Gas diffusion layer made of water jet reinforced non-woven fabric
By using pH-optimized aqueous fluid jet in fuel cell manufacturing, the problem of difficult to achieve low ion concentration and high purity in the prior art is solved, the mechanical performance and service life are improved, and the water needle plate is reduced defect.
Patent Information
- Application Number
- CN202380030246.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-13
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to achieve low ion concentration and high purity in the gas diffusion layer in existing fuel cells, and it is prone to defects in water needle plates during the manufacturing process, affecting mechanical properties and service life.
The water treatment process is optimized to remove non-desired incidental substances and heat and mechanical treatments are performed when necessary for further reinforcement of non-woven fabrics made of carbon fiber or carbon fiber precursors using an aqueous fluid jet with a pH of 5.5 to 8.0. Non-woven fabric.
It realizes low ion concentration and high purity carbon fiber non-woven fabrics and gas diffusion layers, reduces the damage to non-woven fabrics by water treatment, reduces the number of water needle plate defects, and improves the mechanical properties and the service life of fuel cells.
Smart Images

Figure HDA0005059015680000011 
Figure HDA0005059015680000021 
Figure HDA0005059015680000031
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a gas diffusion layer, in which a nonwoven fabric made of carbon fibers or carbon fiber precursors is reinforced with a jet of an aqueous fluid of a specific water quality, the gas diffusion layer obtained according to the method and a fuel cell comprising such a gas diffusion layer. Background Art
[0002] Fuel cells generate electricity by using the chemical reaction of fuel (especially hydrogen) and oxygen to produce water. In hydrogen-oxygen fuel cells, hydrogen or a hydrogen-containing gas mixture is supplied to the anode, where it undergoes electrochemical oxidation and releases electrons (H 2 →2H + +2e - ). Protons are transported from the anode region to the cathode region via a membrane that separates the reaction zones from one another in a gas-tight manner and electrically insulates them. The electrons provided at the anode are transported to the cathode via an external conductor circuit. Oxygen or an oxygen-containing gas mixture is supplied to the cathode, where oxygen is reduced by absorbing electrons. The oxygen anions formed in the process react with the protons transported through the membrane and form water (1 / 2O 2 +2H + +2e - →H 2 O).
[0003] Many applications (especially automotive powertrains) use low-temperature proton exchange membrane fuel cells (PEMFCs), which are core components that allow only protons (or hydronium ions H 3 O + ) and water pass through and spatially separate the oxidant (generally atmospheric oxygen) from the reductant. Catalyst layers are applied on the anode and cathode sides of the gas-tight electrically insulating proton-conducting membrane, which form electrodes and usually contain platinum as a catalytically active metal. The actual redox reaction and charge separation take place in the catalyst layers. The membrane and the catalyst layer form a unit also known as CCM (catalyst coated membrane). Gas diffusion layers (GDL) are provided on both sides of the CCM, which stabilize the cell structure and assume the transport and distribution functions of the reaction gases, water, heat and current. The membrane, electrodes and gas diffusion layers form a membrane-electrode unit (MEA, membraneelectrode assembly). Distribution plates (so-called bipolar plates) are provided between the membrane-electrode units, which have channels for supplying process gas (Prozessgas) to the adjacent cathodes and anodes, and usually also have internal cooling channels.
[0004] The gas diffusion layer between the manifold and the catalyst layer plays a crucial role in the function and performance of the fuel cell. The process components consumed and generated in the electrode reaction must be transported by the gas diffusion layer and must be evenly distributed from the macrostructure of the manifold / bipolar plate to the microstructure of the catalyst layer. The electrons generated and consumed in the half-cell reaction must be conducted to the manifold with as little voltage loss as possible. The heat generated during the reaction must be dissipated into the coolant in the manifold, so the material of the GDL must also have sufficient thermal conductivity. In addition, the GDL must also play a mechanical balancing role between the macrostructured manifold and the catalyst layer.
[0005] The gas diffusion layer used in fuel cells is generally composed of a carbon fiber substrate, which is usually treated with a fluoropolymer (such as PTFE) for hydrophobicity and then coated with a microporous layer (MPL). The MPL is usually composed of a fluoropolymer (such as PTFE) as a binder and a porous conductive carbon material (such as carbon black or graphite powder). Currently, the following three materials are used as carbon fiber substrates for GDL:
[0006] - carbon fiber paper (wet-laid and chemically bonded carbon fiber nonwoven with carbonized chemical binder),
[0007] - carbon fibre fabrics (for example made from yarns of oxidised but not yet carbonised polyacrylonitrile fibres which are carbonised or graphitised after weaving),
[0008] - Carbon fiber nonwovens (for example made of oxidized polyacrylonitrile, dry-laid, carded and water-jet-strengthened nonwovens, subsequently calibrated for thickness and carbonized).
[0009] It is well known that fuel cells can be contaminated by the introduction of foreign ions that are not involved in the electrode processes. For example, there have been studies on the effects of bipolar plate materials on cell performance and the effects of cations and anions introduced from the bipolar plates into the MEA of the fuel cell on cell performance. Other sources, especially sources of metal cations, are emissions from the rest of the cell materials, system components (such as tanks, heat exchangers, piping, etc.), air flow supplied to the cathode, and hydrogen impurities during manufacturing or transportation. A possible problem with introduced metal ions is that they are easily absorbed by the electrolyte membrane. The reason for this is that the affinity of metal cations for the sulfonic acid groups of the perfluorocation exchange membrane is very strong, usually greater than the affinity of protons for the sulfonic acid groups.
[0010] It has now been found that the GDL also plays a role in loading the MEA with foreign ions. Therefore, there is a need for a gas diffusion layer with a very low concentration of ions, especially metal cations, and a method for its production. The GDL should in particular have a low concentration of cations, such as those commonly contained in technical water, such as calcium ions, magnesium ions, sodium ions and potassium ions. At the same time, the remaining mechanical properties of the GDL should not be adversely altered.
