Positive electrode material and preparation method thereof, positive electrode plate, battery and electric device

By introducing a one-dimensional conductive material and a reducing chalcogenide additive onto the surface of the positive electrode active material of a lithium-ion battery, a CEI film is generated, which solves the problem of residual lithium compounds on the surface of the positive electrode active material and improves the conductivity and electrochemical performance of the battery.

CN118969972AActive Publication Date: 2024-11-15CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310543265.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-15
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

Residual lithium compounds (such as LiOH, Li2O, and Li2CO3) on the surface of the positive electrode active material of lithium-ion batteries lead to poor conductivity, increased interfacial impedance, and deterioration of battery performance.

Method used

One-dimensional conductive materials and reducing chalcogenide additives are introduced onto the surface of the positive electrode active material. Intermediate and final products are generated through redox reactions to form a CEI film, eliminate residual lithium compounds, and construct a conductive network.

Benefits of technology

It improves the conductivity and electrochemical performance of the positive electrode active material, reduces battery polarization, and enhances the battery's cycle stability and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969972A_ABST
    Figure CN118969972A_ABST
Patent Text Reader

Abstract

The invention discloses a positive electrode material and a preparation method thereof, a positive electrode plate, a battery and an electric device. The positive electrode material comprises a positive electrode active substance, and a one-dimensional conductive material and an additive which are distributed on the surface of the positive electrode active substance, at least part of the one-dimensional conductive material is wrapped by the additive, and the additive comprises a reducing chalcogen element. According to the scheme, the additive containing the reducing chalcogenide is introduced to the surface of the positive active material, the additive can effectively remove the residual lithium compound on the surface of the positive active material, meanwhile, the one-dimensional conductive material is also introduced to the surface of the positive active material, and at least part of the one-dimensional conductive material is wrapped by the additive; the additive is anchored by using the one-dimensional conductive material as a carrier, and meanwhile, the one-dimensional conductive material can construct a three-dimensional conductive system, so that the conductivity of the positive electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a positive electrode material and a preparation method thereof, a positive electrode plate, a battery and an electrical device. Background Art

[0002] As a secondary battery, lithium-ion batteries can reversibly convert chemical energy into electrical energy and are an ideal carrier for human use and storage of energy. Since the advent of lithium-ion batteries, they have been widely used due to their advantages such as long life, high energy density and low maintenance cost. Currently, lithium-ion batteries have been used in many fields such as portable electronic devices, new energy vehicles, and energy storage systems.

[0003] As a key factor affecting the performance of lithium-ion batteries, positive electrode active materials often determine the cycle life, energy density and power density of lithium-ion batteries. Affected by the preparation process of positive electrode active materials or the characteristics of positive electrode active materials themselves, residual lithium compounds (RLCs) such as lithium hydroxide, lithium carbonate, lithium oxide, etc. are easily formed on the surface of positive electrode active materials. Usually, residual lithium compounds have poor conductivity, which will increase the impedance of the positive electrode / electrolyte interface, aggravate battery polarization, deteriorate discharge capacity and cycle stability, and have a negative impact on battery performance. Summary of the invention

[0004] In view of the above problems, the embodiments of the present application provide a positive electrode material and a preparation method thereof, a positive electrode plate, a battery and an electrical device, aiming to alleviate the negative impact of residual lithium compounds in the positive electrode active material on battery performance.

[0005] In a first aspect, an embodiment of the present application provides a positive electrode material, comprising: a positive electrode active substance and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active substance, at least a portion of the one-dimensional conductive material is wrapped by the additive, and the additive contains a reducing sulfide element.

[0006] The positive electrode material provided in the embodiment of the present application includes a positive electrode active material, a one-dimensional conductive material and an additive, at least part of the one-dimensional conductive material is wrapped by the additive, the one-dimensional conductive material and the additive are distributed on the surface of the positive electrode active material, and the additive includes a sulfide element with reducing property. By introducing the additive on the surface of the positive electrode active material, the additive includes a sulfide element with reducing property (usually a sulfide element in a low-valent state), the sulfide element with reducing property in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing a sulfide element in an intermediate valence state in situ on the surface of the positive electrode active material, and in the subsequent chemical formation process, the intermediate product continues to Reaction, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate the final products containing high-valent sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. Furthermore, a one-dimensional conductive material is introduced on the surface of the positive electrode active material. Since the one-dimensional conductive material is located on the surface of the positive electrode active material and can overlap with each other to construct a conductive system, the overall conductivity of the material is improved; at the same time, at least part of the one-dimensional conductive material is wrapped by the additive, which can increase the area of ​​physical bonding between the additive and the one-dimensional conductive material. Since the one-dimensional conductive material itself has a high specific surface area, the bonding area between the additive and the one-dimensional carbon material is further increased, and the bonding force between the additive and the one-dimensional conductive material is increased, thereby improving the stability of the bonding between the two and achieving anchoring of the additive. Since the additive is wrapped on the surface of the one-dimensional conductive material, when the one-dimensional conductive material is overlapped together, the additive will also wrap the nodes of the one-dimensional conductive material overlap, so as not to affect the conductive system constructed by the one-dimensional conductive material.

[0007] To sum up, in the embodiments of the present application, the one-dimensional conductive material not only acts as a carrier to anchor the additive, but the one-dimensional conductive material is also distributed on the surface of the positive electrode active material. With the help of the conductive network constructed by the one-dimensional conductive material, the overall conductivity of the positive electrode material is better; in addition, the one-dimensional conductive material has a large specific surface area, which not only promotes the anchoring of the additive but also increases the contact area between the one-dimensional conductive material and the positive electrode active material, thereby accelerating the electron / ion transfer rate on the positive electrode material and the kinetic reaction rate of the sulfide element.

[0008] In some embodiments, the chalcogen element includes at least one of sulfur, selenium, and tellurium.

[0009] The additive is set to contain a reducing sulfide element, the sulfide element includes at least one of sulfur, selenium and tellurium, and the above sulfide element can react with the residual lithium compound, consume the residual lithium compound and promote the growth of the CEI film on the positive electrode, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0010] In some embodiments, the chalcogen element includes sulfur, and the additive includes at least one of elemental sulfur, metal sulfide, polysulfide, sulfur-containing organic polymer or copolymer, and polymerized sulfur.

[0011] The above-mentioned additives all contain sulfur element, and the sulfur element has a low valence. The sulfur element has reducing properties, which is beneficial to eliminate residual lithium compounds on the surface of the positive electrode active material.

[0012] In some embodiments, the additive includes a chalcogen.

[0013] The valence of sulfide elements is zero, and sulfide elements themselves have strong reducing properties, which makes it easy for sulfide elements to eliminate residual lithium compounds. At the same time, the composition of sulfide elements is single. Introducing sulfide elements into the surface of the positive electrode active material can reduce the introduction of other elements, thereby reducing the risk of side reactions.

[0014] In some embodiments, the one-dimensional conductive material comprises a one-dimensional conductive carbon material.

[0015] In addition to having a large comparative area, the one-dimensional conductive carbon material also has a strong adsorption capacity, which enables the one-dimensional conductive carbon material to effectively adsorb additives attached to the surface of the one-dimensional conductive carbon material, enhance the binding ability between the one-dimensional conductive carbon material and the additive, and enhance the anchoring effect of the one-dimensional conductive carbon material on the additive.

[0016] In some embodiments, the one-dimensional conductive carbon material includes at least one of short carbon fiber filaments, nanocarbon fibers, and carbon nanotubes.

[0017] The one-dimensional conductive carbon material has good conductivity, which is conducive to building a more developed conductive network. It also has a large specific surface area, which is conducive to increasing the contact area between the one-dimensional conductive carbon material and the additive and enhancing the anchoring effect on the additive.

[0018] In some embodiments, the short carbon fiber filaments include at least one of PAN-based carbon fiber, phenolic-based carbon fiber, viscose-based carbon fiber, pitch-based carbon fiber, biomass-based carbon fiber, and activated carbon fiber.

[0019] The above-mentioned short carbon fiber filaments not only have good conductivity and large specific surface area, but also the raw materials are easily available and have high cost performance.

[0020] In some embodiments, the short carbon fiber filaments have a diameter of 100 nm-500 nm.

[0021] By setting the diameter of the short carbon fiber filaments to 100nm-500nm, it is beneficial to ensure that the short carbon fiber filaments have a larger specific surface area, thereby improving the anchoring effect on additives. At the same time, the short carbon fiber filaments have good dispersibility, which is beneficial to improving the conductivity of the positive electrode material.

[0022] In some embodiments, the length of the short carbon fiber filaments is 1 μm-5 μm.

[0023] By setting the length of the short carbon fiber filaments to 1μm-5μm, it is beneficial to ensure the contact effect between the short carbon fiber filaments and the surface of the positive electrode active material. At the same time, the short carbon fiber filaments can be well overlapped together to build a conductive network, thereby improving the conductivity of the positive electrode material.

[0024] In some embodiments, based on the total mass of the positive electrode material, the mass percentage of the chalcogen element is 0.02 wt % to 5 wt %.

[0025] By setting the mass percentage of the chalcogen element in the positive electrode material to 0.02wt% to 5wt%, the residual lithium compounds on the surface of the positive electrode active material can be effectively removed, while preventing the excessive chalcogen element from causing an increase in battery polarization.

[0026] In some embodiments, based on the total mass of the positive electrode material, the mass percentage of the one-dimensional conductive material is greater than 0 and less than or equal to 1 wt %.

[0027] By setting the mass percentage of the one-dimensional conductive material in the positive electrode material to be greater than 0 and less than or equal to 1wt%, the positive electrode material has both better conductivity and processing performance.

[0028] In some embodiments, the surface of the positive electrode active material is coated with a coating layer, and the coating layer includes a first sub-coating layer, and the first sub-coating layer includes the one-dimensional conductive material and the additive wrapped on the one-dimensional conductive material.

[0029] By wrapping the one-dimensional conductive material wrapped with the additive on the surface of the positive electrode active material and forming a first sub-coating layer, the additive is conducive to eliminating the residual lithium compounds on the surface of the positive electrode active material, thereby improving the performance of the positive electrode active material.

[0030] In some embodiments, the coating layer also includes a second sub-coating layer, which is arranged on a side of the first sub-coating layer away from the positive electrode active material, and the second sub-coating layer contains a conductive agent and a binder, and the content of the sulfide element in the second sub-coating layer is greater than or equal to 0 and less than the content of the sulfide element in the first sub-coating layer.

[0031] The first sub-coating layer and the second sub-coating layer are sequentially coated on the surface of the positive electrode active material, and the content of the sulfide element in the first sub-coating layer is greater than the content of the sulfide element in the first sub-coating layer. The first sub-coating layer serves as an inner layer, and a one-dimensional conductive material with a high specific surface area is used as a conductive material in the first sub-coating layer, which is conducive to fixing the additive and inhibiting the outward diffusion of the sulfide element. The second sub-coating layer serves as an outer layer, and can use a one-dimensional conductive material as a conductive agent or other carbon materials as a conductive agent, thereby expanding the range of material selection and facilitating cost control. The content of the sulfide element in the second sub-coating layer is less than the content of the sulfide element in the first sub-coating layer. On the one hand, the content of the sulfide element in the second sub-coating layer is reduced, which can reduce the outward diffusion of the sulfide element. At the same time, the outer second sub-coating layer can form a barrier to the inner first sub-coating layer, and alleviate the outward diffusion of the sulfide element in the first sub-coating layer. Because the sulfide element is easy to flow to the negative electrode after outward diffusion, the sulfide element in the negative electrode reacts with the active lithium to cause lithium consumption and reduce the battery capacity.

[0032] In some embodiments, the content of the chalcogen element in the second sub-coating layer is greater than 0, and the coating layer further includes a third sub-coating layer, the third sub-coating layer is coated on the surface of the second sub-coating layer, and the third sub-coating layer contains the conductive agent and the binder.

[0033] The surface of the positive electrode active material is coated with a first sub-coating layer, a second sub-coating layer and a third sub-coating layer in sequence, and the content of chalcogens in each sub-coating layer decreases from the inside to the outside. At the same time, the outermost third sub-coating layer does not contain chalcogens, which can provide a diffusion space for chalcogens, enhance the barrier effect on chalcogens, and confine as many chalcogens as possible inside the positive electrode material.

