Method for forming photodiode

Through wet pretreatment and slow temperature drop hydrogen baking technology, the defects caused by high-temperature baking during the formation of high-deep aspect ratio photodiodes are solved, and the reliability and yield of the device are improved.

CN118969916APending Publication Date: 2024-11-15HUA HONG SEMICON WUXI LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410956012.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the manufacturing of semiconductor integrated circuits, high-deep aspect ratio photodiode formation process, high-temperature hydrogen baking can easily lead to trench structure defects, affecting the electrical parameters and reliability of the device.

Method used

采用湿法工艺进行第一预处理,随后通过降低氢气流量和保持烘烤温度缓降的方式进行氢气烘烤,降低沟槽上部和底部的烘烤能力差异,避免缺陷产生。

Benefits of technology

Improve the reliability and yield of the photodiode and reduce the morphological defects of deep grooves due to hydrogen baking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969916A_ABST
    Figure CN118969916A_ABST
Patent Text Reader

Abstract

The invention discloses a photodiode forming method comprising the following steps: forming a hard mask layer on a first epitaxial layer which is formed on a silicon substrate; forming a first groove in the hard mask layer, wherein the first epitaxial layer at the bottom of the first groove is exposed; etching is carried out to reach the preset depth in the first epitaxial layer below the first groove, a second groove is formed in the first epitaxial layer, and the ratio of the depth to the width of the second groove is larger than 4; carrying out first pretreatment through a wet process; second pretreatment is conducted through hydrogen baking, and in the second pretreatment process, baking is conducted in the mode that the flow of hydrogen is reduced and the baking temperature is kept decreased in the pretreatment process; and filling a second epitaxial layer in the second groove. According to the invention, the baking capability difference between the upper part and the bottom part of the groove can be reduced, thereby solving the defect of deep groove morphology caused by hydrogen baking, and improving the reliability and yield of a device product to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor devices and integrated circuit technology, and in particular to a method for forming a photodiode. Background Art

[0002] In the semiconductor integrated circuit manufacturing industry, the epitaxy (EPI) process has been increasingly widely used due to its good quality and easy control of doping concentration. For some special processes, the selective epitaxy growth (SEG) process is usually used to fill the epitaxial layer. In the epitaxial filling process of trenches and holes with high aspect ratios (the ratio of height to depth is greater than 4), defects such as void defects and dislocation defects are very likely to occur.

[0003] Taking complementary metal oxide semiconductor contact image sensor (CIS) as an example, in order to improve the sensitivity on small-sized pixels, a deep photodiode (PD) can be formed first, and then the surface device structure can be formed. This can avoid the process limits of ion implantation and photolithography, thereby expanding the space of the photodiode vertically to avoid the limitation of the aspect ratio of the photoresist.

[0004] However, when forming a deep photodiode structure, it is necessary to first etch to form a trench with a high aspect ratio and then fill the trench with an epitaxial layer. Since the trench to be filled has a columnar structure and the size of the structure is small, the high-temperature hydrogen baking (H2 bake) pretreatment process before the epitaxial layer filling will affect the columnar structure before the epitaxial layer grows, causing certain changes in its structure, thereby causing defects in the subsequent filling, and further affecting the electrical parameters of the device; if a lower temperature is used for pretreatment, since the trench to be filled has a high aspect ratio, the native oxide layer (native oxide) in the trench is often unable to be completely removed, which will also affect the electrical parameters, thereby reducing the reliability and yield of the device. Summary of the invention

[0005] The present application provides a method for forming a photodiode, which can solve the problem that the method for forming a photodiode with a high aspect ratio provided in the related art is prone to defects after high-temperature hydrogen baking. The method comprises:

[0006] forming a hard mask layer on a first epitaxial layer, wherein the first epitaxial layer is formed on a silicon substrate;

[0007] forming a first trench in the hard mask layer, wherein the first epitaxial layer at the bottom of the first trench is exposed;

[0008] Performing etching to a predetermined depth in the first epitaxial layer below the first trench to form a second trench in the first epitaxial layer, wherein a ratio of the depth to the width of the second trench is greater than 4;

[0009] Performing a first pretreatment by a wet process;

[0010] Performing a second pretreatment by hydrogen baking, during which the baking is performed by reducing the flow rate of hydrogen and keeping the baking temperature lowered during the pretreatment;

[0011] A second epitaxial layer is filled in the second trench.

[0012] In some embodiments, after the second trench is formed by etching, a pillar structure is formed in the second trench.

[0013] In some embodiments, during the second pretreatment, the decreasing rate of the baking temperature is 5 degrees Celsius per minute to 20 degrees Celsius per minute.

[0014] In some embodiments, during the second pretreatment, the flow rate of hydrogen is 10 liters per minute to 40 liters per minute.