[0011] In order to produce carbon fiber nonwovens, nonwovens made of carbon fibers or carbon fiber precursors can be reinforced by the action of aqueous fluid jets. Such swirl processes (Verwirbelungsverfahren) (hydroentanglement processes (Spunlace-Verfahren)) for the reinforcement of nonwovens with fluid jets or fluid flows, including swirl with superheated steam jets, are known to those skilled in the art. A special method for mechanical reinforcement of nonwovens is water jet reinforcement, that is, water with a pressure of about 20 bar to more than 400 bar is introduced to the nonwoven to be reinforced through a large number of nozzles. In this case, the pulse force of the water jet causes the fibers to be mechanically anchored in the product. The tool used for this method is a so-called water jet plate (Düsenstreifen), which can be installed in one or more rows. Each row has a large number of nozzles. The maximum number of nozzles can reach 20,000 nozzles per plate, with typical nozzle diameters ranging from 0.05 mm to 0.3 mm.
[0012] WO 2021 / 170608 A1 describes a method for producing spunbond nonwovens, wherein the spunbond nonwovens are water jet consolidated and then rinsed. The water jet consolidation is carried out with clean water, and the waste water from the water jet consolidation is used for rinsing. Generally, completely desalinated water is used as clean water.
[0013] US2003 / 182730 A1 describes a nonwoven fabric with a low content of ionic impurities, which is achieved by washing with water with a low ion concentration. These nonwoven fabrics are mainly used for cleaning cloths and protective clothing in clean rooms. It does not describe the application for the production of gas diffusion layers for fuel cells.
[0014] WO 0231841 A2 describes a conductive nonwoven fabric, which is made from a fiber web made of pre-oxidized fibers for carbon fibers, and is obtained by consolidating the fiber web with a high-pressure fluid jet at a pressure of 100 bar to 300 bar, densifying the consolidated fiber nonwoven fabric, and then carbonizing and / or graphitizing it at a temperature of 800° C. to 2500° C. in a protective atmosphere.
[0015] DE 10 2006 060 932 A1 describes a temperature-stable structure comprising fibers and a coating, wherein the coating is covalently bonded to the fiber surface. Specifically, the structure is a conductive nonwoven fabric which has been subjected to plasma coating with fluorinated hydrocarbons and is suitable as a gas diffusion layer for fuel cells. To produce the conductive nonwoven fabric, carbon fibers or carbon fiber precursors are formed into a fiber web and consolidated by the action of a high-pressure fluid jet, and then predried, calendered and carbonized.
[0016] US2019 / 0165379 A1 describes a material for a gas diffusion layer based on a carbon fiber nonwoven fabric, the carbon fiber nonwoven fabric having a high grammage area and a low grammage area in a plane, wherein at least one surface of the nonwoven fabric has an uneven pattern that is independent of the weight distribution of the fibers. The production of this nonwoven fabric includes a water jet process.
[0017] None of the above four documents contain data on the quality of water used in water jet treatment.
[0018] The unpublished international application PCT / EP2021 / 085452 (WO 2022 / 128895 A1) describes a high-purity gas diffusion layer and a method for its production, wherein a nonwoven made of carbon fibers or carbon fiber precursors is reinforced with a jet of an aqueous fluid, wherein the electrical conductivity of the water at 25° C. is not greater than 250 microsiemens / cm. No data are available on the pH value of the water used for the water jet treatment.
[0019] It has now been found that high-quality and in particular high-purity carbon fiber nonwovens can be produced if dry-laid nonwovens made of carbon fibers or carbon fiber precursors are consolidated by the action of aqueous fluid jets. The quality of the consolidation water plays a crucial role.
[0020] The pH value of the water is a key parameter for removing unwanted incidental substances from the nonwoven during wet consolidation without the aid of detergents. At the same time, additives added before this treatment step should be largely retained. By optimizing the pH value, damage to the nonwoven by the water treatment can also be reduced or avoided.
[0021] Another key parameter is the ion concentration, i.e. the proportion of dissociated substances dissolved in a certain amount of water. Surprisingly, it was through the water jet consolidation process that high-purity nonwovens with an extremely low ion concentration were successfully produced, which can be further processed into GDL with a likewise low ion concentration. Advantageously, the nonwovens obtained are characterized by a very low number of so-called jet strip defects. Such jet strip defects can occur when individual jets of the jet strip become clogged. Summary of the invention
[0022] The first object of the present invention is a method for manufacturing a gas diffusion layer for a fuel cell, wherein:
[0023] a) providing a fiber composition comprising carbon fibers and / or precursors of carbon fibers,
[0024] b) subjecting the fiber composition provided in step a) to a process for producing a fiber web,
[0025] c) consolidating the fiber web to form a nonwoven fabric by the action of jets of aqueous fluid, wherein the water used has a pH value in the range of 5.5 to 8.0,
[0026] d) optionally subjecting the nonwoven fabric obtained in step c) to a thermal and / or mechanical treatment for drying and / or further consolidation,
[0027] e) pyrolyzing the nonwoven at a temperature of at least 1000° C. if the fiber composition used in step a) comprises a precursor of carbon fibers.
[0028] In a particular embodiment, the water used in step c) has an electrical conductivity of at most 250 microSiemens / cm at 25°C.
[0029] In another particular embodiment, the nonwoven from step c), step d) or step e) (ie after the last of these steps, depending on which of these steps is carried out) is sized with a hydrophobic agent (= step f)).
[0030] In another particular embodiment, the nonwoven from step c), step d), step e) or step f) (ie after the last of these steps, depending on which of these steps is carried out) is coated with a microporous layer (= step g)).
[0031] The invention also relates to a fiber web having a very low ion concentration, which is reinforced by the action of an aqueous fluid jet (water jet reinforced nonwoven). Thus, a nonwoven obtainable by a process comprising the following steps is also the subject of the invention:
[0032] a) providing a fiber composition comprising carbon fibers and / or precursors of carbon fibers,
[0033] b) subjecting the fiber composition provided in step a) to a process for producing a fiber web,
[0034] c) Consolidating the fiber web to form a nonwoven fabric by the action of jets of aqueous fluid, wherein the water used has a pH value in the range from 5.5 to 8.0.
[0035] Regarding step a), step b) and step c), please fully refer to the following description of these steps.
[0036] Another object of the invention is a gas diffusion layer as described above and below or a gas diffusion layer obtained by a process as described above and below.