[0034] In some embodiments, the coating layer has a thickness of 100 nm to 1000 nm.

[0035] By setting the thickness of the coating layer to 100 nm to 1000 nm, the theoretical specific capacity of the positive electrode material can be ensured while the residual lithium compound is effectively removed.

[0036] In some embodiments, based on the total mass of the positive electrode material, the mass percentage of the coating layer is 0.01 wt% to 6 wt%; alternatively, the mass percentage of the coating layer is 0.1 wt% to 1 wt%.

[0037] By setting the mass percentage of the coating layer in the positive electrode material to 0.01wt% to 6wt%, the theoretical specific capacity of the positive electrode material can be ensured while the residual lithium compound is effectively removed.

[0038] In some embodiments, the positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2; optionally, m≥0.9.

[0039] The present invention introduces additives on the surface of nickel-rich active materials, wherein the additives include reducing chalcogens, and the Ni, Co, and Mn in the nickel-rich active materials are Ni 3+ / Ni 2+ 、Co 3+ and Mn 4+ The nickel-rich active material exists in the form of ions, and the reducing sulfide in the additive is easily oxidized by the nickel-rich active material and reacts with the residual lithium compound on the surface of the nickel-rich active material, thereby in situ generating an intermediate product containing the sulfide in an intermediate valence state on the surface of the nickel-rich active material. In the subsequent formation process, the intermediate product continues to react, and the reducing sulfide will continue to be oxidized and react with the residual lithium compound, and finally generate a final product containing the sulfide in a high valence state (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, in the formation process, the final product further forms a positive electrode-electrolyte interface (CEI) film on the surface of the nickel-rich active material, thereby removing the residual lithium compound on the surface of the nickel-rich active material and improving the conductivity and electrochemical properties of the nickel-rich active material. In this process, additional lithium ions are also released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery.

[0040] In some embodiments, the DV50 particle size of the positive electrode active material is 5 μm to 15 μm.

[0041] By setting the DV50 particle size of the positive electrode active material to 5 μm to 15 μm, it can be ensured that the positive electrode material has better processing performance and electrochemical performance.

[0042] In a second aspect, an embodiment of the present application provides a method for preparing a positive electrode material, comprising:

[0043] The one-dimensional conductive material and an additive are mixed to obtain a mixture, wherein the additive comprises a chalcogen element having reducing properties;

[0044] Sintering the mixed material to melt the additive, and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby obtaining a sintered material;

[0045] The sintered material is stirred with the positive electrode active material to obtain the positive electrode material.

[0046] The preparation method of the positive electrode material provided in the embodiment of the present application is to mix a one-dimensional conductive material and an additive and then sinter the mixture to melt the additive, so that at least part of the one-dimensional conductive material is wrapped by the additive, thereby increasing the physical contact area between the additive and the one-dimensional conductive material, and combining the large specific surface area of ​​the one-dimensional conductive material itself, so that the binding ability of the additive and the one-dimensional conductive material is enhanced, and the additive containing the sulfide element is effectively fixed. The sintered material obtained after the sintering treatment is further stirred and mixed with the positive electrode active material, so that the one-dimensional conductive material with the additive wrapped on the surface is distributed on the surface of the positive electrode active material, thereby forming a positive electrode material. Since the one-dimensional conductive material itself has good conductivity, a conductive network is overlapped by the one-dimensional conductive material. Even after the additive is wrapped, the conductive network can be well connected, thereby ensuring the overall conductive effect of the positive electrode material. In addition, the additives wrapped on the surface of the one-dimensional conductive material will contact the positive electrode active material. During this process, the reducing sulfide elements in the additives will undergo redox reactions with the metal cations in the positive electrode active material and consume the residual lithium compounds on the surface of the positive electrode active material to in situ generate intermediate products containing sulfide elements with intermediate valence states (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) on the surface of the positive electrode active material. In the subsequent formation process, the intermediate products continue to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate final products containing sulfide elements with high valence states (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. In the process of converting the reducing sulfide element into the CEI film, additional lithium ions are released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery. In addition, the preparation method of the positive electrode material provided in the embodiment of the present application is simple, easy to operate, and conducive to industrialization.

[0047] In some embodiments, the chalcogen element includes at least one of sulfur, selenium, and tellurium.

[0048] The additive is set to contain a reducing sulfide element, the sulfide element includes at least one of sulfur, selenium and tellurium, and the above sulfide element can react with the residual lithium compound, consume the residual lithium compound and promote the growth of the CEI film on the positive electrode, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0049] In some embodiments, the additive includes a chalcogen.

[0050] The valence of sulfide elements is zero, and sulfide elements themselves have strong reducing properties, which makes it easy for sulfide elements to eliminate residual lithium compounds. At the same time, the composition of sulfide elements is single. Introducing sulfide elements into the surface of the positive electrode active material can reduce the introduction of other elements, thereby reducing the risk of side reactions.

[0051] In some embodiments, the one-dimensional conductive material comprises a one-dimensional conductive carbon material.

[0052] In addition to having a large comparative area, the one-dimensional conductive carbon material also has a strong adsorption capacity, which enables the one-dimensional conductive carbon material to effectively adsorb additives attached to the surface of the one-dimensional conductive carbon material, enhance the binding ability between the one-dimensional conductive carbon material and the additive, and enhance the anchoring effect of the one-dimensional conductive carbon material on the additive.

[0053] In some embodiments, the additive includes elemental sulfur, the sintering temperature is 180° C. to 220° C., and / or the sintering time is 5 h to 7 h.

[0054] By using sulfur as an additive, compared with other additives, the chemical properties of sulfur are more active, the effect of removing residual lithium compounds is better, and the raw materials of sulfur are easy to obtain and low in cost. Using sulfur as an additive is cost-effective. Furthermore, by setting the sintering temperature to 180°C to 220°C, sulfur can exist stably in the form of a molten liquid within this temperature range, and then be coated on the surface of a one-dimensional conductive material. In addition, by setting the sintering time to 5h to 7h, the content of sulfur in the positive electrode material can be effectively controlled, so that sulfur can effectively remove residual lithium compounds without increasing the polarization of the battery.

[0055] In some embodiments, the DV50 particle size of the additive is greater than 0 and less than or equal to 1 μm; optionally, the DV50 particle size of the additive is 100 nm to 500 nm.

[0056] By setting the DV50 particle size of the additive to be greater than 0 and less than or equal to 1 μm, within this range, the dispersion effect of the additive is good, and the combination of the additive and the one-dimensional conductive material is good when the additive is pre-loaded.

[0057] In some embodiments, the mixing process includes ball milling.

[0058] By designing a ball milling process in the mixing process, on the one hand, the restriction on the particle size of the additive before the mixing process can be reduced, and on the other hand, the particle size of the additive can be reduced through the ball milling process, thereby improving the bonding stability between the additive and the one-dimensional conductive material.

[0059] In some embodiments, the stirring process has a rotation speed of 400 r / s to 1000 r / s.

[0060] By setting the rotation speed of the stirring process to 400 r / s to 1000 r / s, the sintering material and the positive electrode active material can be effectively mixed together.

[0061] In some embodiments, the positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2; optionally, m≥0.9.

[0062] The present invention introduces additives on the surface of nickel-rich active materials, wherein the additives include reducing chalcogens, and the Ni, Co, and Mn in the nickel-rich active materials are Ni 3+ / Ni 2+ 、Co 3+ and Mn 4+The nickel-rich active material exists in the form of ions, and the reducing sulfide in the additive is easily oxidized by the nickel-rich active material and reacts with the residual lithium compound on the surface of the nickel-rich active material, thereby in situ generating an intermediate product containing the sulfide in an intermediate valence state on the surface of the nickel-rich active material. In the subsequent formation process, the intermediate product continues to react, and the reducing sulfide will continue to be oxidized and react with the residual lithium compound, and finally generate a final product containing the sulfide in a high valence state (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, in the formation process, the final product further forms a positive electrode-electrolyte interface (CEI) film on the surface of the nickel-rich active material, thereby removing the residual lithium compound on the surface of the nickel-rich active material and improving the conductivity and electrochemical properties of the nickel-rich active material. In this process, additional lithium ions are also released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery.

[0063] In a third aspect, an embodiment of the present application provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode material layer bonded to the positive electrode current collector, wherein the positive electrode material layer comprises the positive electrode material provided in the first aspect of the embodiment of the present application or a positive electrode material prepared by the preparation method of the positive electrode material provided in the second aspect of the embodiment of the present application.

[0064] The positive electrode plate provided in the embodiment of the present application includes a positive electrode current collector and a positive electrode material layer, and the positive electrode material layer includes the above-mentioned positive electrode material, so that the content of residual lithium compounds in the positive electrode plate is low, the overall conductive effect of the positive electrode plate is improved, and the cycle performance is improved.

[0065] In a fourth aspect, an embodiment of the present application provides a battery, comprising the positive electrode plate provided in the third aspect of the embodiment of the present application.

[0066] The battery provided in the embodiment of the present application includes the above-mentioned positive electrode plate, and the battery has stable cycle performance and good rate performance.

[0067] In a fifth aspect, an embodiment of the present application provides an electrical device, comprising the battery provided in the fourth aspect of the embodiment of the present application.

[0068] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the optional embodiments below. The accompanying drawings are only used for the purpose of illustrating the optional embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0070] Figure 1 A schematic diagram of the structure of a vehicle according to some embodiments of the present application;

[0071] Figure 2 A schematic diagram of an exploded structure of a battery according to some embodiments of the present application;

[0072] Figure 3 A schematic diagram of the exploded structure of a battery cell according to some embodiments of the present application;

[0073] Figure 4 This is a schematic diagram of the structure of the electrode assembly of some embodiments of the present application;

[0074] Figure 5 Schematic diagram of the structure of the positive electrode material provided in some embodiments of the present application.

[0075] The reference numerals in the specific implementation manner are as follows:

[0076] 10. Pole piece;

[0077] 20. electrode assembly; 101. negative electrode plate; 102. positive electrode plate; 201. negative electrode tab; 202. positive electrode tab; 203. separator;

[0078] 30. Battery cell; 301. Shell; 302. End cover; 303. Negative electrode adapter; 304. Positive electrode adapter; 305. Insulator;

[0079] 40. battery; 401. box body; 4011. box body; 4012. box cover body;

[0080] 50. electrical device; 501. controller; 502. motor;

[0081] 6. Positive electrode active material particles;

[0082] 71. First sub-cladding layer; 72. Second sub-cladding layer; 73. Third sub-cladding layer. DETAILED DESCRIPTION

[0083] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0084] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0085] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0086] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0087] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0088] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0089] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0090] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0091] As a secondary battery, lithium-ion batteries can reversibly convert chemical energy into electrical energy and are an ideal carrier for human use and storage of energy. Since the advent of lithium-ion batteries, they have been widely used due to their advantages such as long life, high energy density and low maintenance cost. Currently, lithium-ion batteries have been used in many fields such as portable electronic devices, new energy vehicles, and energy storage systems.

[0092] As a key factor affecting the performance of lithium-ion batteries, positive electrode active materials often determine the cycle life, energy density and power density of lithium-ion batteries. Affected by the preparation process of positive electrode active materials or the characteristics of positive electrode active materials themselves, residual lithium compounds (RLCs) such as lithium hydroxide, lithium carbonate, lithium oxide, etc. are easily formed on the surface of positive electrode active materials. Usually, residual lithium compounds have poor conductivity, which will increase the impedance of the positive electrode / electrolyte interface, aggravate battery polarization, deteriorate discharge capacity and cycle stability, and have a negative impact on battery performance.

[0093] The related technology is to reduce the content of residual lithium compounds on the surface of the positive electrode active material by introducing additives containing low-valent sulfide elements on the surface of the positive electrode active material, and utilizing the low-valent sulfide elements in the additives to undergo oxidation-reduction conversion into high-valent sulfide elements during the formation process and react with the residual lithium compounds to remove the residual lithium compounds. However, the introduction of additives containing low-valent sulfide elements not only affects the conductivity of the positive electrode active material, but also the additives themselves have the problem of insufficient anchoring, making the additives easily detached from the positive electrode active material, resulting in insufficient reaction and incomplete removal of residual lithium compounds.

