Preparation method of efficient flexible carbon fiber / copper electromagnetic shielding composite film

Through the preparation method of high-efficiency flexible carbon fiber/copper electromagnetic shielding composite film, combined with carbon fiber heat treatment, ultrasonic dispersion and electrochemical copper plating, the problems of cumbersome preparation steps and poor flexibility of carbon fiber composite film in the prior art are solved, and efficient electromagnetic shielding and machinery are achieved Flexible multifunctional material suitable for electromagnetic wave shielding of lightweight and smart devices.

CN118955968AInactive Publication Date: 2024-11-15HARBIN INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411029938.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the steps for preparing carbon fiber/polymer composite films are cumbersome and have poor flexibility, making it difficult to meet the electromagnetic shielding needs of lightweight, intelligent, flexible and micro-device. Moreover, the preparation of continuous carbon fiber is difficult and costly, which affects the widespread application of materials.

Method used

Using the high-efficiency flexible carbon fiber/copper electromagnetic shielding composite film preparation method, high-quality copper plating is formed through carbon fiber heat treatment, ultrasonic dispersion, electroless copper plating and hot pressing molding, combining the connecting structure of chopped carbon fiber and metal copper to obtain excellent electrical conductivity , mechanical flexibility and efficient electromagnetic interference shielding performance.

Benefits of technology

It has achieved the preparation of high-efficiency flexible carbon fiber/copper electromagnetic shielding composite film, with excellent conductivity, mechanical flexibility and efficient electromagnetic interference shielding performance, shielding 99.9% electromagnetic radiation, and is suitable for electromagnetic protection of communication technology and high-precision instruments. It also has low cost and simple processes, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955968A_ABST
    Figure CN118955968A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an efficient flexible carbon fiber / copper electromagnetic shielding composite film, relates to a preparation method of a composite film, and aims to solve the problems that a polymer composite film prepared by an existing method is tedious in step and poor in flexibility. The method comprises the following steps: carbon fibers obtained by high-temperature pretreatment in an inert atmosphere are used as raw materials, copper metal is deposited on the surfaces of the carbon fibers, the design thought of improving the electric conductivity of the composite film is adopted, and then a solution mixing and hot press molding technology is adopted; the high-efficiency, light-weight and flexible carbon fiber / copper electromagnetic shielding composite film is prepared by taking polyethylene powder as a matrix. The high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film obtained by the method can effectively avoid the problems of environmental pollution and high cost caused by use of continuous carbon fibers, and the flexible composite film with excellent processability can effectively shield 99.9% of electromagnetic waves and maintain normal operation of equipment, and can be widely applied to various scenes. The invention relates to the technical field of electromagnetic wave shielding materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a composite film, in particular to a method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film. The invention belongs to the technical field of electromagnetic wave shielding materials. Background Art

[0002] With the rapid development of communication technology and intelligent interactive products, electromagnetic waves, as a carrier of information transmission, play an important role in daily life, military activities, space exploration and other aspects. However, due to the increasing complexity of the current electromagnetic environment, electromagnetic pollution has become inevitable and has become the fourth largest hazard after water pollution, noise pollution and air pollution. At present, the main way to eliminate the negative impact of electromagnetic waves is to use electromagnetic shielding materials to block the propagation path of electromagnetic waves and minimize interference and radiation to the protected targets. Therefore, electromagnetic shielding materials will usher in unprecedented new opportunities and become a key component of electronic materials and even new materials in the future. Metals or metal alloys, such as copper, aluminum, stainless steel, etc., are the earliest materials used for electromagnetic shielding. However, high density, poor specific efficiency, corrosion resistance, high cost, difficult processing and poor mechanical flexibility limit the application of these materials, and they can no longer meet the development trend of equipment towards lightweight, intelligent, flexible and miniature. At present, a large number of research results have shown that polymer-based composites, especially polymer-based composites with carbon materials as conductive fillers, have the characteristics of light weight, flexibility, high cost performance, easy processing and corrosion resistance, and have become new materials for electromagnetic shielding. Carbon fiber is a carbon material composed of a highly oriented turbostratic graphite microcrystalline structure along the fiber axis, and has excellent strength and conductivity in the fiber axis direction. However, the preparation of continuous carbon fiber is difficult, and its brittle nature when exposed to moisture also affects the strength and toughness of the material, which consumes a lot of cost and is harmful to the environment, limiting the further widespread use of polymer-based composite materials with carbon fiber as filler. Summary of the invention

[0003] The present invention aims to solve the problems of complicated steps and poor flexibility in the existing method for preparing carbon fiber / polymer composite films, and further proposes a method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film.