[0015] In some embodiments, filling the second epitaxial layer in the second trench includes:

[0016] forming a buffer layer on the first epitaxial layer and the surface of the trench by an epitaxial process;

[0017] forming a second epitaxial layer on the buffer layer;

[0018] A planarization process is performed to remove the buffer layer and the second epitaxial layer outside the second trench.

[0019] In some embodiments, the hard mask layer includes a silicon nitride layer.

[0020] In some embodiments, forming a buffer layer on the first epitaxial layer and the surface of the trench by an epitaxial process includes:

[0021] The buffer layer is formed on the first epitaxial layer and the surface of the trench by a selective epitaxial process.

[0022] The technical solution of this application has at least the following advantages:

[0023] In the process of forming a photodiode with a high aspect ratio, after forming a groove with a high aspect ratio, a first pretreatment is first performed through a wet process, and then a second pretreatment is performed through hydrogen baking. In the process of the second pretreatment, the flow rate of hydrogen is reduced and the baking temperature is kept decreasing during the pretreatment process. This can reduce the baking capacity difference between the upper and bottom parts of the groove, thereby solving the defects of the deep groove morphology caused by hydrogen baking and improving the reliability and yield of the device product to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0025] Figure 1 is a flow chart of a method for forming a photodiode provided by an exemplary embodiment of the present application;

[0026] Figures 2 to 6 It is a schematic diagram of a photodiode formation process provided by an exemplary embodiment of the present application. DETAILED DESCRIPTION

[0027] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0028] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0029] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0030] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.

[0031] refer to Figure 1 , which shows a flow chart of a method for forming a photodiode provided by an exemplary embodiment of the present application, such as Figure 1 As shown, the method includes:

[0032] Step S1, forming a hard mask layer on a first epitaxial layer, where the first epitaxial layer is formed on a silicon substrate.

[0033] refer to Figure 2 , which shows a cross-sectional schematic diagram of forming a hard mask (HM) layer on the first epitaxial layer. Figure 2 As shown, a first epitaxial layer 220 is formed on a silicon substrate 210 , and a silicon nitride (Si 3 N 4 ) layer may be deposited on the first epitaxial layer 220 as a hard mask layer 230 by a chemical vapor deposition (CVD) process.

[0034] Step S2, forming a first trench in the hard mask layer, exposing the first epitaxial layer at the bottom of the first trench.

[0035] refer to Figure 3 , which shows a cross-sectional schematic diagram after forming a first trench in the hard mask layer. Figure 3 As shown, a photoresist ( Figure 3 ), exposing the target area (the target area is the area corresponding to the first trench 201), etching is performed to form the first trench 201 in the hard mask layer 230, exposing the first epitaxial layer 220 at the bottom of the first trench 201, and then removing the photoresist.

[0036] Step S3, etching is performed to a predetermined depth in the first epitaxial layer below the first trench, and a second trench is formed in the first epitaxial layer, wherein the ratio of the depth to the width of the second trench is greater than 4.

[0037] refer to Figure 4 , which shows a schematic top view after the second trench is formed; refer to Figure 5 , which shows the formation of the second trench trailing edge Figure 4 Schematic diagram of the cross section along the AA' direction. Figure 4 and Figure 5 As shown, etching can be performed by a dry etching process to a predetermined depth in the first epitaxial layer 220 below the first groove 201 to form a second groove 202. The second groove 202 is an irregular groove in which a columnar structure 203 (which can be a cylinder or an elliptical cylinder) is formed, that is, after the second groove 202 is etched, an array consisting of a plurality of columnar structures 203 is formed on the first epitaxial layer 220. The second groove 202 is a groove with a high aspect ratio (that is, the ratio of its depth H and width W (the width W is the spacing between the columnar structures) is greater than 4) (if the columnar structure is a cylinder, the width w is the diameter of the circular cross section of the cylinder; if the columnar structure is an ellipsoid, the width w is the major axis or minor axis of the elliptical cross section of the ellipsoid).

[0038] Step S4, performing a first pretreatment by a wet process.

[0039] The first pretreatment (also referred to as an acid wash process) is performed by a wet process to preliminarily remove impurities on the surface of the second trench 202 , the impurities including the natural oxide layer.

[0040] Step S5, performing a second pretreatment by hydrogen baking. During the second pretreatment, baking is performed by reducing the flow rate of hydrogen and keeping the baking temperature lowered during the pretreatment.

[0041] The applicant found that the main reason for the occurrence of epitaxial defects due to excessive temperature after hydrogen baking is that high-temperature baking can change the morphology of the top of the silicon column of the columnar structure (which includes a silicon column formed by the first epitaxial layer 220 and a cap structure formed by the hard mask layer 230), making the diameter of the cap structure formed by the hard mask layer larger than the diameter of the top of the silicon column, thereby causing the defects to extend downward, affecting reliability and yield.

