Method for manufacturing polarizing plate with protective film
By controlling the temperature difference and tension in the bonding process, the reverse curling problem of polarized plate single-piece body with protective film is solved, the bonding quality is improved, and the risk of bonding errors and bubble mixing is reduced.
Patent Information
- Application Number
- CN202380031566.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-07
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-12
AI Technical Summary
Polarizing plates with protective films are prone to reverse curl when made into monolithic bodies, resulting in bonding errors and bubbles mixed into the image display element.
By controlling the difference between the atmosphere temperature and the polarizing plate temperature in the bonding process, ensuring that 2℃≤T1-T2≤15℃, and applying tension between the bonding rollers, the tension of the polarizing plate is more than 20kgf and less than 100kgf, and the protective film is protected The tension is 10 kgf or more and 50 kgf or less, and the absorption axis of the polarizing plate is bonded in parallel with the MD direction of the protective film.
It effectively suppresses reverse curl in the monolithic body, reduces the risk of fitting errors and bubble mixing, and improves the fitting quality of the polarizing plate.
Smart Images

Figure CN118946835A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a polarizing plate with a protective film. Background Art
[0002] In recent years, image display devices such as liquid crystal display devices and organic EL display devices, and mobile terminals such as smartphones, have been rapidly advancing in terms of design and portability, with larger screens and thinner thicknesses. In order to achieve long-term driving with a limited thickness, the polarizing plates used are also required to be high-brightness, thin and lightweight.
[0003] As a polarizing plate, a polarizing plate obtained by bonding a protective film containing triacetyl cellulose (TAC) to a polarizer containing a polyvinyl alcohol-based resin using an adhesive is generally used in the past. However, in recent years, from the viewpoints of thin filmization, durability, cost, productivity, etc., protective films containing resins other than TAC have also been used (e.g., Patent Document 1).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2004-245925 Summary of the invention
[0007] Problems to be solved by the invention
[0008] A single piece of a polarizing plate obtained by cutting out a long polarizing plate is easily deformed to bend into a bow shape. In this specification, this deformation is also referred to as "curl".
[0009] Polarizing plates are usually circulated in the market in the form of polarizing plates with protective films attached to a protective film (also called a surface protective film) that can be peeled off to protect the surface. In polarizing plates with protective films, there is also a tendency to easily curl when made into a single piece. In the case of polarizing plates with protective films, in addition to curling, there is also the problem of bubbles being easily mixed in when the protective film and the polarizing plate are attached.
[0010] There are two types of curling in a single piece of polarizing plate with a protective film: "positive curling" and "negative curling". In a single piece of polarizing plate with a protective film, the so-called "positive curling" is curling that makes the surface on the polarizing plate side convex, and the so-called "negative curling" is curling that makes the surface on the protective film side convex.
[0011] If reverse curling occurs, it is easy to cause the following undesirable conditions when the polarizing plate side of a single-piece body of a polarizing plate with a protective film is bonded to an image display element such as a liquid crystal unit, an organic EL element, etc. through an adhesive layer, that is, bonding errors occur or bubbles are mixed in at the interface between the adhesive layer and the image display element.
[0012] An object of the present invention is to provide a method for producing a polarizing plate with a protective film, which can suppress reverse curling when forming a single sheet.
[0013] Means for solving problems
[0014] The present invention provides the following method for producing a polarizing plate with a protective film.
[0015] [1] A method for producing a polarizing plate with a protective film, the method comprising a laminating step of laminating the polarizing plate by laminating the protective film on one side of the polarizing plate and then passing the polarizing plate between a pair of laminating rollers for pressing.
[0016] In the bonding step, when the atmosphere temperature is T1 [° C.] and the temperature of the supplied polarizing plate is T2 [° C.], the relationship of the following formula (1) is satisfied.
[0017] 2℃≤T1-T2≤15℃ (1)
[0018] [2] The manufacturing method according to [1], wherein in the laminating step, when the temperature of the supplied pellicle membrane is set to T3 [° C.], the relationship of the following formula (2) is satisfied.
[0019] 2℃≤T3-T2≤15℃ (2)
[0020] [3] The method according to [1] or [2], wherein the polarizing plate comprises, in this order, a first thermoplastic resin film, a polarizer, and a second thermoplastic resin film.
[0021] The thickness of the first thermoplastic resin film is greater than 40 μm.
[0022] The thickness of the second thermoplastic resin film is 40 μm or less.
[0023] In the bonding step, the protective film is stacked on the surface side of the first thermoplastic resin film of the polarizing plate.
[0024] [4] The production method according to any one of [1] to [3], wherein in the laminating step, the tension of the pellicle before passing through the pair of laminating rollers is 10 kgf to 50 kgf.
[0025] [5] The production method according to any one of [1] to [4], wherein in the laminating step, the tension of the polarizing plate before passing through the pair of laminating rollers is 20 kgf to 100 kgf.
[0026] [6] The production method according to any one of [1] to [5], wherein in the laminating step, the laminating is performed so that the absorption axis of the polarizing plate and the MD direction of the protective film are parallel to each other.
[0027] [7] The production method according to any one of [1] to [6], wherein the thickness of the polarizing plate is 100 μm or less.
[0028] [8] The production method according to any one of [1] to [7], wherein in the bonding step, the polarizing plate and the protective film are in a long strip shape.
[0029] [9] The manufacturing method according to [8], further comprising, after the laminating step, a cutting step of cutting out a single piece from the polarizing plate with a protective film.
[0030] Effects of the Invention
[0031] According to the present invention, it is possible to provide a method for producing a polarizing plate with a protective film in which reverse curling when formed into a single sheet is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a side view schematically showing a method for producing a polarizing plate with a protective film according to the present embodiment.
[0033] Figure 2 This is a schematic cross-sectional view showing an example of the layer structure of a polarizing plate.
[0034] Figure 3 It is a schematic cross-sectional view showing another example of the layer structure of the polarizing plate.
[0035] Figure 4 This is a schematic cross-sectional view showing an example of the layer structure of a single body of a polarizing plate with a protective film.
