Light-emitting chip and display panel

By introducing diffusion layers and transition layers with different bandgap widths into the light-emitting chip, the hole propagation angle is increased, which solves the problem of low luminous efficiency caused by uneven current density distribution and achieves more efficient light emission.

CN118969923AActive Publication Date: 2024-11-15CHONGQING KONKA PHOTOELECTRIC TECH RES INST CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310490934.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-15
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

In the existing technology, due to the uneven distribution of current density, some electrons cross the light-emitting layer and enter the second semiconductor layer to interact with holes, which affects the hole transport from the second semiconductor layer to the light-emitting layer and reduces the luminous efficiency of the light-emitting chip.

Method used

A first diffusion layer and a second diffusion layer are introduced into the light-emitting chip. The band gap of the first diffusion layer is greater than the band gap of the second semiconductor layer, and the band gap of the second diffusion layer is greater than or equal to the band gap of the first diffusion layer. By setting a transition layer and an intermediate layer, the hole propagation angle is increased, so that the holes enter the light-emitting layer more uniformly and the recombination rate of electrons and holes is improved.

Benefits of technology

By increasing the hole propagation angle and uniformity, the recombination rate of electrons and holes in the light-emitting layer is improved, thereby enhancing the luminous efficiency of the light-emitting chip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969923A_ABST
    Figure CN118969923A_ABST
Patent Text Reader

Abstract

The invention relates to a light-emitting chip and a display panel. The light-emitting chip comprises a substrate, a first semiconductor layer, a light-emitting layer and a second semiconductor layer, the first semiconductor layer, the light-emitting layer and the second semiconductor layer are stacked on the substrate, the light-emitting layer is located between the first semiconductor layer and the second semiconductor layer, and after being excited, the first semiconductor layer and the second semiconductor layer transmit electrons and holes to the light-emitting layer so as to emit light in a composite mode; a first diffusion layer and a second diffusion layer are further arranged between the light-emitting layer and the second semiconductor layer, the first diffusion layer is located between the second semiconductor layer and the second diffusion layer, and the forbidden bandwidth of the first diffusion layer is larger than that of the second semiconductor layer and smaller than or equal to that of the second diffusion layer. The first diffusion layer and the second diffusion layer are used for increasing the transmission angle of holes so that the holes can enter the light-emitting layer more uniformly. According to the light-emitting chip, the forbidden bandwidth of the first diffusion layer and the forbidden bandwidth of the second diffusion layer are set, so that the transmission angle of holes is increased, the holes can enter the holes of the light-emitting layer more uniformly, and the light-emitting efficiency of the light-emitting chip is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display technology, and in particular to a light-emitting chip and a display panel including the light-emitting chip. Background Art

[0002] In the field of display technology, a light-emitting chip generally includes a substrate, a first semiconductor layer, a light-emitting layer, and a second semiconductor layer stacked in sequence. The first semiconductor layer and the second semiconductor layer are excited by an external current to transfer electrons and holes toward the light-emitting layer, respectively, so that the electrons and holes can recombine in the light-emitting layer and emit light outward.

[0003] However, in the prior art, due to the uneven distribution of current density, some electrons may pass through the light-emitting layer and enter the second semiconductor layer to interact with holes, thereby reducing the transmission angle of holes in the second semiconductor layer and affecting the hole transmission from the second semiconductor layer to the light-emitting layer, making the recombination rate of holes and electrons in the light-emitting layer relatively low, thereby reducing the luminous efficiency of the light-emitting chip. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a light-emitting chip with improved light-emitting efficiency, and a display panel including the light-emitting chip, which specifically includes the following technical solutions:

[0005] In a first aspect, an embodiment of the present application provides a light-emitting chip, including a substrate, and a first semiconductor layer, a light-emitting layer, and a second semiconductor layer stacked on the substrate, wherein the light-emitting layer is located between the first semiconductor layer and the second semiconductor layer, and after being excited, the first semiconductor layer and the second semiconductor layer respectively transmit electrons and holes toward the light-emitting layer to recombine and emit light;

[0006] A first diffusion layer and a second diffusion layer are also provided between the light-emitting layer and the second semiconductor layer. The first diffusion layer is located between the second semiconductor layer and the second diffusion layer. The bandgap width of the first diffusion layer is greater than the bandgap width of the second semiconductor layer and is less than or equal to the bandgap width of the second diffusion layer. The first diffusion layer and the second diffusion layer are used to increase the transmission angle of holes so that the holes can enter the light-emitting layer more evenly.

[0007] The light-emitting chip of the present application is formed by stacking a first semiconductor layer, a light-emitting layer, and a second semiconductor layer on the surface of a substrate, so that the first semiconductor layer can be excited under the action of an external current and transmit electrons toward the light-emitting layer, and the second semiconductor layer can be excited under the action of an external current and transmit holes toward the light-emitting layer. The electrons of the first semiconductor layer and the holes of the second semiconductor layer can recombine in the light-emitting layer and emit light outward, thereby realizing the display function of the light-emitting chip of the present application.