[0042] By comparing the morphology before and after high-temperature baking, it can be found that high-temperature baking mainly has a greater impact on the silicon pillars in a very small range below the cap structure, but has basically no effect on other positions. This is mainly because the hydrogen above is more abundant and the temperature is higher than that inside the silicon pillars. In addition, due to the large changes in the surface environment of the upper and lower areas of the silicon pillars, the hydrogen baking effect of the topmost silicon pillar is much stronger, thus affecting the morphology of the top of the silicon pillar (the area from 30 nanometers (nm) to 80 nanometers below the cap structure).

[0043] In view of this, in an embodiment of the present application, in order to protect the silicon column connected to the cap structure from being damaged, the baking temperature can be set to a ramp down method (it can be set according to the actual application, and a reference numerical range is provided in the embodiment of the present application: the baking temperature decrease rate is 5 degrees Celsius per minute (℃ / min) to 20 degrees Celsius per minute), and at the same time, the hydrogen flow rate is reduced (it can be set according to the actual application, and a reference numerical range is provided in the embodiment of the present application: the hydrogen flow rate is 10 liters per minute (standard litre per minute, SLM) to 40 liters per minute) to protect the structure.

[0044] Due to the complex structure of the CIS photodiode and its high aspect ratio, the change in hydrogen flow has little effect on the hydrogen flow below the silicon column, but can effectively reduce the hydrogen flow above the silicon column, thereby reducing the difference in hydrogen baking capacity between the upper and lower regions of the silicon column. However, simply reducing the hydrogen flow is still insufficient for structural protection. Therefore, the baking temperature can be slowly reduced to further expand the process window. Since the heat diffusion at the bottom of the silicon column takes time and the surface gas flows quickly, the surface temperature is lower than the bottom temperature during the cooling process, which will cause the baking capacity difference between the surface and the bottom to be further reduced. The two solutions are combined to protect the surface morphology of the columnar structure.

[0045] Step S6, filling the second epitaxial layer in the second trench.

[0046] Exemplarily, step S6 includes but is not limited to: forming a buffer layer on the first epitaxial layer and the surface of the groove by an epitaxial process (for example, by a selective epitaxial process); forming a second epitaxial layer on the buffer layer; performing a planarization process (for example, by a chemical mechanical polishing (CMP) process) to remove the buffer layer and the second epitaxial layer outside the second trench.

[0047] refer to Figure 6 , which shows a cross-sectional schematic diagram after the second epitaxial layer is filled in the second trench. Figure 6 As shown, a buffer layer 241 is formed on the surface of the second trench 202 , and the buffer layer 241 covers the second epitaxial layer 242 .

[0048] To summarize, in the embodiments of the present application, in the process of forming a photodiode with a high aspect ratio, after forming a groove with a high aspect ratio, a first pretreatment is first performed through a wet process, and then a second pretreatment is performed through hydrogen baking. In the process of the second pretreatment, the flow rate of hydrogen is reduced and the baking temperature is kept decreasing during the pretreatment process. This can reduce the baking ability difference between the top and bottom of the groove, thereby solving the defects of the deep groove morphology caused by hydrogen baking and improving the reliability and yield of the device product to a certain extent.

[0049] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.

Claims

1. A method for forming a photodiode, It is characterized in that include: forming a hard mask layer on a first epitaxial layer, wherein the first epitaxial layer is formed on a silicon substrate; forming a first trench in the hard mask layer, wherein the first epitaxial layer at the bottom of the first trench is exposed; Performing etching to a predetermined depth in the first epitaxial layer below the first trench to form a second trench in the first epitaxial layer, wherein a ratio of the depth to the width of the second trench is greater than 4; Performing a first pretreatment by a wet process; Performing a second pretreatment by hydrogen baking, during which the baking is performed by reducing the flow rate of hydrogen and keeping the baking temperature lowered during the pretreatment; A second epitaxial layer is filled in the second trench.

2. The method according to claim 1, It is characterized in that After the second trench is formed by etching, a columnar structure is formed in the second trench.

3. The method according to claim 2, It is characterized in that During the second pretreatment, the baking temperature decreases at a rate of 5 degrees Celsius per minute to 20 degrees Celsius per minute.

4. The method according to claim 3, It is characterized in that During the second pretreatment, the flow rate of hydrogen is 10 liters per minute to 40 liters per minute.

5. The method according to any one of claims 1 to 4, It is characterized in that The filling of the second epitaxial layer in the second trench comprises: forming a buffer layer on the first epitaxial layer and the surface of the trench by an epitaxial process; forming a second epitaxial layer on the buffer layer; A planarization process is performed to remove the buffer layer and the second epitaxial layer outside the second trench.

6. The method according to claim 5, It is characterized in that The hard mask layer includes a silicon nitride layer.

7. The method according to claim 6, It is characterized in that The forming of a buffer layer on the first epitaxial layer and the surface of the trench by an epitaxial process comprises: The buffer layer is formed on the first epitaxial layer and the surface of the trench by a selective epitaxial process.