Electrochemical detection method for adsorption form and adsorption quantity of flotation reagent on mineral surface

Through the electrochemical impedance testing method, the problem that the existing technology cannot accurately detect the adsorption form and amount of flotation agents is solved, and the accurate test of mixed ores containing specific minerals is achieved, which improves the monitoring accuracy of the flotation process.

CN118961828APending Publication Date: 2024-11-15SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048118.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing electrochemical testing methods cannot be effectively used in mixed ores containing fluorocarbon cerium ore and calcite ore, mixed ore containing spodumene and feldspar ore ore containing limonite and quartz ore. The precise determination of the adsorption form and adsorption volume of the agent leads to inaccurate monitoring of the flotation process.

Method used

Using electrochemical impedance testing method, electrochemical impedance test is performed by preparing the negative electrode material and coating it on zinc foil, combining polyvinylidene fluoride and N-methylpyrrolidone, and analyzing the mixture of the negative electrode of the original mineral and mineral with the flotation agent. Electrochemical impedance curve, qualitative semi-quantitative judgment of the adsorption form and adsorption volume of the agent.

Benefits of technology

Accurate testing of the above three minerals has been achieved. The test results are highly accurate and reproducible. They can accurately monitor the adsorption of flotation agents, and are suitable for determining the form and quantity of the agent during flotation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118961828A_ABST
    Figure CN118961828A_ABST
Patent Text Reader

Abstract

The invention provides an electrochemical detection method for the adsorption form and the adsorption quantity of a flotation reagent on the surface of a mineral, and belongs to the technical field of mineral flotation separation. The invention discloses an electrochemical detection method for the adsorption form and the adsorption quantity of a beneficiation reagent on the surface of a mineral. The method comprises the following steps: (1) preparing a mineral and flotation reagent negative electrode material; (2) preparing a negative electrode; (3) assembling the battery; and (4) testing electrochemical alternating current impedance. The method has the advantages that the scheme for testing the adsorption form and the adsorption capacity of the flotation reagent on the surface of the mineral through the electrochemical alternating-current impedance is reasonable in design, the mineral and the flotation reagent are pretreated, an electrochemical resistance test is carried out after the battery is manufactured and assembled, the stability is improved to a certain extent, and the test efficiency is improved. On one hand, the medicament and the mineral are combined more tightly and act more sufficiently, and on the other hand, the test accuracy can be improved, and the test reproducibility is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral flotation separation, and in particular relates to an electrochemical detection method for the adsorption form and adsorption amount of a flotation agent on a mineral surface. Background Art

[0002] Electrochemistry is a science that studies the conversion between chemical energy and electrical energy. Electrochemical impedance spectroscopy is an important method for studying the properties of electrode interfaces. By applying a small amplitude sine wave at both ends of the system, the impedance curve with the sine wave frequency ω is obtained through the system's response signal to the sine wave, which is used to analyze structural information such as the electrode-electrolyte contact interface resistance and solution resistance.

[0003] In recent years, in order to improve the properties of batteries, researchers have studied the surface modification technology of forming a protective layer on the surface of zinc, which has attracted widespread attention due to its simple and effective advantages, including the use of natural minerals for surface modification. This technology uses the crystal structure and unique physical and chemical properties of minerals. When negatively charged minerals form a protective layer on the surface of zinc, they show good cation selectivity and desolvation ability. The negatively charged intermediate layer helps promote the Zn 2+ Ions cross mineral interfaces and screen SO4 by electrostatic repulsion 2- In addition, the mineral interface with Zn 2+ The binding energy of the ion is higher than that of Zn 2+ -H2O, thus showing excellent desolvation ability, thus kinetically promoting the rapid and uniform deposition of Zn, at which time the electrochemical impedance becomes smaller. Conversely, when positively charged minerals form a protective layer on the zinc surface, the positively charged intermediate layer inhibits the deposition of Zn. 2+ Ions pass through the mineral interface and electrostatically attract SO4 2- In addition, the mineral interface with Zn 2+ The binding energy of the ion is lower than that of Zn 2+ -H2O, thus showing excellent desolvation ability, thus kinetically inhibiting the rapid and uniform deposition of Zn, and the electrochemical impedance becomes larger. 2+ The analysis is tested by measuring how fast the ions move between the two electrodes.