[0008] The light-emitting chip of the present application also arranges a first diffusion layer and a second diffusion layer between the light-emitting layer and the second semiconductor layer so that the first diffusion layer and the second diffusion layer, both of which have a bandgap width greater than the bandgap width of the second semiconductor layer, can cooperate with each other to increase the transmission angle of holes transmitted from the second semiconductor layer to the light-emitting layer, thereby allowing holes to enter the light-emitting layer more evenly, increasing the recombination rate of holes and electrons in the light-emitting layer, and thereby improving the luminous efficiency of the light-emitting chip of the present application.

[0009] In one embodiment, the first diffusion layer is a P-type semiconductor, wherein the first diffusion layer contains one or more of aluminum, gallium and indium elements; and / or the second diffusion layer is a P-type semiconductor, wherein the second diffusion layer contains one or more of aluminum, gallium and indium elements.

[0010] In this embodiment, based on the fact that the content of electrons in the light-emitting layer is greater than the content of holes, the first diffusion layer and / or the second diffusion layer is set to a P-type semiconductor to cooperate with the second semiconductor layer, thereby increasing the content of holes entering the light-emitting layer and improving the recombination rate of electrons and holes in the light-emitting layer, thereby further improving the luminous efficiency of the light-emitting chip of the present application.

[0011] In one embodiment, the light emitting chip further includes a transition layer, which is disposed between the first diffusion layer and the second diffusion layer, and the bandgap width of the transition layer is smaller than the bandgap width of the first diffusion layer and smaller than the bandgap width of the second diffusion layer.

[0012] In this embodiment, a transition layer having a bandgap width smaller than the bandgap widths of the first diffusion layer and the second diffusion layer is provided so that the holes transported by the second semiconductor layer can be stored in a potential well structure formed by the first diffusion layer, the second diffusion layer and the transition layer, thereby improving the hole distribution between the second semiconductor layer and the light-emitting layer, and further increasing the hole transmission angle, so that the holes in the second semiconductor layer can enter the light-emitting layer more evenly.

[0013] In one embodiment, the thickness of the first diffusion layer is between 5 nm and 40 nm; and / or the thickness of the second diffusion layer is between 5 nm and 40 nm; and / or the thickness of the transition layer is between 5 nm and 40 nm.

[0014] In one embodiment, the light-emitting chip also includes an intermediate layer, which is arranged between the first diffusion layer and the second diffusion layer. The doping source of the first diffusion layer and the doping source of the second diffusion layer both include magnesium elements. The intermediate layer is used to receive the magnesium elements diffused from the first diffusion layer and the second diffusion layer to the intermediate layer to reduce the growth crystal defects on the first diffusion layer and the second diffusion layer.

[0015] In this embodiment, an intermediate layer is provided between the first diffusion layer and the second diffusion layer so that the magnesium element from the first diffusion layer and the second diffusion layer can diffuse into the intermediate layer, and an doped extension region showing a gradient change in the magnesium element doping concentration can be formed between the intermediate layer and the first diffusion layer, and between the intermediate layer and the second diffusion layer, thereby reducing the growth crystal defects on the first diffusion layer and the second diffusion layer.

[0016] In one embodiment, the intermediate layer is arranged between the first diffusion layer and the transition layer, and the intermediate layer is used to receive the magnesium element diffused from the first diffusion layer and the transition layer to the intermediate layer, so as to reduce the growth crystal defects on the first diffusion layer and the transition layer; and / or the intermediate layer is arranged between the second diffusion layer and the transition layer, and the intermediate layer is used to receive the magnesium element diffused from the second diffusion layer and the transition layer to the intermediate layer, so as to reduce the growth crystal defects on the second diffusion layer and the transition layer.

[0017] In this embodiment, an intermediate layer is provided between the first diffusion layer and the transition layer so that the magnesium element from the first diffusion layer and the transition layer can diffuse into the intermediate layer, and an extended doping region showing a gradient change in the magnesium element doping concentration can be formed between the intermediate layer and the first diffusion layer, and between the intermediate layer and the transition layer, thereby reducing the growth crystal defects on the first diffusion layer and the transition layer.

[0018] And / or by arranging an intermediate layer between the second diffusion layer and the transition layer, so that the magnesium element from the second diffusion layer and the transition layer can diffuse into the intermediate layer, and can form a doped extension region with a gradient change in the magnesium element doping concentration between the intermediate layer and the second diffusion layer, and between the intermediate layer and the transition layer, thereby reducing the growth crystal defects on the second diffusion layer and the transition layer.

[0019] In one embodiment, the thickness of the intermediate layer is between 2 nm and 10 nm.

[0020] In this embodiment, the thickness of the intermediate layer is limited to between 2nm and 10nm to avoid affecting the diffusion quality of the magnesium element due to the intermediate layer being too thin, and to avoid affecting the transmission efficiency of holes from the second semiconductor layer to the light-emitting layer due to the intermediate layer being too thick.

[0021] In one embodiment, the distance between the second semiconductor layer and the light emitting layer is between 12 nm and 300 nm.

[0022] In this embodiment, the distance between the second semiconductor layer and the light-emitting layer is limited to between 12nm and 300nm to avoid affecting the transmission efficiency of holes in the second semiconductor layer to the light-emitting layer due to too large a distance, and to avoid affecting the distribution of holes by allowing electrons with higher mobility to pass through the light-emitting layer into the second semiconductor layer due to too small a distance.