[0036] Figure 5 It is a schematic diagram explaining the method of preparing a sample for measuring the TD curl amount and the measurement points of the TD curl amount. DETAILED DESCRIPTION
[0037] <Method for Manufacturing Polarizing Plate with Protective Film>
[0038] Figure 1The manufacturing method of the present embodiment includes a laminating step of laminating a polarizing plate 2 by laminating a pellicle 1 on one side of the polarizing plate 2 and then passing the pellicle 1 through a pair of laminating rollers 5 and 5 to press the pellicle 1 on the one side of the polarizing plate 2 .
[0039] In the method for manufacturing a polarizing plate with a pellicle of this embodiment, in the laminating step, the polarizing plate and the pellicle are in a long strip shape, and after the laminating step, a cutting step of cutting a single piece from the polarizing plate with a pellicle may be further included.
[0040] The term "single sheet" as used herein refers to a film of smaller size cut out from a film of larger size (eg, a long strip (tape) film).
[0041] In the bonding step, when the atmosphere temperature is T1[°C] and the temperature of the supplied polarizing plate is T2[°C], the relationship T1>T2 is satisfied, and the relationship of the following formula (1) is further satisfied, preferably the relationship of the following formula (1a) is satisfied.
[0042] 2℃≤T1-T2≤15℃ (1)
[0043] 3℃≤T1-T2≤12℃ (1a)
[0044] By satisfying the relationship of the above formula (1), the reverse curl in the single body of the polarizing plate with a protective film can be suppressed. The so-called suppression of reverse curl in this specification can be any one of reducing the curling amount of reverse curl, not generating reverse curl, generating forward curl, and increasing the forward curling amount. This is because the increase in the forward curling amount means that the force generating the reverse curl becomes relatively smaller than the force generating the forward curl. Although the reason why the reverse curl can be suppressed by satisfying the relationship of the above formula (1) is not clear, it can be speculated that this is because, in the bonding process, the polarizing plate expands as its temperature slowly rises from temperature T1 to temperature T2, and the expansion after the protective film is bonded acts in the direction of suppressing the reverse curl due to the difference in the amount of expansion of the protective film. In addition, by setting T1-T2≤15°C, it is easy to prevent condensation from occurring on the polarizing plate, etc.
[0045] It should be noted that the protective film usually has a smaller expansion coefficient than the polarizing plate, so even if its temperature rises at the same rate as the polarizing plate, its expansion amount is smaller than that of the polarizing plate. When its temperature rises less than that of the polarizing plate, its expansion amount is smaller than that of the polarizing plate.
[0046] From the above viewpoints, the expansion coefficient of the protective film is preferably smaller than the expansion coefficient of the polarizing plate. In addition, if the temperature of the protective film provided to the bonding process is set to T3 [°C], it is preferred to satisfy the relationship of T3>T2, more preferably satisfy the relationship of the following formula (2), and even more preferably satisfy the relationship of the following formula (2a).
[0047] 2℃≤T3-T2≤15℃ (2)
[0048] 3℃≤T3-T2≤12℃ (2a)
[0049] Here, the curl of the single piece of polarizing plate with a protective film can be classified into two types, "MD curl" and "TD curl" in addition to the above-mentioned classification of "forward curl" and "reverse curl". The so-called "MD curl" is curling caused by stress (contraction force, expansion force, etc.) in a direction parallel to the MD direction of the long strip of polarizing plate with a protective film from which the single piece of polarizing plate with a protective film is cut.
[0050] The so-called "TD curl" is curling caused by stress (contraction force, expansion force, etc.) in a direction parallel to the TD direction of the long strip of polarizing plate with a protective film from which the polarizing plate with a protective film is cut out. Specifically, the TD curling can be measured as follows, that is, a measurement sample (single sheet) is cut out from the long strip of polarizing plate with a protective film according to the description of Example 1 described later, and when the measurement sample is placed on a horizontal table with the concave side facing up, the curling (typically the curling in the transmission axis direction) of the two corners of the measurement sample on the diagonal line with the smaller angle with the TD direction of the long strip of polarizing plate with a protective film is measured and its size is measured.
[0051] The so-called "MD curl" is curling caused by stress (contraction force, expansion force, etc.) in a direction parallel to the MD direction of the long strip of polarizing plate with a protective film from which the polarizing plate with a protective film is cut. When the absorption axis direction of the polarizing plate in the long strip of polarizing plate with a protective film is parallel to the MD direction of the protective film, the MD curl can be measured as curling (curling in the absorption axis direction) of the two corners of the diagonal line of the measurement sample that has a smaller angle with the absorption axis direction of the polarizing plate of the measurement sample.
[0052] In the present invention, TD curling is focused. The so-called ability to suppress reverse curling that can be manufactured using the present invention means being able to suppress reverse curling of TD curling in a single sheet. In the present invention, since the reverse curling of TD curling of a single sheet can be suppressed, when a single sheet of a polarizing plate with a protective film is bonded to an image display element via an adhesive layer, bonding is easy, and the occurrence of bonding errors or the mixing of bubbles at the interface between the adhesive layer and the image display element can be suppressed. The curling generated in the single sheet of a polarizing plate with a protective film that can be manufactured using the present invention is preferably a positive curling in both TD curling and MD curling.
[0053] (1) Lamination process
[0054] (1-1) Polarizing plate provided to bonding process
[0055] (1-1-1) Configuration of Polarizing Plate
[0056] The polarizing plate is a polarizing element including at least a polarizer, and generally further includes a thermoplastic resin film bonded to one or both surfaces thereof.
[0057] The thermoplastic resin film may be a protective film for protecting a polarizing plate, other optical films having an optical function different from that of a polarizing plate, etc. Examples of other optical films include a phase difference film, a brightness enhancement film, and the like.
[0058] The thermoplastic resin film may include a resin layer (eg, an optical layer) laminated on the surface thereof. Examples of the resin layer include a hard coat layer, an antiglare layer, an antireflection layer, an antistatic layer, an antifouling layer, and the like.
[0059] The thermoplastic resin film may be bonded to the polarizing plate via an adhesive layer or a pressure-sensitive adhesive layer.
[0060] The thickness of the polarizing plate is usually 150 μm or less, and is preferably 100 μm or less, more preferably 80 μm or less, and further preferably 70 μm or less from the viewpoint of reducing the thickness of the polarizing plate.
