Lithium ion battery, negative pole piece and electric device
By designing a stacked structure in the negative electrode sheet of lithium-ion batteries, using artificial graphite and natural graphite to optimize particle size and porosity, the problem of taking into account both fast charging performance and energy density is solved, and efficient battery performance improvement is achieved.
Patent Information
- Application Number
- CN202411465863.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
While improving the fast charging performance, existing lithium-ion batteries are difficult to take into account both energy density. Usually, the fast charging performance is improved by increasing the porosity of the pole, but the energy density is lost.
By designing a stacked structure in the negative electrode sheet, using artificial graphite and natural graphite as the negative electrode active materials, adjusting their particle size, powder compaction density and porosity, reasonably matching the first and second negative electrode active material layers to optimize the activity The liquid phase diffusion path of the ions ensures both fast charging performance and energy density.
It achieves the improvement of the energy density of the battery while maintaining high fast charging performance and reduces the energy density loss due to high porosity, thereby improving the overall performance of the battery.
Smart Images

Figure CN118970041A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a lithium-ion battery, a negative electrode sheet and an electrical device. Background Art
[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0003] In recent years, as the application scope of secondary batteries represented by lithium-ion batteries has become more and more extensive, secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. As secondary batteries have made great progress, higher requirements have been put forward for their energy density, fast charging performance, etc. Summary of the invention
[0004] The present application provides a lithium-ion battery, a negative electrode plate and an electrical device. The lithium-ion battery has a relatively high fast charging performance while also taking into account energy density to a certain extent.
[0005] In order to achieve the above-mentioned object, the first aspect of the present application provides a lithium ion battery, comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector;
[0006] The negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, wherein the second negative electrode active material layer is disposed between the negative electrode current collector and the first negative electrode active material layer;
[0007] The first negative electrode active material layer contains a first negative electrode active material, the second negative electrode active material layer contains a second negative electrode active material, the first negative electrode active material includes artificial graphite, the second negative electrode active material includes one or both of natural graphite and artificial graphite, and at least one of the two is natural graphite, the volume average particle size of the first negative electrode active material is Dv501, the volume average particle size of the second negative electrode active material is Dv502, and Dv501 <Dv502;
[0008] The powder compaction density of the first negative electrode active material under a pressure of 5T is ρ1, and the powder compaction density of the second negative electrode active material under a pressure of 5T is ρ2, 0g / cm 3 <ρ2-ρ1≤0.55g / cm 3 ;
[0009] The porosity of the negative electrode plate is P, and 18%≤P≤25%.
[0010] In some embodiments of the present application, the relationship between ρ1 and ρ2 satisfies: 0 g / cm 3 ≤ρ2-ρ1≤0.55g / cm 3 .
[0011] In some embodiments of the present application, the relationship between ρ1 and ρ2 satisfies: 0.05 g / cm 3 ≤ρ2-ρ1≤0.55g / cm 3 .
[0012] In some embodiments of the present application, at least one of the following conditions is met:
[0013] (1) The Dv501 satisfies: 4μm≤Dv501≤16μm;
[0014] (2) The Dv502 satisfies: 8μm≤Dv502≤23μm.
[0015] In some embodiments of the present application, at least one of the following conditions is met:
[0016] (1) The Dv501 satisfies: 4μm≤Dv501≤15.5μm;
[0017] (2) The Dv502 satisfies: 8 μm ≤ Dv502 ≤ 21 μm.
[0018] In some embodiments of the present application, at least one of the following conditions is met:
[0019] (1) The ρ1 satisfies: 1.4 g / cm 3 ≤ρ1≤2g / cm 3 ;
[0020] (2) The ρ2 satisfies: 1.5 g / cm 3 ≤ρ2≤2.2g / cm 3 .
[0021] In some embodiments of the present application, at least one of the following conditions is met:
[0022] (1) The ρ1 satisfies: 1.5 g / cm 3 ≤ρ1≤2g / cm 3 ;
[0023] (2) The ρ2 satisfies: 1.65 g / cm 3 ≤ρ2≤2.1g / cm 3 .
[0024] In some embodiments of the present application, at least one of the following conditions is met:
[0025] (1) The OI value of the first negative electrode active material is 1.5 to 15;
[0026] (2) The OI value of the second negative electrode active material is 3 to 30.
[0027] In some embodiments of the present application, at least one of the following conditions is met:
[0028] (1) The OI value of the first negative electrode active material is 2 to 10;
[0029] (2) The OI value of the second negative electrode active material is 3-25.
[0030] In some embodiments of the present application, at least one of the following conditions is met:
[0031] (1) The tap density of the first negative electrode active material and the second negative electrode active material is independently 0.9 g / cm 3 ~1.2g / cm 3 ;
[0032] (2) The particle size distribution of the first negative electrode active material satisfies: span1≤1.6, span1=(Dv901-Dv101) / Dv501;
[0033] (3) The particle size distribution of the second negative electrode active material satisfies: span2≤1.6, span2=(Dv902-Dv102) / Dv502.
[0034] In some embodiments of the present application, at least one of the following conditions is met:
[0035] (1) The particle size distribution of the first negative electrode active material satisfies: span1≤1.4, span1=(Dv901-Dv101) / Dv501;
[0036] (2) The particle size distribution of the second negative electrode active material satisfies: span2≤1.4, span2=(Dv902-Dv102) / Dv502.
[0037] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include a silicon-based material.
[0038] In some embodiments of the present application, the mass percentage of the silicon-based material in the first negative electrode active material layer and the second negative electrode active material layer is independently less than or equal to 9%.
[0039] In some embodiments of the present application, the first negative electrode active material includes a silicon-based material, and the double-sided thickness of the first negative electrode active material layer is 80 mm to 170 mm.
[0040] In some embodiments of the present application, at least one of the following conditions is met:
[0041] (1) The sphericity of the natural graphite is 0.55-0.9;
[0042] (2) The degree of graphitization of the natural graphite is 92% to 99%;
[0043] (3) The degree of graphitization of the artificial graphite is 88% to 96%.
[0044] In some embodiments of the present application, the first negative electrode active material layer and the second negative electrode active material layer further independently contain a binder, and the mass proportions of the binder in the first negative electrode active material layer and the second negative electrode active material layer are ω1 and ω2, respectively, and ω1<ω2.
[0045] In some embodiments of the present application, 0.5%≤ω2≤5%.
[0046] In some embodiments of the present application, in the second negative electrode active material layer, the binder includes a first binder, and the first binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, styrene acrylic resin and carboxymethyl chitosan.
[0047] In some embodiments of the present application, in the second negative electrode active material layer, the binder further includes a second binder, the glass transition temperature of the first binder is Tg1, the glass transition temperature of the second binder is Tg2, and Tg2 <Tg1。
[0048] In some embodiments of the present application, the second binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, styrene acrylic resin and acrylate compounds, and the second binder is different from the first binder.
[0049] In some embodiments of the present application, in the second negative electrode active material layer, the mass ratio of the second binder to the first binder is σ, and 0≤σ≤10.
[0050] In some embodiments of the present application, the binder contains lithium ions.
[0051] In some embodiments of the present application, an electrolyte is further included, wherein the ionic conductivity of the electrolyte at 25° C. is 10 mS / cm to 20 mS / cm.
[0052] In some embodiments of the present application, the ionic conductivity of the electrolyte is 13mS / cm~20mS / cm.
[0053] The negative electrode sheet in the lithium-ion battery provided by the present application can make the liquid phase diffusion path of active ions in the negative electrode shorter, the active ion conduction more linear, and the number of diffusion paths larger through the reasonable matching of the particle size of the negative electrode active material in the first negative electrode active material layer and the second negative electrode active material layer, the powder compaction density and the negative electrode sheet porosity; at the same time, the porosity of the negative electrode sheet can be adjusted to a suitable range, which can reduce the loss of energy density caused by high porosity. In this way, the battery can have high fast charging performance and also take into account energy density to a certain extent.
[0054] A second aspect of the present application further provides a negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector;
[0055] The negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, wherein the second negative electrode active material layer is disposed between the negative electrode current collector and the first negative electrode active material layer;
[0056] The first negative electrode active material layer contains a first negative electrode active material, the second negative electrode active material layer contains a second negative electrode active material, the first negative electrode active material includes artificial graphite, the second negative electrode active material includes one or both of natural graphite and artificial graphite, and at least one of the two is natural graphite, the volume average particle size of the first negative electrode active material is Dv501, the volume average particle size of the second negative electrode active material is Dv502, and Dv501 <Dv502;
[0057] The powder compaction density of the first negative electrode active material under a pressure of 5T is ρ1, and the powder compaction density of the second negative electrode active material under a pressure of 5T is ρ2, 0g / cm 3 <ρ2-ρ1≤0.55g / cm 3 ;
[0058] The porosity of the negative electrode plate is P, and 18%≤P≤25%.
