Composite, battery, and electronic device

By using a composite of specific lithium composite metal oxides in all-solid lithium-ion batteries, the lithium ion conductivity of lithium-ion batteries is optimized, and the problem of insufficient adhesion between solid electrolytes and active substances is solved, and the lithium-ion battery is realized. High lithium ion conductivity and discharge capacity maintenance rate.

CN118970145APending Publication Date: 2024-11-15SEIKO EPSON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410590081.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In all-solid lithium-ion batteries, the adhesion between the solid electrolyte and the active substance is insufficient, resulting in a decrease in lithium ion conductivity and poor discharge capacity maintenance, especially when repeated charge and discharge, the discharge capacity is difficult to maintain.

Method used

Using a composite containing a specific lithium composite metal oxide, the lithium ion conductivity is optimized through the bonding of the composition of the first electrolyte part and the second electrolyte part, and the specific composition is (Li7-3x+yGax) (La3-yCay )Zr2O12 and Li7-zLa3 (Zr2-zMz)O12, where 0.10≤x≤1.00, 0.00

Benefits of technology

The adhesion between the solid electrolyte and the active substance is significantly improved, grain boundary resistance is suppressed, high lithium ion conductivity is maintained, and the stability of the discharge capacity is ensured. The discharge capacity can be properly maintained even under repeated charging and discharge conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004836989710000011
    Figure HDA0004836989710000011
  • Figure HDA0004836989710000021
    Figure HDA0004836989710000021
  • Figure HDA0004836989710000022
    Figure HDA0004836989710000022
Patent Text Reader

Abstract

The present invention relates to a composite, a battery, and an electronic device. The composite comprises: an active material; a crystalline first electrolyte part containing a lithium composite metal oxide represented by formula (1); and a second electrolyte part that contains a lithium composite metal oxide represented by formula (2) and covers at least a part of the surface of the active material, at least a part of the first electrolyte part is bonded to the active material via the second electrolyte part, (Li7-3x + yGax) (La3-yCay) Zr2O12... (1), in formula (1), the relationships 0.10 < = x < = 1.00 and 0.00 < y < = 0.30 are satisfied, and in formula (2), in formula (2), x < = 1.00 and y < = 0.00 are satisfied. Element M is two or more elements selected from the group consisting of Nb, Ta, and Sb, and satisfies the relationship 0.00 < z < 2.00.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite body, a battery and an electronic device. Background Art

[0002] Lithium-ion batteries (including primary batteries and secondary batteries) are used as power sources for many electronic devices, including portable information devices. Among them, all-solid-state lithium-ion batteries that use solid electrolytes for lithium conduction between positive and negative electrodes have been proposed as lithium-ion batteries that have both high energy density and safety (for example, see Patent Document 1).

[0003] Solid electrolytes can conduct lithium ions without using an organic electrolyte and do not cause electrolyte leakage or volatilization of the electrolyte due to heat generated during driving, and therefore have attracted attention as highly safe materials.

[0004] As solid electrolytes used in such all-solid-state lithium-ion batteries, oxide-based solid electrolytes with high lithium ion conductivity, excellent insulation, and high chemical stability are widely known. As such oxides, lanthanum zirconate-based materials have high lithium ion conductivity, which should be particularly noted, and are expected to be used in batteries.

[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-215130

[0006] However, when such a solid electrolyte is used, the adhesion between the solid electrolyte and the active material and the adhesion between the solid electrolyte particles cannot be sufficiently excellent, and there are technical problems such as increased grain boundary resistance and reduced lithium ion conductivity. As a result, there is a problem that the discharge capacity is easily reduced, especially the retention rate of the discharge capacity during repeated charge and discharge is easily reduced. Summary of the invention

[0007] The composite body according to the application example of the present invention comprises:

[0008] Active substances;

[0009] The crystalline first electrolyte portion contains a lithium composite metal oxide represented by the following composition formula (1); and

[0010] The second electrolyte part contains a lithium composite metal oxide represented by the following composition formula (2), and covers at least a part of the surface of the active material.

[0011] At least a portion of the first electrolyte portion is bonded to the active material via the second electrolyte portion.

[0012] (Li 7-3x+y Ga x )(La 3-y Cay )Zr2O 12 …(1)

[0013] (In formula (1), the relationship of 0.10≤x≤1.00 and 0.00<y≤0.30 is satisfied.)

[0014] Li 7-z La3(Zr 2-z M z ) 12 …(2)

[0015] (In formula (2), the element M is two or more elements selected from the group consisting of Nb, Ta, and Sb, and satisfies the relationship of 0.00<z<2.00.)

[0016] In addition, a battery according to an application example of the present invention includes:

[0017] A composite body according to an application example of the present invention;

[0018] an electrode disposed on one side of the composite body; and

[0019] The current collector is disposed on the other surface side of the composite.

[0020] Furthermore, an electronic device according to an application example of the present invention includes the battery according to the application example of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is an enlarged cross-sectional view schematically showing an example of the composite body of the present invention.

[0022] Figure 2 It is a schematic cross-sectional view schematically showing the structure of a lithium ion secondary battery.

[0023] Figure 3 It is a three-dimensional diagram showing the structure of a wearable device as an electronic device.

[0024] Figure 4 This is a table summarizing the conditions for the composites of Examples A1 to A16 and the heating temperatures in the firing treatment.

[0025] Figure 5 This is a table summarizing the conditions for the composites of Examples A17 to A19 and Comparative Examples A1 to A12 and the heating temperatures in the firing treatment.

[0026] Figure 6 This is a table summarizing the evaluation results of the composites of Examples A1 to A16.

[0027] Figure 7This is a table summarizing the evaluation results of the composites of Examples A17 to A19 and Comparative Examples A1 to A12.

[0028] Figure 8 This is a table showing the evaluation results of the batteries of Examples B1 to B16 in summary.

[0029] Fig. 9 This is a table summarizing the evaluation results of the batteries of Examples B17 to B19 and Comparative Examples B1 to B12.

[0030] Description of Reference Numerals

[0031] P100: composite; P10: active material; P11: first electrolyte part; P12: second electrolyte part; P13: third electrolyte part; 100: lithium-ion battery; 30: negative electrode; 41: collector; 42: collector; 300: wearable device; 301: belt; 302: sensor; 303: display part; 304: processing part; WR: wrist. DETAILED DESCRIPTION

[0032] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0033] [1] Complex

[0034] First, the complex of the present invention will be described.

[0035] Figure 1 This is an enlarged cross-sectional view schematically showing an example of the composite body of the present invention.

[0036] like Figure 1 As shown, the composite P100 includes: an active material P10; a crystalline first electrolyte portion P11; and a second electrolyte portion P12 covering at least a portion of the surface of the active material P10, and at least a portion of the first electrolyte portion P11 is bonded to the active material P10 via the second electrolyte portion P12.

[0037] In other words, the composite P100 includes: an active material P10; a crystalline first electrolyte portion P11 containing a lithium composite metal oxide represented by the following composition formula (1); and a second electrolyte portion P12 containing a lithium composite metal oxide represented by the following composition formula (2), covering at least a portion of the surface of the active material P10. That is, the second electrolyte portion P12 is between the active material P10 and the first electrolyte portion P11.

[0038] The first electrolyte portion P11 contains a lithium mixed metal oxide represented by the following composition formula (1), and the second electrolyte portion P12 contains a lithium mixed metal oxide represented by the following composition formula (2).

[0039] (Li 7-3x+y Ga x )(La 3-y Ca y )Zr2O 12 …(1)

[0040] (In formula (1), the relationship of 0.10≤x≤1.00 and 0.00<y≤0.30 is satisfied.)

[0041] Li 7-z La3(Zr 2-z M z ) 12 …(2)

[0042] (In formula (2), the element M is two or more elements selected from the group consisting of Nb, Ta, and Sb, and satisfies the relationship of 0.00<z<2.00.)

[0043] By means of the above structure, a composite body can be provided, which can make the adhesion between the solid electrolyte and the active material and the adhesion between the solid electrolytes sufficiently excellent, can suppress the increase of the grain boundary resistance, and suppress the reduction of the lithium ion conductivity. In addition, by using such a composite body, a battery can be provided in which the discharge capacity is difficult to decrease, and in particular, the discharge capacity can be appropriately maintained even when repeatedly charged and discharged.

[0044] In contrast, when the above conditions are not met, satisfactory results cannot be obtained. For example, in the case of having an active material and a portion corresponding to the first electrolyte portion, but not having a portion corresponding to the second electrolyte portion, the adhesion between the active material and the portion corresponding to the first electrolyte portion deteriorates, the grain boundary resistance increases, and the lithium ion conductivity deteriorates. As a result, when applied to a battery, the discharge capacity is easily reduced, and in particular, the retention rate of the discharge capacity during repeated charge and discharge is easily reduced.

[0045] In addition, when the portion corresponding to the first electrolyte portion is composed of other electrolytes instead of the lithium composite metal oxide represented by the above composition formula (1), the adhesion between the active material and the portion corresponding to the first electrolyte portion cannot be sufficiently excellent, the grain boundary resistance becomes high, and the lithium ion conductivity cannot be sufficiently excellent. As a result, when applied to a battery, the discharge capacity is easily reduced, and in particular, the retention rate of the discharge capacity during repeated charge and discharge is easily reduced.

[0046] In particular, when the electrolyte constituting the portion corresponding to the first electrolyte portion has a composition in which x in the above composition formula (1) is less than the above lower limit, the lithium ion conductivity, especially the conductivity within the particle body, is significantly reduced.

[0047] In addition, when the electrolyte constituting the portion corresponding to the first electrolyte portion has a composition in which x in the above composition formula (1) exceeds the upper limit value, Ga (gallium) cannot completely enter the crystal lattice of the electrolyte, generating highly insulating gallium oxide, resulting in a problem of reduced overall lithium ion conductivity.

[0048] When the electrolyte constituting the portion corresponding to the first electrolyte portion has a composition in which y in the above composition formula (1) is 0, that is, when Ca is not contained, the lithium ion conductivity is significantly reduced.

[0049] In addition, when the electrolyte constituting the portion corresponding to the first electrolyte portion has a composition in which y in the above composition formula (1) exceeds the above upper limit value, Ca cannot completely enter the electrolyte lattice, and highly insulating calcium oxide is generated, resulting in a problem of reduced total lithium ion conductivity.

[0050] In addition, when the portion corresponding to the second electrolyte portion is composed of other electrolytes instead of the lithium composite metal oxide represented by the above composition formula (2), the adhesion between the active material and the portion corresponding to the first electrolyte portion cannot be sufficiently excellent, the grain boundary resistance becomes high, and the lithium ion conductivity cannot be sufficiently excellent. As a result, when applied to a battery, the discharge capacity is easily reduced, and in particular, the retention rate of the discharge capacity during repeated charge and discharge is easily reduced.

[0051] In particular, when the electrolyte constituting the portion corresponding to the second electrolyte portion has a composition in which z in the above-mentioned composition formula (2) is 0.00, that is, has a composition that does not contain the element M, even if the decrease in the total ion conductivity when placed in the atmosphere can be suppressed, it is difficult to sufficiently improve the initial total ion conductivity itself.

[0052] Furthermore, when the electrolyte constituting the portion corresponding to the second electrolyte portion has a composition in which z in the above composition formula (2) is 2.00 or more, even if the decrease in total ion conductivity when exposed to the atmosphere can be suppressed, it is difficult to sufficiently increase the initial total ion conductivity itself.

[0053] In addition, when the portion corresponding to the second electrolyte portion is composed of other electrolytes instead of the lithium composite metal oxide represented by the above composition formula (2), even if the decrease in the total ion conductivity when placed in the atmosphere can be suppressed, it is difficult to fully improve the initial total ion conductivity itself. In such a case, as the electrolyte constituting the portion corresponding to the second electrolyte portion, for example, an electrolyte in which the element M in the above composition formula (2) is only one selected from the group consisting of Nb, Ta and Sb can be cited.

[0054] [1-1] Active substances

[0055] The active material P10 constituting the composite P100 may be any of a negative electrode active material and a positive electrode active material.

[0056] Examples of negative electrode active materials include Nb2O5, V2O5, TiO2, In2O3, ZnO, SnO2, NiO, ITO, AZO, GZO, ATO, FTO, Li4Ti5O 12 , Li2Ti3O7 and other lithium composite oxides. In addition, for example, metals such as Li, Al, Si, Si-Mn, Si-Co, Si-Ni, Sn, Zn, Sb, Bi, In, Au, and alloys, carbon materials, LiC 24 , LiC6, etc., in which lithium ions are inserted between the layers of carbon materials.

