Negative pole piece as well as preparation method and application thereof

By stacking the first composite material layer and the second composite material layer on the negative electrode sheet of the sodium ion battery, the sodium embedded depth of the alloy-type negative electrode material is optimized, and a second carbon material layer is set on the surface layer, the alloy-type negative electrode is filled in. The expansion problem during discharge improves the stability and performance of the battery.

CN118969961AActive Publication Date: 2024-11-15XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411038827.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Alloy negative electrodes have serious volume expansion problems during the charging and discharging of sodium ion batteries, resulting in the powdering of electrode materials and the loss of active sodium, reducing battery performance.

Method used

A plurality of first composite material layers and second composite material layers are arranged in succession on the current collector surface of the negative electrode sheet. The material of the first composite material layer includes a first carbon material, an alloy negative electrode material and a first conductive agent. The mass content is reduced in turn from the current collector side to the side away from the current collector, the sodium embedding depth is optimized, and a second composite material layer containing a second carbon material is provided on the surface to bind expansion.

Benefits of technology

The sodium ion migration speed is improved, the degree of sodium embeddedness of alloy negative electrode materials is reduced, the problem of electrode sheet crushing is alleviated, and the stability and battery performance of the negative electrode sheet are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969961A_ABST
    Figure CN118969961A_ABST
Patent Text Reader

Abstract

The invention provides a negative pole piece and a preparation method and application thereof. The negative pole piece comprises a current collector, and at least one surface of the current collector is sequentially provided with at least two first composite material layers and second composite material layers in a laminated mode; the materials of all the first composite material layers comprise a first carbon material, an alloy negative electrode material and a first conductive agent; in the materials of any two adjacent first composite material layers, the mass content of the alloy negative electrode material in the material of the first composite material layer close to one side of the current collector is greater than the mass content of the alloy negative electrode material in the material of the first composite material layer close to one side of the second composite material layer; and the material of the second composite material layer comprises a second carbon material and a second conductive agent. According to the negative electrode plate, the problem that a mixed negative electrode of a first carbon material such as hard carbon and an alloy negative electrode material in a sodium ion battery is greatly expanded after sodium is embedded can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a negative electrode plate and a preparation method and application thereof. Background Art

[0002] As the global demand for clean energy grows, sodium-ion batteries, as a new type of battery technology, have attracted widespread attention due to their advantages such as abundant resources, low cost and high safety. Among them, alloy negative electrodes are an important component of sodium-ion batteries. Compared with the currently commonly used soft carbon and hard carbon negative electrodes, alloy negative electrodes have ultra-high capacity, which can significantly improve the energy density of sodium-ion batteries and are the direction of development of sodium-ion battery technology; however, alloy negative electrodes have serious volume expansion problems during the charging and discharging process, which will cause the electrode material to pulverize, accelerate the reaction with the electrolyte, lead to the loss of active sodium, and increase the impedance, thereby reducing the performance of the battery.

[0003] In order to solve the above problems, the relevant technology mainly mixes the alloy negative electrode with hard carbon, and then coats it on the aluminum foil substrate by uniform coating. This method can improve the expansion problem of the alloy negative electrode only when the proportion of the alloy negative electrode is small (for example, 0.5-2wt%). By mixing with the hard carbon material, the expansion of the hard carbon material is small, which can provide a certain buffer space for the alloy negative electrode, ensure structural stability, and improve the cycle life of the battery. However, when the proportion of the alloy negative electrode becomes larger (for example, 5-50wt%), the buffer space provided by the hard carbon negative electrode is insufficient, the pole piece expands, and after several charges and discharges, the material will become powdered, and side reactions will occur with the electrolyte, and the capacity will decay rapidly. Summary of the invention

[0004] In view of this, an object of the present application is to provide a negative electrode plate, in which a plurality of first composite material layers and a second composite material layer are sequentially stacked on at least one surface of a current collector, the materials of all the first composite material layers include a first carbon material, an alloy negative electrode material and a first conductive agent, and the mass contents of the alloy negative electrode material and the first conductive agent in the materials of the plurality of first composite material layers located on the same surface of the current collector decrease sequentially from the side close to the current collector to the side away from the current collector, thereby increasing the migration speed of sodium ions and the like in the negative electrode plate close to the current collector, reducing the difference in the degree of sodium embedding of the alloy negative electrode material on the side away from the current collector and the side close to the current collector (i.e., optimizing the sodium embedding depth of the alloy negative electrode material on the side of the negative electrode plate away from the current collector and the side close to the current collector), alleviating the plate crushing problem caused by the excessive sodium embedding depth of the alloy negative electrode material on the side away from the current collector, and ensuring the stability of the negative electrode plate; in addition, a second composite material layer containing a second carbon material is further provided on the surface to restrain the expansion of the negative electrode plate.

[0005] Another object of the present application is to provide a method for preparing a negative electrode sheet.

[0006] Another object of the present application is to provide a secondary battery.

[0007] To achieve the above-mentioned object, the first aspect of the present application provides a negative electrode sheet, comprising a current collector, at least one surface of the current collector being sequentially laminated with at least two layers of a first composite material layer and a second composite material layer;

[0008] The materials of all the first composite material layers include a first carbon material, an alloy negative electrode material and a first conductive agent; among the materials of any two adjacent first composite material layers located on the same surface of the current collector, the mass content of the alloy negative electrode material in the material of the first composite material layer close to the current collector is greater than the mass content of the alloy negative electrode material in the material of the first composite material layer close to the second composite material layer, and the mass content of the first conductive agent in the material of the first composite material layer close to the current collector is greater than the mass content of the first conductive agent in the material of the first composite material layer close to the second composite material layer;

[0009] The material of the second composite material layer includes a second carbon material and a second conductive agent.

[0010] In some embodiments, the first carbon material and the second carbon material each include at least one of hard carbon and soft carbon;

[0011] And / or, the alloy negative electrode material includes at least one of antimony, tin, phosphorus, silicon, bismuth, and germanium;

[0012] And / or, the first conductive agent and the second conductive agent include at least one of conductive carbon black, superconducting carbon, conductive graphite, carbon nanotubes, and graphene.

[0013] In some embodiments, the total mass content of the alloy negative electrode material in the negative electrode plate is greater than 0% and less than 49.5%.

[0014] In some embodiments, the mass content of the first carbon material in the first composite material layer is greater than or equal to the mass content of the alloy-based negative electrode material.

[0015] In some embodiments, the mass content of the first carbon material in the first composite material layer is less than or equal to the mass content of the second carbon material in the second composite material layer.

[0016] In some embodiments, the mass content of the first conductive agent in the material of the first composite material layer is 0.4-5.0%.

[0017] In some embodiments, the mass content of the second conductive agent in the material of the second composite material layer is 0.5-5.0%.

[0018] In some embodiments, the mass content of the first carbon material in the first composite material layer is 49.5-99%.

[0019] In some embodiments, when the number of layers of the first composite material layer is two, the mass content of the alloy negative electrode material in the first composite material layer is m, 0<m≦49.5%.

[0020] In other embodiments, when the number of the first composite material layer is greater than two, the mass content of the alloy negative electrode material in the first composite material layer is n, 0≦n≦49.5%.

[0021] In some embodiments, the mass content of the second carbon material in the second composite material layer is 90-99%.

[0022] In some embodiments, the materials of all the first composite material layers further include a first binder.

[0023] In some embodiments, the material of the second composite material layer further includes a second binder.