[0037] Another object of the invention is a fuel cell comprising at least one gas diffusion layer as described above and below or obtainable by a method as described above and below. DETAILED DESCRIPTION
[0038] Unless otherwise indicated below, the pH values given relate to a temperature of 25° C.
[0039] The pH value can be determined according to conventional methods known to those skilled in the art. Preferably, the determination is carried out electrometrically based on the voltage measurement of a chain of electrochemical cells, one of the two half-cells being the measuring electrode and the second being the reference electrode. The potential of the measuring electrode is a function of the pH value of the measured solution. The pH value can be determined with commercially available pH measuring chains based on a pH electrode and a reference electrode, for example in the form of a single-rod measuring chain. Suitable methods for the pH determination are described in DIN EN ISO 10523-C5:2012-04 (Water Quality - pH Determination).
[0040] Measuring instruments which measure the pH value in particular electrometrically via proton activity, such as commercially available pH measuring chains, usually have an automatic or manual temperature compensation in order to compensate for the temperature dependence of the ion production of water.
[0041] The gas diffusion layer obtained by the method of the present invention has the following advantages:
[0042] - By optimizing the pH value of the water used for water jet consolidation, it is possible to remove undesirable nonwoven incidental materials during wet consolidation without the aid of detergents. At the same time, additives that have been added before this treatment step, such as hardeners, softeners, antistatic agents, hydrophobic agents, antibacterial, antifungal or fungicidal finishing agents, flame retardants and other additives, are largely retained.
[0043] -By optimizing the pH value, the damage of water treatment to nonwoven fabrics can be reduced or avoided.
[0044] - Carbon fiber nonwovens obtained by water jet consolidation using dry-laid carbon fibers as raw materials and GDL based thereon are characterized by very low ion concentrations.
[0045] - Nonwovens obtained from dry-laid carbon fiber precursors by water jet consolidation and subsequent carbonization or graphitization and GDL based thereon are also characterized by a very low ion concentration.
[0046] The nonwoven obtained by water jet consolidation according to the method of the invention has very few so-called needle board defects.
[0047] - The GDL according to the invention has considerably better mechanical properties compared to the GDL previously used in the prior art.
[0048] - A fuel cell based on the GDL of the present invention has a longer service life compared to a fuel cell based on a conventional GDL.
[0049] The gas diffusion layer according to the present invention and the gas diffusion layer that can be obtained according to the method of the present invention contain a carbon fiber nonwoven fabric as a planar conductive material. The carbon fiber nonwoven fabric and the gas diffusion layer are planar structures that are basically two-dimensionally flat and extend with a relatively small thickness. The base surface of the gas diffusion layer is generally basically consistent with the base surface of the adjacent membrane with a catalyst layer and the base surface of the adjacent distribution plate in the fuel cell. The shape of the base surface of the gas diffusion layer can be, for example, a polygon (n-gon, n≥3, such as a triangle, quadrilateral, pentagon, hexagon, etc.), a circle, a circle segment (such as a semicircle), an ellipse or an ellipse segment. The base surface is preferably rectangular or circular.
[0050] Fabrication of gas diffusion layers
[0051] Step a)
[0052] In step a) of the method according to the invention, a fiber composition comprising carbon fibers and / or precursors of carbon fibers is provided.
[0053] With reference to its total weight, preferred carbon fibers are at least 90 wt% carbon, preferably at least 92 wt% carbon. In a particular embodiment, graphitized carbon fibers can be used. These carbon fibers have a higher carbon content, in particular at least 95 wt% carbon.
[0054] Suitable carbon fiber precursors are fibers from synthetic or natural sources, which can be converted into carbon fibers (carbonization) by one or more treatment steps. For example, such fibers include fibers made of polyacrylonitrile homopolymers and copolymers (PAN fibers), phenolic resins, polyesters, polyolefins, cellulose, aramid, polyetherketone, polyetheresterketone, polyethersulfone, polyvinyl alcohol, lignin, pitch and mixtures thereof. Preferably, the fiber composition provided in step a) contains PAN fibers as precursor fibers or consists of PAN fibers as precursor fibers. In a first preferred embodiment, the fiber composition provided in step a) comprises PAN fibers and fibers different therefrom, the latter preferably being selected from fibers made of phenolic resins, polyesters, polyolefins, cellulose, aramid, polyetherketone, polyetheresterketone, polyethersulfone, polyvinyl alcohol, lignin, pitch and mixtures thereof. With reference to the carbon fiber precursor, the content of such additional polymers is preferably not more than 50 wt%, particularly preferably not more than 25 wt%. In a second preferred embodiment, the fiber composition provided in step a) consists entirely of PAN fibers.
[0055] Suitable PAN fibers are selected from PAN homopolymers, PAN copolymers and mixtures thereof. PAN copolymers contain at least one comonomer in a polymerized form, which is preferably selected from (meth)acrylamide, alkyl acrylates, hydroxyalkyl acrylates, alkyl ether acrylates, polyether acrylates, alkyl vinyl ethers, vinyl halides, vinyl aromatic compounds, vinyl esters, ethylene unsaturated dicarboxylic acids and their monoesters and diesters and mixtures thereof. The comonomer is selected, for example, from acrylamide, methyl acrylate, methyl methacrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, n-octyl acrylate, lauryl acrylate, stearyl acrylate, 2-ethylhexyl acrylate, benzyl acrylate, 2-hydroxyethyl propylene, 2-hydroxypropyl propylene, 4-hydroxybutyl propylene, 2-methoxyethyl acrylate, 4-methoxybutyl acrylate, diethylene glycol ethyl acrylate, 2-butoxyethyl propylene, ethyl vinyl ether, acrylic acid, methacrylic acid, itaconic acid, monomethyl itaconate, monolauryl itaconate, dimethyl fumarate, styrene, vinyl acetate, vinyl bromide, vinyl chloride, etc. If polyacrylonitrile copolymer fibers are used as carbon fiber precursors in step a), the proportion of the comonomer is up to 20 wt%, preferably up to 10 wt%, based on the total weight of the monomers used for polymerization. Preferably, polyacrylonitrile homopolymer fibers are used as carbon fiber precursors in step a).
