Preparation method of efficient hydrogen evolution catalyst Mo / Mo2C

Mo/Mo2C catalyst was synthesized by water bath method and sintering method to form a heterogeneous interface of nanostructures, solving the problem of insufficient activity and stability of Mo2C catalysts, and achieving the effect of efficient water decomposition of hydrogen.

CN118957655APending Publication Date: 2024-11-15SHAANXI UNIV OF SCI & TECH

Patent Information

Application Number
CN202410986086.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Mo2C catalysts are not active and stable in hydrogen evolution reaction, mainly because the d orbital of Mo is not occupied, resulting in strong coupling between H atoms and Mo, and the poor processing capacity of molybdenum carbide particles and the collapse of the surface structure leads to small specific surface area, conductivity and stability. Poor sex.

Method used

Mo/Mo2C catalyst was synthesized by water bath method and sintering method, and the Mo/Mo2C heterogeneity of nanostructured Mo/Mo2C was formed by ultrasonic dispersion, stirring, water bath reaction, centrifugal washing and vacuum drying. Structure, optimize electronic structure and active sites.

Benefits of technology

It improves the activity, conductivity and stability of the catalyst, achieves efficient water decomposition of hydrogen, is suitable for a wide pH range, simplifies the process and improves the purity of the product, and is expected to achieve industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957655A_ABST
    Figure CN118957655A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an efficient hydrogen evolution catalyst Mo / Mo2C, which comprises the following steps: 1, taking molybdenum powder, adding 20-60mL of deionized water, carrying out ultrasonic dispersion to obtain a suspension, weighing 10-30mL of hydrogen peroxide, adding the hydrogen peroxide into the suspension, and stirring until the hydrogen peroxide is completely dissolved to obtain a transparent solution A; 2, filling the solution A into a reaction kettle, sealing the reaction kettle, putting the sealed reaction kettle into a constant-temperature water bath kettle, reacting for 12-24 hours at the water bath temperature of 65-100 DEG C, cooling to room temperature after the reaction is finished, and sequentially carrying out centrifugal washing and vacuum drying to obtain white powder B; and 3, weighing 0.1-3g of the white powder B and 0.5-4g of a carbon source, mixing, grinding, fully and uniformly mixing, filling into a porcelain boat, putting the porcelain boat into a tubular furnace, introducing argon into the tubular furnace, heating from room temperature to 750-950 DEG C at a heating rate of 5-10 DEG C / min, keeping the temperature for 1-5 hours, cooling to room temperature after the reaction is finished, and grinding to obtain the black powdery efficient hydrogen evolution catalyst Mo / Mo2C which has excellent catalytic activity and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water decomposition hydrogen production, and specifically is a method for preparing a high-efficiency hydrogen evolution catalyst Mo / Mo2C. Background Art

[0002] Hydrogen is a clean and efficient energy carrier with the advantages of high energy density and zero emissions of greenhouse gases and environmental pollutants. It has been recognized as a potential alternative to traditional fossil fuels.

[0003] Among all hydrogen production processes, decomposing water to produce hydrogen is a safe, sustainable and environmentally friendly strategy. It has high energy conversion rate, flexible operation and high product purity, and is considered to be one of the most promising hydrogen production technologies in the future. Molybdenum carbide, as a transition metal carbide, has many excellent physical and chemical properties and is an excellent substitute for precious metal catalysts. Considering the diverse electronic states and adjustable phase states of molybdenum, molybdenum carbides represented by Mo2C have attracted special attention in HER.