[0061] The thickness of the polarizing plate is usually 20 μm or more or 30 μm or more.
[0062] Reference Figure 2 and Figure 3 Although examples of the layer configuration of the polarizing plate are described, the layer configuration is not limited to these examples.
[0063] Figure 2 The polarizing plate 2a shown includes a polarizer 10, a first thermoplastic resin film 20 bonded to one surface of the polarizer 10, and a second thermoplastic resin film 30 bonded to the other surface of the polarizer 10. The first and second thermoplastic resin films 20 and 30 are, for example, protective films.
[0064] Can be like Figure 3 One of the first and second thermoplastic resin films 20 and 30 is omitted like the polarizing plate 2b shown. The second thermoplastic resin film 30 is omitted in the polarizing plate 2b. Such a polarizing plate having a thermoplastic resin film only on one surface of the polarizer 10 is advantageous in reducing the thickness of the polarizing plate.
[0065] Although Figure 2 and Figure 3 Although not shown in the figure, the polarizing plate 10 and the first and second thermoplastic resin films 20 and 30 can be preferably bonded together using an adhesive.
[0066] The polarizing plate to be subjected to the bonding step is preferably in a long strip shape.
[0067] The length of the long polarizing plate provided to the laminating step is, for example, 100 to 20000 m, or preferably 1000 to 10000 m. The width of the long polarizing plate provided to the laminating step S101 is, for example, 0.5 to 3 m, or preferably 1 to 2.5 m.
[0068] (1-1—2) Polarizing plate
[0069] The polarizer 10 constituting the polarizing plate is an absorption-type polarizer having the following properties, that is, absorbing linear polarized light having a vibration plane parallel to its absorption axis and transmitting linear polarized light having a vibration plane orthogonal to the absorption axis (parallel to the transmission axis). An example of the polarizer 10 is a polarizer obtained by adsorbing and aligning a dichroic pigment on a uniaxially stretched polyvinyl alcohol resin film. Such a polarizer 10 can be manufactured, for example, by a method including the following steps, namely, a step of uniaxially stretching a polyvinyl alcohol resin film; a step of adsorbing the dichroic pigment by dyeing the polyvinyl alcohol resin film with a dichroic pigment; a step of treating the polyvinyl alcohol resin film adsorbed with the dichroic pigment with a crosslinking liquid such as an aqueous boric acid solution; and a step of washing with water after the treatment with the crosslinking liquid.
[0070] As the polyvinyl alcohol-based resin, a resin obtained by saponifying a polyvinyl acetate-based resin can be used. As the polyvinyl acetate-based resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other copolymerizable monomers can be mentioned. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and (meth)acrylamides having an ammonium group.
[0071] The term "(meth)acrylic" as used herein means at least one selected from acrylic and methacrylic groups, and the same applies to "(meth)acryloyl", "(meth)acrylate" and the like.
[0072] The saponification degree of the polyvinyl alcohol resin is usually 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may also be modified, for example, polyvinyl formal or polyvinyl acetal modified with aldehydes may be used. The average degree of polymerization of the polyvinyl alcohol resin is usually 1000 to 10000, preferably 1500 to 5000.
[0073] The saponification degree and average polymerization degree of the polyvinyl alcohol-based resin can be determined in accordance with JIS K 6726.
[0074] The film obtained by forming such a polyvinyl alcohol resin film can be used as a raw material film of the polarizer 10. There is no particular limitation on the method for forming the polyvinyl alcohol resin film, and a known method can be used. The thickness of the polyvinyl alcohol resin film is not particularly limited, but is, for example, about 10 to 150 μm, preferably 50 μm or less, and more preferably 35 μm or less.
[0075] The uniaxial stretching of the polyvinyl alcohol-based resin film can be carried out before the dyeing of the dichroic pigment, simultaneously with the dyeing, or after the dyeing. In the case of carrying out uniaxial stretching after dyeing, the uniaxial stretching can be carried out before the crosslinking treatment or in the crosslinking treatment. In addition, uniaxial stretching can also be carried out in these multiple stages.
[0076] During uniaxial stretching, the film may be stretched uniaxially between rollers having different peripheral speeds, or may be stretched uniaxially using a heated roller. In addition, the uniaxial stretching may be dry stretching in the air, or wet stretching in a state where the polyvinyl alcohol resin film is swollen using a solvent or water. The stretching ratio is usually 3 to 8 times.
[0077] As the method of dyeing the polyvinyl alcohol resin film with a dichroic pigment, for example, the film is immersed in an aqueous solution containing a dichroic pigment. As the dichroic pigment, iodine or a dichroic organic dye is used. It should be noted that the polyvinyl alcohol resin film is preferably immersed in water before the dyeing process.
[0078] As a crosslinking treatment after dyeing with a dichroic dye, a method of immersing the dyed polyvinyl alcohol-based resin film in an aqueous solution containing boric acid is generally adopted. When iodine is used as the dichroic dye, the aqueous solution containing boric acid preferably contains potassium iodide.
[0079] The thickness of the polarizer 10 is usually about 2 to 40 μm. From the viewpoint of thinning the polarizing plate, the thickness of the polarizer 10 is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less.
[0080] On the other hand, from the viewpoint of facilitating production of a polarizing plate with a protective film having sufficiently large forward curl, the thickness of the polarizer 10 is preferably large, specifically, preferably 10 μm or more, more preferably 15 μm or more, and further preferably 20 μm or more.
[0081] (1-1-3) First and second thermoplastic resin films
[0082] The first and second thermoplastic resin films 20 and 30 are each independently a film made of a light-transmitting thermoplastic resin, preferably an optically transparent thermoplastic resin. The thermoplastic resin constituting the first and second thermoplastic resin films 20 and 30 may be, for example, polyolefin resins such as chain polyolefin resins (polypropylene resins, etc.) and cyclic polyolefin resins (norbornene resins, etc.); cellulose resins such as triacetyl cellulose and diacetyl cellulose; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polycarbonate resins; (meth) acrylic resins such as methyl methacrylate resins; polystyrene resins; polyvinyl chloride resins; acrylonitrile-butadiene-styrene resins; acrylonitrile-styrene resins; polyvinyl acetate resins; polyvinylidene chloride resins; polyamide resins; polyacetal resins; modified polyphenylene ether resins; polysulfone resins; polyethersulfone resins; polyarylate resins; polyamideimide resins; polyimide resins, etc.