[0056] For example, PAN polymers can be spun as solutions into filaments by wet spinning and consolidation and combined into ropes (fiber bundles). PAN copolymers generally have a lower melting point than PAN homopolymers and are therefore suitable not only for wet spinning processes but also for melt spinning processes. The PAN fibers obtained in this way are usually subjected to oxidative cyclization (also referred to as oxidation or stabilization for short) at elevated temperatures of about 180° C. to 300° C. in an oxygen-containing atmosphere. The chemical crosslinking thus produced helps to improve the shape stability of the fibers.
[0057] The fibers obtained during the oxidative cyclization can be used as precursors for carbon fibers in step a) without further treatment. The fibers obtained during the oxidative cyclization can also be subjected to at least one treatment step, which is preferably selected from cleaning, coating with at least one sizing agent, drying and a combination of at least two of these treatment steps. In order to clean the electrochemically oxidized fibers, they can be subjected to a washing treatment. Washing is specifically used to remove fiber fragments. There is usually a drying step after washing. In order to change the surface properties, at least one sizing agent can be at least partially coated on the fibers. For example, the sizing agent can be used in the form of a solution in a suitable solvent or in the form of a dispersion. In order to apply the coating, the fibers can be passed through a sizing bath, for example. During the water jet consolidation process in step c), the slurry will at least partially fall off the fibers. If the water used to consolidate the fiber web in step c) is at least partially recovered, it may be advantageous to treat the wastewater from the water jet consolidation, during which the slurry contained in the wastewater is partially or completely removed.
[0058] After the fibers have been coated with at least one sizing agent, they are usually (further) dried. For example, the drying can be carried out using hot air, hot plates, heated rollers or radiant heat.
[0059] The carbon fiber precursor obtained in this way can be used as a fiber composition in step a) of the method according to the invention and can be further processed. As an alternative, a fiber composition comprising or consisting of PAN fibers can be pyrolyzed at a temperature of at least 1000° C., wherein the PAN precursor is converted into carbon fibers. With regard to the pyrolysis conditions, reference is made to the following explanation of step e). The carbon fibers obtained in this way can likewise be used as a fiber composition in step a) of the method according to the invention and can be further processed.
[0060] Step b)
[0061] In step b) of the method according to the present invention, the fiber composition provided in step a) is subjected to a process for manufacturing a fiber web (carbon fiber nonwoven fabric or carbon fiber precursor nonwoven fabric). Suitable nonwoven fabric manufacturing processes are known to those skilled in the art, for example, as described in H.Fuchs, W.Albrecht, Vliesstoffe (nonwoven fabric), 2.Aufl.2012 (2012 second edition), S.121ff (page 121 and below), Wiley-VCH. These processes include, for example, dry processes, wet processes, extrusion processes, and solvent processes. In a preferred embodiment, in step b), a dry-laid web process is applied to the fiber composition provided in step a) to manufacture a fiber web. In principle, dry-laid nonwoven fabrics can be manufactured according to a carding process or an aerodynamic process. The carding process uses a napping machine or a carding machine to form a fiber web, while the aerodynamic process uses air to form a nonwoven fabric with fibers. If necessary, the fiber web can be stacked together in multiple layers to form a nonwoven fabric. The dry-laid process in step b) can include a change in the properties, for example by stretching the nonwoven. For example, this can achieve a thickness calibration of the nonwoven and / or a pre-consolidation of the fiber web.
[0062] Step c)
[0063] In step c) of the method according to the invention, the fiber web obtained in step b) is consolidated into a nonwoven fabric by the action of aqueous fluid jets. Aqueous fluid jets also include fluid streams and steam jets.
[0064] In principle, the known mechanical reinforcement processes (also known as spunlace processes) used to achieve this purpose are suitable for water jet reinforcement. Steam jet technology, which uses superheated steam jets to reinforce nonwovens, is also applicable in principle. Such processes are known to those skilled in the art. In a specific nonwoven mechanical reinforcement method, water with a pressure of about 20 bar to 500 bar is introduced to the nonwoven to be reinforced through a large number of nozzles. These nozzles are arranged in one or more rows in so-called water needle plates. Each row of these water needle plates has a large number of nozzles. The maximum number of nozzles can reach 20,000 nozzles per plate, with typical nozzle diameters ranging from 0.05 mm to 0.5 mm. The tolerances of the nozzle apertures are usually very small, for example less than 2 mm. In order to obtain defect-free nonwovens, it is necessary that the aperture of the nozzle does not change during operation, in particular that the nozzle is not closed.
[0065] It has been found that the pH value of the water used to consolidate the fiber web (nonwoven) is crucial to the quality of the gas diffusion layer for fuel cells made from the fiber web. Therefore, a key feature of the method of the present invention is that the water used to consolidate the fiber web in step c) has a pH value (25° C.) in the range of 5.5 to 8.0, preferably in the range of 5.5 to 7.0, particularly preferably in the range of 6.0 to 6.9.
[0066] It has also been found that the conductivity of the water used to consolidate the fiber web (nonwoven) is also crucial for the quality of the gas diffusion layer for fuel cells produced from the fiber web. Therefore, the water used to consolidate the nonwoven in step c) preferably has a conductivity of up to 250 microSiemens / cm (μS / cm) at 25° C. Particularly preferably, the water used in step c) has a conductivity of up to 200 microSiemens / cm at 25° C., in particular a conductivity of up to 150 microSiemens / cm at 25° C., and in particular a conductivity of up to 100 microSiemens / cm at 25° C.
[0067] Conductivity is a cumulative indicator of ion concentration (i.e. the proportion of dissociated substances dissolved in a certain amount of water). Conductivity depends mainly on the concentration and degree of dissociation of dissolved substances, the valence and mobility of the formed cations and anions, and temperature. The measurement of conductivity is based on the ohmic resistance or the reciprocal of the resistance (i.e. the conductivity coefficient (in Siemens S = Ω) of the water sample to be analyzed. -1 )) Determination. Conductivity can be measured using a commercially available conductivity meter (conductivity meter). The measured value is usually in S / cm (Siemens / cm), or in microSiemens / cm for water samples with low ion load.
