelaic, succinic, and terephthalic acids fed to the reactor) and 6.47 g of trioctyl phosphate (corresponding to 21 ppm of phosphorus relative to the theoretical amount of PBTADAzSuc that could be obtained by converting all the adipic, azelaic, succinic, and terephthalic acids fed to the reactor, and thus corresponding to a Ti / P ratio of 5 by weight) were added. The reactor temperature was then raised to 257°C, and the pressure was gradually reduced to below 1.2 mbar over 60 minutes. The reaction was allowed to proceed for approximately 4.30 hours (the time required to obtain a PBTADAzSuc MFR of 6.0 g / 10 minutes (at 190°C and 2.16 kg)), after which the material was discharged as strands into a water bath and pelletized.

[0212] Example 7 (Comparative) - Poly(1,4-butylene sebacate-co-1,4-butylene azelate-co-1,4-butylene succinate-co-1,4-butylene terephthalate) [PBTSebAzSuc33.3 / 33.3 / 33.3] was prepared with 40 mol% terephthalic acid relative to the sum of all carboxylic acids and 33.3 mol% sebacic acid, 33.3 mol% azelaic acid, and 33.3 mol% succinic acid relative to the sum of all aliphatic carboxylic acids.

[0213] Esterification stage

[0214] Into a glass reactor equipped with a mechanical stirring system, nitrogen inlet, distillation column, high-boiling distillate removal system, and connection to a high vacuum system were charged the following at a diol to dicarboxylic acid molar ratio (MGR) of 1: 44.82 g terephthalic acid, 27.27 g sebacic acid, 25.38 g azelaic acid, 15.93 g succinic acid, 121.50 g 1,4-butanediol, and 0.23 g tetrabutyl titanate (Tyzor TnBT, corresponding to 215 ppm of metal relative to the amount of PBTSebAzSu theoretically obtainable by converting all sebacic acid, all azelaic acid, all succinic acid, and all terephthalic acid fed to the reactor).

[0215] The temperature of the mass was maintained to 190°C, 200°C and 210°C for 1 hour, 2 hours and 1 hour respectively.

[0216] polycondensation stage

[0217] The reactor temperature was then raised to 240°C and the pressure was gradually reduced to 2 mbar over 45 minutes. The reaction was allowed to proceed for approximately 4 hours (the time required to obtain a PBTSebAzSuc with an MFR of 5.7 g / 10 min (at 190°C and 2.16 kg)) before the material was discharged.

[0218] Table 1

[0219]

[0220] From the data in Table 1, comparing Example 2 with Comparative Example 1, it can be seen that when azelaic acid is present in succinic acid and another saturated aliphatic dicarboxylic acid (adipic acid), the Tg of the mixed aliphatic-aromatic polyester is unexpectedly lower than the Tg of the mixed aliphatic-aromatic polyester containing succinic acid and sebacic acid.

[0221] This effect was also demonstrated for four acids (Example 3), among which azelaic acid and succinic acid were present.

[0222] This effect is even more surprising if we consider that it does not occur in the presence of only two saturated aliphatic dicarboxylic acids, in agreement with what has been described in the literature (Comparative Example 4 compared to Comparative Example 5).

[0223] Comparative Example 7 (Prior Art, Pan et al.) demonstrates that the combination of azelaic acid, succinic acid, and sebacic acid exhibits an MM of 1.62 with a ratio of cyclic oligomers comprising at least two types of dicarboxylic acid aliphatic units below 1000 to cyclic oligomers comprising only one type of dicarboxylic acid aliphatic units below 1000 (ratio between mixed cyclic oligomers), which is outside the present invention.

Claims

1. A mixed aliphatic-aromatic polyester comprising: a) a dicarboxylic acid component, the dicarboxylic acid component comprising: i.a1) 40 mol % to 80 mol % of units derived from at least one aromatic dicarboxylic acid; ii.a2) 20 mol % to 60 mol % of units derived from at least three C4-C24 saturated dicarboxylic acids, their C1-C24 alkyl esters, their salts and mixtures thereof, always with azelaic acid and succinic acid present, b) Diol aliphatic component The mixed aliphatic-aromatic polyester is characterized by containing a content of residual cyclic mixed oligomers, the residual cyclic mixed oligomers being defined as cyclic residual oligomers remaining in the polymer substance after the polycondensation process and having a molecular mass (MM) below 1000, wherein the residual cyclic mixed oligomers are present in a content of 1.0% to 4.0% as measured by the gravimetric method described in the specification, wherein the residual cyclic mixed oligomers are characterized by: a ratio between cyclic oligomers containing at least two types of dicarboxylic aliphatic units with a MM below 1000 and cyclic oligomers containing only one type of dicarboxylic aliphatic units with a MM below 1000 of 0.30 to 1.40, more preferably 0.40 to 1.20, even more preferably 0.81 to 1.14, wherein the ratio is determined by the method described in the specification involving HPLC-MS analysis; and the mixed aliphatic-aromatic polyester is also characterized by a main saturated aliphatic dicarboxylic acid of component a2 of 0.40 mol% to 92 mol% relative to the sum of all other saturated aliphatic dicarboxylic acids.