[0059] In some embodiments of the present application, the negative electrode plate is the negative electrode plate in the lithium-ion battery described in the first aspect of the present application.
[0060] A third aspect of the present application provides an electrical device, comprising the lithium-ion battery of the first aspect of the present application.
[0061] The electric device of the present application includes the lithium-ion battery provided by the present application, and thus has at least the same advantages as the lithium-ion battery.
[0062] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0063] In order to better describe and illustrate the embodiments or examples provided by the present application, reference may be made to one or more drawings. The additional details or examples used to describe the drawings should not be considered as limiting the scope of the disclosed application, the embodiments or examples currently described, and any of the best modes of these applications currently understood. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0064] Figure 1 It is a schematic diagram of a battery cell according to an embodiment of the present application.
[0065] Figure 2 for Figure 1 An exploded view of a battery cell according to an embodiment of the present application is shown.
[0066] Figure 3 FIG. 1 is a schematic diagram of a battery device according to an embodiment of the present application.
[0067] Figure 4 A schematic diagram of a battery pack according to an embodiment of the present application.
[0068] Figure 5 for Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown.
[0069] Figure 6 A schematic diagram of an electrical device using a lithium-ion battery as a power source according to an embodiment of the present application.
[0070] Description of reference numerals:
[0071] 1 battery pack; 2 upper box; 3 lower box; 4 battery device; 5 battery cell; 51 shell; 52 electrode assembly; 53 cover plate; 6 power-consuming device. DETAILED DESCRIPTION
[0072] Below, some embodiments of the lithium-ion battery, negative electrode plate and electrical device of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0073] "Scope" disclosed in the present application can be limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or excluding end values, and any end value can be included or not included independently, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 listed, and if the maximum range values 3,4 and 5 are also listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation for these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to listing the parameter as, for example, integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For example, when a parameter is expressed as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0074] In the present application, "plurality", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0075] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0076] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment or implementation of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. The "implementation methods" mentioned herein have a similar understanding.
[0077] Those skilled in the art will appreciate that, in the methods of each embodiment or example, the order in which each step is written does not mean a strict order of execution and does not constitute any limitation on the implementation process, and the detailed order of execution of each step should be determined by its function and possible internal logic. If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) can be added to the method in any order, for example, the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), etc.
[0078] In this application, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel schemes of "yes" or "no". If there are multiple "options" in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "option" is independent.
[0079] At present, in order to improve the fast charging performance of lithium-ion batteries, the method usually adopted is to improve the overall porosity of the pole piece. For example, by increasing the porosity of the pole piece, the diffusion path of the active ions can be increased, thereby improving the fast charging performance. However, the method of improving the fast charging performance by increasing the porosity of the pole piece will simultaneously lead to a loss of energy density, making it difficult to achieve a balance between fast charging performance and energy density.
[0080] Based on this, the present application provides a lithium-ion battery, in which the design is performed for the negative electrode plate, that is, by optimizing the intrinsic parameters of the negative electrode active material in the negative electrode plate, and combining the matching design of different layers of the negative electrode active material layer in the negative electrode plate, the battery can have a higher fast charging performance while also taking into account the energy density to a certain extent.
[0081] In a first aspect, the present application provides a lithium ion battery, comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector;
[0082] The negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, wherein the second negative electrode active material layer is disposed between the negative electrode current collector and the first negative electrode active material layer;
[0083] The first negative electrode active material layer contains a first negative electrode active material, the second negative electrode active material layer contains a second negative electrode active material, the first negative electrode active material includes artificial graphite, the second negative electrode active material includes one or both of natural graphite and artificial graphite, and at least one of the two is natural graphite, the volume average particle size of the first negative electrode active material is Dv501, the volume average particle size of the second negative electrode active material is Dv502, and Dv501 <Dv502;
[0084] The powder compaction density of the first negative electrode active material under a pressure of 5T is ρ1, and the powder compaction density of the second negative electrode active material under a pressure of 5T is ρ2, 0g / cm 3 <ρ2-ρ1≤0.55g / cm 3 ;
[0085] The porosity of the negative electrode plate is P, and 18%≤P≤25%.
[0086] In some embodiments, P may be 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, or a range thereof.
[0087] In the lithium-ion battery provided in the present application, the negative electrode active material layer in the negative electrode plate is arranged in a stacked manner. The first negative electrode active material in the first negative electrode active material layer (also referred to as the "upper layer" herein) has a relatively small particle size and the same or relatively low powder compaction density. The material is not easy to deform laterally when under pressure, so it is not easy to cause the filling of the pores in the upper layer area, so that the pores in the upper layer are relatively richer, which is conducive to improving the fast charging performance. The second negative electrode active material in the second negative electrode active material layer (also referred to as the "lower layer" herein) has a relatively large particle size and the same or relatively high powder compaction density. The material can serve as the main load-bearing party when under pressure and is easy to deform, so the pores in the lower layer are relatively fewer, which is conducive to maintaining energy density.
[0088] On this basis, the porosity of the negative electrode sheet is adjusted to a suitable range, so that within the porosity range, when the porosity is relatively high, the fast charging performance can be better; when the porosity is relatively low, the energy density drop caused by excessively high porosity can be reduced, and a higher energy density can be obtained. In this way, adjusting the porosity of the negative electrode sheet within this range can not only make the sheet have better fast charging performance, but also take into account the energy density to a certain extent.
[0089] At the same time, the first negative electrode active material includes artificial graphite, and the second negative electrode active material includes one or two of natural graphite and artificial graphite, and when at least one of them is natural graphite, the graphitization degree of the first negative electrode active material and the second negative electrode active material is higher than that of other carbon materials, and is easier to deform, thereby easily achieving the adjustment of the number of pores in the upper and lower layers of the pole piece, as well as the adjustment of the porosity of the pole piece. And the graphite has a strong ability to conduct electrons, which is conducive to the improvement of the fast charging performance of the pole piece. In addition, the volume expansion of graphite after cycling is small, which can reduce the extrusion and filling of the pole piece pores due to cyclic expansion, so that the porosity of the pole piece can basically maintain the state before the cycle; and the cost of graphite is low, which is conducive to the mass production of the lithium-ion battery provided in this application.
[0090] What is more critical is that when the first negative electrode active material includes artificial graphite, the hardness of artificial graphite is relatively higher, which can reduce the deformation when the cold pressing roller directly contacts and presses it, and can reduce the filling of the upper pores, so that the upper pores are relatively more; and the graphitization degree of artificial graphite is relatively higher, the interlayer spacing is relatively small, and it has a stronger ability to conduct electrons, which is conducive to comprehensively improving the fast charging performance of the negative electrode. The lower layer is relatively far away from the cold pressing roller, and can serve as the main force-bearing party when under pressure. Based on this, when the second negative electrode active material includes one or both of artificial graphite and natural graphite, and at least one of them is natural graphite, the second negative electrode active material, especially the natural graphite therein, is relatively easier to deform when under pressure, and can squeeze and fill the pores of the lower layer through deformation, so that the pores of the lower layer are relatively less, which is conducive to suppressing the reduction of the energy density of the negative electrode. In this way, by matching the artificial graphite in the first negative electrode active material layer with the natural graphite included in the second negative electrode active material layer, the battery can have a higher fast charging performance while also taking into account the energy density, so that the matching effect between the first negative electrode active material layer and the second negative electrode active material layer is better. If the first negative electrode active material is natural graphite, since natural graphite is more easily deformed when pressed than artificial graphite, it is the upper material that directly contacts the cold pressing roller. It is very easy to be pressed and deformed (especially lateral deformation) during cold pressing, causing the filling of the upper pores, which will greatly reduce the number of channels for active ion transmission in the upper layer, resulting in a decrease in fast charging performance.
[0091] Therefore, through the reasonable combination of the particle size of the upper and lower negative electrode active materials, the compacted density of the powder and the porosity of the negative electrode sheet, the liquid phase diffusion path of the active ions in the negative electrode can be shorter, the active ion conduction tends to be more linear, and the number of diffusion paths is larger; at the same time, the porosity of the negative electrode sheet can be adjusted to a suitable range, which can reduce the loss of energy density caused by high porosity. In this way, the battery can have a high fast charging performance and also take into account energy density to a certain extent.