[0004] However, since the d orbital of Mo in Mo2C is unoccupied, the adjacent H atoms donate their electrons to Mo, forming a strongly coupled Mo-H, which limits the activity of the hydrogen evolution reaction. In addition, molybdenum carbide particles have problems such as poor processing ability, easy agglomeration and surface structure collapse, resulting in a small specific surface area of ​​the catalyst, poor conductivity and stability during the reaction. Summary of the invention

[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a method for preparing a highly efficient hydrogen evolution catalyst Mo / Mo2C, wherein the prepared hydrogen evolution catalyst Mo / Mo2C has excellent catalytic activity and stability.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a highly efficient hydrogen evolution catalyst Mo / Mo2C comprises the following steps:

[0008] Step 1, take 0.1-3g of molybdenum powder, add 20-60mL of deionized water, and disperse by ultrasonic to obtain a suspension, weigh 10-30mL of hydrogen peroxide, add it to the suspension, and stir until it is completely dissolved to obtain a transparent solution A;

[0009] Step 2, the solution A is loaded into a reactor, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 65 to 100° C. for 12 to 24 hours. After the reaction is completed and cooled to room temperature, the solution is centrifuged and washed and vacuum dried in sequence to obtain a white powder B;

[0010] Step 3, weigh 0.1-3g of white powder B and 0.5-4g of carbon source, mix, grind, mix thoroughly and evenly, put into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat from room temperature to 750-950°C at a heating rate of 5-10°C / min, keep warm for 1-5h, wait for the reaction to be completed, cool to room temperature, grind, and obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

[0011] Furthermore, the ultrasonic dispersion time in step 1 is 10 to 20 minutes.

[0012] Furthermore, the stirring in step 1 is performed using a magnetic stirrer at a speed of 350 to 500 r / min for 5 to 30 min.

[0013] Furthermore, in step 2, the volume filling ratio of the reactor is 1 / 3 to 2 / 3.

[0014] Furthermore, the centrifugal washing in step 2 is performed by centrifugation washing with deionized water and anhydrous ethanol for 2 to 5 times respectively.

[0015] Furthermore, the vacuum drying in step 2 is performed in a vacuum drying oven at 60 to 80° C. for 3 to 8 hours.

[0016] Furthermore, the carbon source in step 3 is melamine, dicyandiamide or urea.

[0017] Furthermore, the grinding time in step 3 is 3 to 10 minutes.

[0018] Compared with the prior art, the present invention has the following technical effects:

[0019] The present invention synthesizes a Mo / Mo2C catalyst with high crystallinity through a water bath method and a sintering method. The Mo / Mo2C heterostructure with interconnected nanostructures exhibits multiple active centers, exposes more active sites, has a richer heterogeneous interface, optimizes the electronic structure of Mo2C, promotes electron transfer and electron-hole separation, reduces the adsorption energy of hydrogen atoms, exhibits good catalytic activity, conductivity and stability, can be applied in a wider pH range, and realizes efficient catalytic water electrolysis to produce hydrogen.

[0020] The preparation process of the present invention is not only simple and easy to implement, but also has mild reaction conditions and easy-to-control process. It has the advantages of flexible operation and high product purity, and is expected to achieve industrial production, thereby improving the energy conversion efficiency of hydrogen production by water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The RXD spectrum of the hydrogen evolution catalyst Mo / Mo2C prepared in Example 1 of the present invention;

[0022] Figure 2 This is a SEM image of the hydrogen evolution catalyst Mo / Mo2C prepared in Example 1 of the present invention;

[0023] Figure 3 This is the LSV diagram of the hydrogen evolution catalyst Mo / Mo2C prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.

[0025] Example 1

[0026] Step 1, take 0.95g of molybdenum powder and add it to 20mL of deionized water, ultrasonically disperse it for 10min to obtain a suspension, weigh 20mL of hydrogen peroxide and add it to the suspension, use a magnetic stirrer, stir it at a speed of 450r / min for 20min, and obtain a transparent solution A;

[0027] Step 2, the solution A is loaded into a reactor with a volume filling ratio of 1 / 3 to 2 / 3, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 90°C for 15 hours. After the reaction is completed and cooled to room temperature, the product is centrifugally washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried in a vacuum drying oven at 75°C for 8 hours to obtain a white powder B;

[0028] Step 3, weigh 0.1g of white powder B and 1.0g of dicyandiamide, mix them, grind for 3min, mix them thoroughly, put them into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat the temperature from room temperature to 750°C at a heating rate of 10°C / min, keep warm for 5h, wait for the reaction to be completed, cool to room temperature, take out the product, and grind it to obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

[0029] from Figure 1 It can be seen that the crystal diffraction peaks of Mo2C at 40.52°, 58.61° and 73.68° correspond to the (110), (200) and (211) crystal planes of Mo, respectively, and the diffraction peak of the (110) crystal plane of Mo is very strong, and the sample has high crystallinity, which proves that Example 1 successfully prepared a highly efficient hydrogen evolution catalyst Mo / Mo2C.

