Positive electrode material and preparation method thereof, positive electrode plate, battery and electric device

By using a combination of cladding and transition metal elements in lithium iron phosphate materials, the problem of low cycling performance of lithium iron phosphate materials after the introduction of transition metal elements is solved, and the high energy density and good cycling performance of the battery are achieved.

CN118970018AActive Publication Date: 2024-11-15NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411427923.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-15
Estimated Expiration
2044-10-14

AI Technical Summary

Technical Problem

After the introduction of transition metal elements, lithium iron phosphate material can improve the energy density of the battery, but its circulation performance is relatively low, resulting in a shortening of the battery's service life.

Method used

Using a positive electrode active material including the chemical formula LiaFe1-bMbPO4 and a material with the chemical formula LimFe1-nM'nPO4-CN of the coating layer, the dissolution of transition metal elements is reduced, the service life is extended, and the introduction of transition metal elements is introduced. Increase the capacity of grams.

Benefits of technology

The positive electrode material has achieved high capacity and good circulation performance, so that the battery has high energy density and circulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970018A_ABST
    Figure CN118970018A_ABST
Patent Text Reader

Abstract

The invention relates to a positive electrode material and a preparation method thereof, a positive electrode plate, a battery and an electric device. The positive electrode material comprises a positive electrode active material and a coating layer located on at least one part of the surface of the positive electrode active material, the positive electrode active material comprises a material with the chemical formula of LiaFe1-bMbPO4 and a material C, the coating layer comprises a material with the chemical formula of LimFe1-nM'nPO4-CN, a is larger than or equal to 0.95 and smaller than or equal to 1.1, b is larger than or equal to 0.4 and smaller than or equal to 0.9, m is larger than or equal to 0.95 and smaller than or equal to 1.1, n is larger than or equal to 0.4 and smaller than or equal to 0.9, and M and M'independently comprise other transition metal elements except Fe. The positive electrode material has relatively high gram volume and relatively good cycle performance. When the positive electrode material is applied to the battery, the battery can have relatively high energy density and relatively good cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet, a battery and an electrical device. Background Art

[0002] Lithium iron phosphate material has good safety and cycle performance, but its gram capacity is low. When it is used as a positive electrode material in a battery, the energy density of the battery is low. In order to improve the energy density of the battery, introducing transition metal elements into lithium iron phosphate materials is a relatively effective method. For example, lithium manganese iron phosphate obtained by introducing manganese elements into lithium iron phosphate materials can show a higher gram capacity than lithium iron phosphate, thereby improving the energy density of the battery. However, after the introduction of transition metal elements into lithium iron phosphate materials, the cycle performance of the material is low, which reduces the cycle performance of the battery. Summary of the invention

[0003] Based on this, it is necessary to provide a positive electrode material based on lithium iron phosphate and a preparation method thereof, as well as a positive electrode sheet, a battery and an electrical device comprising the positive electrode material. The positive electrode material can take into account both a higher gram capacity and better cycle performance, thereby enabling the battery to have a higher energy density and better cycle performance.

[0004] A positive electrode material, comprising a positive electrode active material and a coating layer located on at least a portion of the surface of the positive electrode active material, wherein the positive electrode active material comprises a chemical formula of Li a Fe 1-b M b PO4 material and C material, the coating layer includes a chemical formula of Li m Fe 1-n M' n PO4-CN material, wherein 0.95≤a≤1.1, 0.4≤b≤0.9, 0.95≤m≤1.1, 0.4≤n≤0.9, M and M' independently include other transition metal elements except Fe.

[0005] In the above-mentioned positive electrode material, the chemical formula of Li a Fe 1-b M b The coating of the positive electrode active material of PO4 can reduce the dissolution of the transition metal element M in the positive electrode active material, prolong the service life of the positive electrode material, and further prolong the cycle performance of the positive electrode active material. At the same time, in the above-mentioned positive electrode material, the introduction of the transition metal element can increase the gram capacity of the positive electrode material. Therefore, the above-mentioned positive electrode material has a higher gram capacity and better cycle performance. The application of the positive electrode material in the battery can make the battery have both higher energy density and better cycle performance.