[0092] It can be understood that the "active ions" mentioned in this application refer to ions that are embedded and released back and forth between the positive electrode and the negative electrode during the charging and discharging process of the battery.
[0093] In some embodiments, 0 g / cm 3 <ρ2-ρ1≤0.55g / cm 3 , for example, ρ2-ρ1 can be 0.05 g / cm 3 , 0.07g / cm 3 , 0.09g / cm 3 , 0.15g / cm 3 , 0.2g / cm 3 , 0.25g / cm 3 , 0.3g / cm 3 , 0.35g / cm 3 , 0.4g / cm 3 , 0.45g / cm 3 , 0.5g / cm 3 , 0.55g / cm 3 Or within a range consisting of any of the above values.
[0094] By controlling the powder compaction density difference (i.e., ρ2-ρ1) between the second negative electrode active material and the first negative electrode active material within a suitable range, not only can the aforementioned matching effect between the upper and lower layers be effectively exerted, so that the liquid phase diffusion path of active ions in the negative electrode sheet is shorter and the number is relatively abundant, which is conducive to the faster conduction of active ions in the negative electrode sheet, and then to the improvement of the fast charging performance of the battery. Moreover, the reasonable design of the powder compaction density difference of the negative electrode active material in the upper and lower layers can also make the overall pore distribution of the sheet better, that is, the porosity of the negative electrode sheet can be kept within a suitable range, thereby reducing the rebound of the negative electrode sheet and improving the energy density of the battery to a certain extent.
[0095] It should be noted that, in the negative electrode plates included in the lithium-ion battery of the present application, when the first negative electrode active material and the second negative electrode active material are both fresh materials, and after the two negative electrode active materials have been formed or cycled, there may be slight fluctuations in the powder compaction density difference ρ2-ρ1 of the two negative electrode active materials between these different states; however, regardless of whether the two negative electrode active materials are both fresh materials or have been formed or cycled, the powder compaction density difference ρ2-ρ1 of the two negative electrode active materials can meet the range specified in the present application, and the powder compaction density difference after formation or cycle shall prevail; in other words, the test results of the battery that has been formed or cycled and disassembled shall prevail.
[0096] It should be noted that the negative electrode plate included in the lithium-ion battery of the present application may have a small fluctuation in porosity P between the different states after cold pressing and before being assembled into a battery, and after being assembled into a battery and undergoing formation or circulation; however, whether it is after cold pressing and before being assembled into a battery, or after being assembled into a battery and undergoing formation or circulation, the porosity P can meet the range specified in the present application, and the porosity after being assembled into a battery and undergoing formation or circulation shall prevail; in other words, the result of testing the battery after formation or circulation shall prevail.
[0097] It can be understood that the "fresh material" mentioned in the present application refers to the negative electrode active material before pressure is applied or the negative electrode active material raw material used to prepare the negative electrode plate, for example, it can be the negative electrode active material used to form the negative electrode slurry.
[0098] It is understood that the "5T pressure" mentioned in this application refers to 5 tons of pressure. This application uses 5T pressure to test the powder compaction density of the negative electrode active material because the powder compaction density under 5T pressure tends to bring the deformation degree of the powder close to the limit, which can better reflect the deformation degree of the powder.
[0099] In some embodiments, the relationship between ρ1 and ρ2 is: 0.05 g / cm 3 ≤ρ2-ρ1≤0.55g / cm 3 For example, ρ2-ρ1 can be 0.05 g / cm 3 , 0.1g / cm 3 , 0.12g / cm 3 , 0.14g / cm 3 , 0.16g / cm 3 , 0.18g / cm 3 , 0.2g / cm 3 , 0.23g / cm 3 , 0.26g / cm 3 , 0.29g / cm3 , 0.3g / cm 3 , 0.33g / cm 3 , 0.36g / cm 3 , 0.39g / cm 3 , 0.4g / cm 3 , 0.43g / cm 3 , 0.46g / cm 3 , 0.49g / cm 3 , 0.5g / cm 3 , 0.53g / cm 3 , 0.55g / cm 3 Or within the range of any of the above values. In this way, it is beneficial for the active ions to conduct faster in the negative electrode sheet, and the overall pore distribution of the negative electrode sheet can be better, so that the energy density can be better taken into account while the fast charging performance is improved.
[0100] As an example, in the negative electrode sheet of a battery, the method for obtaining the first negative electrode active material and the second negative electrode active material is as follows: observe / test the pores of the negative electrode sheet by using the ion polishing cross-sectional morphology method. When there is obvious fluctuation in the pores, it indicates that this is the boundary between the first negative electrode active material layer and the second negative electrode active material layer, thereby determining the first negative electrode active material layer and the second negative electrode active material layer. In the first negative electrode active material layer, a sample with a thickness of 2 / 3 is taken on the side relatively far from the second negative electrode active material layer as the upper layer sample; in the second negative electrode active material layer, a sample with a thickness of 2 / 3 is taken on the side relatively far from the first negative electrode active material layer as the lower layer sample. The upper layer sample and the lower layer sample are respectively immersed in a dimethyl carbonate (DMC) solution for washing and then filtered and separated to obtain the first negative electrode active material and the second negative electrode active material; at the same time, the filtered filtrate is evaporated and crystallized to obtain the binder in the first negative electrode active material layer and the binder in the second negative electrode active material layer. The first negative electrode active material and the second negative electrode active material, as well as the binder in the first negative electrode active material layer and the binder in the second negative electrode active material layer can be used for subsequent tests.
[0101] The compacted density (ρ1 or ρ2) of the powder of the negative electrode active material is well known in the art and can be tested by instruments and methods known in the art. For example, it can be measured by an electronic pressure tester (for example, a UTM7305 electronic pressure tester) with reference to GB / T 24533-2009. An exemplary test method is as follows: weigh 1g of sample powder and add a bottom area of 1.327cm 2The mold is pressurized to the required pressure (such as 5T pressure), maintained for 30 seconds, then released, maintained for 10 seconds, and then the powder compaction density of the material under the required pressure is recorded and calculated. Among them, this test is based on the results of the test after the battery has been formed or cycled and disassembled.
[0102] The porosity of the negative electrode sheet is a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, the cold-pressed negative electrode sheet is punched into a small disc sample of a certain area, and the apparent volume V1 of the negative electrode sheet is calculated; referring to GB / T24586-2009, an inert gas (such as helium or nitrogen) is used as a medium, and the gas replacement method is adopted to measure the real volume V2 of the negative electrode sheet using a true density tester. Porosity of negative electrode sheet = (V1-V2) / V1×100%. Multiple (such as 30) negative electrode sheet samples with good appearance and no powder falling on the edges can be taken for testing, and the results are averaged, thereby improving the accuracy of the test results. The test instrument can be a Micromeritics AccuPyc II 1340 true density tester. Among them, this test is based on the result of the test after the battery is formed or cycled and disassembled.
[0103] In some embodiments, the Dv501 satisfies: 4μm≤Dv501≤16μm. For example, Dv501 can be 4μm, 5μm, 7μm, 9μm, 11μm, 13μm, 15μm, 16μm or within the range of any of the above values. In this way, the first negative electrode active material can have a relatively low powder compaction density. Therefore, when the negative electrode plate is subjected to pressure (such as cold pressing treatment when preparing the plate), the first negative electrode active material is not easy to deform laterally, which can reduce the filling of the pores in the upper layer area, making the pores in the upper layer relatively richer, thereby facilitating the infiltration and conduction of active ions that diffuse in the liquid phase, and facilitating the improvement of the fast charging performance of the battery.
[0104] In some embodiments, the Dv502 satisfies: 8μm≤Dv502≤23μm. For example, Dv502 can be 8μm, 10μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm or within the range of any of the above values. In this way, the second negative electrode active material can have a relatively high powder compaction density, so that when the negative electrode plate is under pressure, the second negative electrode active material is easier to deform, which can serve as the main force-bearing party and make the pores in the lower layer relatively less. This is conducive to preventing the overall porosity of the negative electrode plate from being too high, that is, the porosity can still be maintained in a more appropriate range, which can reduce the loss of energy density caused by excessively high porosity, and is conducive to the battery having a higher fast charging performance. Under the condition of better taking into account energy density.