[0057] As the positive electrode active material, for example, an oxide containing Li and O can be used. More specifically, a composite oxide of lithium containing at least Li and composed of one or more elements selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, and Cu can be used. As such a composite oxide, for example, a composite metal compound containing lithium (Li) and one or more elements selected from the group consisting of vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), and copper (Cu) can be listed. As such a composite oxide of lithium, LiCoO2, LiNiO2, LiMn2O4, Li2Mn2O3, NMC (Li p (Ni x Mn 1-x- y Co y )O2)、NCA(Li(Ni x Co y Al 1-x-y )O2)、LiCr 0.5 Mn 0.5 O2, LiFePO4, Li2FeP2O7, LiMnPO4, LiFeBO3, Li3V2(PO4)3, Li2CuO2, Li2FeSiO4, Li2MnSiO4, etc. In addition, it can also be a solid solution in which a part of the atoms in the crystal of the above-mentioned lithium composite oxide are replaced by other transition metals, typical metals, alkali metals, alkali rare earths, lanthanides, chalcogenides, halogens, etc. In addition, as the positive electrode active material, for example, fluorides such as LiFeF3, LiBH4 or Li4BN3H 10 boride complex compounds, iodine complex compounds such as polyvinylpyridine-iodine complex, non-metallic compounds such as sulfur, etc.

[0058] The active material P10 is preferably a positive electrode active material, more preferably a positive electrode active material containing Li, and still more preferably a lithium composite oxide.

[0059] This can further improve the adhesion between the active material P10 and the second electrolyte portion P12. In addition, the battery including the composite P100 can further improve the charge and discharge performance under high load.

[0060] In addition, for example, in order to reduce the interface resistance with the solid electrolyte, especially with the second electrolyte part P12, improve the electronic conductivity, etc., a covering layer can be formed on the surface of the active material P10. For example, by forming a thin film of LiNbO3, Al2O3, ZrO2, Ta2O5, etc. on the surface of the positive electrode active material composed of LiCoO2, the interface resistance of lithium ion conduction can be further reduced. The thickness of the covering layer is not particularly limited, and is preferably greater than 3nm and less than 1μm.

[0061] The active material P10 may be, for example, a porous body having pores inside, and may be in any shape such as spherical, scaly, irregular, columnar, plate-like, sheet-like, flake-like, granular, or block-like. In the illustrated structure, it is in granular form.

[0062] When the active material P10 is in a granular form, the average particle size of the active material P10 is not particularly limited, but is preferably 0.1 μm to 150 μm, more preferably 0.3 μm to 10 μm, and further preferably 0.5 μm to 5 μm.

[0063] This makes it easy to achieve both an actual capacity density close to the theoretical capacity of the active material P10 and a high charge and discharge rate.

[0064] It should be noted that in this specification, the average particle size refers to the average particle size based on volume, which can be obtained, for example, by adding a sample to methanol, dispersing it with an ultrasonic disperser for 3 minutes, and measuring the resulting dispersion with a Coulter counter particle size distribution analyzer (TA-II type manufactured by COULTER ELECTRONICS INS) using an aperture of 50 μm.

[0065] The particle size distribution of the active material P10 is not particularly limited, and for example, in a particle size distribution having one peak, the half-value width of the peak may be 0.1 μm or more and 19 μm or less.

[0066] The volume density of the active material P10 is preferably 50% or more and 90% or less, and more preferably 50% or more and 70% or less.

[0067] This increases the surface area in the pores of the active material P10, and makes it easier to increase the contact area between the active material P10 and the electrolyte, especially the second electrolyte portion P12, making it easier to achieve higher capacity in a battery including the composite P100.

[0068] When the above-mentioned volume density is β (%), the apparent volume of the pores containing the active material P10 is v, the mass of the active material P10 is w, and the density of the particles of the active material P10 is ρ, the following mathematical formula (a) holds. Thus, the volume density can be calculated.

[0069] β={w / (v·ρ)}×100…(a)

[0070] The resistivity of the active material P10 is preferably 700 Ω·cm or less.

[0071] Thus, in a battery including the composite P100, a more excellent C rate (charge and discharge speed) can be obtained.

[0072] The resistivity can be determined, for example, by attaching a copper foil as an electrode to the surface of the active material P10 and performing a DC polarization measurement.

[0073] The proportion of the active material P10 in the composite P100 is preferably 25 mass % to 75 mass %, more preferably 30 mass % to 70 mass %, and even more preferably 40 mass % to 60 mass %.

[0074] This makes it possible to obtain a battery having a particularly excellent balance between battery capacity and C rate (charge and discharge speed).

[0075] [1-2] First electrolyte part

[0076] The composite P100 includes a first electrolyte part P11 containing a crystalline lithium mixed metal oxide represented by the above composition formula (1). In the following description, the lithium mixed metal oxide represented by the above composition formula (1) is also referred to as a "first solid electrolyte."

[0077] In the above composition formula (1), x only needs to satisfy the relationship of 0.10≤x≤1.00, preferably satisfies the relationship of 0.20≤x≤1.00, more preferably satisfies the relationship of 0.20≤x≤0.90, and further preferably satisfies the relationship of 0.20≤x≤0.80.

[0078] This makes it possible to more significantly exhibit the above-mentioned effects. In addition, the affinity and adhesion between the first electrolyte portion P11 and the second electrolyte portion P12 can be made more excellent.

[0079] In the above composition formula (1), y may satisfy the relationship of 0.00<y≤0.30, and preferably satisfies the relationship of 0.01≤y≤0.27, more preferably satisfies the relationship of 0.02≤y≤0.24, and further preferably satisfies the relationship of 0.03≤y≤0.20.

[0080] This makes it possible to more significantly exhibit the above-mentioned effects. In addition, the affinity and adhesion between the first electrolyte portion P11 and the second electrolyte portion P12 can be made more excellent.

[0081] It should be noted that the first solid electrolyte constituting the first electrolyte part P11 may contain other elements, that is, elements other than Li, Ga, La, Ca, Zr and O, as long as they are trace amounts, in addition to the elements constituting the above-mentioned composition formula (1). The other elements may be one or more.

[0082] The content of the other elements contained in the first solid electrolyte is preferably 100 ppm or less, and more preferably 50 ppm or less.

[0083] When two or more elements are contained as the other elements, the sum of the contents of these elements is adopted as the content of the other elements.

[0084] The first electrolyte portion P11 only needs to contain the first solid electrolyte, and may contain components other than the first solid electrolyte.

[0085] The content of components other than the first solid electrolyte in the first electrolyte portion P11 is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 1.0% by mass or less.

[0086] The proportion of the first electrolyte portion P11 in the composite P100 is preferably 25 mass % to 75 mass %, more preferably 30 mass % to 70 mass %, and further preferably 40 mass % to 60 mass %.

[0087] This makes it possible to obtain a battery having a particularly excellent balance between battery capacity and C rate (charge and discharge speed).

[0088] [1-3] Second electrolyte part

[0089] The composite P100 includes a second electrolyte portion P12 containing a lithium composite metal oxide represented by the above composition formula (2). In the following description, the lithium composite metal oxide represented by the above composition formula (2) is also referred to as a "second solid electrolyte". Figure 1In the figure, for convenience, the entire surface of the active material P10 is shown to be covered with the second electrolyte portion P12, but it is sufficient that at least a part of the surface of the active material P10 is covered.

[0090] In the above composition formula (2), z may satisfy the relationship of 0.00<z<2.00, preferably satisfies the relationship of 0.20≤z≤1.80, more preferably satisfies the relationship of 0.40≤z≤1.50, and further preferably satisfies the relationship of 0.50≤z≤1.30.

[0091] This makes it possible to more significantly exert the above-mentioned effects. In addition, the affinity and adhesion of the second electrolyte portion P12 to the active material P10 or the first electrolyte portion P11 can be made more excellent.

[0092] The lithium composite metal oxide represented by the above composition formula (2) constituting the second electrolyte part P12 contains two or more elements selected from the group consisting of Nb, Ta and Sb as the element M. When the element M constituting the lithium composite metal oxide contains at least Nb, it is preferred that when the lithium composite metal oxide is represented by the following composition formula (2'), the value of z' is greater than 0.01 and less than 0.40, and more preferably greater than 0.05 and less than 0.38.

[0093] Li 7-z La3(Zr 2-z Nb z’ M' z” ) 12 …(2')

[0094] (In the formula (2'), the element M' is one or more elements selected from the group consisting of Ta and Sb, and satisfies the relationship of 0.00<z', 0.00<z", and 0.00<z'+z"<2.00.)

[0095] This reduces the crystallinity of the second electrolyte portion, forms a smooth interface, and further improves the lithium ion conductivity.

[0096] It should be noted that the second solid electrolyte constituting the second electrolyte part P12 may contain other elements, that is, elements other than Li, La, Zr, Nb, Ta, Sb and O, as long as they are trace amounts, in addition to the elements constituting the above-mentioned composition formula (2). The other elements may be one or more.

[0097] The content of the other elements contained in the second solid electrolyte is preferably 100 ppm or less, and more preferably 50 ppm or less.

[0098] When two or more elements are contained as the other elements, the sum of the contents of these elements is adopted as the content of the other elements.

[0099] The second electrolyte portion P12 only needs to contain the second solid electrolyte, and may contain components other than the second solid electrolyte.

[0100] The content of components other than the second solid electrolyte in the second electrolyte portion P12 is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 1.0% by mass or less.

[0101] The proportion of the second electrolyte portion P12 in the composite P100 is preferably 0.06 mass % to 19.0 mass %, more preferably 0.09 mass % to 9.3 mass %, and further preferably 0.12 mass % to 4.8 mass %.

[0102] This makes it possible to obtain a battery with a more excellent C rate (charge and discharge speed).

[0103] When the second electrolyte portion P12 is formed in a film shape on the surface of the active material P10, the average thickness of the second electrolyte portion P12 is preferably 0.002 μm to 0.300 μm, more preferably 0.003 μm to 0.150 μm, and further preferably 0.004 μm to 0.080 μm.

[0104] This makes it possible to obtain a battery with a more excellent C rate (charge and discharge speed).

[0105] It should be noted that, in this specification, the average thickness of the second electrolyte part P12 refers to the thickness of the second electrolyte part P12 calculated based on the mass of the active material P10 and the second electrolyte part P12 contained in the composite P100 as a whole, assuming that the second electrolyte part P12 is provided on the entire outer surface of the active material P10 with a uniform thickness. In particular, when the active material P10 is granular, it refers to the thickness of the second electrolyte part P12 calculated based on the mass of the active material P10 and the second electrolyte part P12 contained in the composite P100 as a whole, assuming that each active material P10 is spherical with a diameter equal to the average particle size, and a second electrolyte part P12 of uniform thickness is formed on the entire outer surface of each active material P10, and calculated based on the specific gravity.

[0106] In addition, when the active material P10 is in a granular form, when the average particle size of the active material P10 is set to D [μm] and the average thickness of the second electrolyte portion P12 is set to T [μm], it is preferred that the relationship of 0.0005≤T / D≤0.2500 is satisfied, and it is more preferred that the relationship of 0.0005≤T / D≤0.0700 is satisfied, and it is further preferred that the relationship of 0.0010≤T / D≤0.0200 is satisfied.

[0107] This makes it possible to obtain a battery with a more excellent C rate (charge and discharge speed).

[0108] The second electrolyte portion P12 only needs to cover at least a portion of the surface of the active material P10. The coverage of the second electrolyte portion P12 relative to the outer surface of the active material P10, that is, the ratio of the area of ​​the covered portion of the second electrolyte portion P12 to the total area of ​​the outer surface of the active material P10 is not particularly limited, and is preferably 30% or more, more preferably 40% or more, and further preferably 50% or more. In addition, the upper limit of the coverage may be 100% or less.

[0109] Thereby, the aforementioned effects can be more significantly exerted.

[0110] [1-4] Third electrolyte part

[0111] The composite of the present invention only needs to have the aforementioned structure, that is, the active material, the first electrolyte part, and the second electrolyte part. In the structure shown in the figure, in addition to the active material P10, the first electrolyte part P11, and the second electrolyte part P12, it also has an amorphous third electrolyte part P13 containing Li and connected to the first electrolyte part P11. In particular, the third electrolyte part P13 is provided in the internal space of the composite P100.

[0112] This can further reduce the proportion of voids in the composite P100, and more significantly demonstrate the effects of the present invention described above.

[0113] In the following description, the amorphous solid electrolyte constituting the third electrolyte portion P13 is also referred to as a “third solid electrolyte”.