[0006] In some embodiments, the coating layer includes a sheet-like coating and a granular coating, wherein the sheet-like coating includes a chemical formula of Li m Fe 1-n M' n PO4-CN material, the granular coating includes the C material.

[0007] In some embodiments, the sheet-like coating and the particle-like coating are distributed at intervals on the surface of the positive electrode active material.

[0008] In some embodiments, the granular coating is distributed on the surface of the positive electrode active material, part of the sheet-like coating is connected to the surface of the granular coating, and part of the sheet-like coating is connected to the surface of the positive electrode active material.

[0009] In some embodiments, the thickness of the sheet-like coating is 2 nm to 5 nm.

[0010] In some embodiments, the length of the plate-like coating is ≥ 100 nm.

[0011] In some embodiments, the particle size of the granular coating is 10 nm to 100 nm.

[0012] In some embodiments, in the positive electrode material, the mass percentage of N element in the positive electrode material is 0.005% to 0.5%.

[0013] In some embodiments, in the positive electrode material, the mass percentage of C element in the positive electrode material is 1% to 2%.

[0014] In some embodiments, M and M′ independently include at least one of Mg, Al, Ca, Ti, Mn, Co, Ni, Cu, Zn, Zr, Nb, and Mo.

[0015] A method for preparing the positive electrode material comprises the following steps: The positive electrode active material, carbon source, lithium source, M' source, phosphorus source and Prussian blue material are mixed in a solvent to obtain a slurry. The Prussian blue material includes a chemical formula of M' x Fe 4-x [Fe(CN)6]3 materials, where 0≤x≤4; The slurry is spray-dried to obtain a precursor; The precursor is calcined under a protective gas atmosphere.

[0016] In some embodiments, the molar percentage of Fe in the Prussian blue material to Li in the slurry is 0.3% to 5%.

[0017] In some embodiments, the carbon source includes at least one of glucose, sucrose, citric acid, starch and polyethylene glycol.

[0018] In some embodiments, the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, trilithium phosphate, and lithium oxalate.

[0019] In some embodiments, the source of M' comprises an oxide of M'.

[0020] In some embodiments, the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, trilithium phosphate, and lithium dihydrogen phosphate.

[0021] In some embodiments, the outlet air temperature of the spray drying is controlled to be 90°C to 110°C; the temperature of the calcination treatment is 600°C to 750°C; and the time of the calcination treatment is 6h to 20h.

[0022] A positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active layer contains the positive electrode material or the positive electrode material prepared by the preparation method.

[0023] A battery comprises the positive electrode plate.

[0024] In some embodiments, the total dissolution amount of Fe and the other transition metal elements in the battery is 25 ppm to 55 ppm.

[0025] An electrical device comprises the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope (SEM) image of the positive electrode material in Example 1 of the present application.

[0027] Figure 2 This is a SEM image of the positive electrode material in Example 1 under another scale.

[0028] Figure 3 This is an X-ray photoelectron spectroscopy (XPS) diagram of the positive electrode material in Example 1.

[0029] Figure 4 This is the fitting spectrum of the N element in the positive electrode material in Example 1.

[0030] Figure 5 This is the fitting spectrum of the Fe element in the positive electrode material in Example 1.

[0031] Figure 6 This is the fitting spectrum of Li and C elements in the positive electrode material in Example 1.