[0105] In some embodiments, the Dv501 satisfies: 4μm≤Dv501≤15.5μm. For example, Dv501 can be 4μm, 6μm, 10μm, 12μm, 14μm, 15μm, 15.5μm or within the range of any of the above values. In this way, it is beneficial to further improve the wetting and conduction of the negative electrode plate to the active ions that are diffused in the liquid phase, thereby further improving the fast charging performance of the battery.
[0106] In some embodiments, the Dv502 satisfies: 8 μm ≤ Dv502 ≤ 21 μm. This is conducive to further reducing the loss of energy density, so that the battery can better balance energy density while having a higher fast charging performance.
[0107] The particle size (Dv50, Dv10, Dv90) and particle size distribution parameter (span) of the negative electrode active material are well known in the art, wherein Dv50, Dv10, and Dv90 respectively represent the particle size corresponding to the cumulative volume distribution percentage of the material reaching 50%, 10%, and 90%, and can be measured using instruments and methods known in the art. For example, it can be measured with a laser particle size analyzer with reference to GB / T 19077-2016. The test instrument can be the Mastersizer 3000 laser particle size analyzer of Malvern Instruments Ltd., UK. Among them, the test is based on the result of the test after the battery is formed or cycled and disassembled.
[0108] In some embodiments, the ρ1 satisfies: 1.4 g / cm 3 ≤ρ1≤2g / cm 3 For example, ρ1 can be 1.4 g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3, 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 , 2g / cm 3 Or within the range formed by any of the above values. In this way, the compacted density of the powder of the first negative electrode active material is relatively low. Therefore, when the negative electrode plate is under pressure, the first negative electrode active material is not easy to deform laterally, which can reduce the filling of the pores in the upper layer area, making the pores in the upper layer relatively richer, thereby facilitating the infiltration and conduction of active ions that diffuse in the liquid phase, and improving the fast charging performance of the battery.
[0109] In some embodiments, the ρ2 satisfies: 1.5 g / cm 3 ≤ρ2≤2.2g / cm 3 For example, ρ1 can be 1.5 g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 , 2g / cm 3 , 2.1g / cm 3 , 2.2g / cm 3 Or within the range formed by any of the above values. In this way, the compacted density of the powder of the second negative electrode active material is relatively high. Therefore, when the negative electrode plate is under pressure, the second negative electrode active material is easier to deform, and it can serve as the main force-bearing party, and make the pores in the lower layer relatively less. This is conducive to preventing the overall porosity of the negative electrode plate from being too high, that is, the porosity can still be maintained in an appropriate range, which can reduce the loss of energy density caused by excessively high porosity, and is conducive to the battery having a higher fast charging performance. Better balance energy density.
[0110] In some embodiments, the ρ1 satisfies: 1.5 g / cm 3 ≤ρ1≤2g / cm 3 For example, ρ1 can be 1.5 g / cm 3 , 1.55g / cm 3 , 1.65g / cm 3 , 1.75g / cm 3 , 1.85g / cm 3 , 1.95g / cm 3 , 2g / cm 3 Or within the range of any of the above values. In this way, it is beneficial to further improve the wetting and conduction of the negative electrode plate to the active ions that are diffused in the liquid phase, thereby further improving the fast charging performance of the battery.
[0111] In some embodiments, the ρ2 satisfies: 1.65 g / cm 3 ≤ρ2≤2.1g / cm 3 For example, ρ2 can be 1.65 g / cm 3 , 1.75g / cm 3 , 1.85g / cm 3 , 1.95g / cm 3 , 2.05g / cm 3 , 2.1g / cm 3 Or within the range of any of the above values. This is conducive to further reducing the loss of energy density, so that the battery can better balance energy density while having higher fast charging performance.
[0112] In some embodiments, the OI value of the first negative electrode active material is 1.5 to 15. For example, the OI value of the first negative electrode active material can be 1.5, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or within a range of any of the above values. In this way, the first negative electrode active material has a relatively low OI value, which, combined with the relatively small particle size of the first negative electrode active material, can be more conducive to the conduction of active ions.
[0113] In some embodiments, the OI value of the second negative electrode active material is 3 to 30. For example, the OI value of the second negative electrode active material can be 3, 4, 5, 6, 7, 8, 9, 12, 15, 18, 21, 24, 27, 30 or within the range of any of the above values. In this way, the second negative electrode active material has a relatively high OI value. After the negative electrode plate is subjected to pressure, in the subsequent stress release and charge and discharge process, its high OI value characteristic can make the second negative electrode active material more prone to particle rebound, and pores can be re-formed between particles, improving the liquid phase diffusion and conduction of active ions in the lower region, thereby improving the fast charging performance.
[0114] In some embodiments, the OI value of the first negative electrode active material is 2 to 10. For example, the OI value of the first negative electrode active material can be 2, 2.5, 3.5, 4.5, 5.5, 6.5, 7.5, 8.5, 9.5, 10 or within a range of any of the above values. In this way, the conduction of active ions can be further improved.
[0115] In some embodiments, the OI value of the second negative electrode active material is 3 to 25. For example, the OI value of the second negative electrode active material can be 3, 10, 11, 13, 14, 16, 17, 19, 20, 22, 23, 25 or within the range of any of the above values. In this way, it is beneficial to enrich the pore structure in the second negative electrode active material and improve the resilience of the material particles, thereby further improving the liquid phase diffusion and conduction of active ions in the lower region.
[0116] It can be understood that the "OI value" mentioned in the present application refers to the orientation degree of the grains of the negative electrode active material, that is, the intensity ratio of the (004) crystal plane to the (110) crystal plane in the X-ray diffraction pattern of the powder material.
[0117] The OI value of the negative electrode active material can be tested using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for testing. The test can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain an X-ray diffraction pattern of a powder sample. According to OI value = I 004 / I 110 The powder OI value of the sample is calculated. 004 is the integrated area of the diffraction peak of the (004) crystal plane in the powder sample, I 110 It is the integrated area of the diffraction peak of the (110) crystal plane in the powder sample. In the X-ray diffraction analysis test of the present application, a copper target can be used as an anode target, CuKα rays can be used as a radiation source, the ray wavelength scans the 2θ angle range of 20°~80°, and the scanning rate is 4° / min. Among them, the test is based on the results of the test after the battery is formed or cycled and disassembled.
[0118] In some embodiments, the tap density of the first negative electrode active material and the second negative electrode active material is each independently 0.9 g / cm 3 ~1.2g / cm 3 For example, the tap density can be 0.9 g / cm 3 , 1g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 Or within the range of any of the above values. Optionally, the tap density of the first negative electrode active material and the second negative electrode active material are each independently 1 g / cm 3 ~1.2g / cm 3 .
[0119] In this way, the internal structure of the first negative electrode active material and the second negative electrode active material is relatively compact, the surface roughness is relatively small, the particle structure is relatively stable, the dispersion in the negative electrode active material layer is relatively good, and the grading between particles is relatively good, thereby reducing the ionic impedance of the active ions in the liquid phase diffusion.
[0120] It can be understood that the "ionic impedance" mentioned in this application refers to the resistance of active ions in the liquid phase diffusion process; the greater the resistance, the smaller the conduction rate of the active ions and the worse their conductivity in the electrolyte.
[0121] The tap density of the negative electrode active material is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, it can be measured using a powder tap density tester in accordance with GB / T 5162-2006. The test instrument can be Dandong Better BT-301, and the test parameters are as follows: vibration frequency 250±15 times / minute, amplitude 3±0.2mm, vibration number 5000 times, and measuring cylinder 25mL. Among them, the test is based on the results of the test on the formed or cycled battery after disassembly.
[0122] In some embodiments, the particle size distribution of the first negative electrode active material satisfies: span1≤1.6, span1=(Dv901-Dv101) / Dv501, wherein Dv901 and Dv101 both correspond to the particle size parameters of the first negative electrode active material. For example, span1 may be 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or within the range of any of the above values; optionally, span1≤1.4; further optionally, 0.5≤span1≤1.4. In this way, the particle size distribution of the first negative electrode active material is relatively concentrated, and the more concentrated the particle size distribution, the better the consistency of the active material, thereby reducing the deterioration of the electrode porosity caused by more large or small particles, making the overall pore distribution of the electrode better, and facilitating the improvement of energy density and fast charging performance.
