Method for manufacturing battery having laminated film package

The metal layer of the laminated film packaging body of the lithium-ion battery is covered by a two-stage sealing process, which solves the problem of corrosion caused by contact between the metal layer and the external components, and realizes effective insulation and cost reduction of the metal layer.

CN118947010APending Publication Date: 2024-11-12PANASONIC ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029651.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries with laminated film packaging are prone to corrosion when the metal layer comes into contact with the external components, and existing solutions increase costs and workloads.

Method used

Using a two-stage sealing process, the inner resin layer is welded and pressed to cover the end surface of the metal layer of the laminated film packaging body, avoiding the use of additional insulating parts, thereby achieving insulation of the metal layer.

Benefits of technology

Simple insulation treatment of the end surface of the metal layer is realized, avoiding increasing the demand for components, reducing costs and workloads, and ensuring effective insulation of the metal layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118947010A_ABST
    Figure CN118947010A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a battery provided with a laminated film package in which an electrode body (50) is packaged with a laminated film (120). The method includes: a packaging step of packaging the electrode body (50) with a laminated film packaging body; and a sealing step for sealing the periphery of the electrode body (50) with a laminated film package. The sealing step includes: a first-stage sealing step in which an unwelded portion remains at the tip portion, and the inner resin layer is welded to the inner side of the unwelded portion; and a second-stage sealing step in which the inner resin layer is extruded outward by heating and pressing the unwelded portion, thereby covering the end surface of the metal layer at the tip of the laminated film package with the inner resin layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for producing a battery having a laminated film package, wherein the battery having a laminated film package is obtained by packaging an electrode body including a positive electrode and a negative electrode with a laminated film including an outer resin layer, a metal layer, and an inner resin layer. Background Art

[0002] Secondary batteries such as lithium-ion batteries are used as power sources for various electrical devices. In particular, small and thin secondary batteries are used as power sources for electronic devices such as smartphones, tablet computers, and notebook personal computers.

[0003] As such a small and thin power source, a secondary battery including a laminate film package, in particular, a flat secondary battery is widely used.

[0004] Such a laminate film package has a laminate film in a bag shape and contains an electrode body, but the end of the laminate film is exposed. As described above, the laminate film is a three-layer film of an outer resin layer, a metal layer, and an inner resin layer, and the end of the metal layer is also exposed.

[0005] Furthermore, if the metal layer contacts a member with a negative potential, metal corrosion is likely to occur. The positive electrode and the negative electrode of the battery need to be connected to the outside, so the positive electrode tab is exposed from the main body of the battery, and the negative electrode tab is exposed from the laminated film package. Therefore, there is a possibility that the positive electrode tab, the negative electrode tab and the metal layer of the laminated film package come into contact.

[0006] In Patent Document 1, the above-mentioned problem is solved by covering the end portions of the laminated film package with a thermal adhesive insulating sheet.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2007-95465 Summary of the invention

[0010] According to Patent Document 1, the end portion of the laminated film package can be securely covered and the metal layer can be insulated from the outside.

[0011] However, if such additional components are provided, the cost of the additional components will be incurred and the workload will increase.

[0012] The present disclosure relates to a method for manufacturing a battery with a laminated film packaging body, wherein the battery with a laminated film packaging body is obtained by packaging an electrode body including a positive electrode and a negative electrode with a laminated film including an outer resin layer, a metal layer and an inner resin layer, and the method for manufacturing a battery with a laminated film packaging body comprises: a packaging step of packaging the electrode body with the laminated film packaging body; and a sealing step of sealing the periphery of the electrode body with the laminated film packaging body, wherein the sealing step comprises: a first-stage sealing step of melting the inner resin layer inside an un-melted portion remaining at the front end portion; and a second-stage sealing step of heating and pressing the un-melted portion to extrude the inner resin layer outward, thereby covering the end face of the metal layer at the front end of the laminated film packaging body with the inner resin layer.

[0013] According to the present disclosure, the end face of the metal layer of the laminated film can be covered with the inner resin layer through the second stage sealing process. Therefore, since it is not necessary to cover the end face with other insulating parts, etc., there is no need to increase the parts, and the end face of the metal layer can be insulated by a relatively simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a perspective view schematically showing the shape of a battery including a laminated film package manufactured by the manufacturing method according to the embodiment.