[0023] In one embodiment, the doping concentration of the first diffusion layer and the doping concentration of the second diffusion layer are both greater than or equal to 1E18 atoms / cm 3 .

[0024] In this embodiment, the doping concentration of the first diffusion layer and the second diffusion layer is set to be greater than or equal to 1E18 atoms / cm 3 , so that the hole content in the first diffusion layer and the second diffusion layer is relatively large, so as to increase the hole content entering the light-emitting layer.

[0025] In one embodiment, the light emitting chip further includes a buffer layer, the buffer layer is located between the first semiconductor layer and the light emitting layer, and the buffer layer is used to release stress between the first semiconductor layer and the light emitting layer.

[0026] In this embodiment, a buffer layer is provided between the first semiconductor layer and the light emitting layer to release stress between the first semiconductor layer and the light emitting layer, thereby reducing lattice mismatch between the first semiconductor layer and the light emitting layer.

[0027] In a second aspect, an embodiment of the present application provides a display panel, including a driving backplane and a light-emitting chip, wherein the light-emitting chip is mounted on the driving backplane, and the driving backplane is used to control the light-emitting chip to emit light.

[0028] In this embodiment, the light emitting chip is mounted on a driving backplane so that the driving backplane can control the electrical signal to enter the light emitting chip to drive the light emitting chip to emit light, thereby realizing the display function of the display panel of the present application.

[0029] It can be understood that since the display panel provided in the second aspect of the present application adopts the light-emitting chip provided in the first aspect of the present application, it also has the beneficial effect of improving the light-emitting efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram of the structure of a display panel provided in one embodiment of the present application;

[0031] Figure 2 This is a schematic diagram of the structure of a light-emitting chip provided in one embodiment of the present application;

[0032] Figure 3 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0033] Figure 4 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0034] Figure 5 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0035] Figure 6 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0036] Figure 7 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0037] Figure 8 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0038] Fig. 9 Another structural schematic diagram of a light-emitting chip provided in one embodiment of the present application;

[0039] Fig.10 It is a schematic diagram of the structure of a light-emitting chip in the prior art.

[0040] The figure markings are: 200-display panel; 201-driving backplane; 100-light-emitting chip; 10-substrate; 20-first semiconductor layer; 30-light-emitting layer; 40-second semiconductor layer; S-spacing; 51-first diffusion layer; D1-first thickness; 52-second diffusion layer; D2-second thickness; 53-transition layer; D3-third thickness; 54-middle layer; D4-fourth thickness; 60-buffer layer; 100'-light-emitting chip; 10'-substrate; 20'-first semiconductor layer; 30'-light-emitting layer; 40'-second semiconductor layer. DETAILED DESCRIPTION

[0041] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly and comprehensively understood.

[0042] The following descriptions of the embodiments are with reference to the attached diagrams to illustrate specific embodiments that the present application can be used to implement. The serial numbers for the components herein, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in the present application, unless otherwise specified, include direct and indirect connections (couplings). The directional terms mentioned in the present application, such as "upper", "lower", "front", "back", "left", "right", "inside", "outside", "side", etc., are only with reference to the directions of the attached drawings. Therefore, the directional terms used are for better and clearer explanation and understanding of the present application, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation to the present application.

[0043] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be fixedly connected, detachably connected, or integrally connected; it can be mechanically connected; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances. It should be noted that the terms "first", "second", etc. in the specification, claims, and drawings of this application are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "include", "may include", "include", or "may include" used in this application indicate the existence of the corresponding functions, operations, elements, etc. disclosed, and do not limit one or more other functions, operations, elements, etc. In addition, the terms "include" or "include" indicate the existence of the corresponding features, numbers, steps, operations, elements, components, or combinations thereof disclosed in the specification, and do not exclude the existence or addition of one or more other features, numbers, steps, operations, elements, components, or combinations thereof, and are intended to cover non-exclusive inclusions.

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0045] See also Figure 1 FIG. 2 is a schematic diagram of the structure of a display panel 200 provided in one embodiment of the present application.

[0046] like Figure 1 As shown, the display panel 200 provided in the present application includes a driving backplane 201 and a light-emitting chip 100. There are multiple light-emitting chips 100, and each light-emitting chip 100 is mounted on the same surface of the driving backplane 201. The driving backplane 201 is also provided with a control chip (not shown in the figure) and multiple control circuits (not shown in the figure). The control chip is connected to each light-emitting chip 100 through each control circuit, so that the control chip can provide a control signal to each light-emitting chip 100 through the control circuit. Each light-emitting chip 100 emits light outward under the action of the control signal, thereby realizing the display function of the display panel 200 of the present application.

[0047] like Figure 1 As shown, a plurality of light emitting chips 100 are arrayed on the driving backplane 201. In other embodiments, the arrangement of the light emitting chips 100 may also be other arrangements, and the applicant does not make any special limitation thereto.