[0024] In some embodiments, the mass content of the first binder in the material of the first composite material layer is 0.5-5.0%.

[0025] In some embodiments, the mass content of the second binder in the material of the second composite material layer is 0.5-5.0%.

[0026] In some embodiments, the first binder and the second binder both include at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium alginate, and polyvinylidene fluoride.

[0027] In some embodiments, the number of the first composite material layers located on the same surface of the current collector is two layers, and in the material of the first composite material layer adjacent to the current collector, the mass contents of the alloy negative electrode material and the first conductive agent are a% and b%, respectively; in the material of the first composite material layer adjacent to the second composite material layer, the mass contents of the alloy negative electrode material and the first conductive agent are c% and d%, respectively; c, d, a, and b satisfy:

[0028] 20%≦c / (a+c)<50%, and / or, 20%≦d / (b+d)<50%.

[0029] In some embodiments, the at least two first composite material layers and the second composite material layers are sequentially stacked on both opposite sides of the current collector.

[0030] In some embodiments, the total thickness of all the first composite material layers on the same surface of the current collector is 60-90 μm.

[0031] In some embodiments, the total number of the first composite material layers located on the same surface of the current collector is 2-5 layers.

[0032] In some embodiments, the thickness of the second composite material layer located on the same surface of the current collector is 1-5 μm.

[0033] In some embodiments, the double-sided thickness of the negative electrode plate is 130-210 μm (including the thickness of the current collector, the thickness of the first composite material layer and the second composite material layer on all surfaces of the current collector).

[0034] In some embodiments, the ratio of the areal density of the first composite material layer to the areal density of the second composite material layer is (9-9.9):(0.1-1).

[0035] The second aspect of the present application provides a method for preparing a negative electrode sheet, comprising:

[0036] Prepare the first composite material layer slurry and the second composite material layer slurry respectively;

[0037] The first composite material layer slurry and the second composite material layer slurry are used as raw materials, and the first composite material layer and the second composite material layer are sequentially formed on at least one surface of the current collector by layered coating.

[0038] The third aspect of the present application provides a secondary battery, comprising a positive electrode plate, a separator and a negative electrode plate, wherein the negative electrode plate is the negative electrode plate described in the present application.

[0039] The negative electrode sheet described in this application can at least bring the following technical effects:

[0040] A plurality of first composite material layers and a second composite material layer are sequentially stacked on at least one surface of the current collector, the materials of all the first composite material layers include a first carbon material, an alloy negative electrode material and a first conductive agent, and the mass contents of the alloy negative electrode material and the first conductive agent in the materials of the plurality of first composite material layers on the same surface of the current collector decrease sequentially from the side close to the current collector to the side away from the current collector, thereby increasing the migration speed of sodium ions and the like in the negative electrode sheet close to the current collector, reducing the difference in the degree of sodium embedding of the alloy negative electrode material on the side away from the current collector and the side close to the current collector (i.e., optimizing the sodium embedding depth of the alloy negative electrode material on the side of the negative electrode sheet away from the current collector and the side close to the current collector), alleviating the problem of sheet crushing caused by excessive sodium embedding depth of the alloy negative electrode material on the side away from the current collector, and ensuring the stability of the negative electrode sheet; in addition, a second composite material layer containing a second carbon material is further provided on the surface to restrain the expansion of the negative electrode sheet.

[0041] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the following description of the embodiments in conjunction with the accompanying drawings.

[0043] in:

[0044] Figure 1 This is a schematic structural diagram of a negative electrode plate according to an exemplary embodiment of the present application.

[0045] Figure 2 A schematic structural diagram of a negative electrode plate is shown in another exemplary embodiment of the present application.

[0046] Reference numerals:

[0047] 1 - current collector; 101 - first surface; 102 - second surface; 2 - first composite material layer; 201 - first composite material layer A; 202 - first composite material layer B; 3 - second composite material layer. DETAILED DESCRIPTION

[0048] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, but cannot be understood as limiting the present application.

[0049] In this application, the disclosure of numerical ranges includes all values ​​within the entire range and the disclosure of further subdivided ranges, including the endpoints and sub-ranges given in these ranges.

[0050] In this application, the raw materials, equipment, etc. involved, unless otherwise specified, are all raw materials and equipment that can be made through commercial channels or known methods; the methods involved, unless otherwise specified, are all conventional methods.

[0051] The inventors discovered that in the related technology, when the alloy negative electrode is mixed with hard carbon and the alloy negative electrode material accounts for a large proportion, the buffer space provided by carbon materials such as hard carbon is insufficient, the electrode sheet expands, and after several charges and discharges, the material becomes powdered, reacts with the electrolyte, and the capacity decays rapidly.

[0052] Based on the above findings, the inventors have also found that starting from the structure of the negative electrode plate, the problem of expansion during the use of the alloy negative electrode of the sodium ion battery can be improved; from the perspective of battery dynamics, the sodium ions migrate in the negative electrode plate, and the greater the migration depth, the higher the difficulty of migration, and the amount of sodium ions that migrate gradually decreases. Therefore, in the negative electrode plate, the degree of sodium embedding of the plate on the side away from the current collector is higher than that of the plate on the side close to the current collector, and the degree of expansion of the plate on the side away from the current collector is higher than that of the plate on the side close to the current collector, and the plate on the side away from the current collector pulverizes faster; while the conventional negative electrode plate is evenly coated, the material composition of the side away from the current collector and the side close to the current collector is consistent, and the coating is homogenized. When the negative electrode material used has a large degree of expansion, the problems of this coating scheme are more obvious.

[0053] The inventor further discovered that multiple first composite material layers and second composite material layers are sequentially stacked on the current collector, and the materials of all the first composite material layers include the first carbon material, the alloy negative electrode material and the first conductive agent. The mass content of the alloy negative electrode material and the first conductive agent in the materials of the multiple first composite material layers decreases from the side close to the current collector to the side away from the current collector, which can increase the migration speed of sodium ions and the like in the negative electrode sheet close to the current collector, reduce the difference in the degree of sodium embedding of the alloy negative electrode material on the side away from the current collector and the side close to the current collector (that is, optimize the sodium embedding depth of the alloy negative electrode material on the side away from the current collector and the side close to the current collector of the negative electrode sheet), alleviate the problem of the electrode sheet crushing caused by the excessive sodium embedding depth of the alloy negative electrode material on the side away from the current collector, and thus ensure the stability of the negative electrode sheet. In addition, a second composite material layer containing the second carbon material is arranged on the surface layer to restrain the expansion of the negative electrode sheet.

[0054] <Negative electrode>

[0055] A negative electrode plate according to an embodiment of the present application is described below with reference to the accompanying drawings.

[0056] Figure 1 This is a schematic structural diagram of a negative electrode plate according to an exemplary embodiment of the present application.

[0057] like Figure 1As shown, the negative electrode sheet of this embodiment includes a current collector 1, and at least two first composite material layers 2 and second composite material layers 3 are sequentially stacked on at least one surface of the current collector 1.