[0068] Process water and operating water for industrial processes generally come from the public drinking water network or are extracted from wells, rivers and lakes. Drinking water and process water with high water quality requirements are usually checked for their composition and, if necessary, treated. The purity requirements for water vary greatly in different application areas. For example, drinking water is a colorless, transparent liquid with no odor, free of harmful microorganisms and substances, but rich in important minerals and salts. This water is of food quality, but is not necessarily suitable for many technical applications. For example, according to the Drinking Water Ordinance (TrinkwV 2001, new version of March 10, 2016), drinking water in Germany must have a pH value of 6.5 to 9.0, usually in the range of 7.0 to 8.5. According to the Drinking Water Ordinance, the limit value for conductivity is 2790 microsiemens / cm at 25°C. The conductivity of tap water supplied by German waterworks at 25°C is between 250 microsiemens / cm and 1000 microsiemens / cm, depending on the hardness level. The main inorganic cations are Na + , K + , Ca2+ and Mg 2+ .
[0069] The Na content of the water used in step c) + The ion content is preferably at most 200 ppm (weight ratio), particularly preferably at most 25 ppm (w / w).
[0070] K of the water used in step c) + The ion content is preferably at most 200 ppm (weight ratio), particularly preferably at most 10 ppm (weight ratio).
[0071] Mg of the water used in step c) 2+ The ion content is preferably at most 10 ppm (by weight).
[0072] The Ca content of the water used in step c) 2+ The ion content is preferably at most 200 ppm (weight ratio), particularly preferably at most 40 ppm (weight ratio).
[0073] In order to provide the water used in step c) of the present invention, the existing drinking water or process water can be treated to set the pH value and / or reduce the ion concentration. Such treatments include ion exchange, electrodeionization, membrane processes (such as nanofiltration, reverse osmosis and electrodialysis), thermal treatments (such as distillation, flash evaporation), etc.
[0074] In a preferred first embodiment, nanofiltration, reverse osmosis or a combination of these processes is used to reduce the ion concentration. Both nanofiltration and reverse osmosis are to make the water to be treated pass through a semipermeable membrane at a pressure higher than the osmotic pressure to obtain a permeate with a reduced ion concentration. Nanofiltration is carried out at a lower pressure than reverse osmosis, so its purification capacity is lower than reverse osmosis, but it is sufficient in many cases. It is also possible to first perform pre-purification by nanofiltration and then further reduce the ion concentration by reverse osmosis.
[0075] In a preferred second embodiment, an ion exchange method is used to reduce the ion concentration. To this end, the existing drinking water or process water (raw water) is usually contacted with at least one cation exchange resin and at least one anion exchange resin. In another suitable embodiment, the raw water is first treated with at least one strongly acidic cation exchanger so that the cations in the water are exchanged with hydrogen ions (H + ) exchange. Subsequently, the water thus obtained is treated with at least one strongly basic anion exchanger so that the negatively charged ions are exchanged with hydroxide ions (OH -) exchange. If necessary, the water obtained after contact with the cation exchanger can also be contacted with at least one weakly basic anion exchanger before the strongly basic exchanger. If necessary, the water can be degassed with carbon dioxide after the cation exchanger or (if any) between the weakly basic and strongly basic anion exchangers.
[0076] In order to set the properties of the water used in step c), it is also possible to mix two or more starting waters of different composition. These compositions differ in at least one property, such as pH or the content of a certain ion type. In a particular embodiment, to set the pH of the water used in step c), a mixture of at least one water having a pH value below the target value and at least one water having a pH value above the target value is used. In a very particular embodiment, to set the pH of the water used in step c), a mixture of at least one water having a lower pH value obtained by nanofiltration or reverse osmosis and at least one water having a higher pH value obtained by ion exchange is used.
[0077] CO 2 The content and the resulting dissociation of carbonic acid are of great significance to the pH value of the water used in step c). 2 and water to bicarbonate anions (HCO 3 - ) and oxonium ions (H 3 O + ), which occurs in the range of pH 4.3 to pH 8.2. Depending on the specific source, the concentration of carbon dioxide dissolved in drinking water or process water ranges from a few milligrams per liter to more than 20 milligrams per liter. Depending on the specific source, the concentration of bicarbonate anions in drinking water or process water can reach hundreds of grams per liter. Due to the absorption of carbon dioxide from the surrounding air, the pH value of pure water is mostly weakly acidic, and the pH value of distilled water can reach an acidic pH value of about 5.8. Only freshly distilled water has a pH value of about 7, but once it comes into contact with carbon dioxide, the pH value becomes weakly acidic within a few hours.
[0078] The effect of dissolved CO2 on pH depends on the process chosen to treat the raw water. Bicarbonate anions can be effectively separated from the raw water by processes such as ion exchange, nanofiltration or reverse osmosis. 2 This is different from the case of carbon dioxide, which is essentially not blocked by membranes used for nanofiltration and reverse osmosis, for example. Therefore, the permeate of nanofiltration and reverse osmosis usually has an acidic pH value due to the dissociation of dissolved carbon dioxide, which can have a value of less than pH 6. In addition, the permeate of dissolved CO 2 Bicarbonate anions are then produced, thereby increasing the conductivity. Therefore, in a specific embodiment, the raw water is degassed with carbon dioxide prior to nanofiltration and reverse osmosis treatment.
[0079] For example, CO 2 Degassing tower (CO 2 -Riesler) for carbon dioxide degassing. In this process, water is dripped into the stripping column and the stripping air is guided in countercurrent to remove CO 2 Removal from water. As an alternative or in addition, carbon dioxide can be removed using a membrane degassing process.
[0080] In a particular embodiment of the method according to the invention, the water used for consolidating the fiber web in step c) is partially or completely recycled. The method according to the invention can thus reduce the demand for new water for water jet consolidation and the amount of wastewater to be treated. It can be ensured that the water used for treating the fiber web always has an electrical conductivity within the scope of the invention and it can also be avoided that the fiber web is contaminated by components contained in the wastewater from water jet consolidation. For this purpose, the wastewater from water jet consolidation can be partially or completely treated and / or exchanged.
[0081] The treatment and / or exchange of water jet aggravation wastewater may be performed continuously or intermittently.