[0048] On the other hand, in order to clearly show the structure of the display panel 200, Figure 1 The light-emitting chip 100 and the driving backplane 201 are only introduced as examples, and do not represent the actual structure and shape of the display panel 200. That is, in other embodiments of the display panel 200 of the present application, the shape and area of ​​the driving backplane 201 can be adjusted according to the actual scene. At the same time, the shape, area and arrangement of each light-emitting chip 100 can also be adjusted accordingly. In the actual display panel 200 product, the area of ​​each light-emitting chip 100 is usually small, and the arrangement density is usually large.

[0049] See also Figure 2 The structure diagram of the light-emitting chip 100 provided in one embodiment of the present application is shown.

[0050] like Figure 2 As shown, the light-emitting chip 100 provided in the present application includes a substrate 10, a first semiconductor layer 20, a light-emitting layer 30 and a second semiconductor layer 40. Among them, the first semiconductor layer 20, the light-emitting layer 30 and the second semiconductor layer 40 are sequentially stacked on the surface of the substrate 10. It can be understood that the first semiconductor layer 20 is an N-type semiconductor, which is used to provide electrons for the light-emitting chip 100, and the second semiconductor layer 40 is a P-type semiconductor, which is used to provide holes for the light-emitting chip 100. When an electrical signal flows into the light-emitting chip 100 and makes the light-emitting chip 100 forwardly conductive, the current acting on the first semiconductor layer 20 will excite the electrons in the first semiconductor layer 20 to move toward the second semiconductor layer 40. Correspondingly, the current acting on the second semiconductor layer 40 will excite the holes in the second semiconductor layer 40 to move toward the first semiconductor layer 20. At the same time, when the above-mentioned holes and electrons meet and recombine, they will radiate light outward, thereby achieving the purpose of emitting light.

[0051] Meanwhile, the light emitting layer 30 is located between the first semiconductor layer 20 and the second semiconductor layer 40, and the light emitting layer 30 is used to carry electrons emitted from the first semiconductor layer 20 and holes emitted from the second semiconductor layer 40. It can be understood that the light emitted by the light emitting chip 100 of the present application is emitted from the light emitting layer 30. On the other hand, the light emitting layer 30 increases the recombination rate of electrons and holes, and improves the composite luminescence efficiency of the light emitting chip 100.

[0052] The light emitting chip 100 provided in the present application further includes a first diffusion layer 51 and a second diffusion layer 52, both of which are disposed between the light emitting layer 30 and the second semiconductor layer 40, and the first diffusion layer 51 is located between the second semiconductor layer 40 and the second diffusion layer 52. The bandgap width of the first diffusion layer 51 is greater than the bandgap width of the second semiconductor layer 40, and is less than or equal to the bandgap width of the second diffusion layer 52.

[0053] Since the electron content in the first semiconductor layer 20 is relatively greater than the hole content in the second semiconductor layer 40, when the light-emitting chip 100 is forward-conducted, electrons with relatively high mobility may exist in the first semiconductor layer 20 and pass through the light-emitting layer 30 to enter the second semiconductor layer 40. It can be understood that the bandgap width of the first diffusion layer 51 is greater than the bandgap width of the second semiconductor layer 40, and the bandgap width of the second diffusion layer 52 is also greater than the bandgap width of the second semiconductor layer 40, so that electrons with high mobility cannot pass through the second diffusion layer 52 and the first diffusion layer 51 to enter the second semiconductor layer 40, thereby avoiding the influence of electrons with high mobility on holes in the second semiconductor layer 40.

[0054] At the same time, since the bandgap width of the second diffusion layer 52 is greater than the bandgap width of the second semiconductor layer 40, the holes in the second semiconductor layer 40 may be blocked from entering the light-emitting layer 30. It can be understood that the provision of the first diffusion layer 51 can reduce the difference in the bandgap width between the second diffusion layer 52 and the second semiconductor layer 40, so that the holes in the second semiconductor layer 40 can enter the light-emitting layer 30.

[0055] Therefore, the mutual matching of the first diffusion layer 51 and the second diffusion layer 52 can block the electrons in the first semiconductor layer 20 from entering the second semiconductor layer 40 , thereby ensuring the hole content in the second semiconductor layer 40 .

[0056] At the same time, the setting of the bandgap width of the first diffusion layer 51 and the second diffusion layer 52 enables the holes in the second semiconductor layer 40 to pass through the first diffusion layer 51 and the second diffusion layer 52 to enter the light-emitting layer 30. And the transmission angle of the holes in the second semiconductor layer 40 is increased, so that the holes in the second semiconductor layer 40 can enter the light-emitting layer 30 more uniformly, so that the recombination rate of electrons and holes in the light-emitting layer 30 is increased. Then the luminous efficiency of the light-emitting chip 100 of the present application is improved.

[0057] In one embodiment, the first diffusion layer 51 is a P-type semiconductor layer. Based on the fact that the majority carriers in the P-type semiconductor layer are holes, it is understandable that setting the first diffusion layer 51 as a P-type semiconductor layer is conducive to cooperating with the second semiconductor layer 40 to increase the hole content entering the light-emitting layer 30, thereby improving the recombination rate of electrons and holes in the light-emitting layer 30. The luminous efficiency of the light-emitting chip 100 of the present application is further improved.