[0058] The materials of all first composite material layers 2 include first carbon material, alloy negative electrode material and first conductive agent; among the materials of any two adjacent first composite material layers located on the same surface of the current collector, the mass content of alloy negative electrode material in the material of the first composite material layer close to the current collector is greater than the mass content of alloy negative electrode material in the material of the first composite material layer close to the second composite material layer; among the materials of any two adjacent first composite material layers, the mass content of first conductive agent in the material of the first composite material layer close to the current collector is greater than the mass content of first conductive agent in the material of the first composite material layer close to the second composite material layer. Such a setting increases the migration speed of sodium ions and the like in the negative electrode sheet close to the current collector, reduces the difference in the degree of sodium embedding of alloy negative electrode materials far from the current collector and close to the current collector, alleviates the degree of crushing of alloy negative electrode materials far from the current collector, and ensures the stability of negative electrode sheets.

[0059] The second composite material layer 3 includes a second carbon material and a second conductive agent, which can restrain the expansion of the negative electrode sheet.

[0060] In some embodiments, the first carbon material and the second carbon material both include, but are not limited to, at least one of hard carbon, soft carbon, and the like.

[0061] It should be noted that, in the embodiments of the present application, the first carbon material and the second carbon material may be the same or different, but are preferably the same.

[0062] As a preferred example, the negative electrode plate is a negative electrode plate of a sodium ion battery, and the first carbon material and the second carbon material are both hard carbon.

[0063] Illustratively, the hard carbon in the embodiments of the present application includes, but is not limited to, at least one of polymer-derived hard carbon materials, fossil fuel-derived hard carbon materials, biomass-derived hard carbon materials, and the like.

[0064] In some embodiments, the alloy negative electrode material includes but is not limited to at least one of antimony, tin, phosphorus, silicon, bismuth, germanium, and the like.

[0065] In some embodiments, the first conductive agent and the second conductive agent include, but are not limited to, at least one of conductive carbon black (SP), superconducting carbon, conductive graphite, carbon nanotubes, graphene, and the like.

[0066] It should be noted that the first carbon material in each first composite material layer material may be the same or different, preferably the same; the alloy negative electrode material in each first composite material layer material may be the same or different, preferably the same; the first conductive agent in each first composite material layer material may be the same or different, preferably the same; the first conductive agent and the second conductive agent may be the same or different, preferably the same.

[0067] In some embodiments, the total mass content of the alloy negative electrode material in the negative electrode plate is greater than 0% and below 49.5%, including but not limited to 0.1%, 5%, 10%, 20%, 30%, 40% or 49.5%, etc.

[0068] In some embodiments, the mass content of the first carbon material in the first composite material layer 2 is greater than or equal to the mass content of the alloy-based negative electrode material.

[0069] In some embodiments, the mass content of the first carbon material in the first composite material layer 2 is 49.5-99%, including but not limited to 49.5%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 99%, etc.

[0070] In some embodiments, when the number of layers of the first composite material layer is two, the mass content of the alloy negative electrode material in the first composite material layer is m, 0<m≦49.5%. Exemplary values ​​of m include but are not limited to 0.1%, 0.5%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 49.5%, etc.

[0071] In other embodiments, when the number of layers of the first composite material layer 2 is greater than two layers, the mass content of the alloy negative electrode material in the first composite material layer 2 is n, 0≦n≦49.5%. Exemplary, the value of n includes but is not limited to 0%, 0.5%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 49.5%, etc. In the embodiment of the present application, the mass content of the alloy negative electrode material in the first composite material layer is within the above range, which can ensure that the negative electrode sheet remains flat after multiple charge and discharge of the battery, and the active material is firmly bonded to the current collector; if it is higher than 49.5%, the problem of wrinkling of the electrode sheet and cracking of the surface is prone to occur during the cycle; at the same time, the electrolyte enters the interior of the electrode sheet through the cracks, and will further directly react with the active material inside, further accelerating the expansion and pulverization of the active material.

[0072] In some embodiments, in the material of the first composite material layer 2, the mass content of the first conductive agent is 0.4-5.0%, including but not limited to 0.4%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.

[0073] In some embodiments, the mass content of the first carbon material in the first composite material layer 2 is less than or equal to the mass content of the second carbon material in the second composite material layer 3. The purpose of this arrangement is to increase the content of the conductive agent in the composite material layer close to the current collector side, which is conducive to the diffusion of electrons on the current collector to the surface of each active material through the conductive agent, promote the embedding of active materials into sodium ions, balance the sodium embedding depth of active materials close to the current collector side and away from the current collector side, alleviate the sodium embedding depth of surface active materials, and alleviate the problems of expansion and pulverization.

[0074] In some embodiments, the mass content of the second carbon material in the second composite material layer 3 is 90-99%, including but not limited to 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, etc.

[0075] In some embodiments, in the material of the second composite material layer 3, the mass content of the second conductive agent is 0.5-5.0%, including but not limited to 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.

[0076] In some embodiments, the materials of all first composite material layers 2 further include a first binder.

[0077] In some embodiments, the material of the second composite material layer 3 further includes a second adhesive.

[0078] In some embodiments, in the material of the first composite material layer 2, the mass content of the first binder is 0.5-5.0%, including but not limited to 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.

[0079] In some embodiments, in the material of the second composite material layer, the mass content of the second binder is 0.5-5.0%, including but not limited to 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.

[0080] In some embodiments, the first binder and the second binder both include butadiene styrene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), sodium alginate (SA), polyvinylidene fluoride (PVDF), etc. At least one of the following:

[0081] It should be noted that styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) are both binders in a broad sense, but if further subdivided, styrene butadiene rubber (SBR) is a binder and carboxymethyl cellulose (CMC) is a thickener.

[0082] As an optional example, the masses of materials of each first composite material layer located on the same surface of the current collector are equal, and the ratio of the total mass of materials of all first composite material layers to the mass of the second composite material layer is (9-9.9):(0.1-1), including but not limited to 9.9:0.1, 9.7:0.3, 9.5:0.5, 9.3:0.7 or 9.1:0.9 or 9.0:1.0, etc.

[0083] As another optional example, the masses of materials of each first composite material layer located on the same surface of the current collector are not equal, and gradually decrease from the side close to the current collector to the side away from the current collector; the ratio of the total mass of materials of all first composite material layers to the mass of the second composite material layer is (9-9.9): (0.1-1), including but not limited to 9.9:0.1, 9.7:0.3, 9.5:0.5, 9.3:0.7 or 9.1:0.9 or 9.0:1.0, etc.

[0084] In some embodiments, the total thickness of all first composite material layers 2 located on the same surface of the current collector 1 is 60-90 μm, including but not limited to 60 μm, 70 μm, 80 μm or 90 μm.

[0085] It should be noted that, in the embodiments of the present application, the thicknesses of the first composite material layers may be the same or different.

[0086] It should also be noted that when multiple surfaces of the current collector are provided with at least two layers of the first composite material layer and the second composite material layer, the multiple first composite material layers on each surface may be the same or different, preferably the same; the multiple second composite material layers on each surface may be the same or different, preferably the same.

[0087] As a preferred example, at least two first composite material layers 2 and second composite material layers 3 are sequentially stacked on both opposite sides of the current collector 1 .

[0088] In some embodiments, the total number of first composite material layers 2 located on the same surface of the current collector 1 is 2-5 layers, including but not limited to 2 layers, 3 layers, 4 layers, or 5 layers.

[0089] In some embodiments, the thickness of the second composite material layer 3 located on the same surface of the current collector 1 is 3-5 μm, including but not limited to 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm.

[0090] In some embodiments, the thickness of the negative electrode sheet is 130-210 μm, including but not limited to 130 μm, 150 μm, 170 μm, 190 μm or 210 μm.