[0004] The technical solution adopted by the present invention to solve the above problems is:

[0005] The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film of the present invention is carried out by the following steps:

[0006] Step 1: heat-treating the carbon fiber in a nitrogen environment to obtain pretreated carbon fiber;

[0007] Step 2: dispersing the product obtained in step 1 into a sensitizing solution containing stannous chloride, filtering, washing and drying after ultrasonic treatment to obtain an intermediate product;

[0008] Step 3, dispersing the product obtained in step 2 into an activation solution containing palladium chloride, filtering, washing, and drying after ultrasonic treatment to obtain sensitized and activated carbon fiber;

[0009] Step 4: dispersing the product obtained in step 3 into a chemical copper plating solution, performing ultrasonic treatment, adding a sodium hydroxide solution to adjust the pH value, stirring at 60° C., filtering, washing, and drying after stirring to obtain a red product;

[0010] Step 5: Evenly mix the product obtained in step 4 with a certain amount of polyethylene powder, put it into a stainless steel mold, transfer the whole to a flat vulcanizer, and perform hot pressing at 200° C. to finally obtain a composite film.

[0011] The high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film formed by the method provided by the present invention mainly successfully combines the characteristics of short-cut carbon fiber such as light weight, simple preparation, and flexibility with the characteristics of metallic copper such as high conductivity. By preparing a high-quality copper plating layer and effectively utilizing the connection structure of metal and fiber and their interaction, the composite film is endowed with greater mechanical properties, so that it has excellent conductivity, mechanical flexibility and high-efficiency electromagnetic interference shielding performance.

[0012] The high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared by the present invention can be used in electromagnetic wave shielding, effectively utilizing the excellent structure of metal and polymer and their interaction to achieve various functions such as high electromagnetic interference shielding performance, mechanical flexibility, and light weight. This multifunctional and ultra-high-performance electromagnetic interference shielding material has broad application prospects.

[0013] Preferably, the thickness of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film is 0.5 mm. At this thickness, the average shielding effectiveness in the X-band reaches 31.15 dB, in other words, it can shield 99.9% of electromagnetic radiation.

[0014] The beneficial effects of the present invention are:

[0015] 1. The high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared by the present invention successfully combines the characteristics of short-cut carbon fiber, such as light weight, simple preparation, and flexibility, with the characteristics of metallic copper, such as high conductivity, and effectively utilizes the connection structure of metal and fiber and their interaction, and has excellent conductivity, mechanical flexibility, and high-efficiency electromagnetic interference shielding performance.

[0016] 2. The preparation method of the present invention adopts chemical plating, which is simple to operate and can adjust the loading amount of copper particles by controlling the reaction time. The obtained copper plating layer has fine crystals and high plating quality.

[0017] 3. The copper-plated fibers give the composite film greater mechanical properties, and are expected to replace traditional high-density and brittle metal shielding materials. They have broad application prospects in the fields of electromagnetic wave shielding, electromagnetic leakage prevention, and electromagnetic protection of high-precision instruments in the field of communication technology.

[0018] 4. The high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared by the present invention has a thickness of 0.5 mm, has good adaptability and good resilience, and its shielding mechanism is mainly reflection. The average shielding effectiveness at 8.2-12.4 GHz reaches 31.15 dB. In other words, the composite film can shield 99.9% of electromagnetic radiation.