[0114] The third electrolyte part P13 only needs to be an amorphous electrolyte containing Li, that is, an electrolyte containing a third solid electrolyte. As the third solid electrolyte, for example, Li3BO3, Li3BO3-Li4SiO4, Li3BO3-Li3PO4, Li3BO3-Li2SO4, Li2CO3-Li3BO3, Li2O-TiO2, La2O3-Li2O-TiO2, LiNbO3, LiSO4, Li4SiO4, Li3PO4-Li4SiO4, Li4 GeO4-Li3VO4, Li4SiO4-Li3VO4, Li4GeO4-Zn2GeO2, Li4SiO4-LiMoO4, Li4SiO4-Li4ZrO4, SiO2-P2O5-Li2O, SiO2- P2O5-LiCl, Li2O-LiCl-B2O3, LiI, LiI-CaI2, LiI-CaO, LiAlCl4, LiAlF4, LiF-Al2O3, LiBr-Al2O3, LiI-Al2O3, Li 2.88 PO 3.73 N 0.14 , Li3NI2, Li3N-LiI-LiOH, Li3N-LiCl, Li6NBr3, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-P2S5, etc., and one selected from them or two or more thereof can be used in combination.

[0115] In particular, the third electrolyte portion P13 preferably contains Li, B, and O.

[0116] Thus, the lithium ion conductivity of the composite P100 can be further improved. In addition, such a third solid electrolyte generally has a low melting point, and for example, the molten liquid of the third solid electrolyte can be appropriately filled in the gaps inside the molded body having the active material P10, the first electrolyte portion P11, and the second electrolyte portion P12 by the method described later.

[0117] The third electrolyte portion P13 is in contact with the first electrolyte portion P11 and only needs to contain the third solid electrolyte, and may contain components other than the third solid electrolyte.

[0118] The content of components other than the third solid electrolyte in the third electrolyte portion P13 is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 1.0% by mass or less.

[0119] The proportion of the third electrolyte portion P13 in the composite P100 is preferably 1 mass % to 10 mass %, more preferably 1 mass % to 8 mass %, and even more preferably 1 mass % to 6 mass %.

[0120] This makes it possible to obtain a battery having a particularly excellent balance between battery capacity and C rate (charge and discharge speed).

[0121] [1-5] Other structures

[0122] The composite P100 may have structures other than the above-mentioned active material P10, first electrolyte portion P11, second electrolyte portion P12, and third electrolyte portion P13. Hereinafter, such structures are also referred to as "other structures" in this item.

[0123] As other structures, for example, a fourth electrolyte part containing a crystalline solid electrolyte represented by a composition formula other than the above composition formula (1) and the above composition formula (2) can be cited.

[0124] The ratio of other structures in the composite P100 is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 1.0% by mass or less.

[0125] [1-6] Other conditions

[0126] The size and shape of the complex P100 are not particularly limited.

[0127] In addition, in the illustrated structure, the boundary between the active material P10 and the second electrolyte part P12, the boundary between the second electrolyte part P12 and the first electrolyte part P11, and the boundary between the first electrolyte part P11 and the third electrolyte part P13 are all clear, but these boundaries do not necessarily need to be clear, and adjacent parts, such as a part of the constituent components of one of the active material P10 and the second electrolyte part P12, may move toward the other.

[0128] In the illustrated structure, the third electrolyte portion P13 is in contact only with the first electrolyte portion P11 , but may be in contact with a portion other than the first electrolyte portion P11 , such as the active material P10 or the second electrolyte portion P12 , together with the first electrolyte portion P11 .

[0129] In the illustrated structure, the second electrolyte portion P12 is in contact with only the active material P10 and the first electrolyte portion P11 , but the active material P10 and the first electrolyte portion P11 may be in contact with other portions, such as the third electrolyte portion P13 .

[0130] In the illustrated structure, the first electrolyte portion P11 is in contact with only the second electrolyte portion P12 and the third electrolyte portion P13 , but the second electrolyte portion P12 and the third electrolyte portion P13 may be in contact with other portions, such as the active material P10 .

[0131] [2] Method for producing a composite

[0132] Next, the method for producing the composite of the present invention will be described.

[0133] The composite of the present invention can be appropriately manufactured, for example, using a method comprising the following steps: a second precursor contact step, in which a solution containing a precursor of a second solid electrolyte is brought into contact with the active material P10; a first precursor contact step, in which a solution containing a precursor of the first solid electrolyte is brought into contact with the active material P10 that has undergone the second precursor contact step; and a third electrolyte part forming step, in which the active material P10 that has undergone the second precursor contact step and the first precursor contact step is brought into contact with the third solid electrolyte to form a third electrolyte part P13.

[0134] [2-1] Second Precursor Contact Step

[0135] In the second precursor contact step, a solution containing a precursor of the second solid electrolyte is brought into contact with the active material P10.

[0136] The method for contacting the solution containing the precursor of the second solid electrolyte with the active material P10 is not particularly limited, and examples thereof include a method of adding the active material P10 to the solution containing the precursor of the second solid electrolyte, a method of imparting the solution containing the precursor of the second solid electrolyte to the active material P10, and the like.

[0137] Examples of a method for adding the active material P10 to the solution containing the precursor of the second solid electrolyte include an immersion method.

[0138] Examples of a method for applying the solution containing the precursor of the second solid electrolyte to the active material P10 include a dropping method, a spraying method, a coating method, and a spin coating method.

[0139] As the solution containing the precursor of the second solid electrolyte, for example, a solution in which a lithium compound, a lanthanum compound, a zirconium compound, and a metal compound containing the element M are dissolved can be used.

[0140] Such a solution can be prepared by mixing, for example, a lithium raw material solution in which a lithium compound is dissolved, a lanthanum raw material solution in which a lanthanum compound is dissolved, a zirconium raw material solution in which a zirconium compound is dissolved, and a metal raw material solution in which a metal compound containing the element M is dissolved. In this case, the order of mixing the raw material solutions is not particularly limited.

[0141] As described above, when a raw material solution is used, the solvent and the dispersion medium constituting the raw material solution may have a common composition or different compositions.

[0142] In preparing the solution containing the precursor of the second solid electrolyte, it is preferred to use a lithium compound such that the lithium content in the solution is equal to or greater than and 1.2 times the stoichiometric composition of the composition formula (2).

[0143] In the preparation of the solution containing the precursor of the second solid electrolyte, it is preferred to use a lanthanum compound so that the lanthanum content in the solution is equal to the stoichiometric composition of the composition formula (2).

[0144] In the preparation of the solution containing the precursor of the second solid electrolyte, it is preferred to use a zirconium compound such that the zirconium content in the solution is equal to the stoichiometric composition of the composition formula (2).

[0145] In the preparation of the solution containing the precursor of the second solid electrolyte, it is preferred to use a metal compound containing the element M so that the content of the element M in the solution is equal to the stoichiometric composition of the composition formula (2).

[0146] As lithium compounds, for example, lithium metal salts, lithium alkoxides, etc. can be listed, and one of them or two or more of them can be used in combination. As lithium metal salts, for example, lithium chloride, lithium nitrate, lithium sulfate, lithium acetate, lithium hydroxide, lithium carbonate, (2,4-pentanedione) lithium, etc. can be listed. In addition, as lithium alkoxides, for example, lithium methoxide, lithium ethoxide, lithium n-propoxide, lithium isopropoxide, lithium n-butoxide, lithium isobutoxide, lithium sec-butoxide, lithium tert-butoxide, lithium dipivaloyl methane, etc. can be listed. Among them, as a lithium compound, it is preferably selected from one or more of the group consisting of lithium nitrate, lithium sulfate and (2,4-pentanedione) lithium. As a lithium source, a hydrate can also be used.

[0147] In addition, as a lanthanum compound as a metal compound of a lanthanum source, for example, lanthanum metal salts, lanthanum alkoxides, etc. can be listed, and one of them or two or more thereof can be used in combination. As a lanthanum metal salt, for example, lanthanum chloride, lanthanum nitrate, lanthanum sulfate, lanthanum acetate, tri(2,4-pentanedione) lanthanum, etc. can be listed. As a lanthanum alkoxide, for example, lanthanum trimethylol, lanthanum triethylol, lanthanum tri-n-propoxide, lanthanum tri-isopropoxide, lanthanum tri-n-butoxide, lanthanum tri-isobutoxide, lanthanum tri-sec-butoxide, lanthanum tri-tert-butoxide, lanthanum tri(dipivaloylmethane) lanthanum, etc. can be listed. Among them, as a lanthanum compound, at least one of lanthanum nitrate and tri(2,4-pentanedione) lanthanum is preferred. As a lanthanum source, a hydrate can also be used.

[0148] In addition, as the zirconium compound of the metal compound as the zirconium source, for example, zirconium metal salts, zirconium alkoxides, etc. can be listed, and one of them can be used or two or more can be used in combination. As the zirconium metal salt, for example, zirconium chloride, zirconium oxychloride, zirconium oxynitrate, zirconium oxysulfate, zirconium oxyacetate, zirconium acetate, etc. can be listed. In addition, as zirconium alkoxides, for example, tetramethoxy zirconium, tetraethoxy zirconium, tetra-n-propoxy zirconium, tetraisopropoxy zirconium, tetra-n-butoxy zirconium, tetraisobutoxy zirconium, tetra-sec-butoxy zirconium, tetra-tert-butoxy zirconium, tetrakis(dipivaloylmethane) zirconium, etc. can be listed. Among them, as the zirconium compound, tetra-n-butoxy zirconium is preferred. As the zirconium source, hydrates can also be used.

[0149] In addition, as a tantalum compound of a metal compound as a tantalum source of the element M, for example, tantalum metal salts, tantalum alkoxides, etc. can be listed, and one of them or two or more of them can be used in combination. As tantalum metal salts, for example, tantalum chloride, tantalum bromide, etc. can be listed. In addition, as tantalum alkoxides, for example, pentamethoxy tantalum, pentaethoxy tantalum, pentaisopropoxy tantalum, penta-propoxy tantalum, pentaisobutoxy tantalum, penta-n-butoxy tantalum, penta-sec-butoxy tantalum, penta-tert-butoxy tantalum, etc. can be listed. Among them, as a tantalum compound, it is preferred that one or more selected from the group consisting of pentaethoxy tantalum, penta-n-propoxy tantalum and penta-n-butoxy tantalum. As a tantalum source, a hydrate can also be used.

[0150] In addition, as the antimony compound of the metal compound as the antimony source of the element M, for example, antimony metal salts, antimony alkoxides, etc. can be listed, and one of them or two or more of them can be used in combination. As antimony metal salts, for example, antimony bromide, antimony chloride, antimony fluoride, etc. can be listed. In addition, as antimony alkoxides, for example, trimethoxy antimony, triethoxy antimony, triisopropoxy antimony, tri-n-propoxy antimony, triisobutoxy antimony, tri-n-butoxy antimony, etc. can be listed. Among them, as the antimony compound, at least one of triisobutoxy antimony and tri-n-butoxy antimony is preferred. As the antimony source, hydrates can also be used.

[0151] In addition, as the niobium compound of the metal compound as the niobium source of the element M, for example, niobium metal salts, niobium alkoxides, niobium acetylacetonate, etc. can be listed, and one of them or two or more of them can be used in combination. As the niobium metal salt, for example, niobium chloride, niobium oxychloride, niobium oxalate, etc. can be listed. In addition, as niobium alkoxides, for example, pentaethoxy niobium, penta-n-propoxy niobium, penta-n-butoxy niobium, penta-isopropoxy niobium, penta-sec-butoxy niobium, etc. can be listed. Among them, as the niobium compound, penta-n-butoxy niobium is preferred. As the niobium source, a hydrate can also be used.

[0152] In addition, the solution containing the precursor of the second solid electrolyte described above preferably contains oxyanions.

[0153] Thus, the second solid electrolyte can be appropriately formed in the subsequent heat treatment, especially the heat treatment under relatively mild conditions. In addition, the second electrolyte part P12 composed of the second solid electrolyte formed in this way has excellent adhesion with the first electrolyte part P11 composed of the active material P10 or the first solid electrolyte. As a result, the reliability of the composite P100 finally obtained can be made more excellent.

[0154] In this process, when preparing a solution containing the precursor of the above-mentioned second solid electrolyte into a solution containing oxygen-containing anions, it is preferred to use metal salts containing oxygen-containing anions as various metal compounds used as raw materials for forming the above-mentioned second solid electrolyte, but in the preparation of the solution containing the precursor of the above-mentioned second solid electrolyte, as a component different from the various metal compounds, oxygen-containing acid compounds that do not contain metal elements but contain oxygen-containing anions can also be used.

[0155] Examples of the oxygen-containing anions include halogen oxygen-containing acid ions, borate ions, carbonate ions, orthocarbonate ions, carboxylate ions, silicate ions, nitrite ions, nitrate ions, phosphite ions, phosphate ions, arsenate ions, sulfite ions, sulfate ions, sulfonate ions, and sulfite ions. Examples of the halogen oxygen-containing acids include hypochlorite ions, chlorite ions, chlorate ions, perchlorate ions, hypobromite ions, bromite ions, bromate ions, perbromate ions, hypoiodite ions, iodite ions, iodate ions, and periodate ions.