[0094] Based on this, the present application introduces an additive on the surface of the positive electrode active material, wherein the additive includes a reducing sulfide element (usually a low-valent sulfide element), and the reducing sulfide element in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing an intermediate sulfide element on the surface of the positive electrode active material in situ, and in the subsequent chemical process, the intermediate product The substances continue to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate final products containing high-valent sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. Furthermore, a one-dimensional conductive material is introduced on the surface of the positive electrode active material. Since the one-dimensional conductive material is located on the surface of the positive electrode active material and can overlap with each other to construct a conductive system, the overall conductivity of the material is improved; at the same time, at least part of the one-dimensional conductive material is wrapped by the additive, which can increase the area of ​​physical bonding between the additive and the one-dimensional conductive material. At the same time, since the one-dimensional conductive material itself has a high specific surface area, the bonding area between the additive and the one-dimensional conductive material is further increased, and the bonding force between the additive and the one-dimensional conductive material is increased, thereby improving the stability of the bonding between the two and achieving anchoring of the additive. Since the additive is wrapped on the surface of the one-dimensional conductive material, when the one-dimensional conductive material is overlapped together, the additive will also wrap the nodes of the one-dimensional conductive material overlap, so as not to affect the conductive system constructed by the one-dimensional conductive material.

[0095] The batteries disclosed in some embodiments of the present application may be used, but not limited to, in electrical devices such as vehicles, ships, or aircraft. A power supply system having the batteries disclosed in the present application and the like may be used to form the electrical device.

[0096] Some embodiments of the present application provide an electric device using a battery as a power source, and the electric device may be, but is not limited to, a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, an electric tool, etc. The vehicle may be, but is not limited to, a fuel vehicle, a gas vehicle, or a new energy vehicle, and the new energy vehicle may be, but is not limited to, a pure electric vehicle, a hybrid vehicle, or an extended-range vehicle, etc.; the spacecraft includes an airplane, a rocket, a space shuttle, and a spacecraft, etc.; the electric toy includes a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc.; the electric tool includes a metal cutting electric tool, a grinding electric tool, an assembly electric tool, and a railway electric tool, such as an electric drill, an electric grinder, an electric wrench, an electric screwdriver, an electric hammer, an impact drill, a concrete vibrator, and an electric planer, etc.

[0097] For the convenience of description, the following embodiments are described by taking a vehicle as an example of an electrical device in an embodiment of the present application.

[0098] Please refer to Figure 1 , Figure 1 A schematic diagram of the structure of a vehicle provided for some embodiments of the present application. A battery 40 is provided inside the vehicle, and the battery 40 can be provided at the bottom, head, or tail of the vehicle. The battery 40 can be used to power the vehicle, for example, the battery 40 can be used as an operating power source for the vehicle. The vehicle can also include a controller 501 and a motor 502, and the controller 501 is used to control the battery 40 to power the motor 502, for example, for starting, navigating, and operating power requirements of the vehicle during driving.

[0099] In some embodiments of the present application, the battery 40 can be used not only as an operating power source for the vehicle, but also as a driving power source for the vehicle, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle.

[0100] In some embodiments of the present application, the battery 40 is a secondary battery, which has many different forms, including but not limited to battery cells, battery modules, and battery packs, etc. A secondary battery here refers to a battery that can be used continuously by activating the active material by charging after the battery is discharged.

[0101] Please refer to Figure 2 , Figure 2 The exploded view of the battery 40 provided in some embodiments of the present application. The battery 40 includes a box body 401 and a battery cell 30, and the battery cell 30 is accommodated in the box body 401. The box body 401 is a component used to provide a space for accommodating the battery cell 30, and the box body 401 can adopt a variety of structures.

[0102] In some embodiments, the box body 401 may include a box body 4011 and a box cover 4012, which cover each other and define a storage space for accommodating the battery cell 30. Optionally, the box body 4011 may be a hollow structure with one end open, and the box cover 4012 may be a plate-like structure, and the box cover 4012 covers the open side of the box body 4011.

[0103] In the battery 40, there can be multiple battery cells 30, and the multiple battery cells 30 can be connected in series, in parallel, or in a mixed connection. Mixed connection means that multiple battery cells 30 are both connected in series and in parallel. Multiple battery cells 30 can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 30 is accommodated in the box 401; of course, the battery 40 can also be a battery module formed by connecting multiple battery cells 30 in series, in parallel, or in a mixed connection, and then the multiple battery modules are connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the box 401. The battery 40 may also include other structures, such as a confluence component (not shown), which is used to realize the electrical connection between the multiple battery cells 30. Among them, the battery cells 30 may be cylindrical, flat, rectangular, or in other shapes.

[0104] Please refer to Figure 3 , Figure 3 1 is an exploded view of a battery cell 30 in some embodiments of the present application. The battery cell 30 refers to a basic unit for realizing the mutual conversion between chemical energy and electrical energy, and is also the smallest unit of a battery. Figure 3 The battery cell 30 includes a shell 301, an end cover 302, an electrode assembly 20 and other functional components.

[0105] The shell 301 is a hollow structure with one end open. The shell 301 is used to cooperate with the end cap 302 to form an internal environment for accommodating the electrode assembly 20, the electrolyte and other functional components. The shell 301 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism shape, etc. Specifically, the shape of the shell 301 can be determined according to the specific shape and size of the electrode assembly 20. The material of the shell 301 can be but not limited to copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., which is not limited here.

[0106] The end cap 302 refers to a component that covers the opening of the shell 301 to isolate the internal environment of the battery cell 30 from the external environment. Optionally, the shape of the end cap 302 can be adapted to the shape of the shell 301 to match the shell 301. Optionally, the end cap 302 can be made of a material with a certain hardness and strength (such as aluminum alloy), so that the end cap 302 is not easily deformed when squeezed and collided, so that the battery cell 30 can have a higher structural strength and the safety performance can also be improved. The material of the end cap 302 can be but not limited to copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., which is not limited here.

[0107] In some embodiments, the battery cell 30 further includes functional components such as a negative electrode adapter 303 and a positive electrode adapter 304, wherein the negative electrode adapter 303 is used to electrically connect to the negative electrode tab on the electrode assembly 20, and the positive electrode adapter 304 is used to electrically connect to the positive electrode tab on the electrode assembly 20, so as to output or input the electric energy of the battery cell 30. It can be understood that the negative electrode adapter 303 is made of a conductive material, and the material of the negative electrode adapter 303 can be but not limited to copper, iron, aluminum, etc. The positive electrode adapter 304 is made of a conductive material, and the material of the positive electrode adapter 304 can be but not limited to copper, iron, aluminum, etc.

[0108] In some embodiments, the battery cell 30 further includes an insulating member 305, which is located inside the housing 301 to isolate the housing 301 from the electrode assembly 20 and reduce the risk of short circuit. For example, the insulating member 305 may be plastic, rubber, or the like.

[0109] One or more electrode assemblies 20 may be contained in the housing 301 .

[0110] Please refer to Figure 4 , Figure 4 Schematic diagram of the structure of the electrode assembly 20 in some embodiments of the present application. The electrode assembly 20 is a component in the battery cell 30 where electrochemical reactions occur. The electrode assembly 20 is mainly formed by winding or stacking a negative electrode sheet 101 and a positive electrode sheet 102 as an integrated electrode sheet structure, and a separator 203 is usually provided between adjacent negative electrode sheets 101 and positive electrode sheets 102.

[0111] The negative electrode sheet 101 includes a negative electrode current collector and a negative electrode material layer, and the negative electrode material layer is coated on the surface of the negative electrode current collector. Taking a lithium-ion battery as an example, the material of the negative electrode current collector may include copper, the negative electrode material layer includes a negative electrode material, and the negative electrode material may include a silicon-based material.

[0112] The positive electrode sheet 102 includes a positive current collector and a positive electrode material layer, and the positive electrode material layer is coated on the surface of the positive current collector. Taking a lithium-ion battery as an example, the material of the positive current collector may include aluminum, and the positive electrode material layer includes a positive electrode material, and the positive electrode material may include lithium cobalt oxide, lithium iron phosphate, ternary lithium or lithium manganese oxide.

[0113] The isolation membrane 203 is a porous plastic film that allows lithium ions in the electrolyte to pass freely, but isolates the negative electrode plate 101 and the positive electrode plate 102, so that electrons inside the battery cannot pass freely.

[0114] There are also parts of the negative electrode current collector and the positive electrode current collector that are not coated with the active material layer, and these parts without the active material layer are provided with connecting tabs. Specifically, the negative electrode current collector is connected to the negative electrode tab 201, and the positive electrode current collector is connected to the positive electrode tab 202. During the charge and discharge process of the battery, the positive electrode material layer and the negative electrode material layer react with the electrolyte, the tab 201 is connected to the negative electrode adapter 303 and the positive electrode tab 202 is connected to the positive electrode adapter 304 to form a current loop. Of course, in some embodiments, the parts of the negative electrode current collector and the positive electrode current collector that are not coated with the active material layer each constitute a tab.

[0115] Some embodiments of the present application provide a positive electrode material, a positive electrode active material, and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active material, at least part of the one-dimensional conductive material is wrapped by the additive, and the additive contains a reducing sulfide element.

[0116] The positive electrode material includes a positive electrode active material, which refers to a compound with a three-dimensional lithium ion channel, which is used on the positive electrode for reversible insertion and removal of lithium ions. Optionally, the positive electrode active material includes but is not limited to at least one of lithium nickel cobalt oxide, lithium nickel manganese oxide and lithium nickel cobalt manganese oxide. Lithium nickel cobalt oxide (LiNi 1-x Co x O2, referred to as NC binary material) is a layered structure with good electrochemical performance and thermal stability. x Mn 2-xO4, referred to as NM binary material) is a material with a spinel structure prepared based on the improvement of the original spinel lithium manganese oxide. Compared with lithium manganese oxide, it has higher cycle stability and voltage platform. Nickel cobalt manganese oxide (referred to as NCM ternary material) contains three transition metal elements Ni, Co and Mn. It effectively overcomes the shortcomings of the three materials LiNiO2, LiCoO2 and LiMnO2, and in the electrochemical performance and thermal stability tests, these three transition metals can show their own characteristics in this material, and have high development potential. Optionally, the positive active material can also be doped and modified. Optionally, the doping elements include but are not limited to at least one of Zr, Zn, Cu, V, Ti, Sr, Sb, Y, W, Nb, B, Ba, Ce, Si, Ga, Sn, Mo, P, Al, Fe, Mg, Cr, F, N, S, and Cl.

[0117] One-dimensional conductive materials refer to fibrous or tubular materials in which electrons can move freely in only one non-nanoscale direction. One-dimensional conductive materials include, but are not limited to, metal nanowires and one-dimensional conductive carbon materials. Metal nanowires include, but are not limited to, silver nanowires, copper nanowires, etc. One-dimensional conductive carbon materials can be one-dimensional nanocarbon materials or one-dimensional micron carbon materials. Optionally, the one-dimensional conductive carbon material includes at least one of carbon fibers, nanocarbon fibers, and carbon nanotubes.

[0118] The additive includes a chalcogen with reducing properties, where the chalcogen refers to sulfur and elements with similar chemical properties to sulfur. Optionally, the chalcogen includes elements other than oxygen in the oxygen group. Optionally, the chalcogen includes at least one of sulfur (S), selenium (Se) and tellurium (Te). The additive includes a chalcogen, where the additive can be a compound, with the chalcogen as one of the constituent elements of the compound, and the additive can also be a single substance, such as a chalcogen itself used as an additive. Chalcogen has reducing properties, that is, the chalcogen can increase the valence state through oxidation-reduction reactions. Optionally, the valence of the chalcogen is less than or equal to zero, that is, a low-valent chalcogen, and the chalcogen is easily oxidized to a high-valent chalcogen. As an example, the chalcogen includes sulfur, the valence of low-valent sulfur is -2 or zero, and the valence of high-valent sulfur is +6 or +4.

[0119] The one-dimensional conductive material and additives are distributed on the surface of the positive electrode active material. The one-dimensional conductive material and additives may be loosely distributed on the surface of the positive electrode active material, or the one-dimensional conductive material and additives may form a coating layer wrapped around the surface of the positive electrode active material.

