Secondary battery, electric device and method for manufacturing negative plate

By installing a multi-part colloid coating on the negative electrode sheet of the secondary battery to wrap and bind the current collecting burrs, the angular corrosion and internal short circuit caused by the burrs are solved, and the stability and voltage retention ability of the battery are improved.

CN118970228AActive Publication Date: 2024-11-15NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202411044497.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

During the battery cell preparation process, burrs are easily generated at the edge of the current collector, causing the electrode plate to conduct and the shell to cause angular corrosion, or the burrs fall between the electrode plate and the diaphragm and cause internal short circuit, resulting in abnormal voltage drop.

Method used

By providing a first colloid coating on the negative electrode sheet, the edge burrs of the negative electrode current collector are reduced, and the risk of internal short circuit is reduced. The coating includes a first part, a second part and a third part, respectively connecting different sides of the negative current collector to ensure that the burrs are effectively wrapped and fixed.

Benefits of technology

It effectively reduces the risk of burrs on the edge of the negative electrode current collector puncture of the shell and the diaphragm, reduces the possibility of internal short circuit, improves the problem of poor K value of the secondary battery, and improves the stability and energy density of the electrode assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970228A_ABST
    Figure CN118970228A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a secondary battery, electric equipment and a manufacturing method of a negative electrode plate, the secondary battery comprises the negative electrode plate, a positive electrode plate and a diaphragm, and the negative electrode plate, the positive electrode plate and the diaphragm are sequentially laminated along the thickness direction of the negative electrode plate. The negative plate comprises a negative current collector, a first negative active material layer, a second negative active material layer and a first colloid coating. The negative current collector comprises a first surface, a second surface and a third surface, the first negative active material layer is arranged on the first surface, and the second negative active material layer is arranged on the second surface; the first colloid coating comprises a first part, a second part and a third part, the first part is arranged on the first surface, the second part is arranged on the second surface, the third part is arranged on the third surface, and the third part is connected with the first part and the second part. In the secondary battery, by arranging the first colloid coating, the possibility of corner corrosion of the secondary battery can be reduced, and the problem of poor K value of the secondary battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of energy storage technology, and in particular relates to a secondary battery, an electrical device and a method for manufacturing a negative electrode sheet. Background Art

[0002] The secondary battery includes a shell and a pole piece and a diaphragm arranged in the shell. The shell usually includes two protective layers and a metal layer sandwiched between the two protective layers; the pole piece includes a positive pole piece and a negative pole piece, and the diaphragm is arranged between the positive pole piece and the negative pole piece. The pole piece includes a current collector. During the preparation of the battery cell, burrs are often generated on the edge of the current collector. The burrs can easily pierce the protective layer of the battery shell facing the pole piece, causing the pole piece to be conductive with the metal layer in the shell and causing corner corrosion. When the secondary battery vibrates, the burrs may also fall off and fall between the pole piece and the diaphragm, and then pierce the diaphragm to cause an internal short circuit, resulting in abnormal voltage drop of the secondary battery. Summary of the invention

[0003] In view of the above situation, it is necessary to provide a secondary battery, an electrical device and a method for manufacturing a negative electrode sheet, which is conducive to wrapping and restraining the edge burrs of the negative electrode current collector.

[0004] The first aspect of the embodiment of the present application provides a secondary battery, including a negative electrode sheet, a positive electrode sheet and a separator, wherein the negative electrode sheet, the separator and the positive electrode sheet are stacked in sequence in the thickness direction of the negative electrode sheet. The negative electrode sheet includes a negative electrode current collector, a first negative electrode active material layer, a second negative electrode active material layer and a first colloidal coating. The negative electrode current collector includes a first face and a second face arranged oppositely along the thickness direction of the negative electrode sheet, and the negative electrode current collector also includes a third face located at one end of the negative electrode sheet along the first direction, the first direction is perpendicular to the thickness direction of the negative electrode sheet, and the third face connects the first face and the second face; the first negative electrode active material layer is arranged on the first face, and the second negative electrode active material layer is arranged on the second face; the first colloidal coating connects the negative electrode current collector, and the first colloidal coating includes a first part, a second part and a third part, the first part connects the first face, the second part connects the second face, the third part is arranged on the third face, and the third part connects the first part and the second part. Along the thickness direction of the negative electrode sheet, the projection of the first part is located in the first face, and the projection of the second part is located in the second face.

[0005] In this secondary battery, by providing a first colloidal coating to wrap and restrain the burrs on the edge of the negative electrode current collector, at least the following two beneficial effects can be brought about: (1) wrapping the burrs on the edge of the negative electrode current collector can reduce the possibility that the burrs on the edge of the negative electrode current collector pierce the protective layer of the shell; (2) restraining the burrs on the edge of the negative electrode current collector, reducing the possibility of the burrs falling between the negative electrode sheet and the diaphragm or between the positive electrode sheet and the diaphragm, and reducing the risk of internal short circuit caused by the burrs piercing the diaphragm.

[0006] In one or more embodiments of the present application, along the thickness direction of the negative electrode sheet, at least part of the first portion is overlapped on a portion of the surface of the first negative electrode active material layer on the side away from the first surface. The first portion can restrain the first negative electrode active material layer, reduce the possibility of the active material in the first negative electrode active material layer falling off, reduce the impact of the active material falling off on the energy density, and reduce the possibility of internal short circuit of the secondary battery, and improve the poor K value problem of the secondary battery, where the K value refers to the voltage drop per unit time.

[0007] In one or more embodiments of the present application, along the thickness direction of the negative electrode sheet, at least part of the second portion is overlapped on a portion of the surface of the second negative electrode active material layer on the side away from the second surface. The second portion can restrain the second negative electrode active material layer, reduce the possibility of the active material in the second negative electrode active material layer falling off, reduce the impact of the active material falling off on the energy density, and reduce the possibility of internal short circuit of the secondary battery, thereby improving the problem of poor K value of the secondary battery.

[0008] In one or more embodiments of the present application, the negative electrode sheet, the separator and the positive electrode sheet are stacked in sequence and then wound to form a winding structure. The negative electrode sheet also includes a negative electrode ear, which is welded to the negative electrode current collector; the positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer and a positive electrode ear, the positive electrode current collector includes a fourth surface and a fifth surface arranged opposite to each other along its thickness direction, a positive electrode active material layer is arranged on the fourth surface, a positive electrode active material layer is arranged on the fifth surface, and the positive electrode ear is welded to the positive electrode current collector.

[0009] In one or more embodiments of the present application, the negative electrode sheet, the separator and the positive electrode sheet are stacked in sequence and then wound to form a winding structure. The negative electrode sheet also includes a negative electrode ear, which is integrally arranged with the negative electrode current collector. The positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer and a positive electrode ear, the positive electrode current collector includes a fourth face and a fifth face arranged oppositely along its thickness direction, a positive electrode active material layer is arranged on the fourth face, a positive electrode active material layer is arranged on the fifth face, and the positive electrode ear is integrally arranged with the positive electrode current collector.

[0010] In one or more embodiments of the present application, a plurality of negative electrode sheets, a plurality of separators, and a plurality of positive electrode sheets are stacked along the thickness direction of the negative electrode sheets to form a stacked structure, and adjacent negative electrode sheets and positive electrode sheets are separated by separators; the negative electrode sheet also includes a negative electrode ear, and the negative electrode ear is integrally arranged with the negative electrode current collector. The positive electrode sheet includes a positive electrode current collector, a positive electrode active material layer, and a positive electrode ear, and the positive electrode current collector includes a fourth face and a fifth face that are relatively arranged along the thickness direction of the positive electrode sheet, and the positive electrode active material layer is arranged on at least one of the fourth face and the fifth face, and the positive electrode ear is integrally arranged with the positive electrode current collector.

[0011] In one or more embodiments of the present application, along the first direction, the width of the negative electrode sheet is D1, and the width of the positive electrode sheet is D2, and D1>D2. Both ends of the negative electrode sheet along the first direction exceed the positive electrode sheet, which is conducive to increasing the CB (Cell Balance, the ratio of the negative electrode capacity per unit area to the positive electrode capacity per unit area) of the positive and negative electrode sheets, and is conducive to reducing the possibility of lithium deposition in the electrode assembly during the cycle. The first colloidal coating is located at the portion of the negative electrode sheet that exceeds the positive electrode sheet in the first direction, which can minimize the influence of the setting of the first colloidal coating on the overall thickness of the electrode assembly.

[0012] In one or more embodiments of the present application, the separator is bonded to the first colloidal coating, which helps to reduce the possibility of relative movement between the negative electrode sheet and the positive electrode sheet.