[0156] In addition, the oxoacid compound can be added, for example, after this step, during the heat treatment described later, or at a certain time during the heat treatment.

[0157] In the second precursor contact step, the active material P10 that contacts the solution containing the precursor of the second solid electrolyte may, for example, satisfy the same conditions as those of the active material P10 constituting the composite P100, or may satisfy different conditions. More specifically, for example, in the second precursor contact step, the active material P10 that contacts the solution containing the precursor of the second solid electrolyte may also differ from the active material P10 constituting the composite P100 in terms of shape, size, and other conditions.

[0158] As the solvent and the dispersion medium, there is no particular limitation, and for example, water or various organic solvents can be used. As the organic solvent, for example, alcohols, glycols, ketones, esters, ethers, organic acids, aromatics, amides, etc. can be listed, and a mixed solvent selected from one or a combination of two or more thereof can be used. As alcohols, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-propylene-1-ol, 2-n-butoxyethanol, etc. can be listed. As glycols, for example, ethylene glycol, propylene glycol, butanediol, hexanediol, pentanediol, hexanediol, heptanediol, dipropylene glycol, etc. can be listed. As ketones, for example, dimethyl ketone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, etc. can be listed. As esters, for example, methyl formate, ethyl formate, methyl acetate, methyl acetoacetate, etc. can be listed. As ethers, for example, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, dipropylene glycol monomethyl ether, etc. can be listed. As organic acids, for example, formic acid, acetic acid, 2-ethylbutyric acid, propionic acid, etc. can be listed. As aromatics, for example, toluene, o-xylene, p-xylene, etc. can be listed. As amides, for example, formamide, N,N-dimethylformamide, N,N-diethylformamide, dimethylacetamide, N-methylpyrrolidone, etc. can be listed. Among them, as the solvent and the dispersion medium, at least one of 2-n-butoxyethanol and ethanol is preferred.

[0159] [2-2] First heat treatment step

[0160] In the present embodiment, the active material P10 that has undergone the above-described second precursor contact step, that is, the active material P10 to which the precursor of the second solid electrolyte is attached, is heated before the first precursor contact step described later.

[0161] Thus, for example, the solvent and dispersion medium contained in the solution containing the precursor of the second solid electrolyte can be appropriately removed, and at least a part of the precursor of the second solid electrolyte can be converted into a metal oxide such as the second solid electrolyte. In particular, when the solution containing the precursor of the second solid electrolyte contains oxygen-containing anions, an oxide different from the second solid electrolyte can be appropriately formed in this process. Hereinafter, the oxide is also referred to as the "second precursor oxide". As a result, for example, the precursor of the second solid electrolyte or the second solid electrolyte attached to the active material P10 can be effectively prevented from accidentally peeling off in subsequent processes. In addition, the second electrolyte part P12 composed of the second solid electrolyte in the composite P100 can be made to have better adhesion with respect to the first electrolyte part P11 composed of the active material P10 or the first solid electrolyte. As a result, the reliability of the composite P100 obtained in the end can be made better.

[0162] In the following description, the case where the solution containing the precursor of the second solid electrolyte contains oxyanions and the second precursor oxide is formed in this step will be mainly described.

[0163] The heating in this step is preferably performed under conditions such that the content of the liquid component in the solution containing the precursor of the second solid electrolyte becomes sufficiently low.

[0164] More specifically, the content of the liquid component contained in the solid composition obtained in this step, that is, the content of the above-mentioned solvent and dispersion medium is preferably 1.0 mass % or less, and more preferably 0.1 mass % or less.

[0165] The heat treatment in this step may be performed under constant conditions or may be performed by combining different conditions.

[0166] For example, a heat treatment A whose main purpose is to remove the aforementioned solvent and dispersion medium and a heat treatment B whose main purpose is to react with the precursor of the second solid electrolyte, namely the aforementioned lithium compound, lanthanum compound, zirconium compound and metal compound containing element M, may be performed in combination.

[0167] In this case, for example, the portion corresponding to the solution containing the precursor of the second solid electrolyte provided in the second precursor contact step can be made of a gelled composition by heat treatment A, and can be made into a state containing almost no liquid component as described above by subsequent heat treatment B. In particular, when the solution containing the precursor of the second solid electrolyte contains oxygen-containing anions, heat treatment B can efficiently form the second precursor oxide.

[0168] The conditions of heat treatment A also depend on the boiling point or vapor pressure of the solvent or dispersion medium. The heating temperature in heat treatment A is preferably 50°C to 250°C, more preferably 60°C to 230°C, and further preferably 80°C to 200°C.

[0169] The heating time in the heat treatment A is preferably 10 minutes to 180 minutes, more preferably 20 minutes to 120 minutes, and even more preferably 30 minutes to 60 minutes.

[0170] Heat treatment A can be carried out in any atmosphere, can be carried out in an oxidizing atmosphere such as air or oxygen atmosphere, can also be carried out in a non-oxidizing atmosphere such as an inert gas such as nitrogen, helium, argon, etc. In addition, heat treatment A can also be carried out under reduced pressure or vacuum, under pressure.

[0171] In the heat treatment A, the atmosphere may be maintained at substantially the same conditions or may be changed to different conditions.

[0172] The conditions of heat treatment B also depend on the composition of the second precursor oxide to be formed, but the heating temperature in heat treatment B is preferably 400°C to 600°C, more preferably 430°C to 600°C, and further preferably 450°C to 600°C.

[0173] The heating time in the heat treatment B is preferably 5 minutes to 180 minutes, more preferably 10 minutes to 120 minutes, and even more preferably 15 minutes to 120 minutes.

[0174] Heat treatment B can be carried out in any atmosphere, can be carried out in oxidizing atmospheres such as air or oxygen atmosphere, can also be carried out in non-oxidizing atmospheres such as inert gases such as nitrogen, helium, argon. In addition, heat treatment B can also be carried out under reduced pressure or vacuum, under pressure. Especially, heat treatment B is preferably carried out in an oxidizing atmosphere.

[0175] It should be noted that the heat treatment A and the heat treatment B may be performed continuously. For example, in the heat treatment A, the temperature may be increased at a constant temperature increase rate without setting a time for maintaining the temperature within a predetermined range.

[0176] In the case where the solid composition obtained in this step contains a second precursor oxide, the second precursor oxide preferably has a crystalline structure different from the crystalline structure of the second solid electrolyte. In the present invention, regarding the crystalline structure, "different" means: in addition to different types of crystalline structures, it also includes a broad concept such as the same type but at least one lattice constant is different.

[0177] In particular, the second solid electrolyte is composed of a solid electrolyte having a cubic garnet-type crystal structure, whereas the crystal structure of the second precursor oxide is preferably a tetragonal garnet-type crystal structure or a pyrochlore oxide structure.

[0178] Therefore, when the conditions for the heat treatment after this step are relaxed, for example, even at a lower temperature and a shorter time, it is possible to appropriately form a second electrolyte part P12 composed of a solid electrolyte that has excellent adhesion to the active material P10 or the first electrolyte part P11 and particularly excellent properties such as ion conductivity.

[0179] It should be noted that the crystal structure of the second precursor oxide may also be the above-mentioned tetragonal garnet-type crystal structure, or a crystal structure other than the pyrochlore oxide structure, such as cubic crystals such as perovskite structure, rock salt structure, diamond structure, fluorite structure, spinel structure, orthorhombic crystals such as orthorhombic crystals such as ramsbillite type, and trigonal crystals such as corundum type.

[0180] The crystal grain size of the second precursor oxide is not particularly limited, but is preferably 10 nm to 200 nm, more preferably 15 nm to 180 nm, and further preferably 20 nm to 160 nm.

[0181] Thus, the melting point of the second precursor oxide can be further reduced by the phenomenon of melting point reduction accompanied by the increase of surface energy, i.e., the so-called Gibbs-Thomson effect, and the conditions for the heat treatment after this step can be further relaxed. In addition, the adhesion between the active material P10 and the second electrolyte part P12, and the adhesion between the second electrolyte part P12 and the first electrolyte part P11 in the final composite P100 can be made better.

[0182] The second precursor oxide is preferably composed of substantially a single crystalline structure.

[0183] Therefore, in the heat treatment after this process, the crystal phase transition that occurs when forming a solid electrolyte having a cubic garnet-type crystal structure essentially becomes one, thereby suppressing the formation of included crystals caused by segregation or thermal decomposition of elements accompanying the crystal phase transition, thereby further improving various properties of the second solid electrolyte.

[0184] It should be noted that, when only one exothermic peak is observed in the range of 300°C to 1000°C when measuring the object at a heating rate of 10°C / min using TG-DTA, the object can be judged to be "substantially composed of a single crystal structure".

[0185] [2-3] First Precursor Contact Step

[0186] In the first precursor contact step, a solution containing a precursor of the first solid electrolyte is brought into contact with the active material P10 that has undergone the second precursor contact step.

[0187] There is no particular limitation on the method for contacting a solution containing a precursor of the first solid electrolyte with the active material P10 that has undergone a second precursor contact process. Examples include a method of adding the active material P10 that has undergone a second precursor contact process to a solution containing a precursor of the first solid electrolyte, a method of imparting a solution containing a precursor of the first solid electrolyte to the active material P10 that has undergone a second precursor contact process, and the like.

[0188] Examples of a method for adding the active material P10 that has undergone the second precursor contact step to the solution containing the precursor of the first solid electrolyte include an impregnation method.

[0189] Examples of a method for applying the solution containing the precursor of the first solid electrolyte to the active material P10 that has undergone the second precursor contact step include a dropping method, a spraying method, a coating method, and a spin coating method.

[0190] As the solution containing the precursor of the first solid electrolyte, for example, a solution in which a lithium compound, a gallium compound, a lanthanum compound, a calcium compound, and a zirconium compound are dissolved can be used.

[0191] Such a solution can be prepared by mixing, for example, a lithium raw material solution in which a lithium compound is dissolved, a gallium raw material solution in which a gallium compound is dissolved, a lanthanum raw material solution in which a lanthanum compound is dissolved, a calcium raw material solution in which a calcium compound is dissolved, and a zirconium raw material solution in which a zirconium compound is dissolved. In this case, the order of mixing the raw material solutions is not particularly limited.

[0192] As described above, when a raw material solution is used, the solvent and the dispersion medium constituting the raw material solution may have a common composition or different compositions.

[0193] In preparing the solution containing the precursor of the first solid electrolyte, a lithium compound is preferably used so that the lithium content in the solution is 1.05 times or more and 1.30 times or less relative to the stoichiometric composition of the composition formula (1).

[0194] In the preparation of the solution containing the precursor of the first solid electrolyte, it is preferred to use a gallium compound so that the gallium content in the solution is equal to the stoichiometric composition of the composition formula (1).

[0195] In the preparation of the solution containing the precursor of the first solid electrolyte, it is preferred to use a lanthanum compound such that the lanthanum content in the solution is equal to the stoichiometric composition of the composition formula (1).

[0196] In the preparation of the solution containing the precursor of the first solid electrolyte, it is preferred to use a calcium compound so that the content of calcium in the solution is equal to the stoichiometric composition of the composition formula (1).

[0197] In the preparation of the solution containing the precursor of the first solid electrolyte, it is preferred to use a zirconium compound such that the zirconium content in the solution is equal to the stoichiometric composition of the composition formula (1).

[0198] As the lithium source, lanthanum source and zirconium source contained in the solution of the precursor containing the first solid electrolyte, for example, the lithium compounds, lanthanum compounds and zirconium compounds exemplified as components contained in the solution of the precursor containing the second solid electrolyte in [2-1] above can be used, preferably under the same conditions as those described in [2-1] above.

[0199] In addition, as a gallium compound of a metal compound serving as a gallium source, for example, a gallium metal salt, a gallium alkoxide, etc. can be listed, and one of them or two or more thereof can be used in combination. As a gallium metal salt, for example, gallium bromide, gallium chloride, gallium iodide, gallium nitrate, etc. can be listed. As a gallium alkoxide, for example, trimethoxygallium, triethoxygallium, tri-n-propoxygallium, tri-isopropoxygallium, tri-n-butoxygallium, etc. can be listed. Among them, as a gallium compound, gallium nitrate is preferred. As a gallium source, a hydrate can also be used.

[0200] In addition, as the calcium compound of the metal compound as the calcium source, for example, calcium metal salts, calcium alkoxides, etc. can be listed, and one of them or two or more thereof can be used in combination. As the calcium metal salt, for example, calcium bromide, calcium chloride, calcium fluoride, calcium iodide, calcium oxalate, calcium acetate, calcium nitrate, etc. can be listed. In addition, as the calcium alkoxide, for example, dimethoxy calcium, diethoxy calcium, diisopropoxy calcium, di-n-propoxy calcium, diisobutoxy calcium, di-n-butoxy calcium, di-sec-butoxy calcium, etc. can be listed. Among them, as the calcium compound, calcium nitrate is preferred. As the calcium source, hydrates can also be used.