[0004] However, for mixed ores containing bastnaesite and calcite, mixed ores containing spodumene and feldspar, or mixed ores containing limonite and quartz, the existing electrochemical testing methods cannot be effectively used to accurately determine the adsorption form and approximate adsorption ratio of flotation agents in the flotation of the above three minerals, and thus cannot accurately monitor the flotation process.

[0005] Therefore, it is urgent to propose a method that can accurately detect the above three mixed minerals. Summary of the invention

[0006] The present invention is to solve the above technical problems, thereby providing an electrochemical detection method for the adsorption form and adsorption amount of flotation reagents on the mineral surface. The adsorption form and adsorption amount of flotation reagents on the mineral surface are characterized by electrochemical impedance testing, the flotation performance of the reagents on the mineral is predicted, and the flotation mechanism is deeply explored. The sample preparation process and operation method of the method are simple, and the test results are accurate and reproducible.

[0007] The present invention relates to an electrochemical detection method for the adsorption form and adsorption amount of a flotation agent on a mineral surface, which characterizes the adsorption form and adsorption amount difference of a flotation agent on a mineral surface through electrochemical impedance testing, predicts the flotation performance of the agent on the mineral, and conducts an in-depth study of the flotation mechanism. The method has a simple sample preparation process and operation method, and the test results are highly accurate and reproducible.

[0008] The technical solution provided by the present invention to solve the above problems is:

[0009] An electrochemical detection method for the adsorption form and adsorption amount of a flotation agent on a mineral surface comprises the following steps:

[0010] (1) preparing negative electrode materials, wherein the negative electrode materials to be prepared include raw mineral negative electrode materials and mixed negative electrode materials of minerals and flotation agents;

[0011] (2) preparing a negative electrode using the negative electrode material obtained in step (1), uniformly and fully mixing the negative electrode material with polyvinylidene fluoride and N-methylpyrrolidone in proportion, and coating the mixture on a zinc foil using a doctor blade method;

[0012] (3) Assembling a symmetrical battery with the negative electrode obtained in step (2), pressing the zinc foil into a circular electrode piece with a diameter of 12 mm, and using a glass fiber separator with a diameter of 16 mm to assemble a CR2025 button battery.

[0013] (4) connecting the battery of step (3) and testing it using an electrochemical workstation, and performing electrochemical impedance tests on the original mineral negative electrode and the mixed negative electrode of the mineral and the flotation agent;

[0014] (5) Analyze the electrochemical impedance test results obtained in step (4) by comparing the impedance differences in the electrochemical impedance curves of the original mineral negative electrode material and the mixed negative electrode material of the mineral and the flotation agent, so as to qualitatively and semi-quantitatively determine the adsorption form of the agent in the mineral and the approximate adsorption amount ratio.

[0015] The above-mentioned test method provided by the present invention realizes the use of electrochemical impedance to accurately test the adsorption of minerals and agents. Through the test method of the present invention, the mineral is coated on the zinc foil. When the mineral has good water dispersibility and rheological properties, and the interlayer of the layered lattice is negatively charged, it shows good cation selectivity and the electrochemical impedance becomes smaller; when the mineral acts on the agent, the mineral property changes and becomes positively charged. At this time, the cation selectivity becomes worse and the electrochemical impedance becomes larger, thereby realizing the accurate testing of three minerals, namely, a mixed ore containing fluorocarbon cerium and calcite ore, a mixed ore containing spodumene ore and feldspar ore, or a mixed ore containing limonite and quartz ore, and the test has high accuracy and good reproducibility.

[0016] Furthermore, the raw mineral negative electrode material in step (1) is a negative electrode material made from the mineral to be measured, and the mixed negative electrode material of the mineral and the flotation agent is a negative electrode material prepared by uniformly mixing the mineral to be measured and the flotation agent under optimal flotation conditions.

[0017] Furthermore, the raw mineral includes any one of a mixed ore containing bastnaesite and calcite, a mixed ore containing spodumene and feldspar, and a mixed ore containing limonite and quartz.

[0018] Furthermore, the flotation reagent is a cationic collector, and the cationic collector includes N-dodecylpropanolamine, dodecylamine or ethane-1,2-dodecyldimethylammonium bromide.