[0091] In the embodiment of the present application, the thickness of the negative electrode sheet includes the thickness of the current collector 1 and the thickness of the first composite material layer 2 and the second composite material layer 3 on all surfaces of the current collector 1 .

[0092] In some embodiments, the ratio of the surface density of the first composite material layer 2 to the surface density of the second composite material layer 1 is (9-9.9):(0.1-1), including but not limited to 9.9:0.1, 9.7:0.3, 9.5:0.5, 9.3:0.7 or 9.1:0.9 or 9.0:1.0, etc.

[0093] In some embodiments, Figure 2 As shown, the number of first composite material layers located on the same surface of the current collector 1 is two, and the mass contents of the alloy negative electrode material and the first conductive agent in the material of the first composite material layer adjacent to the current collector 1 (for the convenience of subsequent description, marked as the first composite material layer A 201) are a% and b% respectively; the mass contents of the alloy negative electrode material and the first conductive agent in the material of the first composite material layer adjacent to the second composite material layer 3 (for the convenience of subsequent description, marked as the first composite material layer B 202) are c% and d% respectively; c, d, a, b satisfy:

[0094] 20%≦c / (a+c)<50%, and / or, 20%≦d / (b+d)<50%.

[0095] In an embodiment of the present application, when the number of first composite material layers is two, the mass content a% of the alloy negative electrode material in the first composite material layer A201 and the mass content c% of the alloy negative electrode material in the first composite material layer B202 meet the above relationship of 20%≦c / (a+c)<50%. This can solve the problem that when the proportions of alloy negative electrode materials and first carbon material negative electrodes such as hard carbon are the same in the upper and lower layers (that is, the first composite material layer A201), the upper layer (that is, the first composite material layer B202) has excessive sodium embedding depth, which causes the electrode to easily pulverize. When the alloy negative electrode content of the first composite material layer B 202 is less than 20% (that is, the value of c / (a+c) is less than 20%), the alloy negative electrode material content of the upper layer (that is, the first composite material layer B 202) is too little, and the upper alloy negative electrode material has enough first carbon material to buffer; but the corresponding alloy negative electrode material content of the first composite material layer A 201 (close to the current collector layer) will be too large, and the content of the first carbon material will not be enough to buffer the expansion of the alloy negative electrode material, and the pole piece will crack from the inside to the outside. Similarly, when the alloy negative electrode content of the first composite material layer B202 is more than 50% (that is, the value of c / (a+c) is greater than or equal to 50%), the alloy negative electrode material content of the upper layer (that is, the first composite material layer B 202) is too large, and the upper alloy negative electrode material does not have enough first carbon material to buffer the expansion of the alloy negative electrode material, and the pole piece will crack from the inside to the outside.

[0096] The mass content b% of the first conductive agent in the first composite material layer A 201 and the mass content d% of the first conductive agent in the first composite material layer B 202 meet the above relationship of 20%≦d / (b+d)<50%, that is, ensuring that the content of the first conductive agent in the first composite material layer A close to the current collector is higher than the content of the first conductive agent in the first composite material layer B far from the current collector can accelerate the conversion rate of sodium ions and increase the speed of sodium ion insertion and extraction (because, as sodium ions migrate into the interior of the electrode, the deeper the migration depth, the more difficult it is for sodium ions to diffuse, and the fewer sodium ions enter the inner layer. If the conductive agent content is insufficient at this time, it will affect the speed at which sodium ions gain or lose electrons. Therefore, ensuring that there are conductive agents at more sites will allow sodium ions that migrate to the inner layer to gain or lose electrons faster, so the content of the first conductive agent close to the inner side of the current collector is required to be higher). If the value of d / (b+d) is less than 20%, there is too little first conductive agent in the first composite material layer B 202, which will limit the electron migration rate; if the value of d / (b+d) is greater than or equal to 50%, the content of the first conductive agent in the first composite material layer A 201 is low, and this layer is closer to the current collector. The low content of the first conductive agent will further deteriorate the rate at which sodium ions gain or lose electrons.

[0097] When the values ​​of c / (a+c) and d / (b+d) satisfy the above relationship of 20%≦c / (a+c)<50% and 20%≦d / (b+d)<50%, it is because the sodium ions are more difficult to embed in the negative electrode sheet from the outside to the inside (closer to the current collector), the more sodium ions are on the surface, and the deeper they are embedded in the negative electrode material; the layered distribution of alloy negative electrode materials, the less alloy negative electrode material in the first composite material layer B away from the current collector, and the less the amount of alloy negative electrode material in the first composite material layer A on the inside. There is a little more alloy negative electrode material in 201, which can slow down the expansion and differentiation when there is more alloy negative electrode material on the surface and the embedding depth is greater; the alloy is distributed in layers to balance the embedding depth of sodium ions in the surface and inner layers of the negative electrode; at the same time, with the assistance of the layered distribution of the conductive agent, the rate of gaining and losing electrons of sodium ions in the thickness direction of the entire electrode can be optimized, and the alloy negative electrode close to the current collector side can also gain and lose electrons faster, which is more conducive to balancing the sodium embedding depth of the upper and lower alloy materials; at the same time, the upper layer (that is, the first composite material layer B 202) has less alloy negative electrode material, and the depth of sodium embedding is alleviated, which can play a protective role, and can cover the cracks caused by the expansion of the alloy negative electrode material close to the inner side of the current collector, and further prevent the electrolyte from reacting with the fresh alloy negative electrode material.

[0098] It should be noted that in the embodiments of the present application, the sum of the mass contents of each component in the first composite material layer material (the first carbon material, the first conductive agent, the alloy negative electrode material, etc. (for example, if there is a first binder, it also includes the first binder)) is 100%, and the sum of the mass contents of each component in the second composite material layer material (the second carbon material, the second conductive agent, etc. (if there is a second binder, it also includes the second binder)) is 100%.

[0099] As a more preferred example, Figure 2 As shown, two first composite material layers and a second composite material layer 3 are sequentially stacked on opposite sides of the current collector 1. As described above, among the two first composite material layers, the first composite material layer adjacent to the current collector 1 is marked as the first composite material layer A 201, and the first composite material layer adjacent to the second composite material layer 3 is marked as the first composite material layer B 202.

[0100] For example, when the negative electrode is Figure 2 When the number of first composite material layers shown is two layers of negative electrode sheets, the material of the first composite material layer A 201 and the material of the first composite material layer B 202 both include a first carbon material, an alloy negative electrode material, a first conductive agent and a first binder, and the material of the second composite material layer 3 includes a second carbon material, a second conductive agent and a second binder.

[0101] The negative electrode sheet of the embodiment of the present application can at least bring the following technical effects:

[0102] A plurality of first composite material layers and a second composite material layer are sequentially stacked on at least one surface of the current collector, the materials of all the first composite material layers include a first carbon material, an alloy negative electrode material and a first conductive agent, and the mass contents of the alloy negative electrode material and the first conductive agent in the materials of the plurality of first composite material layers on the same surface of the current collector decrease sequentially from the side close to the current collector to the side away from the current collector, thereby increasing the migration speed of sodium ions and the like in the negative electrode sheet close to the current collector, reducing the difference in the degree of sodium embedding of the alloy negative electrode material on the side away from the current collector and the side close to the current collector (i.e., optimizing the sodium embedding depth of the alloy negative electrode material on the side of the negative electrode sheet away from the current collector and the side close to the current collector), alleviating the problem of sheet crushing caused by excessive sodium embedding depth of the alloy negative electrode material on the side away from the current collector, and ensuring the stability of the negative electrode sheet; in addition, a second composite material layer containing a second carbon material is further provided on the surface to restrain the expansion of the negative electrode sheet.