[0015] Figure 2 This is a diagram showing a cross section of a laminate film used in a laminate film package.

[0016] Figure 3 The diagram shows an electrode body manufacturing process for manufacturing an electrode body.

[0017] Figure 4 It is a figure which shows the lamination film packaging process and the sealing process.

[0018] Figure 5 It is a diagram showing the liquid injection and pressure reduction and sealing process.

[0019] Figure 6 This figure shows the process of main sealing, side cutting and side bending.

[0020] Figure 7 It is a diagram schematically showing a sealing process.

[0021] Figure 8 It is a figure explaining the top sealing process.

[0022] Fig. 9 It is a figure explaining the side sealing process.

[0023] Fig.10 This is a diagram for explaining the main sealing process. DETAILED DESCRIPTION

[0024] Hereinafter, embodiments of the present disclosure will be described below with reference to the accompanying drawings. In addition, the following embodiments do not limit the present disclosure, and structures in which a plurality of examples are selectively combined are also included in the present disclosure.

[0025] "Battery structure"

[0026] Figure 1 It is a perspective view schematically showing the shape of a battery including a laminated film package manufactured by the manufacturing method according to the embodiment.

[0027] The battery 10 has a thin rectangular parallelepiped shape as a whole, and is covered with a laminate film package 12. In this example, the battery 10 is a lithium ion battery.

[0028] The laminate film package 12 is a thin film, and contains the electrode body 50 and the electrolyte in a thick portion of a rectangular parallelepiped.

[0029] As described later, the large laminate film is folded in half to wrap the electrode body 50 , and the remaining three sides are sealed.

[0030] In this example, the top seal 16 is on the upper side, the side seal 18 is on the left side, and the main seal 20 is on the left side. The side seal 18 and the main seal 20 overlap with the side wall of the battery 10 by being folded back in the thickness direction.

[0031] In addition, the positive electrode tab 22 and the negative electrode tab 24 protrude from the top seal portion 16. These positive electrode tab 22 and negative electrode tab 24 are connected to the positive electrode 30 and the negative electrode 40, respectively. Insulating tab films 26 and 28 are interposed between the laminate film package 12 and the base of the positive electrode tab 22 and the negative electrode tab 24.

[0032] The battery 10 including the laminated film package 12 is connected to the outside via the positive electrode tab 22 and the negative electrode tab 24 .

[0033] In the figure, regarding the front end faces 12a and the upper end faces 12b on both sides of the laminate film package 12 shown by bold lines, the two laminate films folded in half are overlapped and bonded so that the inner resin layers are in contact.

[0034] "Structure of laminated film"

[0035] Figure 2 1 is a diagram showing a cross section of a laminate film 120 used in the laminate film package 12. As described above, the laminate film 120 has a three-layer structure of an outer resin layer 122, a metal layer 124, and an inner resin layer 126.

[0036] The metal layer 124 is made of, for example, aluminum or an aluminum alloy. The outer resin layer 122 is made of, for example, nylon, and the inner resin layer 126 is made of, for example, polypropylene. The metal layer 124 and the outer resin layer 122 are bonded together, for example, by a dry lamination adhesive, and the metal layer 124 and the inner resin layer 126 can be bonded together by carboxylic acid-modified polypropylene obtained by adding carboxyl groups to polypropylene.

[0037] In addition, the above-mentioned structure is an example and is not limited to this.

[0038] "Description of the manufacturing process"

[0039] based on Figure 3 to Figure 6 The manufacturing process of the battery 10 including the laminated film package 12 will be briefly described.

[0040] Electrode body manufacturing process

[0041] Figure 3 The following is an electrode body manufacturing process for manufacturing the electrode body 50. First, the tab films 26 and 28 are welded to the positive electrode tab 22 and the negative electrode tab 24, respectively.