[0013] In one or more embodiments of the present application, the first negative electrode active material layer extends to the edge of the negative electrode current collector provided with the first colloidal coating, and along the thickness direction of the negative electrode sheet, the first part is overlapped on the partial surface of the first negative electrode active material layer on the side away from the first surface; along the first direction, the distance from the third surface to the positive electrode sheet is L1. Along the first direction, the width of the overlapping area of ​​the first part and the first negative electrode active material layer is W1, and W1 satisfies: 0.1L1≤W1≤0.5L1. W1≥0.1L1, the width of the first part covering the first negative electrode active material layer is not too small, which is conducive to reducing the possibility of the active material of the first negative electrode active material layer being separated; W1≤0.5L1, the distance between the first part and the positive electrode sheet is not too close, which is conducive to reducing the possibility of the positive electrode sheet and the first part being overlapped along the thickness direction of the negative electrode sheet, reducing the influence of the setting of the first part on the thickness of the electrode assembly, and reducing the possibility of energy density loss in the secondary battery.

[0014] In one or more embodiments of the present application, W1 satisfies: 0.2L1≤W1≤0.4L1. W1≥0.2L1 is conducive to further reducing the possibility of the active material of the first negative electrode active material layer being separated; W1≤0.4L1 is conducive to further reducing the possibility of the positive electrode sheet and the first part being overlapped along the thickness direction of the negative electrode sheet.

[0015] In one or more embodiments of the present application, the second negative electrode active material layer extends to the edge of the negative electrode current collector provided with the first colloidal coating, and along the thickness direction of the negative electrode sheet, the second part is superimposed on a portion of the surface of the second negative electrode active material layer on the side away from the first surface. Along the first direction, the distance from the third surface to the positive electrode sheet is L1. Along the first direction, the width of the superimposed region of the second part and the second negative electrode active material layer is W2, and W2 satisfies: 0.1L1≤W2≤0.5L1. W2≥0.1L1, the width of the second part covering the second negative electrode active material layer is not too small, which is conducive to reducing the possibility of the active material of the second negative electrode active material layer being separated; W2≤0.5L1, the distance between the second part and the positive electrode sheet is not too close, which is conducive to reducing the possibility of the positive electrode sheet and the second part being superimposed along the thickness direction of the negative electrode sheet, reducing the influence of the setting of the first part on the thickness of the electrode assembly, and reducing the possibility of energy density loss in the secondary battery.

[0016] In one or more embodiments of the present application, W2 satisfies: 0.2L1≤W2≤0.4L1. W2≥0.2L1 is conducive to further reducing the possibility of the active material of the first negative electrode active material layer being separated; W2≤0.4L1 is conducive to further reducing the possibility of the positive electrode sheet and the second part being overlapped along the thickness direction of the negative electrode sheet.

[0017] In one or more embodiments of the present application, the thickness of the positive electrode sheet is T. Along the thickness direction of the negative electrode sheet, the maximum distance from the surface of the first part to the first face is greater than the thickness of the first negative electrode active material layer, and the maximum distance from the surface of the first part to the surface of the first negative electrode active material layer is T1; along the thickness direction of the negative electrode sheet, the maximum distance from the surface of the second part to the second face is greater than the thickness of the second negative electrode active material layer, and the maximum distance from the surface of the second part to the surface of the second negative electrode active material layer is T2, T1+T2≤T. In a laminated electrode assembly, the first part of two adjacent negative electrode sheets is arranged opposite to the second part, while in a wound electrode assembly, the first part of the wound negative electrode sheet is arranged opposite to the second part. Setting T1+T2≤T is conducive to reducing the possibility of contact between the first part and the second part, reducing the influence of the setting of the first colloidal coating on the thickness of the electrode assembly, and reducing the possibility of loss of energy density of the secondary battery.

[0018] In one or more embodiments of the present application, T, T1 and T2 satisfy: 0.1T≤T1≤0.5T; 0.1T≤T2≤0.5T. Setting T1≥0.1T and T2≥0.1T, so that T1 and T2 are not too small, is conducive to ensuring the wrapping and restraining effect of the first colloid coating on the burrs, and setting T1≤0.5T and T2≤0.5T is conducive to reducing the influence of the setting of the first colloid coating on the thickness of the electrode assembly.

[0019] In one or more embodiments of the present application, T, T1 and T2 satisfy: 0.2T≤T1≤0.4T; 0.2T≤T2≤0.4T. Setting 0.2T≤T1 and 0.2T≤T2 is conducive to further enhancing the wrapping and restraining effect of the first colloidal coating on the burrs, and setting T1≤0.4T and T2≤0.4T is conducive to further reducing the influence of the setting of the first colloidal coating on the thickness of the electrode assembly.

[0020] In one or more embodiments of the present application, the negative electrode current collector includes a sixth surface, the third surface and the sixth surface are arranged opposite to each other along the first direction, and the sixth surface connects the first surface and the second surface. The negative electrode sheet includes a second colloidal coating, and the second colloidal coating includes a fourth part, a fifth part and a sixth part, the fourth part is arranged on part of the first surface, the fifth part is arranged on part of the second surface, the sixth part is arranged on the sixth surface, and the sixth part connects the fourth part and the fifth part. In this way, the burrs can be wrapped and bound from the opposite sides of the negative electrode sheet, which is conducive to further reducing the possibility of the burrs on the edge of the negative electrode current collector piercing the protective layer of the shell, and is also conducive to further reducing the possibility of the burrs falling between the negative electrode sheet and the diaphragm or between the positive electrode sheet and the diaphragm, reducing the risk of internal short circuit caused by the burrs piercing the diaphragm.

[0021] In one or more embodiments of the present application, the material of the first colloid coating layer includes: hot-melt resin.

[0022] In one or more embodiments of the present application, the hot melt resin is selected from at least one of ethylene-vinyl acetate copolymer and polyethylene oxide.

[0023] A second aspect of the embodiments of the present application provides an electrical device, comprising a secondary battery as described in any of the aforementioned embodiments.

[0024] A third aspect of an embodiment of the present application provides a method for manufacturing a negative electrode sheet, the method comprising the following steps:

[0025] Providing a negative electrode active material layer: coating a negative electrode active material on at least a portion of the surface of the first surface to form the first negative electrode active material layer; coating a negative electrode active material on at least a portion of the surface of the second surface to form the second negative electrode active material layer;

[0026] Setting the first colloid coating: coating a polymer material on a portion of the first surface, the third surface and a portion of the second surface to form the first colloid coating.

[0027] In one or more embodiments of the present application, the negative electrode sheet manufacturing method further includes the following steps:

[0028] A second colloidal coating is provided: the negative electrode current collector includes a sixth surface, the third surface and the sixth surface are arranged opposite to each other along the first direction, and the sixth surface connects the first surface and the second surface; a polymer material is coated on part of the first surface, the sixth surface and part of the second surface to form a second colloidal coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the overall structure of a secondary battery in one embodiment of the present application.

[0030] Figure 2 This application Figure 1 Schematic diagram of the cross-sectional structure at II in FIG.

[0031] Figure 3 yes Figure 2 Enlarged view of point A in the middle.

[0032] Figure 4 yes Figure 2 Enlarged view of point B in the middle.

[0033] Figure 5 It is a schematic diagram of the structure of a negative electrode sheet in one embodiment of the present application.

[0034] Figure 6 yes Figure 5 Cross-sectional view at CC.

[0035] Figure 7 It is a schematic diagram of the cross-sectional structure of a negative electrode sheet in one embodiment of the present application.

[0036] Figure 8 It is a schematic diagram of the overall structure of a secondary battery in one embodiment of the present application.

[0037] Fig. 9 yes Figure 8 Schematic diagram of the cross-sectional structure at point I II I in the figure.

[0038] Fig.10 It is a schematic diagram of the structure of the negative electrode sheet in an unfolded state in one embodiment of the present application.

[0039] Fig.11 It is a schematic diagram of the structure of the positive electrode sheet in an unfolded state in one embodiment of the present application.

[0040] Fig.12 It is a schematic diagram of the structure of an electrical device in an embodiment of the present application.