[0103] <Method for preparing negative electrode sheet>

[0104] The method for preparing the negative electrode sheet of the embodiment of the present application can be used to prepare the negative electrode sheet of the embodiment of the present application.

[0105] The method for preparing the negative electrode sheet of the embodiment of the present application comprises the following steps:

[0106] S101, prepare the first composite material layer slurry and the second composite material layer slurry respectively.

[0107] As an optional example, the slurry of each first composite material layer is composed of the above-mentioned first carbon material, the above-mentioned alloy negative electrode material, the above-mentioned first conductive agent and the above-mentioned first binder. When preparing, the above-mentioned first carbon material, the above-mentioned alloy negative electrode material, the above-mentioned first conductive agent and the above-mentioned first binder are mixed according to the ratio of each first composite material layer, and then added into deionized water and evenly mixed to obtain the slurry of the corresponding first composite material layer.

[0108] As an optional example, the second composite material layer slurry is composed of the above-mentioned second carbon material, the above-mentioned second conductive agent and the above-mentioned second binder; during preparation, the above-mentioned second carbon material, the above-mentioned second conductive agent and the above-mentioned second binder are mixed, and then added to deionized water and evenly mixed to obtain the slurry of the second composite material layer.

[0109] It should be noted that the material selection of the above-mentioned first carbon material, the above-mentioned alloy negative electrode material, the above-mentioned first conductive agent, the above-mentioned first binder, the above-mentioned second carbon material, the above-mentioned second conductive agent and the above-mentioned second binder are all consistent with those in the negative electrode sheet of this embodiment and will not be repeated here.

[0110] S102, using the first composite material layer slurry and the second composite material layer slurry as raw materials, sequentially forming the first composite material layer and the second composite material layer on the surface of the current collector by layered coating.

[0111] <Secondary Battery>

[0112] The secondary battery of the embodiment of the present application comprises a positive electrode plate, a separator and a negative electrode plate, wherein the negative electrode plate is the negative electrode plate of the embodiment of the present application.

[0113] In some embodiments, the secondary battery includes but is not limited to a sodium ion battery, a sodium ion battery, etc., preferably a sodium ion battery.

[0114] The method for preparing the negative electrode sheet and the secondary battery of the embodiment of the present application both have at least the beneficial effects of the negative electrode sheet of the embodiment of the present application.

[0115] Certain features of the present technology are further illustrated in the following non-limiting examples.

[0116] 1. Examples and Comparative Examples

[0117] Example 1

[0118] (Negative electrode)

[0119] like Figure 2 As shown, the negative electrode sheet of this embodiment includes a current collector 1, and the current collector 1 has a first surface 201 and a second surface 202 arranged opposite to each other, and a first composite material layer A201, a first composite material layer B202, and a second composite material layer 3 are sequentially laminated on the first surface 201 and the second surface 202. The first composite material layer A201 on the first surface 101 is completely identical to the first composite material layer A201 on the second surface 102, the first composite material layer B202 on the first surface 101 is completely identical to the first composite material layer B202 on the second surface 102, and the second composite material layer 3 on the first surface 101 is completely identical to the second composite material layer 3 on the second surface 102. Specifically:

[0120] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 90.9%, Sb 4.0%, conductive carbon black (SP) 1.6%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0121] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 95.1%, Sb 1.0%, conductive carbon black (SP) 0.4%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0122] The materials of the second composite material layer 3 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: 94.5% hard carbon, 2% conductive carbon black (SP), 1.5% carboxymethyl cellulose (CMC), and 2.0% styrene-butadiene rubber (SBR).

[0123] The mass ratios of the materials of the first composite material layer A 201, the first composite material layer B 202, and the second composite material layer 3 on the first surface 201 and the second surface 202 are all 7.84:1.96:0.2; the hard carbon is all biomass-derived hard carbon material; the thickness of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 67 μm (single-sided thickness), the thickness of the first composite material layer B 202 on the first surface 201 and the second surface 202 is 17 μm (single-sided thickness), and the thickness of the second composite material layer 3 on the first surface 201 and the second surface 202 is 1.7 μm (single-sided thickness); the negative electrode current collector is an aluminum foil with a thickness of 13 μm, and the thickness of the negative electrode sheet is 184.4 μm (double-sided thickness 67*2+17*2+1.7*2+13); the first composite material layer A 201 and the first composite material layer B 202 on the first surface 201 and the second surface 202 are 67 μm (single-sided thickness). The surface density ratio of the first surface 201 and the second surface 202 is 8:2, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 128 g / m 2 (Double-sided surface density), the surface density of the first composite material layer B 202 on the first surface 201 and the second surface 202 is 32 g / m 2 (Double-sided surface density), the surface density of the second composite material layer 3 on the first surface 201 and the second surface 202 is 3.0 g / m 2 (double-sided surface density); the surface density of the negative electrode is 163.2g / m 2 (Double-sided areal density).

[0124] (Method for preparing negative electrode sheet)

[0125] The method for preparing the negative electrode sheet of this embodiment comprises the following steps:

[0126] (1) Preparation of the first composite material layer A slurry: hard carbon, Sb, SP, CMC, and SBR are mixed according to the proportions of the material components of the first composite material layer A 201 in the negative electrode plate of this embodiment, and then added into deionized water and mixed to obtain the first composite material layer A slurry.

[0127] (2) Preparation of the first composite material layer B slurry: hard carbon, Sb, SP, CMC, and SBR are mixed according to the proportions of the material components of the first composite material layer B 202 in the negative electrode plate of this embodiment, and then added into deionized water and mixed to obtain the first composite material layer B slurry.

[0128] (3) Preparation of second composite material layer slurry: hard carbon, SP, CMC and SBR are mixed according to the proportions of the material components of the second composite material layer 3 in the negative electrode plate of this embodiment, and then added into deionized water and mixed to obtain second composite material layer slurry.

[0129] (4) Layered coating: comprising the following steps:

[0130] 1) First, the first composite material layer A slurry is coated on the first surface 101 and the second surface 102 of the current collector so that the coating surface density is 128 g / m 2 , and then drying to obtain a current collector containing the first composite material layer A;

[0131] 2) The first composite material layer B slurry is then coated on the surface of the first composite material layer A away from the current collector in the current collector containing the first composite material layer A, so that the coating surface density is 32 g / m 2 , and then drying to obtain a current collector containing the first composite material layers A and B;

[0132] 3) Finally, the second composite material layer slurry is coated on the surface of the first composite material layer B away from the current collector in the current collector containing the first composite material layers A and B, so that the coating surface density is 3g / m 2 , and then baked to obtain the negative electrode sheet of this embodiment.

[0133] Example 2

[0134] This embodiment is basically the same as Embodiment 1, except that:

[0135] In the negative electrode:

[0136] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 91.6%, Sb 3.5%, conductive carbon black (SP) 1.4%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0137] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 94.4%, Sb 1.5%, conductive carbon black (SP) 0.6%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0138] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 7:3, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 112 g / m 2 .

[0139] In the method for preparing the negative electrode sheet:

[0140] Step (4) Layered coating step 1) to achieve a coating surface density of 112 g / m 2 ;

[0141] Step (4) Layered coating step 2) to achieve a coating surface density of 48 g / m 2 .