[0019] Furthermore, the optimal flotation conditions for preparing the mixed negative electrode material of the mineral and the flotation agent in step (1) include the pH of the ore pulp and the concentration of the flotation agent.

[0020] Furthermore, in the step (1), the mineral used to prepare the negative electrode material needs to be ground using a planetary ball mill for 0.5 to 3 hours to grind the mineral to a particle size of 1 to 10 microns.

[0021] Furthermore, the detailed sample preparation process of the negative electrode in step (2) is:

[0022] 1) Add 2 grams of ground mineral to 40 ml of deionized water, adjust the solution pH to the optimal value, and add appropriate concentration of flotation reagent as needed. The mixture is mechanically stirred for 0.5 to 3 hours and then dried;

[0023] 2) Using polyvinylidene fluoride (PVDF) and the above-mentioned minerals as raw materials, with a mass ratio of 2:8, adding an appropriate amount of n-methylpyrrolidone (NMP) solvent, putting them into a mortar and grinding them evenly;

[0024] 3) The slurry was evenly scraped onto zinc foil and dried under vacuum at 60°C.

[0025] Furthermore, the electrochemical impedance test workstation of step (2) is a three-electrode system, the negative electrode material of the electrode test is metallic zinc, the test quiet time sampling interval is 1ms, the test frequency range is 100kHz to 100mHz, and the AC excitation amplitude is 10mV.

[0026] Compared with the prior art, the advantages of the present invention are as follows:

[0027] The present invention applies the impedance test method in electrochemistry to the determination of the adsorption form and adsorption amount of flotation reagents on the mineral surface. 2+ The difference in the speed of ion passage is compared with the resistance difference in the electrochemical impedance curve of the original ore electrode and the mixed electrode of the mineral and the flotation agent, so as to qualitatively and quantitatively determine the adsorption form of the agent in the mineral and the approximate adsorption amount ratio. The method of the present invention is aimed at three minerals: a mixed ore containing bastnaesite and calcite, a mixed ore containing spodumene and feldspar, or a mixed ore containing limonite and quartz. The test results are highly accurate and close to the flotation test results, and can be well used for determining the adsorption form of the agent and the approximate adsorption amount ratio during the flotation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The present invention is a schematic diagram showing the principle of using the electrochemical detection method provided by the present invention to determine the adsorption form and adsorption amount of flotation reagents on the mineral surface. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the embodiments. It is necessary to point out that the following embodiments are only used to explain and illustrate the present invention and are not used to limit the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above invention content still belong to the protection scope of the present invention.

[0030] Example 1

[0031] Preparation and electrochemical testing of bastnaesite and calcite anode materials

[0032] (1) Preparation of bastnaesite and calcite negative electrode materials

[0033] Add appropriate amount of deionized water and raw mineral (fluorocarbon cerium ore / calcite) into a ball mill, grind in a planetary ball mill for 0.5 to 3 hours to obtain a mineral material with a particle size of 1 to 10 μm, and freeze-dry for later use;

[0034] A beaker containing 1 g of mineral material and 35 mL of deionized water was placed on a magnetic stirrer, and the mixture was stirred for 3 minutes. The pH value of the slurry was adjusted to 8 and stirred for 1 hour. The obtained material was centrifuged at 5000 rpm, and then washed with deionized water for 5 times and freeze-dried to obtain the original fluorocarbon cerium ore / calcite negative electrode material.

[0035] A beaker containing 1 g of mineral material and 35 mL of deionized water was placed on a magnetic stirrer and stirred for 3 minutes. The pH value of the slurry was adjusted to 8, and 0.1 mM N-dodecylpropanolamine cationic collector was added. After adding the collector, the pH value of the slurry was continued to be adjusted to 8, and then stirred for 1 hour. The obtained material was centrifuged at 5000 rpm, then washed with deionized water 5 times, and freeze-dried to obtain the original fluorocarbon cerium ore / calcite and the mixed negative electrode material of fluorocarbon cerium ore / calcite and N-dodecylpropanolamine collector.