[0042] Next, the positive electrode tab 22 is welded to the core material 32 of the positive electrode 30, and the negative electrode tab 24 is welded to the core material 42 of the negative electrode 40. In addition, a positive electrode active material layer 34 is formed on the surface of the core material 32 of the positive electrode 30, and a negative electrode active material layer 44 is formed on the surface of the core material 42 of the negative electrode 40. The core material 32 is, for example, aluminum foil, and the core material 42 is, for example, copper foil. The positive electrode active material layer 34 contains a positive electrode active material such as a lithium transition metal composite oxide, and the negative electrode active material layer 44 contains a negative electrode active material such as graphite.

[0043] The positive electrode 30 and the negative electrode 40 thus produced, and a separator made of, for example, an olefin resin, are wound by a winding machine to form an electrode body 50. The winding ends are fixed with a tape 52.

[0044] "Lamination film packaging process, sealing process"

[0045] Figure 4 1 is a diagram showing the laminating film packaging process and the sealing process. In this way, the laminating film 120 is folded in half and the electrode body 50 is enclosed. At this time, the positive electrode tab 22 and the negative electrode tab 24 are protruded from the side opposite to the side of the folded laminating film 120. The side where the positive electrode tab 22 and the negative electrode tab 24 protrude is called the top. In this way, a semi-finished product 60 containing the electrode body 50 in the laminating film 120 can be obtained.

[0046] Then, the top end of the laminate film 120 is heated and pressed to weld the inner resin layers 126 to each other, thereby performing top sealing. In addition, the top sealing is performed in the following state: the positive electrode tab 22 and the negative electrode tab 24 are sandwiched by the laminate film 120 with the tab films 26 and 28 interposed therebetween, and the positive electrode tab 22 and the negative electrode tab 24 protrude to the outside.

[0047] Next, the side edge is sealed by welding one side of the laminate film 120 that wraps the electrode body 50. Thus, the semi-finished product 60 can be obtained in which only the other side of the laminate film 120 that wraps the electrode body 50 is open.

[0048] Figure 5 7 is a diagram showing the liquid injection and decompression sealing process. In this way, the electrolyte is injected into the semi-finished product 60 from its opening in the drying box 70. The electrolyte contains a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Non-aqueous solvents include esters, ethers, nitriles, amides, and mixed solvents of two or more of these. The non-aqueous solvent may also contain a halogen substituted body in which at least a portion of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. As an example of a non-aqueous solvent, ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and mixed solvents of these can be cited. Electrolyte salts include lithium salts such as LiPF6.

[0049] After the electrolyte solution is injected, the opening side is temporarily sealed. Next, after the electrolyte solution is permeated, a predetermined charge is performed.

[0050] After the charging is completed, the semi-finished product 60 is stored in the decompression box 74, and the semi-finished product 60 is decompressed and sealed. After that, a part of the decompression sealed portion is cut once.

[0051] Figure 6 1 is a diagram showing the process of final sealing, side cutting and finishing. For the semi-finished product 60 sealed by pressure reduction, the temporary sealed side is final sealed to form a final sealing portion 20. The final sealing portion 20 is set as the semi-finished product 60 side of the once cut portion. As a result, the inner resin layer 126 extruded by the final sealing can be expanded like a free end. In addition, the side cutting is performed on this portion to remove the unnecessary laminate film 120.

[0052] In this manner, the semi-finished product 60 in which the electrode body 50 is sealed in the laminate film package 12 is obtained.

[0053] Then, the two side edges of the laminated film package 12 are folded toward the side of the semi-finished product 60. Figure 1 The battery 10 is completed.

[0054] "Sealing process"

[0055] As described above, in the present embodiment, the laminate film 120 is sealed in three sealing steps, namely, the top sealing step, the side sealing step, and the main sealing step. Then, in this sealing step, a two-step sealing step is performed.