[0142] Example 3

[0143] This embodiment is basically the same as Embodiment 1, except that:

[0144] In the negative electrode:

[0145] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 92.3%, Sb 3.0%, conductive carbon black (SP) 1.2%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0146] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 93.7%, Sb 2.0%, conductive carbon black (SP) 0.8%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0147] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 6:4, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 96 g / m 2 .

[0148] In the method for preparing the negative electrode sheet:

[0149] Step (4) Layered coating step 1) to achieve a coating surface density of 96 g / m 2 ;

[0150] Step (4) Layered coating step 2) to achieve a coating surface density of 64 g / m 2 .

[0151] Example 4

[0152] This embodiment is basically the same as Embodiment 1, except that:

[0153] In the negative electrode:

[0154] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 92.86%, Sb 2.6%, conductive carbon black (SP) 1.04%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0155] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 93.14%, Sb 2.4%, conductive carbon black (SP) 0.96%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0156] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 52:48, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 83.2 g / m 2 .

[0157] In the method for preparing the negative electrode sheet:

[0158] Step (4) Layered coating step 1) to achieve a coating surface density of 83.2 g / m 2 ;

[0159] Step (4) Layered coating step 2) to achieve a coating surface density of 76.8 g / m 2 .

[0160] Example 5

[0161] This embodiment is basically the same as Embodiment 1, except that:

[0162] In the negative electrode:

[0163] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 91.3%, Sb 4.0%, conductive carbon black (SP) 1.2%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0164] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 94.7%, Sb 1.0%, conductive carbon black (SP) 0.8%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0165] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 8:2, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 128 g / m 2 .

[0166] In the method for preparing the negative electrode sheet:

[0167] Step (4) Layered coating step 1) to achieve a coating surface density of 128 g / m 2 ;

[0168] Step (4) Layered coating step 2) to achieve a coating surface density of 32 g / m 2 .

[0169] Example 6

[0170] This embodiment is basically the same as Embodiment 1, except that:

[0171] In the negative electrode:

[0172] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 91.9%, Sb 3.0%, conductive carbon black (SP) 1.6%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0173] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 94.1%, Sb 2.0%, conductive carbon black (SP) 0.4%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0174] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 6:4, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 96 g / m 2 .

[0175] In the method for preparing the negative electrode sheet:

[0176] Step (4) Layered coating step 1) to achieve a coating surface density of 96 g / m 2 ;

[0177] Step (4) Layered coating step 2) to achieve a coating surface density of 64 g / m 2 .

[0178] Example 7

[0179] This embodiment is basically the same as Embodiment 1, except that:

[0180] In the negative electrode:

[0181] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 49.5%, Sb 49.5%, conductive carbon black (SP) 0.5%, carboxymethyl cellulose (CMC) 0.25%, styrene butadiene rubber (SBR) 0.25%.

[0182] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 87%, Sb 12.375%, conductive carbon black (SP) 0.125%, carboxymethyl cellulose (CMC) 0.25%, styrene butadiene rubber (SBR) 0.25%.

[0183] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 3:7, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 48 g / m 2 .

[0184] In the method for preparing the negative electrode sheet:

[0185] Step (4) Layered coating step 1) to achieve a coating surface density of 48 g / m 2 ;

[0186] Step (4) Layered coating step 2) to achieve a coating surface density of 112 g / m 2 .

[0187] Example 8

[0188] This embodiment is basically the same as Embodiment 1, except that:

[0189] In the negative electrode:

[0190] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 94.5%, Sb 0.4%, conductive carbon black (SP) 1.6%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0191] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 96%, Sb 0.1%, conductive carbon black (SP) 0.4%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0192] The surface density ratio of the first composite material layer A 201 to the first composite material layer B 202 on the first surface 201 and the second surface 202 is 52:48, and the surface density of the first composite material layer A 201 is 83.2 g / m 2 .

[0193] In the method for preparing the negative electrode sheet:

[0194] Step (4) Layered coating step 1) to achieve a coating surface density of 83.2 g / m 2 ;

[0195] Step (4) Layered coating step 2) to achieve a coating surface density of 76.8 g / m 2 .

[0196] Example 9

[0197] This embodiment is basically the same as Embodiment 1, except that:

[0198] In the negative electrode:

[0199] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 6:4, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 96 g / m 2 .

[0200] In the method for preparing the negative electrode sheet:

[0201] Step (4) Layered coating step 1) to achieve a coating surface density of 96 g / m 2 ;

[0202] Step (4) Layered coating step 2) to achieve a coating surface density of 64 g / m 2 .

[0203] Example 10

[0204] This embodiment is basically the same as Embodiment 1, except that:

[0205] In the negative electrode:

[0206] A first composite material layer C is added between the first composite material layer B 202 on the first surface 201 and the second composite material layer 3 on the second surface 202 ; the first composite material layer C on the first surface 101 is completely identical to the first composite material layer C on the second surface 102 .

[0207] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 69%, Sb 25%, conductive carbon black (SP) 2.5%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0208] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 80%, Sb 15%, conductive carbon black (SP) 1.5%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0209] The materials of the first composite material layer C on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 86%, Sb 10%, conductive carbon black (SP) 0.5%, carboxymethyl cellulose (CMC) 1.5%, and styrene-butadiene rubber (SBR) 2.0%.

[0210] The mass ratios of the first composite material layer A 201, the first composite material layer B 202, the first composite material layer C and the second composite material layer 3 on the first surface 201 and the second surface 202 are all 80:48:32:3; the thicknesses of the first composite material layer A 201 on the first surface 201 and the second surface 202 are both 42.0 μm, the thicknesses of the first composite material layer B 202 on the first surface 201 and the second surface 202 are both 26.0 μm, the thicknesses of the first composite material layer C on the first surface 201 and the second surface 202 are both 17.0 μm, the thicknesses of the second composite material layer 3 on the first surface 201 and the second surface 202 are both 1.6 μm, and the thickness of the negative electrode sheet is 186.2 μm (42*2+26*2+17*2+1.6*2+13); the first composite material layer A 201, the first composite material layer B 202 on the first surface 201 and the second surface 202 The surface density ratio of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 80 g / m 2 .

[0211] In the method for preparing the negative electrode sheet:

[0212] It also includes: preparation of the first composite material layer C slurry: mixing hard carbon, Sb, SP, CMC, and SBR according to the proportions of the material components of the first composite material layer C in the negative electrode plate of this embodiment, and then adding them into deionized water and mixing them to obtain the first composite material layer C slurry.

[0213] Step (4) layered coating: comprising the following steps:

[0214] 1) First, the first composite material layer A slurry is coated on the first surface 101 and the second surface 102 of the current collector so that the coating surface density is 80 g / m 2 , and then drying to obtain a current collector containing the first composite material layer A;

[0215] 2) The first composite material layer B slurry is then coated on the surface of the first composite material layer A away from the current collector in the current collector containing the first composite material layer A, so that the coating surface density is 48 g / m 2 , and then drying to obtain a current collector containing the first composite material layers A and B;

[0216] 3) The first composite material layer C slurry is then coated on the surface of the first composite material layer B away from the current collector in the current collector containing the first composite material layers A and B, so that the coating surface density is 32 g / m 2 , and then drying to obtain a current collector containing the first composite material layers A, B, and C;

[0217] 4) Finally, the second composite material layer slurry is coated on the surface of the first composite material layer C away from the current collector in the current collector containing the first composite material layers A, B, and C, so that the coating surface density is 3 g / m 2 , the discharge capacity is 300 mAh / g, and then baked to obtain the negative electrode sheet of this embodiment.