[0019] 5. The high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film obtained through ingenious design of the present invention not only effectively avoids the problems of environmental pollution and high costs caused by the use of continuous carbon fiber, but also can effectively shield 99.9% of electromagnetic waves and maintain the normal operation of equipment, and can be widely used in various scenarios; in addition, the composite film has a low production cost and a simple process, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope image of the cross section of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1;

[0021] Figure 2 This is a scanning electron microscope image of the chemically plated carbon fiber in the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1;

[0022] Figure 3 The XRD graphs of the carbon fiber after chemical plating and the carbon fiber only after pretreatment in the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1, wherein curve a is the XRD of the carbon fiber only after pretreatment; curve b is the XRD of the carbon fiber after chemical plating;

[0023] Figure 4 This is a flexibility test diagram of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1;

[0024] Figure 5 It is the average electromagnetic shielding performance of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1. In the figure, group a is the average shielding performance of the comparison sample, and group b is the average shielding performance of the high-efficiency flexible electromagnetic shielding composite film, where the frequency is 8.2~12.4GHz and the thickness is 0.5mm. DETAILED DESCRIPTION

[0025] Specific implementation method 1: The preparation method of a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film described in this implementation method is carried out by the following steps:

[0026] Step 1: heat-treating the carbon fiber in a nitrogen environment to obtain pretreated carbon fiber;

[0027] Step 2: dispersing the product obtained in step 1 into a sensitizing solution containing stannous chloride, filtering, washing and drying after ultrasonic treatment to obtain an intermediate product;

[0028] Step 3, dispersing the product obtained in step 2 into an activation solution containing palladium chloride, filtering, washing, and drying after ultrasonic treatment to obtain sensitized and activated carbon fiber;

[0029] Step 4: dispersing the product obtained in step 3 into a chemical copper plating solution, performing ultrasonic treatment, adding a sodium hydroxide solution to adjust the pH value, stirring at 60° C., filtering, washing, and drying after stirring to obtain a red product;

[0030] Step 5: Evenly mix the product obtained in step 4 with a certain amount of polyethylene powder, put it into a stainless steel mold, transfer the whole to a flat vulcanizer, and perform hot pressing at 200° C. to finally obtain a composite film.

[0031] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the diameter of the carbon fiber used in step 1 is 7 μm, the specific density is 1.8, the tensile strength and Young's modulus are 4.1 GPa and 230 GPa respectively, and the fiber length is 1 mm. Other aspects are the same as specific embodiment 1.

[0032] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the pretreatment temperature in step 1 is 400° C. and the pretreatment time is 30 min. The rest is the same as specific implementation method 1 or 2.

[0033] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that: in step 2, the sensitizing solution is mixed with stannous chloride dihydrate, tin particles, deionized water, and hydrochloric acid (concentration of 36%) in a ratio of 3g:2g:96mL:4mL, and the ultrasonic time is 30min. Others are the same as specific embodiments 1 to 3.

[0034] Specific embodiment 5: This embodiment is different from specific embodiments 1 to 4 in that the activation solution in step 3 is prepared by mixing palladium chloride, deionized water, and hydrochloric acid (36% concentration) in a ratio of 0.04 g: 98 mL: 2 mL, and the ultrasonic time is 30 min. The rest is the same as specific embodiments 1 to 4.

[0035] Specific implementation six: This implementation is different from the specific implementations one to five in that: in step four, the chemical plating solution is made of copper sulfate dihydrate, disodium ethylenediaminetetraacetate, formaldehyde solution, and 2,2-bipyridine mixed in proportion, wherein 3.75g of copper sulfate dihydrate is dissolved in 50mL of deionized water, recorded as liquid A; 8g of disodium ethylenediaminetetraacetate and 2,2-bipyridine are dissolved in 100mL of deionized water, recorded as liquid B; 6.25mL of formaldehyde (concentration of 37%) is dissolved in 100mL of deionized water, recorded as liquid C, and liquid A and liquid B are poured into liquid C in turn and ultrasonically mixed for 30 minutes. The rest is the same as the specific implementations one to five.