[0083] As the chain polyolefin resin, in addition to the homopolymers of chain olefins such as polyethylene resin and polypropylene resin, copolymers containing two or more chain olefins can also be mentioned. More specific examples include polypropylene resins (polypropylene resins as homopolymers of propylene, copolymers with propylene as the main body), polyethylene resins (polyethylene resins as homopolymers of ethylene, copolymers with ethylene as the main body).
[0084] Cyclic polyolefin resin is a general term for resins polymerized with cyclic olefin as a polymerization unit. Specific examples of cyclic polyolefin resins include ring-opening (co)polymers of cyclic olefins, addition polymers of cyclic olefins, copolymers of cyclic olefins with chain olefins such as ethylene and propylene (representatively random copolymers), and graft polymers obtained by modifying them with unsaturated carboxylic acids and their derivatives, and hydrogenated products thereof. Among them, it is preferred to use a norbornene resin using norbornene monomers such as norbornene and polycyclic norbornene monomers as cyclic olefins.
[0085] The so-called cellulose resin refers to a cellulose organic acid ester or a cellulose mixed organic acid ester in which a part or all of the hydrogen atoms in the hydroxyl groups of cellulose obtained from raw material cellulose such as cotton linters and wood pulp (broadleaf pulp, conifer pulp) are replaced by acetyl groups, propionyl groups and / or butyryl groups. For example, resins containing cellulose acetate, propionate, butyrate and mixed esters thereof can be cited. Among them, triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate and cellulose acetate butyrate are preferred.
[0086] Polyester resins are resins other than the above-mentioned cellulose resins having an ester bond, and generally include polycondensates of polycarboxylic acids or their derivatives and polyols. As polycarboxylic acids or their derivatives, dibasic dicarboxylic acids or their derivatives can be used, for example, terephthalic acid, isophthalic acid, dimethyl terephthalate, dimethyl naphthalate, etc. can be mentioned. As polyols, dibasic diols can be used, for example, ethylene glycol, propylene glycol, butanediol, neopentyl glycol, cyclohexanedimethanol, etc. can be mentioned. Examples of suitable polyester resins include polyethylene terephthalate.
[0087] Polycarbonate resins are engineering plastics containing polymers obtained by bonding monomer units via carbonate groups, and are resins with high impact resistance, heat resistance, flame retardancy, and transparency. Polycarbonate resins may also be resins called modified polycarbonates in which the polymer skeleton is modified to reduce the photoelastic coefficient, copolymerized polycarbonates in which the wavelength dependence is improved, and the like.
[0088] (Meth) acrylic resin is a polymer containing structural units derived from (meth) acrylic monomers. The polymer is typically a polymer containing methacrylate. Preferably, the proportion of structural units derived from methacrylate is a polymer containing 50% by weight or more relative to all structural units. (Meth) acrylic resin can be a homopolymer of methacrylate, or a copolymer containing structural units derived from other polymerizable monomers. In this case, the proportion of structural units derived from other polymerizable monomers is preferably less than 50% by weight relative to all structural units.
[0089] As the methacrylate that can constitute the (meth)acrylic resin, alkyl methacrylate is preferred. As the alkyl methacrylate, alkyl methacrylates having an alkyl group with a carbon number of 1 to 8 such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, and 2-hydroxyethyl methacrylate can be cited. The carbon number of the alkyl group contained in the alkyl methacrylate is preferably 1 to 4. In the (meth)acrylic resin, the methacrylate may be used alone or in combination of two or more.
[0090] As the above-mentioned other polymerizable monomers that can constitute the (meth)acrylic resin, acrylates and other compounds having polymerizable carbon-carbon double bonds in the molecule can be mentioned. Other polymerizable monomers can be used alone or in combination of two or more. As acrylates, alkyl acrylates are preferred. As alkyl acrylates, alkyl acrylates having an alkyl group with a carbon number of 1 to 8 such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, and 2-hydroxyethyl acrylate can be mentioned. The carbon number of the alkyl group contained in the alkyl acrylate is preferably 1 to 4. In the (meth)acrylic resin, acrylates can be used alone or in combination of two or more.
[0091] Examples of other compounds having polymerizable carbon-carbon double bonds in the molecule include vinyl compounds such as ethylene, propylene, and styrene, and vinyl cyanide compounds such as acrylonitrile. Other compounds having polymerizable carbon-carbon double bonds in the molecule may be used alone or in combination of two or more.
[0092] The first and second thermoplastic resin films 20 and 30 may be protective films laminated on one surface of the polarizing plate 10 to protect the polarizing plate 10. The first or second thermoplastic resin film 20 and 30 may be protective films having optical functions such as retardation films and brightness enhancement films.
[0093] For example, a retardation film having an arbitrary retardation value can be prepared by stretching a thermoplastic resin film containing the above-mentioned materials (uniaxial stretching or biaxial stretching, etc.), or forming a liquid crystal layer on the film, etc. The first and / or second thermoplastic resin films 20, 30 may have a surface treatment layer (coating layer) such as a hard coating layer, an antiglare layer, an antireflection layer, an antistatic layer, and an antifouling layer laminated on the surface thereof.
[0094] The thickness of the first and second thermoplastic resin films 20 and 30 is usually 1 to 100 μm, but is preferably 5 to 60 μm, and more preferably 5 to 50 μm, from the viewpoint of strength, handling properties, and the like.
[0095] In the image Figure 2 When the two sides of the polarizer 10 are provided with thermoplastic resin films, the thermoplastic resin films may be composed of the same thermoplastic resin or different thermoplastic resins. In addition, the thickness may be the same or different. In addition, the same phase difference characteristics may be provided or different phase difference characteristics may be provided.