[0120] At least part of the one-dimensional conductive material is wrapped by the additive, which means that at least part of the surface of the one-dimensional conductive material is covered with the additive. The additive may be attached to the surface of the one-dimensional conductive material in the form of a film layer, so that the additive and the one-dimensional conductive material form a skin-core structure, wherein the one-dimensional conductive material is the core layer and the additive is the skin layer; or the additive may be formed as a substrate layer, and the one-dimensional conductive material is at least partially embedded in the substrate layer and forms a conductive network structure. As an example, the additive may be melted and solidified on the surface of the one-dimensional conductive material, so that the additive is wrapped and covered on the surface of the one-dimensional conductive material. As an example, the additive may be sublimated into a gaseous state and solidified on the surface of the one-dimensional conductive material, so that the additive is wrapped on the surface of the one-dimensional conductive material. Here, the additive is wrapped on the surface of the one-dimensional conductive material. For a single one-dimensional conductive material, the surface of the one-dimensional conductive material may be completely wrapped by the additive, or part of the surface of the one-dimensional conductive material may be wrapped by the additive. For example, when the additive content is low, most of the surface of the one-dimensional conductive material may be wrapped by the additive, and a small part of the surface of the one-dimensional conductive material may be exposed, or the additive content is high but affected by the process, there is a small part of the surface of the one-dimensional conductive material that is not wrapped with the additive and is exposed. At least part of the one-dimensional conductive material is wrapped by the additive. This refers to all the one-dimensional conductive materials. Part of the one-dimensional conductive material may be wrapped by the additive, or all of the one-dimensional conductive material (ie, every one-dimensional conductive material) may be wrapped by the additive.

[0121] The positive electrode material provided in the embodiment of the present application includes a positive electrode active material, a one-dimensional conductive material and an additive, at least part of the one-dimensional conductive material is wrapped by the additive, the one-dimensional conductive material and the additive are distributed on the surface of the positive electrode active material, and the additive includes a sulfide element with reducing property. By introducing the additive on the surface of the positive electrode active material, the additive includes a sulfide element with reducing property (usually a sulfide element in a low-valent state), the sulfide element with reducing property in the additive is easily oxidized and reacts with the residual lithium compound (such as LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material to generate an intermediate product (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) containing a sulfide element in an intermediate valence state in situ on the surface of the positive electrode active material, and in the subsequent chemical formation process, the intermediate product continues to Reaction, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate the final products containing high-valent sulfide elements (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. Furthermore, a one-dimensional conductive material is introduced on the surface of the positive electrode active material. Since the one-dimensional conductive material is located on the surface of the positive electrode active material and can overlap with each other to construct a conductive system, the overall conductivity of the material is improved; at the same time, at least part of the one-dimensional conductive material is wrapped in the additive, which can increase the area of ​​physical bonding between the additive and the one-dimensional conductive material. At the same time, since the one-dimensional conductive material itself has a high specific surface area, the bonding area between the additive and the one-dimensional conductive material is further increased, and the bonding force between the additive and the one-dimensional conductive material is increased, thereby improving the stability of the bonding between the two and achieving anchoring of the additive. Since the additive is wrapped on the surface of the one-dimensional conductive material, when the one-dimensional conductive material is overlapped together, the additive will also wrap the nodes of the one-dimensional conductive material overlap, so as not to affect the conductive system constructed by the one-dimensional conductive material.

[0122] To sum up, in the embodiments of the present application, the one-dimensional conductive material not only acts as a carrier to anchor the additive, but the one-dimensional conductive material is also distributed on the surface of the positive electrode active material. With the help of the conductive network constructed by the one-dimensional conductive material, the overall conductivity of the positive electrode material is better; in addition, the one-dimensional conductive material has a large specific surface area, which not only promotes the anchoring of the additive, but also increases the contact area between the one-dimensional conductive material and the positive electrode active material, thereby accelerating the electron / ion transfer rate on the positive electrode material and the kinetic reaction rate of the sulfide element.

[0123] In some embodiments, the chalcogen element includes at least one of sulfur, selenium, and tellurium.

[0124] Optionally, the chalcogen element includes sulfur, that is, the additive contains a reducing sulfur element. As an example, the additive is sulfur element, and the positive electrode material is obtained by introducing sulfur element S and a one-dimensional conductive material into the surface of the positive electrode active material (e.g., nickel-rich active material). Part of the sulfur element S in the positive electrode material will undergo an oxidation-reduction reaction with the metal cations in the positive electrode active material, and the residual lithium compounds (e.g., LiOH, Li2O, Li2CO3, etc.) on the surface of the positive electrode active material will also participate in the reaction. In this process, the sulfur element S is oxidized and combined with the residual lithium compound to form Li2S2O3. The positive electrode material is further prepared into a positive electrode sheet and applied to the battery. During the formation of the battery, Li2S2O3 will be further oxidized and converted into Li2SO3 and / or Li2SO4. At the same time, the sulfur element S in the positive electrode material will continue to react with the residual lithium compound to generate Li2SO3 and / or Li2SO4. During the formation process, the battery is charged and discharged, and a CEI film is formed on the positive electrode of the battery. Li2SO3 and / or Li2SO4 can participate in the growth of the CEI film, thereby converting residual lithium compounds that have a negative impact on battery performance into a CEI film, thereby improving the electrochemical performance of the battery. In addition, when sulfur element S reacts with residual lithium compounds and generates Li2SO3 and / or Li2SO4, additional lithium ions are usually released. The lithium ions can be used to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery.

[0125] Optionally, the chalcogen element includes tellurium, that is, the additive contains a reducible tellurium element. As an example, the additive is tellurium element, and the positive electrode material is obtained by introducing tellurium element Te and a one-dimensional conductive material into the surface of the positive electrode active material (e.g., nickel-rich active material). Similar to sulfur element S, part of the tellurium element Te in the positive electrode material first combines with the residual lithium compound to form Li2Te2O3, and in the subsequent battery formation process, Li2Te2O3 and tellurium element Te are further converted into Li2TeO3 and / or Li2TeO4 and participate in the growth of CEI film, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of SEI film, thereby ensuring the capacity of the battery.

[0126] Optionally, the chalcogen includes selenium, that is, the additive includes selenium with reducing properties. As an example, the additive is selenium element, and the positive electrode material is obtained by introducing selenium element Se and a one-dimensional conductive material into the surface of the positive electrode active material (e.g., nickel-rich active material). Similar to sulfur element S, part of the selenium element Se in the positive electrode material first combines with the residual lithium compound to form Li2Se2O3, and in the subsequent battery formation process, Li2Se2O3 and selenium element Se are further converted into Li2SeO3 and / or Li2SeO4 and participate in the growth of CEI film, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of SEI film, thereby ensuring the capacity of the battery.

[0127] Optionally, the chalcogen element includes selenium and sulfur. Optionally, the chalcogen element includes sulfur and tellurium. Optionally, the chalcogen element includes selenium and tellurium. Optionally, the chalcogen element includes sulfur, selenium and tellurium.

[0128] The additive is set to contain a reducing sulfide element, the sulfide element includes at least one of sulfur, selenium and tellurium, and the above sulfide element can react with the residual lithium compound, consume the residual lithium compound and promote the growth of the CEI film on the positive electrode, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film in the battery, thereby ensuring the capacity of the battery.

[0129] In some embodiments, the chalcogen element includes elemental sulfur, and the additive includes at least one of elemental sulfur, metal sulfide, polysulfide, sulfur-containing organic polymer or copolymer, and polymerized sulfur.

[0130] Sulfur elements include sulfur elements, that is, the additive contains sulfur elements, and the additive can be a sulfur element or a sulfur-containing compound. Optionally, the sulfur-containing compound includes metal sulfides. Optionally, the metal sulfides include transition metal sulfides, and the basic chemical formula of transition metal sulfides (TMDs) is MS2, where M represents transition metal elements, including Ti, V, Ta, Mo, W, Re, etc. Optionally, the sulfur-containing compound includes polysulfides, which are compounds containing polysulfide ions. Optionally, the polysulfide is a polysulfide of an alkali metal or an alkaline earth metal. Optionally, the polysulfide includes lithium polysulfide (Li2S n , wherein n=2-8). Optionally, the sulfur-containing compound includes a sulfur-containing organic polymer or copolymer. Optionally, the sulfur-containing compound includes polymerized sulfur, which is a product obtained by polymerization reaction of sulfur element and organic matter at high temperature.

[0131] The above-mentioned additives all contain sulfur element, and the sulfur element has a low valence. The sulfur element has reducing properties, which is beneficial to eliminate residual lithium compounds on the surface of the positive electrode active material.

[0132] In some embodiments, the additive includes a chalcogen.

[0133] The additive includes a chalcogen element, and optionally, the chalcogen element includes at least one of sulfur, selenium and tellurium. Then the additive includes at least one of sulfur, selenium and tellurium.

[0134] The valence of sulfide elements is zero, and sulfide elements themselves have strong reducing properties, which makes it easy for sulfide elements to eliminate residual lithium compounds. At the same time, the composition of sulfide elements is single. Introducing sulfide elements into the surface of the positive electrode active material can reduce the introduction of other elements, thereby reducing the risk of side reactions.

[0135] In some embodiments, the one-dimensional conductive material includes a one-dimensional conductive carbon material.

[0136] One-dimensional conductive carbon materials refer to fibrous or tubular carbon materials in which electrons can move freely in only one non-nanoscale direction.

[0137] In addition to having a large comparative area, the one-dimensional conductive carbon material also has a strong adsorption capacity, which enables the one-dimensional conductive carbon material to effectively adsorb additives attached to the surface of the one-dimensional conductive carbon material, enhance the binding ability between the one-dimensional conductive carbon material and the additive, and enhance the anchoring effect of the one-dimensional conductive carbon material on the additive.

[0138] In some embodiments, the one-dimensional conductive carbon material includes at least one of short carbon fiber filaments, nanocarbon fibers, and carbon nanotubes.

[0139] Short carbon fiber filaments refer to carbon fiber filaments with shorter length and smaller diameter. Optionally, the length of the short carbon fiber filaments is less than 10 microns. Optionally, the diameter of the short carbon fiber filaments is less than 1 micron.

[0140] Nanocarbon fiber is also called carbon nanofiber (CNF), which has a diameter of 50nm to 500nm and a length of 50μm to 100μm. It is a one-dimensional conductive carbon material between carbon nanotubes and ordinary carbon fibers.

[0141] Carbon nanotubes (CNTs) are tubular nanoscale graphite crystals, which are seamless nanoscale tubes formed by single or multi-layer graphite sheets curled around a central axis at a certain helical angle. The diameter of carbon nanotubes is usually less than 50nm.

[0142] The one-dimensional conductive carbon material has good conductivity, which is conducive to building a more developed conductive network. It also has a large specific surface area, which is conducive to increasing the contact area between the one-dimensional conductive carbon material and the additive and enhancing the anchoring effect on the additive.

[0143] In some embodiments, the short carbon fiber filaments include at least one of PAN-based carbon fiber, phenolic-based carbon fiber, viscose-based carbon fiber, pitch-based carbon fiber, biomass-based carbon fiber, and activated carbon fiber.

[0144] PAN-based carbon fiber is made of polyurethane (PA) and nylon (N) through high-temperature hot solid-liquid phase polymerization.

[0145] Phenolic carbon fiber is an amorphous carbon fiber made from phenolic precursor.

[0146] Viscose-based carbon fiber refers to carbon fiber prepared by pre-oxidation and carbonization of viscose fiber.

[0147] Pitch-based carbon fiber refers to a type of carbon fiber that is made from materials rich in polycyclic aromatic hydrocarbons such as asphalt through polymerization, spinning, infusibility, and carbonization treatment.

[0148] Bio-based carbon fibers are made from cellulose and lignin, which come from trees.

[0149] Activated carbon fiber is an activated carbon fiber. Specifically, a certain carbon fiber (such as phenolic-based fiber, PAN-based fiber, viscose-based fiber, asphalt-based fiber, etc.) is activated at high temperature (different activation methods have different activation temperatures) to produce nano-scale pores on its surface and increase the specific surface area.

[0150] The above-mentioned short carbon fiber filaments not only have good conductivity and large specific surface area, but also the raw materials are easily available and have high cost performance.