[0036] Specific embodiment 7: This embodiment differs from Specific embodiments 1 to 6 in that the concentration of the sodium hydroxide solution in step 4 is 10 g / L, and the pH value is adjusted to 12. The rest is the same as Specific embodiments 1 to 6.

[0037] Specific implementation eight: This implementation differs from specific implementations one to seven in that: the amount of fiber sample added in step four is 0.5 g, and the reaction time is 1 hour. The rest is the same as specific implementations one to seven.

[0038] Specific embodiment 9: This embodiment is different from specific embodiments 1 to 8 in that: the mixing method in step 5 is solution mixing, and the carbon fiber after chemical plating, polyethylene powder, and anhydrous ethanol are mixed in a ratio of 3g:7g:20mL, wherein anhydrous ethanol is used as a solvent, the mixing time is 30min, and then placed in a 100°C oven for 24h to remove the solvent to obtain a mixed powder. The rest is the same as specific embodiments 1 to 8.

[0039] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the conditions for hot pressing in step 5 are: hot pressing temperature 200° C., pressure 15 MPa, hot pressing time 1 hour. Others are the same as specific embodiments 1 to 9.

[0040] The following examples are used to verify the beneficial effects of the present invention:

[0041] Embodiment 1:

[0042] The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film described in this embodiment is specifically carried out according to the following steps:

[0043] First, a carbon fiber with a diameter of 7 μm, a specific density of 1.8, a tensile strength and a Young's modulus of 4.1 GPa and 230 GPa respectively, and a length of 1 mm was placed in a nitrogen environment at 400°C for 30 minutes to obtain a pretreated carbon fiber;

[0044] 2. Disperse the product obtained in step 1 into a sensitizing solution prepared by mixing stannous chloride dihydrate, tin particles, deionized water, and hydrochloric acid (concentration of 36%) in a ratio of 3g:2g:96mL:4mL, and perform ultrasonic treatment for 30 minutes, followed by filtering, washing, and drying to obtain an intermediate product;

[0045] 3. Disperse the product obtained in step 2 into an activation solution prepared by mixing palladium chloride, deionized water, and hydrochloric acid (concentration of 36%) in a ratio of 0.04 g: 98 mL: 2 mL, and perform ultrasonic treatment for 30 min, then filter, wash, and dry to obtain an intermediate product;

[0046] 4. Disperse 0.5 g of the product obtained in step 3 into a chemical copper plating solution prepared by mixing copper sulfate dihydrate, disodium ethylenediaminetetraacetate, formaldehyde solution, and 2,2-bipyridine in proportion, wherein 3.75 g of copper sulfate dihydrate is dissolved in 50 mL of deionized water, recorded as solution A; 8 g of disodium ethylenediaminetetraacetate and 2,2-bipyridine are dissolved in 100 mL of deionized water, recorded as solution B; 6.25 mL of formaldehyde (concentration of 37%) is dissolved in 100 mL of deionized water, recorded as solution C, and successively pour solution A and solution B into solution C and mix them evenly by ultrasonication for 30 min, add 10 g / L sodium hydroxide solution to adjust the pH value to 12, stir at 60°C for 1 h, filter, wash, and dry to obtain a red product;

[0047] 5. Mix the product obtained in step 4 with polyethylene powder and anhydrous ethanol in a ratio of 3g:7g:20mL, wherein anhydrous ethanol is used as the solvent, and the mixing time is 30min. Then, dry it in an oven at 100°C for 24h to remove the solvent to obtain a mixed powder, and then dry it in an oven at 100°C for 24h. Put the mixed powder into a stainless steel mold, transfer it as a whole to a flat vulcanizer, and hot press it at a temperature of 200°C and a pressure of 15MPa for 1h to finally obtain a composite film.

[0048] Comparative Example 1 is that the filler used in step 5 is only pretreated carbon fiber, and the pretreatment process is consistent with the above, that is, under a nitrogen environment, the treatment temperature is 400°C, and the treatment time is 30 minutes; the mixing ratio is consistent with the above, that is, the pretreated carbon fiber, polyethylene powder, and anhydrous ethanol are mixed in a ratio of 3g:7g:20mL.