[0082] The following method is preferred: the fiber web is consolidated into a nonwoven fabric by the action of a jet of aqueous fluid, a wastewater flow is discharged from the treatment of the fiber web, a set value for the conductivity of the wastewater flow is determined, the actual value of the conductivity of the wastewater flow is determined, after the deviation of the actual value from the set value reaches a limit value, the wastewater flow is at least partially treated and / or exchanged with water with a lower ion concentration, and the wastewater flow is at least partially returned to the treatment of the fiber web.
[0083] For treatment, the wastewater stream may be subjected to a reduction in ion concentration as previously described. In addition, the wastewater stream may be further purified, for example to remove fibers and fiber fragments.
[0084] Step d)
[0085] The nonwoven obtained in step c) can be subjected to a thermal and / or mechanical treatment as required for drying and / or further consolidation. Suitable drying methods are convection drying, contact drying, radiation drying and combinations thereof.
[0086] The nonwoven obtained in step c) is preferably treated by calendering. Calendering allows a further thermal consolidation of the nonwoven and a simultaneous thickness calibration. In the process, a plurality of nonwoven layers can also be joined together. In a particular embodiment, the nonwoven obtained in step c) contains thermoplastic fibers which are used as bonding fibers and are usually carbonizable. In this case, the nonwoven can be consolidated by hot calendering in step d) and bonding points can be formed at which the fibers are plasticized and welded together (thermal bonding).
[0087] Step e)
[0088] If the fiber composition used in step a) contains a precursor of carbon fibers, the nonwoven fabric is pyrolyzed at a temperature of at least 1000° C. in step e). Depending on the temperature during the pyrolysis, a distinction is made between carbonization and graphitization. Carbonization refers to a treatment at a temperature of about 1000° C. to 1500° C. in an inert atmosphere in order to remove volatile products. By graphitization (i.e. heating to about 2000° C. to 3000° C. in an inert gas), so-called high modulus fibers or graphite fibers can be obtained. During the pyrolysis process, the carbon content increases, for example, from about 67 wt % when the treatment is carried out at a temperature below 1000° C. to about 99 wt % when the treatment is carried out at a temperature above 2000° C. In particular, the fibers obtained by graphitization are of high purity, light weight, high strength, and have very good electrical and thermal conductivity.
[0089] Step f)
[0090] Optionally, after step c), step d) or step e), the nonwoven fabric may be sized with at least one additive. These additives are preferably selected from hydrophobic agents f1), conductivity-improving additives f2), other additives f3) different from f1) and f2), and mixtures thereof.
[0091] The nonwoven fabric is preferably coated and / or impregnated (sized) with a hydrophobic agent f1), which comprises at least one fluoropolymer. Preferably, the fluoropolymer is selected from polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), perfluoroalkoxy polymer (PFA) and mixtures thereof. Perfluoroalkoxy polymers are, for example, copolymers of tetrafluoroethylene (TFE) and perfluoroalkoxy vinyl ethers, such as perfluorovinyl propyl ether. Polytetrafluoroethylene is preferably used as the fluoropolymer.
[0092] The mass proportion of the fluoropolymer f1) is preferably 0.5% to 40%, particularly preferably 1% to 20%, and in particular 1% to 10%, based on the mass of the nonwoven fabric. In a specific embodiment, the fluoropolymer is PTFE, and its mass proportion is 0.5% to 40%, preferably 1% to 20%, and in particular 1% to 10%, based on the mass of the nonwoven fabric.
[0093] Even without conductivity-improving additives, nonwovens often already have good electrical and thermal conductivity due to the carbon fibers used. However, in order to improve the electrical and thermal conductivity, the nonwoven can be further sized with at least one conductivity-improving additive f2). The nonwoven is preferably sized with a conductivity-improving additive f2), which is selected from metal particles, carbon black, graphite, graphene, carbon nanotubes (CNT), carbon nanofibers and mixtures thereof. Preferably, the conductivity-improving additive f2) contains carbon black or consists of carbon black. For example, the sizing of the nonwoven with at least one conductivity-improving additive f2) can be carried out together with the sizing with the polymer f1) and / or other additives f3). The nonwoven is preferably sized with an aqueous dispersion.
[0094] Preferably, the mass of the conductivity improving additive f2) is 0.5% to 45%, preferably 1% to 25%, based on the mass of the non-woven fabric. In a specific embodiment, the conductivity improving additive f2) contains carbon black or consists of carbon black, and its mass is 0.5% to 45%, preferably 1% to 25%, based on the mass of the non-woven fabric.
[0095] The nonwoven fabric can be further sized with at least one other additive f3). These additives include, for example, polymer binders different from components f1) and f2), surface-active substances, etc. Suitable binders f3) are, for example, furan resins, etc. Specifically, the nonwoven fabric can be further sized with at least one polymer different from f1), wherein high-performance polymers are preferably used. The other polymer f3) is preferably selected from polyaryletherketones, polyphenylene sulfides, polysulfones, polyethersulfones, partially arylated (co)polyamides, polyimides, polyamide-imides, polyetherimides, and mixtures thereof. For example, the sizing of the nonwoven fabric with at least one additive f3) can be carried out together with the sizing with polymer f1) and / or conductivity-improving additive f2). The binder f3) can then be cured as needed. For example, the curing can be carried out together with drying and / or sintering after sizing with polymer f1), or separately therefrom.
[0096] Preferably, the total mass of the other additives f3) is 0% to 80%, preferably 0% to 50%, based on the mass of the nonwoven fabric. If the nonwoven fabric further comprises at least one other additive f3), the total mass of the other additives f3) is 0.1% to 80%, preferably 0.5% to 50%, based on the mass of the nonwoven fabric.
[0097] The nonwoven preferably has a thickness in the range of 50 μm to 500 μm, particularly preferably 100 μm to 400 μm. This thickness relates to the nonwoven in the uncompressed state without sizing, ie before the GDL is installed in the fuel cell.
[0098] The nonwoven fabric can be sized with components f1), f2) and / or f3) by application methods known to those skilled in the art, in particular by coating and / or impregnating. The nonwoven fabric is preferably coated and / or impregnated by a process selected from the group consisting of padding, brushing, spraying, surface padding and combinations thereof.