[0201] In addition, the solution containing the precursor of the first solid electrolyte described above preferably contains oxyanions.

[0202] Thus, the first solid electrolyte can be properly formed in the subsequent heat treatment, especially the heat treatment under relatively mild conditions. In addition, the first electrolyte part P11 composed of the first solid electrolyte and the second electrolyte part P12 composed of the second solid electrolyte formed in this way have excellent adhesion. As a result, the reliability of the composite body P100 finally obtained can be made more excellent.

[0203] In this process, when a solution containing the precursor of the above-mentioned first solid electrolyte is prepared into a solution containing oxygen-containing anions, it is preferred to use metal salts containing oxygen-containing anions as the various metal compounds used as raw materials for forming the above-mentioned first solid electrolyte, but in the preparation of the solution containing the precursor of the above-mentioned first solid electrolyte, as a component different from the various metal compounds, oxygen-containing acid compounds that do not contain metal elements but contain oxygen-containing anions can also be used.

[0204] Examples of the oxyanion include the anions listed in the above-mentioned [2-1].

[0205] In addition, the oxoacid compound can be added, for example, after this step, during the heat treatment described later, or at a certain time during the heat treatment.

[0206] The solvent and the dispersion medium constituting the solution of the precursor containing the first solid electrolyte are not particularly limited, and examples thereof include the solvents and dispersion medium exemplified in [2-1] above. Among them, at least one of 2-n-butoxyethanol and ethanol is preferred as the solvent and the dispersion medium.

[0207] [2-4] Second heat treatment step

[0208] In this embodiment, before the third electrolyte part forming step described later, the active material P10 having undergone the first precursor contact step, that is, the active material P10 to which the second precursor oxide and the precursor of the first solid electrolyte are attached, is heated.

[0209] Thus, for example, the solvent and dispersion medium contained in the solution containing the precursor of the above-mentioned first solid electrolyte can be appropriately removed, and at least a part of the precursor of the first solid electrolyte can be converted into a metal oxide such as the first solid electrolyte. In particular, when the solution containing the precursor of the above-mentioned first solid electrolyte contains oxygen-containing anions, an oxide different from the first solid electrolyte can be appropriately formed in this process. Hereinafter, the oxide is also referred to as the "first precursor oxide". As a result, for example, the second precursor oxide on the active material P10 or the precursor of the first solid electrolyte attached to the second solid electrolyte or the first solid electrolyte can be effectively prevented from accidentally peeling off in the subsequent process. In addition, the first electrolyte part P11 composed of the first solid electrolyte in the composite P100 can have better adhesion with respect to the second electrolyte part P12 or the third electrolyte part P13. As a result, the reliability of the composite P100 obtained in the end can be made better.

[0210] In the following description, the case where the solution containing the precursor of the above-mentioned first solid electrolyte contains oxyanions and the first precursor oxide is formed in this step will be mainly described.

[0211] The heating in this step is preferably performed under the condition that the content rate of the liquid component contained in the solution containing the precursor of the first solid electrolyte is sufficiently low.

[0212] More specifically, the content of the liquid component contained in the solid composition obtained in this step, that is, the content of the above-mentioned solvent and dispersion medium is preferably 1.0 mass % or less, and more preferably 0.1 mass % or less.

[0213] The heat treatment in this step may be performed under constant conditions or may be performed by combining different conditions.

[0214] For example, a heat treatment A mainly for removing the aforementioned solvent and dispersion medium and a heat treatment B mainly for reacting the precursors of the first solid electrolyte, namely the aforementioned lithium compound, gallium compound, lanthanum compound, calcium compound and zirconium compound, may be performed in combination.

[0215] In this case, for example, the portion corresponding to the solution containing the precursor of the first solid electrolyte provided in the first precursor contact step can be made of a gelled composition by heat treatment A, and can be made into a state containing almost no liquid component as described above by subsequent heat treatment B. In particular, when the solution containing the precursor of the first solid electrolyte contains oxygen-containing anions, heat treatment B can efficiently form the first precursor oxide.

[0216] The conditions of heat treatment A also depend on the boiling point or vapor pressure of the solvent or dispersion medium, but the heating temperature in heat treatment A is preferably 50°C to 250°C, more preferably 60°C to 230°C, and further preferably 80°C to 200°C.

[0217] The heating time in the heat treatment A is preferably 10 minutes to 180 minutes, more preferably 20 minutes to 120 minutes, and even more preferably 30 minutes to 60 minutes.

[0218] Heat treatment A can be carried out in any atmosphere, can be carried out in an oxidizing atmosphere such as air or oxygen atmosphere, can also be carried out in a non-oxidizing atmosphere such as an inert gas such as nitrogen, helium, argon, etc. In addition, heat treatment A can also be carried out under reduced pressure or vacuum, under pressure.

[0219] In the heat treatment A, the atmosphere may be maintained at substantially the same conditions or may be changed to different conditions.

[0220] The conditions of heat treatment B also depend on the composition of the first precursor oxide to be formed, but the heating temperature in heat treatment B is preferably 400°C to 600°C, more preferably 430°C to 600°C, and further preferably 450°C to 600°C.

[0221] The heating time in the heat treatment B is preferably 5 minutes to 180 minutes, more preferably 10 minutes to 120 minutes, and even more preferably 15 minutes to 120 minutes.

[0222] Heat treatment B can be carried out in any atmosphere, can be carried out in oxidizing atmospheres such as air or oxygen atmosphere, can also be carried out in non-oxidizing atmospheres such as inert gases such as nitrogen, helium, argon. In addition, heat treatment B can also be carried out under reduced pressure or vacuum, under pressure. Especially, heat treatment B is preferably carried out in an oxidizing atmosphere.

[0223] It should be noted that the heat treatment A and the heat treatment B may be performed continuously. For example, in the heat treatment A, the temperature may be increased at a constant temperature increase rate without setting a time for maintaining the temperature within a predetermined range.

[0224] In the case where the solid composition obtained in this step contains a first precursor oxide, the first precursor oxide preferably has a crystalline structure different from the crystalline structure of the first solid electrolyte. In the present invention, regarding the crystalline structure, "different" means a broad concept including the same type but at least one lattice constant being different, in addition to different types of crystalline structures.

[0225] In particular, the first solid electrolyte is composed of a solid electrolyte having a cubic garnet-type crystal structure, whereas the crystal structure of the first precursor oxide is preferably a tetragonal garnet-type crystal structure or a pyrochlore oxide structure.

[0226] Therefore, by relaxing the conditions of the heating treatment after this step, for example, even at a lower temperature and a shorter time, it is possible to appropriately form the first electrolyte part P11 composed of a solid electrolyte that has excellent adhesion with the second electrolyte part P12 or the third electrolyte part P13 and particularly excellent properties such as ion conductivity.

[0227] It should be noted that the crystal structure of the first precursor oxide may also be the above-mentioned tetragonal garnet-type crystal structure, or a crystal structure other than the pyrochlore oxide structure, such as cubic crystals such as perovskite structure, rock salt structure, diamond structure, fluorite structure, spinel structure, orthorhombic crystals such as orthorhombic crystals such as ramsbillite type, and trigonal crystals such as corundum type.

[0228] The crystal grain size of the first precursor oxide is not particularly limited, but is preferably 10 nm to 200 nm, more preferably 15 nm to 180 nm, and further preferably 20 nm to 160 nm.

[0229] Thus, the melting point of the first precursor oxide can be further reduced by the phenomenon of melting point reduction accompanied by the increase of surface energy, i.e., the so-called Gibbs-Thomson effect, and the conditions for the heat treatment after this step can be further relaxed. In addition, the adhesion between the second electrolyte part P12 and the first electrolyte part P11, and the adhesion between the first electrolyte part P11 and the third electrolyte part P13 in the finally obtained composite P100 can be made more excellent.

[0230] The first precursor oxide is preferably composed substantially of a single crystalline structure.

[0231] Therefore, in the heat treatment after this process, the crystal phase transition that occurs when forming a solid electrolyte having a cubic garnet-type crystal structure essentially becomes one, thereby suppressing the formation of included crystals caused by segregation or thermal decomposition of elements accompanying the crystal phase transition, thereby further improving various properties of the first solid electrolyte.

[0232] [2-5] Third Heat Treatment Step

[0233] In this embodiment, the active material P10 that has undergone the first precursor contact step is heated before the third electrolyte part forming step described later. In particular, the active material P10 that has undergone the first precursor contact step and the second heat treatment step is heated.

[0234] Thus, the second precursor oxide becomes the second solid electrolyte to form the second electrolyte portion P12 , and the first precursor oxide becomes the first solid electrolyte to form the first electrolyte portion P11 .

[0235] Furthermore, even when a raw material containing oxyanions is used in the production of the composite P100, the oxyanions can generally be sufficiently removed in this step, and the content of oxyanions contained in the composite P100 finally obtained can be sufficiently low. As a result, the reliability of the composite P100 can be made even better.

[0236] This step is generally performed at a higher temperature than the heat treatment in the first heat treatment step or the second heat treatment step.

[0237] The heating temperature in this step is, for example, preferably 700°C or higher and 1000°C or lower, more preferably 730°C or higher and 980°C or lower, and further preferably 750°C or higher and 900°C or lower.

[0238] Therefore, by heat treatment at a relatively low temperature and in a relatively short time, the second solid electrolyte and the first solid electrolyte can be efficiently formed. In addition, the close adhesion between the active material P10 and the second electrolyte part P12, and the close adhesion between the second electrolyte part P12 and the first electrolyte part P11 can be made better, and the lithium ion conductivity of the composite P100 can be made higher.

[0239] In the third heat treatment process, the heating temperature may also be changed. For example, the third heat treatment process may also include a first stage in which the heat treatment is performed at a relatively low temperature, and a second stage in which the heat treatment is performed at a relatively high temperature after the first stage. In such a case, the highest temperature in the third heat treatment process is preferably included in the aforementioned range.

[0240] The heating time in the third heat treatment step is not particularly limited, but is preferably 2 hours to 15 hours, more preferably 4 hours to 12 hours, and even more preferably 4 hours to 10 hours.

[0241] Thereby, the aforementioned effects can be more significantly exerted.

[0242] The third heat treatment step can be carried out in any atmosphere, can be carried out in an oxidizing atmosphere such as air or an oxygen atmosphere, can also be carried out in a non-oxidizing atmosphere such as an inert gas such as nitrogen, helium, argon, etc. In addition, the third heat treatment step can also be carried out under reduced pressure or vacuum, under pressure.

[0243] In addition, in the third heat treatment step, the atmosphere may be maintained at substantially the same conditions or may be changed to different conditions.

[0244] [2-6] Third Electrolyte Part Forming Step

[0245] In the third electrolyte portion forming step, the active material P10 that has undergone the second precursor contact step and the first precursor contact step is brought into contact with the third solid electrolyte to form the third electrolyte portion P13.

[0246] In this way, the composite P100 can be obtained.

[0247] As a method for forming the third electrolyte part P13, for example, there can be listed a method of supplying a molten solution of a third solid electrolyte to the active material P10 that has undergone the second precursor contact step and the first precursor contact step, a method of melting the third solid electrolyte while the solid third solid electrolyte is in contact with the active material P10 that has undergone the second precursor contact step and the first precursor contact step, and the like.

[0248] When forming the third electrolyte portion P13 in this step, the third solid electrolyte is usually heated to a temperature equal to or higher than its melting point.

[0249] The heating temperature in this step varies depending on the composition of the third solid electrolyte, etc. When the melting point of the third solid electrolyte is set to Tm [°C], it is preferably above (Tm+5)°C and below (Tm+150)°C, more preferably above (Tm+10)°C and below (Tm+100)°C, and further preferably above (Tm+15)°C and below (Tm+80)°C.

[0250] Even if the composite P100 obtained as described above is a composite produced using a raw material containing oxyanions, the oxyanions can usually be sufficiently removed in the third heat treatment step, so the content of oxyanions contained in the composite P100 finally obtained is sufficiently low. More specifically, the content of oxyanions in the composite P100 is usually 100 ppm or less, particularly preferably 50 ppm or less, and more preferably 10 ppm or less.

[0251] [3]Battery

[0252] Next, the battery of the present invention will be described.

[0253] The battery of the present invention comprises the above-described composite of the present invention, an electrode provided on one surface side of the composite, and a current collector provided on the other surface side of the composite.