[0041] Main component symbols

[0042] Secondary battery 100

[0043] Housing 10

[0044] Electrode assembly 20

[0045] Negative electrode 21

[0046] Negative electrode current collector 211

[0047] First page 2111

[0048] Second side 2112

[0049] The third side

[0050] Sixth page 2114

[0051] First negative electrode active material layer 212

[0052] Second negative electrode active material layer 213

[0053] Negative ear 214

[0054] First colloid coating 215

[0055] Part 12151

[0056] Part II 2152

[0057] Part III 2153

[0058] Second colloid coating 216

[0059] Part 4 2161

[0060] Part 5 2162

[0061] Part 6 2163

[0062] Positive electrode 22

[0063] Positive electrode current collector 221

[0064] Fourth side 2211

[0065] Fifth side 2212

[0066] Positive electrode active material layer 222

[0067] Positive ear 223

[0068] Insulation layer 224

[0069] Diaphragm 23

[0070] First adapter 30

[0071] Second adapter 40

[0072] First direction X

[0073] The following specific implementation methods will further illustrate the present application in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION

[0074] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0075] It should be noted that when an element is considered to be "connected" to another element, it may be directly connected to the other element or there may be a centrally disposed element at the same time. When an element is considered to be "disposed on" another element, it may be directly disposed on the other element or there may be a centrally disposed element at the same time. The term "and / or" as used herein includes any and all combinations of one or more of the related listed items.

[0076] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0077] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0078] In the description of the embodiments of the present application, the term "perpendicular" is used to describe an ideal state between two components. In actual production or use, there may be a state that is approximately perpendicular between the two components. The two components described as "perpendicular" may not be absolutely straight lines or planes, but may be roughly straight lines or planes. From a macroscopic point of view, if the overall extension direction is a straight line or a plane, the components can be considered to be "straight lines" or "planes".

[0079] The term "parallel" is used to describe the ideal state between two parts. In actual production or use, two parts may be approximately parallel. The two parts described as "parallel" may not be absolutely straight lines or planes, but may be roughly straight lines or planes. From a macroscopic point of view, if the overall extension direction is a straight line or a plane, the parts can be considered "straight" or "plane".

[0080] Reference to "embodiment" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. The various embodiments in the present application may be combined with each other in the absence of conflict.

[0081] The embodiment of the present application provides a secondary battery, including a negative electrode sheet, a positive electrode sheet and a separator, wherein the negative electrode sheet, the separator and the positive electrode sheet are sequentially stacked in the thickness direction of the negative electrode sheet. The negative electrode sheet includes a negative electrode current collector, a first negative electrode active material layer, a second negative electrode active material layer and a first colloidal coating. The negative electrode current collector includes a first face and a second face arranged opposite to each other in the thickness direction of the negative electrode sheet, and the negative electrode current collector also includes a third face located at one end of the negative electrode sheet in the first direction, the first direction is perpendicular to the thickness direction of the negative electrode sheet, and the third face connects the first face and the second face; the first negative electrode active material layer is arranged on the first face, and the second negative electrode active material layer is arranged on the second face; the first colloidal coating connects the negative electrode current collector, and the first colloidal coating includes a first part, a second part and a third part, the first part connects the first face of the part, the second part connects the second face of the part, the third part is arranged on the third face, and the third part connects the first part and the second part; along the thickness direction of the negative electrode sheet, the projection of the first part is located in the first face, and the projection of the second part is located in the second face.

[0082] In this secondary battery, by providing a first colloidal coating to wrap and restrain the burrs on the edge of the negative electrode current collector, at least the following two beneficial effects can be brought about: (1) wrapping the burrs on the edge of the negative electrode current collector can reduce the possibility that the burrs on the edge of the negative electrode current collector pierce the protective layer of the shell; (2) restraining the burrs on the edge of the negative electrode current collector, reducing the possibility that the burrs fall between the negative electrode sheet and the diaphragm or between the positive electrode sheet and the diaphragm, and reducing the risk of internal short circuit caused by the burrs piercing the diaphragm.

[0083] The embodiments of the present application are further described below in conjunction with the accompanying drawings.

[0084] like Figure 1 and Figure 2 As shown, an embodiment of the present application provides a secondary battery 100 , including a housing 10 and an electrode assembly 20 , wherein the electrode assembly 20 is disposed in the housing 10 .

[0085] In some embodiments, Figure 2 As shown, the electrode assembly 20 includes a negative electrode sheet 21 , a positive electrode sheet 22 and a separator 23 . The negative electrode sheet 21 , the separator 23 and the positive electrode sheet 22 are stacked in sequence along the thickness direction of the negative electrode sheet 21 .

[0086] In some embodiments, the separator is an insulating film material such as a polyethylene film, a polypropylene film, a polyester film or a polyimide film, so as to isolate the positive electrode sheet 22 from the negative electrode sheet 21 .

[0087] In some embodiments, Figure 2 , Figure 5 and Figure 6 As shown, the negative electrode sheet 21 includes a negative electrode current collector 211, a first negative electrode active material layer 212 and a second negative electrode active material layer 213. The negative electrode current collector 211 includes a first surface 2111 and a second surface 2112 that are arranged opposite to each other along the thickness direction of the negative electrode sheet 21. The first negative electrode active material layer 212 is arranged on the first surface 2111, and the second negative electrode active material layer 213 is arranged on the second surface 2112.

[0088] In some embodiments, the negative electrode sheet 21 , the separator 23 , and the positive electrode sheet 22 are stacked in sequence and then wound to form a winding structure.

[0089] In some embodiments, Figure 6 As shown, for the electrode assembly 20 with a wound structure, the positive electrode sheet 22 includes a positive electrode current collector 221 and a positive electrode active material layer 222, the positive electrode current collector 221 includes a fourth surface 2211 and a fifth surface 2212 arranged relatively along the thickness direction of the positive electrode sheet 22, one positive electrode active material layer 222 is arranged on the fourth surface 2211, and one positive electrode active material layer 222 is arranged on the fifth surface 2212.

[0090] In some embodiments, Figure 1 , Figure 2 and Figure 5 As shown, for the wound electrode assembly 20 , the negative electrode sheet 21 further includes a negative electrode ear 214 , which is welded to the negative electrode collector 211 ; the positive electrode sheet 22 further includes a positive electrode ear 223 , which is welded to the positive electrode collector 221 .

[0091] In other embodiments, Fig.10 and Fig.11 As shown, for the electrode assembly 20 with a multi-electrode winding structure, the negative electrode ear 214 is integrally arranged with the negative electrode current collector 211 , and the positive electrode ear 223 is integrally arranged with the positive electrode current collector 221 . Figure 8 is a schematic diagram of the negative electrode sheet in the multi-electrode winding electrode assembly 20 in an unfolded state, Fig. 9 It is a schematic diagram of the positive electrode sheet in the multi-electrode winding electrode assembly 20 in the unfolded state.

[0092] In some embodiments, multiple negative electrode sheets 21 , multiple separators 23 and multiple positive electrode sheets 22 are stacked along the thickness direction of the negative electrode sheet 21 to form a stacked structure, and any adjacent negative electrode sheet 21 and any adjacent positive electrode sheet 22 are separated by the separator 23 .

[0093] In some embodiments, Figure 8 and Fig. 9 As shown, for the laminated electrode assembly 20, the positive electrode sheet 22 includes a positive electrode current collector 221, a positive electrode active material layer 222, and a positive electrode ear 223. The positive electrode current collector 221 includes a fourth surface 2211 and a fifth surface 2212 that are arranged opposite to each other along the thickness direction of the positive electrode sheet 22, and the positive electrode active material layer 222 is arranged on at least one of the fourth surface 2211 and the fifth surface 2212. Specifically, the laminated electrode assembly 20 includes two ends along the thickness direction of the negative electrode sheet 21. The positive electrode sheets 22 located at the two ends of the electrode assembly 20 are provided with the positive electrode active material layer 222 only on one side of the positive electrode current collector 221, and the positive electrode active material layer 222 is arranged toward the inside of the electrode assembly 20. The positive electrode sheets 22 located at the non-ends of the electrode assembly 20 are provided with the positive electrode active material layer 222 on both the fourth surface 2211 and the fifth surface 2212 of the positive electrode current collector 221.

[0094] In some embodiments, for the stacked electrode assembly 20 , the negative electrode sheet 21 further includes a negative electrode ear 214 , which is integrally arranged with the negative electrode current collector 211 , and the positive electrode sheet 22 further includes a positive electrode ear 223 , which is integrally arranged with the positive electrode current collector 221 .

[0095] In some embodiments, Fig.11 As shown, for the electrode assembly 20 with a multi-electrode winding structure, when the positive electrode ear 223 and the positive electrode current collector 221 are integrally arranged, the positive electrode sheet 22 further includes an insulating layer 224, and the insulating layer 224 is located on the side of the positive electrode active material layer 222 close to the positive electrode ear 223. The first insulating layer 224 is connected to the positive electrode active material layer 222 and extends to the edge of the positive electrode current collector 221 on the side where the positive electrode ear 223 is arranged. The provision of the insulating layer 224 can reduce the possibility of a short circuit between the positive electrode sheet 22 and the negative electrode sheet 21, which is beneficial to improving the safety of the secondary battery 100.