[0151] In some embodiments, the diameter of the short carbon fiber filaments is 100 nm to 500 nm.

[0152] Generally, the diameter of short carbon fiber filaments will affect the specific surface area of ​​the short carbon fiber filaments. The smaller the diameter of the short carbon fiber filaments, the larger the specific surface area of ​​the short carbon fiber filaments. However, if the diameter of the short carbon fiber filaments is too small, it will cause the short carbon fiber filaments to aggregate, which is not conducive to the dispersion of the short carbon fiber filaments. Instead, it will affect the construction of the conductive system, and thus affect the conductivity of the positive electrode material.

[0153] Optionally, the diameter of the short carbon fiber filaments is any value among 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm and 500 nm, or a range value between any two values.

[0154] By setting the diameter of the short carbon fiber filaments to 100nm-500nm, it is beneficial to ensure that the short carbon fiber filaments have a larger specific surface area, thereby improving the anchoring effect on additives. At the same time, the short carbon fiber filaments have good dispersibility, which is beneficial to improving the conductivity of the positive electrode material.

[0155] In some embodiments, the short carbon fiber filaments have a length of 1 μm to 5 μm.

[0156] The longer the short carbon fiber filaments are, the easier it is for them to entangle and overlap together, thereby building a three-dimensional conductive network. However, the positive electrode active material is usually granular, and the short carbon fiber filaments are distributed on the surface of the positive electrode active material. If the short carbon fiber filaments are too long, it will be unfavorable for the short carbon fiber filaments to contact with the positive electrode active material, affecting the transmission of current between different materials; if the short carbon fiber filaments are too short, it will affect the overlapping effect between the short carbon fiber filaments, especially after the short carbon fiber filaments are wrapped with additives, the short carbon fiber filaments are easily completely wrapped by the additives to produce conductive dead corners, thereby reducing the conductive effect of the positive electrode material.

[0157] Optionally, the length of the short carbon fiber filaments is any value among 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm and 5 μm, or a range value between any two values.

[0158] By setting the length of the short carbon fiber filaments to 1μm-5μm, it is beneficial to ensure the contact effect between the short carbon fiber filaments and the surface of the positive electrode active material. At the same time, the short carbon fiber filaments can be well overlapped together to build a conductive network, thereby improving the conductivity of the positive electrode material.

[0159] In some embodiments, based on the total mass of the positive electrode material, the mass percentage of the chalcogen element is 0.02 wt % to 5 wt %.

[0160] The content of sulfide in the positive electrode material will affect the removal effect of residual lithium compounds. When the content of sulfide in the positive electrode material is too low, especially when the mass percentage of sulfide in the positive electrode material is less than 0.02wt%, the residual lithium compounds on the surface of the positive electrode active material are difficult to be eliminated, and the presence of residual lithium compounds will affect the conductivity of the positive electrode material, and will also cause side reactions, thereby causing the battery's cycle stability to deteriorate. Generally, the greater the amount of sulfide loaded in the positive electrode material, the more conducive it is for the sulfide to be dispersed on the surface of the positive electrode active material and to react with the residual lithium compounds to eliminate the residual lithium compounds. However, when the mass percentage of sulfide in the positive electrode material is greater than 5wt%, it is easy to cause additive residues, reduce the conductivity of the positive electrode material, increase battery polarization, increase the battery internal resistance (DRC), and continue to consume the active lithium inside the battery during battery storage, and the battery performance will deteriorate.

[0161] Optionally, based on the total mass of the positive electrode material, the mass percentage of the sulfide element is any point value among 0.02wt%, 0.05wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% and 5wt%, or a range value between any two points.

[0162] By setting the mass percentage of the chalcogen element in the positive electrode material to 0.02wt% to 5wt%, the residual lithium compounds on the surface of the positive electrode active material can be effectively removed, while preventing the excessive chalcogen element from causing an increase in battery polarization.

[0163] In some embodiments, based on the total mass of the positive electrode material, the mass percentage of the one-dimensional conductive material is greater than 0 and less than or equal to 1 wt %.

[0164] One-dimensional conductive materials are mainly used to improve the conductivity of positive electrode materials. The higher the content of one-dimensional conductive materials in the positive electrode material, the better the conductivity of the positive electrode material. However, the one-dimensional conductive material itself is easy to agglomerate. If the content of one-dimensional conductive materials in the positive electrode material is too high, especially when the content of one-dimensional conductive materials in the positive electrode material is greater than 1wt%, it will easily lead to an increase in the surface energy of the positive electrode material particles, physical gelation will easily occur, and the processing performance of the positive electrode material will deteriorate.

[0165] Optionally, based on the total mass of the positive electrode material, the mass percentage of the one-dimensional conductive material is any point value among 0.001wt%, 0.05wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% and 1wt%, or the range value between any two points.

[0166] By setting the mass percentage of the one-dimensional conductive material in the positive electrode material to be greater than 0 and less than or equal to 1wt%, the positive electrode material has both better conductivity and processing performance.

[0167] See also Figure 5 In some embodiments, the surface of the positive electrode active material is coated with a coating layer, and the coating layer includes a first sub-coating layer 71, and the first sub-coating layer 71 includes a one-dimensional conductive material and an additive wrapped on the one-dimensional conductive material.

[0168] Specifically, the positive electrode active material includes positive electrode active material particles 6, and the one-dimensional conductive material and the additive are distributed on the surface of the positive electrode active material. The one-dimensional conductive material and the additive are wrapped on the surface of the positive electrode active material particles 6 and form a coating layer. For the sake of distinction, the coating layer including the one-dimensional conductive material and the additive wrapped on the one-dimensional conductive material is defined as the first sub-coating layer 71. The coating layer includes the first sub-coating layer 71. In some embodiments, the coating layer may only include the first sub-coating layer 71. In other embodiments, the coating layer may also include other sub-coating layers.

[0169] By wrapping the one-dimensional conductive material wrapped with the additive on the surface of the positive electrode active material and forming the first sub-coating layer 71, the additive is helpful to eliminate the residual lithium compounds on the surface of the positive electrode active material, thereby improving the performance of the positive electrode active material.

[0170] See also Figure 5 In some embodiments, the coating layer further includes a second sub-coating layer 72, which is disposed on a side of the first sub-coating layer 71 away from the positive electrode active material. The second sub-coating layer 72 contains a conductive agent, a binder and an additive. The content of the sulfide element in the second sub-coating layer 72 is greater than or equal to 0 and less than the content of the sulfide element in the first sub-coating layer 71.

[0171] Specifically, the coating layer includes at least two sub-coating layers, namely, a first sub-coating layer 71 and a second sub-coating layer 72, wherein the first sub-coating layer 71 is directly coated on the surface of the positive electrode active material particles 6, and the second sub-coating layer 72 is arranged on the outside of the first sub-coating layer 71, that is, the first sub-coating layer 71 is arranged between the positive electrode active material particles 6 and the second sub-coating layer 72. Here, the first sub-coating layer 71 and the second sub-coating layer 72 can be in direct contact or can be arranged at intervals. Further, the second sub-coating layer 72 contains a conductive agent, a binder and an additive. The conductive agent in the second sub-coating layer 72 includes but is not limited to at least one of conductive carbon black, carbon nanotubes, conductive graphite, graphene, acetylene black and nano-carbon fibers. That is to say, the conductive agent in the second sub-coating layer 72 can be selected from the above-mentioned one-dimensional conductive material, or other conductive materials can be used, which increases the material selection range of the second sub-coating layer 72, which is conducive to controlling the cost of the positive electrode material. The binder in the second sub-coating layer 72 is used to bond the conductive agent and the additive together and further bond with the first sub-coating layer 71. The binder includes but is not limited to at least one of polyvinylidene fluoride, copolymer of vinylidene fluoride-fluorinated olefin, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl acrylate, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyurethane, fluorinated rubber and polyvinyl alcohol. The content of chalcogen in the second sub-coating layer 72 is greater than or equal to 0 and less than the content of chalcogen in the first sub-coating layer 71. It can be understood that the second sub-coating layer 72 may contain additives (i.e., the content of chalcogen is greater than 0) or may not contain additives (i.e., the content of chalcogen is equal to 0). When the second sub-coating layer 72 contains additives, the content of chalcogen in the second sub-coating layer 72 is less than the content of chalcogen in the first sub-coating layer 71.

[0172] The first sub-coating layer 71 and the second sub-coating layer 72 are sequentially coated on the surface of the positive electrode active material, and the content of the chalcogen in the first sub-coating layer 71 is greater than the content of the chalcogen in the second sub-coating layer 71. The first sub-coating layer 71 is used as an inner layer, and a one-dimensional conductive material with a high specific surface area is used as a conductive material in the first sub-coating layer 71, which is conducive to fixing the additive and inhibiting the chalcogen from diffusing outward. The second sub-coating layer 72 is used as an outer layer, which can use a one-dimensional conductive material as a conductive agent or other carbon materials as a conductive agent, thereby expanding the The material selection range is expanded, which is beneficial to control costs. The content of sulfide in the second sub-coating layer 72 is less than that in the first sub-coating layer 71. On the one hand, the content of sulfide in the second sub-coating layer 72 is reduced, which can reduce the outward diffusion of sulfide. At the same time, the outer second sub-coating layer 72 can form a barrier to the inner first sub-coating layer 71, alleviating the outward diffusion of sulfide in the first sub-coating layer 71. Because the sulfide is easy to flow to the negative electrode after diffusing outward, the sulfide reacts with the active lithium at the negative electrode to cause lithium consumption, thereby reducing the battery capacity.

[0173] See also Figure 5 In some embodiments, the content of chalcogen in the second sub-coating layer 72 is greater than 0, and the coating layer further includes a third sub-coating layer 73, which is coated on the surface of the second sub-coating layer 72, and the third sub-coating layer 73 contains a conductive agent and a binder.

[0174] Specifically, the coating layer includes at least three sub-coating layers, namely, a first sub-coating layer 71, a second sub-coating layer and a third sub-coating layer 73, wherein the second sub-coating layer 72 contains additives, while the third sub-coating layer 73 does not contain additives. The third sub-coating layer 73 contains a conductive agent and a binder.

[0175] The surface of the positive electrode active material is coated with a first sub-coating layer 71, a second sub-coating layer and a third sub-coating layer 73 in sequence, and the content of chalcogen in each sub-coating layer decreases from the inside to the outside. At the same time, the outermost third sub-coating layer 73 does not contain chalcogen, which can provide a diffusion space for chalcogen, enhance the barrier effect on chalcogen, and confine as much chalcogen as possible inside the positive electrode material.

[0176] In some embodiments, the coating layer has a thickness of 100 nm to 1000 nm.

[0177] The thickness of the coating layer refers to the total thickness of the coating layer. When the coating layer includes multiple sub-coating layers, the thickness of the coating layer is the sum of the thicknesses of the respective coating layers. As an example, when the coating layer includes only the first sub-coating layer 71, the thickness of the coating layer is the thickness of the first sub-coating layer 71. As an example, when the coating layer includes the first sub-coating layer 71, the second sub-coating layer and the third sub-coating layer 73, the thickness of the coating layer is the sum of the thicknesses of the above three.

[0178] The coating layer mainly contains conductive materials and additives, which have almost no contribution to the battery capacity. If the thickness of the coating layer is too large, the theoretical specific capacity of the positive electrode material will be reduced. If the thickness of the coating layer is too small, the coating will be uneven, thereby affecting the removal effect of the residual lithium compound. Optionally, the thickness of the coating layer is 100nm to 1000nm. Specifically, the thickness of the coating layer can be any point value among 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm and 1000nm, or a range value between any two points.

[0179] By setting the thickness of the coating layer to 100 nm to 1000 nm, the theoretical specific capacity of the positive electrode material can be ensured while the residual lithium compound is effectively removed.

[0180] In some embodiments, based on the total mass of the positive electrode material, the mass percentage of the coating layer is 0.01 wt % to 6 wt %.

[0181] As mentioned above, the coating layer has almost no contribution to the battery capacity. If the mass percentage of the coating layer in the positive electrode material is too large, the theoretical specific capacity of the positive electrode material will be reduced, and if it is too small, the removal effect of the residual lithium compound will be affected. Optionally, the mass percentage of the coating layer in the positive electrode material is 0.01wt% to 6wt%, specifically, the mass percentage of the coating layer is 0.01wt%, 0.05wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt% and 6wt% at any point or a range between any two points.