[0049] Figure 1 This is a scanning electron microscope image of the chemically plated carbon fiber in the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1; it can be seen from the figure that the diameter of a single fiber is relatively small, only about 7μm, and the coating thickness is about 1μm and begins to fill the gaps between the fibers. At this time, the metal clusters completely cover the entire carbon fiber, forming a rod-shaped core-shell structure of carbon fiber / copper. There is no cracking or shedding of the metal layer, indicating that it is well bonded to the fiber matrix.

[0050] Figure 2 This is a scanning electron microscope image of the cross-section of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1; it can be seen from the figure that the mutual contact between the fibers forms a tight and strong three-dimensional conductive network, and there are many micro-conical structures on the surface of the carbon fiber after chemical plating. This rough fiber surface can promote better bonding strength between it and the matrix, so the surface is obviously stained with matrix material, which strongly proves that chemical copper plating can improve the surface roughness of carbon fiber.

[0051] Figure 3 The XRD diagram of the carbon fiber after chemical plating and the carbon fiber only pretreated in the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1, curve a in the figure is the XRD of the carbon fiber only pretreated; curve b is the XRD of the carbon fiber after chemical plating; by comparing the X-ray diffraction standard card, it can be seen that the obtained samples all contain the diffraction peak of graphite carbon, and the carbon fiber after chemical plating has no impurity peak, indicating that no obvious oxidation is caused during chemical copper plating. In addition to the graphite peak, there are diffraction peaks at 2θ=43.3°, 50.4°, and 73.1°, corresponding to the (111), (200) and (220) crystal planes of Cu (JCPDS No.04-0836), and the (111) crystal plane peak is significantly higher than the (200) and (220) crystal plane peaks, indicating that the coating is a copper crystal with a preferred orientation plane of (111).

[0052] Figure 4 This is a flexibility test diagram of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1; it can be seen from the figure that the prepared composite film has good flexibility and is easy to process. This film can be freely bent, curled or sheared according to the needs of use, has good adaptability and good resilience, can be processed into flexible materials of various shapes, and has potential application value in the shielding materials required for complex-shaped equipment.

[0053] Figure 5 The electromagnetic shielding performance average of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1, group a in the figure is the shielding performance average of the comparison sample, and group b is the shielding performance average of the high-efficiency flexible electromagnetic shielding composite film, where the frequency is 8.2-12.4 GHz and the thickness is 0.5 mm; it can be seen from the figure that the average SE of the high-efficiency flexible electromagnetic shielding composite film at a thickness of 0.5 mm is 31.35 dB, far exceeding the SE value (20.0 dB) that can be used as commercial electromagnetic interference shielding. This is attributed to the complete interpenetrating conductive network constructed by the fiber, which can effectively reflect most of the electromagnetic waves, and the difference in dielectric properties of the heterogeneous core-shell structure composed of carbon fiber and coating will cause the redistribution of charge, which increases its shielding effectiveness by 6.57 dB, indicating that the high-efficiency flexible electromagnetic shielding composite film has excellent electromagnetic wave shielding ability.

[0054] Table 1 is a comparison of the mechanical properties and conductive properties of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film prepared in Example 1 and Comparative Example 1.

[0055] Tensile strength(MPa) Elongation at break (%) Electrical conductivity (S / m) Embodiment 1 22.85 24.42 76.53 Comparative Example 1 17.18 16.85 48.60

[0056] Compared with comparative example 1, the tensile strength, elongation at break, and conductivity of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film are significantly improved. The enhancement of mechanical properties means that the two composite films have different interface conditions, and the substantial increase in conductivity can be attributed to the fact that with the coverage of the copper layer on the fiber surface, the copper particles and the carbon fibers are in contact with each other to form a new continuous conductive network, which can connect more conductive areas, and the composite film has a synergistic conductive effect. In general, the mechanical properties and conductive properties of the high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film are excellent.