[0032] Figure 7 This is the X-ray diffraction (XRD) diagram of the positive electrode material in Example 1. DETAILED DESCRIPTION

[0033] In order to make the above-mentioned purpose, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0034] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0035] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0037] One embodiment of the present application provides a positive electrode material. The positive electrode material includes a positive electrode active material and a coating layer located on at least a portion of the surface of the positive electrode active material. The positive electrode active material includes a chemical formula of Li a Fe 1-b M b PO4 material, the coating layer includes a chemical formula of Li m Fe 1-n M' nPO4-CN material and C material, wherein 0.95≤a≤1.1, 0.4≤b≤0.9, 0.95≤m≤1.1, 0.4≤n≤0.9, M and M' independently include other transition metal elements except Fe. In the positive electrode material of this embodiment, by a Fe 1-b M b The positive electrode active material of the material of PO4 is coated, which can reduce the dissolution of the transition metal element M in the positive electrode active material, prolong the service life of the positive electrode material, and then prolong the cycle performance of the positive electrode active material. At the same time, in the positive electrode material of this embodiment, the introduction of the transition metal element can increase the gram capacity of the positive electrode material. Therefore, the positive electrode material of this embodiment has a higher gram capacity and better cycle performance. The positive electrode material is applied to the battery, which can make the battery have both higher energy density and better cycle performance.

[0038] Optionally, in Li a Fe 1-b M b In PO4, a may be, but is not limited to, 0.95, 0.98, 1, 1.05, 1.1, and any value in a range consisting of any two of these values. b may be, but is not limited to, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and any value in a range consisting of any two of these values.

[0039] Optionally, in Li m Fe 1-n M' n In PO4-CN, m can be, but is not limited to, 0.95, 0.98, 1, 1.05, 1.1, and any value in a range consisting of any two of these values. n can be, but is not limited to, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and any value in a range consisting of any two of these values. It is understood that Li m Fe 1-n M' n PO4-CN represents Li m Fe 1-n M' n PO4 is connected to a cyano group (-CN).

[0040] In some embodiments, as some optional examples of M and M', M and M' independently include at least one of Mg, Al, Ca, Ti, Mn, Co, Ni, Cu, Zn, Zr, Nb and Mo. That is, M includes at least one of Mg, Al, Ca, Ti, Mn, Co, Ni, Cu, Zn, Zr, Nb and Mo. M' includes at least one of Mg, Al, Ca, Ti, Mn, Co, Ni, Cu, Zn, Zr, Nb and Mo.

[0041] In some embodiments, in the positive electrode material, M and M' are the same, so that in the positive electrode material, the coating layer and the positive electrode active material maintain a high consistency in elemental composition, so that the coating layer and the positive electrode active material are better matched, and the contribution to the gram capacity and cycle performance of the positive electrode material is more fully demonstrated. Further, in the positive electrode material, M and M' are the same, a and m are the same, and b and n are the same, which can further promote the matching of the coating layer and the positive electrode active material, and further improve the gram capacity and cycle performance of the positive electrode material.

[0042] In some embodiments, the coating layer includes a sheet-like coating and a granular coating, wherein the sheet-like coating includes a chemical formula of Li m Fe 1-n M' n PO4-CN material, the granular coating includes the C material. The coexistence of the sheet coating and the granular coating can make the coating layer show a better coating effect, further promoting the improvement of the positive electrode material's gram capacity and cycle performance. The chemical formula is Li m Fe 1-n M' n The PO4-CN material as a sheet coating can further inhibit the dissolution of transition metal elements in the positive electrode active material, thereby further improving the cycle performance of the positive electrode material and maintaining a high gram capacity of the positive electrode material. m Fe 1-n M' n The PO4-CN material contains cyano groups (-CN), and the sheet-like coating can be combined with the positive electrode active material and / or the particulate coating through the cyano groups.

[0043] In some embodiments, the sheet-like coating and the granular coating are distributed at intervals on the surface of the positive electrode active material. It is understood that the sheet-like coating and the granular coating are distributed at intervals on the surface of the positive electrode active material, indicating that on the surface of the positive electrode active material, there are gaps between the sheet-like coatings, and the granular coating is located in the gaps between adjacent sheet-like coatings. At the same time, there are gaps between the granular coatings, and the sheet-like coating is located between adjacent granular coatings. When the sheet-like coating and the granular coating are distributed at intervals on the surface of the positive electrode active material, the sheet-like coating and the granular coating can play a better role and synergistically promote the further improvement of the cycle performance and gram capacity of the positive electrode material.