[0096] In the image Figure 2In the case of a layer structure including a first thermoplastic resin film 20 and a second thermoplastic resin film 30 as in the polarizing plate 2a shown in the figure, when a single sheet is formed, curling that makes the thick thermoplastic resin film side convex is likely to occur. Therefore, in the case where a protective film is attached to the side of the first thermoplastic resin film 20 and the first thermoplastic resin film is thicker than the second thermoplastic resin film, reverse curling is likely to occur. In the present invention, reverse curling can be suppressed even in such a case. As an example, in the present invention, reverse curling can be suppressed even in the case where a protective film is attached to the side of the first thermoplastic resin film 20 and the thickness of the first thermoplastic resin film 20 is greater than 40 μm and the thickness of the second thermoplastic resin film 30 is less than 40 μm.
[0097] (1.1.4) Adhesive
[0098] As described above, the first and second thermoplastic resin films 20 and 30 can be bonded to the polarizer 10 via an adhesive layer, for example. As the adhesive forming the adhesive layer, an aqueous adhesive, an active energy ray-curable adhesive or a thermosetting adhesive can be used, and an aqueous adhesive or an active energy ray-curable adhesive is preferred.
[0099] As water-based adhesives, adhesives containing polyvinyl alcohol resin aqueous solutions, water-based two-component urethane emulsion adhesives, etc. can be cited. Among them, water-based adhesives containing polyvinyl alcohol resin aqueous solutions can be appropriately used. As polyvinyl alcohol resins, in addition to using vinyl alcohol homopolymers obtained by saponifying polyvinyl acetate, which is a homopolymer of vinyl acetate, polyvinyl alcohol copolymers obtained by saponifying copolymers of vinyl acetate and other monomers copolymerizable therewith, or modified polyvinyl alcohol polymers obtained by partially modifying their hydroxyl groups, etc. can also be used. Water-based adhesives can contain crosslinking agents such as aldehyde compounds (such as glyoxal), epoxy compounds, melamine compounds, methylol compounds, isocyanate compounds, amine compounds, and polyvalent metal salts.
[0100] When a water-based adhesive is used, a drying step for removing water contained in the water-based adhesive is preferably performed after bonding the polarizer 10 to the first and second thermoplastic resin films 20 and 30. After the drying step, a curing step of curing at a temperature of, for example, 20 to 45°C may be performed.
[0101] The active energy ray-curable adhesive is an adhesive containing a curable compound that is cured by irradiation with active energy rays such as ultraviolet rays, visible light, electron beams, and X-rays, and is preferably an ultraviolet ray-curable adhesive.
[0102] The curable compound may be a cationically polymerizable curable compound or a radically polymerizable curable compound. Examples of cationically polymerizable curable compounds include epoxy compounds (compounds having one or more epoxy groups in the molecule), oxetane compounds (compounds having one or more oxetane rings in the molecule), or combinations thereof. Examples of radically polymerizable curable compounds include (meth)acrylic compounds (compounds having one or more (meth)acryloyloxy groups in the molecule), other vinyl compounds having radically polymerizable double bonds, or combinations thereof. It is also possible to use cationically polymerizable curable compounds and radically polymerizable curable compounds in combination. Active energy ray-curable adhesives generally also include a cationic polymerization initiator and / or a radical polymerization initiator for initiating the curing reaction of the curable compound.
[0103] When the polarizer 10 is bonded to the first and second thermoplastic resin films 20 and 30, in order to improve the adhesion, a surface activation treatment may be applied to the bonding surface of at least any one of them. As the surface activation treatment, dry treatments such as corona treatment, plasma treatment, discharge treatment (glow discharge treatment, etc.), flame treatment, ozone treatment, UV ozone treatment, ionizing active ray treatment (ultraviolet treatment, electron beam treatment, etc.) and wet treatments such as ultrasonic treatment using solvents such as water and acetone, saponification treatment, and anchor coating treatment may be cited. These surface activation treatments may be performed alone or in combination of two or more.
[0104] When thermoplastic resin films are bonded to both surfaces of the polarizing plate 10 , the adhesive used to bond these thermoplastic resin films may be of the same type or of different types.
[0105] (1-2) Protective film provided for lamination process
[0106] The protective film is a film for protecting the surface of the polarizing plate, and is usually peeled off together with the adhesive layer when a single piece of the polarizing plate with the protective film is attached to, for example, an image display element. Therefore, the protective film 1 is attached to the surface of the polarizing plate 2 in a removable manner.
[0107] The protective film can be composed of, for example, a base film and an adhesive layer laminated thereon.
[0108] The substrate film can be made of thermoplastic resins, such as polyolefin resins such as polyethylene resins, polypropylene resins, and cyclic polyolefin resins; polyester resins such as polyethylene terephthalate and polyethylene naphthalate; polycarbonate resins; (meth) acrylic resins, etc. The substrate film can be a single-layer structure or a multi-layer structure.
[0109] The adhesive layer can be formed of a (meth)acrylic adhesive, an epoxy adhesive, a urethane adhesive, a silicone adhesive, or the like.
[0110] The pellicle film may be a self-adhesive resin film such as a polypropylene resin or a polyethylene resin. In this case, the pellicle film does not have an adhesive layer.
[0111] The thickness of the protective film can be, for example, 5 to 150 μm, preferably 10 to 100 μm, more preferably 20 to 75 μm, and further preferably 25 to 70 μm (for example, 60 μm or less, further 55 μm or less). When the thickness of the protective film is less than 5 μm, the polarizing plate may not be sufficiently protected, and it is also disadvantageous in terms of operability. If the thickness of the protective film is greater than 150 μm, it is disadvantageous in terms of thin filmization of the polarizing plate monolith with the protective film and reworkability of the protective film.
[0112] The pellicle film used in the laminating step is preferably in a long strip shape.
[0113] The length of the long strip of pellicle membrane provided to the laminating step is, for example, 100 to 20000 m, or preferably 1000 to 10000 m. The width of the long strip of pellicle membrane provided to the laminating step S101 is, for example, 0.5 to 3 m, or preferably 1 to 2.5 m.
[0114] (1-3) Bonding of polarizing plate and protective film
[0115] Reference Figure 1 The polarizing plate 2 and the pellicle film 1 can be bonded together using, for example, a pair of rollers (bonding rollers) 5, 5. From the viewpoint of production efficiency, this method is particularly advantageous when the polarizing plate 2 and the pellicle film 1 are in a long shape.