[0096] In some embodiments, Figure 8 and Fig. 9 As shown, for the electrode assembly 20 of the winding structure or the stacked structure, when the negative electrode ear 214 is integrally arranged with the negative electrode current collector 211, and the positive electrode ear 223 is integrally arranged with the positive electrode current collector 221, the electrode assembly 20 further includes a first adapter 30 and a second adapter 40. There are multiple negative electrode ears 214, and the multiple negative electrode ears 214 are stacked to form a negative electrode ear bundle, and the first adapter 30 is welded to the negative electrode ear bundle, and a part of the first adapter 30 is exposed to the shell 10; there are multiple positive electrode ears 223, and the multiple positive electrode ears 223 are stacked to form a positive electrode ear bundle, and the second adapter 40 is welded to the positive electrode ear bundle, and a part of the second adapter 40 is exposed to the shell 10.

[0097] In some embodiments, both the positive electrode current collector 221 and the negative electrode current collector 211 are metal layers. As an illustrative example, the positive electrode current collector 221 may be a metal layer including at least one of aluminum, nickel, tantalum, and titanium, such as aluminum foil. The negative electrode current collector 211 may be a metal layer including at least one of copper, nickel, tantalum, and titanium, such as copper foil.

[0098] In some embodiments, the positive electrode active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium manganese iron phosphate, or lithium manganese oxide.

[0099] In some embodiments, the negative electrode active material includes at least one of graphite, hard carbon, soft carbon, silicon, silicon-oxygen material, and silicon-carbon material.

[0100] In some embodiments, the negative electrode tab 214 and the positive electrode tab 223 are disposed on the same side or different sides of the electrode assembly 20 .

[0101] In some embodiments, Figure 5 and Figure 6 As shown, the negative electrode current collector 211 also includes a third surface 2113 located at one end of the negative electrode sheet 21 along the first direction X, the first direction X is perpendicular to the thickness direction of the negative electrode sheet 21, and the third surface 2113 connects the first surface 2111 and the second surface 2112. The negative electrode sheet 21 also includes a first colloidal coating 215, the first colloidal coating 215 connects the negative electrode current collector 211, and the first colloidal coating 215 includes a first portion 2151, a second portion 2152, and a third portion 2153, the first portion 2151 connects part of the first surface 2111, the second portion 2152 connects part of the second surface 2112, the third portion 2153 is disposed on the third surface 2113, and the third portion 2153 connects the first portion 2151 and the second portion 2152. Along the thickness direction of the negative electrode sheet 21, the projection of the first portion 2151 is located within the first surface 2111, and the projection of the second portion 2152 is located within the second surface 2112.

[0102] It should be noted that if Figure 3 As shown ( Figure 3The first part 2151, the second part 2152 and the third part 2153 are indicated by a dot-dash line in the figure. The first part 2151, the second part 2152 and the third part 2153 are defined as follows: along the thickness direction of the negative electrode sheet 21, when the projection of a certain part of the first colloidal coating 215 is located inside the negative electrode current collector 211, if the part is on the same side of the negative electrode current collector 211 as the first surface 2111, then the part belongs to the first part 2151; if the part is on the same side of the negative electrode current collector 211 as the second surface 2112, then the part belongs to the second part 2152; the rest is the third part 2153. In addition, the division of the first part 2151, the second part 2152 and the third part 2153 is the division of the overall structure of the first colloidal coating 215, and does not mean that the first colloidal coating 215 is formed by splicing three independent structures. In other words, the first colloidal coating 215 can be formed by assembling a plurality of components, or can be an integrated structure.

[0103] It should be added that the first portion 2151 is disposed on the first surface 2111 in any of the following cases: first, the first portion 2151 is disposed on one side of the first negative electrode active material layer 212 along the length or width direction of the negative electrode current collector 211, the first portion 2151 is in contact with or separated from the first negative electrode active material layer 212, and the surface of the first portion 2151 facing the negative electrode current collector 211 is only in contact with the first surface 2111. More generally, the first portion 2151 is in contact with the first negative electrode active material layer 212. 2; second, the first negative electrode active material layer 212 is disposed between the first portion 2151 and the first surface 2111, and the surface of the first portion 2151 facing the negative electrode current collector 211 only contacts the first negative electrode active material layer 212; third, the first negative electrode active material layer 212 is disposed between the first portion 2151 and the first surface 2111, and a portion of the surface of the first portion 2151 facing the negative electrode current collector 211 contacts the first negative electrode active material layer 212, and a portion contacts the first surface 2111.

[0104] The second portion 2152 is disposed on the second surface 2112 including the following situations: First, if Figure 7 As shown, the second portion 2152 is disposed on one side of the second negative electrode active material layer 213 along the length or width direction of the negative electrode current collector 211, the second portion 2152 is in contact with or separated from the second negative electrode active material layer 213, and the surface of the second portion 2152 facing the negative electrode current collector 211 is only in contact with the second surface 2112. More generally, the second portion 2152 is in contact with the second negative electrode active material layer 213; secondly, as Figure 4As shown, the second negative electrode active material layer 213 is arranged between the second part 2152 and the second surface 2112, and the surface of the second part 2152 facing the negative electrode current collector 211 is only in contact with the second negative electrode active material layer 213; thirdly, the second negative electrode active material layer 213 is arranged between the second part 2152 and the second surface 2112, and a part of the surface of the second part 2152 facing the negative electrode current collector 211 is in contact with the second negative electrode active material layer 213, and a part of it is in contact with the second surface 2112.

[0105] In this secondary battery 100, by providing the first colloidal coating 215 to wrap and restrain the edge of the negative electrode current collector 211, at least the following two beneficial effects can be brought about: (1) wrapping the burrs on the edge of the negative electrode current collector 211 can reduce the possibility that the burrs on the edge of the negative electrode current collector 211 pierce the protective layer of the shell 10, thereby helping to reduce the possibility of corner corrosion of the secondary battery 100; (2) restraining the burrs on the edge of the negative electrode current collector 211, reducing the possibility of the burrs falling between the negative electrode sheet 21 and the diaphragm 23 or between the positive electrode sheet 22 and the diaphragm 23, reducing the risk of internal short circuit caused by the burrs piercing the diaphragm 23, and improving the poor K value problem of the secondary battery 100, where the K value refers to the voltage drop per unit time.

[0106] In some embodiments, Figure 6 As shown, along the thickness direction of the negative electrode sheet 21, at least part of the first portion 2151 is overlapped on a part of the surface of the first negative electrode active material layer 212 which is away from the first surface 2111. The first portion 2151 can restrain the first negative electrode active material layer 212, reduce the possibility of the active material in the first negative electrode active material layer 212 falling off, thereby reducing the possibility of the internal short circuit of the secondary battery 100, and improving the problem of poor K value of the secondary battery 100.

[0107] In some embodiments, Figure 6 As shown, along the thickness direction of the negative electrode sheet 21, at least part of the second portion 2152 is overlapped on a part of the surface of the second negative electrode active material layer 213 that is away from the second surface 2112. The second portion 2152 can restrain the second negative electrode active material layer 213, reduce the possibility of the active material in the second negative electrode active material layer 213 falling off, thereby reducing the possibility of internal short circuit of the secondary battery 100, and improving the problem of poor K value of the secondary battery 100.

[0108] In some embodiments, Fig.10As shown, the negative electrode ear 214 is integrally arranged with the negative electrode current collector 211, and the negative electrode ear 214 and the first colloidal coating 215 are arranged on the same side of the negative electrode current collector 211. The first colloidal coating 215 can wrap and restrain the burrs generated during the die-cutting process of the negative electrode ear 214, thereby reducing the possibility of the burrs piercing the protective layer of the housing 10 and the possibility of the burrs piercing the separator 23.

[0109] In some embodiments, the negative electrode tab 214 is integrally arranged with the negative electrode current collector 211, and the negative electrode tab 214 and the first colloidal coating 215 are arranged on different sides of the negative electrode current collector 211. The first colloidal coating 215 is not blocked by the negative electrode tab 214 during arrangement, which helps to reduce the difficulty of arranging the first colloidal coating 215.

[0110] In some embodiments, Figure 2 As shown, along the first direction X, the width of the negative electrode sheet 21 is D1, the width of the positive electrode sheet 22 is D2, D1>D2, the third surface 2113 is located at one end of the negative electrode sheet 21 along the first direction X, and both ends of the negative electrode sheet 21 along the first direction X exceed the positive electrode sheet 22. This is conducive to increasing the CB (Cell Balance, the ratio of the negative electrode capacity per unit area to the positive electrode capacity per unit area) of the positive and negative electrode sheets, and is conducive to reducing the possibility of lithium deposition in the electrode assembly during the cycle process.