[0030] from Figure 2 It can be seen that most of the sample morphologies present uniformly distributed particles, which increases the number of active sites. The rich structural interface optimizes the hydrogen adsorption energy, is beneficial to increase the contact between the material and the electrolyte, exposes more catalytic active sites, helps to regulate the electronic structure of Mo, promotes hydrogen release, and achieves optimization of hydrogen evolution performance.

[0031] from Figure 3 It can be seen that in the 1M KOH electrolyte, the excellent HER performance is maintained at 10mA / cm 2 The overpotential at a current density of 171 mV is excellent, which shows excellent catalytic activity, thus providing a new idea for the development of non-precious metal-based efficient hydrogen evolution catalysts with low cost, excellent performance and good stability.

[0032] Example 2

[0033] Step 1: Take 0.1 g of molybdenum powder and add it to 30 mL of deionized water, and ultrasonically disperse it for 15 minutes to obtain a suspension. Weigh 10 mL of hydrogen peroxide and add it to the suspension. Use a magnetic stirrer to stir it at a speed of 450 r / min for 5 minutes to obtain a transparent solution A.

[0034] Step 2, the solution A is loaded into a reactor with a volume filling ratio of 1 / 3 to 2 / 3, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 65°C for 24 hours. After the reaction is completed and cooled to room temperature, the product is centrifuged and washed twice with deionized water and anhydrous ethanol respectively, and dried in a vacuum drying oven at 80°C for 4 hours to obtain a white powder B;

[0035] Step 3, weigh 1.0g of white powder B and 0.5g of dicyandiamide, mix them, grind for 5min, mix them thoroughly, put them into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat the temperature from room temperature to 950°C at a heating rate of 5°C / min, keep it warm for 1h, wait for the reaction to be completed, cool to room temperature, take out the product, and grind it to obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

[0036] Example 3

[0037] Step 1: 1.42 g of molybdenum powder was added to 40 mL of deionized water, and ultrasonically dispersed for 15 min to obtain a suspension. 20 mL of hydrogen peroxide was weighed and added to the suspension. A magnetic stirrer was used to stir at a speed of 350 r / min for 30 min to obtain a transparent solution A.

[0038] Step 2, the solution A is loaded into a reactor with a volume filling ratio of 1 / 3 to 2 / 3, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 70°C for 20 hours. After the reaction is completed and cooled to room temperature, the product is centrifugally washed with deionized water and anhydrous ethanol for 4 times, respectively, and dried in a vacuum drying oven at 80°C for 3 hours to obtain a white powder B;

[0039] Step 3, weigh 1.5g of white powder B and 3.0g of melamine, mix them, grind for 7min, mix them thoroughly, put them into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat the temperature from room temperature to 800°C at a heating rate of 8°C / min, keep warm for 4h, wait for the reaction to be completed, cool to room temperature, take out the product, and grind it to obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

[0040] Example 4

[0041] Step 1: Take 2.0 g of molybdenum powder and add it to 50 mL of deionized water, and ultrasonically disperse it for 10 min to obtain a suspension. Weigh 30 mL of hydrogen peroxide and add it to the suspension. Use a magnetic stirrer to stir it at a speed of 500 r / min for 15 min to obtain a transparent solution A.