[0123] In some embodiments, the particle size distribution of the second negative electrode active material satisfies: span2≤1.6, span2=(Dv902-Dv102) / Dv502, wherein Dv902 and Dv102 both correspond to the particle size parameters of the second negative electrode active material. For example, span2 may be 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or within the range of any of the above values; optionally, span2≤1.4; further optionally, 0.5≤span2≤1.4. In this way, the particle size distribution of the second negative electrode active material is more concentrated, and the consistency of the active material is better, thereby reducing the deterioration of the electrode porosity caused by more large or small particles, making the overall pore distribution of the electrode better, and facilitating the improvement of energy density and fast charging performance.
[0124] In some embodiments, the first negative electrode active material and the second negative electrode active material each independently further include a silicon-based material.
[0125] In some embodiments, the mass percentage of the silicon-based material in the first negative electrode active material layer and the second negative electrode active material layer is independently less than or equal to 9%. For example, the mass percentage may be 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or any range thereof.
[0126] In some embodiments, the first negative electrode active material includes a silicon-based material, and the double-sided thickness of the first negative electrode active material layer is 80 mm to 170 mm. For example, the thickness can be 80 mm, 100 mm, 120 mm, 140 mm, 160 mm, 170 mm, or within a range of any of the above values. This is beneficial to improving the fast charging performance of the battery.
[0127] It should be noted that the double-sided thickness of the first negative electrode active material layer refers to the total thickness of two first negative electrode active material layers located on opposite sides of the negative electrode current collector when the first negative electrode active material layers are arranged on opposite sides of the negative electrode current collector.
[0128] In some embodiments, the silicon-based material may include one or more of elemental silicon, silicon-oxygen compounds, silicon-carbon compounds, silicon-nitrogen compounds, and silicon alloys, and elemental silicon may be selected.
[0129] As an example, natural graphite and artificial graphite can be distinguished by the appearance of the particles. For example, the first negative electrode active material and the second negative electrode active material obtained above are subjected to X-ray diffraction analysis and testing. In the XRD spectrum, if the characteristic peak around 2θ=26.5° is very sharp and has a high intensity, it is natural graphite; if the characteristic peak around 2θ=26.5° is relatively wide and has a weak intensity, it is artificial graphite.
[0130] In some embodiments, the degree of graphitization of the natural graphite is 92% to 99%. For example, the degree of graphitization of the natural graphite may be 92%, 93%, 94%, 95%, 96%, 97%, 98% or any range thereof. In this way, it is easier to adjust the pores of the upper and lower layers of the pole piece, as well as the porosity of the pole piece.
[0131] In some embodiments, the degree of graphitization of the artificial graphite is 88% to 96%. For example, the degree of graphitization of the artificial graphite can be 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96% or any range thereof. In this way, it is easier to adjust the pores of the upper and lower layers of the pole piece, as well as the porosity of the pole piece.
[0132] The degree of graphitization of the negative electrode active material is well known in the art and can be tested using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for testing. The test can refer to JISK 0131-1996 and JB / T 4220-2011 to obtain the average interlayer spacing d002 of the (002) crystal plane in the material crystal structure, and then the degree of graphitization is calculated according to the formula g = (0.344-d002) / (0.344-0.3354)×100%. In the above formula, d002 is the average interlayer spacing of the (002) crystal plane in the material crystal structure expressed in nanometers (nm). Among them, the test is based on the results of the test after the battery is formed or cycled and disassembled.
[0133] In some embodiments, the sphericity of the natural graphite is 0.55 to 0.9, and can be 0.82 to 0.9. In this way, the expansion of the negative electrode active material during the cycle is small, and the fast charging performance is more stable.
[0134] Sphericity is a well-known meaning in the art and can be tested by methods known in the art. For example, natural graphite particles are photographed using a scanning electron microscope, and then the shape of the particles is analyzed using image analysis software to calculate the sphericity.
[0135] In some embodiments, the first negative electrode active material layer and the second negative electrode active material layer each independently further include a binder.
[0136] In some embodiments, in the first negative electrode active material layer, the binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0137] In some embodiments, the mass proportions of the binder in the first negative electrode active material layer and the second negative electrode active material layer are ω1 and ω2, respectively, and ω1<ω2. In this way, it is conducive to forming a stacked structure with relatively richer pores in the upper layer and relatively fewer pores in the lower layer, thereby improving the liquid phase diffusion and conduction of active ions.
[0138] In some embodiments, 0.5%≤ω2≤5%. For example, ω2 can be 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any range thereof. This helps improve the pore distribution of the lower layer and the total porosity of the electrode, thereby helping to reduce the ionic impedance of the liquid phase diffusion of active ions.
[0139] In some embodiments, in the second negative electrode active material layer, the binder includes a first binder, and the first binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), styrene acrylic resin and carboxymethyl chitosan (CMCS).
[0140] In some embodiments, in the second negative electrode active material layer, the binder further comprises a second binder, the glass transition temperature of the second binder is Tg2, and the glass transition temperature of the first binder is Tg1, Tg2 <Tg1。
[0141] When the lower layer contains the first binder and the second binder, since the second binder has a relatively lower glass transition temperature and relatively higher elasticity, a more obvious rebound can occur during the cold pressing and static process of the electrode and the battery charging and discharging process, thereby significantly improving the pore distribution of the lower layer and the porosity of the electrode, thereby significantly improving the ionic impedance of the liquid phase diffusion of active ions, which is beneficial to the improvement of fast charging performance.
[0142] The glass transition temperature of the binder is a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, differential scanning calorimetry (DSC) can be used for testing. The specific heat capacity before and after the glass transition temperature will change significantly, and the glass transition temperature can be determined based on the DSC curve. The glass transition temperature is usually a step in the direction of heat absorption, and the glass transition is a region. This method usually uses the intersection of the line with equal distance from the two extrapolated baselines and the curve as the glass transition temperature.
[0143] In some embodiments, in the second negative electrode active material layer, the mass ratio of the second binder to the first binder is σ, 0≤σ≤10. Optionally, 0.25≤σ≤4. In this way, it is beneficial to better balance energy density and fast charging performance.
[0144] In some embodiments, the second binder may include one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, styrene acrylic resin and acrylate compounds, and the second binder is different from the first binder.
[0145] In some embodiments, the second binder includes styrene acrylic resin. In styrene acrylic resin, the presence of ester groups can increase the affinity of the binder with the electrolyte; at the same time, there are a large number of electronegative elements in the molecular chain of styrene acrylic resin, which have lone pairs of electrons and will continuously undergo complexation / decomplexation reactions with active ions under the action of an electric field, which is beneficial to reducing the ionic impedance of liquid phase diffusion of active ions and improving the conductivity of active ions.
[0146] In some embodiments, the acrylate compound includes but is not limited to one or more of methyl acrylate, ethyl acrylate, 2-methyl methacrylate and 2-ethyl methacrylate. The acrylate compound binder can swell after being infiltrated by the electrolyte, which can improve the pore structure of the lower layer and has good dynamic performance. At the same time, there are also more electronegative elements in the molecular chain of the acrylate compound binder, which has lone pairs of electrons and will continuously react with active ions to form complexes / decomplexes under the action of the electric field, which is beneficial to reduce the ionic impedance of the active ions for liquid phase diffusion and improve the conductivity of the active ions.
[0147] It should be noted that the "acrylate compounds" mentioned in the present application refer to the general term for acrylate and its derivatives.
[0148] In some embodiments, the binder contains lithium ions. During the battery charging and discharging process, when the binder contains lithium ions, additional lithium ions can be provided inside the pole piece, which is beneficial to improve the ionic impedance of lithium ion liquid phase diffusion and enhance the conductivity of lithium ions in the electrolyte.
[0149] As a non-limiting example, the manner in which lithium ions are incorporated into a binder such as styrene-butadiene rubber is as follows:
[0150] Disperse butadiene monomer and styrene monomer in an aqueous emulsion with rosin soap or fatty acid soap as an emulsifier, use mercaptan as a molecular weight regulator, and add an oxidation-reduction initiation system consisting of an organic peroxide, a ferrous salt and an activator for free radical polymerization. Emulsion polymerization is carried out continuously in multiple series-connected kettles, and the conversion rate is controlled at about 65%. Afterwards, the unreacted butadiene and styrene are successively removed by a horizontal flash tank and a distillation tower, and then refined and reused. The copolymer emulsion from which the unreacted monomers have been removed is coagulated with sodium chloride, calcium chloride and acid, and the resulting rubber is separated from the whey by a vibrating screen, and a weak alkaline solution such as (LiOH) is added to neutralize the pH, and then dehydrated and dried to obtain the finished product.