[0111] In some embodiments, Figure 2 As shown, the first colloidal coating 215 is located at a portion of the negative electrode sheet 21 that exceeds the positive electrode sheet 22 in the first direction X. In this way, the influence of the first colloidal coating 215 on the overall thickness of the electrode assembly 20 can be minimized.

[0112] In some embodiments, Figure 2 As shown, along the first direction X, the distance from the third surface 2113 to the positive electrode sheet 22 is L1. The value of L1 is measured by the following method: the width of the negative electrode current collector 211 along the first direction X is measured by a CCD length measuring instrument, which is recorded as the first width, and the width of the positive electrode current collector 221 along the first direction X is measured by a CCD length measuring instrument, which is recorded as the second width, L1 = (first width - second width) / 2.

[0113] In some embodiments, Figure 5 and Figure 6 As shown, the first negative electrode active material layer 212 extends to the edge of the negative electrode current collector 211 provided with the first colloidal coating 215 , and along the thickness direction of the negative electrode sheet 21 , the first portion 2151 is overlapped on a portion of the surface of the first negative electrode active material layer 212 away from the first surface 2111 .

[0114] In some embodiments, Figure 5 and Figure 6As shown, along the first direction X, the width of the overlapping region of the first portion 2151 and the first negative electrode active material layer 212 is W1, and W1 satisfies: 0.1L1≤W1≤0.5L1. W1≥0.1L1, the width of the first portion 2151 covering the first negative electrode active material layer 212 is not too small, which is beneficial to reduce the possibility of the active material of the first negative electrode active material layer 212 being separated; W1≤0.5L1, the distance between the first portion 2151 and the positive electrode sheet 22 is not too close, which is beneficial to reduce the possibility of the positive electrode sheet 22 and the first portion 2151 being overlapped along the thickness direction of the negative electrode sheet 21, reduce the influence of the setting of the first portion 2151 on the thickness of the electrode assembly 20, reduce the possibility of energy density loss in the secondary battery 100, and facilitate the electrolyte to infiltrate the electrode assembly 20.

[0115] Here, the overlapping region of the first portion 2151 and the first negative active material layer 212 refers to a region where a surface of the first negative active material layer 212 facing away from the negative current collector 211 along the thickness direction of the negative electrode sheet 21 contacts the first portion 2151 .

[0116] In some embodiments, W1 satisfies: 0.2L1≤W1≤0.4L1. W1≥0.2L1 is conducive to further reducing the possibility of the active material of the first negative electrode active material layer 212 being separated; W1≤0.4L1 is conducive to further reducing the possibility of the positive electrode sheet 22 and the first part 2151 being overlapped along the thickness direction of the negative electrode sheet 21.

[0117] In some embodiments, Figure 5 and Figure 6 As shown, the second negative active material layer 213 extends to the edge of the negative current collector 211 provided with the first colloidal coating 215 , and along the thickness direction of the negative electrode sheet 21 , the second portion 2152 is stacked on a portion of the surface of the second negative active material layer 213 away from the first surface 2111 .

[0118] In some embodiments, Figure 5 and Figure 6As shown, along the first direction X, the width of the overlapping region of the second portion 2152 and the second negative electrode active material layer 213 is W2, and W2 satisfies: 0.1L1≤W2≤0.5L1. W2≥0.1L1, the width of the second portion 2152 covering the second negative electrode active material layer 213 is not too small, which is beneficial to reduce the possibility of the active material of the second negative electrode active material layer 213 being separated; W2≤0.5L1, the distance between the second portion 2152 and the positive electrode sheet 22 is not too close, which is beneficial to reduce the possibility of the positive electrode sheet 22 and the second portion 2152 being overlapped along the thickness direction of the negative electrode sheet 21, reducing the influence of the setting of the first portion 2151 on the thickness of the electrode assembly 20, and reducing the possibility of energy density loss in the secondary battery 100.

[0119] Here, the overlapping region of the second portion 2152 and the second negative electrode active material layer 213 refers to a region where the surface of the second negative electrode active material layer 213 facing away from the negative electrode current collector 211 along the thickness direction of the negative electrode sheet 21 contacts the second portion 2152 .

[0120] In some embodiments, W2 satisfies: 0.2L1≤W2≤0.4L1. W2≥0.2L1 is conducive to further reducing the possibility of the active material of the first negative electrode active material layer 212 being separated; W2≤0.4L1 is conducive to further reducing the possibility of the positive electrode sheet 22 and the second part 2152 being overlapped along the thickness direction of the negative electrode sheet 21.

[0121] In some embodiments, Figure 2 and Figure 6 As shown, the thickness of the positive electrode sheet 22 is T. Along the thickness direction of the negative electrode sheet 21, the maximum distance from the surface of the first portion 2151 to the first surface 2111 is greater than the thickness of the first negative electrode active material layer 212, and the maximum distance from the surface of the first portion 2151 to the surface of the first negative electrode active material layer 212 is T1; along the thickness direction of the negative electrode sheet 21, the maximum distance from the surface of the second portion 2152 to the second surface 2112 is greater than the thickness of the second negative electrode active material layer 213, and the maximum distance from the surface of the second portion 2152 to the surface of the second negative electrode active material layer 213 is T2, T1+T2≤T. In the laminated electrode assembly 20, the first part 2151 and the second part 2152 of two adjacent negative electrode sheets 21 are arranged opposite to each other, while in the wound electrode assembly 20, the first part 2151 and the second part 2152 of the negative electrode sheet 21 after winding exist opposite to each other. Setting T1+T2≤T is helpful to reduce the possibility of contact between the first part 2151 and the second part 2152, reduce the influence of the setting of the first colloidal coating 215 on the thickness of the electrode assembly 20, and reduce the possibility of loss of energy density of the secondary battery 100.

[0122] It should be noted that the thickness of the positive electrode sheet 22 refers to the thickness of one positive electrode current collector 221 and two positive electrode active material layers 222 .

[0123] In some embodiments, T, T1 and T2 satisfy: 0.1T≤T1≤0.5T; 0.1T≤T2≤0.5T. Setting T1≥0.1T and T2≥0.1T, so that T1 and T2 are not too small, is conducive to ensuring the wrapping and restraining effect of the first colloid coating 215 on the burrs. Setting T1≤0.5T and T2≤0.5T is conducive to reducing the influence of the setting of the first colloid coating 215 on the thickness of the electrode assembly 20, and is conducive to the electrolyte infiltration of the electrode assembly 20.

[0124] In some embodiments, T, T1, and T2 satisfy: 0.2T≤T1≤0.4T; 0.2T≤T2≤0.4T. Setting 0.2T≤T1 and 0.2T≤T2 is conducive to further enhancing the wrapping and restraining effect of the first colloid coating 215 on the burrs, and setting T1≤0.4T and T2≤0.4T is conducive to further reducing the influence of the setting of the first colloid coating 215 on the thickness of the electrode assembly 20.

[0125] In the embodiment where the negative electrode current collector 211 and the negative electrode ear 214 are integrally arranged, the first negative electrode active material layer 212 and the second negative electrode active material layer 213 both include a main region and a thinning region. The reason for forming the thinning region is that when coating the first negative electrode active material layer 212 and the second negative electrode active material layer 213, it is necessary to leave an empty foil region not covered by the first negative electrode active material layer 212 and the second negative electrode active material layer 213 in the negative electrode current collector 211. The negative electrode ear 214 is formed by die-cutting the negative electrode current collector 211 in the empty foil region. At the edge of the first negative electrode active material layer 212 and the second negative electrode active material layer 213 near the empty foil region, the negative electrode ear 214 is formed by die-cutting the negative electrode current collector 211 in the empty foil region. The negative electrode active material flows toward the empty foil area and a thinning area appears. The thickness of the first negative electrode active material layer 212 and the second negative electrode active material layer 213 in the thinning area along the thickness direction of the negative electrode sheet 21 is less than the thickness of the main area. When measuring T1, if there is a thinning area in the first negative electrode active material layer 212, T1 refers to the maximum distance from the surface of the first part 2151 to the surface of the main area of ​​the first negative electrode active material layer 212. When measuring T2, if there is a thinning area in the second negative electrode active material layer 213, T2 refers to the maximum distance from the surface of the second part 2152 to the surface of the main area of ​​the second negative electrode active material layer 213.

[0126] It should be added that Figure 7As shown, for the solution in which the first portion 2151 is not completely overlapped on the partial surface of the first negative electrode active material layer 212 which is away from the first surface 2111, T1 is still the maximum distance from the surface of the first portion 2151 to the surface of the first negative electrode active material layer 212; for the solution in which the second portion 2152 is not completely overlapped on the partial surface of the second negative electrode active material layer 213 which is away from the first surface 2111, T2 is still the maximum distance from the surface of the second portion 2152 to the surface of the second negative electrode active material layer 213.