[0218] Embodiment 11

[0219] This embodiment is basically the same as Embodiment 1, except that:

[0220] All Sb is replaced by silicon-germanium alloy, in which the mass ratio of silicon to germanium is 5:5.

[0221] Example 12

[0222] This embodiment is basically the same as Embodiment 1, except that:

[0223] In the negative electrode:

[0224] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 89.9%, Sb 1.6%, conductive carbon black (SP) 5%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0225] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 94.85%, Sb 0.4%, conductive carbon black (SP) 1.25%, carboxymethyl cellulose (CMC) 1.5%, styrene butadiene rubber (SBR) 2.0%.

[0226] The surface density ratio of the first composite material layer A 201 on the first surface 201 and the first composite material layer B 202 on the second surface 202 is 8:2, and the surface density of the first composite material layer A 201 on the first surface 201 and the second surface 202 is 128 g / m 2 .

[0227] In the method for preparing the negative electrode sheet:

[0228] Step (4) Layered coating step 1) to achieve a coating surface density of 128 g / m 2 ;

[0229] Step (4) Layered coating step 2) to achieve a coating surface density of 32 g / m 2 .

[0230] Example 13

[0231] This embodiment is basically the same as Embodiment 1, except that:

[0232] The hard carbon in all first composite material layers A 201 , all first composite material layers B 202 and all second composite material layers 3 is replaced with soft carbon, and the conductive carbon black (SP) is replaced with carbon nanotubes.

[0233] Comparative Example 1

[0234] The negative electrode sheet of this comparative example includes a current collector, the current collector has a surface A and a surface B arranged opposite to each other, and a composite material layer is provided on both the surface A and the surface B. Among them:

[0235] The materials of the composite material layers on the surface A and the surface B are composed of the following components in mass percentage: hard carbon 89.5%, Sb 5%, conductive carbon black (SP) 2%, carboxymethyl cellulose (CMC) 1.5%, and styrene-butadiene rubber (SBR) 2.0%.

[0236] The total mass of the composite material layer on surface A is the same as the total mass of the first composite material layer A201, the first composite material layer B202 and the second composite material layer 3 on the first surface 101 in Example 1; the total mass of the composite material layer on surface B is the same as the total mass of the first composite material layer A201, the first composite material layer B202 and the second composite material layer 3 on the first surface 102 in Example 1; the hard carbon is a biomass-derived hard carbon material, the thickness of the composite material layer on surface A and surface B is 86μm (the total thickness of the composite material layer on surface A and surface B is 172μm), the negative electrode current collector is an aluminum foil with a thickness of 13μm, and the thickness of the negative electrode plate is 185μm; the surface density of the composite material layer on surface A and surface B is 163.2g / m 2 .

[0237] The preparation method of the negative electrode sheet of this comparative example is: mix the hard carbon, Sb, SP, CMC and SBR in the formula, add them into deionized water and mix them well to obtain a composite material layer slurry. Then, the composite material layer slurry is coated on one surface of the current collector so that the coating surface density is 163.2 g / m 2 , discharge capacity 310 mAh / g, and then baked to obtain the negative electrode sheet of this comparative example.

[0238] Comparative Example 2

[0239] This comparative example is basically the same as Example 1, except that:

[0240] In the negative electrode sheet, the first surface 201 and the second surface 202 do not contain the second composite material layer 3 .

[0241] In the method for preparing the negative electrode sheet:

[0242] The step (3) and step (4) are not included.

[0243] Comparative Example 3

[0244] This comparative example is basically the same as Example 1, except that:

[0245] In the negative electrode:

[0246] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 95.1%, Sb 1.0%, conductive carbon black (SP) 0.4%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0247] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 80.9%, Sb 4.0%, conductive carbon black (SP) 1.6%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0248] Comparative Example 4

[0249] This comparative example is basically the same as Example 1, except that:

[0250] In the negative electrode:

[0251] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 93.9%, Sb 1.0%, conductive carbon black (SP) 1.6%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0252] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 92.1%, Sb 4.0%, conductive carbon black (SP) 0.4%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0253] Comparative Example 5

[0254] This comparative example is basically the same as Example 1, except that:

[0255] In the negative electrode:

[0256] The materials of the first composite material layer A 201 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 93.9%, Sb 4.0%, conductive carbon black (SP) 0.4%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0257] The materials of the first composite material layer B 202 on the first surface 201 and the second surface 202 are composed of the following components in mass percentage: hard carbon 92.1%, Sb 1.0%, conductive carbon black (SP) 1.6%, carboxymethyl cellulose (CMC) 1.5%, styrene-butadiene rubber (SBR) 2.0%.

[0258] 2. Performance Test

[0259] The negative electrode sheets of each embodiment or comparative example were assembled into sodium ion batteries, and the assembled sodium ion batteries were tested for electrochemical performance.

[0260] The method for assembling a sodium ion battery comprises the following steps:

[0261] (1) Preparation of positive electrode sheet: Layered oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, binder polyvinylidene fluoride, and conductive agent carbon black were mixed at a fixed mass ratio of 96%, 2%, and 2%, and then solvent N-methylpyrrolidone was added and stirred to form a positive electrode slurry; the positive electrode slurry was evenly coated on the opposite sides of the aluminum foil with a thickness of 13μm, and the coating surface density was 350g / m 2 The coated positive electrode sheet is baked, and then cold pressed, trimmed, cut into pieces, and striped, and the tabs are welded to obtain a spare positive electrode sheet.

[0262] (2) The negative electrode sheets of each embodiment or comparative example are cold pressed, trimmed, cut into pieces, and stripped, and then the tabs are welded to obtain spare negative electrode sheets.

[0263] (3) Preparation of electrolyte: First, in a glove box, sodium salt was added to a mixture of propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) at a volume ratio of 1:1:1:1, and the mixture was mixed evenly to prepare an electrolyte. The sodium salt concentration was 1.2 mol / L.

[0264] (4) Battery assembly: The spare positive electrode plate, spare negative electrode plate and separator (polyethylene (PE) base film + single-sided ceramic, PE base film thickness 9 μm, ceramic thickness 2 μm) are stacked to form a bare battery cell, and placed in an aluminum-plastic film; then vacuum baked at 95°C to remove moisture, and then the electrolyte is injected to seal; after standing, forming, degassing, sealing, and capacity separation, a sodium ion battery is obtained.

[0265] Electrochemical performance test:

[0266] The test method of the expansion rate of the fully charged negative electrode is as follows: first, fully charge the battery according to the following steps; the full charging process is 1C constant current and constant voltage charging, the upper limit voltage is 3.95V, and the cut-off current is 0.05C; then the battery is disassembled, the negative electrode plate is separated, and the thickness of the negative electrode plate is tested and recorded as d1. The thickness of the negative electrode plate after rolling in each embodiment and comparative example is d0; the thickness of the negative electrode plate collector is recorded as d; the full charge expansion rate of the negative electrode plate η1 = (d1-d0) / (d0-d).