[0182] Optionally, the mass percentage of the coating layer is 0.1 wt % to 1 wt %. Within this range, the removal effect of the residual lithium compound in the positive electrode material and the theoretical specific capacity of the positive electrode material reach an optimal balance.

[0183] By setting the mass percentage of the coating layer in the positive electrode material to 0.01wt% to 6wt%, the theoretical specific capacity of the positive electrode material can be ensured while the residual lithium compound is effectively removed.

[0184] In some embodiments, the positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2.

[0185] The chemical formula of nickel-rich active material is Li a Ni m Co n M 1-m-n O2, wherein M includes at least one of Mn and Al. As an example, M includes Mn, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Mn 1-m-n As an example, M includes Al, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Al 1-m-nO2. Specifically, m≥0.6, and the content of nickel in the nickel-rich active material is increased by increasing the value of m, thereby increasing the reversible lithium insertion capacity of the positive electrode material. Optionally, m is any one of 0.6, 0.7, 0.8, 0.9, 0.95 and 0.99, or a range value between any two of them. Optionally, m≥0.9, and the reversible lithium insertion capacity of the positive electrode material is large within this range. Specifically, n≤0.2, the nickel-rich active material is usually a layered structure, and Co can stabilize the layered structure, but the high price of Co will increase the cost of the nickel-rich active material. The cost of the nickel-rich active material can be controlled by controlling n≤0.2. Optionally, n is any one of 0.05, 0.1, 0.15 and 0.2, or a range value between any two of them. 0.9≤a≤1.2, that is, the lithium content in the nickel-rich active material can be greater than 1, equal to 1, or less than 1. When a is greater than 1, the nickel-rich active material is a lithium-rich positive electrode material. As an example, for the nickel-rich active material obtained by pre-lithiation, the Li content can be greater than 1. Optionally, a is any one of 0.9, 0.95, 1, 1.05, 1.1, 1.15 and 1.2, or a range between any two of them.

[0186] However, the nickel element in the nickel-rich active material is alkaline. As the nickel content increases, the nickel-rich active material is easily exposed to the air to absorb moisture and carbon dioxide, and residual lithium compounds (RLCs) are generated on its surface, such as lithium hydroxide (LiOH) and lithium carbonate (Li2CO3), which further increase the pH of the nickel-rich active material and seriously affect the electrochemical properties and storage performance of the nickel-rich active material.

[0187] Based on this, the present invention introduces an additive on the surface of the nickel-rich active material, wherein the additive comprises a reducing sulfide element, and the Ni, Co, and Mn in the nickel-rich active material are Ni 3+ / Ni 2+ 、Co 3+ and Mn 4+The nickel-rich active material exists in the form of ions, and the reducing sulfide in the additive is easily oxidized by the nickel-rich active material and reacts with the residual lithium compound on the surface of the nickel-rich active material, thereby in situ generating an intermediate product containing the sulfide in an intermediate valence state on the surface of the nickel-rich active material. In the subsequent formation process, the intermediate product continues to react, and the reducing sulfide will continue to be oxidized and react with the residual lithium compound, and finally generate a final product containing the sulfide in a high valence state (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, in the formation process, the final product further forms a positive electrode-electrolyte interface (CEI) film on the surface of the nickel-rich active material, thereby removing the residual lithium compound on the surface of the nickel-rich active material and improving the conductivity and electrochemical properties of the nickel-rich active material. In this process, additional lithium ions are also released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery.

[0188] In some embodiments, the DV50 particle size of the positive electrode active material is 5 μm to 15 μm.

[0189] The average particle size is generally expressed as DV50, which means that the powder particles larger and smaller than this particle size each account for 50%. Usually, the positive electrode active material is granular, and the particle size of the positive electrode active material will affect the processing performance and electrochemical performance of the positive electrode material. Generally, the larger the particle size of the positive electrode active material, the longer the migration path of lithium ions in the positive electrode active material, which affects the rate performance of the battery. However, the smaller the particle size of the positive electrode active material, the more unstable the viscosity of the slurry will be during the slurrying process of the positive electrode material, which will affect the subsequent slurry coating effect.

[0190] Optionally, the DV50 particle size of the positive electrode active material is any one of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm and 15 μm, or a range value between any two of them.

[0191] By setting the DV50 particle size of the positive electrode active material to 5 μm to 15 μm, it can be ensured that the positive electrode material has better processing performance and electrochemical performance.

[0192] Some embodiments of the present application also provide a method for preparing a positive electrode material, comprising:

[0193] The one-dimensional conductive material and an additive are mixed to obtain a mixture, wherein the additive comprises a reducing chalcogen element;

[0194] Sintering the mixed material to melt the additive and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby obtaining a sintered material;

[0195] The sintered material is stirred with the positive electrode active material to obtain the positive electrode material.

[0196] As mentioned above, one-dimensional conductive materials refer to fibrous or tubular materials in which electrons can move freely in only one non-nanoscale direction. One-dimensional conductive materials include, but are not limited to, metal nanowires and one-dimensional conductive carbon materials. Metal nanowires include, but are not limited to, silver nanowires, copper nanowires, etc. One-dimensional conductive carbon materials can be one-dimensional nanocarbon materials or one-dimensional micron carbon materials. Optionally, the one-dimensional conductive carbon material includes at least one of carbon fibers, nanocarbon fibers, and carbon nanotubes.

[0197] The additive includes a chalcogen with reducing properties, where the chalcogen refers to sulfur and elements with similar chemical properties to sulfur. Optionally, the chalcogen includes elements other than oxygen in the oxygen group. Optionally, the chalcogen includes at least one of sulfur (S), selenium (Se) and tellurium (Te). The additive includes a chalcogen, where the additive can be a compound, with the chalcogen as one of the constituent elements of the compound, and the additive can also be a single substance, such as a chalcogen itself used as an additive. Chalcogen has reducing properties, that is, the chalcogen can increase the valence state through oxidation-reduction reactions. Optionally, the valence of the chalcogen is less than or equal to zero, that is, a low-valent chalcogen, and the chalcogen is easily oxidized to a high-valent chalcogen. As an example, the chalcogen includes sulfur, the valence of low-valent sulfur is -2 or zero, and the valence of high-valent sulfur is +6 or +4.

[0198] The mixing process of the one-dimensional conductive material and the additive refers to mixing the additive and the one-dimensional conductive material together so that the additive is pre-attached to the one-dimensional conductive material.

[0199] Sintering treatment refers to heat treating the mixture at a suitable temperature so that the additive melts, but the additive only changes in physical form without chemical reaction. The additive melts into a more fluid liquid during the sintering process. The liquid additive spreads and disperses on the surface of the one-dimensional conductive material. After the temperature is reduced, the liquid additive solidifies into a solid additive and maintains a spread state, and the additive wraps the one-dimensional conductive material in the form of a film and / or a block. At this time, the one-dimensional conductive material and the additive are physically combined, but because the contact area is relatively large, the bonding stability of the additive is enhanced. Optionally, the mixture is sintered under a protective atmosphere, and the protective atmosphere is used to isolate oxygen to prevent the mixture from high-temperature oxidation. The protective atmosphere here can be an inert gas or nitrogen. It can be understood that there are many types of chalcogens, so there will be more types of additives, and different additives have different melting temperatures, so the temperature of the sintering treatment will also be different, as long as the sintering temperature is controlled to melt the additive.

[0200] The preparation method of the positive electrode material provided in the embodiment of the present application is to mix the one-dimensional conductive material and the additive and then sinter the mixture so that the additive is melted, and at least part of the one-dimensional conductive material is wrapped by the additive, thereby increasing the physical contact area between the additive and the one-dimensional conductive material, and combining the large specific surface area of ​​the one-dimensional conductive material itself, so that the binding ability of the additive and the one-dimensional conductive material is enhanced, and the additive containing the sulfide element is effectively fixed. The sintered material obtained after the sintering treatment is further stirred and mixed with the positive electrode active material, so that the one-dimensional conductive material with the additive wrapped on the surface is distributed on the surface of the positive electrode active material, thereby forming a positive electrode material. Since the one-dimensional conductive material itself has good conductivity, a conductive network is overlapped by the one-dimensional conductive material. Even after the additive is wrapped, the conductive network can be well connected, thereby ensuring the overall conductive effect of the positive electrode material. In addition, the additives wrapped on the surface of the one-dimensional conductive material will contact the positive electrode active material. During this process, the reducing sulfide elements in the additives will undergo redox reactions with the metal cations in the positive electrode active material and consume the residual lithium compounds on the surface of the positive electrode active material to in situ generate intermediate products containing sulfide elements with intermediate valence states (such as Li2S2O3, Li2Se2O3, Li2Te2O3, etc.) on the surface of the positive electrode active material. In the subsequent formation process, the intermediate products continue to react, and the reducing sulfide elements will continue to be oxidized and react with the residual lithium compounds, and finally generate final products containing sulfide elements with high valence states (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, during the formation process, the final products further form a positive electrode-electrolyte interface (CEI) film on the surface of the positive electrode active material, thereby removing the residual lithium compounds on the surface of the positive electrode active material and improving the conductivity and electrochemical properties of the positive electrode active material. In the process of converting the reducing sulfide element into the CEI film, additional lithium ions are released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery. In addition, the preparation method of the positive electrode material provided in the embodiment of the present application is simple, easy to operate, and conducive to industrialization.

[0201] In some embodiments, the chalcogen element includes at least one of sulfur, selenium, and tellurium.

[0202] As mentioned above, by setting the additive to include a reducing sulfide element, the sulfide element includes at least one of sulfur, selenium and tellurium, and the above sulfide element can react with the residual lithium compound, consume the residual lithium compound and promote the growth of the CEI film on the positive electrode, thereby improving the electrochemical performance of the battery; in this process, additional lithium ions are simultaneously released to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery.

[0203] In some embodiments, the additive includes a chalcogen.

[0204] The additive includes a chalcogen element, and optionally, the chalcogen element includes at least one of sulfur, selenium and tellurium. Then the additive includes at least one of sulfur, selenium and tellurium.

[0205] The valence of sulfide elements is zero, and sulfide elements themselves have strong reducing properties, which makes it easy for sulfide elements to eliminate residual lithium compounds. At the same time, the composition of sulfide elements is single. Introducing sulfide elements into the surface of the positive electrode active material can reduce the introduction of other elements, thereby reducing the risk of side reactions.

[0206] In some embodiments, the one-dimensional conductive material includes a one-dimensional conductive carbon material.

[0207] One-dimensional conductive carbon materials refer to fibrous or tubular carbon materials in which electrons can move freely in only one non-nanoscale direction.

[0208] In addition to having a large comparative area, the one-dimensional conductive carbon material also has a strong adsorption capacity, which enables the one-dimensional conductive carbon material to effectively adsorb additives attached to the surface of the one-dimensional conductive carbon material, enhance the binding ability between the one-dimensional conductive carbon material and the additive, and enhance the anchoring effect of the one-dimensional conductive carbon material on the additive.

[0209] In some embodiments, the additive includes elemental sulfur, the sintering temperature is 180° C. to 220° C., and / or the sintering time is 5 h to 7 h.

[0210] Usually, the temperature of sintering treatment will affect the melting effect of sulfur. If the temperature is too low, sulfur cannot melt, and if the temperature is too high, sulfur will undergo a chemical reaction.

[0211] Optionally, the temperature of the sintering process is any one of 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C and 220°C, or a range value between any two of them.

[0212] The sintering time will affect the amount of sulfur coated on the surface of the one-dimensional conductive material. If the sintering time is too short, the sulfur content in the positive electrode material will be too low, and the effect of removing residual lithium compounds will be poor. If the sintering time is too long, the sulfur content in the positive electrode material will be too high, resulting in sulfur residue, which will eventually affect the internal resistance of the battery and increase the battery polarization.

[0213] Optionally, the sintering time is any one of 5 h, 5.5 h, 6 h, 6.5 h and 7 h, or a range value between any two of them.