[0044] In some embodiments, the particulate coating is distributed on the surface of the positive electrode active material, part of the plate-like coating is connected to the surface of the particulate coating, and part of the plate-like coating is connected to the surface of the positive electrode active material.

[0045] In some embodiments, the thickness of the sheet-like coating is 2 nm to 5 nm. For example, the thickness of the sheet-like coating can be, but is not limited to, 2 nm, 3 nm, 4 nm, 5 nm, and any value in a range consisting of any two of these values.

[0046] In some embodiments, the length of the sheet-like coating is ≥100 nm. For example, the length of the sheet-like coating can be, but is not limited to, 150 nm, 180 nm, 200 nm, 220 nm, 250 nm, 280 nm, 300 nm, 400 nm, 700 nm, and any value in a range of values ​​consisting of any two of these values. Optionally, the length of the sheet-like coating is 100 nm to 1000 nm.

[0047] In some embodiments, the particle size of the granular coating is 10 nm to 100 nm. For example, the particle size of the granular coating can be, but is not limited to, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, and any value in a numerical range consisting of any two of these values.

[0048] In some embodiments, in the positive electrode material, the mass percentage of the N element in the positive electrode material is 0.005% to 0.5%. For example, the mass percentage of the N element in the positive electrode material can be, but is not limited to, 0.005%, 0.01%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, and any value in a numerical range consisting of any two of these values.

[0049] In some embodiments, the mass percentage of the C element in the positive electrode material is 1% to 2%. Optionally, the mass percentage of the C element in the positive electrode material can be, but is not limited to, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, and any value in a numerical range consisting of any two of these values.

[0050] It can be understood that, in the positive electrode material, a portion of the N element is used to form a cyano group, and a portion of the C element is used to form a cyano group.

[0051] In some embodiments, the cathode material includes spherical secondary particles.

[0052] Another embodiment of the present application provides a method for preparing the above-mentioned positive electrode material. The method for preparing the positive electrode material comprises the following steps: The positive electrode active material, the carbon source, the lithium source, the M' source, the phosphorus source and the Prussian blue material are mixed in a solvent to obtain a slurry, wherein the Prussian blue material includes a chemical formula of M' x Fe 4-x [Fe(CN)6]3 materials, where 0≤x≤4; The slurry is spray-dried to obtain a precursor; The precursor is calcined under a protective gas atmosphere.

[0053] In the preparation method of this embodiment, based on the coating of the positive electrode active material with the Prussian blue material, during the preparation process, a lithium source, an M' source, and a phosphorus source are introduced to obtain a slurry, and then the slurry is spray-dried and calcined to generate a Li+ / -2-carbon nanotube on the surface of the positive electrode active material. m Fe 1-n M' n The coating layer of PO4-CN material enables the obtained positive electrode material to have both higher gram capacity and better cycle performance.

[0054] In some embodiments, the molar percentage of Fe in the Prussian blue material to the Li in the slurry is 0.3% to 5%. The molar percentage of Fe in the Prussian blue material to the Li in the slurry can further reduce the total dissolution amount of Fe and other transition metal elements within this range. Optionally, the molar percentage of Fe in the Prussian blue material to the Li in the slurry can be but is not limited to 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% and any value in the numerical range consisting of any two of these values. Further optionally, the molar percentage of Fe in the Prussian blue material to the Li in the slurry is 0.3% to 0.5%.

[0055] In some embodiments, when the positive electrode active material, the carbon source, the lithium source, the M' source, the phosphorus source and the Prussian blue material are mixed in a solvent, the lithium source, the M' source and the phosphorus source can be first mixed in a solvent to obtain a first mixed solution, and then the first mixed solution is added to the second mixed solution including the carbon source and the positive electrode active material to obtain a third mixed solution. Then the Prussian blue material is added to the third mixed solution. It is understood that during the mixing process, the mixed solution is stirred and mixed to promote mixing. Optionally, the temperature of the stirring and mixing is 25°C, the time of the stirring and mixing is 0.5h, and the frequency of the stirring and mixing is 20Hz. Further, after the Prussian blue material is added to the third mixed solution, the obtained mixed solution is ball milled to further promote mixing. Optionally, the temperature of the ball milling is 25°C, the time of the ball milling is 4h, and the speed of the ball milling is 200r / min.