[0099] In the padding process, the nonwoven is guided through a padder (immersion tank) with a solution or dispersion containing the additive and is then pressed to the desired additive dosage by means of a roller pair with adjustable pressure and, if necessary, gap.
[0100] The coating process is divided into gravure printing and screen printing. In gravure printing, for example, a blade-shaped ground steel belt with or without a supporting blade is used as a doctor blade. The supporting blade has the function of wiping (scraping off) excess additive-containing solution or dispersion from the connecting strip of the impression cylinder. In screen printing, the doctor blade is usually made of rubber or plastic with a sharpened or rounded edge.
[0101] The spraying process is to apply a solution or dispersion containing additives to the nonwoven to be sized by means of at least one nozzle (particularly at least one slot nozzle).
[0102] The surface rolling process (licking roller) is preferably used to coat the material bottom side of the horizontal web. The coating medium can be applied to the web in the opposite or same direction. Indirect coating with a smaller application amount can be achieved by means of a transfer roller.
[0103] In a particular embodiment, the nonwoven sized with components f1), f2) and / or f3) in step f) of the process according to the invention is dried and / or heat treated. Suitable processes for drying and / or heat treating nonwovens which have been coated and / or impregnated with solutions or dispersions containing additives are known in principle. The drying and / or heat treatment is preferably carried out at a temperature in the range of 20° C. to 250° C., particularly preferably at a temperature in the range of 40° C. to 200° C.
[0104] Step g)
[0105] In a preferred embodiment, the gas diffusion layer according to the invention consists of a two-layered composite based on a nonwoven fabric and a microporous layer (MPL) on one surface of the nonwoven fabric. To produce the gas diffusion layer, the nonwoven fabric obtained in step c), step d), step e) or step f) can be coated with a microporous layer, respectively.
[0106] Compared to macroporous nonwovens, MPL is microporous, with a pore size generally well below one micrometer, preferably up to 900 nm, particularly preferably up to 500 nm, in particular up to 300 nm. The average pore size of MPL is preferably in the range of 5 nm to 200 nm, particularly preferably 10 nm to 100 nm. The average pore size can be determined by mercury intrusion. MPL contains conductive carbon particles, preferably carbon black or graphite, in a matrix consisting of a polymer binder. Preferred binders are the aforementioned fluorinated polymers, in particular polytetrafluoroethylene (PTFE).
[0107] The microporous layer preferably has a thickness in the range of 10 μm to 100 μm (micrometers), particularly preferably 20 μm to 50 μm. This thickness relates to the uncompressed state of the microporous layer B), ie before the GDL is installed in a fuel cell.
[0108] The gas diffusion layer according to the invention preferably has a thickness (total thickness of nonwoven and MPL) in the range of 80 μm to 1000 μm, particularly preferably 100 μm to 500 μm. This thickness relates to the uncompressed state of the GDL, ie before the GDL is installed in a fuel cell.
[0109] Another subject of the invention is a fuel cell comprising at least one gas diffusion layer as described above or a gas diffusion layer obtained by a method as described above. In principle, the gas diffusion layer according to the invention is suitable for all common fuel cell types, in particular low-temperature proton exchange membrane fuel cells (PEMFC). Please make full reference to the above description of the construction of the fuel cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] Figure 1 The metal content (Ca) of untreated nonwovens and nonwovens reinforced with water of different conductivity is shown. 2+ 、Na + Mg 2+ and K + ).
[0111] Figure 2 The Ca of the base nonwoven fabric reinforced with water of different conductivity, the carbon fiber nonwoven fabric obtained by carbonizing the base nonwoven fabric, and the gas diffusion layer obtained by applying MPL are shown. 2+ Ions and Na + The content of ions.
[0112] Figure 3 and Figure 2 Similarly, Ca 2+ Ions and Na + The total content of ions.
[0113] The present invention will be described below with the aid of examples, which should not be construed as limiting.
[0114] Examples
[0115] The metal contents (Ca) of the base nonwoven fabric made of oxidized polyacrylonitrile fibers, the carbonized nonwoven fabric produced therefrom and GDL were determined by ICP-AES (Inductively Coupled Argon Plasma Atomic Emission Spectrometry). 2+ 、Na + Mg 2+ and K + ). The samples can be pretreated (digested) according to the acid digestion method EPA 3050A for sediments, silts, and soils. This process includes the following steps:
[0116] 1.) Perform nitric acid digestion at 95°C for 15 minutes.
[0117] 2.) Further nitric acid was added while continuing the digestion for 1 hour.
[0118] 3.) Remove from hot plate; add deionized water and 20% hydrogen peroxide solution.
[0119] 4.) Heat again on the hot plate for about 15 minutes, and remove from the hot plate again after bubbles have completely stopped forming.
[0120] 5.) Add concentrated hydrochloric acid and digest again for 1 hour.
[0121] Water with conductivity in accordance with Table 1 below was used for water jet consolidation. Comparative water 1 corresponds to the process water commonly used in the conventional nonwoven water jet consolidation process. For the water of batches 2 and 3, the ion concentration was reduced by nanofiltration.
[0122] Table 1
[0123] Batch of water Conductivity [μSiemens / cm] <![CDATA[pH value #) > V1(Comparison) 290 - 2 100 6.1 3 22 6.1
[0124] #) Determined according to DIN EN ISO 10523-C5:2012-04
[0125] Manufacturing Examples
[0126] To produce the base nonwoven, a dry-laid web made of 100% oxidized polyacrylonitrile fibers was placed on a carding device. The web was fed into a consolidation unit, where the fibers were interlaced and interwoven on both sides by means of high-energy water jets at a pressure of about 100 bar in the first stage and about 200 bar in the second stage. The water quality used was in accordance with Table 1. The nonwoven was dried and rolled up, with a grammage of 150 g / m after water jet consolidation and drying. 2The nonwoven is subsequently subjected to thickness calibration, whereby the thickness of the water jet reinforced nonwoven is reduced to 0.25 mm. The nonwoven is then fed into a carbonization unit, where carbonization takes place at approximately 1000° C. to 1400° C. in a nitrogen atmosphere.