[0151] In some embodiments, an electrolyte is also included, and the ionic conductivity of the electrolyte at 25°C is 10mS / cm~20mS / cm. For example, the ionic conductivity of the electrolyte at 25°C can be 10mS / cm, 11mS / cm, 12mS / cm, 14mS / cm, 16mS / cm, 18mS / cm, 20mS / cm or within the range of any of the above values. In this way, the electrolyte can better cooperate with the laminated structure of the negative electrode plate, thereby further improving the conductivity of the active ions in the electrolyte, so that the fast charging performance of the battery can be further improved.
[0152] In some embodiments, the ionic conductivity of the electrolyte at 25° C. is 13 mS / cm to 20 mS / cm. For example, the ionic conductivity of the electrolyte at 25° C. may be 13 mS / cm, 15 mS / cm, 17 mS / cm, 18 mS / cm, 19 mS / cm, 20 mS / cm, or within a range of any of the above values. This is beneficial to further improve the fast charging performance of the battery.
[0153] The ionic conductivity of the electrolyte is well known in the art and can be tested using instruments and methods known in the art. For example, the following method can be used for testing: First, pre-treat the electrolyte, take the electrolyte to be tested and keep it at a constant temperature to the temperature to be tested and the standard solution to keep it at a constant temperature of 25°C (deviation ±0.1°C); then, test the two standard solutions at 25°C to calibrate the instrument. After the calibration is completed, clean the electrode and vertically place the test sample electrode into the electrolyte to be tested. Use the conductivity meter to start the test, and record the test results after the data is stable for more than 10 seconds to obtain the ionic conductivity of the electrolyte. Among them, this test is based on the result of the test after the battery is formed or cycled and disassembled.
[0154] In a second aspect, the present application provides a negative electrode sheet, which includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector;
[0155] The negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, wherein the second negative electrode active material layer is disposed between the negative electrode current collector and the first negative electrode active material layer;
[0156] The first negative electrode active material layer contains a first negative electrode active material, the second negative electrode active material layer contains a second negative electrode active material, the first negative electrode active material includes artificial graphite, the second negative electrode active material includes one or both of natural graphite and artificial graphite, and at least one of the two is natural graphite, the volume average particle size of the first negative electrode active material is Dv501, the volume average particle size of the second negative electrode active material is Dv502, and Dv501 <Dv502;
[0157] The powder compaction density of the first negative electrode active material under a pressure of 5T is ρ1, and the powder compaction density of the second negative electrode active material under a pressure of 5T is ρ2, 0g / cm 3 <ρ2-ρ1≤0.55g / cm 3 ;
[0158] The porosity of the negative electrode plate is P, and 18%≤P≤25%.
[0159] In some embodiments, the negative electrode plate is the negative electrode plate in the lithium-ion battery provided in the first aspect of the present application.
[0160] It should be noted that the beneficial effects related to the negative electrode plate can be found in the previous description and will not be repeated here.
[0161] In addition, the lithium ion battery and the electric device of the present application will be described below with reference to the drawings as appropriate.
[0162] Generally, lithium-ion batteries include a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0163] Negative electrode
[0164] As a non-limiting example, the negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0165] In some of the embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be obtained by forming a metal material on a polymer material substrate. In the negative electrode current collector, non-limiting examples of the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the negative electrode current collector, non-limiting examples of the polymer material substrate may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0166] In some embodiments, the negative electrode active material layer may further include a conductive agent, which may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0167] In some of the embodiments, the negative electrode active material layer may further include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0168] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the first negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form a first negative electrode slurry; the second negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form a second negative electrode slurry; the two negative electrode slurries are coated on at least one side of the negative electrode current collector by a double-layer coating machine, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. The surface of the negative electrode current collector coated with the negative electrode slurry can be on a single surface of the negative electrode current collector or on both surfaces of the negative electrode current collector. The solid content of each of the first negative electrode slurry and the second negative electrode slurry can be 40wt%~60wt%. The viscosity of each of the first negative electrode slurry and the second negative electrode slurry at room temperature can be adjusted to 2000mPa·s~10000mPa·s. When the negative electrode slurry is applied, the coating single surface density of the first negative electrode active material layer and the second negative electrode active material layer can be 80 mg / 1540.25 mm2 on a dry weight basis (excluding the solvent). 2 ~200mg / 1540.25mm 2 The compaction density of the negative electrode sheet can be 1.0g / cm 3 ~1.8g / cm 3 .
[0169] Positive electrode
[0170] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material.
[0171] As a non-limiting example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0172] In some of the embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be obtained by forming a metal material on a polymer material substrate. In the positive electrode current collector, non-limiting examples of the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the positive electrode current collector, non-limiting examples of the polymer material substrate may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0173] In some of the embodiments, the positive electrode may adopt a positive electrode active material for a battery known in the art. As a non-limiting example, the positive electrode active material may include one or more of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide (such as LiCoO2), lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Non-limiting examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. Non-limiting examples of lithium cobalt oxides may include LiCoO2; non-limiting examples of lithium nickel oxides may include LiNiO2; non-limiting examples of lithium manganese oxides may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333)、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxide may include LiNi 0.8 Co 0.15 Al 0.05 O2.
[0174] It is understandable that the battery will be accompanied by lithium (Li) deintercalation and consumption during the charging and discharging process, and the content of Li in the positive electrode plate is different when the battery is discharged to different states. In the list of positive electrode materials in this application, unless otherwise specified, the content of Li is the initial state of the material. The positive electrode material is applied to the positive electrode plate in the battery system, and after the charge and discharge cycle, the content of Li in the positive electrode material contained in the plate usually changes. Among them, the content of Li can be measured by molar content, but is not limited to this. Regarding "the content of Li is the initial state of the material", the initial state of the material refers to the state before the material is added to the positive electrode slurry. It is understandable that the new material obtained by appropriate modification on the basis of the listed positive electrode materials is also within the scope of the positive electrode material. The aforementioned appropriate modification refers to the acceptable modification method for the positive electrode material, and non-limiting examples include coating modification.
[0175] In the list of positive electrode materials in this application, the content of oxygen (O) is only a theoretical state value. The release of oxygen from the lattice will cause the molar content of oxygen to change, and the actual content of O will fluctuate. Among them, the content of O can be measured by molar content, but is not limited to this.
[0176] In some embodiments, the positive electrode active material layer may further include a binder. As non-limiting examples, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0177] In some embodiments, the positive electrode active material layer may further include a conductive agent. As non-limiting examples, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0178] In some of the embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on at least one side of the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained. The type of solvent can be selected from but not limited to any one of the aforementioned embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode collector coated with the positive electrode slurry can be on a single surface of the positive electrode collector or on both surfaces of the positive electrode collector. The solid content of the positive electrode slurry can be 40wt%~80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000~25000mPa·s. When the positive electrode slurry is coated, the single-sided surface density of the coating on a dry weight basis (excluding the solvent) can be 0.22g / 1540.25mm 2 ~0.35g / 1540.25mm 2 The compaction density of the positive electrode can be 3.0~3.6 g / cm 3 , can be selected as 3.3~3.5 g / cm 3 .
[0179] Electrolyte
[0180] The electrolyte has the function of conducting ions between the positive electrode and the negative electrode.
[0181] In some of these embodiments, the electrolyte includes an electrolyte salt and a solvent.
[0182] In some of the embodiments, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0183] In some embodiments, the solvent includes a carboxylic acid ester solvent.
[0184] In some embodiments, the carboxylate solvent includes one or more of methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, and 1,4-butyrolactone. The carboxylate solvent is conducive to making the electrolyte have a higher ionic conductivity.
[0185] In some of the embodiments, the solvent may also include one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate, fluoroethylene carbonate (FEC), cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0186] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0187] In some embodiments, the additive in the electrolyte may include, but is not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), and the like.
[0188] Isolation film
[0189] In some embodiments, the lithium-ion battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0190] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0191] In some embodiments, the isolation film has a thickness of 6 μm to 40 μm, and may be 12 μm to 20 μm.
[0192] In some of the embodiments, the positive electrode sheet, the negative electrode sheet and the separator can be formed into an electrode assembly by a winding process or a lamination process.
[0193] In some embodiments, the lithium-ion battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.
[0194] In some embodiments, the outer packaging of the lithium-ion battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium-ion battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0195] A lithium-ion battery includes at least one battery cell. A lithium-ion battery may include one or more battery cells.