[0127] In the aforementioned embodiment, when measuring T, a slice may be taken from the positive electrode sheet 22, and an optical microscope (OM) may be used to observe the cross section of the positive electrode sheet 22 along its thickness direction at a magnification of 5 to 25 times and measure its thickness. When measuring W1, W2, T1 and T2, a slice may be taken from the negative electrode sheet 21, and an optical microscope (OM) may be used to observe the cross section of the negative electrode sheet 21 along its thickness direction at a magnification of 5 to 25 times. Specifically, when measuring T1, a tangent is made at the first portion 2151, the tangent is perpendicular to the thickness direction of the negative electrode sheet 21, and a line is drawn between the tangent and the surface of the first negative electrode active material layer 212, the line being perpendicular to the tangent, and the length of the line is T1; when measuring T2, a tangent is made at the second portion 2152, the tangent is perpendicular to the thickness direction of the negative electrode sheet 21, and a line is drawn between the tangent and the surface of the second negative electrode active material layer 213, the line being perpendicular to the tangent, and the length of the line is T2; when measuring W1, the negative electrode current collector is used as the length of the negative electrode current collector. The distance from the end face of the body 211 to the edge of the first part 2151 on the surface of the first negative active material layer 212 is W1, and the end face of the negative current collector 211 refers to its end face on the same side as the first colloidal coating 215 in the first direction X; when measuring W2, the distance from the end face of the negative current collector 211 to the edge of the second part 2152 on the surface of the second negative active material layer 213 is W2, and the end face of the negative current collector 211 refers to its end face on the same side as the first colloidal coating 215 in the first direction X.

[0128] In some embodiments, Figure 6 and Figure 7 As shown, the negative electrode current collector 211 includes a sixth surface 2114, the third surface 2113 and the sixth surface 2114 are arranged opposite to each other along the first direction X, and the sixth surface 2114 connects the first surface 2111 and the second surface 2112. The negative electrode sheet 21 includes a second colloidal coating 216, and the second colloidal coating 216 includes a fourth portion 2161, a fifth portion 2162 and a sixth portion 2163. Figure 4The dotted lines indicate the boundaries of the fourth part 2161, the fifth part 2162 and the sixth part 2163. The fourth part 2161 is provided on part of the first surface 2111, the fifth part 2162 is provided on part of the second surface 2112, the sixth part 2163 is provided on the sixth surface 2114, and the sixth part 2163 connects the fourth part 2161 and the fifth part 2162. In this way, the burrs can be wrapped and bound from the opposite sides of the negative electrode sheet 21, which is conducive to further reducing the possibility that the burrs on the edge of the negative electrode current collector 211 pierce the protective layer of the shell 10, and is also conducive to further reducing the possibility that the burrs fall between the negative electrode sheet 21 and the separator 23 or between the positive electrode sheet 22 and the separator 23, and reducing the risk of internal short circuit caused by the burrs piercing the separator 23.

[0129] In some embodiments, the separator 23 is bonded to the first colloid coating 215 , which helps to reduce the possibility of relative movement between the negative electrode sheet 21 and the positive electrode sheet 22 .

[0130] In some embodiments, the separator 23 is also bonded to the second colloid coating 216 , which helps to further reduce the possibility of relative movement between the negative electrode sheet 21 and the positive electrode sheet 22 .

[0131] In some embodiments, the material of at least one of the first colloid coating layer 215 and the second colloid coating layer 216 includes hot melt resin.

[0132] In some embodiments, the hot melt resin is selected from at least one of ethylene-vinyl acetate copolymer and polyethylene oxide.

[0133] In some embodiments, the material of at least one of the first colloid coating 215 and the second colloid coating 216 further includes a viscosity enhancer.

[0134] In some embodiments, the tackifier is at least one of an acrylic resin, an EVA resin, and a polyurethane.

[0135] In some embodiments, the mass percentage of the hot melt resin in the first colloid coating 215 or the second colloid coating 216 is 50 wt % to 90 wt %, and the mass percentage of the tackifier in the first colloid coating 215 or the second colloid coating 216 is 10 wt % to 50 wt %.

[0136] In some embodiments, the material of at least one of the first colloid coating 215 and the second colloid coating 216 further includes a cellulose reinforcement.

[0137] like Fig.12 As shown, an embodiment of the present application further provides an electrical device, which includes a secondary battery 100 as described in any of the above embodiments.

[0138] In some embodiments, the power-consuming devices include, but are not limited to, mobile phones, watches, laptop computers, power tools, and power toys.

[0139] The embodiment of the present application also provides a method for manufacturing a negative electrode sheet 21, the method comprising the following steps:

[0140] Disposing a negative electrode active material layer: coating a negative electrode active material on at least a portion of the surface of the first surface 2111 to form a first negative electrode active material layer 212, and coating a negative electrode active material on at least a portion of the surface of the second surface 2112 to form a second negative electrode active material layer 213;

[0141] Providing the first colloid coating 215 : coating a polymer material on a portion of the first surface 2111 , the third surface 2113 , and a portion of the second surface 2112 to form the first colloid coating 215 .

[0142] In some embodiments, the method for manufacturing the negative electrode sheet 21 includes the following steps:

[0143] Welding: The negative electrode tab 214 is welded to the portion of the negative electrode current collector 211 that is not covered by the negative electrode active material layer after the segmentation. The portion that is not covered by the negative electrode active material layer may be the end portion of the negative electrode sheet 21 in the length direction, or may be the middle portion of the negative electrode sheet 21 in the length direction. If the tab is welded in the middle portion of the length direction of the negative electrode sheet 21, then after coating the negative electrode active material layer material, part of the negative electrode active material layer needs to be removed to form an empty foil area for welding the tab. The method of removing the negative electrode active material layer includes: removing by laser etching, and pasting the area where the negative electrode active material material needs to be removed with foam glue or removable glue before coating the negative electrode active material layer.

[0144] It should be noted that there is no strict time sequence requirement for the steps of setting the first colloid coating 215 and welding. The first colloid coating 215 may be set first and then welded, or welding may be performed first and then the first colloid coating 215 is set.

[0145] In some embodiments, the method for manufacturing the negative electrode sheet 21 includes the following steps:

[0146] Die cutting: the negative electrode current collector 211 has an empty foil area not covered by the first negative electrode active material layer 212 and the second negative electrode active material layer 213, and the empty foil area is die cut to form a plurality of negative electrode ears 214; the surface of the negative electrode current collector 211 located on the side where the negative electrode ear 214 is provided is the third surface 2113; or, the cut surface of the negative electrode current collector 211 formed in the splitting step on the opposite side of the negative electrode ear 214 is the third surface 2113; the first negative electrode active material layer 212 and the second negative electrode active material layer 213 both extend to the edge of the negative electrode current collector 211 on the same side as the third surface 2113.

[0147] It should be supplemented that, when the third surface 2113 is the surface of the negative electrode current collector 211 located on the side where the negative electrode ear 214 is provided, the first colloidal coating 215 needs to be set after die-cutting. When the third surface 2113 is the surface of the negative electrode current collector 211 on the opposite side of the negative electrode ear 214, there is no strict timing requirement for the step of setting the die-cutting and the step of setting the first colloidal coating 215. The first colloidal coating 215 can be set after die-cutting, or die-cutting can be performed after the first colloidal coating 215 is set.

[0148] In some embodiments, the method for manufacturing the negative electrode sheet 21 further includes the following steps:

[0149] A second colloidal coating 216 is provided: the negative electrode current collector 211 includes a sixth surface 2114, the third surface 2113 and the sixth surface 2114 are arranged opposite to each other along the first direction, and the sixth surface 2114 connects the first surface 2111 and the second surface 2112; a polymer material is coated on a portion of the first surface 2111, the sixth surface 2114 and a portion of the second surface 2112 to form a second colloidal coating 216.

[0150] In order to verify the influence of various dimensions of the first colloid coating 215 on the performance of the secondary battery 100, the inventors conducted the following experiments:

[0151] The experiment includes a group of comparative examples and 14 groups of embodiments, each group of comparative examples and embodiments includes 35 secondary batteries 100. The negative electrode sheet 21 of the secondary battery 100 used in the comparative example is not provided with the first colloidal coating 215, and the negative electrode sheet 21 of the secondary battery 100 in the embodiment is provided with the first colloidal coating 215, and other aspects are the same. The secondary batteries 100 in different groups of embodiments differ only in the parameters listed in Table 1 below, and other aspects are the same.