[0116] Specifically, while the long polarizing plate 2 is continuously conveyed, the long protective film 1 is continuously conveyed, and the protective film 1 is overlapped on one side of the polarizing plate 2 and then sandwiched between a pair of laminating rollers 5, 5, thereby manufacturing a polarizing plate 3 with a protective film in which the two films are laminated.
[0117] The MD direction (conveying direction) of the polarizing plate 2 is usually parallel to the MD direction (conveying direction) of the pellicle 1. Parallel means that the angle between the MD direction of the polarizing plate 2 and the pellicle 1 is 0°±5°, preferably 0°±2°.
[0118] From the viewpoint of suppressing the change in the MD curl of the obtained single body of the polarizing plate with a protective film, it is preferred to laminate the two films so that the absorption axis of the polarizing plate 2 is parallel to the MD direction of the protective film 1. The term "parallel" means that the angle formed by the absorption axis of the polarizing plate 2 and the MD direction of the protective film 1 is 0 degrees ± 5 degrees, preferably 0 degrees ± 2 degrees.
[0119] The laminate of the polarizing plate 2 and the protective film 1 is passed between a pair of laminating rollers 5 and 5 , whereby the laminate is pressed from above and below, thereby bonding the two films to each other.
[0120] The polarizing plate 2 may have a transparent hard coating layer (a hard coating layer having a smooth surface) on its outermost surface.
[0121] When the protective film 1 is composed of a base film and an adhesive layer laminated thereon, the protective film 1 is laminated on one side of the polarizing plate 2 and then passed between a pair of laminating rollers 5, 5, so that the adhesive layer of the protective film 1 is laminated in contact with the above-mentioned one side of the polarizing plate 2. Before laminating the protective film 1 and the polarizing plate 2, the laminating surface of at least one of the protective film 1 and the polarizing plate 2 may be subjected to a surface activation treatment such as plasma treatment, corona treatment, ultraviolet irradiation treatment, flame treatment, or saponification treatment.
[0122] In the step of laminating using a pair of laminating rollers 5, 5, the pressure (clamping pressure) applied to the laminate of the protective film 1 and the polarizing plate 2 is, for example, 0.01 to 0.5 MPa, or 0.05 to 0.3 MPa. As the laminating rollers 5, 5, conventionally known laminating rollers such as rollers with metal surfaces (including alloys such as SUS) or rubber can be used.
[0123] In the process of laminating the polarizing plate 2 and the protective film 1, it is preferred to laminarize the polarizing plate 2 and the protective film 1 while applying tension. The pre-laminating tension of the polarizing plate 2 and the pre-laminating tension of the protective film 1 can be adjusted according to the rigidity of each film. For example, when the rigidity of the polarizing plate 2 is greater than that of the protective film 1, it is preferred to make the pre-laminating tension of the polarizing plate 2 greater than the pre-laminating tension of the protective film 1. This tension control is advantageous from the perspective of controlling the curling amount of the obtained single-piece body of the polarizing plate with the protective film. The pre-laminating tension refers to the tension applied to the film in the MD direction just before laminating the two films (the laminate of the two films passes through a pair of laminating rollers 5, 5).
[0124] From the viewpoint of reducing the amount of change in MD curl of the obtained polarizing plate with a pellicle, the tension before lamination in the MD direction of the pellicle 1 is preferably 10 kgf to 50 kgf, more preferably 20 kgf to 40 kgf.
[0125] From the same viewpoint, the tension before lamination in the MD direction of the polarizing plate 2 is preferably 20 kgf or more and 100 kgf or less, and more preferably 30 kgf or more and 70 kgf or less.
[0126] (1-4) Atmosphere temperature T1 in bonding process
[0127] In this embodiment, the temperature of the laminating process refers to the temperature of the atmosphere in which the pair of laminating rollers 5, 5 are arranged. The atmosphere temperature is set to T1 [°C]. T1 is usually room temperature, and can be appropriately adjusted to a temperature different from room temperature by temperature control. T1 is not limited as long as it satisfies the above formula (1), for example, it is 20°C or more and 30°C or less, preferably 22°C or more and 28°C or less. Room temperature is, for example, 23°C.
[0128] (1-5) Temperature T2 of the polarizing plate provided in the bonding step
[0129] In the present embodiment, the temperature of the polarizing plate provided to the laminating process refers to the temperature of the polarizing plate before it is in contact with a pair of laminating rollers 5, 5. The temperature is set to T2 [°C]. T2 is not limited as long as it satisfies the temperature of the above formula (1), for example, it is above 5°C and below 28°C, preferably above 7°C and below 26°C, and more preferably above 10°C and below 22°C. In order to set T2 to the above temperature range, the manufacturing method of the present embodiment preferably has a cooling process for cooling the polarizing plate provided to the laminating process. The cooling process can be a process for cooling the polarizing plate to be transported, or it can be a process for cooling the polarizing plate roller to be stored. The method for cooling the polarizing plate to be transported is not limited, for example, a method for cooling by close contact with a cooling roller, a method for cooling by blowing cooling air, a method for cooling by transporting under a cooling air flow or a nitrogen flow, etc. In the case of the method of cooling by blowing cooling air, the cooling air can be blown from one side or both sides of the polarizing plate, for example, it can be a method of blowing from the side of the first thermoplastic resin film.
[0130] The temperature T2 of the polarizing plate supplied to the bonding step is a value obtained by measuring the temperature of the polarizing plate supplied to the bonding step. It is preferable to implement the cooling step so that the temperature of the polarizing plate is the same regardless of where the temperature is measured.
[0131] (1-6) Temperature T3 of the pellicle film provided in the lamination process
[0132] In the present embodiment, the temperature of the protective film provided to the laminating process refers to the temperature of the protective film immediately before it comes into contact with a pair of laminating rollers 5, 5. This temperature is set to T3 [°C]. T3 is not limited as long as it satisfies the above formula (2), for example, it is above 20°C and below 30°C, preferably above 22°C and below 28°C, and more preferably room temperature. Room temperature is, for example, 23°C. T3 is preferably the same as T1. T3 may also be a temperature higher than T1, in which case there is a heating process for heating the protective film provided to the laminating process. T3 may also be a temperature lower than T1, in which case there is a cooling process for cooling the protective film provided to the laminating process.