[0196] In this application, unless otherwise specified, "battery cell" refers to a basic unit that can realize the mutual conversion of chemical energy and electrical energy, and further, generally speaking, at least includes a positive electrode sheet, a negative electrode sheet and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting active ions between the positive electrode sheet and the negative electrode sheet.
[0197] The present application has no particular limitation on the shape of the battery cell, which may be cylindrical, square or any other shape. Figure 1 The battery cell 5 is a square structure as an example.
[0198] In some of these embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to actual needs.
[0199] The lithium-ion battery may be a battery device 4 or a battery pack 1 .
[0200] The battery device includes at least one battery cell. The number of battery cells contained in the battery device can be one or more, and those skilled in the art can select a suitable number according to the application and capacity of the battery device.
[0201] Figure 3 4 is an example of a battery device. Figure 3 In the battery device 4, the plurality of battery cells 5 may be arranged in sequence along the length direction of the battery device 4. Of course, they may also be arranged in any other manner. Further, the plurality of battery cells 5 may be fixed by fasteners.
[0202] Optionally, the battery device 4 may further include a housing having a receiving space, and the plurality of battery cells 5 are received in the receiving space.
[0203] In some of the embodiments, the battery devices described above may also be assembled into a battery pack. The number of battery devices contained in the battery pack may be one or more. Those skilled in the art may select a suitable number according to the application and capacity of the battery pack.
[0204] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5 The battery pack 1 may include a battery box and a plurality of battery devices 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery devices 4. The plurality of battery devices 4 can be arranged in the battery box in any manner.
[0205] In addition, the present application also provides an electrical device, which includes the lithium-ion battery provided in the present application. The lithium-ion battery can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited to these. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited to these.
[0206] As an electrical device, a lithium-ion battery can be selected according to its usage requirements.
[0207] Figure 6 The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of lithium-ion batteries, a battery pack or a battery device can be used.
[0208] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a lithium-ion battery may be used as a power source.
[0209] Below, some embodiments of the present application are described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If the technology or conditions are not specified in the embodiments, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.
[0210] Example 1
[0211] (1) Preparation of positive electrode
[0212] The positive electrode active material lithium iron phosphate (LFP), the conductive agent carbon black (Super P), and the binder polyvinylidene fluoride (PVDF) were mixed uniformly in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 97.5:0.4:2.1 to obtain a positive electrode slurry; the positive electrode slurry was coated on the double-sided surface of the positive electrode current collector aluminum foil, and the positive electrode sheet was obtained through drying, cold pressing, slitting, cutting and other processes, wherein the coating amount per unit area on one side was 0.27g / 1540.25mm 2 .
[0213] (2) Preparation of negative electrode sheet
[0214] The first negative electrode active material artificial graphite, the conductive agent carbon black (Super P), the binder styrene butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC-Na) were uniformly mixed in a solvent deionized water at a mass ratio of 97.8:0.7:0.8:0.7 to obtain a first negative electrode slurry (corresponding to the first negative electrode active material layer).
[0215] The second negative electrode active material natural graphite, conductive agent carbon black (Super P), binder styrene acrylic resin and sodium carboxymethyl cellulose (CMC) were uniformly mixed in a solvent deionized water at a mass ratio of 97.4:0.4:1.5:0.7 to obtain a second negative electrode slurry (corresponding to the second negative electrode active material layer).
[0216] The two negative electrode slurries were coated on the opposite sides of the negative electrode current collector copper foil using a double-layer coating machine, and after drying, cold pressing, slitting, and cutting, a negative electrode sheet including a first negative electrode active material layer and a second negative electrode active material layer was obtained, wherein the coating amount per unit area of the first negative electrode active material layer and the second negative electrode active material layer on one side was 0.13 g / 1540.25 mm 2 , the weight ratio of the first negative electrode active material layer to the second negative electrode active material layer is 5:5.
[0217] (3) Preparation of isolation membrane
[0218] A 7 μm thick polypropylene diaphragm was used.
[0219] (4) Preparation of electrolyte
[0220] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed at a mass ratio of 30:70 to obtain an organic solvent, and fully dried LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0221] (5) Preparation of lithium-ion batteries
[0222] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a lithium-ion battery is obtained.
[0223] Embodiments 2 to 9
[0224] The preparation method is similar to that of Example 1, with the main difference being that at least one of the parameters ρ1, ρ2, ρ2-ρ1, Dv501, Dv502, etc. is different. For specific differences, please see Table 1.
[0225] Embodiment 10-12
[0226] The preparation method is similar to that of Example 1, with the main difference being that first negative electrode active materials with different OI values are used. For specific differences, please refer to Table 2.
[0227] Embodiments 13 to 15
[0228] The preparation method is similar to that of Example 1, with the main difference being that a second negative electrode active material with a different OI value is used. For specific differences, please refer to Table 2.
[0229] Example 16
[0230] The preparation method is similar to that of Example 1, with the main difference being that in the second negative electrode slurry, part of the binder styrene butadiene rubber with higher elasticity is used to replace the styrene acrylic resin, and the mass ratio of the styrene acrylic resin to the styrene butadiene rubber in the binder is 1:1. Please see Table 3 for the specific differences.
[0231] Embodiments 17 to 19
[0232] The preparation method is similar to that of Example 1, with the main difference being that the mass proportion of the binder in the second negative electrode slurry is different. Please refer to Table 3 for the specific differences.
[0233] Embodiment 20-22
[0234] The preparation method is similar to that of Example 1, with the main difference being that the concentration of the electrolyte salt LiPF6 in the electrolyte is adjusted to make the ion conductivity different. For specific differences, please see Table 4.
[0235] Comparative Example 1
[0236] The preparation method is similar to that of Example 1, with the main difference being that at least one of ρ1, ρ2, ρ2-ρ1, Dv501, Dv502, etc. is different, so that ρ2<ρ1. For specific differences, please see Table 1.
[0237] Comparative Example 2
[0238] The preparation method is similar to that of Example 1, with the main difference being that Dv501 and Dv502 are adjusted so that Dv501>Dv502. For specific differences, please see Table 1.
[0239] Comparative Examples 3~4
[0240] The preparation method is similar to that of Example 1, with the main difference being that the porosity of the negative electrode sheet is adjusted to 17% and 26%. For specific differences, please see Table 1.
[0241] Comparative Example 5
[0242] The preparation method is similar to that of Example 1, with the main difference being that in step (2), the second negative electrode active material uses artificial graphite with the same material parameters (such as ρ2, Dv502, etc.) as natural graphite instead of natural graphite. For specific differences, please refer to Table 1.
[0243] Comparative Example 6
[0244] The preparation method is similar to that of Example 1, with the main difference being that at least one of the parameters ρ1, ρ2, ρ2-ρ1, Dv501, Dv502, etc. is different. For specific differences, please see Table 1.
[0245] In addition, the lithium ion batteries obtained in the above Examples 1 to 22 and Comparative Examples 1 to 6 were subjected to performance tests, and the test results are shown in Tables 1 to 4 below.
[0246] Test Section
[0247] (1) Fast charging performance
[0248] After the prepared lithium-ion battery is fully charged at an equivalent xC (actually a step rate charge) and fully discharged at 1C for 10 cycles, the battery is fully charged at an equivalent xC again, the negative electrode is disassembled and the lithium deposition on the surface is observed. If no lithium is deposited on the negative electrode surface, the equivalent charge rate xC is increased by 0.1C as a gradient until lithium is deposited on the negative electrode surface. The test is stopped and the charge rate xC at this time is recorded. 0.1)C is denoted as the critical charging rate of the battery. The average value of 10%~80%SOC is taken as the equivalent charging rate, which reflects the relative size of the fast charging performance.
[0249] (2) Volume energy density
[0250] At 25°C, the lithium ion batteries prepared in the embodiments and comparative examples were fully charged at a rate of 0.33C and fully discharged at a rate of 0.33C. After three times of charge and discharge, the actual discharge energy C0 was recorded. Under the same temperature condition, the lithium ion battery was weighed using an electronic balance, and the length, width and height of the lithium ion battery were measured using a micrometer to obtain the volume V of the battery. The ratio of the actual discharge energy C0 of the lithium ion battery at 0.33C to the volume V of the lithium ion battery is the actual volume energy density of the lithium ion battery.
[0251] (3) Electrode rebound rate
[0252] The designed thickness of the negative electrode plate after cold pressing is recorded as h1, the thickness of the plate obtained after the battery is fully charged (100% SOC state of charge) is recorded as h2, and (h2-h1) / h1 is recorded as the rebound rate of the plate.