[0056] <Phase 1>

[0057] Figure 7 : is a diagram schematically showing the sealing process. First, in the first stage, the front end portion of the laminate film 120 in which the inner resin layer 126 overlaps face to face is sealed by folding it in half. In this sealing, a mold 80 having a shape corresponding to the sealing portion is prepared, and the overlapping laminate films 120 are pressed from both sides with the mold 80, and heated. As a result, the inner resin layer 126 is melted. The heating temperature is set to about 180 to 200°C. As mentioned above, the outer resin layer 122 is made of nylon, for example, and the inner resin layer 126 is made of polypropylene, for example, so that the inner resin layers 126 can be melted to each other. In addition, there are various types of resins, and by using a resin with weaker heat resistance than the outer resin layer 122 for the inner resin layer 126, the inner resin layers 126 can be melted to each other.

[0058] By applying pressure with the mold 80, the portion pressing the mold 80 is recessed in a corresponding shape. Here, a strip-shaped front end region not pressed by the mold 80 remains on the front end side of the laminate film 120. This is to prevent a large load from being applied to the front end portion, thereby preventing the front end portion from being damaged.

[0059] Therefore, the front end region of the laminate film 120 is bent outward with the front end portion of the die 80 as a starting point, and the front end is directed obliquely upward.

[0060] Thus, through the first stage sealing process, the portion heated and pressed by the mold 80 becomes a sealed area for welding, and a strip-shaped unwelded portion remains on the front end side. In addition, in the pressed pair of laminated films 120, a pair of inner resin layers 126 move toward the front end that becomes the free end, and become a bulging shape with a protruding central portion.

[0061] <Phase 2>

[0062] When the first stage sealing process is completed, the second stage sealing process is performed next. In the second stage sealing process, the unwelded portion on the front end side is heated and pressed by the mold 82. At this time, the mold 82 stops moving toward the laminate film 120 side halfway. That is, the front end portions of the pair of laminate films 120 that are expanding outward stop moving at a position where they become parallel.

[0063] Thus, the combined portion of the pair of inner resin layers 126 bulging toward the front end is pressed from both sides, but in this case, the metal layer 124 and the outer resin layer 122 move inward to press the inner resin layer 126, so that the front end side end surfaces of the metal layer 124 and the outer resin layer 122 are covered by the inner resin layer 126. That is, the heating and pressing of the mold 82 is performed at a relatively low temperature and the pressing is performed only halfway, and the bulging portion 126a of the combined pair of inner resin layers 126 expands outward to cover at least the end surface of the metal layer 124.

[0064] Here, different molds are used for the mold 80 of the first-stage sealing step and the mold 82 of the second-stage sealing step, but the same mold may be used.

[0065] <Top seal>

[0066] Figure 8 1 is a diagram for explaining a top sealing step. As shown in the figure, the top sealing is performed by sealing the vicinity of the front end of the top side where the positive electrode tab 22 and the negative electrode tab 24 of the semi-finished product 60 protrude with a band-shaped sealing portion 90 - 1 .

[0067] In the first stage sealing process, the sealing portion 90-1 is heated and pressed by the mold 86 for welding. At this time, an unwelded portion 90-2 remains on the front end side of the sealing portion 90. A top view and a side cross-sectional view of the mold 86 used in the first stage sealing process are shown on the right. In this way, the mold 86 is a rod-shaped cross-section of the entire quadrilateral that crosses one side (top) of the semi-finished product 60, and a strip-shaped sealing portion is formed by clamping the side of the semi-finished product 60 with a pair of molds 86. In addition, a pair of molds 86 have a recessed portion corresponding to the thickness of the positive electrode tab 22 and the negative electrode tab 24 in the portion where they are clamped, namely, the tab avoidance portion 84. As a result, the portion where the electrode tab exists can be included for appropriate sealing.

[0068] Then, in the second sealing step, by heating and pressing the unwelded portion 90-2 with the unwelded portion mold 88, the end surface of the metal layer 124 can be covered by the bulging portion 126b of the inner resin layer 126. In the top sealing, the same mold can be used for the mold 86 of the first stage sealing step and the mold 88 of the second stage sealing step.

[0069] <Side seal>

[0070] Fig. 9 1 and 2 are diagrams for explaining the side edge sealing step. In this way, the vicinity of the front end of one side of the semi-finished product 60 is sealed by the strip-shaped sealing portion 92-1.