2. The mixed aliphatic-aromatic polyester of claim 1, wherein the residual cyclic mixed oligomer content is 2.0% to 3.5%.

3. The mixed aliphatic-aromatic polyester according to any one of the preceding claims, wherein the diol aliphatic component b) comprises at least 50 mol% of one or more diols selected from 1,2-ethanediol, 1-3-propylene glycol, 1,4-butanediol.

4. A mixed aliphatic-aromatic polyester according to any of the preceding claims, wherein the dicarboxylic acid component a) comprises 40 to 75 mol %, more preferably 42 to 52 mol %, even more preferably 45 to 49 mol %, of units derived from at least an aromatic dicarboxylic acid (component a1), relative to the total dicarboxylic acid component, and 25 to 60 mol %, more preferably 45 to 58 mol %, even more preferably 51 to 55 mol %, relative to the total dicarboxylic acid component, of units derived from at least three saturated aliphatic dicarboxylic acids (component a2).

5. The mixed aliphatic-aromatic polyester according to any of the preceding claims, wherein the mol % of saturated aliphatic dicarboxylic acids of renewable origin in component a2) relative to the sum of the total saturated dicarboxylic acids is preferably equal to or higher than 30%, more preferably higher than 40%, even more preferably higher than 50%.

6. The mixed aliphatic-aromatic polyester according to any of the preceding claims, wherein the succinic acid of component a2) is further characterized in that it accounts for 5 to 67 mol % relative to the sum of the total saturated dicarboxylic acids, preferably for 10 to 50 mol % relative to the sum of the total saturated dicarboxylic acids, even more preferably for 20 to 35 mol %.

7. The mixed aliphatic-aromatic polyester according to any of the preceding claims, wherein the azelaic acid of component a2) preferably accounts for 3 to 92 mol %, more preferably for 10 to 50 mol %, even more preferably for 15 to 35 mol %, relative to the sum of the total saturated dicarboxylic acids.

8. A mixed aliphatic-aromatic polyester according to any one of the preceding claims, wherein the saturated aliphatic dicarboxylic acid of component a2) is advantageously selected from: C4-C24, preferably C4-C13, more preferably C4-C11 saturated dicarboxylic acids; their C1-C24, preferably C1-C4 alkyl esters; their salts; and mixtures thereof.

9. The mixed aliphatic-aromatic polyester according to claim 8, wherein the saturated aliphatic dicarboxylic acid of component a2) is advantageously selected from the group consisting of succinic acid, glutaric acid, 2-methylglutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanoic acid, dodecanoic acid, brassylic acid, C1-C24 alkyl esters thereof.

10. A mixed aliphatic-aromatic polyester according to any one of the preceding claims, comprising repeating units derived from an aromatic dicarboxylic acid of the phthalic acid type, preferably terephthalic acid, an aromatic dicarboxylic acid and an aliphatic diol (AAPE-A), characterized in that The content of the aromatic unit is 42 mol% to 52 mol%, preferably 45 mol% to 49 mol%, relative to the total moles of the dicarboxylic acid component.

11. A mixed aliphatic-aromatic polyester according to any one of the preceding claims, comprising repeating units derived from 2,5-furandicarboxylic acid, an aromatic dicarboxylic acid and an aliphatic diol (AAPE-B), characterized in that The aromatic unit content is 40 mol% to 80 mol%, preferably 40 mol% to 75 mol%, relative to the total moles of the dicarboxylic acid component.