[0152] The assembly process of the secondary battery in the comparative example is as follows:

[0153] (1) Preparation of positive electrode sheet 22: Active materials lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), CNT (carbon nanotube), polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 97.5:0.5:0.5:1.5, N-methylpyrrolidone (NMP) is added as a solvent, and a positive active material material with a solid content of 75wt% is prepared, and stirred evenly for use. Aluminum foil with a thickness of 10μm is used as the positive current collector 221. The above active material material is evenly coated on the fourth side 2211 of the positive current collector 221 using a slit coater, and then dried at 90°C to obtain a positive electrode sheet 22 coated with a single-sided positive active material material. At this time, the thickness of the positive active material layer 222 along the thickness direction of the positive current collector 221 is 90μm. Then repeat the above coating steps on the fifth side 2212 of the positive current collector 221. The coated positive electrode sheet 22 is then cold pressed, and after cold pressing, the thickness of the positive electrode active material layer 222 is 80 μm. The positive electrode tab 223 is then welded to the portion of the positive electrode current collector 221 not covered by the positive electrode active material layer 222, wherein the portion not covered by the positive electrode active material layer 222 is the end of the positive electrode sheet 22 in the length direction.

[0154] (2) Preparation of negative electrode sheet 21: Active materials artificial graphite, conductive carbon black (Super P), styrene-butadiene rubber (SBR), and CMC (sodium carboxymethyl cellulose) are mixed in a weight ratio of 97:0.5:1.3:1.2, and deionized water is added as a solvent to prepare a negative electrode active material material with a weight percentage of 50 wt%, and stirred evenly for use. A copper foil with a thickness of 10 μm is used as the negative electrode current collector 211. The above negative electrode active material is evenly coated on the first surface 2111 of the negative electrode current collector 211 using a slit coater, and then dried at 110° C. to obtain a negative electrode sheet 21 coated with a first negative electrode active material layer 212. Then, the above steps are repeated on the second surface 2112 of the negative electrode current collector 211 to obtain a negative electrode sheet 21 coated with a second negative electrode active material layer 213. At this time, the thickness of the first negative electrode active material layer 212 and the second negative electrode active material layer 213 along the thickness direction of the negative electrode current collector 211 is 90 μm. The coated negative electrode sheet 21 is then cold pressed, and the thickness of the first negative electrode active material layer 212 and the second negative electrode active material layer 213 is 80 μm after cold pressing. The negative electrode ear 214 is then welded to the portion of the negative electrode current collector 211 that is not covered by the first negative electrode active material layer 212 and the second negative electrode active material layer 213, wherein the portion that is not covered by the first negative electrode active material layer 212 and the second negative electrode active material layer 213 is the end of the negative electrode sheet 21 in the length direction.

[0155] (3) Preparation of electrolyte: In a dry argon atmosphere, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were first mixed in a mass ratio of EC:EMC:DEC=30:50:20 to form a basic organic solvent, and then lithium salt lithium hexafluorophosphate (LiPF6) was added to the basic organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.

[0156] (4) Preparation of isolation membrane: A 7 μm thick polyethylene porous polymer film was used as the isolation membrane.

[0157] (5) Preparation of the electrode assembly 20 : The positive electrode sheet 22 , the separator, and the negative electrode sheet 21 are stacked and wound along the thickness direction of the negative electrode sheet 21 to obtain the electrode assembly 20 .

[0158] (6) Assembly of secondary battery 100: Place the aluminum-plastic film with a hole punched into an assembly fixture, with the hole facing upward, place the electrode assembly 20 in the hole, and apply external force to press it. Then, cover the electrode assembly 20 with another aluminum-plastic film with a hole punched into it, with the hole facing downward. Heat-seal the three edges of the two aluminum-plastic films by hot pressing. The unsealed edge is the side where the negative electrode ear 214 and the positive electrode ear 223 extend out of the shell 10. Then, inject electrolyte through the unsealed edge, and after vacuum packaging, static placement, hot pressing, shaping and other processes, the secondary battery 100 is manufactured.

[0159] The manufacturing method of the negative electrode sheet 21 in the secondary battery 100 in Examples 1-14 also includes the step of setting the first colloid coating 215 in the above content, and other preparation processes and parameters are the same as those in the comparative example. Within the range of manufacturing error allowed, the secondary battery 100 in Examples 1-14 satisfies: T1=T2, W1=W2.

[0160] After the secondary batteries 100 in the comparative example and embodiments 1-14 were prepared, the thickness of the secondary batteries 100 in the group was measured and the voltage drop per unit time was tested.

[0161] The thickness was measured by using a flat plate thickness gauge (PPG) under a force of 700 g.

[0162] The method of the voltage drop per unit time test is: when the secondary battery 100 stores 60% of the power, at 25±5°C, measure its voltage, record it as the first voltage, and after standing for 48 hours, measure its voltage again, record it as the second voltage, and the voltage drop per unit time is recorded as K, K=(first voltage-second voltage) / standing time. The average value of the voltage drop per unit time in the comparative example and the embodiment is the average value of the voltage drop per unit time of the 35 secondary batteries in the group.

[0163] After measuring the voltage drop per unit time, 10 secondary batteries 100 are randomly selected from each group for a drop test, and another 10 secondary batteries 100 are randomly selected for a cycle test.

[0164] The drop test includes the following steps:

[0165] (1) Testing the voltage of the secondary battery 100 at 25±5° C., recorded as the third voltage;

[0166] (2) The secondary battery 100 is placed in a drop fixture (the fixture weighs 150 g and is made of PP). The secondary battery 100 is dropped from a height of 1.5 m onto a cement floor in the directions of top, bottom, left, right, front, back, upper left corner, upper right corner, lower right corner, and lower left corner, for three rounds of testing.

[0167] (3) After standing at 25±5°C for 48 hours, the secondary battery is tested for 100 voltage again. The test result is recorded as the fourth voltage. The voltage drop of each secondary battery 48 hours after 3 rounds of drops = the third voltage - the fourth voltage. The average voltage drop of each group 48 hours after 3 rounds of drops is the average voltage drop of the 10 secondary batteries in the group 48 hours after 3 rounds of drops.

[0168] The cycle test includes the following steps:

[0169] (1) The secondary battery 100 prepared above was charged at a constant current of 0.5C at room temperature (25±5°C), charged at a constant voltage of 0.05C to an upper cut-off voltage, left standing for 10 min, and discharged at 1C to a lower cut-off voltage, left standing for 10 min. The above process was recorded as one cycle (1cl). The above charge and discharge process was repeated 800 times (800cls).

[0170] (2) Disassemble the secondary battery 100, observe the lithium deposition, and record the lithium deposition as no lithium deposition, slight lithium deposition, and moderate lithium deposition according to the degree of lithium deposition, wherein no lithium deposition: the lithium deposition area is equal to 0; slight lithium deposition: 0<lithium deposition area / negative electrode area ≤5%; moderate lithium deposition: 5%<lithium deposition area / negative electrode area ≤15%; severe lithium deposition: 15%<lithium deposition area / negative electrode area. Here, the negative electrode area refers to the negative electrode active material layer where the precipitated lithium crystals are located (the area of ​​the first negative electrode active material layer 212 or the second negative electrode active material layer 213).

[0171] After the experiment, the experimental data were sorted out to obtain the following Table 1:

[0172] Table 1

[0173]

[0174] Note: “ / ” means there is no experimental data for this item.

[0175] By comparing the comparative example with any one of the groups in Examples 1-14, it can be seen that when the first colloidal coating 215 is not provided, the voltage drop of the secondary battery 100 after falling is large, and the average voltage drop per unit time is also large. It can be seen that by providing the first colloidal coating 215, the possibility of burrs falling between the positive electrode sheet and the diaphragm or between the negative electrode sheet and the diaphragm can be reduced, which is beneficial to improving the problem of poor K value (i.e., voltage drop per unit time) of the secondary battery 100.

[0176] W1 in Example 3-7 satisfies: 0.1L1≤W1≤0.5L1. Compared with Example 1-2, the average thickness of the secondary battery is only slightly increased, and the average voltage drop per unit time and the average voltage drop 48H after 3 rounds of drops are significantly decreased. It can be seen that under this condition, the width of the first part 2151 covering the first negative electrode active material layer 212 is not too small, which is beneficial to reduce the possibility of separation of the active material in the first negative electrode active material layer 212; compared with Example 8, the secondary battery in Example 3-7 did not show lithium deposition in the 800cl s cycle test. It can be seen that under this condition, the width of the first part 2151 covering the first negative electrode active material layer 212 is not too large, which is beneficial to the electrolyte infiltration of the electrode assembly 20.