[0071] In the first stage sealing process, the sealing portion 92-1 is welded by heating and pressing with the mold 80. At this time, an unwelded portion 92-2 is left at the front end side of the sealing portion 92-1. The top view and side cross-sectional view of the mold 80 used in the first stage sealing process are shown on the right, and have a shape corresponding to the sealing portion 92-1.

[0072] Then, in the second-stage sealing step, the unwelded portion 92 - 2 is partially heated and pressed by the mold 82 , so that the end surface of the metal layer 124 can be covered with the bulging portion 126 b of the inner resin layer 126 .

[0073] <Officially sealed>

[0074] Fig.10 1 and 2 are diagrams for explaining a main sealing process. The vicinity of the semi-finished product 60 on the unsealed side opposite to the sealed side of the semi-finished product 60 is sealed with a strip-shaped sealing portion 90 .

[0075] In the first stage sealing process, the sealing portion 94-1 is heated and pressed by a mold 80 of the same shape as the side sealing, so that the unwelded portion 94-2 remains on the front end side of the sealing portion 94-1. Here, in the case of formal sealing, the pair of laminated films 120 overlapped by folding in half are not cut. However, since the pair of laminated films 120 are cut at one time, the inner resin layer 126 bulges here, and the outer side of the sealing portion 90 bulges in the same way as in the case of side cutting.

[0076] Then, the unwelded portion 94-2 is left outside the sealed portion 90 of the pair of laminated films 120, and the side cutting is performed to cut off the unnecessary overlapping portion of the laminated film 120 on the side. In addition, the side cutting is performed after the first stage sealing process, and then the second stage sealing process can be implemented.

[0077] Next, the unwelded portion 94 - 2 remaining inside the cut portion is partially heated and pressed by the mold 82 , so that the end surface of the metal layer 124 can be covered with the bulging portion 126 b of the inner resin layer 126 .

[0078] “Effects of implementation”

[0079] In the present embodiment, a two-stage sealing process is performed in the sealing process of the semi-finished product 60 based on the laminate film 120, and the end surface of the metal layer 124 of the laminate film 120 can be covered with the inner resin layer 126 through the second-stage sealing process. Therefore, it is not necessary to cover the end surface with other insulating members, etc., and the number of parts is not increased, and the insulation treatment of the end surface of the metal layer 124 can be performed in a relatively simple process.

[0080] Description of Reference Numerals

[0081] 10: battery, 12: laminated film packaging body, 16: top sealing part, 18: side sealing part, 20: main sealing part, 22: positive electrode tab, 24: negative electrode tab, 50: electrode body, 60: semi-finished product, 80, 82: mold, 120 laminated film, 122: outer resin layer, 124: metal layer, 126: inner resin layer.

Claims

1. A method for producing a battery having a laminated film package, wherein the battery having a laminated film package is obtained by packaging an electrode body including a positive electrode and a negative electrode with a laminated film including an outer resin layer, a metal layer and an inner resin layer, The method for manufacturing a battery having a laminated film package comprises: a packaging step of packaging the electrode body with the laminated film packaging body; and a sealing step of sealing the periphery of the electrode body with the laminated film packaging body, The sealing process comprises: In a first-stage sealing step, an unwelded portion is left at the front end portion, and the inner resin layer is welded inside the unwelded portion; and In the second-stage sealing step, the unwelded portion is heated and pressed to extrude the inner resin layer outward, thereby covering the end surface of the metal layer at the front end of the laminated film package with the inner resin layer.

2. The method for producing a battery having a laminated film package according to claim 1, in, The positive electrode and the negative electrode have a positive electrode tab and a negative electrode tab respectively. In the packaging step, the electrode assembly is packaged with the laminated film packaging body in a state where the positive electrode tab and the negative electrode tab protrude to the outside. In the first-stage sealing step, the inner resin layers around the electrode body are welded to each other in a state where the positive electrode tab and the negative electrode tab protrude to the outside.

3. The method for producing a battery having a laminated film package according to claim 2, in, In the packaging step, the laminated film packaging body is folded in half and the electrode body is accommodated therein, and in the sealing step, both sides and the top of the electrode body are sealed. On the upper side, the positive electrode tab and the negative electrode tab are sealed in a state where they are exposed to the outside.