[0254] Thus, a battery can be provided, which has sufficiently excellent adhesion between the solid electrolyte and the active material, and the adhesion between the solid electrolytes, can suppress the increase in grain boundary resistance and the decrease in lithium ion conductivity, and the discharge capacity is unlikely to decrease, and in particular, the discharge capacity can be appropriately maintained even under repeated charge and discharge.

[0255] Hereinafter, the specific structure of the lithium ion secondary battery as the battery of the present invention will be described.

[0256] Figure 2 2 is a schematic cross-sectional view schematically showing the structure of a lithium-ion secondary battery. In particular, Figure 2 A coin-type battery is shown as an example of a lithium-ion secondary battery.

[0257] in particular, Figure 2 The lithium ion battery 100 shown has the above-mentioned composite P100, the negative electrode 30 as the electrode provided in contact with one surface of the composite P100, and the current collector 41 provided in contact with the surface of the composite P100 opposite to the surface in contact with the negative electrode 30. Figure 2The lithium ion battery 100 shown has a current collector 42 provided in contact with the surface of the negative electrode 30 opposite to the surface in contact with the composite P100. That is, the lithium ion battery 100 of this embodiment has a structure in which the current collector 41, the composite P100, the negative electrode 30, and the current collector 42 are stacked in this order.

[0258] The shape of the lithium ion battery 100 is not particularly limited, and may be, for example, a polygonal disk, etc., but in the illustrated structure, it is a disk. The size of the lithium ion battery 100 is not particularly limited, and for example, the diameter of the lithium ion battery 100 is, for example, greater than 10 mm and less than 20 mm, and the thickness of the lithium ion battery 100 is, for example, greater than 0.1 mm and less than 1.0 mm.

[0259] Thus, if the lithium ion battery 100 is small and thin, it can be charged and discharged and is all solid, so it can be appropriately used as a power source for portable information terminals such as smartphones. It should be noted that, as described later, the lithium ion battery 100 can also be a battery for purposes other than the power source of portable information terminals.

[0260] [3-1] Complex

[0261] As described above, the composite P100 constituting the lithium ion battery 100 includes an active material P10, a first electrolyte portion P11, and a second electrolyte portion P12. At least a portion of the first electrolyte portion P11 is bonded to the active material P10 via the second electrolyte portion P12. In particular, the active material P10 contains a positive electrode active material.

[0262] In the composite P100, the active material P10 may be unevenly distributed on one surface side. In this case, the composite P100 is preferably in contact with the negative electrode 30 on the surface opposite to the side on which the active material P10 is unevenly distributed. When the active material P10 is unevenly distributed on one surface side of the composite P100, the first electrolyte portion P11 or the third electrolyte portion P13 may be unevenly distributed on the other surface side.

[0263] The thickness of the composite P100 constituting the lithium ion battery 100 is not particularly limited, but is preferably 0.1 μm or more and 500 μm or less, and more preferably 0.3 μm or more and 100 μm or less.

[0264] [3-2] Negative electrode

[0265] The negative electrode 30 may be any material as long as it is composed of a so-called negative electrode active material that repeatedly electrochemically inserts and extracts lithium ions at a lower potential than the positive electrode active material constituting the composite P100.

[0266] The negative electrode 30 is composed of a material containing a negative electrode active material.

[0267] Examples of negative electrode active materials include Nb2O5, V2O5, TiO2, In2O3, ZnO, SnO2, NiO, ITO, AZO, GZO, ATO, FTO, Li4Ti5O 12 , Li2Ti3O7 and other lithium composite oxides. In addition, for example, metals such as Li, Al, Si, Si-Mn, Si-Co, Si-Ni, Sn, Zn, Sb, Bi, In, Au, and alloys, carbon materials, LiC 24 , LiC6, etc., in which lithium ions are inserted between the layers of carbon materials.

[0268] In particular, the negative electrode 30 is preferably composed of metal Li.

[0269] As a result, the effect of storing about 10 times more electricity per unit weight and several times more electricity per unit volume can be achieved compared to the carbon negative electrode widely used in lithium ion batteries.

[0270] In addition, the negative electrode active material may form a covering layer on the surface for the purpose of reducing the interface resistance with the solid electrolyte or improving the electronic conductivity, etc. The thickness of the covering layer is not particularly limited, but is preferably 3 nm or more and 1 μm or less.

[0271] The average particle size of the negative electrode active material is not particularly limited, but is preferably 0.1 μm or more and 150 μm or less, and more preferably 0.3 μm or more and 60 μm or less.

[0272] This makes it easy to achieve both an actual capacity density close to the theoretical capacity of the active material and a high charge and discharge rate.

[0273] The thickness of the negative electrode 30 is not particularly limited, but is preferably 0.1 μm or more and 500 μm or less, and more preferably 0.3 μm or more and 100 μm or less.

[0274] As a method for forming the negative electrode 30, for example, there can be cited a vacuum evaporation method, a sputtering method, a CVD method (chemical vapor deposition method), a PLD method (pulsed laser deposition method), an ALD method (atomic layer deposition method), a vapor deposition method such as an aerosol deposition method, a chemical deposition method using a solution such as a sol-gel method or a MOD method (model deposition method), etc. In addition, for example, the particles of the negative electrode active material can also be slurried together with an appropriate binder, and a coating film can be formed by scraper or screen printing, and the coating film can be dried and fired to be sintered on the surface of the composite P100.

[0275] [3-3] Current Collector

[0276] The current collectors 41 and 42 are conductors that are responsible for transmitting and receiving electrons to the composite P100 as the positive electrode or the negative electrode 30. The current collectors 41 and 42 are generally made of a material having sufficiently low resistance and whose conductive properties or mechanical structure do not substantially change due to charge and discharge.

[0277] Examples of the constituent materials of the current collectors 41 and 42 include a metal selected from the group consisting of Cu, Mg, Ti, Fe, Co, Ni, Zn, Al, Ge, In, Au, Pt, Ag and Pd, and an alloy containing two or more metals selected from the group.

[0278] In particular, Cu is preferably used as a constituent material of the current collectors 41 and 42 .

[0279] The current collectors 41 and 42 are usually provided so as to reduce the contact resistance with the composite P100 and the negative electrode 30. Examples of the shape of the current collectors 41 and 42 include a plate shape and a mesh shape.

[0280] The thickness of the current collectors 41 and 42 is not particularly limited, but is preferably 7 μm or more and 85 μm or less, and more preferably 10 μm or more and 60 μm or less.

[0281] It should be noted that the lithium-ion battery 100 does not necessarily have a pair of collectors 41 and 42. It only needs to have a collector 41 arranged on at least one surface of the composite P100, that is, on the side opposite to the surface on which the negative electrode 30 serving as the electrode is arranged, and does not need to have a collector 42.

[0282] For example, when a plurality of lithium ion batteries 100 are stacked and used so as to be electrically connected in series, the lithium ion battery 100 may be configured to include only the current collector 41 of the pair of current collectors 41 and 42 .

[0283] [4] Electronic equipment

[0284] Next, the electronic device of the present invention will be described.

[0285] The electronic device of the present invention includes the above-mentioned battery of the present invention.

[0286] This makes it possible to provide an electronic device including a battery whose discharge capacity is unlikely to decrease and which can appropriately maintain the discharge capacity even when repeatedly charged and discharged.

[0287] As electronic equipment, for example, personal computers, digital cameras, mobile phones, smart phones, music players, tablet terminals, clocks, smart watches, inkjet printers and other printers, televisions, projectors, head-up displays, wireless headsets, wireless headphones, smart glasses, head-mounted displays and other wearable devices, cameras, tape recorders, car navigation devices, driving recorders, pagers, electronic notebooks, electronic dictionaries, electronic translators, calculators, video game consoles, toys, word processors, workstations, robotic arms, video phones, anti-crime image monitors, electronic binoculars, POS terminals, medical equipment, fish finders, various measuring equipment, mobile terminal base station equipment, vehicles, railway vehicles, aircraft, helicopters, ships and other various measuring instruments, flight simulators, network servers, etc. In addition, lithium ion battery 100, for example, can also be applied to mobile bodies such as cars or ships. More specifically, for example, it can be appropriately applied to batteries for electric vehicles, plug-in hybrid vehicles, hybrid vehicles, fuel cell vehicles, etc. In addition, for example, it can also be applied to batteries for household power supplies, industrial power supplies, and solar power generation.

[0288] In the following, a wearable device is taken as a specific example of the electronic device of the present invention.

[0289] Figure 3 It is a three-dimensional diagram showing the structure of a wearable device as an electronic device.

[0290] like Figure 3 As shown, the wearable device 300 as an electronic device is an information device that is worn on a human body, such as a wrist WR, like a watch and can obtain information related to the human body. It includes a band 301, a sensor 302, a display unit 303, a processing unit 304 and a lithium ion battery 100.

[0291] The band 301 is in the form of a band made of a flexible resin such as rubber, and has a coupling portion at the end of the band whose coupling position can be adjusted so that the band can fit closely to the wrist WR when worn.

[0292] The sensor 302 is, for example, an optical sensor, and is disposed on the inner surface side of the band 301 , that is, on the wrist WR side, so as to contact the wrist WR when the band 301 is worn.

[0293] The display unit 303 is, for example, a light-receiving liquid crystal display device, and is disposed on the outer surface side of the belt 301 , that is, on the side opposite to the inner surface on which the sensor 302 is mounted, so that the wearer can read the information displayed on the display unit 303 .

[0294] The processing unit 304 is, for example, an integrated circuit, which is built into the belt 301 and electrically connected to the sensor 302 or the display unit 303. The processing unit 304 performs calculations for measuring pulse or blood sugar level based on the output from the sensor 302. In addition, the display unit 303 is controlled to display the measurement results.

[0295] The lithium ion battery 100 is built in the belt 301 in a detachable state as a power supply source for supplying power to the sensor 302 , the display unit 303 , the processing unit 304 , and the like.

[0296] According to the wearable device 300 of this embodiment, it is possible to electrically detect information related to the pulse or blood sugar level of the wearer from the wrist WR through the sensor 302, and display the pulse or blood sugar level on the display unit 303 after calculation processing in the processing unit 304. The display unit 303 can display not only the measurement results but also information indicating the human body condition or time predicted based on the measurement results.

[0297] In addition, since a small lithium ion battery 100 having excellent charge and discharge characteristics is used as the lithium ion battery 100, a lightweight and thin wearable device 300 that can withstand repeated use for a long time can be provided. In addition, since the lithium ion battery 100 is a solid secondary battery, it can be repeatedly used by charging, and there is no worry about leakage of electrolyte, etc., so a wearable device 300 that can be used safely for a long time can be provided.

[0298] In this embodiment, a watch-type wearable device 300 is exemplified, but the wearable device 300 may be worn on an ankle, head, ear, waist, or the like, for example.

[0299] As mentioned above, although the preferred embodiment of the present invention was described, the present invention is not limited thereto.

[0300] For example, in the above-mentioned embodiments, the description is mainly focused on the case where the composite has a third electrolyte portion in addition to the active material, the first electrolyte portion, and the second electrolyte portion, but the composite of the present invention may not have a third electrolyte portion.

[0301] In addition, the composite of the present invention can be produced by any method, and is not limited to the above-mentioned method.

[0302] More specifically, in the aforementioned embodiment, the case of performing three heat treatment processes, namely the first heat treatment process, the second heat treatment process and the third heat treatment process, is described, but the number of heat treatment processes is not limited thereto, and the number of heat treatment processes may also be reduced. In addition, the timing of performing the heat treatment process is also not limited to the timing described in the aforementioned embodiment.

[0303] Furthermore, in the above-mentioned embodiment, the case where the molten solution of the third solid electrolyte is used to form the third electrolyte portion is described, but the third electrolyte portion may be formed using a precursor of the third solid electrolyte.

[0304] Furthermore, the composite of the present invention can also be produced by a method having other steps in addition to the above-mentioned steps.

[0305] In addition, the battery of the present invention is not limited to the battery of the above-mentioned embodiment.

[0306] For example, in the battery of the aforementioned embodiment, the composite contains a positive electrode active material and has a negative electrode as the electrode, but it may be that in the battery of the present invention, the composite contains a negative electrode active material and has a positive electrode as the electrode. In addition, it may be that the battery of the present invention is composed of two composites, one composite contains a positive electrode active material, and the other composite contains a negative electrode active material.

[0307] Furthermore, in the above-mentioned embodiment, a coin-shaped battery is described as a representative example, but the battery of the present invention may have a shape other than the coin shape.

[0308] Example

[0309] Next, specific examples of the present invention will be described.

[0310] [5] Fabrication of composites

[0311] [5-1] Preparation of Metal Compound Solution for Production of Solid Electrolyte

[0312] First, a solution of a metal compound used for manufacturing a solid electrolyte, in particular, manufacturing a first solid electrolyte and a second solid electrolyte, was prepared as follows.