[0042] Step 2, the solution A is loaded into a reactor with a volume filling ratio of 1 / 3 to 2 / 3, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 100° C. for 12 hours. After the reaction is completed and cooled to room temperature, the product is centrifugally washed with deionized water and anhydrous ethanol for 3 times, respectively, and dried in a vacuum drying oven at 70° C. for 5 hours to obtain a white powder B;

[0043] Step 3, weigh 2.5g of white powder B and 2.0g of melamine, mix them, grind for 9min, mix them thoroughly, put them into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat the temperature from room temperature to 850°C at a heating rate of 5°C / min, keep it warm for 2h, wait for the reaction to be completed, cool to room temperature, take out the product, and grind it to obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

[0044] Example 5

[0045] Step 1: 3.0 g of molybdenum powder was added to 60 mL of deionized water, and ultrasonically dispersed for 20 min to obtain a suspension. 30 mL of hydrogen peroxide was weighed and added to the suspension. A magnetic stirrer was used to stir at a speed of 500 r / min for 10 min to obtain a transparent solution A.

[0046] Step 2, the solution A is loaded into a reactor with a volume filling ratio of 1 / 3 to 2 / 3, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 80°C for 18 hours. After the reaction is completed and cooled to room temperature, the product is centrifugally washed with deionized water and anhydrous ethanol for 5 times, respectively, and dried in a vacuum drying oven at 60°C for 7 hours to obtain a white powder B;

[0047] Step 3, weigh 3.0g of white powder B and 4.0g of urea, mix them, grind for 10min, mix them thoroughly, put them into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat the temperature from room temperature to 900°C at a heating rate of 10°C / min, keep warm for 3h, wait for the reaction to be completed, cool to room temperature, take out the product, and grind it to obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

Claims

1. A method for preparing a highly efficient hydrogen evolution catalyst Mo / Mo2C, characterized in that: The steps include: Step 1, take 0.1-3g of molybdenum powder, add 20-60mL of deionized water, and disperse by ultrasonic to obtain a suspension, weigh 10-30mL of hydrogen peroxide, add it to the suspension, and stir until it is completely dissolved to obtain a transparent solution A; Step 2, the solution A is loaded into a reactor, the reactor is sealed and placed in a constant temperature water bath, and the reaction is carried out at a water bath temperature of 65 to 100° C. for 12 to 24 hours. After the reaction is completed and cooled to room temperature, the solution is centrifuged and washed and vacuum dried in sequence to obtain a white powder B; Step 3, weigh 0.1-3g of white powder B and 0.5-4g of carbon source, mix, grind, mix thoroughly and evenly, put into a porcelain boat, put the porcelain boat into a tube furnace, introduce argon into the tube furnace, heat from room temperature to 750-950°C at a heating rate of 5-10°C / min, keep warm for 1-5h, wait for the reaction to be completed, cool to room temperature, grind, and obtain a black powdery high-efficiency hydrogen evolution catalyst Mo / Mo2C.

2. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The ultrasonic dispersion time in step 1 is 10 to 20 minutes.

3. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The stirring in step 1 is performed by using a magnetic stirrer at a speed of 350 to 500 r / min for 5 to 30 min.

4. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The volume filling ratio of the reactor in step 2 is 1 / 3 to 2 / 3.

5. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The centrifugal washing in step 2 is performed by centrifugation washing with deionized water and anhydrous ethanol for 2 to 5 times respectively.

6. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The vacuum drying in step 2 is carried out in a vacuum drying oven at 60 to 80° C. for 3 to 8 hours.

7. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The carbon source in step 3 is melamine, dicyandiamide or urea.

8. The method for preparing the highly efficient hydrogen evolution catalyst Mo / Mo2C according to claim 1, characterized in that: The grinding time of step 3 is 3 to 10 minutes.

Citation Information

Patent Citations

  • Preparation method of three-dimensional bouquet structure alpha-molybdenum carbide@carbon with efficient photothermal conversion characteristic

    CN112194136A

  • Transition metal-Mo-C hydrogen production catalyst, hydrogen evolution electrode, preparation and application

    CN116575073A

Cited By

  • Thin layer preparation process of NiMC self-growing hydrogen evolution cathode