12. The mixed aliphatic-aromatic polyester according to any one of the preceding claims, comprising a cyclic oligomer containing only one type of aliphatic dicarboxylic acid unit selected from the following: (ADA-BDO)2, (AZA-BDO)2, (SEBA-BDO)2, (BRA-BDO)2, (SUC-BDO)2, (ADA-BDO)3, (AZA-BDO)3, (SEBA-BDO)3, (BRA-BDO)3, (SUC-BDO)3, (ADA-BDO)4, (AZA-BDO)4, (SUC-BDO)4; wherein ADA corresponds to the ester of adipic acid with a diol component, AZA corresponds to the ester of azelaic acid with a diol component, SUC corresponds to the ester of succinic acid with a diol component, SEBA corresponds to the ester of sebacic acid with a diol component, BRA corresponds to the ester of brassic acid with a diol component, PTA corresponds to the ester of terephthalic acid and BDO is the diol component 1,4-butanediol. (AD) A-BDO-AZA-BDO), (ADA-BDO-SEBA-BDO), (ADA-BDO-BRA-BDO), (ADA-BDO-S UC-BDO), (AZA-BDO-SEBA-BDO), (AZA-BDO-BRA-BDO), (AZA-BDO-SUC-BDO), (SEBA-BDO-BRA-BDO), (SEBA-BDO-SUC-BDO), (SUC-BDO-BRA-BDO)(ADA-BD O)2-(AZA-BDO), (ADA-BDO)-(AZA-BDO)2, (ADA-BDO)2-(SEBA-BDO), (ADA-BDO)-(SEBA-BDO)2, (ADA-BDO)2-(BRA-BDO), (ADA-BDO)-(BRA-BDO)2, (ADA -BDO)2-(SUC-BDO), (ADA-BDO)-(SUC-BDO)2, (AZA-BDO)2-(SUC-BDO), (AZA-BDO)-(SUC-BDO)2, (SEB-BDO)2-(SUC-BDO), (SEB-BDO)-(SUC-BDO)2, (BR A-BDO)2-(SUC-BDO), (BRA-BDO)-(SUC-BDO)2, (AZA-BDO)2-(SEBA-BDO), (AZA-BDO)-(SEBA-BDO)2, (AZA-BDO)2-(BRA-BDO), (AZA-BDO)-(BRA-BDO)2, (SEBA-BDO)2-(BRA-BDO), (SEBA-BDO)-(BRA-BDO)2, (ADA-BDO)-(PTA-BDO)-(AZ-BDO), (ADA-BDO)-(PTA-BDO)-(SEBA-BDO), (ADA-BDO)-(PTA-BDO)-( BRA-BDO), (SEBA-BDO)-(PTA-BDO)-(AZ-BDO), (BRA-BDO)-(PTA-BDO)-(AZ-BDO), (BRA-BDO)-(PTA-BDO)-(SEBA-BDO), (ADA-BDO)-(PTA-BDO)-(SUC-B DO), (AZA-BDO)-(PTA-BDO)-(SUC-BDO), (SEB-BDO)-(PTA-BDO)-(SUC-BDO), (BRA-BDO)-(PTA-BDO)-(SUC-BDO), (ADA-BDO)-(AZA-BDO)-(SEBA-BDO),(ADA-BDO)-(AZA-BDO)-(BRA-BDO), (ADA-BDO)-(BRA-BDO)-(SEBA-BDO), (BRA-BDO)-(AZA-BDO)-(SEBA-BDO), (ADA-BDO)-(AZA- BDO)-(SUC-BDO), (SEBA-BDO)-(AZA-BDO)-(SUC-BDO), (BRA-BDO)-(AZA-BDO)-(SUC-BDO), (SEBA-BDO)-(BRA-BDO)-(SUC-BDO), ( SEBA-BDO)-(ADA-BDO)-(SUC-BDO), (ADA-BDO)2-(AZA-BDO)2, (ADA-BDO)2-(SEBA-BDO)2, (ADA-BDO)2-(BRA-BDO)2, wherein ADA corresponds to the ester of adipic acid and a diol component, AZA corresponds to the ester of azelaic acid and a diol component, SUC corresponds to the ester of succinic acid and a diol component, SEBA corresponds to the ester of sebacic acid and a diol component, BRA corresponds to the ester of brazilic acid and a diol component, PTA corresponds to the ester of terephthalic acid, and BDO is the diol component 1,4-butanediol.

14. A mixture of a mixed aliphatic-aromatic polyester according to any of the preceding claims with other biodegradable polymers both of synthetic and natural origin and possibly with polyhydroxyalkanoates, inorganic fillers, crosslinkers and / or chain extenders.

15. A film obtained with the mixture of mixed aliphatic-aromatic polyesters according to claim 14, comprising: i) 30 to 95% by weight, relative to the sum of components i. to v., of at least mixed aliphatic-aromatic polyesters, ii) from 0.1 to 50% by weight, relative to the sum of components i. to v., of at least a polymer of natural origin, iii) 0 to 40% by weight, relative to the sum of components i. to v., of at least polyhydroxyalkanoate, iv) 0 to 15% by weight, relative to the sum of components i. to v., of at least an inorganic filler, v) 0 to 5% by weight of at least a crosslinker and / or chain extender comprising at least a difunctional and / or polyfunctional compound with: isocyanates, peroxides, carbodiimides, isocyanurates, oxazolines, epoxides, anhydrides, divinyl ethers and mixtures thereof.

16. A product comprising the mixed aliphatic-aromatic polyester according to claims 1 to 13, selected from: - films, including mono-oriented and bi-oriented films, and multilayer films with other polymeric materials; - As mulch films for use in agricultural fields; - stretch films, including those for food, for bales in agriculture and for wrapping waste; - Bags and liners for collecting organic material such as food waste and grass clippings; - Both single-layer and multi-layer thermoformed food packaging, such as containers for milk, yoghurt, meat, beverages, etc.; - coatings obtained by extrusion coating technique; - multilayer laminates having layers of paperboard, plastic material, aluminum and metal film; - expanded or expandable beads for producing components formed by sintering; - expanded and semi-expanded products, including expanded masses formed from pre-expanded granules; - Expanded sheets, thermoformed expanded sheets, containers for food packaging obtained therefrom; -Containers generally used for fruits and vegetables; - Compositions containing as fillers gelatinized starch, destructurized starch and / or complex starch, native starch, flour, other fillers of natural, vegetable or inorganic origin.