[0056] In some embodiments, when the positive electrode active material, the carbon source, the lithium source, the M' source, the phosphorus source and the Prussian blue material are mixed in a solvent, the solvent used is deionized water.

[0057] In some embodiments, the carbon source includes at least one of glucose, sucrose, citric acid, starch and polyethylene glycol. The lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, trilithium phosphate and lithium oxalate. The M' source includes an oxide of M'. The phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, trilithium phosphate and lithium dihydrogen phosphate.

[0058] In some embodiments, the temperature of spray drying is 90°C to 110°C. The temperature of calcination is 600°C to 750°C. The time of calcination is 6h to 20h. Alternatively, the temperature of spray drying can be but is not limited to 90°C, 95°C, 100°C, 105°C, 110°C, and any value in the numerical range consisting of any two of these values. The temperature of calcination is 600°C, 620°C, 650°C, 680°C, 700°C, 720°C, 750°C, and any value in the numerical range consisting of any two of these values. The time of calcination is 6h, 8h, 10h, 12h, 15h, 18h, 20h, and any value in the numerical range consisting of any two of these values.

[0059] Another embodiment of the present application provides a positive electrode sheet, which includes a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active layer contains the positive electrode material or the positive electrode material prepared by the preparation method.

[0060] Another embodiment of the present application provides a battery. The battery includes the above-mentioned positive electrode plate.

[0061] In some embodiments, the total dissolution amount of Fe and other transition metal elements in the battery is 25ppm to 55ppm. For example, the total dissolution amount of Fe and other transition metal elements in the battery is 25ppm, 30ppm, 35ppm, 40ppm, 45ppm, 50ppm, 55ppm, and any value in the numerical range consisting of any two of these values.

[0062] Another embodiment of the present application provides an electric device, which includes the above-mentioned battery.

[0063] Example 1 The preparation method of the positive electrode material in this embodiment includes: S101: Mix lithium carbonate, manganese tetraoxide and phosphoric acid in deionized water to obtain a first mixed solution.

[0064] S102: Add the first mixed solution including carbon source PEG-2000 and glucose (Glu) and positive electrode active material LiFe 0.4 Mn 0.6 PO4 in the second mixed solution to obtain a third mixed solution.

[0065] S103: Add the Prussian blue material Fe4[Fe(CN)6]3 to the third mixed solution, stir and mix, and obtain a slurry. The molar percentage of Fe in the Prussian blue material to Li in the slurry is 0.5%. The stirring and mixing temperature is 25°C, the stirring and mixing time is 0.5h, and the stirring and mixing frequency is 20Hz.

[0066] S104: ball milling the slurry obtained in S103. The ball milling temperature is 25° C., the ball milling time is 4 h, and the ball milling speed is 200 r / min.

[0067] S105: spray-dry the slurry to obtain a precursor. The spray-drying temperature is 110°C.

[0068] S106: calcining the precursor in a nitrogen atmosphere at a temperature of 600° C. for 20 hours.

[0069] S107: After the calcination treatment, the mixture is naturally cooled to obtain the positive electrode material in this embodiment.

[0070] Compared with Example 1, the differences between Examples 2 to 5 and Comparative Examples 1 to 2 are shown in Table 1.

[0071] Table 1

[0072] Figure 1 is a SEM image of the positive electrode material in Example 1. Figure 1 It can be seen that the cathode material is in the form of spherical secondary particles.