[0214] By using sulfur as an additive, compared with other additives, the chemical properties of sulfur are more active, the effect of removing residual lithium compounds is better, and the raw materials of sulfur are easy to obtain and low in cost. Using sulfur as an additive is cost-effective. Furthermore, by setting the sintering temperature to 180°C to 220°C, sulfur can exist stably in the form of a molten liquid within this temperature range, and then be coated on the surface of a one-dimensional conductive material. In addition, by setting the sintering time to 5h to 7h, the content of sulfur in the positive electrode material can be effectively controlled, so that sulfur can effectively remove residual lithium compounds without increasing the polarization of the battery.

[0215] In some embodiments, the additive has a DV50 particle size greater than 0 and less than or equal to 1 μm.

[0216] Usually, in the preparation of positive electrode materials, it is necessary to first mix the additive and the one-dimensional conductive material so that the additive is pre-loaded on the one-dimensional conductive material. In this process, the binding force between the additive and the one-dimensional conductive material is very weak. If the particle size of the additive is too large, it is not conducive to the pre-loading of the additive. However, if the particle size of the additive is too small, the additive may agglomerate and cannot be well dispersed on the one-dimensional conductive material, which will also affect the pre-loading effect.

[0217] Optionally, the DV50 particle size of the additive is any one of 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm and 1 μm, or a range value between any two of them.

[0218] Optionally, the DV50 particle size of the additive is 100 nm to 500 nm. Within this particle size range, the dispersibility of the additive and the bonding property with the one-dimensional conductive material reach an optimal balance.

[0219] By setting the DV50 particle size of the additive to be greater than 0 and less than or equal to 1 μm, within this range, the dispersion effect of the additive is good, and the combination of the additive and the one-dimensional conductive material is good when the additive is pre-loaded.

[0220] In some embodiments, the mixing process includes a ball milling process.

[0221] In order to prevent the additives from agglomerating, the additives usually have a larger particle size. However, the larger particle size of the additives will make the binding between the additives and the one-dimensional conductive material during pre-loading poor. Based on this, ball milling is designed in the mixing process to make the additive particles larger and better dispersed during the initial mixing of the additives and the one-dimensional conductive material. Then, the particle size of the additive is reduced through ball milling to improve the binding stability between the additives and the one-dimensional conductive material.

[0222] By designing a ball milling process in the mixing process, on the one hand, the restriction on the particle size of the additive before the mixing process can be reduced, and on the other hand, the particle size of the additive can be reduced through the ball milling process, thereby improving the bonding stability between the additive and the one-dimensional conductive material.

[0223] In some embodiments, the stirring process has a rotation speed of 400 r / s to 1000 r / s.

[0224] Optionally, the rotation speed of the stirring process is any one of 400 r / s, 500 r / s, 600 r / s, 700 r / s, 800 r / s, 900 r / s and 1000 r / s, or a range value between any two of them.

[0225] By setting the rotation speed of the stirring process to 400 r / s to 1000 r / s, the sintering material and the positive electrode active material can be effectively mixed together.

[0226] In some embodiments, the positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2.

[0227] The chemical formula of nickel-rich active material is Li a Ni m Co n M 1-m-n O2, wherein M includes at least one of Mn and Al. As an example, M includes Mn, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Mn 1-m-n As an example, M includes Al, and the chemical formula of the nickel-rich active material is Li a Ni m Co n Al 1-m-nO2. Specifically, m≥0.6, and the content of nickel in the nickel-rich active material is increased by increasing the value of m, thereby increasing the reversible lithium insertion capacity of the positive electrode material. Optionally, m is any one of 0.6, 0.7, 0.8, 0.9, 0.95 and 0.99, or a range value between any two of them. Optionally, m≥0.9, and the reversible lithium insertion capacity of the positive electrode material is large within this range. Specifically, n≤0.2, the nickel-rich active material is usually a layered structure, and Co can stabilize the layered structure, but the high price of Co will increase the cost of the nickel-rich active material. The cost of the nickel-rich active material can be controlled by controlling n≤0.2. Optionally, n is any one of 0.05, 0.1, 0.15 and 0.2, or a range value between any two of them. 0.9≤a≤1.2, that is, the lithium content in the nickel-rich active material can be greater than 1, equal to 1, or less than 1. When a is greater than 1, the nickel-rich active material is a lithium-rich positive electrode material. As an example, for the nickel-rich active material obtained by pre-lithiation, the Li content can be greater than 1. Optionally, a is any one of 0.9, 0.95, 1, 1.05, 1.1, 1.15 and 1.2, or a range between any two of them.

[0228] However, the nickel element in the nickel-rich active material is alkaline. As the nickel content increases, the nickel-rich active material is easily exposed to the air to absorb moisture and carbon dioxide, and residual lithium compounds (RLCs) are generated on its surface, such as lithium hydroxide (LiOH) and lithium carbonate (Li2CO3), which further increase the pH of the nickel-rich active material and seriously affect the electrochemical properties and storage performance of the nickel-rich active material.

[0229] Based on this, the present invention introduces an additive on the surface of the nickel-rich active material, wherein the additive comprises a reducing sulfide element, and the Ni, Co, and Mn in the nickel-rich active material are Ni 3+ / Ni 2+ 、Co 3+ and Mn 4+The nickel-rich active material exists in the form of ions, and the reducing sulfide in the additive is easily oxidized by the nickel-rich active material and reacts with the residual lithium compound on the surface of the nickel-rich active material, thereby in situ generating an intermediate product containing the sulfide in an intermediate valence state on the surface of the nickel-rich active material. In the subsequent formation process, the intermediate product continues to react, and the reducing sulfide will continue to be oxidized and react with the residual lithium compound, and finally generate a final product containing the sulfide in a high valence state (such as Li2SO3, Li2SO4, Li2SeO3, Li2SeO4, Li2TeO3, Li2TeO4, etc.). At the same time, in the formation process, the final product further forms a positive electrode-electrolyte interface (CEI) film on the surface of the nickel-rich active material, thereby removing the residual lithium compound on the surface of the nickel-rich active material and improving the conductivity and electrochemical properties of the nickel-rich active material. In this process, additional lithium ions are also released synchronously to compensate for the lithium ion loss caused by the formation of the SEI film, thereby ensuring the capacity of the battery.

[0230] See also Figure 4 Some embodiments of the present application also provide a positive electrode plate 102, including a positive electrode current collector and a positive electrode material layer combined with the positive electrode current collector, the positive electrode material layer includes the above-mentioned positive electrode material or the positive electrode material prepared according to the above-mentioned positive electrode material preparation method.

[0231] The current collector is a structure or part used to collect current in a battery. The current collector is usually a metal foil. The positive electrode current collector refers to the structure or part used to collect current in the positive electrode of a battery. The positive electrode current collector includes but is not limited to aluminum foil.

[0232] The positive electrode material layer refers to a film layer disposed on the positive electrode current collector and containing positive electrode active materials. The positive electrode material layer may be disposed on one side of the positive electrode current collector, or may be disposed on both sides of the positive electrode current collector. Optionally, the positive electrode material layer includes a conductive agent and a binder.

[0233] The positive electrode plate 102 provided in the embodiment of the present application includes a positive electrode current collector and a positive electrode material layer, and the positive electrode material layer includes the above-mentioned positive electrode material, so that the content of residual lithium compounds in the positive electrode plate 102 is low, the overall conductive effect of the positive electrode plate 102 is improved, and the cycle performance is improved.

[0234] See also Figure 2 Some embodiments of the present application further provide a battery 40 , which includes the above-mentioned positive electrode plate 102 .

[0235] Optionally, the battery 40 is a secondary battery, which has many different forms, including but not limited to battery cells, battery modules, and battery packs.

[0236] The battery 40 provided in the embodiment of the present application includes the above-mentioned positive electrode plate 102, and the battery 40 has stable cycle performance and good rate performance.

[0237] See also Figure 1 Some embodiments of the present application further provide an electrical device 50 , which includes the battery 40 described above.

[0238] As described above, the electric device 50 may be, but is not limited to, a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy, an electric tool, and the like.

[0239] The following describes the invention in conjunction with specific embodiments.

[0240] Example 1

[0241] S1. Preparation of positive electrode material: sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere at a sintering temperature of 200°C for 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM (LiNi 0.9 Co 0.05 Mn 0.05 ) were mixed and stirred at a rotation speed of 600 r / s to obtain a modified positive electrode material, wherein the mass ratio of sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material was 0.02:0.5:99.48.

[0242] S2. Preparation of positive electrode sheets: The positive electrode material prepared in the above S1, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are dissolved in the solvent N-methylpyrrolidone (NMP) in a weight ratio of 96.5:1.5:2, and the positive electrode slurry is obtained after being fully stirred and mixed; the positive electrode slurry is then evenly coated on the positive electrode collector with a primer, and then dried, cold pressed, and cut to obtain the positive electrode sheet.

[0243] S3. Preparation of negative electrode sheets: The negative electrode active material graphite, silicon, conductive agent acetylene black, styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are dissolved in deionized water as a solvent in a weight ratio of 90:5:2:2:1, and mixed evenly to prepare negative electrode slurry. The slurry is coated on copper foil, dried, and then cold-pressed and cut to obtain negative electrode sheets.

[0244] S4. Preparation of secondary battery: stack the positive electrode sheet, separator, and negative electrode sheet in order, so that the separator is between the positive electrode sheet and the negative electrode sheet to play an isolating role, then wind to obtain a bare cell, weld the pole ear to the bare cell, and put the bare cell into an aluminum shell, bake at 80°C to remove water, then inject electrolyte and seal to obtain an uncharged battery. The uncharged battery then undergoes the processes of standing, hot and cold pressing, formation, shaping, capacity testing, etc. to obtain a secondary battery product. The above-mentioned separator is a PE separator, and its surface is coated with PVDF and alumina coating to improve adhesion and heat resistance. The preparation process of the above-mentioned electrolyte is to mix ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1, and then evenly dissolve LiPF6:LiFSI (2:8) in the above solution to obtain an electrolyte, in which the concentration of lithium salt is 1 mol / L.

[0245] Example 2

[0246] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 1:0.5:98.5.

[0247] Example 3

[0248] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:0.5:96.5.

[0249] Example 4

[0250] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 5:0.5:94.5.

[0251] Example 5

[0252] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 6:0.5:93.5.

[0253] Example 6

[0254] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 6:1.5:92.5.

[0255] Example 7

[0256] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:0.02:96.98.

[0257] Example 8

[0258] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:1:96.

[0259] Example 9

[0260] The same as Example 1, except that S1: the sulfur element and polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material. In terms of mass ratio, the sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 3:1.5:95.5.

[0261] Example 10

[0262] The same as Example 3, except that S1: the sulfur element and the polypropylene-based carbon fiber are ball-milled and mixed evenly, and then sintered in an inert atmosphere, wherein the sintering temperature is 200°C and the sintering time is 6 hours. Finally, the sintered material is mixed with the positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a positive electrode material having a first coating layer on the surface. The mass ratio of sulfur element: polypropylene-based carbon fiber: positive electrode active material NCM in the positive electrode material is 2.5:0.5:96.5; the obtained positive electrode material is then mixed with sulfur element, conductive carbon black, and PVDF in a mass ratio of 100:2:2:1 to obtain a positive electrode material having a double-layer coating on the surface; and then mixed with conductive carbon black and PVDF in a mass ratio of 95:3:2 to obtain a three-layer coated positive electrode material.

[0263] Comparative Example 1

[0264] Same as Example 1, except that S1: no sulfur and polypropylene-based carbon fiber filaments are added.

[0265] Comparative Example 2

[0266] The same as Example 1, except that S1: sulfur element and positive electrode active material NCM are mixed, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material, in which the mass ratio of sulfur element in the positive electrode material to positive electrode active material NCM is 0.02:99.98.

[0267] Comparative Example 3

[0268] The same as Example 1, except that S1: polypropylene-based carbon fiber filaments are mixed with positive electrode active material NCM, and stirred and mixed at a rotation speed of 600 r / s to obtain a modified positive electrode material, in which the mass ratio of polypropylene-based carbon fiber filaments to positive electrode active material NCM in the positive electrode material is 0.5:99.5.