[0058] The first diffusion layer 51 contains one or more of aluminum, gallium, and indium. x Ga (1-x-y) In x N. Wherein, x is greater than or equal to 0 and less than or equal to 1; y is greater than or equal to 0 and less than or equal to 1.

[0059] The second diffusion layer 52 is a P-type semiconductor layer to cooperate with the first diffusion layer 51 and the second semiconductor layer 40 to further increase the hole content in the light-emitting chip 100 of the present application and improve the recombination rate of electrons and holes in the light-emitting layer 30 .

[0060] The second diffusion layer 52 contains one or more of aluminum, gallium, and indium. x Ga (1-x-y) In x N. Wherein, x is greater than or equal to 0 and less than or equal to 1; y is greater than or equal to 0 and less than or equal to 1.

[0061] In this embodiment, the materials of the first diffusion layer 51 and the second diffusion layer 52 may be different, so that the bandgap width of the first diffusion layer 51 is smaller than the bandgap width of the second diffusion layer 52 .

[0062] It is understandable that the composition size of each element of the first diffusion layer 51 and the second diffusion layer 52 can be adjusted by the growth conditions. For example, when the first diffusion layer 51 and the second diffusion layer 52 are generated, one or more of the growth temperature, growth rate, growth pressure and growth atmosphere in the growth conditions can be changed. And the growth temperature is between 700°C and 1100°C, and the growth rate is between The growth pressure is between 50mbar-600mbar, and the ratio of nitrogen to hydrogen in the growth atmosphere is between 0%-100%.

[0063] In another embodiment, only the first diffusion layer 51 may be set as a P-type semiconductor layer. In another embodiment, only the second diffusion layer 52 may be set as a P-type semiconductor layer.

[0064] See also Figure 3 Another structural schematic diagram of a light-emitting chip 100 provided in an embodiment of the present application is shown.

[0065] like Figure 3 As shown, the light emitting chip 100 of the present application further includes a transition layer 53 , which is located between the first diffusion layer 51 and the second diffusion layer 52 . The bandgap width of the transition layer 53 is smaller than the bandgap width of the first diffusion layer 51 and smaller than the bandgap width of the second diffusion layer 52 .

[0066] The setting of the bandgap width of the transition layer 53 enables the transition layer 53 to cooperate with the first diffusion layer 51 and the second diffusion layer 52 to form a potential well structure. It can be understood that the holes in the second semiconductor layer 40 can be stored in the potential well structure when being transported to the light-emitting layer 30. Therefore, before the holes enter the light-emitting layer 30, they can be stored in the potential well structure formed by the transition layer 53, thereby increasing the hole distribution range between the second semiconductor layer 40 and the light-emitting layer 30.

[0067] At the same time, when the light-emitting chip 100 is forward-conducting, the holes stored in the potential well structure can also be transmitted toward the light-emitting layer 30 , thereby increasing the transmission angle of the holes, so that the holes transmitted by the second semiconductor layer 40 can enter the light-emitting layer 30 more uniformly.

[0068] In another embodiment, the transition layer 53 may also be disposed between the first diffusion layer 51 and the second semiconductor layer 40. In another embodiment, the transition layer 53 may also be disposed between the second diffusion layer 52 and the light emitting layer 30.

[0069] See also Figure 4 Another structural schematic diagram of a light-emitting chip 100 provided in an embodiment of the present application is shown.

[0070] like Figure 4 As shown, the light emitting chip 100 of the present application further includes an intermediate layer 54, which is disposed between the first diffusion layer 51 and the second diffusion layer 52. The doping source of the first diffusion layer 51 and the doping source of the second diffusion layer 52 include magnesium, while the intermediate layer 54 does not contain magnesium. Due to the memory diffusion effect of magnesium, it can be understood that the magnesium in the first diffusion layer 51 can diffuse into the intermediate layer 54, and a doping extension region with a gradient doping concentration of magnesium can be formed between the first diffusion layer 51 and the intermediate layer 54, thereby reducing the growth crystal defects on the first diffusion layer 51.

[0071] At the same time, the magnesium element in the second diffusion layer 52 can also diffuse into the intermediate layer 54 , and a doped extension region with a gradient magnesium doping concentration can be formed between the second diffusion layer 52 and the intermediate layer 54 , thereby reducing growth crystal defects on the second diffusion layer 52 .

[0072] It can be understood that the provision of the intermediate layer 54 can reduce the growth crystal defects on the first diffusion layer 51 and the second diffusion layer 52, and may even eliminate the growth crystal defects on the first diffusion layer 51 and the second diffusion layer 52, thereby improving the transmission efficiency of holes entering the light-emitting layer 30 through the first diffusion layer 51, the second diffusion layer 52 and the intermediate layer 54, and improving the antistatic performance of the light-emitting chip 100 of the present application.

[0073] On the other hand, the magnesium element in the doping source of the first diffusion layer 51 and the doping source of the second diffusion layer 52 can also improve the electrical properties of the first diffusion layer 51 and the second diffusion layer 52 .