[0267] The test method for the capacity retention rate after 500 cycles is as follows: empty the battery and then charge and discharge it according to the following process. Each complete charge and discharge is counted as 1 week. The capacity in the first week is the initial capacity C1, and the capacity in the 500th week is C 500 . Cycle 500 cycles capacity retention rate η2 = C 500 / C1; where

[0268] Battery emptying process: 1C constant current discharge to the lower limit voltage of 1.5V;

[0269] Charge and discharge process: 1C constant current and constant voltage charging, upper limit voltage 3.95V, cut-off current 0.05C; stand for 10 minutes; 1C constant current discharge to lower limit voltage 1.5V; stand for 10 minutes.

[0270] The test method for the increase ratio of internal resistance after 500 cycles is as follows: using a conventional voltage internal resistance tester, the AC internal resistance of the battery in the first cycle is R1; the AC internal resistance of the battery in the 500th cycle is R 500 ; The internal resistance growth rate of the battery after 500 cycles is η3=R 500 / R1.

[0271] The electrochemical performance test results of the sodium ion batteries corresponding to the negative electrode sheets of each embodiment and comparative example are shown in Table 1.

[0272] Table 1 Electrochemical performance test results

[0273]

[0274]

[0275] According to Table 1:

[0276] By comparing Examples 1-13 and Comparative Example 1, it can be seen that the solution of the embodiment of the present application has obvious improvements in the full-charge rebound of the negative electrode plate, the battery cycle life, and the impedance increase ratio after the battery cycle.

[0277] By comparing Example 1 and Comparative Example 2, it can be seen that when the second composite material layer is not included, the expansion rate of the fully charged negative electrode and the increase rate of the internal resistance after 500 cycles are significantly increased, and the capacity retention rate after 500 cycles is reduced.

[0278] By comparing Example 1 and Comparative Examples 3-5, it can be seen that when the contents of the alloy negative electrode material and the first conductive agent in the first composite material layer A 201 and the first composite material layer B 202 do not conform to the rules of the present application, the expansion rate of the fully charged negative electrode and the increase ratio of the internal resistance after 500 cycles both increase significantly, and the capacity retention rate after 500 cycles decreases significantly.

[0279] In summary, the negative electrode pole piece and its preparation method of the present application improve the problem of large expansion of the mixed negative electrode of the first carbon material such as hard carbon and the alloy negative electrode material after sodium embedding in the sodium ion battery; through layered coating, the proportion of the alloy negative electrode material and the first conductive agent in the first composite material layer material away from the current collector and the side close to the current collector is optimized, and the sodium embedding depth of the alloyed negative electrode on the side of the pole piece away from the current collector and the side close to the current collector is optimized, which alleviates the problem of pole piece crushing caused by excessive sodium embedding depth in the surface layer.

[0280] In the present application, the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0281] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0282] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A negative electrode sheet, It is characterized in that A current collector is included, wherein at least one surface of the current collector is sequentially laminated with at least two first composite material layers and a second composite material layer; The materials of all the first composite material layers include a first carbon material, an alloy negative electrode material and a first conductive agent; among the materials of any two adjacent first composite material layers located on the same surface of the current collector, the mass content of the alloy negative electrode material in the material of the first composite material layer close to the current collector is greater than the mass content of the alloy negative electrode material in the material of the first composite material layer close to the second composite material layer, and the mass content of the first conductive agent in the material of the first composite material layer close to the current collector is greater than the mass content of the first conductive agent in the material of the first composite material layer close to the second composite material layer; The material of the second composite material layer includes a second carbon material and a second conductive agent.

2. The negative electrode sheet according to claim 1, It is characterized in that The first carbon material and the second carbon material both include at least one of hard carbon and soft carbon; And / or, the alloy negative electrode material includes at least one of antimony, tin, phosphorus, silicon, bismuth, and germanium; And / or, the first conductive agent and the second conductive agent include at least one of conductive carbon black, superconducting carbon, conductive graphite, carbon nanotubes, and graphene.

3. The negative electrode sheet according to claim 1, It is characterized in that The total mass content of the alloy negative electrode material in the negative electrode plate is greater than 0% and less than 49.5%; And / or, the mass content of the first carbon material in the first composite material layer material is greater than or equal to the mass content of the alloy negative electrode material; and / or, the mass content of the first carbon material in the first composite material layer material is less than or equal to the mass content of the second carbon material in the second composite material layer material; And / or, in the material of the first composite material layer, the mass content of the first conductive agent is 0.4-5.0%; And / or, in the material of the second composite material layer, the mass content of the second conductive agent is 0.5-5.0%.

4. The negative electrode sheet according to claim 3, It is characterized in that The mass content of the first carbon material in the first composite material layer is 49.5-99%; And / or, when the number of layers of the first composite material layer is two, the mass content of the alloy negative electrode material in the first composite material layer is m, 0<m≦49.5%; or, when the number of layers of the first composite material layer is greater than two, the mass content of the alloy negative electrode material in the first composite material layer is n, 0≦n≦49.5%; And / or, the mass content of the second carbon material in the second composite material layer is 90-99%.

5. The negative electrode sheet according to claim 1, It is characterized in that All materials of the first composite material layer further include a first binder; And / or, the material of the second composite material layer further includes a second adhesive.

6. The negative electrode sheet according to claim 5, It is characterized in that In the material of the first composite material layer, the mass content of the first binder is 0.5-5.0%; And / or, in the material of the second composite material layer, the mass content of the second binder is 0.5-5.0%; And / or, the first binder and the second binder both include at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium alginate, and polyvinylidene fluoride.

7. The negative electrode sheet according to any one of claims 1 to 6, It is characterized in that The number of the first composite material layers located on the same surface of the current collector is two, and, In the material of the first composite material layer adjacent to the current collector, the mass contents of the alloy negative electrode material and the first conductive agent are a% and b% respectively; In the material of the first composite material layer adjacent to the second composite material layer, the mass contents of the alloy negative electrode material and the first conductive agent are c% and d% respectively; c, d, a, and b satisfy: 20%≦c / (a+c)<50%, and / or, 20%≦d / (b+d)<50%.

8. The negative electrode sheet according to claim 1, It is characterized in that The at least two first composite material layers and the second composite material layers are sequentially stacked on both opposite sides of the current collector; and / or, the total thickness of all the first composite material layers located on the same surface of the current collector is 60-90 μm; and / or, the total number of the first composite material layers located on the same surface of the current collector is 2-5 layers; and / or, the thickness of the second composite material layer located on the same surface of the current collector is 1-5 μm; And / or, the thickness of the negative electrode plate is 130-210 μm; And / or, the ratio of the surface density of the first composite material layer to the surface density of the second composite material layer is (9-9.9):(0.1-1).

9. A method for preparing a negative electrode sheet according to any one of claims 1 to 8, It is characterized in that include: Prepare the first composite material layer slurry and the second composite material layer slurry respectively; The first composite material layer slurry and the second composite material layer slurry are used as raw materials, and the first composite material layer and the second composite material layer are sequentially formed on at least one surface of the current collector by layered coating.

10. A secondary battery comprising a positive electrode sheet, a separator and a negative electrode sheet, It is characterized in that The negative electrode plate is the negative electrode plate as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Multilayer cathode sheet, method for producing cathode sheet and lithium ion battery

    CN104538584A

  • Negative pole piece, secondary battery and electric equipment

    CN115249793A

  • Multi-layer coated battery pole piece and preparation method thereof

    CN115832203A

  • Negative pole piece, secondary battery, battery module, battery pack and electric device

    CN116034497A

  • Low-expansion silicon-carbon negative electrode and lithium ion battery thereof

    CN217641407U