[0073] Figure 2 is a SEM image of the positive electrode material in Example 1 under another scale. Figure 2 It can be seen that the coating layer of the positive electrode material includes a sheet-like coating and a granular coating, wherein the length of the sheet-like coating is between 100nm and 1000nm, and the particle size of the granular coating is within 100nm.

[0074] Figure 3 This is the XPS overall spectrum of the positive electrode material in Example 1.

[0075] Figure 4 This is the N1s fitting spectrum of the positive electrode material in Example 1. The binding energy is at 400.87 eV, which is consistent with the peak position corresponding to C-NH2, indicating that there is a CN bond structure in the positive electrode material.

[0076] Figure 5 This is the fitting spectrum of the Fe element of the positive electrode material in Example 1. The peaks near 711eV and 725eV correspond to Fe2p3 / 2, respectively, and Fe2p1 / 2 is blue-shifted, indicating that Fe atoms form coordination bonds Fe-C≡N-Fe with C atoms and N atoms, respectively, and an interface with high electronic conductivity and high ionic conductivity is formed between the positive electrode active material and the coating layer, inducing rapid movement of electrons and rapid deintercalation and embedding of ions in the positive electrode material, thereby obtaining a positive electrode material with high electronic conductivity and high ionic conductivity.

[0077] Figure 6 Li and CO3 are the positive electrode materials in Example 1 2- Spectrum, fitting the peaks yields 54.84eV and 55.67eV, corresponding to Li1s and CO3, respectively. 2- Peak position.

[0078] Figure 7 This is the XRD spectrum of the positive electrode material in Example 1, corresponding to the lithium iron phosphate structure, with no obvious impurity peaks, the material purity is high, and there is no obvious impurity phase.

[0079] The gram capacity and battery cycle performance of the positive electrode materials of the embodiments and comparative examples were tested.

[0080] The test method is: 1. Button cell production: Made of 2032 standard battery shell, the positive electrode ratio is positive electrode material: SP: PVDF = 9: 0.5: 0.5, the pole piece compaction density is 2.0g / cm 3 , the active material loading is 6 mg, and the negative electrode material is Li sheet.

[0081] 2. The gram capacity of button batteries is tested according to the theoretical capacity of 150mAh / g, 0.1C, 2.5V~4.5V.

[0082] 3. Cycle retention rate of button battery: voltage window is 2.5V~4.3V, charge and discharge 100 times under 1C condition, take the average value of the first three cycle capacities as the initial gram capacity, and the average value of the last three cycle gram capacity as the final gram capacity, and the cycle retention rate is final gram capacity / initial gram capacity×100%.

[0083] 4. The Mn+Fe dissolution test method is: after completing 100 cycles, the battery is discharged to 2.0V and disassembled, the negative electrode material is taken, and the Mn and Fe contents therein are detected by ICP-OES and added.

[0084] The coating layer of Comparative Example 1 is a carbon coating layer, and the coating layer of Comparative Example 2 is a Prussian blue coating layer. Compared with Comparative Examples 1 to 2, the batteries in Examples 1 to 5 can better balance higher energy density and higher cycle retention rate. This shows that the coating layer includes a chemical formula of Li m Fe 1-n M' n PO4-CN materials and C materials can improve the energy density and cycle performance of positive electrode materials.

[0085] It can be seen from Examples 1 to 3 that when the molar percentage of Fe in the Prussian blue material to Li in the slurry is within an appropriate range, the amount of Mn+Fe dissolved in the battery can be reduced.

[0086] It can be seen from Examples 2, 4, and 5 that the positive electrode active material includes a chemical formula of Li a Fe 1-b M b PO4 materials, the battery can obtain higher energy density and better cycle performance.

[0087] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0088] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application.

Claims

1. A positive electrode material, characterized in that: The invention comprises a positive electrode active material and a coating layer located on at least a portion of the surface of the positive electrode active material, wherein the positive electrode active material comprises a positive electrode having a chemical formula of Li a Fe 1-b M b PO4 material, the coating layer includes a chemical formula of Li m Fe 1-n M' n PO4-CN material and C material, wherein 0.95≤a≤1.1, 0.4≤b≤0.9, 0.95≤m≤1.1, 0.4≤n≤0.9, M and M' independently include other transition metal elements except Fe.