[0177] The secondary batteries in Examples 10-13 satisfy 0.1T≤T1≤0.5T. Compared with Example 9, the average thickness of the secondary batteries is only slightly increased, and the average voltage drop per unit time and the average voltage drop 48H after 3 rounds of drops are significantly decreased. It can be seen that under this condition, the maximum distance from the surface of the first part 2151 to the surface of the first negative electrode active material layer 212 is not too small, which is beneficial to ensure the wrapping and restraining effect of the first colloidal coating 215 on the burrs; compared with Example 14, the secondary batteries in Examples 10-13 did not show lithium plating in the 800c ls cycle test. It can be seen that under this condition, the maximum distance from the surface of the first part 2151 to the surface of the first negative electrode active material layer 212 is not too large, which is beneficial to the electrolyte infiltration of the electrode assembly 20.

[0178] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present application and are not intended to be limiting of the present application. As long as they are within the spirit and scope of the present application, appropriate changes and modifications to the above embodiments are within the scope of the present application.

Claims

1. A secondary battery, characterized in that: It comprises a negative electrode sheet, a positive electrode sheet and a separator, wherein the negative electrode sheet, the separator and the positive electrode sheet are sequentially stacked along the thickness direction of the negative electrode sheet; The negative electrode sheet comprises: A negative electrode current collector, the negative electrode current collector comprising a first surface and a second surface arranged opposite to each other along the thickness direction of the negative electrode sheet, the negative electrode current collector further comprising a third surface located at one end of the negative electrode sheet along the first direction, the first direction being perpendicular to the thickness direction of the negative electrode sheet, the third surface connecting the first surface and the second surface; a first negative electrode active material layer and a second negative electrode active material layer, wherein the first negative electrode active material layer is disposed on the first surface, and the second negative electrode active material layer is disposed on the second surface; a first colloidal coating connected to the negative electrode current collector, the first colloidal coating comprising a first portion, a second portion and a third portion, the first portion connecting a portion of the first surface, the second portion connecting a portion of the second surface, the third portion being disposed on the third surface, and the third portion connecting the first portion and the second portion; Along the thickness direction of the negative electrode sheet, the projection of the first portion is located within the first plane, and the projection of the second portion is located within the second plane.

2. The secondary battery according to claim 1, wherein: Along the thickness direction of the negative electrode sheet, at least part of the first portion is overlapped on a part of the surface of the first negative electrode active material layer on a side away from the first surface; and / or Along the thickness direction of the negative electrode sheet, at least part of the second portion is overlapped on a portion of the surface of the second negative electrode active material layer on a side away from the second surface.

3. The secondary battery according to claim 1, wherein: The negative electrode sheet, the separator and the positive electrode sheet are stacked in sequence and then wound to form a winding structure; The negative electrode sheet further includes a negative electrode ear, and the negative electrode ear is welded to the negative electrode current collector; The positive electrode sheet includes a positive electrode collector, a positive electrode active material layer and a positive electrode ear. The positive electrode collector includes a fourth surface and a fifth surface arranged opposite to each other along its thickness direction. One positive electrode active material layer is arranged on the fourth surface, and one positive electrode active material layer is arranged on the fifth surface. The positive electrode ear is welded to the positive electrode collector.

4. The secondary battery according to claim 1, wherein: The negative electrode sheet, the separator and the positive electrode sheet are stacked in sequence and then wound to form a winding structure; The negative electrode sheet further includes a negative electrode ear, and the negative electrode ear is integrally arranged with the negative electrode current collector; The positive electrode sheet includes a positive electrode collector, a positive electrode active material layer and a positive electrode ear. The positive electrode collector includes a fourth surface and a fifth surface arranged opposite to each other along the thickness direction of the positive electrode sheet. One positive electrode active material layer is arranged on the fourth surface, and one positive electrode active material layer is arranged on the fifth surface. The positive electrode ear is integrally arranged with the positive electrode collector.

5. The secondary battery according to claim 1, wherein: A plurality of the negative electrode sheets, a plurality of the separators and a plurality of the positive electrode sheets are stacked along the thickness direction of the negative electrode sheets to form a stacked structure, and adjacent negative electrode sheets and positive electrode sheets are separated by the separators; The negative electrode sheet further includes a negative electrode ear, and the negative electrode ear is integrally arranged with the negative electrode current collector; The positive electrode sheet includes a positive electrode collector, a positive electrode active material layer and a positive electrode ear. The positive electrode collector includes a fourth surface and a fifth surface arranged opposite to each other along the thickness direction of the positive electrode sheet. The positive electrode active material layer is arranged on at least one of the fourth surface and the fifth surface. The positive electrode ear is integrally arranged with the positive electrode collector.

6. The secondary battery according to claim 2, wherein: Along the first direction, the width of the negative electrode sheet is D1, the width of the positive electrode sheet is D2, and D1>D2; Both ends of the negative electrode sheet along the first direction extend beyond the positive electrode sheet; The first colloid coating is located at a portion of the negative electrode sheet that exceeds the positive electrode sheet in the first direction.

7. The secondary battery according to claim 6, characterized in that: The diaphragm is bonded to the first colloid coating.

8. The secondary battery according to claim 7, characterized in that The first negative electrode active material layer extends to the edge of the negative electrode current collector provided with the first colloidal coating, and along the thickness direction of the negative electrode sheet, the first portion is overlapped on a portion of the surface of the first negative electrode active material layer on a side away from the first surface; Along the first direction, the distance from the third surface to the positive electrode sheet is L1; Along the first direction, a width of an overlapping region between the first portion and the first negative electrode active material layer is W1, and W1 satisfies: 0.1L1≤W1≤0.5L1.

9. The secondary battery according to claim 8, characterized in that W1 satisfies: 0.2L1≤W1≤0.4L1.

10. The secondary battery according to claim 7, wherein: The thickness of the positive electrode sheet is T; Along the thickness direction of the negative electrode sheet, the maximum distance from the surface of the first portion to the first surface is greater than the thickness of the first negative electrode active material layer, and the maximum distance from the surface of the first portion to the surface of the first negative electrode active material layer is T1; Along the thickness direction of the negative electrode sheet, the maximum distance from the surface of the second portion to the second surface is greater than the thickness of the second negative electrode active material layer, and the maximum distance from the surface of the second portion to the surface of the second negative electrode active material layer is T2; T1+T2≤T.

11. The secondary battery according to claim 10, characterized in that: T, T1 and T2 meet the following requirements: 0.1T≤T1≤0.5T; 0.1T≤T2≤0.5T.

12. The secondary battery according to claim 11, wherein: T, T1 and T2 satisfy: 0.2T≤T1≤0.4T; 0.2T≤T2≤0.4T.

13. The secondary battery according to claim 1, wherein: The negative electrode current collector includes a sixth surface, the third surface and the sixth surface are arranged opposite to each other along the first direction, and the sixth surface connects the first surface and the second surface; The negative electrode sheet includes a second colloidal coating, the second colloidal coating includes a fourth part, a fifth part and a sixth part, the fourth part is arranged on part of the first surface, the fifth part is arranged on part of the second surface, the sixth part is arranged on the sixth surface, and the sixth part connects the fourth part and the fifth part.

14. The secondary battery according to claim 1, wherein: The material of the first colloid coating layer includes hot-melt resin.

15. The secondary battery according to claim 14, characterized in that: The hot melt resin is selected from at least one of ethylene-vinyl acetate copolymer and polyethylene oxide.

16. An electrical equipment, characterized in that: The invention comprises the secondary battery according to any one of claims 1 to 15.

17. A method for manufacturing a negative electrode sheet, used for manufacturing the negative electrode sheet in the secondary battery as claimed in claim 1, characterized in that: The following steps are involved: Providing a negative electrode active material layer: coating a negative electrode active material on at least a portion of the surface of the first surface to form the first negative electrode active material layer; coating a negative electrode active material on at least a portion of the surface of the second surface to form the second negative electrode active material layer; Providing a first colloid coating: coating a polymer material on a portion of the first surface, the third surface and a portion of the second surface to form the first colloid coating.

18. The method for manufacturing a negative electrode sheet according to claim 17, wherein: The following steps are involved: A second colloidal coating is provided: the negative electrode current collector includes a sixth surface, the third surface and the sixth surface are arranged opposite to each other along the first direction, and the sixth surface connects the first surface and the second surface; a polymer material is coated on part of the first surface, the sixth surface and part of the second surface to form the second colloidal coating.

Citation Information

Patent Citations

  • Electrode assembly, battery monomer, battery and electric equipment

    CN115275092A

  • Pole piece and battery

    CN218602503U

  • Lamination structure and battery cell

    CN219626720U

  • Electrode assembly and manufacturing method and manufacturing system therefor, battery cell and battery

    WO2022165689A1

Cited By

  • Secondary battery, electric device, and preparation method for secondary battery

    WO2026199411A1