[0313] [5-1-1] Preparation of lithium nitrate solution in 2-n-butoxyethanol

[0314] 1.3789 g of 3N5 lithium nitrate and 18.6211 g of 2-n-butoxyethanol (ethylene glycol monobutyl ether) manufactured by Kanto Chemical Co., Ltd. were weighed into a reagent bottle made of 30 g of Pyrex (Pyrex: trademark of CORNING Co., Ltd. Pyrex and Pyrex are registered trademarks) with a magnetic stirring head added. Then, the reagent bottle was placed on a hot plate with a magnetic stirrer function, and the lithium nitrate was completely dissolved in the 2-n-butoxyethanol while stirring at 170°C for 1 hour, and then slowly cooled to room temperature to obtain a 1 mol / kg lithium nitrate 2-n-butoxyethanol solution.

[0315] [5-1-2] Preparation of lanthanum nitrate solution in 2-n-butoxyethanol

[0316] 8.6608 g of 4N lanthanum nitrate hexahydrate manufactured by Kanto Chemical Co., Ltd. and 11.3392 g of deer-grade 2-n-butoxyethanol manufactured by Kanto Chemical Co., Ltd. were weighed into a reagent bottle made of 30 g of Pyrex (Pyrex: trademark of CORNING Co., Ltd. Pyrex and Pyrex are registered trademarks) with a magnetic stirring head added. Next, the reagent bottle was placed on a hot plate with a magnetic stirrer function, and the lanthanum nitrate hexahydrate was completely dissolved in the 2-n-butoxyethanol while stirring at 140° C. for 30 minutes, and then slowly cooled to room temperature to obtain a 1 mol / kg concentration of lanthanum nitrate in 2-n-butoxyethanol solution.

[0317] [5-1-3] Preparation of tetra-n-butoxyzirconium solution in 2-n-butoxyethanol

[0318] 3.8368 g of tetra-n-butoxyzirconium produced by Kojun Chemical Research Institute and 6.1632 g of deer-grade 2-n-butoxyethanol produced by Kanto Chemical Co., Ltd. were weighed into a reagent bottle made of 20 g of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks) to which a magnetic stirring head was added. Then, the reagent bottle was placed on a hot plate with a magnetic stirrer function and stirred at room temperature for 30 minutes while the tetra-n-butoxyzirconium was completely dissolved in the 2-n-butoxyethanol to obtain a 1 mol / kg concentration of tetra-n-butoxyzirconium 2-n-butoxyethanol solution.

[0319] [5-1-4] Preparation of Gallium Nitrate Ethanol Solution

[0320] 3.5470 g of gallium nitrate n-hydrate (n=5.5) manufactured by Kojun Chemical Research Institute Co., Ltd. and 6.4530 g of ethanol that had been previously dehydrated were weighed into a reagent bottle made of 20 g of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks) with a magnetic stirring head added. Next, the reagent bottle was placed on a hot plate with a magnetic stirrer function, and the gallium nitrate n-hydrate (n=5.5) was completely dissolved in the ethanol while stirring at 90°C for 1 hour, and then slowly cooled to room temperature to obtain an ethanol solution of gallium nitrate with a concentration of 1 mol / kg. It should be noted that the hydration number n of the gallium nitrate n-hydrate used was 5.5 based on the results of the mass reduction in the combustion experiment (differential thermal analysis).

[0321] [5-1-5] Preparation of Calcium Nitrate Solution in 2-n-Butoxyethanol

[0322] 2.3600 g of calcium nitrate tetrahydrate from Kanto Chemical Co., Ltd. and 7.6400 g of 2-n-butoxyethanol that had been dehydrated in advance were weighed into a reagent bottle made of 20 g of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks) with a magnetic stirring head added. Next, the reagent bottle was placed on a hot plate with a magnetic stirrer function, and the calcium nitrate tetrahydrate was completely dissolved in the 2-n-butoxyethanol while stirring at 100°C for 30 minutes, and then slowly cooled to room temperature to obtain a 1 mol / kg concentration of calcium nitrate in 2-n-butoxyethanol solution.

[0323] [5-1-6] Preparation of 2-n-butoxyethanol solution of penta-n-butoxyniobium

[0324] 4.5848 g of penta-n-butoxyniobium manufactured by Kojun Chemical Research Institute Co., Ltd. and 5.4152 g of deer-grade 2-n-butoxyethanol manufactured by Kanto Chemical Co., Ltd. were weighed into a reagent bottle made of 20 g of Pyrex (Pyrex: trademark of CORNING Co., Ltd. Pyrex and Pyrex are registered trademarks) with a magnetic stirring head added thereto. Then, the reagent bottle was placed on a hot plate with a magnetic stirring function, and the penta-n-butoxyniobium was completely dissolved in the 2-n-butoxyethanol while stirring at room temperature for 30 minutes, thereby obtaining a 2-n-butoxyethanol solution of penta-n-butoxyniobium with a concentration of 1 mol / kg.

[0325] [5-1-7] Preparation of 2-n-butoxyethanol solution of pentaethoxytantalum

[0326] 5.4640 g of pentaethoxytantalum manufactured by Kojun Chemical Research Institute and 4.5360 g of deer-grade 2-n-butoxyethanol manufactured by Kanto Chemical Co., Ltd. were weighed into a reagent bottle made of 20 g of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks) with a magnetic stirring head added thereto. Next, the reagent bottle was placed on a hot plate with a magnetic stirrer function and stirred at room temperature for 30 minutes while pentaethoxytantalum was completely dissolved in 2-n-butoxyethanol to obtain a 2-n-butoxyethanol solution of pentaethoxytantalum with a concentration of 1 mol / kg.

[0327] [5-1-8] Preparation of 2-n-butoxyethanol solution of tri-n-butoxyantimony

[0328] 3.4110 g of tri-n-butoxyantimony manufactured by Wako Pure Chemical Industries, Ltd. and 6.5890 g of deer-grade 2-n-butoxyethanol manufactured by Kanto Chemical Co., Ltd. were weighed into a reagent bottle made of 20 g of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks) to which a magnetic stirring head was added. Then, the reagent bottle was placed on a hot plate with a magnetic stirrer function and stirred at room temperature for 30 minutes while completely dissolving tri-n-butoxyantimony in 2-n-butoxyethanol to obtain a 2-n-butoxyethanol solution of tri-n-butoxyantimony with a concentration of 1 mol / kg.

[0329] [5-2] Fabrication of composites

[0330] Example A1

[0331] First, using the solution prepared in the above [5-1], a composition for forming a second solid electrolyte and a composition for forming a first solid electrolyte were prepared.

[0332] The composition for forming the second solid electrolyte is prepared by mixing the solutions prepared in [5-1-1], [5-1-2], [5-1-3], [5-1-7] and [5-1-8] above and Triton (registered trademark) X-100 (manufactured by MP Biomedicals, Inc.) as a nonionic surfactant in a prescribed ratio.

[0333] The composition for forming the first solid electrolyte is prepared by mixing the solutions prepared in [5-1-1], [5-1-2], [5-1-3], [5-1-4] and [5-1-5] above and Triton (registered trademark) X-100 (manufactured by MP Biomedicals, Inc.) as a nonionic surfactant in a prescribed ratio.

[0334] LiCoO2 particles as a positive electrode active material were placed on the hot plate via a silicon substrate. As LiCoO2 particles, particles in the shape of a rectangular parallelepiped of 10 mm×10 mm×0.1 mm were used.

[0335] Using a micropipette, 15 μL of the second solid electrolyte-forming composition was dripped onto the upper surface of the LiCoO2 particles. The second solid electrolyte-forming composition then permeated into the interior of the LiCoO2 particles by capillary action and wetted and spread throughout the particles.

[0336] Next, the temperature of the hot plate was raised to 90° C. and maintained for 15 minutes to volatilize the solvent of the second solid electrolyte-forming composition.

[0337] Then, the temperature of the hot plate was raised to 360° C. and maintained for 10 minutes to burn and decompose the organic components. By such a heat treatment, a second precursor oxide having a pyrochlore oxide crystal structure was formed.

[0338] Then, 20 μL of the composition for forming the first solid electrolyte was dripped from the upper surface of the particles of LiCoO2 provided with the second precursor oxide using a micropipette. Thus, the composition for forming the first solid electrolyte penetrated into the particles of LiCoO2 provided with the second precursor oxide by capillary action and wetted and spread in a manner that included the entire particles.

[0339] Next, the temperature of the hot plate was raised to 90° C. and maintained for 15 minutes to volatilize the solvent in the composition for forming the first solid electrolyte.

[0340] Then, the heating plate was heated to 360°C and maintained for 10 minutes to burn and decompose the organic components. Through such heat treatment, a first precursor oxide having a crystalline structure of pyrochlore oxide was formed. The dripping of the composition for forming the first solid electrolyte, the volatilization of the solvent by heating, and the combustion and decomposition of the organic components were performed 20 times in total.

[0341] Next, a sintering treatment was performed as a heating treatment at 900°C for 8 hours. As a result, the second precursor oxide became the second solid electrolyte, and the first precursor oxide became the first solid electrolyte. The second solid electrolyte had Li 6.30 Ln3Z 1.30 Sb 0.50 Ta 0.20 O 12 The first solid electrolyte has a cubic garnet crystal structure. 5.51 Ga 0.50 La 2.99 Ca 0.01 Zr2O 12 It has a cubic garnet-type crystal structure.

[0342] Next, as described above, the amorphous third solid electrolyte Li 2.2 C 0.8 B 0.2 The molten O3 solution is infiltrated into the particles of LiCoO2 formed with the second solid electrolyte and the first solid electrolyte, and then cooled to room temperature, thereby obtaining a composite. 2.2 C 0.8 B 0.2 The melting point of O 3 is 685° C., and the temperature of the melt of the third solid electrolyte during the infiltration is 725° C.

[0343] Examples A2 to A6

[0344] A composite was produced in the same manner as in Example A1 except that the composition of the second solid electrolyte-forming composition and the composition of the first solid electrolyte-forming composition were adjusted by adjusting the type and amount of the solution prepared in [5-1] above.

[0345] Example A7

[0346] The composite was produced in the same manner as in Example A3 except that the amorphous third solid electrolyte was not provided after the calcination treatment at 900°C for 8 hours. That is, the composite of this example had an active material, a first electrolyte portion, and a second electrolyte portion, but did not have a third electrolyte portion.

[0347] Example A8

[0348] First, using the solution prepared in the above [5-1], a composition for forming a second solid electrolyte and a composition for forming a first solid electrolyte were prepared.

[0349] The composition for forming the second solid electrolyte is prepared by mixing the solutions prepared in [5-1-1], [5-1-2], [5-1-3], [5-1-7] and [5-1-8] above and Triton (registered trademark) X-100 (manufactured by MP Biomedicals, Inc.) as a nonionic surfactant in a prescribed ratio.

[0350] The composition for forming the first solid electrolyte is prepared by mixing the solutions prepared in [5-1-1], [5-1-2], [5-1-3], [5-1-4] and [5-1-5] above and Triton (registered trademark) X-100 (manufactured by MP Biomedicals, Inc.) as a nonionic surfactant in a prescribed ratio.

[0351] The above-mentioned second solid electrolyte forming composition was placed in a reagent bottle made of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks), and LiCoO2 powder as a positive electrode active material was added therein. The average particle size of the LiCoO2 powder was 5.5 μm.

[0352] The reagent bottle was immersed in an ultrasonic cleaner filled with water, and ultrasonic waves were applied to disperse the LiCoO 2 powder.

[0353] Then, the excess second solid electrolyte forming composition was removed using a centrifugal separation device, and the powder of LiCoO2 with the second solid electrolyte forming composition attached to the surface was transferred to a titanium petri dish with an inner diameter of 50 mm and a depth of 20 mm, and heated on a hot plate. At this time, the solvent contained in the second solid electrolyte forming composition was volatilized by heating at 90°C for 30 minutes, and then heated at 360°C for 30 minutes to burn and decompose the organic components. Through such a heat treatment, a second precursor oxide with a crystalline structure of pyrochlore oxide was formed.

[0354] Then, the powder of LiCoO2 covered with the second precursor oxide as described above is placed in a reagent bottle made of Pyrex (Pyrex: trademark of CORNING. Pyrex and Pyrex are registered trademarks) to which the first solid electrolyte-forming composition is added.

[0355] The reagent bottle was immersed in an ultrasonic cleaner filled with water, and ultrasonic waves were applied to disperse the powder of LiCoO 2 covered with the second precursor oxide.