[0074] In this embodiment, the material of the middle layer 54 can be set to GaN. In another embodiment, the material of the middle layer 54 can also be set to Al x Ga (1-x-y) In x N. Wherein, x is greater than or equal to 0 and less than or equal to 1; y is greater than or equal to 0 and less than or equal to 1. It can be understood that during the growth of the intermediate layer 54, the growth conditions of the intermediate layer 54 are between the growth conditions of the first diffusion layer 51 and the growth conditions of the second diffusion layer 52, so that the composition of each element of the intermediate layer 54 is inconsistent with the composition of each element of the first diffusion layer 51 and the second diffusion layer 52.

[0075] See also Figure 5 Another structural schematic diagram of a light-emitting chip 100 provided in an embodiment of the present application is shown.

[0076] like Figure 5 As shown, the intermediate layer 54 is disposed between the first diffusion layer 51 and the transition layer 53. The doping source of the first diffusion layer 51 and the doping source of the transition layer 53 include magnesium, while the intermediate layer 54 does not contain magnesium. Due to the memory diffusion effect of magnesium, it can be understood that the magnesium in the first diffusion layer 51 can diffuse into the intermediate layer 54, and a doping extension region with a gradient doping concentration of magnesium can be formed between the first diffusion layer 51 and the intermediate layer 54, thereby reducing the growth crystal defects on the first diffusion layer 51.

[0077] On the other hand, Figure 5 As shown, the intermediate layer 54 is also disposed between the second diffusion layer 52 and the transition layer 53. The doping source of the second diffusion layer 52 and the doping source of the transition layer 53 include magnesium, while the intermediate layer 54 does not contain magnesium. It can be understood that the magnesium in the second diffusion layer 52 can diffuse into the intermediate layer 54, and a doped extension region with a gradient doping concentration of magnesium can be formed between the second diffusion layer 52 and the intermediate layer 54, thereby reducing the growth crystal defects on the second diffusion layer 52.

[0078] At the same time, the magnesium element in the transition layer 53 can also diffuse into the middle layer 54 , and a doped extension region with a gradient magnesium doping concentration can be formed between the transition layer 53 and the middle layer 54 , thereby reducing growth crystal defects on the transition layer 53 .

[0079] It can be understood that the provision of the intermediate layer 54 can reduce the growth crystal defects on the first diffusion layer 51, the second diffusion layer 52 and the transition layer 53, and may even eliminate the growth crystal defects on the first diffusion layer 51, the second diffusion layer 52 and the transition layer 53, thereby improving the transmission efficiency of the holes entering the light-emitting layer 30 through the first diffusion layer 51, the second diffusion layer 52, the transition layer 53 and the intermediate layer 54, and improving the antistatic performance of the light-emitting chip 100 of the present application.

[0080] On the other hand, the magnesium element in the doping source of the first diffusion layer 51 , the doping source of the second diffusion layer 52 and the doping source of the transition layer 53 can be used to improve the electrical properties of the first diffusion layer 51 , the second diffusion layer 52 and the transition layer 53 .

[0081] In another embodiment, if Figure 6 As shown, the intermediate layer 54 may also be disposed between the first diffusion layer 51 and the second semiconductor layer 40 to reduce or eliminate growth crystal defects on the first diffusion layer 51 and the second semiconductor layer 40. In another embodiment, as shown in FIG. Figure 7 As shown, the intermediate layer 54 may also be disposed between the second diffusion layer 52 and the light emitting layer 30 to reduce or eliminate growth crystal defects between the second diffusion layer 52 and the light emitting layer 30. In another embodiment, as shown in FIG. Figure 8 As shown, the intermediate layer 54 may also be disposed between the first diffusion layer 51 and the second semiconductor layer 40 , and between the second diffusion layer 52 and the light emitting layer 30 , respectively.

[0082] In one embodiment, please refer to Figure 5 , a fourth thickness D4 of the intermediate layer 54 is between 2 nm and 10 nm.

[0083] The doping concentration of the magnesium element based on the first diffusion layer 51, the second diffusion layer 52 and the transition layer 53 is relatively high. It can be understood that when the fourth thickness D4 is less than 2nm, the quality of the magnesium element in forming the doped extension region with the doping concentration gradient in the intermediate layer 54 is relatively poor, which may result in a small difference between the magnesium doping concentration of the intermediate layer 54 and the magnesium doping concentration of the adjacent structure. As a result, the diffusion quality of the magnesium element is relatively poor, and it is difficult to ensure the reduction of the growth crystal defects of the first diffusion layer 51, the second diffusion layer 52 and the transition layer 53.

[0084] The middle layer 54 may be undoped gallium nitride. It is understandable that when the fourth thickness D4 is greater than 10 nm, the resistance of the middle layer 54 is relatively large, thereby reducing the efficiency of hole transmission from the second semiconductor layer 40 to the light emitting layer 30.

[0085] Therefore, setting an intermediate layer 54 between 2nm and 10nm can ensure that the intermediate layer 54 reduces the growth crystal defects of the adjacent first diffusion layer 51, the second diffusion layer 52 and the transition layer 53, while also ensuring the hole transport efficiency of the second semiconductor layer 40 to the light-emitting layer 30.