[0253] Table 1
[0254]
[0255] Table 2
[0256]
[0257] Table 3
[0258]
[0259] Table 4
[0260]
[0261] In Table 1, it can be seen from the comparison between Examples 1 to 9 and Comparative Examples 1 to 4 and 6 that Examples 1 to 9 can simultaneously satisfy the equivalent charge rate of 1.8C or more and the energy density of more than 557Wh / L; while when the energy density of Comparative Examples 1 to 4 and 6 is more than 557Wh / L, the equivalent charge rate is less than 1.8C, indicating that the lithium-ion battery of the present application can take into account the energy density to a certain extent while having relatively high fast charging performance. It can be seen from the comparison between Example 1 and Comparative Example 5 that when the second positive electrode active material uses pure artificial graphite, the fast charging performance and energy density will decrease to a certain extent.
[0262] In Table 2, when Example 1 is compared with Examples 10 to 15, it can be seen that adjusting the OI value of the first negative electrode active material or the second negative electrode active material can improve the fast charging performance or energy density of the battery. In Table 3, when Example 1 is compared with Examples 17 to 19, it can be seen that adjusting the mass proportion of the binder in the second negative electrode active material layer can improve the fast charging performance or energy density of the battery; when Example 1 is compared with Example 16, it can be seen that in the second negative electrode active material layer, replacing the styrene butadiene emulsion with styrene butadiene rubber having relatively higher elasticity can improve the rebound rate of the pole piece, thereby improving the fast charging performance of the battery. In Table 4, when Example 1 is compared with Examples 20 to 22, it can be seen that the fast charging performance of the battery can be improved by adjusting the ionic conductivity of the electrolyte.
[0263] The above description of various embodiments tends to emphasize the differences between the various embodiments. The same or similar aspects can be referenced to each other, and for the sake of brevity, they will not be repeated herein.
[0264] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A lithium ion battery, characterized in that: A negative electrode sheet is included, wherein the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector; The negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, wherein the second negative electrode active material layer is disposed between the negative electrode current collector and the first negative electrode active material layer; The first negative electrode active material layer contains a first negative electrode active material, the second negative electrode active material layer contains a second negative electrode active material, the first negative electrode active material includes artificial graphite, the second negative electrode active material includes one or both of natural graphite and artificial graphite, and at least one of the two is natural graphite, the volume average particle size of the first negative electrode active material is Dv501, the volume average particle size of the second negative electrode active material is Dv502, and Dv501 <Dv502; The powder compaction density of the first negative electrode active material under a pressure of 5T is ρ1, and the powder compaction density of the second negative electrode active material under a pressure of 5T is ρ2, 0g / cm 3 <ρ2-ρ1≤0.55g / cm 3 ; The porosity of the negative electrode plate is P, and 18%≤P≤25%.
2. The lithium-ion battery according to claim 1, characterized in that The relationship between ρ1 and ρ2 is: 0.05 g / cm 3 ≤ρ2-ρ1≤0.55g / cm 3 .
3. The lithium ion battery according to claim 1 or 2, characterized in that: At least one of the following conditions is met: (1) The Dv501 satisfies: 4μm≤Dv501≤16μm; (2) The Dv502 satisfies: 8μm≤Dv502≤23μm.
4. The lithium ion battery according to claim 1 or 2, characterized in that: At least one of the following conditions is met: (1) The ρ1 satisfies: 1.4 g / cm 3 ≤ρ1≤2g / cm 3 ; (2) The ρ2 satisfies: 1.5 g / cm 3 ≤ρ2≤2.2g / cm 3 .
5. The lithium ion battery according to claim 1 or 2, characterized in that: At least one of the following conditions is met: (1) The OI value of the first negative electrode active material is 1.5 to 15; (2) The OI value of the second negative electrode active material is 3 to 30.
6. The lithium ion battery according to claim 1 or 2, characterized in that: At least one of the following conditions is met: (1) The tap density of the first negative electrode active material and the second negative electrode active material is independently 0.9 g / cm 3 ~1.2g / cm 3 ; (2) The particle size distribution of the first negative electrode active material satisfies: span1≤1.6, span1=(Dv901-Dv101) / Dv501; (3) The particle size distribution of the second negative electrode active material satisfies: span2≤1.6, span2=(Dv902-Dv102) / Dv502.
7. The lithium ion battery according to claim 1 or 2, characterized in that: The first negative electrode active material and the second negative electrode active material each independently further include a silicon-based material.
8. The lithium-ion battery according to claim 7, characterized in that: The mass percentage of the silicon-based material in the first negative electrode active material layer and the second negative electrode active material layer is independently less than or equal to 9%.
9. The lithium-ion battery according to claim 7, characterized in that: The first negative electrode active material includes a silicon-based material, and the double-sided thickness of the first negative electrode active material layer is 80 mm to 170 mm.
10. The lithium ion battery according to claim 1 or 2, characterized in that: At least one of the following conditions is met: (1) The sphericity of the natural graphite is 0.55-0.9; (2) The degree of graphitization of the natural graphite is 92% to 99%; (3) The degree of graphitization of the artificial graphite is 88% to 96%.
11. The lithium ion battery according to claim 1 or 2, characterized in that: The first negative electrode active material layer and the second negative electrode active material layer further independently contain a binder, and the mass proportions of the binder in the first negative electrode active material layer and the second negative electrode active material layer are ω1 and ω2 respectively, and ω1<ω2.
12. The lithium ion battery according to claim 11, characterized in that: 0.5%≤ω2≤5%.
13. The lithium ion battery according to claim 11, characterized in that: In the second negative electrode active material layer, the binder includes a first binder, and the first binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, styrene acrylic resin and carboxymethyl chitosan.
14. The lithium ion battery according to claim 13, characterized in that: In the second negative electrode active material layer, the binder further includes a second binder, the glass transition temperature of the first binder is Tg1, the glass transition temperature of the second binder is Tg2, and Tg2 <Tg1。 15. The lithium ion battery according to claim 14, characterized in that: The second binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, styrene-acrylic resin and acrylate compounds, and the second binder is different from the first binder.
16. The lithium ion battery according to claim 14, characterized in that: In the second negative electrode active material layer, a mass ratio of the second binder to the first binder is σ, and 0≤σ≤10.
17. The lithium ion battery according to claim 11, characterized in that: The binder contains lithium ions.
18. The lithium ion battery according to claim 1 or 2, characterized in that: The invention also includes an electrolyte, wherein the ion conductivity of the electrolyte at 25° C. is 10 mS / cm to 20 mS / cm.
19. A negative electrode plate, characterized in that: The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector; The negative electrode active material layer includes a first negative electrode active material layer and a second negative electrode active material layer, wherein the second negative electrode active material layer is disposed between the negative electrode current collector and the first negative electrode active material layer; The first negative electrode active material layer contains a first negative electrode active material, the second negative electrode active material layer contains a second negative electrode active material, the first negative electrode active material includes artificial graphite, the second negative electrode active material includes one or both of natural graphite and artificial graphite, and at least one of the two is natural graphite, the volume average particle size of the first negative electrode active material is Dv501, the volume average particle size of the second negative electrode active material is Dv502, and Dv501 <Dv502; The powder compaction density of the first negative electrode active material under a pressure of 5T is ρ1, and the powder compaction density of the second negative electrode active material under a pressure of 5T is ρ2, 0g / cm 3 <ρ2-ρ1≤0.55g / cm 3 ; The porosity of the negative electrode plate is P, and 18%≤P≤25%.
20. The negative electrode sheet according to claim 19, characterized in that: The negative electrode plate in the lithium-ion battery according to any one of claims 2 to 18.
21. An electrical device, characterized in that: A lithium ion battery comprising any one of claims 1 to 18.
Citation Information
Patent Citations
Secondary battery, production method therefor, and device comprising same
CN113875048A
Secondary battery and electric device
CN115832201A
Negative plate and battery comprising same
CN115954436A
Secondary battery and electronic device
CN116487526A
Secondary battery and electric device
CN116964770A
Cited By
Battery cell, battery device, and electric device
CN120341342A
Negative plate, battery, battery pack and electric device
CN121355187A
Battery monomer, battery device, energy storage device and power utilization device
CN122291410A
Rechargeable battery and electric apparatus
WO2026118580A1
Secondary battery, manufacturing method therefor, and electrical device
WO2026184250A1