[0356] Then, the excess composition for forming the first solid electrolyte is removed using a centrifugal separation device, and the powder of LiCoO2 covered with the second precursor oxide and with the composition for forming the first solid electrolyte attached to the surface is transferred to a titanium petri dish with an inner diameter of 50 mm and a depth of 20 mm, and heated on a hot plate. At this time, the solvent contained in the composition for forming the first solid electrolyte is volatilized by heating at 90°C for 30 minutes, and then the organic component is burned and decomposed by heating at 360°C for 30 minutes. Through such a heat treatment, the first precursor oxide of the crystalline structure of the pyrochlore oxide is formed.

[0357] Next, using a molding die with an inner diameter of 10 mm and an exhaust port, the LiCoO2 powder covered with the second precursor oxide and the first precursor oxide was pressed at a pressure of 624 MPa for 2 minutes to obtain a disc-shaped molding with a diameter of 10 mm, an effective diameter of 8 mm, and a thickness of 150 μm.

[0358] The disc-shaped molded product thus obtained is subjected to a calcination treatment, which is a heat treatment at 900°C for 8 hours, so that the second precursor oxide becomes the second solid electrolyte and the first precursor oxide becomes the first solid electrolyte. The second solid electrolyte has Li 6.30 Ln3Z 1.30 Sb 0.50 Ta 0.20 O 12 The first solid electrolyte has a cubic garnet crystal structure. 5.51 Ga 0.50 La2.99 Ca 0.01 Zr2O 12 It has a cubic garnet-type crystal structure.

[0359] Next, as described above, the amorphous third solid electrolyte Li 2.2 C 0.8 B 0.2 The disk-shaped molded product formed with the second solid electrolyte and the first solid electrolyte is impregnated with a melt of O3 and then cooled to room temperature to obtain a composite. 2.2 C 0.8 B 0.2 The melting point of O 3 is 685° C., and the temperature of the melt of the third solid electrolyte during the infiltration is 725° C.

[0360] Embodiments A9 to A12

[0361] A composite was produced in the same manner as in Example A8 except that the composition of the second solid electrolyte-forming composition and the composition of the first solid electrolyte-forming composition were adjusted by adjusting the type and amount of the solution prepared in [5-1] above.

[0362] Embodiment A13

[0363] A composite was produced in the same manner as in Example A10 except that the amorphous third solid electrolyte was not provided after the calcination treatment at 900°C for 8 hours. That is, the composite of this example had an active material, a first electrolyte portion, and a second electrolyte portion, but did not have a third electrolyte portion.

[0364] Embodiment A14

[0365] First, using the solution prepared in the above [5-1], a composition for forming a second solid electrolyte and a composition for forming a first solid electrolyte were prepared.

[0366] The composition for forming the second solid electrolyte is prepared by mixing the solutions prepared in [5-1-1], [5-1-2], [5-1-3], [5-1-7] and [5-1-8] above and Triton (registered trademark) X-100 (manufactured by MP Biomedicals, Inc.) as a nonionic surfactant in a prescribed ratio.

[0367] The composition for forming the first solid electrolyte is prepared by mixing the solutions prepared in [5-1-1], [5-1-2], [5-1-3], [5-1-4] and [5-1-5] above and Triton (registered trademark) X-100 (manufactured by MP Biomedicals, Inc.) as a nonionic surfactant in a prescribed ratio.

[0368] A LiCoO2 sheet (manufactured by Toyoshima Seisakusho Co., Ltd., 50 mm square, 1 mm thick) was prepared as a positive electrode active material, and the above-mentioned second solid electrolyte forming composition was applied from one side thereof using a spatula. Thus, the second solid electrolyte forming composition permeated into the interior of the LiCoO2 sheet by capillary phenomenon and wetted and spread in a manner that included the entire sheet.

[0369] Next, a LiCoO2 sheet coated with the second solid electrolyte forming composition was placed on a hot plate via a silicon substrate, and the hot plate was heated to 90°C and maintained for 15 minutes to volatilize the solvent of the second solid electrolyte forming composition.

[0370] Then, the temperature of the hot plate was raised to 360° C. and maintained for 10 minutes to burn and decompose the organic components. By such a heat treatment, a second precursor oxide having a pyrochlore oxide crystal structure was formed.

[0371] Then, the first solid electrolyte forming composition is applied from one side of the LiCoO2 sheet on which the second precursor oxide is formed as described above using a scraper. Thus, the first solid electrolyte forming composition permeates into the interior of the LiCoO2 sheet by capillary action and wets and spreads in a manner that includes the entire sheet.

[0372] Next, the temperature of the hot plate was raised to 90° C. and maintained for 15 minutes to volatilize the solvent in the composition for forming the first solid electrolyte.

[0373] Then, the temperature of the hot plate was raised to 360° C. and maintained for 10 minutes to burn and decompose the organic components. Through such heat treatment, a first precursor oxide having a pyrochlore oxide crystal structure was formed.

[0374] Next, a sintering treatment was performed as a heating treatment at 900°C for 8 hours. As a result, the second precursor oxide became the second solid electrolyte, and the first precursor oxide became the first solid electrolyte. The second solid electrolyte had Li 6.30 LqCy 1.30 Sb 0.50 Ta 0.20 O 12The first solid electrolyte has a cubic garnet crystal structure. 5.51 Ga 0.50 La 2.99 Ca 0.01 Zr2O 12 It has a cubic garnet-type crystal structure.

[0375] Next, as described above, the amorphous third solid electrolyte Li 2.2 C 0.8 B 0.2 The melt of O3 is infiltrated into the LiCoO2 sheet formed with the second solid electrolyte and the first solid electrolyte, and then cooled to room temperature, thereby obtaining a composite. 2.2 C 0.8 B 0.2 The melting point of O 3 is 685° C., and the temperature of the melt of the third solid electrolyte during the infiltration is 725° C.

[0376] Embodiments A15 to A18

[0377] A composite was produced in the same manner as in Example A14 except that the composition of the second solid electrolyte forming composition and the composition of the first solid electrolyte forming composition were adjusted by adjusting the type and amount of the solution prepared in [5-1] above.

[0378] Embodiment A19

[0379] A composite was produced in the same manner as in Example A16 except that the amorphous third solid electrolyte was not provided after the calcination treatment at 900°C for 8 hours. That is, the composite of this example had an active material, a first electrolyte portion, and a second electrolyte portion, but did not have a third electrolyte portion.

[0380] Comparative Example A1

[0381] The composite was manufactured in the same manner as in Example A3 except that the step of imparting the composition for forming the second solid electrolyte to the positive electrode active material and the step of forming the second precursor oxide by heat-treating the positive electrode active material imparted with the composition for forming the second solid electrolyte were omitted. That is, the composite of this comparative example has an active material, a first electrolyte portion, and a third electrolyte portion, but does not have a second electrolyte portion.

[0382] Comparative Example A2

[0383] A composite was produced in the same manner as in Comparative Example A1 except that the amorphous third solid electrolyte was not provided after the calcination treatment at 900°C for 8 hours. That is, the composite of this Comparative Example had an active material and a first electrolyte portion, but did not have a second electrolyte portion and a third electrolyte portion.

[0384] Comparative Example A3

[0385] A composite was produced in the same manner as in Comparative Example A1 except that the composition of the first solid electrolyte-forming composition was adjusted by adjusting the type and amount of the solution prepared in [5-1] above.

[0386] Comparative Example A4

[0387] In addition to replacing Li 5.75 LqCy 0.75 Nb 0.35 Sb 0.50 Ta 0.40 O 12 A composite was produced in the same manner as in Example A4 except that a second solid electrolyte with a composition of was formed and a coating composed of LiAlO 2 was formed.

[0388] The film composed of LiAlO 2 was formed by the same method and conditions as in Example 1, except that the composition for forming LiAlO 2 was used instead of the composition for forming the second solid electrolyte.

[0389] Comparative Examples A5 to A12

[0390] A composite was produced in the same manner as in Example A1 except that the composition of the first solid electrolyte-forming composition was adjusted by adjusting the type and amount of the solution prepared in [5-1] and the heating temperature in the calcination treatment.

[0391] The conditions of the composites of the above-mentioned embodiments and comparative examples, and the heating temperature in the firing treatment, i.e., the firing temperature, are summarized as follows: Figure 4 , Figure 5 It should be noted that Figure 4 , Figure 5In the figure, LiCoO2 is represented as "LCO", and the proportion of each part constituting the composite in the composite is represented as "occupancy". In addition, the content of the solvent in the composite obtained in each of the embodiments and comparative examples is less than 0.1 mass%, and the content of oxygen-containing anions is less than 100 ppm. In addition, in each of the embodiments, the crystal grain sizes of the first precursor oxide and the second precursor oxide formed in the manufacturing process of the composite are both values ​​within the range of 20 nm to 160 nm. In addition, the composites obtained in each of the embodiments are composites in which the second electrolyte part is formed in a film-like shape on the surface of the positive electrode active material, and the average thickness of the second electrolyte part is a value within the range of 0.004 μm to 0.080 μm.

[0392] [6] Evaluation of the complex

[0393] The composites of the above-described examples and comparative examples were evaluated for lithium ion conductivity as an index of lithium ion conductivity by the following method.

[0394] That is, 8 mm φ lithium electrodes (ion activated electrodes) were made on both the front and back surfaces of the composite by lithium vapor deposition. Then, AC impedance was measured using an impedance analyzer SI1260 (Solartron). It should be noted that the AC amplitude during the measurement was 10 mV and the measurement frequency was 10 7 Hz~10 -1 Hz.

[0395] These results are summarized in Figure 6 , Figure 7 .

[0396] from Figure 6 , Figure 7 It is clear that, while excellent results were obtained in the present invention, satisfactory results were not obtained in the comparative examples.

[0397] [7] Battery manufacturing

[0398] Example B1

[0399] A lithium negative electrode was formed on one surface of the composite body produced in Example A1 by vacuum deposition. The thickness of the formed negative electrode was 20 μm.

[0400] Next, copper current collectors were formed on both surfaces of the laminate of the composite and the negative electrode by vacuum sputtering, thereby obtaining a battery. The thickness of the current collectors was 10 μm.

[0401] Embodiments B2 to B19

[0402] Batteries were produced in the same manner as in Example B1, except that the composites produced in Examples A2 to A19 were used as composites.

[0403] Comparative Examples B1 to B12

[0404] Batteries were produced in the same manner as in Example B1, except that the composites produced in Comparative Examples A1 to A12 were used as composites.

[0405] [8] Battery evaluation

[0406] The batteries of Examples B1 to B19 and Comparative Examples B1 to B12 obtained as described above were connected to a battery charge and discharge evaluation system HJ1001SD8 manufactured by Hokuto Electric Co., Ltd. immediately after production. Figure 8 , Fig. 9 The charge and discharge were repeated under the conditions shown, and the charge and discharge characteristics of the battery at the first and tenth times were evaluated.

[0407] These results are summarized together with the charge and discharge conditions. Figure 8 , Fig. 9 It should be noted that Figure 8 , Fig. 9 The “discharge capacity maintenance ratio” in refers to the ratio of the tenth discharge capacity to the first discharge capacity.

[0408] from Figure 8 , Fig. 9 It is clear that, while excellent results were obtained in the present invention, satisfactory results were not obtained in the comparative examples.

Claims

1. A composite, characterized in that: The complex comprises: Active substances; The crystalline first electrolyte portion contains a lithium composite metal oxide represented by the following composition formula (1); and The second electrolyte part contains a lithium composite metal oxide represented by the following composition formula (2), and covers at least a part of the surface of the active material. At least a portion of the first electrolyte portion is bonded to the active material via the second electrolyte portion, (Li 7-3x+y Ga x )(The 3-y Ca y )Zr2O 12 …(1), In formula (1), the relationship of 0.10≤x≤1.00 and 0.00<y≤0.30 is satisfied. <h2 style=";text-align:left;direction:ltr">Li<h2 style=";text-align:left;direction:ltr"> 7-z <h2 style=";text-align:left;direction:ltr"> La3(Zr<h2 style=";text-align:left;direction:ltr"> 2-z <h2 style=";text-align:left;direction:ltr"> M<h2 style=";text-align:left;direction:ltr"> z <h2 style=";text-align:left;direction:ltr"> )O<h2 style=";text-align:left;direction:ltr"> 12 <h2 style=";text-align:left;direction:ltr"> …(2) In formula (2), the element M is two or more elements selected from the group consisting of Nb, Ta and Sb, and satisfies the relationship of 0.00<z<2.

00.

2. The composite according to claim 1, wherein The composite further includes an amorphous third electrolyte portion containing Li and in contact with the first electrolyte portion.

3. The composite according to claim 2, wherein: The third electrolyte portion contains Li, B, and O.

4. The composite according to claim 1, wherein The active material is a positive electrode active material containing Li.

5. A battery, characterized in that: The battery has: The complex according to any one of claims 1 to 4; an electrode disposed on one side of the composite body; and The current collector is disposed on the other surface side of the composite.

6. An electronic device, characterized in that: A battery according to claim 5.