[0036] (2) Preparation of bastnaesite and calcite negative electrodes and battery assembly

[0037] Polyvinylidene fluoride (PVDF) and the negative electrode material prepared above were used as raw materials in a mass ratio of 2:8. An appropriate amount of n-methylpyrrolidone (NMP) solvent was added, and the slurry was evenly ground in a mortar for 10 minutes. The slurry was cast on a zinc foil with a thickness of 100 μm by a simple scraping method, and vacuum dried overnight at 60 ° C to obtain a zinc foil with a thickness of 10 μm. Pure zinc foil and zinc foil with a protective layer of raw mineral or raw mineral and N-dodecyl propanolamine were pressed into a circular pole piece with a diameter of 12 mm, and a CR2025 button cell was assembled using a glass fiber separator with a diameter of 16 mm. In order to standardize the measurement, a fixed amount of 2M ZnSO4 electrolyte was used in each battery. The batteries were assembled in an open environment.

[0038] (3) Zeta potential test of bastnaesite and calcite negative electrode materials

[0039] At pH 8, the zeta potential of bastnaesite and calcite with or without 0.1mM N-dodecyl propanolamine was measured to verify the effect of the charge state of the mineral protective layer on the electrochemical impedance. After testing, the zeta potentials of the original minerals bastnaesite and calcite were -2.79mV and +2.51mV, respectively. After adding 0.1mM N-dodecyl propanolamine, the zeta potential of bastnaesite moved from -2.79mV to +28.7mV, indicating that the positively charged N-dodecyl propanolamine has a strong adsorption force on the surface of bastnaesite. For calcite, the Zeta potential of the calcite surface remained basically unchanged (5.08mV) after the action of N-dodecyl propanolamine, which means that the adsorption force between the positively charged N-dodecyl propanolamine and the positively charged calcite between the layers is very weak, and it can be used for the electrochemical test of the flotation reagent.

[0040] (4) Electrochemical impedance spectroscopy of bastnaesite and calcite negative electrode materials

[0041] Compared with the impedance of pure zinc (72Ω), the impedance of the zinc negative electrode coated with the bastnaesite raw ore protective layer decreased, while the resistance of the zinc negative electrode coated with the calcite raw ore protective layer increased slightly, indicating that the negatively charged bastnaesite has cation selective permeability, which is beneficial to Zn 2+ The rapid passage of Zn near the surface 2+ The sufficient concentration of SO4 2- .

[0042] The electrochemical impedance test results of the mixed negative electrode after the interaction between bastnaesite / calcite and N-dodecyl propanolamine showed that the impedance of the mixed zinc negative electrode of bastnaesite and N-dodecyl propanolamine increased significantly, from 60Ω to 130Ω. On the contrary, the impedance of the mixed zinc negative electrode of calcite and N-dodecyl propanolamine changed little, indicating that a large amount of positively charged N-dodecyl propanolamine adsorbed on the negatively charged surface of bastnaesite made the mineral interlayer positively charged, which repelled the positively charged Zn 2+ , there is no guarantee that there is sufficient Zn near the surface 2+ concentration, and attracts negatively charged SO4 2- The above results show that the method of the present invention can be used for electrochemical testing of the flotation reagent.

[0043] Example 2

[0044] Preparation and electrochemical testing of spodumene and feldspar anode materials

[0045] (1) Preparation of spodumene and feldspar negative electrode materials

[0046] Add appropriate amount of deionized water and raw mineral (spodumene / feldspar) into a ball mill, grind in a planetary ball mill for 0.5 to 3 hours to obtain a mineral material with a particle size of 1 to 10 μm, and freeze-dry for later use;

[0047] A beaker containing 1 g of mineral material and 35 mL of deionized water was placed on a magnetic stirrer, and the mixture was stirred for 3 minutes. The pH value of the slurry was adjusted to 8 and stirred for 1 hour. The obtained material was centrifuged at 5000 rpm, and then washed with deionized water for 5 times and freeze-dried to obtain the original spodumene / feldspar negative electrode material.

[0048] A beaker containing 1 g of mineral material and 35 mL of deionized water was placed on a magnetic stirrer, stirred thoroughly for 3 minutes, the pH value of the slurry was adjusted to 8, 0.1 mM dodecylamine cationic collector was added, and the pH value of the slurry was continued to be adjusted to maintain at 8 after adding the collector, and then stirred for 1 hour. The obtained material was centrifuged at 5000 rpm, then washed 5 times with deionized water, and freeze-dried to obtain a mixed negative electrode material of original spodumene / feldspar and dodecylamine.