[0086] In one embodiment, please refer to Figure 5 , the spacing S between the second semiconductor layer 40 and the light emitting layer 30 is between 12nm-300nm. It can be understood that when the spacing S between the second semiconductor layer 40 and the light emitting layer 30 is greater than 300nm, the holes in the second semiconductor layer 40 will be difficult to be transmitted to the light emitting layer 30 due to the excessive spacing S, thereby reducing the hole transmission efficiency of the second semiconductor layer 40.

[0087] When the spacing S between the second semiconductor layer 40 and the light-emitting layer 30 is less than 12 nm, the blocking ability of the first diffusion layer 51 and the second diffusion layer 52 located between the second semiconductor layer 40 and the light-emitting layer 30 to electrons decreases, so that electrons with higher mobility in the first semiconductor layer 20 can enter the second semiconductor layer 40 to affect the distribution of holes.

[0088] Therefore, setting the interval S between 12 nm and 300 nm can ensure the blocking effect of the first diffusion layer 51 and the second diffusion layer 52 on electrons with high mobility while also ensuring the transmission efficiency of holes in the second semiconductor layer 40 .

[0089] In one embodiment, if Figure 5 As shown, the first thickness D1 of the first diffusion layer 51 is between 5 nm and 40 nm.

[0090] In one embodiment, if Figure 5 As shown, the second thickness D2 of the second diffusion layer 52 is between 5 nm and 40 nm.

[0091] In one embodiment, if Figure 5 As shown, the third thickness D3 of the transition layer 53 is between 5 nm and 40 nm.

[0092] In one embodiment, the doping concentration of the first diffusion layer 51 and the doping concentration of the second diffusion layer 52 are both greater than or equal to 1E18 atoms / cm 3 The doping concentration of the structure can affect the hole content in the structure. It is understandable that the setting is greater than or equal to 1E18atoms / cm 3 The doping concentration of 51 and 52 ensures the hole content in the first diffusion layer 51 and the second diffusion layer 52. The first diffusion layer 51 and the second diffusion layer 52 further ensure the improvement effect of the hole content of the light emitting chip 100 of the present application.

[0093] In one embodiment, the doping concentration of the transition layer 53 is also greater than or equal to 1E18 atoms / cm 3 The doping concentration of the structure can affect the hole content in the structure. It is understandable that the setting is greater than or equal to 1E18atoms / cm 3 The doping concentration of the transition layer 53 ensures the hole content in the transition layer 53. This further ensures the effect of the transition layer 53 on improving the hole content of the light-emitting chip 100 of the present application. Fig. 9 Another structural schematic diagram of a light-emitting chip 100 provided in an embodiment of the present application is shown.

[0094] like Fig. 9 As shown, the transition layer 53 can be provided in multiple numbers, and an intermediate layer 54 is provided between each two adjacent transition layers 53. The bandgap width of the intermediate layer 54 is smaller than the bandgap width of the two adjacent transition layers 53. It can be understood that the matching arrangement of the multiple transition layers 53 and the intermediate layer 54 enables alternately distributed potential barriers and potential wells to be formed between the first diffusion layer 51 and the second diffusion layer 52, thereby expanding the storage range of the holes in the second semiconductor layer 40, further increasing the transmission angle of the holes, so that the holes in the second semiconductor layer 40 can be more evenly transmitted to the light-emitting layer 30.

[0095] In this embodiment, when preparing a plurality of transition layers 53, the growth conditions of any two adjacent transition layers 53 may be different, and the intermediate layer 54 may serve as a transition between the growth conditions of the two adjacent transition layers 53. In another embodiment, the growth conditions of the two adjacent transition layers 53 may also be the same, and the bandgap width of the intermediate layer 54 is smaller than the bandgap width of the two adjacent transition layers 53.

[0096] See also Fig.10 The structure diagram of the light emitting chip 100' in the prior art is shown.

[0097] like Fig.10 As shown, in the prior art, the light emitting chip 100' comprises a substrate 10', a first semiconductor layer 20', a light emitting layer 30' and a second semiconductor layer 40' which are stacked in sequence, wherein the first semiconductor layer 20' is an N-type semiconductor for providing electrons for the light emitting chip 100', and the second semiconductor layer 40' is a P-type semiconductor for providing holes for the light emitting chip 100'. When an electrical signal flows into the light emitting chip 100' and makes the light emitting chip 100' forwardly conductive, the electrons in the first semiconductor layer 20' and the holes in the second semiconductor layer 40' will be transmitted toward the light emitting layer 30', and emit light outward after being recombined in the light emitting layer 30', thereby realizing the display function of the light emitting chip 100'.

[0098] In the prior art, the density of the current applied to the first semiconductor layer 20' and the second semiconductor layer 40' is unevenly distributed. It is understandable that some electrons in the first semiconductor layer 20' will have a higher mobility under the action of the current. Among them, the electrons with higher mobility may pass through the light-emitting layer 30' and enter the second semiconductor layer 40', and interact with the holes in the second semiconductor layer 40'.

[0099] Since the content of electrons in the light-emitting chip 100' is greater than the content of holes, when the electrons with higher mobility interact with the holes, the hole content in the second semiconductor layer 40' will be reduced, and the transmission angle of the second semiconductor layer 40' will be reduced. This will affect the distribution of holes in the second semiconductor layer 40' in the light-emitting layer 30', reduce the recombination rate of electrons and holes in the light-emitting layer 30', and make the light-emitting efficiency of the light-emitting chip 100' relatively low.