[0269] In order to verify the progress of the embodiments of the present application, the secondary batteries prepared in embodiments 1 to 10 and comparative examples 1 to 3 were tested as follows:

[0270] 1. Secondary battery discharge DCR test:

[0271] Each secondary battery was placed at 25°C for 30 minutes, charged to 4.25V at a rate of 1 / 3C, and ended at a constant voltage of 0.05C. After being placed at rest for 10 minutes, the battery was discharged at a rate of 1 / 3C until the battery cell's capacity was 50% of the full charge, which was called 50% SOC; after being placed at rest for 60 minutes, the battery was discharged at a rate of 4C for 10 seconds, and the DCR value of the battery cell was recorded.

[0272] 2. Storage test:

[0273] Each secondary battery was stored at 60℃ and 97% SOC. Before and during storage, C0 and Cn were taken as the initial reversible capacity and actual reversible capacity of the battery, respectively. The battery was taken out for testing every 15 days. The testing process is as follows: each secondary battery was placed at 25℃ for 30 minutes, charged to 4.25V at a rate of 1 / 3C, and the constant voltage was terminated to 0.05C. The battery was placed for 30 minutes, and discharged to 2.8V at a rate of 1 / 3C, and the initial reversible capacity C0 was recorded. The battery was tested every 15 days, and Cn (n=1, 2, 3, 4, 5...) was recorded; when Cn / C0≤80%, n was recorded; the number of days of EOL storage = 15*n.

[0274] 3. Cycle test:

[0275] Adjust the temperature to 45℃ and keep warm for 2 hours. Let it stand for 5 minutes, charge at 1 / 3C to 4.25V, charge at 4.25V constant voltage to 0.05C. Let it stand for 5 minutes, discharge at 0.5C to 2.8V. Let it stand for 5 minutes, repeat the above process until the capacity decays to 80%.

[0276] The test results are shown in Table 1.

[0277] Table 1

[0278]

[0279] From the comparison of Example 1 and Comparative Example 1 in Table 1, it can be seen that compared with not adding sulfur and carbon fiber, sulfur and carbon fiber are added simultaneously to the positive electrode active material NCM, and the capacity retention rate of the battery after storage and the capacity retention rate after cycling are improved. This is because sulfur and carbon fiber filaments are simultaneously introduced on the surface of the positive electrode active material NCM. The carbon fiber filaments can construct a conductive network on the surface of the positive electrode active material NCM to improve the conductivity of the positive electrode material and reduce the polarization loss of the battery. At the same time, the carbon fiber filaments anchor the sulfur element, thereby introducing sulfur element on the surface of the positive electrode active material NCM, promoting the sulfur element to fully react with the residual lithium compound on the surface of the positive electrode active material NCM and generating an artificial CEI film on the surface of the positive electrode active material NCM, effectively reducing the amount of residual lithium compounds, thereby reducing the occurrence of side reactions in the battery, improving the stability of the positive electrode material structure and the interface stability on the positive electrode, and maintaining the capacity of the battery. In the process of the action of sulfur element and residual lithium compound, additional lithium ions will be released synchronously to compensate for the lithium ion loss caused by the formation of SEI film in the battery, ensuring the stock of active lithium, and further ensuring the capacity of the battery.

[0280] From the comparison of Example 1 and Comparative Example 2 in Table 1, it can be seen that compared with adding only sulfur, adding sulfur and carbon fiber simultaneously to the positive electrode active material NCM, the capacity retention rate of the battery after storage and the capacity retention rate after cycling are improved. This is because the conductivity of sulfur itself is poor. Adding only sulfur will make the conductivity of the positive electrode material poor, increase the polarization of the battery, and at the same time, the sulfur is not sufficiently anchored in the positive electrode active material NCM, and it is easy to detach from the positive electrode active material NCM, so that the sulfur reacts insufficiently with the residual lithium compound, and the capacity of the battery cannot be effectively maintained.

[0281] From the comparison between Example 1 and Comparative Example 3 in Table 1, it can be seen that, compared with adding only carbon fiber, adding sulfur and carbon fiber simultaneously to the positive electrode active material NCM, the capacity retention rate of the battery after storage and the capacity retention rate after cycling are improved. This is because the conductivity of the positive electrode material is improved by adding only carbon fiber, but the residual lithium compounds on the surface of the positive electrode active material NCM cannot be eliminated. The presence of residual lithium compounds will affect the conductivity of the positive electrode active material NCM on the one hand, and will also promote the occurrence of side reactions, thereby affecting the capacity of the battery.

[0282] It can be seen from Examples 1 to 5 in Table 1 that the carbon fiber content is fixed. As the sulfur content increases, the capacity retention rate after storage and the capacity retention rate after cycle of the battery both increase. However, when the sulfur content is greater than 5wt%, the capacity retention rate after storage and the capacity retention rate after cycle decrease instead. This is because the excessive sulfur content leads to sulfur residue, which reduces the conductivity of the positive electrode material, increases the battery polarization, and continuously consumes the active lithium inside the battery during battery storage, causing the battery performance to deteriorate.

[0283] It can be seen from Example 7, Example 3, Example 8 and Example 9 in Table 1 that when the sulfur content is fixed and the carbon fiber content is increased, the battery DCR decreases, and the battery capacity retention rate after storage and the capacity retention rate after cycle are relatively high.

[0284] It can be seen from Example 6 and Example 9 in Table 1 that although increasing the content of carbon fiber can reduce the battery DCR, when the content of carbon fiber is greater than 1wt%, for example 1.4wt% or 1.5wt%, physical gelation of the positive electrode material is prone to occur during slurrying, and the processing performance of the positive electrode material deteriorates.

[0285] In addition, from the comparison of Example 3 and Example 10 in Table 1, it can be seen that a plurality of coating layers are arranged on the surface of the positive electrode active material NCM, and from the inside to the outside, the content of elemental sulfur in each coating layer decreases successively, and the capacity retention rate of the battery after storage is significantly improved. This is because the outer coating layer with a low content of elemental sulfur can block the inner coating layer with a high content of elemental sulfur, and limit the elemental sulfur as much as possible inside the positive electrode material, inhibiting the flow of elemental sulfur to the negative electrode to react with the active lithium and cause lithium consumption, thereby improving the battery capacity retention rate.

[0286] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A positive electrode material, characterized in that: include: A positive electrode active material and a one-dimensional conductive material and an additive distributed on the surface of the positive electrode active material, at least part of the one-dimensional conductive material is wrapped by the additive, and the additive contains a reducing chalcogen element.

2. The positive electrode material according to claim 1, characterized in that The chalcogen element includes at least one of sulfur, selenium and tellurium.

3. The positive electrode material according to claim 1 or 2, characterized in that The chalcogen element includes sulfur element, and the additive includes at least one of sulfur element, metal sulfide, polysulfide, sulfur-containing organic polymer or copolymer, and polymerized sulfur.

4. The positive electrode material according to any one of claims 1 to 3, characterized in that The additive includes a simple substance of chalcogen.

5. The positive electrode material according to any one of claims 1 to 4, characterized in that: The one-dimensional conductive material includes a one-dimensional conductive carbon material.

6. The positive electrode material according to claim 5, characterized in that The one-dimensional conductive carbon material includes at least one of short carbon fiber filaments, nano carbon fibers and carbon nanotubes; optionally, the short carbon fiber filaments include at least one of PAN-based carbon fibers, phenolic-based carbon fibers, viscose-based carbon fibers, asphalt-based carbon fibers, biomass-based carbon fibers and activated carbon fibers.

7. The positive electrode material according to claim 6, characterized in that The diameter of the short carbon fiber filaments is 100 nm-500 nm; and / or the length of the short carbon fiber filaments is 1 μm-5 μm.

8. The positive electrode material according to any one of claims 1 to 7, characterized in that: Based on the total mass of the positive electrode material, the mass percentage of the chalcogen element is 0.02 wt % to 5 wt %.

9. The positive electrode material according to any one of claims 1 to 8, characterized in that Based on the total mass of the positive electrode material, the mass percentage of the one-dimensional conductive material is greater than 0 and less than or equal to 1 wt %.

10. The positive electrode material according to any one of claims 1 to 9, characterized in that: The surface of the positive electrode active material is coated with a coating layer, wherein the coating layer includes a first sub-coating layer, and the first sub-coating layer includes the one-dimensional conductive material and the additive wrapped on the one-dimensional conductive material.

11. The positive electrode material according to claim 10, characterized in that The coating layer also includes a second sub-coating layer, which is arranged on a side of the first sub-coating layer away from the positive electrode active material, the second sub-coating layer contains a conductive agent and a binder, and the content of the chalcogen element in the second sub-coating layer is greater than or equal to 0 and less than the content of the chalcogen element in the first sub-coating layer.

12. The positive electrode material according to claim 11, characterized in that The content of the chalcogen element in the second sub-coating layer is greater than 0, and the coating layer further includes a third sub-coating layer, which is coated on the surface of the second sub-coating layer, and the third sub-coating layer contains the conductive agent and the binder.

13. The positive electrode material according to any one of claims 10 to 12, characterized in that: The coating layer has a thickness of 100 nm to 1000 nm.

14. The positive electrode material according to any one of claims 10 to 13, characterized in that: Based on the total mass of the positive electrode material, the mass percentage of the coating layer is 0.01wt% to 6wt%; optionally, the mass percentage of the coating layer is 0.1wt% to 1wt%.

15. The positive electrode material according to any one of claims 1 to 14, characterized in that: The positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2; optionally, m≥0.

9.

16. The positive electrode material according to any one of claims 1 to 15, characterized in that: The DV50 particle size of the positive electrode active material is 5 μm to 15 μm.

17. A method for preparing a positive electrode material, characterized in that: include: The one-dimensional conductive material and an additive are mixed to obtain a mixture, wherein the additive comprises a chalcogen element having reducing properties; Sintering the mixed material so that the additive is melted and at least a portion of the one-dimensional conductive material is wrapped by the additive, thereby obtaining a sintered material; The sintered material is stirred with the positive electrode active material to obtain the positive electrode material.

18. The method for preparing the positive electrode material according to claim 17, characterized in that: The chalcogen element includes at least one of sulfur, selenium and tellurium.

19. The method for preparing a positive electrode material according to any one of claims 17 or 18, characterized in that: The additive includes a chalcogen element; and / or the one-dimensional conductive material includes a one-dimensional conductive carbon material.

20. The method for preparing the positive electrode material according to claim 19, characterized in that: The additive includes elemental sulfur, the sintering temperature is 180° C. to 220° C., and / or the sintering time is 5 h to 7 h.

21. The method for preparing a positive electrode material according to any one of claims 17 to 20, characterized in that: The DV50 particle size of the additive is greater than 0 and less than or equal to 1 μm; optionally, the DV50 particle size of the additive is 100 nm to 500 nm.

22. The method for preparing a positive electrode material according to any one of claims 17 to 21, characterized in that: The mixing process includes ball milling; and / or the stirring process has a rotation speed of 400 r / s to 1000 r / s.

23. The method for preparing a positive electrode material according to any one of claims 17 to 22, characterized in that: The positive electrode active material includes a chemical formula of Li a Ni m Co n M 1-m-n O2-rich nickel active material, wherein M includes at least one of Mn and Al, wherein m≥0.6, n≤0.2, 0.9≤a≤1.2; optionally, m≥0.

9.

24. A positive electrode plate, characterized in that: It comprises a positive electrode current collector and a positive electrode material layer bonded to the positive electrode current collector, wherein the positive electrode material layer comprises the positive electrode material according to any one of claims 1 to 16 or the positive electrode material prepared by the method for preparing the positive electrode material according to any one of claims 17 to 23.

25. A battery, characterized in that: Comprising the positive electrode sheet according to claim 24.

26. An electrical device, characterized in that: Comprising a battery according to claim 25.

Citation Information

Patent Citations

  • Sulfur-containing composite anode, preparation method thereof and lithium-sulfur battery using sulfur-containing composite anode as anode

    CN104716296A

  • Anode active material, preparation method of anode active material, high-performance anode slurry containing anode active material, and all-solid-state lithium ion battery

    CN106784798A

  • Preparation method of positive electrode composite material for lithium sulfur battery

    CN107978741A

  • Low-temperature vapor deposition coated high-nickel ternary layered positive electrode material and preparation method thereof

    CN112768662A

  • Slurry, positive pole piece, secondary battery, battery module, battery pack and electric device

    CN115832299A