[0049] (2) Preparation of spodumene and feldspar negative electrodes and battery assembly

[0050] Polyvinylidene fluoride (PVDF) and the negative electrode material prepared above were used as raw materials in a mass ratio of 2:8. An appropriate amount of n-methylpyrrolidone (NMP) solvent was added, and the slurry was evenly ground in a mortar for 10 minutes. The slurry was cast on a zinc foil with a thickness of 100 μm by a simple scraping method, and vacuum dried overnight at 60 ° C to obtain a protective layer with a thickness of 10 μm. Pure zinc foil and zinc foil with a protective layer of raw mineral or raw mineral and dodecylamine were pressed into circular pole pieces with a diameter of 12 mm, and a CR2025 button cell was assembled using a glass fiber separator with a diameter of 16 mm. In order to standardize the measurement, a fixed amount of 2M ZnSO4 electrolyte was used in each battery. The batteries were assembled in an open environment.

[0051] (3) Electromechanical potential test of spodumene and feldspar negative electrode materials

[0052] At pH 8, the electrokinetic potentials of spodumene and feldspar were measured with or without the action of 0.1mM dodecylamine. The test showed that the electrokinetic potentials of the original minerals spodumene and feldspar were -40.21mV and -60.24mV respectively; when 0.1mM dodecylamine was added, the electrokinetic potentials of spodumene and feldspar shifted to +2.79 and +10.23mV respectively, indicating that dodecylamine has a strong adsorption force on the surface of both spodumene and feldspar, but the adsorption force between feldspar is stronger. It can be used for electrochemical testing of the flotation reagent.

[0053] (4) Electrochemical impedance test of spodumene and feldspar negative electrode materials

[0054] Compared with the impedance of pure zinc (72Ω), the impedance of the zinc negative electrode coated with spodumene and feldspar raw ore protective layers decreased to 58Ω and 48Ω, respectively, indicating that the two negatively charged minerals have cation selective permeability, which is beneficial to Zn 2+ The rapid passage of Zn near the surface 2+ Adequate concentration while eliminating SO4 2- .

[0055] The electrochemical impedance test results of the mixed negative electrode after the interaction between spodumene and feldspar and dodecylamine showed that the impedance of the mixed negative electrode increased significantly. The impedance of the mixed negative electrode after the interaction between spodumene and dodecylamine was 124Ω, and the impedance of the mixed negative electrode after the interaction between feldspar and dodecylamine was 133Ω, indicating that a large amount of positively charged dodecylamine was adsorbed on the negatively charged surface of spodumene and feldspar, making the mineral interlayer positively charged, and repelling the positively charged Zn 2+ , there is no guarantee that there is sufficient Zn near the surface 2+ concentration, and attracts negatively charged SO4 2- The above results show that the method of the present invention can be used for electrochemical testing of the flotation reagent.

[0056] Example 3

[0057] Preparation and electrochemical testing of limonite and quartz negative electrode materials

[0058] (1) Preparation of limonite and quartz negative electrode materials

[0059] Add appropriate amount of deionized water and raw mineral (limonite / quartz) into a ball mill, grind in a planetary ball mill for 0.5 to 3 hours to obtain a mineral material with a particle size of 1 to 10 μm, and freeze-dry for later use;

[0060] A beaker containing 1 g of mineral material and 35 mL of deionized water was placed on a magnetic stirrer, and the mixture was stirred for 3 minutes. The pH value of the slurry was adjusted to 8 and stirred for 1 hour. The obtained material was centrifuged at 5000 rpm, and then washed with deionized water for 5 times and freeze-dried to obtain the original spodumene / feldspar negative electrode material.

[0061] A beaker containing 1 g of mineral material and 35 mL of deionized water was placed on a magnetic stirrer and stirred thoroughly for 3 minutes. The pH value of the slurry was adjusted to 8, and 0.1 mM ethane-1,2-dodecyldimethylammonium bromide cationic collector was added. After adding the collector, the pH value of the slurry was continued to be adjusted to maintain at 8, and then stirred for 1 hour. The obtained material was centrifuged at 5000 rpm, then washed 5 times with deionized water, and freeze-dried to obtain a mixed negative electrode material of original limonite / quartz and ethane-1,2-dodecyldimethylammonium bromide.