[0100] Therefore, based on the larger bandgap width of the first diffusion layer 51 and the second diffusion layer 52, the light-emitting chip 100 of the present application increases the transmission angle of holes transmitted from the second semiconductor layer 40 to the light-emitting layer 30 by providing the first diffusion layer 51 and the second diffusion layer 52, so that the holes in the second semiconductor layer 40 can enter the light-emitting layer 30 more uniformly, thereby improving the luminous efficiency of the light-emitting chip 100 of the present application.

[0101] In one embodiment, please refer to Fig. 9 The light emitting chip 100 of the present application further includes a buffer layer 60, which is disposed between the first semiconductor layer 20 and the light emitting layer 30 to serve as a growth buffer between the first semiconductor layer 20 and the light emitting layer 30. Thus, the stress between the first semiconductor layer 20 and the light emitting layer 30 is released, and the lattice mismatch between the first semiconductor layer 20 and the light emitting layer 30 is reduced.

[0102] It should be understood that the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more features. In the description of the embodiments of the present application, "plurality" means two or more, unless otherwise clearly and specifically defined.

[0103] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiments or examples are included in at least one embodiment or example of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0104] It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in the field, improvements or changes can be made according to the above description, and all these improvements and changes should fall within the scope of protection of the claims attached to this application. Ordinary technicians in the field can understand that all or part of the processes of the above embodiments are implemented, and equivalent changes made according to the claims of the present invention still fall within the scope of the present invention.

Claims

1. A light-emitting chip, characterized in that: The invention comprises a substrate, and a first semiconductor layer, a light-emitting layer and a second semiconductor layer stacked on the substrate, wherein the light-emitting layer is located between the first semiconductor layer and the second semiconductor layer, and the first semiconductor layer and the second semiconductor layer are excited to transmit electrons and holes respectively toward the light-emitting layer to recombine and emit light; A first diffusion layer and a second diffusion layer are also provided between the light-emitting layer and the second semiconductor layer. The first diffusion layer is located between the second semiconductor layer and the second diffusion layer. The bandgap width of the first diffusion layer is greater than the bandgap width of the second semiconductor layer and is less than or equal to the bandgap width of the second diffusion layer. The first diffusion layer and the second diffusion layer are used to increase the transmission angle of holes so that the holes can enter the light-emitting layer more evenly.

2. The light-emitting chip according to claim 1, characterized in that: The first diffusion layer is a P-type semiconductor, wherein the first diffusion layer contains one or more of aluminum, gallium and indium; and / or The second diffusion layer is a P-type semiconductor, wherein the second diffusion layer contains one or more of aluminum, gallium and indium.

3. The light-emitting chip according to claim 1, characterized in that: The light emitting chip further includes a transition layer, which is disposed between the first diffusion layer and the second diffusion layer, and has a bandgap width smaller than the bandgap width of the first diffusion layer and smaller than the bandgap width of the second diffusion layer.

4. The light-emitting chip according to claim 3, characterized in that: The thickness of the first diffusion layer is between 5nm and 40nm; and / or the thickness of the second diffusion layer is between 5nm and 40nm; and / or the thickness of the transition layer is between 5nm and 40nm.

5. The light emitting chip according to claim 1, characterized in that: The light-emitting chip also includes an intermediate layer, which is arranged between the first diffusion layer and the second diffusion layer. The doping source of the first diffusion layer and the doping source of the second diffusion layer both include magnesium elements. The intermediate layer is used to receive the magnesium elements diffused from the first diffusion layer and the second diffusion layer to the intermediate layer, so as to reduce the growth crystal defects on the first diffusion layer and the second diffusion layer.

6. The light emitting chip according to claim 5, characterized in that: The thickness of the intermediate layer is between 2nm and 10nm.

7. The light-emitting chip according to any one of claims 1 to 6, characterized in that: The distance between the second semiconductor layer and the light emitting layer is between 12nm and 300nm.

8. The light-emitting chip according to any one of claims 1 to 6, characterized in that: The doping concentration of the first diffusion layer and the doping concentration of the second diffusion layer are both greater than or equal to 1E18 atoms / cm 3 .

9. The light-emitting chip according to any one of claims 1 to 6, characterized in that: The light emitting chip further includes a buffer layer, wherein the buffer layer is located between the first semiconductor layer and the light emitting layer, and the buffer layer is used to release stress between the first semiconductor layer and the light emitting layer.

10. A display panel, characterized in that: It comprises a driving backplane, and a light-emitting chip as described in any one of claims 1 to 9, wherein the light-emitting chip is mounted on the driving backplane, and the driving backplane is used to control the light-emitting chip to emit light.

Citation Information

Patent Citations

  • Light-emitting diode structure

    CN102237455A

  • Nitride semiconductor light emitting device

    CN103066176A

  • GaN-based light-emitting diode epitaxial structure

    CN110635006A

  • Micro light-emitting diode

    CN114450810A

  • Semiconductor epitaxial structure and manufacturing method thereof, and LED chip