[0057] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent replacement and improvement made to the above embodiments without departing from the content of the technical solution of the present invention, based on the technical essence of the present invention, within the spirit and principles of the present invention, still fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film, characterized in that: The method is carried out by the following steps: Step 1: heat-treating the carbon fiber in a nitrogen environment to obtain pretreated carbon fiber; Step 2: dispersing the product obtained in step 1 into a sensitizing solution containing stannous chloride, filtering, washing and drying after ultrasonic treatment to obtain an intermediate product; Step 3, dispersing the product obtained in step 2 into an activation solution containing palladium chloride, filtering, washing, and drying after ultrasonic treatment to obtain sensitized and activated carbon fiber; Step 4: dispersing the product obtained in step 3 into a chemical copper plating solution, performing ultrasonic treatment, adding a sodium hydroxide solution to adjust the pH value, stirring at 60° C., filtering, washing, and drying after stirring to obtain a red product; Step 5: Evenly mix the product obtained in step 4 with a certain amount of polyethylene powder, put it into a stainless steel mold, transfer the whole to a flat vulcanizer, and perform hot pressing at 200° C. to finally obtain a composite film.

2. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: The carbon fiber used in step 1 has a diameter of 7 μm, a specific density of 1.8, a tensile strength and a Young's modulus of 4.1 GPa and 230 GPa respectively, and a fiber length of 1 mm.

3. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: The pretreatment temperature in step 1 is 400° C. and the pretreatment time is 30 min.

4. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: The sensitizing solution described in step 2 is prepared by mixing stannous chloride dihydrate, tin particles, deionized water, and hydrochloric acid in a ratio of 3g:2g:96mL:4mL, and the ultrasonic time is 30min; the concentration of the hydrochloric acid is 36%.

5. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: In step 3, the activation solution is prepared by mixing palladium chloride, deionized water, and hydrochloric acid in a ratio of 0.04 g: 98 mL: 2 mL, the ultrasonic time is 30 min, and the concentration of the hydrochloric acid is 36%.

6. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: In step 4, the chemical plating solution is prepared by mixing copper sulfate dihydrate, disodium ethylenediaminetetraacetate, formaldehyde solution, and 2,2-bipyridine in proportion, wherein 3.75 g of copper sulfate dihydrate is dissolved in 50 mL of deionized water, recorded as liquid A; 8 g of disodium ethylenediaminetetraacetate and 2,2-bipyridine are dissolved in 100 mL of deionized water, recorded as liquid B; 6.25 mL of formaldehyde was dissolved in 100 mL of deionized water, which was recorded as liquid C. Liquid A and liquid B were poured into liquid C in sequence and ultrasonicated for 30 minutes. The formaldehyde concentration was 37%.

7. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: In step 4, the concentration of the sodium hydroxide solution is 10 g / L, and the pH value is adjusted to 12.

8. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: In step 4, the amount of fiber sample added is 0.5 g, and the reaction time is 1 h.

9. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: In step five, the mixing method is solution mixing, which is prepared by mixing the chemically plated carbon fiber, polyethylene powder, and anhydrous ethanol in a ratio of 3g:7g:20mL, wherein anhydrous ethanol is used as the solvent, and the mixing time is 30min. The mixture is then placed in an oven at 100°C and dried for 24h to remove the solvent to obtain a mixed powder.

10. The method for preparing a high-efficiency flexible carbon fiber / copper electromagnetic shielding composite film according to claim 1, characterized in that: In step five, the hot pressing molding conditions are: hot pressing temperature 200° C., pressure 15 MPa, and hot pressing time 1 h.

Citation Information

Patent Citations

  • Preparation method for electromagnetic wave shield composite material using copper- and nickel- plated carbon fiber prepared by electroless and electrolytic continuous processes, and electromagnetic wave shield composite material

    CN105284199A

  • Laminated ultra-thin high-performance electromagnetic shielding film and preparation method thereof

    CN108312680A

  • Carbon fiber cloth-nano copper composite material as well as preparation method and application thereof

    CN109207970A

  • Nonwoven fabric or nonwoven composite material for shielding and absorbing electromagnetic wave

    US20160319471A1