[0062] (3) Preparation of limonite and quartz negative electrodes and battery assembly

[0063] Polyvinylidene fluoride (PVDF) and the negative electrode material prepared above were used as raw materials in a mass ratio of 2:8. An appropriate amount of n-methylpyrrolidone (NMP) solvent was added, and the slurry was evenly ground in a mortar for 10 minutes. The slurry was cast on a zinc foil with a thickness of 100 μm by a simple scraping method, and vacuum dried overnight at 60 ° C to obtain a thickness of 10 μm. Pure zinc foil and zinc foil with a protective layer of raw mineral or raw mineral and ethane-1,2-dodecyldimethylammonium bromide were pressed into circular pole pieces with a diameter of 12 mm, and a CR2025 button cell was assembled using a glass fiber separator with a diameter of 16 mm. In order to standardize the measurement, a fixed amount of 2M ZnSO4 electrolyte was used in each battery. The batteries were assembled in an open environment.

[0064] (3) Electrodynamic potential test of limonite and quartz negative electrode materials

[0065] At pH 8, the electrokinetic potential test of limonite and quartz with or without 0.15mM ethane-1,2-dodecyldimethylammonium bromide was measured to verify the effect of the charge state of the mineral protective layer on the electrochemical impedance. After testing, the electrokinetic potentials of the original minerals limonite and quartz were -42.84mV and -20.74mV, respectively. After adding 0.15mM ethane-1,2-dodecyldimethylammonium bromide, the electrokinetic potentials of spodumene and feldspar shifted positively to +20.54 and +0.24mV, respectively, indicating that ethane-1,2-dodecyldimethylammonium bromide has a certain adsorption force on the surface of limonite and quartz. Since quartz has more negative charge at this time, it adsorbs more cationic collector ethane-1,2-dodecyldimethylammonium bromide. It can be used for electrochemical testing of the flotation reagent.

[0066] (4) Electrochemical impedance spectroscopy of limonite and quartz negative electrode materials

[0067] Compared with the impedance of pure zinc (72Ω), the impedance of the zinc negative electrode coated with limonite and quartz ore protective layers decreased to varying degrees, 65Ω and 38Ω, respectively, indicating that the two negatively charged minerals have cation selective permeability, which is beneficial to Zn 2+ The rapid passage of Zn 2+The electrochemical impedance test results of the mixed negative electrode after the interaction between limonite and quartz and ethane-1,2-dodecyldimethylammonium bromide showed that the impedance of the mixed negative electrode increased significantly. The impedance of the mixed negative electrode after the interaction between limonite and ethane-1,2-dodecyldimethylammonium bromide was 114Ω, and the impedance of the mixed negative electrode after the interaction between quartz and ethane-1,2-dodecyldimethylammonium bromide was 158Ω, indicating that a large amount of positively charged ethane-1,2-dodecyldimethylammonium bromide is more easily adsorbed on the negatively charged surface of limonite and quartz, making the mineral interlayer positively charged and more strongly repelling Zn 2+ , making the surface Zn 2+ The above results show that the method of the present invention can be used for electrochemical testing of the flotation reagent.

[0068] According to the test results of the above-mentioned Examples 1-3, the electrochemical testing method of the present invention can be used to qualitatively and semi-quantitatively determine the approximate situation of the adsorption morphology and adsorption amount ratio of the agent on the mineral surface, and it has the advantages of high test accuracy and good reproducibility.

[0069] Comparative Example 1

[0070] Comparison between existing electrochemical testing methods and this method:

[0071] (1) Fluorine carbon ore, limonite and spodumene were ground to -38 μm respectively to prepare pure mineral electrodes and calcite pure mineral electrodes. The working electrode was a glassy carbon electrode with a diameter of 4 mm and a binder of Nafion.

[0072] (2) Cyclic voltammetry curve test was carried out using CHI760E electrochemical workstation. The test used a three-phase electrode system, in which the prepared pure mineral electrode was used as the working electrode, the reference electrode was a saturated Ag / AgCl electrode, the auxiliary electrode was a platinum electrode, and a 0.1 mol / L sodium sulfate solution was used as the electrolyte. The scanning rate was 0 / 1 V / S, and the scanning voltage range was -0.8 V to 0.8 V to carry out electrochemical impedance spectroscopy.