[0133] (2) Cutting process
[0134] This step is a step of cutting out the polarizing plate with a pellicle film obtained in the laminating step to obtain a single piece of the polarizing plate with a pellicle film.
[0135] Cutting (cutting) can be performed using a conventionally known cutting tool such as a cutting cutter.
[0136] The size, shape and cutting angle of the cut polarizing plate with a protective film are not particularly limited.
[0137] The single body of the polarizing plate with a protective film is preferably in a square shape, more preferably in a square shape having long sides and short sides. The square shape is preferably a rectangular shape.
[0138] When the shape of the single body of the polarizing plate with a pellicle is rectangular, the length of the long side is, for example, 50 mm to 300 mm, or preferably 70 mm to 150 mm, and the length of the short side is, for example, 30 mm to 200 mm, or preferably 40 mm to 100 mm.
[0139] Although there is no particular restriction, when the shape of a single piece of the polarizing plate with a protective film is rectangular, the single piece of the polarizing plate with a protective film can be cut out from the polarizing plate with a protective film 3 as shown below, that is, when the single piece of the polarizing plate with a protective film is observed from the protective film side, the absorption axis direction of the polarizing plate (MD direction of the polarizing plate) forms an angle of 45 degrees with the long side and the short side of the polarizing plate single piece.
[0140] Alternatively, in the case where the shape of a single piece of the polarizing plate with a protective film is a rectangle, the single piece of the polarizing plate with a protective film can also be cut out from the polarizing plate with a protective film 3 as shown below, that is, when the single piece of the polarizing plate with a protective film is observed from the protective film side, the absorption axis direction of the polarizing plate (MD direction of the polarizing plate) is parallel to the long side of the polarizing plate single piece, or forms an angle of 90 degrees.
[0141] Figure 4FIG. 1 is a cross-sectional view showing an example of the layer structure of a single piece of a polarizing plate with a protective film. Figure 4 As shown, when the protective film 1 is composed of the base film 40 and the adhesive layer 50 laminated thereon, the protective film 1 is laminated so that the adhesive layer 50 included in the protective film 1 is in contact with one surface of the polarizing plate 2 .
[0142] <Multilayer structure>
[0143] On the polarizing plate side of the polarizing plate with a protective film or the long polarizing plate with a protective film, one or more other optical functional layers, a separator (release film), etc. may be laminated via a pressure-sensitive adhesive layer or an adhesive layer.
[0144] The optical function layer may be a phase difference layer or the like, and the optical function layer may be laminated on the surface on the polarizing plate side via a pressure-sensitive adhesive layer or an adhesive layer.
[0145] Example
[0146] Hereinafter, the present invention will be described in more detail with reference to experimental examples; however, the present invention is not limited to these examples.
[0147] <Examples 1, 2, Comparative Examples 1, 2>
[0148] (A) Preparation of polarizing film
[0149] While continuously conveying a long polyvinyl alcohol film [thickness 40μm, width 2980mm, VF-PE#4000, saponification degree 99.9 mol% or more, manufactured by Kuraray Co., Ltd.], it was uniaxially stretched to about 4 times in a dry manner, and then immersed in 40°C pure water for 1 minute while maintaining the tension state, and then immersed in a 28°C aqueous solution with a weight ratio of iodine / potassium iodide / water of 0.1 / 5 / 100 for 60 seconds. Thereafter, it was immersed in a 68°C aqueous solution with a weight ratio of potassium iodide / boric acid / water of 10.5 / 7.5 / 100 for 300 seconds. Next, after washing with 5°C pure water for 5 seconds, it was dried at 70°C for 180 seconds to obtain a long strip of polarizer in which iodine was adsorbed and oriented on the uniaxially stretched polyvinyl alcohol film. The thickness of the polarizer is 15μm.
[0150] (B) Preparation of polarizing plate
[0151] As the first thermoplastic resin film to be bonded to the pellicle, a long first thermoplastic resin film A (manufactured by TOPPAN TOMOEGAWA OPTICAL FILM, transparent HC-TAC, hard coat layer thickness 7 μm, TAC film thickness 40 μm, trade name: 40FJCHCN-TC) was prepared.
[0152] As the second thermoplastic resin film to be bonded to the side opposite to the first thermoplastic resin film, a second thermoplastic resin film A [manufactured by Konica Minolta, TAC film, thickness 20 μm, trade name: KC2CT1W] and a second thermoplastic resin film B [manufactured by Konica Minolta, TAC film, thickness 40 μm, trade name: KC4CT1W] were prepared.
[0153] While continuously conveying the long strip polarizer obtained in (A) above, continuously convey the long strip first thermoplastic resin film A and the long strip second thermoplastic resin film A or B, inject a water-based adhesive between the polarizer and the first thermoplastic resin film and between the polarizer and the second thermoplastic resin film, and pass through a pair of laminating rollers. Next, convey the obtained laminated film, pass it through a hot air dryer and heat it at 80°C for 300 seconds, thereby drying the water-based adhesive layer to obtain a long strip polarizer. In this way, a polarizer consisting of the first thermoplastic resin film / water-based adhesive layer / polarizer / water-based adhesive layer / second thermoplastic resin film is obtained. The thickness of the polarizer is 102μm and 82μm, respectively.
[0154] In the above-mentioned water-based adhesive, 50 g of a modified PVA resin containing acetoacetyl (GOHSENX Z-410 manufactured by Mitsubishi Chemical Co., Ltd.) was dissolved in 950 g of pure water, heated at 90° C. for 2 hours, and then cooled to room temperature to obtain a PVA solution. The PVA solution, maleic acid, and glyoxal were mixed so that the PVA resin was 3.0% by mass, the maleic acid was 0.01% by mass, and the glyoxal was 0.15% by mass to prepare a PVA adhesive.
[0155] (C) Production of a long polarizing plate with a protective film
[0156] While continuously conveying the long strip polarizing plate obtained in the above (B), a long strip protective film [a product name of AY-638 manufactured by Fujimori Industries, Ltd., which is a biaxially stretched polyethylene terephthalate (thickness: 19 μm) laminated with a (meth) acrylic adhesive layer (thickness: 15 μm)] with the isolation film peeled off is continuously conveyed, and after overlapping them, they are passed between a pair of laminating rollers, thereby pressing the laminate of the protective film and the polarizing plate from the top and bottom, thereby continuously manufacturing a long strip polarizing plate with a protective film.