[0127] The nonwoven fabric was sized with an impregnation composition, which, calculated on solids, contained 70% carbon black and 30% PTFE. The sizing was performed by impregnation with an aqueous dispersion using a padding machine, the sizing weight accounting for 15% of the mass of the GDL substrate (equivalent to 15 g / m 2 ). It was then dried at 180°C and sintered at 400°C. An MPL slurry containing 2.0 wt% PTFE and 7.8 wt% carbon in distilled water was then applied to the substrate obtained in this way. The nonwoven was subsequently dried at 160°C and sintered at 400°C. The resulting MPL loading was 24 g / m 2 .
Claims
1. A method for manufacturing a gas diffusion layer for a fuel cell, characterized in that: in, a) providing a fiber composition comprising carbon fibers and / or precursors of carbon fibers, b) subjecting the fiber composition provided in step a) to a process for producing a fiber web, c) consolidating the fiber web to form a nonwoven fabric by the action of jets of aqueous fluid, wherein the water used has a pH value in the range of 5.5 to 8.0, d) optionally subjecting the nonwoven fabric obtained in step c) to a thermal and / or mechanical treatment for drying and / or further consolidation, e) pyrolyzing the nonwoven at a temperature of at least 1000° C. if the fiber composition used in step a) comprises a precursor of carbon fibers.
2. The method according to claim 1, characterized in that The water used in step c) for consolidating the fiber web has a pH value in the range from 5.5 to 7.0, particularly preferably in the range from 6.0 to 6.
9.
3. The method according to claim 1 or 2, characterized in that: The water used for consolidating the fiber web in step c) has an electrical conductivity of up to 250 microSiemens / cm at 25°C, preferably up to 200 microSiemens / cm at 25°C, and in particular up to 150 microSiemens / cm at 25°C.
4. The method according to any one of the preceding claims, characterized in that The method further comprises sizing the nonwoven fabric obtained in step c), step d) or step e) with at least one additive (step f), wherein the additive is preferably selected from hydrophobic agents f1), conductivity improving additives f2), other additives f3), and mixtures thereof.
5. The method according to any one of the preceding claims, characterized in that The method further comprises coating a microporous layer on the nonwoven fabric (step g) obtained in step c), step d), step e) or step f).
6. The method according to any one of the preceding claims, characterized in that The fiber composition provided in step a) comprises a precursor of carbon fiber, and the precursor of carbon fiber is selected from non-oxidized polyacrylonitrile fiber, oxidized polyacrylonitrile fiber and a mixture thereof.
7. The method according to any one of claims 1 to 6, characterized in that The fiber composition provided in step a) further comprises other fibers, and the other fibers are selected from fibers made of phenolic resin, polyester, polyolefin, cellulose, aramid, polyether ketone, polyether ester ketone, polyether sulfone, polyvinyl alcohol, lignin, asphalt and mixtures thereof.
8. The method according to any one of claims 1 to 6, characterized in that The fiber composition provided in step a) consists of polyacrylonitrile fibers, in particular, polyacrylonitrile homopolymer fibers.
9. The method according to any one of the preceding claims, characterized in that In step b), the fiber composition provided in step a) is subjected to a dry-laid web forming process to produce a fiber web.
10. The method according to any one of the preceding claims, characterized in that Therein, the water used in step c) for consolidating the fiber web is at least partially recovered.
11. The method according to claim 10, characterized in that The fiber web is consolidated into a nonwoven fabric by the action of a jet of aqueous fluid, a wastewater flow is discharged from the treatment of the fiber web, a set value for the electrical conductivity of the wastewater flow is determined, an actual value of the electrical conductivity of the wastewater flow is measured, and after the deviation of the actual value from the set value reaches a limit value, the wastewater flow is at least partially treated and / or exchanged with water with a lower ion concentration, and the wastewater flow is at least partially returned to the treatment of the fiber web.
12. The method according to any one of the preceding claims, characterized in that In step d), the nonwoven obtained in step c) is further consolidated by calendering.
13. The method according to any one of claims 4 to 12, characterized in that The hydrophobizing agent f1) comprises at least one fluorine-containing polymer.
14. The method according to any one of claims 4 to 13, characterized in that The conductivity improving additive f2) is selected from metal particles, carbon black, graphite, graphene, carbon nanotubes (CNTs), carbon nanofibers and mixtures thereof.
15. The method according to any one of claims 4 to 14, characterized in that The other additives f3) are selected from polymer binders different from the components f1) and f2), surface-active substances and mixtures thereof.
16. The method according to any one of claims 4 to 15, characterized in that The nonwoven fabric is subjected to heat treatment during or after coating and / or impregnating with the hydrophobic agent in step f1).
17. A nonwoven fabric obtainable by a method comprising the following steps, characterized in that in: a) providing a fiber composition comprising carbon fibers and / or precursors of carbon fibers, b) subjecting the fiber composition provided in step a) to a process for producing a fiber web, c) consolidating the fiber web to form a nonwoven by the action of jets of aqueous fluid, wherein the water used has a pH value in the range from 5.5 to 8.0, preferably in the range from 5.5 to 7.0, particularly preferably in the range from 6.0 to 6.
9.
18. The nonwoven fabric according to claim 17, characterized in that The water used in step c) has an electrical conductivity of up to 250 microSiemens / cm at 25°C, preferably, has an electrical conductivity of up to 200 microSiemens / cm at 25°C, and in particular, has an electrical conductivity of up to 150 microSiemens / cm at 25°C.
19. A gas diffusion layer obtained by the method according to any one of claims 1 to 16.
20. A fuel cell, characterized in that: It comprises at least one gas diffusion layer obtained by a method as claimed in any one of claims 1 to 16.
Citation Information
Patent Citations
Processing technology of spunlace non-woven fabric for cotton soft towel
CN111691063A
Antibacterial anti-radiation non-woven fabric
CN113043670A
Processing method of water electret melt-blown fabric
CN113337964A
Textile structures, for use in gas diffusion layers for fuel cells, comprise fibers, to which coating is covalently bonded
DE102006060932A1
Hydrophilic carbon fiber sheetlike material, carbon fiber electrode material and method for producing the same