[0073] (3) The test results show that the electrochemical impedance of pure bastnaesite is 65Ω when fluorine bastnaesite, spodumene and limonite are respectively acted with cationic collectors. The electrochemical impedance of pure fluorine bastnaesite is 65Ω, and the electrochemical impedance measured after the action of cationic collector N-dodecyl propanolamine is 64Ω. The electrochemical impedance of spodumene and dodecylamine does not increase but decreases. The electrochemical impedance of pure spodumene electrode test is 58Ω, and the electrochemical impedance of the action is 50Ω. The electrochemical impedance of limonite changes from 69Ω to 75Ω after the action of cationic collector ethane-1,2-dodecyl dimethyl ammonium bromide. The above test results are inconsistent with the flotation results, indicating that the existing test method cannot be widely applied to the electrochemical test of oxide ores, but has a good test effect on the above three mixed minerals of the present invention.

[0074] It can be seen that the test method of the present invention has more accurate results than the previous test methods and is more consistent with the flotation test results.

Claims

1. An electrochemical detection method for the adsorption form and adsorption amount of a flotation agent on a mineral surface, characterized in that: The following steps are involved: (1) preparing negative electrode materials, wherein the prepared negative electrode materials include raw mineral negative electrode materials and mixed negative electrode materials of minerals and flotation agents; (2) preparing a negative electrode, uniformly and fully mixing the negative electrode material with polyvinylidene fluoride and N-methylpyrrolidone in proportion, and coating the mixture on a zinc foil using a doctor blade method; (3) Assembling symmetrical cells, pressing zinc foil into a circular electrode with a diameter of 12 mm, and assembling the cell using a glass fiber separator with a diameter of 16 mm; (4) Connecting the electrodes and using an electrochemical workstation to perform electrochemical impedance spectroscopy on the negative electrode of the original mineral and the mixed negative electrode of the mineral and flotation reagent; (5) Analysis of electrochemical impedance test results: By comparing the impedance differences in the electrochemical impedance curves of the original mineral negative electrode material and the mixed negative electrode material of the mineral and the flotation agent, the adsorption morphology and adsorption ratio of the agent on the mineral surface can be qualitatively and semi-quantitatively determined.

2. The detection method according to claim 1, characterized in that: The raw mineral negative electrode material is a negative electrode material made of the mineral to be measured, and the mixed negative electrode material of the mineral and the flotation agent is a negative electrode material prepared by uniformly mixing the mineral to be measured and the flotation agent under optimal flotation conditions.

3. The detection method according to claim 1 or 2, characterized in that: The raw mineral includes any one of a mixed ore containing bastnaesite and calcite, a mixed ore containing spodumene and feldspar, and a mixed ore containing limonite and quartz.

4. The detection method according to claim 1 or 2, characterized in that: The flotation reagent is a cationic collector, and the cationic collector includes N-dodecylpropanolamine, dodecylamine or ethane-1,2-dodecyldimethylammonium bromide.

5. The detection method according to claim 1 or 2, characterized in that: In the step (1), the mineral used to prepare the negative electrode material is ground using a planetary ball mill for 0.5 to 3 hours to grind the mineral into a particle size of 1 to 10 microns.

6. The detection method according to claim 1 or 2, characterized in that: The optimal flotation conditions include pulp pH and flotation reagent concentration.

7. The detection method according to claim 1 or 2, characterized in that: The raw ore negative electrode material is prepared by adding 2 grams of ground minerals to 40 milliliters of deionized water, adjusting the solution pH to the optimum, adding a flotation agent of appropriate concentration as required, and drying the mixture after mechanical stirring for 0.5 to 3 hours; using polyvinylidene fluoride and the above-mentioned minerals as raw materials, the mass ratio is 2:8, adding an appropriate amount of n-methylpyrrolidone solvent, putting them in a mortar and grinding them evenly, scraping the slurry evenly on zinc foil, and vacuum drying at 60°C.

8. The detection method according to claim 1 or 2, characterized in that: The electrochemical impedance test workstation is a three-electrode system, the test quiet time sampling interval is 1 ms, the test frequency range is 100 kHz to 100 mHz, and the AC excitation amplitude is 10 mV.