[0157] The protective film is bonded to the first thermoplastic resin film (clear hard coat film) surface of the polarizing plate via the adhesive layer thereof. In the bonding step, the absorption axis of the polarizing plate is parallel to the MD direction of the protective film.
[0158] In Examples 1 and 2, cooling air at 17° C. was blown from the first thermoplastic resin film side of the polarizing plate in a conveying path for continuously conveying a long polarizing plate, and the polarizing plate was supplied to the laminating roll after adjusting the temperature T2 to 17° C.
[0159] In Comparative Examples 1 and 2, the polarizing plate was supplied to the laminating roller without adjusting the temperature T2 of the polarizing plate in the conveying path for continuously conveying the long polarizing plate. Therefore, the temperature T2 of the polarizing plate can be regarded as 23° C., which is the room temperature.
[0160] In the examples and comparative examples, since the temperature of the atmosphere in which the laminating roll is placed is not adjusted, the atmosphere temperature T1 can be regarded as 23° C., which is the room temperature.
[0161] In the examples and comparative examples, the pellicle membrane was supplied to the laminating roll without temperature control. Therefore, the temperature T3 of the pellicle membrane can be regarded as 23°C, which is the room temperature.
[0162] The pressure (nip pressure) applied to the laminate of the pellicle and the polarizing plate by the laminating rollers was 0.1 MPa. At this time, the pre-lamination tension in the MD direction of the polarizing plate was 70 kgf, and the pre-lamination tension in the MD direction of the pellicle was 40 kgf.
[0163] (D) Production of a single piece of polarizing plate with protective film
[0164] like Figure 5 As shown, from the long strip of polarizing plate with a protective film obtained in the above (C), a super cutter is used to cut out small square pieces (single piece) (200 mm on one side) in a manner that the absorption axis of the polarizing plate is 45 degrees relative to each side when observed from the protective film side, thereby obtaining a single piece of polarizing plate with a protective film.
[0165] <Evaluation>
[0166] (Determination of curl amount)
[0167] like Figure 5 As shown in FIG. 1 , a square (200 mm on each side) small piece (single piece) was cut out from the obtained long strip polarizing plate 60 with a protective film using a super cutter so that the absorption axis 61 of the polarizing plate was at 45 degrees relative to each side when viewed from the protective film side, and this small piece was used as a sample 70 for measuring the TD curl amount. The sample 70 for measurement was cut out in an environment of 23° C. and a relative humidity of 55% immediately after the polarizing plate and the protective film were attached.
[0168] The measuring sample 70 is placed on a reference plane (horizontal table) with the concave side facing upward. In this state, the heights of two corners 80 on the diagonal line of the measuring sample 70 in the transmission axis direction of the polarizing plate of the measuring sample 70 are measured relative to the reference plane, and the TD curl amount [mm] is calculated as the average of the heights of the two corners 80.
[0169] The state where the pellicle side is concave is a state with forward curl, and the state where the polarizing plate side is concave is a state with reverse curl.
[0170] The TD curl amount is shown in Table 1. When the TD curl amount is a positive value, it means that the curl is a forward curl, and when it is a negative value, it means that the curl is a reverse curl.
[0171] [Table 1]
[0172]
[0173] The results shown in Table 1 show that, when Example 1 and Comparative Example 1 and Example 2 and Comparative Example 2 are compared, in which only the temperature of the supplied polarizing plates is different, reverse curl is suppressed in Example 1 compared with Comparative Example 1 and reverse curl is suppressed in Example 2 compared with Comparative Example 2.
[0174] Description of Reference Numerals
[0175] 1 protective film, 2, 2a, 2b polarizing plate, 3 polarizing plate with protective film, 5 bonding roller, 10 polarizing plate, 20 first thermoplastic resin film, 30 second thermoplastic resin film, 40 base film, 50 adhesive layer, 60 long strip polarizing plate with protective film, 61 absorption axis of polarizing plate, 70 sample for measuring TD curl amount, 80 angle of measuring sample.
Claims
1. A method for manufacturing a polarizing plate with a protective film, the method comprising a laminating step of laminating the polarizing plate by laminating the protective film on one side of the polarizing plate and then passing the polarizing plate between a pair of laminating rollers for pressing. In the bonding step, if the ambient temperature is T1 and the temperature of the supplied polarizing plate is T2, the following relationship (1) is satisfied, where the units of T1 and T2 are °C. 2℃≤T1-T2≤15℃ (1).
2. The manufacturing method according to claim 1, wherein: In the lamination process, if the temperature of the supplied pellicle membrane is set to T3, the following relationship (2) is satisfied, where the unit of T3 is °C: 2℃≤T3-T2≤15℃ (2).
3. The manufacturing method according to claim 1 or 2, wherein: The polarizing plate comprises a first thermoplastic resin film, a polarizer, and a second thermoplastic resin film in this order. The thickness of the first thermoplastic resin film is greater than 40 μm, The thickness of the second thermoplastic resin film is 40 μm or less, In the bonding step, the protective film is stacked on the surface side of the first thermoplastic resin film of the polarizing plate.
4. The manufacturing method according to claim 1 or 2, wherein: In the laminating step, the tension of the pellicle before passing through the pair of laminating rollers is 10 kgf or more and 50 kgf or less.
5. The manufacturing method according to claim 1 or 2, wherein: In the laminating step, the tension of the polarizing plate before passing through the pair of laminating rollers is 20 kgf or more and 100 kgf or less.
6. The manufacturing method according to claim 1 or 2, wherein: In the bonding step, the polarizing plate is bonded to the pellicle film so that the absorption axis of the polarizing plate is parallel to the MD direction of the pellicle film.
7. The manufacturing method according to claim 1 or 2, wherein: The polarizing plate has a thickness of 100 μm or less.
8. The manufacturing method according to claim 1 or 2, wherein: In the bonding step, the polarizing plate and the protective film are in a long strip shape.
9. The manufacturing method according to claim 8, wherein: After the laminating step, the method further includes a cutting step of cutting out a single piece from the polarizing plate with a protective film.