2. The positive electrode material according to claim 1, characterized in that The coating layer includes a sheet-like coating and a granular coating, wherein the sheet-like coating includes a chemical formula of Li m Fe 1-n M' n PO4-CN material, the granular coating includes the C material.

3. The positive electrode material according to claim 2, characterized in that The sheet-like covering and the particle-like covering are distributed on the surface of the positive electrode active material at intervals.

4. The positive electrode material according to claim 2, characterized in that The granular coating is distributed on the surface of the positive electrode active material, part of the sheet-like coating is connected to the surface of the granular coating, and part of the sheet-like coating is connected to the surface of the positive electrode active material.

5. The positive electrode material according to claim 2, characterized in that The coating layer satisfies at least one of the following characteristics: (1) The thickness of the sheet-like coating is 2 nm to 5 nm; (2) The length of the sheet-like coating is ≥100 nm; (3) The particle size of the granular coating is 10nm~100nm.

6. The positive electrode material according to any one of claims 1 to 5, characterized in that The positive electrode material satisfies at least one of the following characteristics: (1) In the positive electrode material, the mass percentage of N element in the positive electrode material is 0.005% to 0.5%; (2) In the positive electrode material, the mass percentage of C element in the positive electrode material is 1% to 2%; (3) M and M′ independently include at least one of Mg, Al, Ca, Ti, Mn, Co, Ni, Cu, Zn, Zr, Nb and Mo.

7. A method for preparing the positive electrode material according to any one of claims 1 to 6, characterized in that: The steps include: The positive electrode active material, carbon source, lithium source, M' source, phosphorus source and Prussian blue material are mixed in a solvent to obtain a slurry. The Prussian blue material includes a chemical formula of M' x Fe 4-x [Fe(CN)6]3 materials, where 0≤x≤4; The slurry is spray-dried to obtain a precursor; The precursor is calcined under a protective gas atmosphere.

8. The method for preparing the positive electrode material according to claim 7, characterized in that: The molar percentage of Fe in the Prussian blue material to Li in the slurry is 0.3% to 5%.

9. The method for preparing a positive electrode material according to any one of claims 7 to 8, characterized in that: The carbon source comprises at least one of glucose, sucrose, citric acid, starch and polyethylene glycol; and / or, The lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, trilithium phosphate and lithium oxalate; and / or, The M' source comprises an oxide of M'; and / or, The phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, trilithium phosphate and lithium dihydrogen phosphate.

10. The method for preparing a positive electrode material according to any one of claims 7 to 8, characterized in that: The outlet air temperature of the spray drying is controlled to be 90°C to 110°C; the temperature of the calcination treatment is 600°C to 750°C; and the time of the calcination treatment is 6h to 20h.

11. A positive electrode sheet, characterized in that: The invention comprises a positive electrode current collector and a positive electrode active layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active layer contains the positive electrode material according to any one of claims 1 to 6 or the positive electrode material prepared by the preparation method according to any one of claims 7 to 10.

12. A battery, characterized in that: Including the positive electrode sheet as claimed in claim 11.

13. The battery according to claim 12, characterized in that The total dissolution amount of Fe and other transition metal elements in the battery is 25ppm~55ppm.

14. An electrical device, characterized in that: A battery comprising the battery according to any one of claims 12 to 13.

Citation Information

Patent Citations

  • Core-shell composite anode material for lithium ion battery and preparation method thereof

    CN101740752A

  • LiFePO4 / N combination electrode material and preparation method thereof

    CN101894942A

  • Surface modified positive electrode material and preparation method and application thereof

    CN107240676A

  • A lithium ion battery composite cathode material and a preparation method thereof

    CN109273683A

  • Double-coated lithium iron phosphate cathode material and preparation method thereof

    CN109888281A